Method for producing silica-coated boron nitride particles, silica-coated boron nitride particles

By coating boron nitride particles with a specific organic silicone compound and heating to form a silica film, the method addresses the issue of reduced thermal conductivity and adhesive properties in conventional coatings, resulting in silica-coated particles with enhanced moisture resistance and thermal conductivity for use in heat dissipating resin compositions.

JP7582190B2Active Publication Date: 2024-11-13RESONAC CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021530726
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-11
Filing Date
2020-07-09
Publication Date
2024-11-13
Estimated Expiration
2040-07-09

AI Technical Summary

Technical Problem

Conventional methods for improving the moisture resistance of boron nitride particles by agglomeration or surface coating reduce their thermal conductivity and adhesive properties, making it difficult to blend them at high filling rates in various materials.

Method used

Coating boron nitride particles with a specific organic silicone compound and heating them at 500°C to 1000°C to form a silica film with a carbon content of 1000 mass ppm or less, maintaining high thermal conductivity and enhancing moisture resistance.

Benefits of technology

The method produces silica-coated boron nitride particles with improved moisture resistance and adhesive properties while preserving thermal conductivity, suitable for use in heat dissipating resin compositions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582190000012
    Figure 0007582190000012
  • Figure 0007582190000001
    Figure 0007582190000001
  • Figure 0007582190000002
    Figure 0007582190000002
Patent Text Reader

Abstract

The purpose of the invention is to provide a method for producing silica-coated boron nitride particles which is capable of producing silica-coated boron nitride particles which keep the high thermal conductivity of boron nitride particles while having improved moisture resistance and adhesiveness, a method for producing a heat-dissipating resin composition containing silica-coated boron nitride particles, and silica-coated boron nitride particles. The invention provides a method for producing silica-coated boron nitride particles comprising boron nitride particles and silica coating covering the surface of the boron nitride particles, said method comprising a first step of coating the surface of the boron nitride particles with an organic silicone compound containing a specific structure and a second step of heating the boron nitride particles coated with the organic silicone compound at a temperature of between 500°C and 1,000°C inclusive, thereby allowing boron nitride particles coated with a rigid, homogeneous, and ultra-thin film silica to be obtained.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to silica-coated boron nitride particles and a method for producing the same, as well as a method for producing a heat-dissipating resin composition containing the silica-coated boron nitride particles. [Background technology]

[0002] Boron nitride has high thermal conductivity and excellent electrical insulation. In particular, boron nitride with a hexagonal crystal structure has a layered structure similar to graphite, and is relatively easy to synthesize and has excellent thermal conductivity, electrical insulation, low dielectric constant, solid lubrication, chemical stability, and heat resistance. Therefore, boron nitride is promising as a filler for resin compositions used in products such as heat dissipation sheets, thermally conductive insulating sheets, and sealing materials for electronic components. However, boron nitride reacts with moisture to cause hydrolysis and denature into boron oxide, which has low thermal conductivity. In addition, boron nitride also generates ammonia, which is corrosive, during hydrolysis.

[0003] The hydrolysis of boron nitride also progresses due to moisture in the air. Therefore, products containing boron nitride may experience performance degradation under high temperature and humidity conditions, including reduced moisture resistance and thermal conductivity, as well as corrosion caused by ammonia produced by the hydrolysis of boron nitride.

[0004] As a technique for improving the moisture resistance of boron nitride, for example, a method of aggregating primary particles of hexagonal boron nitride to form secondary aggregate particles (see, for example, Patent Document 1), a method of surface treatment with a silane coupling agent having an amino group or a mercapto group (see, for example, Patent Document 2), a method of surface treatment with a silane coupling agent having a vinyl group and assembling without orientation (see, for example, Patent Document 3), a method of mechanochemical treatment with a coupling agent such as a silane coupling agent (see, for example, Patent Document 4), and a method of overlapping and aggregating the (0001) faces of primary particles of hexagonal boron nitride treated with a coupling agent (see, for example, Patent Document 5), etc. have been proposed. It has also been proposed to improve the hydrophobicity by modifying the surface of boron nitride particles using a cyclic silicone compound (Patent Document 6). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2016-127046 A [Patent Document 2] Patent No. 4070345 [Patent Document 3] JP 2012-56818 A [Patent Document 4] JP 2015-71730 A [Patent Document 5] JP 2018-30752 A [Patent Document 6] Patent No. 5074012 Summary of the Invention [Problem to be solved by the invention]

[0006] However, the conventional techniques have the following problems. In the above-mentioned conventional techniques, the boron nitride powder is agglomerated or a coating layer or surface modification layer is formed using a coupling agent in order to improve moisture resistance. As a result, the moisture resistance is improved to a certain extent, but it is still not at a sufficient level. Conversely, the coating used as a means for improving moisture resistance often reduces the thermal conductivity of boron nitride itself, or reduces the adhesiveness when the boron nitride powder is blended as a filler in various materials. Furthermore, there is a problem that it becomes difficult to blend the boron nitride powder as a filler in various materials at a high filling rate. The method described in Patent Document 6 is a technology that uses active hydrogen derived from cyclic silicone as a starting point and expands into various chemical modifications, and is completely different in purpose and focus from the treatment method of the present invention described below, which forms an ultra-thin layer by baking. Although some improvement in moisture resistance was observed, the coating on the surface reduced the thermal conductivity of the original boron nitride.

[0007] The present invention has been made to solve the above-mentioned problems, and has an object to provide a method for producing silica-coated boron nitride particles that can produce silica-coated boron nitride particles that maintain the high thermal conductivity of the boron nitride particles and have improved moisture resistance and adhesion, a method for producing a heat-dissipating resin composition containing the silica-coated boron nitride particles, and silica-coated boron nitride particles. [Means for solving the problem]

[0008] As a result of intensive research, the present inventors have found that the above-mentioned problems can be solved by coating boron nitride particles with a specific organosilicon compound by a specific method, and have completed the present invention. That is, the present invention has the following configuration.

[0009] [1] A method for producing silica-coated boron nitride particles comprising boron nitride particles and a silica coating covering the surfaces of the boron nitride particles, the method comprising: a first step of covering the surfaces of the boron nitride particles with an organosilicon compound having a structure represented by the following formula (1); and a second step of heating the boron nitride particles covered with the organosilicon compound at a temperature of 500°C or higher and 1000°C or lower, wherein the silica-coated boron nitride particles have a carbon atom content of 1000 ppm by mass or less. [ka] (In formula (1), R is an alkyl group having 4 or less carbon atoms.)

[0010] [2] The mass of silicon atoms (ppm by mass) on the surface of silica-coated boron nitride particles is calculated by multiplying the BET specific surface area (m 2 / g), i.e., the surface area of ​​a boron nitride particle per m 2 The mass of silicon atoms per unit mass (μg) is 50 to 500 (μg / m 2 The method for producing silica-coated boron nitride particles according to [1],

[0011] [3] The method for producing silica-coated boron nitride particles according to [1] or [2], wherein the first step is carried out by a dry mixing method or a gas phase adsorption method.

[0012] [4] The method for producing silica-coated boron nitride particles according to any one of [1] to [3], wherein the first step is carried out in an atmosphere not containing oxygen gas.

[0013] [5] The method for producing silica-coated boron nitride particles according to any one of [1] to [4], wherein the organosilicone compound having the structure represented by formula (1) comprises at least one of a compound represented by the following formula (2) and a compound represented by the following formula (3): [ka] (In formula (2), R1 and R2 each independently represent a hydrogen atom or a methyl group, at least one of R1 and R2 represents a hydrogen atom, and m represents an integer of 0 to 10.) [ka] (In formula (3), n is an integer of 3 to 6.)

[0014] [6] The method for producing silica-coated boron nitride particles according to any one of [1] to [5], wherein the first step is carried out under a temperature condition of 10° C. or higher and 200° C. or lower.

