CURED BODY LAYER, PRINTED WIRING BOARD, SEMICONDUCTOR DEVICE, RESIN SHEET, METHOD FOR MANUFACTURING PRINTED WIRING BOARD, AND METHOD FOR MANUFACTURING RESIN SHEET

A cured body layer with controlled resin composition and plasma treatment effectively addresses the challenge of high-density wiring in multilayer printed wiring boards by ensuring smear removability and adhesion without fluorine-based gases, enhancing the efficiency and environmental sustainability of the manufacturing process.

JP7582227B2Active Publication Date: 2024-11-13AJINOMOTO CO INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022021262
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-02-15
Publication Date
2024-11-13
Estimated Expiration
2038-06-19

AI Technical Summary

Technical Problem

Existing methods for forming conductor layers on insulating layers in multilayer printed wiring boards face challenges in achieving high-density wiring due to the need for high adhesion despite low surface roughness, and plasma treatments using fluorine-based gases are costly and environmentally harmful, while nitrogen and oxygen plasma treatments are ineffective in removing inorganic fillers.

Method used

A cured body layer with a specific resin composition containing 40% inorganic filler by mass, where the resin component area ratio in certain regions near the conductor layer exceeds the inorganic filler, ensuring sufficient smear removability without fluorine-based gases, achieved through controlled plasma treatment with nitrogen and oxygen.

Benefits of technology

The solution provides excellent smear removability and high peel strength between the conductor and insulating layers, enabling high-density wiring without the use of fluorine-based gases, thus reducing environmental impact and costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582227000002
    Figure 0007582227000002
  • Figure 0007582227000003
    Figure 0007582227000003
  • Figure 0007582227000004
    Figure 0007582227000004
Patent Text Reader

Abstract

A hardened layer is provided that can ensure sufficient smear removal even when using plasma from N2 gas or O2 gas, which has low inorganic filler removal ability. The present invention provides a cured body layer formed of a cured product of a resin composition having an inorganic filler content of 40% by mass or more, the cured body layer being provided on the surface of a substrate having a conductor layer on at least a portion of the outermost layer, the surface being on the conductor layer side, the cured body layer comprising: A 0-1 / A 1-2 Hardened layer that satisfies >1.1.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cured layer, a printed wiring board, a semiconductor device, a resin sheet, a method for producing a printed wiring board, and a method for producing a resin sheet. [Background technology]

[0002] In recent years, electronic devices have become smaller and more powerful, and in multilayer printed wiring boards, build-up layers have become multi-layered, and wiring has become finer and denser. As a conductor formation method, for example, a semi-additive method in which a conductor layer is formed by electroless plating and electrolytic plating is known. The adhesion between an insulating layer and a plated conductor layer is affected by the degree of unevenness formed by roughening treatment of the insulating layer, and generally, in order to improve adhesion, it is considered to increase the roughness of the insulating layer surface.

[0003] However, when the surface roughness of an insulating layer is large, the width between circuits formed on the surface is inevitably restricted, which is disadvantageous for high-density wiring. Therefore, in order to realize high-density wiring, a method for forming a conductor layer having excellent adhesion even if the surface roughness after roughening treatment is small on the insulating layer surface is required.

[0004] Patent Document 1 discloses a method for producing a multilayer printed wiring board in which an adhesive film having a resin composition layer formed on a support film is laminated on a circuit board, the support film is peeled off after the resin composition layer is thermally cured, and a conductor layer is formed on the surface of an insulating layer by a sputtering method, thereby producing a multilayer printed wiring board in which the conductor layer exhibits high peel strength despite the relatively small roughness. Patent Document 2 also discloses that a resin composition is highly blended with an inorganic filler in order to eliminate the mismatch in the thermal expansion coefficient between the insulating layer and the copper wiring, and further discloses that a high peel strength is obtained despite the relatively small roughness in order to meet the demands of high density and miniaturization. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2007-273615 A [Patent Document 2] JP 2015-150885 A DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]

[0006] When a dry roughening process is applied to a conventional insulating layer (hardened layer) containing a high content of inorganic filler, plasma treatment using fluorine-based gases such as CF4 gas has good smear removal properties, but requires expensive equipment investment and has issues with its impact on the human body and the environment. On the other hand, plasma treatment using N2 gas or O2 gas, which has low inorganic filler removal properties, is unable to fully remove the inorganic filler and the resin components located below the inorganic filler, and therefore is unable to ensure sufficient smear removal properties.

[0007] Therefore, an object of the present invention is to provide a cured body layer that can ensure sufficiently good smear removal properties by plasma treatment with N2 gas or O2 gas, which have low inorganic filler removal ability, even without using a fluorine-based gas in the dry roughening step; a printed wiring board including the cured body layer and a manufacturing method thereof; a semiconductor device including the cured body layer; and a resin sheet from which the cured body layer can be obtained and a manufacturing method thereof. [Means for solving the problem]

[0008] As a result of intensive research into the above-mentioned problems, the inventors discovered that the above-mentioned problems can be solved by keeping the amount of inorganic filler relative to the resin component (inorganic filler / resin component) in the region of the cured body layer near the conductor layer relatively low, and thus completed the present invention.

[0009] That is, the present invention includes the following.

[0010] [1] A cured body layer formed on a surface of a substrate on the side of the conductor layer, the cured body layer being made of a cured resin composition having an inorganic filler content of 40% by mass or more, the cured body layer being provided on the surface of the conductor layer side of the substrate, In the cross-section of the cured body layer perpendicular to the main surface of the cured body layer, the area of the resin component per unit area in the region where the distance from the conductor layer is from 0 μm to 1 μm is A 0-1 and the area of the resin component per unit area in the region where the distance from the conductor layer is from 1 μm to 2 μm is A 1-2 When this is the case, A 0-1 / A 1-2 > 1.1 is satisfied, the cured body layer. [2] In the cross-section, the area of the resin component per unit area in the region where the distance from the conductor layer is from 0 μm to 0.5 μm is A 0-0.5 and the area of the resin component per unit area in the region where the distance from the conductor layer is from 0.5 μm to 1 μm is A 0.5-1 When this is the case, A 0-0.5 / A 0.5-1 > 1.1 is satisfied, the cured body layer according to [1]. [3] In the cross-section, the area of the resin component per unit area in the region where the distance from the conductor layer is from 0.5 μm to d μm is A 0.5-d and the area of the resin component per unit area in the region where the distance from the conductor layer is from d μm to 0.5D μm is A d-0.5D When this is the case, 0.9 ≦ A 0.5-d / A d-0.5D ≦ 1.1 (where d is a number satisfying 0.5 < d < 0.5D, and D is the thickness of the cured body layer.) is satisfied, the cured body layer according to [1] or [2]. [4] The cured body layer according to any one of [1] to [3], wherein the resin composition contains an epoxy resin. [5] The cured body layer according to [4], wherein the resin composition further contains an active ester-based curing agent. [6] The cured body layer according to [4] or [5], wherein the resin composition further contains a cyanate ester-based curing agent, and the content thereof is 15% by mass or more when the resin component in the resin composition is 100% by mass. [7] The cured body layer according to any one of [1] to [6], wherein the nitrogen atom content of the resin composition is 1% by mass or more when the resin component in the resin composition is 100% by mass. [8] The cured body layer according to any one of [1] to [7], wherein the cured body layer comprises a first cured body layer formed of a cured product of a first resin composition, and a second cured body layer formed of a cured product of a second resin composition having a composition different from that of the first resin composition, in this order from the side opposite to the substrate. [9] The cured body layer described in [8], wherein the thickness of the second cured body layer is less than 2 μm.

[10] The cured layer according to [8] or [9], wherein the second resin composition has an inorganic filler content of less than 20 mass%.

[11] The cured layer according to any one of [1] to

[10] , which is intended to be subjected to plasma treatment with one or more gases selected from the group consisting of O2 gas and N2 gas.

[0011]

[12] A printed wiring board comprising the cured body layer according to any one of [1] to

[11] and a substrate having a conductor layer.

[13] The printed wiring board according to

[12] , wherein a via hole having a top diameter of 15 μm or less is formed in the cured layer.

[14] A semiconductor device comprising the cured body layer according to any one of [1] to

[11] .

[0012]

[15] A resin sheet having a support and a resin composition layer having an inorganic filler content of 40% by mass or more, When the resin composition layer is cured to form a cured body layer, in a cross section of the cured body layer perpendicular to the main surface of the cured body layer, the area of ​​the resin component per unit area in a region from 0 μm to 1 μm away from the main surface of the cured body layer on the side opposite to the support is defined as A. 0-1 The area of ​​the resin component per unit area in the region from 1 μm to 2 μm is A 1-2 In this case, A 0-1 / A 1-2 > Resin sheet that meets 1.1.

[16] In the cross section, the area of ​​the resin component per unit area in the region from 0 μm to 0.5 μm away from the main surface of the cured body layer on the opposite side to the support is defined as A 0-0.5wherein, the area of the resin component per unit area in the region from 0.5 μm to 1 μm is A 0.5-1 in the case where 0-0.5 / A 0.5-1 > 1.1 is satisfied, the resin sheet according to

[15] .

[17] In the cross section, the area of the resin component per unit area in the region where the distance from the main surface of the cured body layer on the side opposite to the support is from 0.5 μm to d μm is A 0.5-d wherein, the area of the resin component per unit area in the region from d μm to 0.5D μm is A d-0.5D in the case where 0.9 ≦ 0.5-d / A d-0.5D ≦ 1.1 (where d is a number satisfying 0.5 < d < 0.5D, and D is the thickness of the cured body layer). The resin sheet according to

[15] or

[16] .

[18] The resin sheet according to any one of

[15] to

[17] , wherein the resin composition layer contains an epoxy resin.

[19] The resin sheet according to

[18] , wherein the resin composition layer further contains an active ester-based curing agent.

[20] The resin sheet according to

[18] or

[19] , wherein the resin composition layer further contains a cyanate ester-based curing agent, and the content thereof is 15% by mass or more when the resin component in the resin composition is 100% by mass.

[21] The resin sheet according to any one of

[15] to

[20] , wherein the nitrogen atom content of the resin composition layer is 1% by mass or more when the resin component in the resin composition is 100% by mass.

[22] The resin sheet according to any one of

[15] to

[21] , wherein the resin composition layer includes a first layer formed of a first resin composition and a second layer formed of a second resin composition having a composition different from that of the first resin composition, in this order from the support side.

[23] The resin sheet according to

[22] , wherein the thickness of the second layer is less than 2 μm.

[24] The resin sheet according to

[22] or

[23] , wherein the inorganic filler content of the second resin composition is less than 20% by mass.

[25] The resin sheet according to any one of

[15] to

[24] , wherein after the resin composition layer is cured to form a cured body layer, the cured body layer is subjected to a plasma treatment with one or more gases selected from the group consisting of O2 gas and N2 gas.

[0013]

[26] (A) laminating a resin sheet including a resin composition layer having an inorganic filler content of 40% by mass or more onto a substrate having a conductor layer in at least a part of an outermost layer, such that the resin composition layer is bonded to a surface of the substrate on the conductor layer side; (B) a step of curing the resin composition layer to form a cured body layer; (C) forming a via hole in the cured body layer; and (D) A step of subjecting the hardened body layer to a plasma treatment using one or more gases selected from the group consisting of O2 gas and N2 gas. A method for producing a printed wiring board comprising: In a cross section of the cured body layer perpendicular to the main surface of the cured body layer, the area of ​​the resin component per unit area in a region from 0 μm to 1 μm away from the conductor layer is defined as A 0-1 The area of ​​the resin component per unit area in the region from 1 μm to 2 μm is A 1-2 In this case, A 0-1 / A 1-2 A method for manufacturing a printed wiring board that satisfies 1.1.

[27] In the cross section, the area of ​​the resin component per unit area in the region from the conductor layer at a distance of 0 μm to 0.5 μm is defined as A 0-0.5 The area of ​​the resin component per unit area in the region from 0.5 μm to 1 μm is A 0.5-1 In this case, A 0-0.5 / A 0.5-1 The method for producing a printed wiring board according to

[26] , which satisfies the above requirement.

[28] In the cross section, the area of ​​the resin component per unit area in the region from 0.5 μm to d μm away from the conductor layer is defined as A 0.5-d The area of ​​the resin component per unit area in the region from dμm to 0.5Dμm is A d-0.5D In this case, 0.9≦A 0.5-d / A d-0.5D The manufacturing method of the printed wiring board according to

[26] or

[27] , satisfying ≦1.1 (where d is a number satisfying 0.5 < d < 0.5D, and D is the thickness of the cured body layer).

[29] The manufacturing method of the printed wiring board according to any one of

[26] to

[28] , wherein the resin composition layer contains an epoxy resin.

[30] The manufacturing method of the printed wiring board according to

[29] , wherein the resin composition layer further contains an active ester-based curing agent.

[31] The manufacturing method of the printed wiring board according to

[29] or

[30] , wherein the resin composition layer further contains a cyanate ester-based curing agent, and its content is 15% by mass or more when the resin component in the resin composition is 100% by mass.

[32] The manufacturing method of the printed wiring board according to any one of

[26] to

[31] , wherein the nitrogen atom content of the resin composition layer is 1% by mass or more when the resin component in the resin composition is 100% by mass.

[33] The manufacturing method of the printed wiring board according to any one of

[26] to

[32] , wherein the resin composition layer includes a first layer formed of a first resin composition and a second layer formed of a second resin composition having a composition different from that of the first resin composition.

[34] The manufacturing method of the printed wiring board according to

[33] , wherein the thickness of the second layer is less than 2 μm, and the second layer is joined to the substrate.

[35] The manufacturing method of the printed wiring board according to

[33] or

[34] , wherein the inorganic filler content of the second resin composition is less than 20% by mass.

[36] The manufacturing method of the printed wiring board according to any one of

[26] to

[35] , wherein step (A) includes laminating a resin sheet having a support and the resin composition layer formed on the support so that the resin composition layer is joined to the surface of the substrate on the conductor layer side.

[37] The manufacturing method of the printed wiring board according to any one of

[26] to

[36] , wherein the top diameter of the via hole is 15 μm or less.

[38] The manufacturing method of the printed wiring board according to any one of

[26] to

[37] , wherein step (D) is a step of performing plasma treatment with O2 gas.

[39] A method for manufacturing a resin sheet having a support and a resin composition layer with an inorganic filler content of 40% by mass or more, (α) A step of forming a second layer formed of a second resin composition having a composition different from that of the first resin composition on a first layer formed of the first resin composition formed on the support to obtain a resin composition layer including In a cross-section of the cured body layer perpendicular to the main surface of the cured body layer when the resin composition layer is cured to form a cured body layer, the area of the resin component per unit area in the region where the distance from the main surface of the cured body layer on the side opposite to the support is from 0 μm to 1 μm is A 0-1 and the area of the resin component per unit area in the region from 1 μm to 2 μm is A 1-2 When it is 0-1 / A 1-2 > 1.1 is satisfied, a method for manufacturing a resin sheet.

[40] In the cross-section, the area of the resin component per unit area in the region where the distance from the main surface of the cured body layer on the side opposite to the support is from 0 μm to 0.5 μm is A 0-0.5 and the area of the resin component per unit area in the region from 0.5 μm to 1 μm is A 0.5-1 When it is 0-0.5 / A 0.5-1 > 1.1 is satisfied, the method for manufacturing a resin sheet according to

[39] .