[0015] [7] A method for producing a heat-dissipating resin composition, comprising: a step of producing silica-coated boron nitride particles by the method for producing silica-coated boron nitride particles according to any one of [1] to [6]; and a mixing step of mixing the silica-coated boron nitride particles with a resin.

[0016] [8] Silica-coated boron nitride particles comprising boron nitride particles and a silica coating covering the surfaces of the boron nitride particles, the silica-coated boron nitride particles having a carbon atom content of 1000 ppm by mass or less.

[0017] [9] The mass of silicon atoms (mass ppm) on the surface of silica-coated boron nitride particles is calculated by multiplying the BET specific surface area (m 2 / g), i.e., the surface area of ​​a boron nitride particle per m 2 The mass of silicon atoms per unit mass (μg) is 50 to 500 (μg / m 2 The silica-coated boron nitride particles according to [8], Effect of the Invention

[0018] According to the present invention, it is possible to provide a method for producing silica-coated boron nitride particles that can produce silica-coated boron nitride particles that maintain high thermal conductivity and have improved moisture resistance and adhesion, a method for producing a heat-dissipating resin composition containing the silica-coated boron nitride particles, and silica-coated boron nitride particles. [Brief description of the drawings]

[0019] [Figure 1] 1 is a flow chart showing a method for producing silica-coated boron nitride particles of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] The present invention will be described in detail below.

[0021] <<Manufacturing method of silica-coated boron nitride particles>> The method for producing silica-coated boron nitride particles of the present invention produces silica-coated boron nitride particles comprising boron nitride particles and a silica coating covering the surfaces of the boron nitride particles. The method for producing silica-coated boron nitride particles of the present invention comprises a first step of covering the surfaces of boron nitride particles with an organosilicon compound having a structure represented by the following formula (1), and a second step of heating the boron nitride particles covered with the organosilicon compound at a temperature of 500°C or higher and 1000°C or lower, and the silica-coated boron nitride particles are characterized in that they have a carbon atom content of 1000 ppm by mass or less. [ka] (In formula (1), R is an alkyl group having 4 or less carbon atoms.)

[0022] Such a method for producing silica-coated boron nitride particles of the present invention will be described in detail with reference to Figure 1. Figure 1 is a flow chart showing the method for producing silica-coated boron nitride particles of the present invention.

[0023] [Boron nitride particles] In the method for producing silica-coated boron nitride particles of the present invention, the boron nitride particles used as raw materials can be commercially available or other known products. There is no particular limitation on the method for producing boron nitride particles, and for example, a method of reacting molten boric anhydride with nitrogen or ammonia using calcium phosphate as a catalyst, a method of reacting boric acid or an alkali borate with an organic nitrogen compound such as urea, guanidine, or melamine in a high-temperature nitrogen-ammonia atmosphere, a method of reacting molten sodium borate with ammonium chloride in an ammonia atmosphere, or a method of reacting boron trichloride with ammonia at high temperatures, and the like, may be obtained by any of these methods. In addition, boron nitride (BN) is known to have various crystal structures such as hexagonal boron nitride, cubic boron nitride, and rhombohedral boron nitride, and any of these can be used in the present invention. Among these boron nitrides, hexagonal boron nitride is particularly preferred because it has excellent thermal conductivity and voltage resistance, is easily available on an industrial scale, and is inexpensive.

[0024] In addition, as boron nitride particles, aggregates of boron nitride fine particles (primary particles) and particles obtained by sintering aggregates into granules can also be used. In particular, sintered granules made from high-purity boron nitride fine particles having a cumulative volume d50 of about 0.1 to 20 μm can be suitably used as boron nitride particles. Although the spray-drying method is generally used as a granulation method, it is not limited thereto, and for example, crushed and classified sintered molded products are also used industrially.

[0025] Here, the high-purity boron nitride microparticles refer to particles with a low oxygen content and low metal impurities. Specifically, for example, high-purity boron nitride with an oxygen content of 1 mass% or less and a total metal impurity content of 1000 mass ppm or less is suitable for obtaining higher thermal conductivity of the boron nitride particles contained in the silica-coated boron nitride particles.

[0026] The boron nitride particles can be used alone or in combination.

[0027] The oxygen content can be measured by an inorganic analyzer equipped with an infrared detector for oxygen detection. Specifically, the oxygen content can be measured by using an oxygen / nitrogen / hydrogen analyzer (ONH836: manufactured by LECO Japan LLC).

[0028] Furthermore, the total content of metal atoms contained in the boron nitride particles can be measured using an ICP (Inductively Coupled Plasma) mass spectrometer, etc. Specifically, the total content of metal atoms can be measured using an ICP mass spectrometer (ICPMS-2030: manufactured by Shimadzu Corporation).

[0029] In this specification, the cumulative volume d50 of particles refers to the particle size at which the cumulative volume is 50% for a certain particle size distribution. The cumulative volume d50 is determined from the particle size distribution by the laser diffraction scattering method, and specifically, the cumulative volume d50 can be measured using a laser diffraction / scattering type particle size distribution analyzer (Microtrac MT3300EX2: manufactured by Microtrac BEL Co., Ltd.).

[0030] The shape of the boron nitride particles used in the present invention is not particularly limited, and for example, the particle shape of the primary particles of boron nitride is not particularly limited, and examples thereof include, for example, scale-like, flat, granular, spherical, amorphous (crushed), spherical, elliptical, fibrous, whisker-like, and the like, with the scale-like being preferred. In addition, when the silica-coated boron nitride particles are dispersed and contained in a heat-dissipating resin composition as a filler for a heat-dissipating material, the boron nitride particles may be only the same type of boron nitride particles (single object) having the same shape and structure, or may be a mixture of two or more different types of boron nitride particles having different shapes and structures mixed in various ratios.

[0031] When silica-coated boron nitride particles are dispersed and contained in a heat-dissipating resin composition, the larger the volume ratio (filling amount) of the boron nitride particles constituting the silica-coated boron nitride particles to the heat-dissipating resin composition, the higher the thermal conductivity of the heat-dissipating resin composition. Therefore, it is preferable that the shape of the boron nitride particles is close to a sphere, which reduces the increase in viscosity of the heat-dissipating resin composition due to the addition of the silica-coated boron nitride particles.

[0032] The average aspect ratio of boron nitride particles (index of particle shape) is preferably in the range of 0.8 to 1.0, more preferably in the range of 0.85 to 1.0, and even more preferably in the range of 0.9 to 1.0. Here, the average aspect ratio of boron nitride particles is the arithmetic mean value of the ratio (D1 / D2) of the minor axis (D1) and major axis (D2) measured for each of 100 randomly selected particles in an electron microscope photograph. The minor axis (D1) is the minimum length between two parallel lines in the electron microscope photograph of the boron nitride particle, and the major axis (D2) is the maximum length between two parallel lines in the electron microscope photograph.

[0033] The cumulative volume d50 of the boron nitride particles used in the present invention is preferably in the range of 0.1 μm to 200 μm, more preferably 0.2 μm to 100 μm, and further preferably 0.5 μm to 50 μm.

[0034] When the cumulative volume d50 of the boron nitride particles is within the above-mentioned range, even when a heat-dissipating resin composition containing silica-coated boron nitride particles is used in a heat-dissipating material for mounting electric power electronic components, it becomes possible to supply a thin heat-dissipating material with a minimum thickness, and the moisture resistance of the boron nitride particles is further improved, probably because the coating can easily uniformly cover the surface of the boron nitride particles.

[0035] Furthermore, since the method for producing silica-coated boron nitride particles of the present invention can form a thin silica coating layer, the effect on thermal conductivity is small even when relatively fine boron nitride particles with a cumulative volume d50 of 50 μm or less are used.