[41] In the cross-section, the area of the resin component per unit area in the region where the distance from the main surface of the cured body layer on the side opposite to the support is from 0.5 μm to d μm is A 0.5-d and the area of the resin component per unit area in the region from d μm to 0.5D μm is A d-0.5D When it is 0.5-d / A d-0.5D ≦ 1.1 (where d is a number satisfying 0.5 < d < 0.5D, and D is the thickness of the cured body layer.) is satisfied, the method for manufacturing a resin sheet according to

[39] or

[40] .

[42] The method for manufacturing a resin sheet according to any one of

[39] to

[41] , wherein the resin composition layer contains an epoxy resin.

[43] The method for producing a support-attached resin sheet according to

[42] , wherein the resin composition layer further contains an active ester-based curing agent.

[44] The method for producing a resin sheet according to any one of

[39] to

[43] , wherein the second layer has a thickness of less than 2 μm.

[45] The method for producing a resin sheet according to any one of

[39] to

[44] , wherein the second resin composition has an inorganic filler content of less than 20 mass %.

[46] (α) process, (α1) a step of preparing a support-attached temporary resin sheet including a support and a first layer made of a first resin composition formed on the support; and (α2) A step of applying a coating liquid containing the second resin composition onto the first layer and drying the coating liquid to form a second layer. The method for producing a resin sheet according to any one of

[39] to

[45] , comprising:

[47] The method for producing a resin sheet according to any one of

[39] to

[46] , wherein the resin sheet is intended to subject the cured body layer to a plasma treatment with one or more gases selected from the group consisting of O2 gas and N2 gas after the resin composition layer is cured to form a cured body layer. Effect of the Invention

[0014] According to the present invention, it is possible to provide: a cured body layer that can ensure sufficient smear removability even when plasma from N gas or O gas, which has low inorganic filler removal ability, is used in a desmear treatment; a printed wiring board including the cured body layer and a method for manufacturing the same; a semiconductor device including the cured body layer; and a resin sheet from which the cured body layer can be obtained and a method for manufacturing the same. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1 is a cross-sectional view that illustrates a cross section of a cured body layer in one embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view that illustrates a cross section of a cured body layer in which via holes are formed in one embodiment of the present invention. [Diagram 3] FIG. 3 is a cross-sectional view that illustrates a cross section of a cured body layer in one embodiment of the present invention. [Figure 4] FIG. 4 is a cross-sectional view that illustrates a cross section of a resin sheet having a support and a resin composition layer in one embodiment of the present invention. [Diagram 5] FIG. 5 is a cross-sectional view that shows a schematic cross section of a support and a cured body layer when a cured body layer is formed by curing a resin composition layer of a resin sheet in one embodiment of the present invention. [Figure 6] FIG. 6 is a cross-sectional view that shows a schematic cross section of a support and a cured body layer when a cured body layer is formed by curing a resin composition layer of a resin sheet in one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The present invention will be described in detail below with reference to preferred embodiments. However, the present invention is not limited to the following embodiments and examples, and can be modified and implemented as desired without departing from the scope of the claims of the present invention and their equivalents.

[0017] <Outline of the hardened layer> Fig. 1 is a cross-sectional view that typically illustrates a cross section of a cured body layer 100 in one embodiment of the present invention. The cured body layer 100 illustrated in Fig. 1 is provided on a surface 210U of a substrate 200 that includes a conductor layer 210, the surface 210U being on the conductor layer 210 side. Thus, Fig. 1 illustrates not only the cured body layer 100, but also the substrate 200 that includes the conductor layer 210.

[0018] 1, the cured body layer 100 according to one embodiment of the present invention is formed of a cured product of a resin composition containing 40% by mass or more of an inorganic filler. The cured body layer 100 is provided on a surface 210U of a substrate 200 on the conductor layer 210 side, the surface 210U being provided with the conductor layer 210. The conductor layer 210 is provided as at least a part of the outermost layer of the substrate 200. Thus, at least a part of the cured body layer 100 is provided on the conductor layer 210.

[0019] In a cross section of the cured body layer 100 perpendicular to a main surface 100D of the cured body layer 100 (here, the surface of the cured body layer 100 on the conductor layer 210 side), the area of ​​the resin component per unit area in a region 110 at a distance of 0 μm to 1 μm from the conductor layer 210 is defined as A 0-1 In addition, in a cross section of the cured body layer 100 perpendicular to the main surface 100D of the cured body layer 100, the area of ​​the resin component per unit area in the region 120 at a distance of 1 μm to 2 μm from the conductor layer 210 is represented by A 1-2 In this case, the cured body layer 100 is A 0-1 / A 1-2 >1.1 (hereinafter referred to as "condition (1)") is satisfied.

[0020] In this specification, the term "resin component" refers to the components constituting the resin composition excluding inorganic fillers. Also, the term "area of ​​the resin component per unit area" refers to the area occupied by the resin component per unit area of ​​the cross section of the cured body layer 100.

[0021] Condition (1) indicates that region 110 from 0 μm to 1 μm away from conductor layer 210 has a larger area of ​​resin component and a smaller amount of inorganic filler than region 120 from 1 μm to 2 μm away.

[0022] Condition (1) is to ensure sufficient smear removal. 0-1 / A 1-2 >1.13 is preferable, and A 0-1 / A 1-2 >1.15 is preferable, A 0-1 / A 1-2 It is even more preferable that it is >1.2.

[0023] Furthermore, in a cross section of the cured body layer 100 perpendicular to the main surface 100D of the cured body layer 100, the area of ​​the resin component per unit area in a region 130 at a distance of 0 μm to 0.5 μm from the conductor layer 210 is defined as A 0-0.5In addition, in a cross section of the cured body layer 100 perpendicular to the main surface 100D of the cured body layer 100, the area of ​​the resin component per unit area in the region 140 at a distance of 0.5 μm to 1 μm from the conductor layer 210 is represented by A 0.5-1 In this case, the cured body layer 100 is A 0-0.5 / A 0.5-1 It is preferable that the condition (2) is satisfied.

[0024] Condition (2) indicates that region 130 from 0 μm to 0.5 μm away from conductor layer 210 has a larger area of ​​resin component and a smaller amount of inorganic filler than region 140 from 0.5 μm to 1 μm away.

[0025] Condition (2) is to ensure sufficient smear removal. 0-0.5 / A 0.5-1 >1.13 is preferable, and A 0-0.5 / A 0.5-1 >1.15 is preferable, A 0-0.5 / A 0.5-1 It is even more preferable that it is >1.2.

[0026] Fig. 2 is a cross-sectional view that typically illustrates a cross section of the cured body layer 100 in one embodiment of the present invention. Fig. 2 illustrates a state after a via hole 300 is formed in the cured body layer 100 and before a desmear treatment is performed.

[0027] When a via hole 300 is formed in the cured body layer 100 as shown in FIG. 2, a smear 310 may occur on the side surface 300S of the via hole 300. The diameter of the via hole 300 is generally smaller as it is closer to the conductor layer 210. Therefore, if the smear 310 remains on the bottom 320 of the via hole 300 close to the conductor layer 210, the via hole 300 may be blocked, which may cause poor conduction. Therefore, it is desirable to remove such smear 310 on the bottom 320 of the via hole 300 by a desmear process. However, when the smear 310 contains a large amount of inorganic filler, it is difficult to sufficiently remove the smear 310 by a desmear process as a plasma process using a gas that does not contain fluorine, such as N2 gas and O2 gas.

[0028] In contrast, the cured body layer 100 according to this embodiment satisfies condition (1) or condition (2) in addition to condition (1), so that the amount of inorganic filler is relatively small in the region near the conductor layer 210, and the ratio of inorganic filler increases with a continuous or stepwise gradient as it moves away from the conductor layer 210. Therefore, in the via hole 300 formed in the cured body layer 100, the amount of inorganic filler contained in the smear 310 formed in the bottom 320 is small. Therefore, even when the cured body layer 100 containing a high amount of inorganic filler is used as the insulating layer, the smear 310 generated in the via hole 300 can be effectively removed by plasma using N2 gas or O2 gas, which has low inorganic filler removal ability. Therefore, good smear removal performance can be achieved without using fluorine-based gas.

[0029] 3 is a cross-sectional view that typically illustrates a cross section of the cured body layer 100 according to one embodiment of the present invention. As illustrated in FIG. 3, in a cross section of the cured body layer 100 perpendicular to a main surface 100D of the cured body layer 100, the area of ​​the resin component per unit area in a region 150 that is from 0.5 μm to d μm away from the conductor layer 210 is represented as A 0.5-d In addition, in a cross section of the cured body layer 100 perpendicular to the main surface 100D of the cured body layer 100, the area of ​​the resin component per unit area in a region 160 at a distance from the conductor layer 210 between d μm and 0.5D μm is defined as A d-0.5DLet it be so. In this case, it is preferable that 0.9 ≦ A 0.5-d / A d-0.5D ≦ 1.1 (hereinafter, also referred to as "condition (3)"). Here, d is a number satisfying 0.5 < d < 0.5D, and D is the thickness of the cured body layer 100.

[0030] Condition (3) indicates that when moving away from the conductor layer 100 by a certain distance or more, the ratio of the amount of the inorganic filler and the resin component does not change, and a phase with a relatively uniform composition is formed.

[0031] Condition (3) is preferably 0.92 ≦ A 0.5-d / A d-0.5D ≦ 1.08, more preferably 0.95 ≦ A 0.5-d / A d-0.5D ≦ 1.05, and even more preferably 0.98 ≦ A 0.5-d / A d-0.5D ≦ 1.02.

[0032] By satisfying condition (3), since there is a sharp composition gradient in a limited region near the conductor layer 210, it is possible to ensure sufficient smear removability while ensuring high peel strength.

[0033] From the viewpoints of thinning the printed wiring board and providing a cured product with excellent insulation even if the cured product of the resin composition is a thin film, the thickness D of the cured body layer 100 is preferably 50 μm or less, more preferably 40 μm or less. The lower limit of the thickness of the cured body layer 100 is not particularly limited, but usually can be 5 μm or more, etc.

[0034] As described above, the cured body layer 100 exhibits the characteristic of excellent smear removability by plasma treatment using N2 gas or O2 gas. The smear removability can be evaluated by the maximum smear length. The maximum smear length is preferably less than 5 μm, more preferably less than 3 μm, and even more preferably less than 2 μm. The "maximum smear length" means the maximum length of the smear from the circumference of the bottom surface of the via hole to the center of the circle. The evaluation of the maximum smear length can be measured according to the method described in the examples below.

[0035] The cured body layer 100 also exhibits the property of being able to obtain a high level of peel strength between it and the conductor layer 210. The peel strength is not particularly limited, but is preferably 0.40 kgf / cm or more, more preferably 0.50 kgf / cm or more, and even more preferably 0.55 kgf / cm or more. Meanwhile, the upper limit may be 5 kgf / cm or less. The peel strength can be measured according to the method described in the examples below.

[0036] In one embodiment, the cured body layer satisfies condition (1) by having a first cured body layer formed of a cured product of a first resin composition and a second cured body layer formed of a cured product of a second resin composition in this order from the side opposite to the substrate (hereinafter also referred to as "layered gradient type"). In this case, the inorganic filler content of the second resin composition forming the second cured body layer on the side bonded to the substrate having a conductor layer is lower than the inorganic filler content of the first resin composition, so that the area of ​​the resin component in the region near the conductor layer can be increased. The thickness of the second cured body layer is not limited as long as the desired effect of the present invention is obtained, but is preferably less than 2 μm, more preferably less than 1.5 μm, even more preferably 1 μm, and particularly preferably 0.8 μm. The inorganic filler content of the second resin composition in this embodiment will be described in detail below. In this embodiment, the cured body layer is not limited to a two-layer form consisting of a first cured body layer and a second cured body layer, and may be a cured body layer having three or more layers. Therefore, the cured body layer may further include a cured body layer formed of a cured product of a resin composition having a composition different from the first and second resin compositions.

[0037] In another embodiment, the cured body layer is a cured body layer obtained by curing a resin composition having a homogeneous composition on a substrate having a conductor layer, and is a cured body layer (hereinafter also referred to as "conductive layer vicinity gradient type") that satisfies condition (1) by having a non-uniform composition in the conductive layer vicinity region. As long as condition (1) can be satisfied, there is no particular limitation, but for example, a cured body layer of the conductive layer vicinity gradient type can be obtained by adding a certain amount of a nitrogen-containing component such as a cyanate ester-based curing agent to the resin composition. Specific examples or the content of the cyanate ester-based curing agent will be described in detail below. In this embodiment, the cured body layer may be a single layer or multiple layers. That is, it may be a form in which the layered gradient type and the conductive layer vicinity gradient type are combined.

[0038] <Area of ​​resin component per unit area> The area of ​​the resin component per unit area can be measured and calculated by the method described later in [Measurement of resin area ratio]. Specifically, it can be measured by (1) preparing a cross-section sample by cutting out a cross section perpendicular to the main surface of the cured body layer, and (2) observing the cross-section sample with a scanning electron microscope (SEM) and performing image analysis on the obtained SEM image to determine the resin area.

[0039] In image analysis, the resin component part and the inorganic filler part are binarized, and the number of pixels in the resin component part is treated as the resin area. In measuring the resin area, the width of the measurement area (for example, the measurement distance in the direction parallel to the main surface of the cured body layer) is set to be equal.

[0040] Naturally, when measuring the resin area ratio, the conditions are calibrated to ensure the accuracy of image analysis. Such calibration can be performed by setting a binarization threshold so that the value of (number of pixels in the inorganic filler part) / (total number of pixels in the cross section of the cross section sample)×100 substantially coincides with the volume percent value of the inorganic filler in the cross section sample.

[0041] <Resin composition> The resin composition includes a resin component and an inorganic filler (A). The resin composition preferably includes an epoxy resin (B) as the resin component. The resin composition may further include optional components in addition to the components (A) and (B). Examples of the optional components include a curing agent (C), a thermoplastic resin (D), an organic filler (E), a flame retardant (F), a curing accelerator (G), and other additives (H). Each component included in the resin composition will be described in detail below.

[0042] <(A) Inorganic filler> The resin composition contains 40% by mass or more of component (A) when the non-volatile components in the resin composition are taken as 100% by mass. It is not intended that component (A) be uniformly contained throughout the resin composition, but rather that component (A) be contained in an amount of 40% by mass or more relative to the entire resin composition.

[0043] (A) The material of the inorganic filler is not particularly limited, but examples thereof include silica, alumina, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium zirconate titanate, barium zirconate, calcium zirconate, zirconium phosphate, and zirconium tungstate phosphate, and silica is particularly preferred. Examples of silica include amorphous silica, fused silica, crystalline silica, synthetic silica, and hollow silica. Moreover, spherical silica is preferred as the silica. The inorganic filler may be used alone or in combination of two or more.

[0044] (A) Commercially available inorganic fillers include, for example, "UFP-30" manufactured by Denka Chemical Industry Co., Ltd.; "SP60-05" and "SP507-05" manufactured by Nippon Steel & Sumitomo Metal Materials Co., Ltd.; "YC100C", "YA050C", "YA050C-MJE", and "YA010C" manufactured by Admatechs Co., Ltd.; "UFP-30" manufactured by Denka Company, Limited; "Silfill NSS-3N", "Silfill NSS-4N", and "Silfill NSS-5N" manufactured by Tokuyama Corporation; and "SC2500SQ", "SO-C4", "SO-C2", and "SO-C1" manufactured by Admatechs Co., Ltd.