[0036] Furthermore, although not particularly limited, the boron nitride particles may be surface-treated with, for example, a silane coupling agent before or after silica coating with an organic silicone compound described later. Although no synergistic effect is observed between the silica coating according to the present invention and the improvement in thermal conductivity or adhesion by performing treatment with a silane coupling agent, it can be used in combination from the viewpoint of dispersibility in resin when, for example, silica-coated boron nitride particles are added to various resins to prepare a heat dissipating resin composition, or agglomeration when forming aggregates of boron nitride particles (primary particles).

[0037] The above-mentioned silane coupling agent can be one having an alkyl group, an aryl group, an amino group, an epoxy group, an isocyanato group, an alkoxy group, or a mercapto group. The above-mentioned coupling agent is not particularly limited, but it is also possible to use, for example, silane coupling agents having a crosslinked structure such as 1,6-bis(trimethoxysilyl)hexane, tris-(trimethoxysilylpropyl)isocyanurate, bis(triethoxysilylpropyl)tetrasulfide, and hexamethyldisilazane.

[0038] In addition, the silane coupling agent having the above-mentioned crosslinked structure can also be obtained by reacting and crosslinking between organic functional groups.The combination of organic functional groups in this case is not limited to the following, but can be, for example, the combination of organic functional groups of coupling agent such as amino group-epoxy group, epoxy group-isocyanato group, amino group-isocyanato group, amino group-sulfo group, amino group-halogen, mercapto group-isocyanato group, etc.

[0039] The above-mentioned various coupling agents may be used alone or in combination of two or more.

[0040] [Organosilicone compounds used for coating] In the method for producing silica-coated boron nitride particles of the present invention, the organosilicon compound used as the raw material for the silica coating constituting the silica-coated boron nitride particles can be any organosilicon compound containing the structure represented by the above formula (1), regardless of whether it is linear, cyclic or branched. The structure represented by formula (1) is a hydrogensiloxane unit in which hydrogen is directly bonded to a silicon atom.

[0041] In the above formula (1), R, which is an alkyl group having 4 or less carbon atoms, is preferably a methyl group, an ethyl group, a propyl group, a t-butyl group, etc., and is particularly preferably a methyl group. In the method for producing silica-coated boron nitride particles of the present invention, the organosilicon compound used as a raw material is, for example, an oligomer or polymer containing a structure represented by formula (1).

[0042] As the organosilicone compound, for example, a compound represented by the following formula (2) and a compound represented by the following formula (3) are suitable. [ka] (In formula (2), R1 and R2 each independently represent a hydrogen atom or a methyl group, at least one of R1 and R2 represents a hydrogen atom, and m represents an integer of 0 to 10.) [ka] (In formula (3), n is an integer of 3 to 6.)

[0043] In particular, the cyclic hydrogen siloxane oligomer in which n is 4 in the above formula (3) is excellent in that it can form a uniform coating on the surface of boron nitride particles. The mass average molecular weight of the organosilicone compound containing the structure shown in formula (1) is preferably 100 to 2000, more preferably 150 to 1000, and even more preferably 180 to 500. It is presumed that by using an organosilicone compound containing the structure shown in formula (1) with a mass average molecular weight in this range, it is easy to form a thin and uniform coating on the surface of boron nitride particles. In addition, in formula (2), m is preferably 0 to 6, more preferably 0 to 3, and most preferably 1.

[0044] In this specification, the mass average molecular weight is a polystyrene equivalent mass average molecular weight measured by gel permeation chromatography (GPC), and specifically, it can be measured by using a column (Shodex (registered trademark) LF-804, manufactured by Showa Denko K.K.) in combination with a differential refractive index detector (Shodex (registered trademark) RI-71S, manufactured by Showa Denko K.K.).

[0045] <1st process> In the first step, the surfaces of the boron nitride particles are covered with an organosilicone compound containing the structure represented by the above formula (1). In the first step, the method is not particularly limited as long as the surface of the boron nitride particles can be covered with an organic silicone compound containing the structure represented by formula (1). The method of the first step includes a dry mixing method in which an organic silicone compound is added by spraying or the like while stirring the raw material boron nitride particles using a general powder mixer, and then dry-mixed to coat the particles. Examples of powder mixers include a Henschel mixer (registered trademark), a container-rotating V-type blender, a double cone blender, a ribbon blender with a mixing blade, a screw-type blender, a closed rotary kiln, and stirring with a stirrer in a closed container using a magnetic coupling. The temperature conditions in this case are not particularly limited depending on the boiling point and vapor pressure of the silicone compound containing the structure represented by formula (1), but are preferably in the range of 10°C to 200°C, more preferably 20°C to 150°C, and even more preferably 40°C to 100°C.

[0046] As a method for the first step, a gas-phase adsorption method can be used in which the vapor of an organosilicon compound containing the structure represented by formula (1) alone or a mixed gas with an inert gas such as nitrogen gas is attached or deposited on the surface of boron nitride particles placed at rest. The temperature conditions in this case are not particularly limited depending on the boiling point and vapor pressure of the silicone compound containing the structure represented by formula (1), but the preferred temperature is 10°C to 200°C, more preferably 20°C to 150°C, and even more preferably 40°C to 90°C. If the temperature conditions are 10°C to 200°C, the organosilicon compound containing the structure represented by formula (1) can be efficiently attached to the surface of boron nitride particles. Furthermore, if necessary, the system can be pressurized or depressurized. In this case, a closed system and a system that can easily replace the gas in the system are preferred, and for example, a glass container, a desiccator, a CVD device, etc. can be used. When covering boron nitride particles with an organosilicon compound without stirring, the treatment time needs to be longer. However, by intermittently placing the processing container on the vibrator, even areas where powder particles are in contact with each other and in the shadow, or powder particles far from the air layer above, can be efficiently processed by moving the position.

[0047] Gas phase treatment can also be carried out by making a vaporized organosilicon compound present in the atmosphere of equipment such as a Henschel mixer, a container-rotating V blender, a double cone blender or the like, which are given as examples of powder mixing equipment in the section explaining the dry mixing method, a ribbon blender having mixing blades, a screw blender, a sealed rotary kiln, a sealed container using a magnetic coupling, or a multistage band dryer using a belt conveyor.

[0048] The amount of the organosilicon compound containing the structure represented by formula (1) used in the first step is not particularly limited. However, organosilicon compounds are expensive, and there is a reasonable upper reference value. Finally, the mass of silicon atoms (ppm by mass) on the surface of the silica-coated boron nitride particles derived from the organosilicon compound containing the structure represented by formula (1) is calculated by multiplying the BET specific surface area (m 2 / g), i.e., the surface area of ​​a boron nitride particle per m 2 The mass of silicon atoms per unit mass (μg) is 50 to 500 (μg / m 2 ), and more preferably 60 to 400 (μg / m 2 ), and more preferably 70 to 300 (μg / m 2 Within the above range, silica-coated boron nitride particles that are particularly excellent in both thermal conductivity and moisture resistance can be obtained.

[0049] The specific surface area determined by the BET method can be measured by a nitrogen adsorption BET one-point method using a gas flow method. As an evaluation device, Macsorb HM model-1210 manufactured by Mountech can be used.

[0050] <Second process> In the second step, the boron nitride particles covered with the organosilicon compound obtained in the first step are heated at a temperature of 500° C. or more and 1000° C. or less, thereby forming a silica coating on the surface of the boron nitride particles. In the second step, a general heating furnace can be used as long as it can heat the boron nitride particles coated with the organosilicon compound obtained in the first step at a temperature of 500°C or higher and 1000°C or lower, that is, as long as it can maintain the boron nitride particles coated with the organosilicon compound obtained in the first step in a temperature range of 500°C or higher and 1000°C or lower.