[0045] The average particle size of the inorganic filler is preferably 4 μm or less, more preferably 3 μm or less, even more preferably 2.5 μm or less, even more preferably 2 μm or less, particularly preferably 1 μm or less, 0.7 μm or less. The lower limit of the average particle size of the inorganic filler is preferably 0.01 μm or more, more preferably 0.03 μm or more, even more preferably 0.05 μm or more, 0.07 μm or more, or 0.1 μm or more. The average particle size of the inorganic filler can be measured by a laser diffraction / scattering method based on the Mie scattering theory. Specifically, the particle size distribution of the inorganic filler is prepared on a volume basis using a laser diffraction / scattering particle size distribution measuring device, and the median diameter is taken as the average particle size. The measurement sample can be prepared by weighing 100 mg of the inorganic filler and 10 g of methyl ethyl ketone into a vial and dispersing it by ultrasonic waves for 10 minutes. The measurement sample was measured using a laser diffraction type particle size distribution measuring device with blue and red light source wavelengths, and the particle size distribution of the inorganic filler on a volume basis was measured using a flow cell method, and the average particle size was calculated as the median diameter from the particle size distribution obtained. An example of a laser diffraction type particle size distribution measuring device is the "LA-960" manufactured by Horiba, Ltd.

[0046] From the viewpoint of improving moisture resistance and dispersibility, the inorganic filler is preferably treated with one or more surface treatment agents such as an aminosilane coupling agent, an epoxysilane coupling agent, a mercaptosilane coupling agent, an alkoxysilane compound, an organosilazane compound, or a titanate coupling agent. Examples of commercially available surface treatment agents include Shin-Etsu Chemical Co., Ltd.'s "KBM403" (3-glycidoxypropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM803" (3-mercaptopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBE903" (3-aminopropyltriethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM573" (N-phenyl-3-aminopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "SZ-31" (hexamethyldisilazane), Shin-Etsu Chemical Co., Ltd.'s "KBM103" (phenyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM-4803" (long-chain epoxy-type silane coupling agent), and Shin-Etsu Chemical Co., Ltd.'s "KBM-7103" (3,3,3-trifluoropropyltrimethoxysilane).

[0047] The degree of surface treatment with the surface treatment agent is preferably within a predetermined range from the viewpoint of improving the dispersibility of the inorganic filler. Specifically, 100 parts by mass of the inorganic filler is preferably surface-treated with 0.2 parts by mass to 5 parts by mass of the surface treatment agent, more preferably 0.2 parts by mass to 3 parts by mass, and even more preferably 0.3 parts by mass to 2 parts by mass.

[0048] The degree of surface treatment with the surface treatment agent can be evaluated by the amount of carbon per unit surface area of ​​the inorganic filler. From the viewpoint of improving the dispersibility of the inorganic filler, the amount of carbon per unit surface area of ​​the inorganic filler is set to 0.02 mg / m 2 More than 0.1 mg / m is preferable. 2 More preferably, 0.2 mg / m or more 2 On the other hand, from the viewpoint of preventing an increase in the melt viscosity of the resin varnish or the melt viscosity in the form of a sheet, it is more preferable that the content be 1 mg / m 2 Less than 0.8 mg / m is preferred. 2 Less than 0.5 mg / m is more preferable.2 The following is even more preferred:

[0049] The amount of carbon per unit surface area of ​​the inorganic filler can be measured after the surface-treated inorganic filler is washed with a solvent (e.g., methyl ethyl ketone (MEK)). Specifically, a sufficient amount of MEK as a solvent is added to the inorganic filler that has been surface-treated with a surface treatment agent, and ultrasonic cleaning is performed at 25°C for 5 minutes. After removing the supernatant and drying the solid content, the amount of carbon per unit surface area of ​​the inorganic filler can be measured using a carbon analyzer. The carbon analyzer that can be used is the "EMIA-320V" manufactured by Horiba, Ltd.

[0050] From the viewpoint of further improving the effects of the present invention, the specific surface area of ​​the (A) inorganic filler is preferably 1 m 2 / g or more, more preferably 1.5m 2 / g or more, particularly preferably 2m 2 / g or more. There is no particular upper limit, but it is preferably 50m 2 / g or less, 45m 2 / g or less or 40m 2 The specific surface area of ​​the inorganic filler is obtained by adsorbing nitrogen gas onto the surface of a sample using a specific surface area measuring device (Macsorb HM-1210 manufactured by Mountech Co., Ltd.) according to the BET method, and calculating the specific surface area using the BET multipoint method.

[0051] The content of the inorganic filler (A) relative to the entire resin composition is preferably 45% by mass or more, more preferably 50% by mass or more, or 55% by mass or more, from the viewpoint of obtaining a cured product with a low linear thermal expansion coefficient and dielectric loss tangent, when the non-volatile components in the resin composition are taken as 100% by mass. The upper limit is preferably 90% by mass or less, more preferably 85% by mass or less, and even more preferably 80% by mass or less, from the viewpoint of the mechanical strength of the obtained cured product.

[0052] When the cured body layer is a layered gradient type consisting of two layers, a first cured body layer and a second cured body layer, the content F of the inorganic filler (A) in the entire resin composition is calculated as follows. F(mass%)=(F1L1+F2L2) / (L1+L2) (In the formula, F1 represents the content (mass%) of the inorganic filler in the first resin composition, F2 represents the content (mass%) of the inorganic filler in the second resin composition, L1 represents the thickness of the first resin composition before curing, and L2 represents the thickness of the second resin composition before curing.)

[0053] When the first resin composition and the second resin composition are used to obtain a layered gradient type cured body layer, the inorganic filler content of the second resin composition (second layer) forming the second cured body layer on the side bonded to the substrate having a conductor layer is not particularly limited as long as it satisfies the condition (1), but is preferably less than 20 mass%, more preferably less than 10 mass%, even more preferably less than 5 mass%, and particularly preferably 0 mass%, when the non-volatile components in the resin composition are taken as 100 mass%. In this case, the inorganic filler content of the first resin composition (first layer) forming the first cured body layer on the side opposite to the second cured body layer, that is, on the side bonded to the support when a support is present, is not particularly limited as long as it satisfies the condition of the content of the inorganic filler (A) of the entire resin composition, but is preferably 50 mass% or more, more preferably 55 mass% or more, 60 mass% or more, when the non-volatile components in the resin composition are taken as 100 mass%, from the viewpoint of obtaining a cured body with a low linear thermal expansion coefficient and dielectric loss tangent. The upper limit is preferably 90% by mass or less, more preferably 85% by mass or less, and even more preferably 80% by mass or less, from the viewpoint of the mechanical strength of the obtained cured product.

[0054] <(B) Epoxy resin> The resin composition optionally contains (B) an epoxy resin.

[0055] (B) Epoxy resins include, for example, bixylenol type epoxy resins, bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bisphenol AF type epoxy resins, dicyclopentadiene type epoxy resins, trisphenol type epoxy resins, naphthol novolac type epoxy resins, phenol novolac type epoxy resins, tert-butyl-catechol type epoxy resins, naphthalene type epoxy resins, naphthol type epoxy resins, anthracene type epoxy resins, glycidylamine type epoxy resins, glycidyl ester type epoxy resins, cresol novolac type epoxy resins, biphenyl type epoxy resins, linear aliphatic epoxy resins, epoxy resins having a butadiene structure, alicyclic epoxy resins, heterocyclic epoxy resins, spiro ring-containing epoxy resins, cyclohexane type epoxy resins, cyclohexane dimethanol type epoxy resins, naphthylene ether type epoxy resins, trimethylol type epoxy resins, tetraphenylethane type epoxy resins, etc. Epoxy resins may be used alone or in combination of two or more types.

[0056] The resin composition preferably contains, as the epoxy resin (B), an epoxy resin having two or more epoxy groups in one molecule. From the viewpoint of significantly obtaining the desired effects of the present invention, the proportion of the epoxy resin having two or more epoxy groups in one molecule is preferably 50% by mass or more, more preferably 60% by mass or more, and particularly preferably 70% by mass or more, based on 100% by mass of the non-volatile components of the epoxy resin (B).