[0051] In the heat treatment of the second step, the organosilicon compounds containing the structure represented by formula (1) that coat the surface of the boron nitride particles in the early stage of the heat treatment are bonded to each other or to hydroxyl groups on the surface of the boron nitride particles by dehydrogenation, which is thought to further strengthen the coating. Then, at the end of the heat treatment, the organic groups of the organosilicon compounds (alkyl groups having 4 or less carbon atoms) are decomposed and volatilized. Therefore, the silica coating formed has a low carbon atom content, and the carbon atom content of the silica-coated boron nitride particles also decreases. Therefore, silica-coated boron nitride particles having a carbon atom content of 1000 mass ppm or less can be obtained. If the carbon atom content of the silica-coated boron nitride particles is 1000 mass ppm or less, the moisture resistance is good, and unevenly distributed carbon particles are unlikely to affect the insulation properties. The carbon atom content of the silica-coated boron nitride particles is preferably 700 mass ppm or less, more preferably 500 mass ppm or less.

[0052] Note that silica coating means that the material is coated with a thin film whose main component is silica (SiO2). However, since there may be multiple inorganic compounds at the interface between the coated silica and the boron nitride particle, when analyzing with ToF-SIMS (Time of Flight Secondary Ion Mass Spectrometry, ION-TOF, TOF.SIMS5), recombination of secondary ions and decomposition during ionization may occur, and segments such as BSiO4 ions and SiNO ions may be detected as secondary components. The composite segments analyzed by ToF-SIMS analysis can also be defined as partial detections when boron nitride is silicaized. As a guideline, if the amount of secondary electrons of silica is greater than that of other fractions, silica can be considered to be the main component.

[0053] As an experiment to confirm the purity of silica with further accuracy, a sample surface in which a silica film was formed on a boron nitride polycrystalline substrate in the same manner was measured with a photoelectron spectroscopy device (XPS: X-ray Photoelectron Spectroscopy, ULVAC-PHI, Inc., Quantera II). The kinetic energy of the detected Si-derived photoelectrons was almost identical to the standard peak of silica, 103.7 eV, so it is presumed that most of the silica has a SiO2 structure. Depending on the heating temperature, organic components may remain. As long as the effect of the present invention is not impaired, it is quite possible that organic siloxane components are mixed in.

[0054] The carbon atom content can be measured using a carbon-sulfur analyzer that uses a non-dispersive infrared absorption method using a tubular electric furnace. Specifically, it can be measured using a carbon-sulfur analyzer (Carbon Anlyzer EMIA-821: manufactured by Horiba, Ltd.).

[0055] The heating temperature (heat treatment temperature) in the second step is 500°C or higher and 1000°C or lower. By performing the process within this temperature range, a silica coating having good moisture resistance and thermal conductivity is formed. Specifically, when the silica coating is heated at 500°C or higher, the moisture resistance is good, possibly because the silica coating becomes dense and difficult to transmit moisture. In addition, when the silica coating is heated at 1000°C or lower, the thermal conductivity is good. In addition, when the heating temperature is 500°C or higher and 1000°C or lower, a silica coating is uniformly formed on the surface of the boron nitride particles. In addition, when the heating temperature is 500°C or higher, the silica coating has excellent insulating properties, and when the heating temperature is 1000°C or lower, it is effective in terms of energy cost. The heating temperature is more preferably 550°C or higher, and even more preferably 600°C or higher. In addition, in the case of an oxidizing atmosphere such as air, the upper limit is preferably 950°C or lower, and even more preferably 900°C or lower. In the case of an inert atmosphere or a reducing gas atmosphere, there is no problem if the temperature is 1000°C or lower.

[0056] The heating time is preferably 30 minutes to 20 hours, more preferably 45 minutes to 10 hours, and even more preferably 1 hour to 8 hours. A heat treatment time of 30 minutes or more is preferable in that no decomposition products of the organic group (alkyl group having 4 or less carbon atoms) of the organosilicon compound remain, and a silica coating with a very low carbon atom content is obtained on the surface of the boron nitride particles. In addition, a heating time of 20 hours or less is preferable in that silica-coated boron nitride particles can be produced efficiently.

[0057] The heat treatment in the second step may be performed in an atmosphere containing oxygen gas, for example in the atmosphere (air), or in an inert atmosphere such as nitrogen, or in a reducing gas atmosphere such as nitrogen containing 2% hydrogen.

[0058] After the heat treatment in the second step, silica-coated boron nitride particles may be partially fused together. In that case, by crushing the particles, silica-coated boron nitride particles that are not stuck or aggregated can be obtained. The device used for crushing is not particularly limited, but a general crusher such as a roller mill, hammer mill, jet mill, or ball mill can be used.

[0059] Furthermore, after the second step is completed, the first step and the second step may be carried out in sequence. That is, the step of carrying out the first step and the second step in sequence may be repeated.

[0060] When the surface of the boron nitride particles is covered with an organic silicone compound by gas-phase adsorption in the first step, the gas-phase adsorption coating method is capable of forming a uniform and thin silica coating compared to the liquid treatment coating method. Therefore, even if the first step and the second step are performed in sequence multiple times, for example 2 to 5 times, the boron nitride particles can exhibit good thermal conductivity.

[0061] On the other hand, regarding moisture resistance, a positive correlation is observed between the number of steps of sequentially performing the first step and the second step and the moisture resistance. Therefore, the number of steps of sequentially performing the first step and the second step can be freely selected according to the level of moisture resistance required for practical applications.

[0062] The silica-coated boron nitride particles obtained by the above-mentioned method for producing silica-coated boron nitride particles of the present invention maintain the high thermal conductivity inherent to boron nitride particles and also have excellent moisture resistance, and therefore can be widely used as a filler for heat dissipation materials used in the electrical and electronic fields, etc.

[0063] <<Silica-coated boron nitride particles>> The method for producing silica-coated boron nitride particles of the present invention described above makes it possible to obtain the silica-coated boron nitride particles of the present invention, i.e., silica-coated boron nitride particles comprising boron nitride particles and a silica coating covering the surfaces of the boron nitride particles, and having a carbon atom content of 1000 ppm by mass or less.

[0064] As shown in the examples described later, the silica-coated boron nitride particles of the present invention maintain the high thermal conductivity of boron nitride particles and have excellent moisture resistance. For example, when the silica-coated boron nitride particles of the present invention are put into a hydrochloric acid aqueous solution adjusted to pH 4 and treated at 85°C for 2 hours (i.e., the silica-coated boron nitride particles are immersed in a hydrochloric acid aqueous solution adjusted to pH 4 at 85°C for 2 hours), the concentration of ammonia extracted in the hydrochloric acid aqueous solution can be 20mg / L or less, and the particles have extremely excellent moisture resistance. Since the hydrolysis reaction is promoted in an acidic solution more than in air, an accelerated moisture resistance test can be performed by exposing the particles to a hydrochloric acid aqueous solution adjusted to pH 4. Therefore, the moisture resistance of the silica-coated boron nitride particles can be evaluated by using a hydrochloric acid aqueous solution with a pH of 4, and if the concentration of the ammonia is 20mg / L or less, it can be said that the moisture resistance is good. In addition, the use of a hydrochloric acid aqueous solution with a pH of 4 also allows comparison of chemical resistance.

[0065] The concentration of the extracted ammonia is preferably 10 mg / L or less, and more preferably 6 mg / L or less.

[0066] From the viewpoint of moisture resistance, the lower the carbon atom content, the better.Here, in the manufacturing method of silica-coated boron nitride particles of the present invention, since the organic silicone compound having the structure represented by formula (1) is used as raw material, silica-coated boron nitride particles often contain carbon atoms, for example, 50 mass ppm or more, or even 60 mass ppm or more.However, as mentioned above, if the carbon atom content is 1000 mass ppm or less, moisture resistance is excellent.

[0067] The silicon atom content can be quantified using an inductively coupled plasma (ICP) emission spectrometer. Specifically, the sample was heated and melted together with sodium carbonate and boric acid in a platinum crucible, and then dissolved in sulfuric acid (concentrated sulfuric acid / distilled water = 1 / 1 (mass ratio)) for measurement.

[0068] In addition, the surface area of ​​a boron nitride particle is 1 m 2 Silicon atom mass per unit (μg / m 2 ) is calculated by subtracting the silicon atom content of the raw material boron nitride particles from the total silicon atom content of the silica-coated boron nitride particles, to obtain the silicon atom content (ppm by mass) derived from the coating layer, and multiplying it by the BET specific surface area (m 2 / g), the value is 50 to 500 (μg / m 2 ), and more preferably 60 to 400 (μg / m 2 ), and more preferably 70 to 300 (μg / m 2 ) or less. 2 ) or more, sufficient moisture resistance is obtained, and 500 (μg / m 2 ) or less, sufficient thermal conductivity can be obtained.

[0069] <<Method for producing heat dissipating resin composition>> The silica-coated boron nitride particles of the present invention can be used to produce a heat-dissipating resin composition. That is, the method for producing a heat-dissipating resin composition of the present invention includes a mixing step of mixing the silica-coated boron nitride particles produced by the method for producing silica-coated boron nitride particles with a resin.

[0070] The silica-coated boron nitride particles produced by the above-mentioned method for producing silica-coated boron nitride particles maintain the high thermal conductivity of boron nitride particles and have improved moisture resistance, so the heat-dissipating resin composition obtained by the method for producing a heat-dissipating resin composition of the present invention has excellent moisture resistance and thermal conductivity.

[0071] In the mixing step, the silica-coated boron nitride particles produced by the above-mentioned method for producing silica-coated boron nitride particles are mixed with a resin.

[0072] The resin to be mixed in the mixing step is not particularly limited, but is preferably a thermosetting resin, a thermoplastic resin, or a mixture of a thermosetting resin and a thermoplastic resin, in that the resulting heat dissipating resin composition has excellent heat resistance. Examples of the thermosetting resin include silicone resin, epoxy resin, phenol resin, bismaleimide resin, cyanate resin, urethane resin, (meth)acrylic resin, vinyl ester resin, unsaturated polyester resin, polyvinyl alcohol acetal resin, etc., and can be used alone or in combination of two or more kinds. Furthermore, a mixture of a thermosetting resin with a curing agent or a curing accelerator may be used. In particular, epoxy resin is preferable in terms of good heat resistance, adhesiveness, and electrical properties after curing, and silicone resin is preferable for applications in which flexibility and adhesion are important.

[0073] Silicone resins include addition reaction curing silicone resins, condensation reaction curing silicone resins, and organic peroxide curing silicone resins, and can be used alone or in combination of two or more types with different viscosities. In particular, when the obtained heat dissipating resin composition is used in an application that emphasizes soft adhesion, the silicone resin can be, for example, an addition reaction curing liquid silicone resin that does not generate by-products that can cause bubbles, and a silicone resin cured product can be obtained by reacting an organopolysiloxane having an alkenyl group as a base polymer with an organopolysiloxane having a Si-H group as a crosslinking agent at room temperature or by heating in the presence of a curing agent. Specific examples of the organopolysiloxane as a base polymer include those having a vinyl group, an allyl group, a propenyl group, a hexenyl group, etc. as an alkenyl group. In particular, a vinyl group is preferable as an organopolysiloxane. In addition, a platinum metal-based curing catalyst can be used as the curing catalyst, and the amount of addition can be adjusted to achieve the desired hardness of the resin cured product.

[0074] Examples of epoxy resins include bifunctional glycidyl ether type epoxy resins such as bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, hydrogenated bisphenol A type epoxy resins, and biphenyl type epoxy resins; glycidyl ester type epoxy resins such as hexahydrophthalic acid glycidyl ester and dimer acid glycidyl ester; linear aliphatic epoxy resins such as epoxidized polybutadiene and epoxidized soybean oil; heterocyclic epoxy resins such as triglycidyl isocyanurate; and N,N,N',N'-tetraglycidyl-4,4' -diaminodiphenylmethane, N,N,N',N'-tetraglycidyl-1,3-benzenedi(methanamine), 4-(glycidyloxy)-N,N-diglycidylaniline, 3-(glycidyloxy)-N,N-diglycidylaniline and other glycidylamine type epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, biphenyl aralkyl type epoxy resins, naphthalene aralkyl type epoxy resins, tetrafunctional naphthalene type epoxy resins, triphenylmethane type epoxy resins and other polyfunctional glycidyl ether type epoxy resins. The above-mentioned epoxy resins can be used alone or in combination of two or more kinds.

[0075] When the above-mentioned epoxy resin is used, a curing agent and a curing accelerator may be blended therein. Examples of the curing agent include alicyclic acid anhydrides such as methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, and himic anhydride, aliphatic acid anhydrides such as dodecenylsuccinic anhydride, aromatic acid anhydrides such as phthalic anhydride and trimellitic anhydride, bisphenols such as bisphenol A, bisphenol F, and bisphenol S, phenol resins such as phenol-formaldehyde resin, phenol-aralkyl resin, naphthol-aralkyl resin, and phenol-dicyclopentadiene copolymer resin, and organic dihydrazides such as dicyandiamide and adipic acid dihydrazide. Examples of the curing catalyst include amines such as tris(dimethylaminomethyl)phenol, dimethylbenzylamine, 1,8-diazabicyclo(5,4,0)undecene and derivatives thereof, imidazoles such as 2-methylimidazole, 2-ethyl-4-methylimidazole, and 2-phenylimidazole and derivatives thereof. These can be used alone or in combination of two or more kinds.

[0076] In the mixing step, in addition to the silica-coated boron nitride particles, a commonly used filler such as alumina, silica, aluminum nitride, zinc oxide, etc. may be used in combination.

[0077] In the mixing step, the silica-coated boron nitride particles and fillers other than the silica-coated boron nitride particles may be mixed in amounts sufficient to provide a desired heat dissipating resin composition. The total content of the silica-coated boron nitride particles and fillers other than the silica-coated boron nitride particles in the obtained heat-dissipating resin composition is preferably 50% by volume or more and 95% by volume or less, more preferably 60% by volume or more and 90% by volume or less, and even more preferably 70% by volume or more and 90% by volume or less. If the total content is 50% by volume or more, good heat dissipation properties can be exhibited, and if it is 95% by volume or less, good workability can be obtained when using the heat-dissipating resin composition.

[0078] The content of the silica-coated boron nitride particles in the obtained heat-dissipating resin composition is preferably 30% by volume or more and 100% by volume or less of the total content of the silica-coated boron nitride particles and fillers other than the silica-coated boron nitride particles, more preferably 40% by volume or more and 100% by volume or less, and even more preferably 50% by volume or more and 100% by volume or less. When the total content is 30% by volume or more, good heat dissipation properties can be exhibited.

[0079] In the mixing step, further, flexibility imparting agents such as silicone, urethane acrylate, butyral resin, acrylic rubber, diene rubber and copolymers thereof, silane coupling agents, titanium coupling agents, inorganic ion scavengers, pigments, dyes, diluents, solvents and the like can be appropriately added as necessary.

[0080] The mixing method in the mixing step is not particularly limited, and examples thereof include a method in which the silica-coated boron nitride particles, resin, other additives, etc. are mixed, dissolved, and kneaded together or divided into portions using a dispersing / dissolving device such as a grinder, planetary mixer, rotation / revolution mixer, kneader, or roll mill, either alone or in appropriate combination, and heated as necessary.

[0081] The obtained heat dissipating resin composition can be formed into a sheet and reacted as necessary to form a heat dissipating sheet. The heat dissipating resin composition and heat dissipating sheet described above can be suitably used for bonding applications such as semiconductor power devices and power modules.

[0082] Examples of manufacturing methods for heat dissipation sheets include a method of molding a heat dissipation resin composition by a compression press or the like in a form in which both sides are sandwiched between substrate films, and a method of applying a heat dissipation resin composition onto a substrate film using a device such as a bar coater, screen printing, blade coater, die coater, or comma coater. Furthermore, the heat dissipation sheet after molding and application can be subjected to additional processing steps such as a process of removing the solvent, heating to bring the composition into a B-stage, or complete curing. As described above, various forms of heat dissipation sheets can be obtained by the process, making it possible to widely respond to the target fields of application and methods of use.