[0057] Epoxy resins include epoxy resins that are liquid at a temperature of 20° C. (hereinafter sometimes referred to as "liquid epoxy resins") and epoxy resins that are solid at a temperature of 20° C. (hereinafter sometimes referred to as "solid epoxy resins"). The resin composition may contain only a liquid epoxy resin or only a solid epoxy resin as the (B) epoxy resin, but it is preferable to contain a combination of a liquid epoxy resin and a solid epoxy resin.

[0058] The liquid epoxy resin is preferably a liquid epoxy resin having two or more epoxy groups in one molecule.

[0059] As the liquid epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AF type epoxy resin, naphthalene type epoxy resin, glycidyl ester type epoxy resin, glycidyl amine type epoxy resin, phenol novolac type epoxy resin, alicyclic epoxy resin having an ester skeleton, cyclohexane type epoxy resin, cyclohexane dimethanol type epoxy resin, glycidyl amine type epoxy resin, and epoxy resin having a butadiene structure are preferred, and bisphenol A type epoxy resin and bisphenol F type epoxy resin are more preferred.

[0060] Specific examples of liquid epoxy resins include "HP4032", "HP4032D", and "HP4032SS" (naphthalene type epoxy resins) manufactured by DIC Corporation; "828US", "jER828EL", "825", and "Epikote 828EL" (bisphenol A type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER807" and "1750" (bisphenol F type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER152" (phenol novolac type epoxy resin) manufactured by Mitsubishi Chemical Corporation; and "630" and "630LSD" (glycidylamine type epoxy resins) manufactured by Mitsubishi Chemical Corporation. epoxy resin); "ZX1059" manufactured by Nippon Steel & Sumitomo Metal Chemical Co., Ltd. (a mixture of bisphenol A type epoxy resin and bisphenol F type epoxy resin); "EX-721" manufactured by Nagase ChemteX Corporation (glycidyl ester type epoxy resin); "Celloxide 2021P" manufactured by Daicel Corporation (alicyclic epoxy resin having an ester skeleton); "PB-3600" manufactured by Daicel Corporation (epoxy resin having a butadiene structure); "ZX1658" and "ZX1658GS" (liquid 1,4-glycidylcyclohexane type epoxy resin) manufactured by Nippon Steel & Sumitomo Metal Chemical Co., Ltd. may be used alone or in combination of two or more types.

[0061] As the solid epoxy resin, a solid epoxy resin having three or more epoxy groups in one molecule is preferable, and an aromatic solid epoxy resin having three or more epoxy groups in one molecule is more preferable.

[0062] As the solid epoxy resin, bixylenol type epoxy resin, naphthalene type epoxy resin, naphthalene type tetrafunctional epoxy resin, cresol novolac type epoxy resin, dicyclopentadiene type epoxy resin, trisphenol type epoxy resin, naphthol type epoxy resin, biphenyl type epoxy resin, naphthylene ether type epoxy resin, anthracene type epoxy resin, bisphenol A type epoxy resin, bisphenol AF type epoxy resin, and tetraphenylethane type epoxy resin are preferred, and naphthalene type epoxy resin is more preferred.

[0063] Specific examples of solid epoxy resins include "HP4032H" (naphthalene type epoxy resin) manufactured by DIC Corporation; "HP-4700" and "HP-4710" (naphthalene type tetrafunctional epoxy resins) manufactured by DIC Corporation; "N-690" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "N-695" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "HP-7200" (dicyclopentadiene type epoxy resin) manufactured by DIC Corporation; and "HP -7200HH, "HP-7200H", "EXA-7311", "EXA-7311-G3", "EXA-7311-G4", "EXA-7311-G4S", "HP6000" (naphthylene ether type epoxy resin); "EPPN-502H" (trisphenol type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; "NC7000L" (naphthol novolac type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; "NC3000H", "NC3000", "NC 3000L, "NC3100" (biphenyl type epoxy resin); "ESN475V" (naphthol type epoxy resin) manufactured by Nippon Steel & Sumitomo Metal Chemical Co., Ltd.; "ESN485" (naphthol novolac type epoxy resin) manufactured by Nippon Steel & Sumitomo Metal Chemical Co., Ltd.; "YX4000H", "YX4000", "YL6121" (biphenyl type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "YX4000HK" (bixylenol type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "YX8" manufactured by Mitsubishi Chemical Co., Ltd. Examples of epoxy resins include "800" (anthracene type epoxy resin), "PG-100" and "CG-500" manufactured by Osaka Gas Chemicals, "YL7760" (bisphenol AF type epoxy resin) manufactured by Mitsubishi Chemical, "YL7800" (fluorene type epoxy resin) manufactured by Mitsubishi Chemical, "jER1010" (solid bisphenol A type epoxy resin) manufactured by Mitsubishi Chemical, and "jER1031S" (tetraphenylethane type epoxy resin) manufactured by Mitsubishi Chemical. These may be used alone or in combination of two or more.

[0064] When a liquid epoxy resin and a solid epoxy resin are used in combination as the (B) epoxy resin, the ratio by mass between them (liquid epoxy resin:solid epoxy resin) is preferably 1:1 to 1:20, more preferably 1:1 to 1:10, and particularly preferably 1:1 to 1:5. When the ratio by mass between the liquid epoxy resin and the solid epoxy resin is within this range, the desired effects of the present invention can be significantly obtained.

[0065] The epoxy equivalent of the (B) epoxy resin is preferably 50 g / eq to 5000 g / eq, more preferably 50 g / eq to 3000 g / eq, even more preferably 80 g / eq to 2000 g / eq, and even more preferably 110 g / eq to 1000 g / eq. When it is in this range, the crosslink density of the cured product of the resin composition layer is sufficient, and an insulating layer with small surface roughness can be obtained. The epoxy equivalent is the mass of an epoxy resin containing one equivalent of epoxy groups. This epoxy equivalent can be measured according to JIS K7236.

[0066] From the viewpoint of significantly obtaining the desired effects of the present invention, the weight average molecular weight (Mw) of the epoxy resin (B) is preferably 100 to 5000, more preferably 250 to 3000, and further preferably 400 to 1500. The weight average molecular weight of the resin can be measured as a polystyrene-equivalent value by gel permeation chromatography (GPC).

[0067] The content of the (B) epoxy resin is not particularly limited, but when the resin component in the resin composition is taken as 100 mass%, from the viewpoint of obtaining the desired effect of the present invention remarkably, it is preferably 20 mass% or more, more preferably 30 mass% or more, even more preferably 40 mass% or more, and particularly preferably 45 mass% or more. From the viewpoint of obtaining the desired effect of the present invention remarkably, the upper limit is preferably 80 mass% or less, more preferably 70 mass% or less, even more preferably 65 mass% or less, and particularly preferably 60 mass% or less. In the resin composition, the (B) component is not intended to be contained uniformly throughout the resin composition, and the content of the (B) component herein means the content relative to the entire resin composition.

[0068] <(C) Hardener> The resin composition optionally contains (C) a curing agent.

[0069] The (C) curing agent is not particularly limited as long as it has the function of curing the epoxy resin, and examples thereof include phenol-based curing agents, naphthol-based curing agents, acid anhydride-based curing agents, active ester-based curing agents, benzoxazine-based curing agents, cyanate ester-based curing agents, and carbodiimide-based curing agents. The curing agents may be used alone or in combination of two or more.