[0083] When applying or forming the heat dissipating resin composition on the substrate film, a solvent can be used to improve workability. The solvent is not particularly limited, but includes ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, and cyclohexanone, ether solvents such as 1,4-dioxane, tetrahydrofuran, and diglyme, glycol ether solvents such as methyl cellosolve, ethyl cellosolve, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monobutyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, and diethylene glycol methyl ethyl ether, as well as benzyl alcohol, N-methylpyrrolidone, γ-butyrolactone, ethyl acetate, and N,N-dimethylformamide, which can be used alone or in combination.

[0084] In order to form the heat dissipating resin composition into a sheet, it is necessary to have sheet formability that maintains the sheet shape. In order to obtain sheet formability, a high molecular weight component can be added to the heat dissipating resin composition. For example, phenoxy resin, polyimide resin, polyamide resin, polycarbodiimide resin, cyanate ester resin, (meth)acrylic resin, polyester resin, polyethylene resin, polyethersulfone resin, polyetherimide resin, polyvinyl acetal resin, urethane resin, acrylic rubber, etc. can be mentioned. Among them, from the viewpoint of excellent heat resistance and film formability, phenoxy resin, polyimide resin, (meth)acrylic resin, acrylic rubber, cyanate ester resin, polycarbodiimide resin, etc. are preferable, and phenoxy resin, polyimide resin, (meth)acrylic resin, acrylic rubber are more preferable. They can be used alone or as a mixture or copolymer of two or more kinds.

[0085] The molecular weight of the high molecular weight component is preferably in the range of 10,000 to 100,000, and more preferably 20,000 to 50,000.

[0086] The good sheet shape with good handleability can be maintained by adding a component having a mass average molecular weight within the above-mentioned range.

[0087] The amount of the high molecular weight component added is not particularly limited, but in order to maintain the sheet properties, it is preferably 0.1% by mass to 20% by mass, more preferably 1% by mass to 15% by mass, and even more preferably 2% by mass to 10% by mass, based on the heat dissipating resin composition. Note that an amount of 0.1% by mass to 20% by mass provides good handling and allows the formation of a good sheet or film.

[0088] The substrate film used in the manufacture of the heat dissipation sheet is not particularly limited as long as it can withstand the process conditions such as heating and drying during manufacture, and examples thereof include films made of polyesters having aromatic rings, such as polyethylene terephthalate (PET) and polybutylene terephthalate (PBT), polypropylene films, polyimide films, and polyetherimide films. The above-mentioned films may be multi-layer films combining two or more types, and may have a surface treated with a release agent such as a silicone-based release agent. The thickness of the substrate film is preferably 10 μm or more and 100 μm or less.

[0089] The thickness of the heat dissipation sheet formed on the base film is preferably 20 μm to 500 μm, more preferably 50 μm to 200 μm. When the thickness of the heat dissipation sheet is 20 μm or more, a heat dissipation sheet with a uniform composition can be obtained, and when the thickness is 500 μm or less, good heat dissipation properties can be obtained. EXAMPLES

[0090] The present invention will be specifically described below with reference to examples and comparative examples, but the scope of the present invention is not limited to these examples in any way.

[0091] [Measurement of carbon atom content in silica-coated boron nitride particles] The carbon atom content of the silica-coated boron nitride particles was measured using a carbon-sulfur analyzer (Carbon Anlyzer EMIA-821: manufactured by Horiba, Ltd.) using the non-dispersive infrared absorption method with a tubular electric furnace.

[0092] [Measurement of silicon atom content in silica-coated boron nitride particles] The silicon atom content of the silica-coated boron nitride particles was measured by the following procedure. (1) A 30 cc platinum crucible was placed in a 50 cc Teflon (registered trademark) container. (2) 10 cc of a solution of 98% by mass sulfuric acid (super grade, manufactured by Wako Pure Chemical Industries, Ltd.) and ion-exchanged water mixed in a 2:1 (volume ratio) and 0.5 g of a sample (silica-coated boron nitride particles) were placed in a platinum crucible. (3) The Teflon (registered trademark) container was placed in a stainless steel pressure container and maintained at 230°C for 15 hours to dissolve the placed sample. (4) The solution mixed in (1) was taken out, and the concentration of silicon atoms was measured using an ICP (Shimadzu Corporation, ICPS-7510) to determine the silicon concentration per 1 g of silica-coated boron nitride particles. The atomic content (μg) was calculated and the obtained value was expressed in ppm by mass. The silicon content of the raw material boron nitride can also be measured in the same manner.

[0093] [Measurement of specific surface area of ​​boron nitride particles using the BET method] The specific surface area of ​​the boron nitride particles was measured by the BET method using a Macsorb HM model-1210 manufactured by Mountech Co., Ltd. A mixed gas of 70% by volume of He and 30% by volume of N2 was used as the adsorption gas.

[0094] [Boron nitride particle surface area 1m 2 [silicon atomic mass per The content of silicon atoms derived from the coating layer (mass ppm: μg / g), which is calculated by subtracting the silicon atom content of the raw material boron nitride particles from the total silicon atom content of the silica-coated boron nitride particles obtained above, is calculated as the BET specific surface area (m 2 / g) to obtain the surface area of ​​the boron nitride particles per square meter. 2 Silicon atom mass per unit (μg / m 2 The calculated surface area of ​​the boron nitride particles per m 2 The silicon atomic mass per surface area is given in the "Silicon atomic mass per surface area" column of the table.

[0095] [Evaluation of moisture resistance of silica-coated boron nitride particles] The moisture resistance of the silica-coated boron nitride particles was measured by placing 17 g of hydrochloric acid aqueous solution adjusted to pH 4 and 3 g of silica-coated boron nitride particles in a 50 ml sample tube, sealing it, shaking it in a shaking thermostatic bath at 85°C, 80 rpm, for 2 hours, leaving it to stand, and then cooling it to room temperature (25°C).The ammonia concentration in the supernatant was measured at a temperature of 25°C using LAQUA manufactured by Horiba, Ltd.

[0096] [Measurement of thermal conductivity of resin sheet (heat dissipation sheet)] (1) Measurement of thermal conductivity of epoxy resin sheet using the laser flash method The thermal diffusivity of the resin sheet was measured at 25° C. using a laser flash thermal diffusivity measuring device (LFA447 NanoFlash: manufactured by NETZSCH).

[0097] For the thermal diffusivity measurement, the resin sheet was cut into a size of 10 mm x 10 mm, the thickness was measured, and the specific gravity of the 10 mm square sample was measured by Archimedes' method. The specific heat was calculated from the volume fraction of the resin and the filler used. The device obtains thermal diffusivity, so Thermal conductivity = thermal diffusivity x specific gravity (density) x specific heat The thermal conductivity was calculated using the formula: The resin sheet used for the measurement was gold-coated on both sides using an ion coater (IB-3, manufactured by Eiko Co., Ltd.), and then graphite-coated on both sides.

[0098] (2) Measurement of thermal conductivity of cured silicone resin using the hot disk method Using pellets prepared by the method described below, measurements were carried out using a hot disk heat dissipation physical property measuring device TPS 2500 (hereinafter referred to as hot disk) manufactured by Kyoto Electronics Manufacturing Co., Ltd. The specific heat capacity was calculated from the resin and the volume fraction of the filler used. The pellet was clamped at two points on the center of the measuring terminal and fixed in place. The output power was 0.3 W, the measurement time was 5 s, and the calculated specific heat capacity was input, and the measurement was carried out to obtain the thermal conductivity.

[0099] [Adhesion (90° peel strength) test measurement] The adhesiveness was evaluated by 90° peel strength using a digital force gauge / measurement stand ZTS-5N manufactured by Imada Co., Ltd. The preparation of the test samples was in accordance with the method for preparing the epoxy resin sheet described below. Both sides were adhered and cured to the treated side of 35 μm thick copper foil, and processed into a 1.5 cm wide strip. Only one side of the strip was fixed to a plate of appropriate thickness with double-sided tape and used for the measurement. Both ends of the copper foil on the side opposite the fixed side were peeled off, leaving 1 cm in the center of the 1.5 cm strip, and the remaining 1 cm wide copper foil was used to perform a 90° peel strength test using a specified jig at a peel speed of 200 mm / min to determine the peel strength (kN / mm). The basic measurement method was based on the peel strength test method of JIS C 6481:1996 for laminates for printed wiring boards.

[0100] [Particle preparation] (boron nitride filler) The following was used as the boron nitride filler (boron nitride particles). A: Scaly boron, ShowbN (registered trademark) UHP-2 (manufactured by Showa Denko K.K.), volume-based median diameter (d 50 ) 11 μm, silicon content 143 mass ppm B: Scaly boron, ShowbN (registered trademark) UHP-1K (manufactured by Showa Denko K.K.), volume-based median diameter (d 50 ) 8 μm, silicon content 232 mass ppm C: Scaly boron, ShowbN (registered trademark) UHP-S2 (manufactured by Showa Denko K.K.), volume-based median diameter (d 50 ) 0.5 μm, silicon content 557 mass ppm D: Aggregated boron, ShowbN (registered trademark) UHP-G1H (manufactured by Showa Denko K.K.), volume-based median diameter (d 50 ) 15 μm, silicon content 251 mass ppm

[0101] (Surface treatment with silane coupling agent) The boron nitride particles used were prepared by pre-surface treatment with a silane coupling agent, and by post-addition of a silane coupling agent to silica-coated boron nitride particles. The silane coupling agent used was an epoxy silane coupling agent (KBM-403, Shin-Etsu Chemical Co., Ltd.) when preparing a composition with an epoxy resin, and an alkylalkoxysilane (Z-6210Silane, Dow-Toray Co., Ltd.) when preparing a composition with a silicone resin. The treatment method was to add 0.5 parts by mass of a silane coupling agent to 100 parts by mass of the filler to be treated, and then to stir for 30 seconds at 2000 rpm in a rotary mixer. The mixture was poured onto a tray and heated at 120°C for 30 minutes to obtain a pre-surface-treated filler. In the case of the integral blend method in which the silane coupling agent is added to the resin in advance, each silane coupling agent was added in an amount of 0.5 parts by mass to 100 parts by mass of the filler in advance when preparing the resin composition.

[0102] (Production of silica-coated boron nitride particles) Example 1 In the first step, the surface of the boron nitride particles was coated using a vacuum desiccator made of acrylic resin with a plate thickness of 20 mm, with inner dimensions of 260 mm x 260 mm x 100 mm, and divided into two levels by a partition with a through hole. Approximately 30 g of boron nitride particles A were evenly spread on a stainless steel tray in the upper level of the vacuum desiccator and left to stand. Next, 10 g of organosilicon compound-A (cyclic methylhydrogensiloxane tetramer: manufactured by Tokyo Chemical Industry Co., Ltd.) in which n = 4 in formula (3) was placed in a glass petri dish in the lower level of the vacuum desiccator and left to stand. After that, the vacuum desiccator was closed and heated in an oven at 80 ° C for 30 hours. The operation was performed with safety measures such as releasing hydrogen gas generated by the reaction through an open valve attached to the vacuum desiccator. After completing the first step, the sample was removed from the desiccator and placed in an alumina crucible. The sample was then subjected to heat treatment in the second step at 650°C for 1.5 hours in air to obtain silica-coated boron nitride particles.

[0103] Example 2 The surface coating of boron nitride particles was carried out in the same manner as in Example 1, except that the heat treatment time in the oven at 80° C. was changed to 30 minutes, to obtain silica-coated boron nitride particles.

[0104] (Reference example 1) In Example 1, the surface treatment with organosilicon compound-A was carried out by a liquid addition method, not a gas phase method. 30 g of boron nitride particles A and 2.5 g of organosilicon compound-A were added to a 150 ml resin container for a planetary mixer (Awatori Rentaro ARE-310), and then mixed for 1 minute at 2000 rpm with the planetary mixer, then mixed with a medicine spoon, and further mixed for 1 minute at 2000 rpm. The removed contents were transferred to an alumina crucible and fired under the same conditions as in Example 1 to obtain silica-coated boron nitride particles.

[0105] Example 3 The silica-coated boron nitride particles obtained in Example 1 were subjected to a surface treatment with a silane coupling agent by the above-mentioned method to obtain silica-coated boron nitride particles to which the silane coupling agent was added later.

[0106] Example 4 The same production as in Example 1 was carried out, except that the boron nitride particles A used as the raw material in Example 1 were replaced with boron nitride particles A that had been previously surface-treated with a silane coupling agent by the above-mentioned method.

[0107] Example 5 The same production as in Example 1 was carried out except that the boron nitride particles A used as the raw material in Example 1 were replaced with the boron nitride particles B.

[0108] Example 6 The same production as in Example 1 was carried out except that the boron nitride particles A used as the raw material in Example 1 were replaced with the boron nitride particles C.

[0109] Example 7 The same production as in Example 1 was carried out except that the boron nitride particles A used as the raw material in Example 1 were replaced with the boron nitride particles D.

[0110] Example 8 In Example 1, the heat treatment conditions in the second step were changed from 650°C for 1.5 hours to 800°C for 3 hours. In the same manner as in Example 1, surface coating of boron nitride particles was performed to obtain silica-coated boron nitride particles.

[0111] Example 9 In Example 6, the surface coating of boron nitride particles was carried out in the same manner as in Example 1, except that the heat treatment temperature in the second step was changed from 600° C. to 800° C., to obtain silica-coated boron nitride particles.

[0112] Comparative Example 1 The boron nitride particles A used as a raw material in Example 1, which were untreated and did not undergo any of the steps in Example 1, were used as particles in Comparative Example 1.

[0113] Comparative Example 2 The boron nitride particles A used as the raw material in Example 1 were not surface-treated, and when preparing a sheet for evaluating the composition characteristics, a sheet was prepared using an epoxy resin to which a specified amount of silane coupling agent had been added (integral blend method), and the sheet was used to measure the various characteristics of Comparative Example 2.

[0114] Comparative Example 3 The boron nitride particles A used as the raw material in Example 1 were subjected to a silane coupling treatment according to a specified recipe to obtain particles of Comparative Example 3.

[0115] Comparative Example 4 The boron nitride particles B used as the raw material in Example 5, which were untreated and did not undergo any of the steps in Example 5, were used as the particles in Comparative Example 4.

[0116] Comparative Example 5 The boron nitride particles C used as the raw material in Example 6, which were untreated and did not undergo any of the steps in Example 6, were used as the particles in Comparative Example 5.

[0117] Comparative Example 6 The boron nitride particles D used as the raw material in Example 7, which were untreated without undergoing any of the steps in Example 6, were used as the particles in Comparative Example 6.

[0118] (Examples 10 to 11 and Comparative Examples 7 to 8) In Example 10, particles similar to the silica-coated boron nitride particles of Example 1, in Example 11, particles similar to the silica-coated boron nitride particles of Example 3 to which a silane coupling agent was added later, in Comparative Example 7, particles similar to the untreated boron nitride particles of Comparative Example 1, and in Comparative Example 8, particles similar to the silica-coated untreated boron nitride particles of Comparative Example 2 to which a silane coupling agent was added later were prepared in order to prepare a composition using a silicone resin.