[0070] As the phenol-based curing agent and naphthol-based curing agent, from the viewpoint of heat resistance and water resistance, a phenol-based curing agent having a novolac structure or a naphthol-based curing agent having a novolac structure is preferred. Also, from the viewpoint of adhesion to the adherend, a nitrogen-containing phenol-based curing agent or a nitrogen-containing naphthol-based curing agent is preferred, and a triazine skeleton-containing phenol-based curing agent or a triazine skeleton-containing naphthol-based curing agent is more preferred. Among them, from the viewpoint of highly satisfying heat resistance, water resistance, and adhesion, a triazine skeleton-containing phenol novolac resin is preferred. Specific examples of phenol-based curing agents and naphthol-based curing agents include, for example, "MEH-7700", "MEH-7810", and "MEH-7851" manufactured by Meiwa Kasei Co., Ltd., "NHN", "CBN", and "GPH" manufactured by Nippon Kayaku Co., Ltd., "SN-170", "SN-180", "SN-190", "SN-475", "SN-485", "SN-495", "SN-375", and "SN-395" manufactured by Nippon Steel & Sumikin Chemical Co., Ltd., and "LA-7052", "LA-7054", "LA-3018", "LA-3018-50P", "LA-1356", and "TD2090" manufactured by DIC Corporation.

[0071] Examples of the acid anhydride curing agent include a curing agent having one or more acid anhydride groups in one molecule. Specific examples of the acid anhydride curing agent include phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride, hydrogenated methylnadic anhydride, trialkyltetrahydrophthalic anhydride, dodecenyl succinic anhydride, 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, trimellitic anhydride, pyromellitic anhydride, and benzophenonetetracarboxylic dianhydride. Examples of acid anhydrides include anhydrides, biphenyltetracarboxylic dianhydride, naphthalenetetracarboxylic dianhydride, oxydiphthalic dianhydride, 3,3'-4,4'-diphenylsulfonetetracarboxylic dianhydride, 1,3,3a,4,5,9b-hexahydro-5-(tetrahydro-2,5-dioxo-3-furanyl)-naphtho[1,2-C]furan-1,3-dione, ethylene glycol bis(anhydrotrimellitate), and polymeric acid anhydrides such as styrene-maleic acid resin, which is a copolymer of styrene and maleic acid.

[0072] The active ester curing agent is not particularly limited, but generally, compounds having two or more highly reactive ester groups in one molecule, such as phenol esters, thiophenol esters, N-hydroxyamine esters, and esters of heterocyclic hydroxy compounds, are preferably used. The active ester curing agent is preferably one obtained by a condensation reaction between a carboxylic acid compound and / or a thiocarboxylic acid compound and a hydroxy compound and / or a thiol compound. In particular, from the viewpoint of improving heat resistance, an active ester curing agent obtained from a carboxylic acid compound and a hydroxy compound is preferred, and an active ester curing agent obtained from a carboxylic acid compound and a phenol compound and / or a naphthol compound is more preferred. Examples of the carboxylic acid compound include benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, and pyromellitic acid. Examples of phenol compounds or naphthol compounds include hydroquinone, resorcin, bisphenol A, bisphenol F, bisphenol S, phenolphthaline, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucin, benzenetriol, dicyclopentadiene-type diphenol compounds, phenol novolac, etc. Here, the term "dicyclopentadiene-type diphenol compounds" refers to diphenol compounds obtained by condensing one molecule of dicyclopentadiene with two molecules of phenol.

[0073] Specifically, active ester compounds containing a dicyclopentadiene-type diphenol structure, active ester compounds containing a naphthalene structure, active ester compounds containing an acetylated product of phenol novolac, and active ester compounds containing a benzoylated product of phenol novolac are preferred, and among these, active ester compounds containing a naphthalene structure and active ester compounds containing a dicyclopentadiene-type diphenol structure are more preferred. The "dicyclopentadiene-type diphenol structure" refers to a divalent structural unit consisting of phenylene-dicyclopentalene-phenylene.

[0074] Commercially available active ester curing agents include active ester compounds containing a dicyclopentadiene-type diphenol structure, such as "EXB9451", "EXB9460", "EXB9460S", "HPC-8000", "HPC-8000H", "HPC-8000-65T", "HPC-8000H-65TM", "EXB-8000L", and "EXB-8000L-65TM" (manufactured by DIC Corporation); active ester compounds containing a naphthalene structure, such as "EXB9416-70BK" and "EXB-8150-65T" (manufactured by DIC Corporation); and phenol novolac. Examples of active ester compounds containing an acetylated product include "DC808" (manufactured by Mitsubishi Chemical Corporation); active ester compounds containing a benzoylated product of phenol novolac include "YLH1026" (manufactured by Mitsubishi Chemical Corporation); active ester-based hardeners which are acetylated products of phenol novolac include "DC808" (manufactured by Mitsubishi Chemical Corporation); and active ester-based hardeners which are benzoylated products of phenol novolac include "YLH1026" (manufactured by Mitsubishi Chemical Corporation), "YLH1030" (manufactured by Mitsubishi Chemical Corporation), and "YLH1048" (manufactured by Mitsubishi Chemical Corporation).

[0075] Specific examples of benzoxazine-based curing agents include "JBZ-OP100D" and "ODA-BOZ" manufactured by JFE Chemical Corporation; "HFB2006M" manufactured by Showa Polymer Co., Ltd.; and "Pd" and "Fa" manufactured by Shikoku Chemical Industry Co., Ltd.

[0076] Examples of the cyanate ester curing agent include bifunctional cyanate resins such as bisphenol A dicyanate, polyphenol cyanate (oligo(3-methylene-1,5-phenylene cyanate)), 4,4'-methylenebis(2,6-dimethylphenyl cyanate), 4,4'-ethylidene diphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanate phenylmethane), bis(4-cyanate-3,5-dimethylphenyl)methane, 1,3-bis(4-cyanate phenyl-1-(methylethylidene))benzene, bis(4-cyanate phenyl)thioether, and bis(4-cyanate phenyl)ether; polyfunctional cyanate resins derived from phenol novolac and cresol novolac; and prepolymers in which these cyanate resins are partially converted to triazine. Specific examples of cyanate ester-based curing agents include "PT30" and "PT60" (both of which are phenol novolac-type multifunctional cyanate ester resins), "BA230" and "BA230S75" (prepolymers in which part or all of bisphenol A dicyanate has been converted to triazine to form a trimer), all of which are manufactured by Lonza Japan.

[0077] Specific examples of carbodiimide-based curing agents include "V-03" and "V-07" manufactured by Nisshinbo Chemical Inc.

[0078] When a curing agent is included, the ratio of the amount of the epoxy resin to the curing agent is preferably in the range of 1:0.2 to 1:2, more preferably 1:0.3 to 1:1.5, and even more preferably 1:0.4 to 1:1.2, in terms of the ratio of [total number of epoxy groups in the epoxy resin]:[total number of reactive groups in the curing agent]. Here, the reactive groups in the curing agent are active hydroxyl groups, active ester groups, etc., and vary depending on the type of curing agent. The total number of epoxy groups in the epoxy resin is the total value of the non-volatile component mass of each epoxy resin divided by the epoxy equivalent weight, and the total number of reactive groups in the curing agent is the total value of the non-volatile component mass of each curing agent divided by the reactive group equivalent weight, for all curing agents. By setting the ratio of the amount of the epoxy resin to the curing agent in this range, the heat resistance of the obtained cured product is further improved.

[0079] When the resin composition contains a (C) curing agent, the content of the (C) curing agent is not particularly limited, but is preferably 1% by mass or more, more preferably 10% by mass or more, even more preferably 20% by mass or more, and particularly preferably 30% by mass or more, from the viewpoint of significantly obtaining the desired effect of the present invention, when the resin component in the resin composition is 100% by mass. The upper limit is preferably 60% by mass or less, more preferably 55% by mass or less, even more preferably 50% by mass or less, and particularly preferably 45% by mass or less, from the viewpoint of significantly obtaining the desired effect of the present invention. In the resin composition, the (C) component is not intended to be contained uniformly throughout the resin composition, and the content of the (C) component herein means the content relative to the entire resin composition.