[0119] [Preparation of a composition using an epoxy resin and production of an epoxy resin sheet using the same] For each of the silica-coated boron nitride particles of Examples 1 to 9 and the boron nitride particles of Comparative Examples 1 to 6, a resin mixture in which a bisphenol A type epoxy resin (YD128: Nippon Steel Chemical & Material Co., Ltd.) having an epoxy equivalent of 189 as a resin component and a bisphenol A type phenoxy resin (YP-50S: Nippon Steel Chemical & Material Co., Ltd.) having a polystyrene equivalent weight average molecular weight of 40,000 as a high molecular weight component were mixed so that the mass ratio of the bisphenol A type epoxy resin to the phenoxy resin was 90:10 was dissolved in 1-methoxy-2-propanol (solvent) at 30 mass%, and 2-ethyl-4-methylimidazole (2E4MZ: Shikoku Chemical Industry Co., Ltd.) as a curing agent was mixed in the mass parts shown in Tables 1 and 2, and a resin sheet was obtained by the following procedure. The curing agent was mixed in an amount of 0.3 mass parts per 100 mass parts of the resin component (epoxy resin). Specifically, the necessary masses of the filler (silica-coated boron nitride particles of Examples 1 to 9 and boron nitride particles of Comparative Examples 1 to 6), resin component, high molecular weight component, and curing agent corresponding to the desired filling amount were calculated, and were weighed in the order listed. After manual stirring, a solvent was dropped to dilute the mixture to a concentration suitable for sheet coating, and the mixture was stirred five times at 2000 rpm for 30 seconds using a planetary mixer. Stirring was performed using a Thinky Foam Mixer. Note that the state of the composition was checked after each stirring. The composition thus obtained was made into a sheet. A 35 μm copper foil with electrolytic treatment on one side was used as the coating substrate. Note that the electrolytic surface was used as the coating surface. The resin composition layer was formed by coating the mixture to a thickness of 400 μm using a coater, and dried at 50° C. for 20 minutes and in a vacuum at 50° C. for 20 minutes. The two sheets were stacked so that the resin composition layers were in contact with each other, and passed through a roll, and the sheet pressure was adjusted so that the resin sheet had a thickness of 200 μm. Thereafter, the resin composition layer was cured by heat pressing at 120° C. for 30 minutes to prepare an epoxy resin sheet.

[0120] [Preparation of a composition using a silicone resin and production of pellets using the composition] A liquid two-component thermosetting silicone resin (product name "KE-109E A / B", manufactured by Shin-Etsu Chemical Co., Ltd.) was added as a resin component to each of the silica-coated boron nitride particles of Examples 10 to 11 and the boron nitride particles of Comparative Examples 7 to 8 in the amounts shown in Table 2 in parts by mass. Resin pellets were obtained by the following procedure. Specifically, the necessary masses of the filler (silica-coated boron nitride particles of Examples 10-11 and boron nitride particles of Comparative Examples 7-8) and resin components corresponding to the desired filling amount were calculated, and were weighed in the order listed. Since the silicone resin is a two-liquid curing type, the liquid without the curing catalyst and the filler were mixed first, and then the liquid containing the catalyst was added. After manual mixing, the mixture was mixed five times at 2000 rpm for 30 seconds using a planetary mixer. Mixing was performed using a Thinky Mixer. The composition was cooled during mixing to prevent curing from starting due to frictional heat generated during mixing. Next, the obtained composition was cured and molded according to the following procedure. A PET substrate and copper foil coated with a release agent were prepared on a steel plate, and a mold similarly coated with a release agent was placed on top of them. The composition was filled into the mold, sandwiched between the copper foil, PET substrate, and steel plate, and pressed in this state under a pressure of 8 tons. A curing treatment was performed at 120°C for 30 minutes, and cured pellets of the silicone composition (silicone resin sheets) were obtained.

[0121] For the boron nitride particles used and the silica-coated boron nitride particles obtained in the examples and comparative examples, [measurement of the specific surface area of ​​the boron nitride particles obtained by the BET method], [measurement of the carbon atom content of the silica-coated boron nitride particles], and [surface area of ​​the boron nitride particles per square meter calculated from the above] were measured. 2 The results of [Silicon atomic mass per unit area], [Evaluation of particle moisture resistance], [Adhesion (90° peel strength) test measurement], and [Measurement of thermal conductivity of resin sheet (heat dissipation sheet)] are shown in Table 2.

[0122] From these results, it can be seen that Examples 1, 3-7, 10 and 11 using silica-coated boron nitride particles obtained by the method for producing silica-coated boron nitride particles of the present invention can maintain high thermal conductivity of boron nitride particles and can remarkably improve moisture resistance and adhesiveness of boron nitride particles, respectively, compared with Comparative Examples 1-8 in which silica coating treatment was not performed. Furthermore, Examples 8 and 9, in which the heat treatment conditions in the second step were higher in temperature and / or longer in time than Examples 1 and 6, were comparable to Examples 1 and 6 in thermal conductivity and adhesiveness, while even better results were obtained in moisture resistance. In addition, comparing Examples 1-2 and Reference Example 1, if the silicon atomic mass per surface area is within a predetermined range, all of the moisture resistance, peel strength and thermal conductivity can be obtained with a certain degree of satisfaction, but there was a tendency that the moisture resistance decreased as the amount of silicon decreased, while the thermal conductivity decreased as the amount of silicon increased. In particular, in Examples 1, 5, 6, 7, 8, 9, and 10 in which the silane coupling treatment was not performed, good values ​​were shown not only in thermal conductivity but also in adhesiveness.

[0123] [Table 1]

[0124] [Table 2]

Claims

1. A method for producing silica-coated boron nitride particles comprising: boron nitride particles; and a silica coating covering a surface of the boron nitride particles, the method comprising the steps of: A first step of covering the surface of the boron nitride particles with an organosilicon compound having a structure represented by the following formula (1); A second step of heating the boron nitride particles covered with the organosilicon compound at a temperature of 500° C. or more and 1000° C. or less, The silica-coated boron nitride particles have a carbon atom content of 1000 ppm by mass or less, A method for producing silica-coated boron nitride particles, in which the mass of silicon atoms (ppm by mass) on the surface of the silica-coated boron nitride particles divided by the BET specific surface area (m2 / g) of the boron nitride particles before silica coating, i.e., the mass of silicon atoms (μg) per m2 of the surface area of ​​the boron nitride particles, is 50 to 500 (μg / m2). [Formula 1] (In formula (1), R is an alkyl group having 4 or less carbon atoms.)

2. 2. The method for producing silica-coated boron nitride particles according to claim 1, wherein the first step is carried out by a dry mixing method or a gas phase adsorption method.

3. 3. The method for producing silica-coated boron nitride particles according to claim 1, wherein the first step is carried out in an atmosphere not containing oxygen gas.

4. The method for producing silica-coated boron nitride particles according to any one of claims 1 to 3, wherein the organosilicon compound having a structure represented by formula (1) comprises at least one of a compound represented by the following formula (2) and a compound represented by the following formula (3): [chemical 2] (In formula (2), R1 and R2 each independently represent a hydrogen atom or a methyl group, at least one of R1 and R2 represents a hydrogen atom, and m represents an integer of 0 to 10.) [C3] (In formula (3), n is an integer from 3 to 6.)

5. The method for producing silica-coated boron nitride particles according to any one of claims 1 to 4, wherein the first step is carried out under a temperature condition of 10°C or higher and 200°C or lower.

6. A method for producing a heat dissipating resin composition, comprising: a step of producing silica-coated boron nitride particles by the method for producing silica-coated boron nitride particles according to any one of claims 1 to 5; and a mixing step of mixing the silica-coated boron nitride particles with a resin.

Citation Information

Patent Citations

  • Enhanced boron nitride composition and compositions made therewith

    CN101157770A

  • JP1975074012A

  • Hexagonal boron nitride powder and high heat conductivity and high moisture resistance heat radiation sheet using the same

    JP2012056818A

  • Surface-modified particle

    JP2015071730A

  • Granulated powder, resin composition for heat dissipation, heat dissipation sheet, semiconductor device, and heat dissipation member

    JP2016127046A