[0080] The resin composition preferably contains an active ester curing agent. When the resin composition contains an active ester curing agent, the content of the active ester curing agent is not particularly limited, but when the resin component in the resin composition is 100 mass%, from the viewpoint of obtaining the desired effect of the present invention remarkably, it is preferably 1 mass% or more, more preferably 5 mass% or more, even more preferably 10 mass% or more, and particularly preferably 12 mass% or more. From the viewpoint of obtaining the desired effect of the present invention remarkably, the upper limit is preferably 50 mass% or less, more preferably 40 mass% or less, even more preferably 35 mass% or less, and particularly preferably 30 mass% or less.

[0081] In a particular preferred embodiment, it is preferable to include a cyanate ester-based curing agent, which can effectively provide a cured body layer with a gradient type near the conductor layer, or a cured body layer that combines a layered gradient type and a gradient type near the conductor layer.

[0082] By including a cyanate ester-based curing agent in the resin composition, even if a resin composition with a homogeneous composition is used, the proportion of inorganic filler in the area near the conductor layer decreases during curing, so that smears that occur in via holes can be effectively removed even when using plasma from N2 gas or O2 gas, which has a low inorganic filler removal ability.

[0083] In this embodiment, the content of the cyanate ester curing agent is preferably 15% by mass or more, more preferably 20% by mass or more, and even more preferably 25% by mass or more, from the viewpoint of ensuring sufficient smear removability, when the resin component in the resin composition is taken as 100% by mass. The upper limit is preferably 60% by mass or less, more preferably 50% by mass or less, even more preferably 40% by mass or less, and particularly preferably 30% by mass or less, from the viewpoint of significantly obtaining the desired effects of the present invention.

[0084] <(D) Thermoplastic resin> The resin composition optionally contains (D) a thermoplastic resin.

[0085] Examples of the thermoplastic resin as component (D) include phenoxy resin, polyvinyl acetal resin, polyolefin resin, polybutadiene resin, polyimide resin, polyamideimide resin, polyetherimide resin, polysulfone resin, polyethersulfone resin, polyphenylene ether resin, polycarbonate resin, polyetheretherketone resin, polyester resin, etc. Among them, phenoxy resin is preferred from the viewpoint of obtaining the desired effect of the present invention remarkably and from the viewpoint of obtaining an insulating layer having small surface roughness and particularly excellent adhesion to the conductor layer. Moreover, the thermoplastic resin may be used alone or in combination of two or more kinds.

[0086] Examples of the phenoxy resin include phenoxy resins having one or more skeletons selected from the group consisting of bisphenol A skeleton, bisphenol F skeleton, bisphenol S skeleton, bisphenolacetophenone skeleton, novolac skeleton, biphenyl skeleton, fluorene skeleton, dicyclopentadiene skeleton, norbornene skeleton, naphthalene skeleton, anthracene skeleton, adamantane skeleton, terpene skeleton, and trimethylcyclohexane skeleton. The terminal of the phenoxy resin may be any functional group such as a phenolic hydroxyl group or an epoxy group.

[0087] Specific examples of phenoxy resins include "1256" and "4250" manufactured by Mitsubishi Chemical Corporation (both of which are phenoxy resins containing a bisphenol A skeleton); "YX8100" manufactured by Mitsubishi Chemical Corporation (phenoxy resin containing a bisphenol S skeleton); "YX6954" manufactured by Mitsubishi Chemical Corporation (phenoxy resin containing a bisphenol acetophenone skeleton); "FX280" and "FX293" manufactured by Nippon Steel & Sumikin Chemical Co., Ltd.; "YL7500BH30", "YX6954BH30", "YX7553", "YX7553BH30", "YL7769BH30", "YL6794", "YL7213", "YL7290", and "YL7482" manufactured by Mitsubishi Chemical Corporation.

[0088] Examples of polyvinyl acetal resin include polyvinyl formal resin and polyvinyl butyral resin, and polyvinyl butyral resin is preferred.Specific examples of polyvinyl acetal resin include "Denka Butyral 4000-2", "Denka Butyral 5000-A", "Denka Butyral 6000-C", and "Denka Butyral 6000-EP" manufactured by Denki Kagaku Kogyo Co., Ltd.; S-LEC BH series, BX series (e.g. BX-5Z), KS series (e.g. KS-1), BL series, and BM series manufactured by Sekisui Chemical Co., Ltd.

[0089] Specific examples of polyimide resins include "Rikacoat SN20" and "Rikacoat PN20" manufactured by New Japan Chemical Co., Ltd. Specific examples of polyimide resins also include modified polyimides such as linear polyimides obtained by reacting bifunctional hydroxyl-terminated polybutadiene, a diisocyanate compound, and a tetrabasic acid anhydride (polyimides described in JP-A-2006-37083), and polysiloxane skeleton-containing polyimides (polyimides described in JP-A-2002-12667 and JP-A-2000-319386, etc.).

[0090] Specific examples of polyamide-imide resins include "Viromax HR11NN" and "Viromax HR16NN" manufactured by Toyobo Co., Ltd. Specific examples of polyamide-imide resins also include modified polyamide-imides such as "KS9100" and "KS9300" (polysiloxane skeleton-containing polyamide-imide) manufactured by Hitachi Chemical Co., Ltd.

[0091] A specific example of the polyethersulfone resin is "PES5003P" manufactured by Sumitomo Chemical Co., Ltd.

[0092] A specific example of the polyphenylene ether resin is the oligophenylene ether-styrene resin "OPE-2St 1200" manufactured by Mitsubishi Gas Chemical Company.

[0093] Specific examples of polysulfone resins include polysulfones "P1700" and "P3500" manufactured by Solvay Advanced Polymers.

[0094] From the viewpoint of significantly obtaining the desired effects of the present invention, the weight average molecular weight (Mw) of the (D) thermoplastic resin is preferably 8,000 or more, more preferably 10,000 or more, and particularly preferably 20,000 or more, and is preferably 70,000 or less, more preferably 60,000 or less, and particularly preferably 50,000 or less.

[0095] When the resin composition contains the thermoplastic resin (D), the content of the thermoplastic resin (D) is not particularly limited, but when the resin component in the resin composition is 100 mass%, from the viewpoint of obtaining the desired effect of the present invention remarkably, it is preferably 0.1 mass% or more, more preferably 1 mass% or more, and even more preferably 2 mass% or more. The upper limit is preferably 40 mass% or less, more preferably 30 mass% or less, and even more preferably 20 mass% or less. In the resin composition, the component (D) is not intended to be contained uniformly throughout the resin composition, and the content of the component (D) here means the content relative to the entire resin composition.

[0096] <(E)Organic filler> The resin composition optionally contains (E) an organic filler.

[0097] As the (E) organic filler, any organic filler that can be used for sealing electronic components may be used. Examples of the organic filler include rubber particles, polyamide fine particles, and silicone particles, with rubber particles being preferred.

[0098] The rubber particles are not particularly limited as long as they are fine particles of resin that is insoluble and infusible in organic solvents by chemically crosslinking a resin that exhibits rubber elasticity, and examples of such particles include acrylonitrile butadiene rubber particles, butadiene rubber particles, acrylic rubber particles, etc. Specific examples of rubber particles include XER-91 (manufactured by Japan Synthetic Rubber Co., Ltd.), Staphyloid AC3355, AC3816, AC3816N, AC3832, AC4030, AC3364, IM101 (all manufactured by Aica Kogyo Co., Ltd.), PARALOID EXL2655, EXL2602 (all manufactured by The Dow Chemical Company), etc.

[0099] The average particle size of the (E) organic filler is preferably in the range of 0.005 μm to 1 μm, more preferably in the range of 0.2 μm to 0.6 μm. The average particle size of the (E) organic filler can be measured using a dynamic light scattering method. For example, the organic filler is uniformly dispersed in a suitable organic solvent by ultrasonic waves or the like, and a particle size distribution of the organic filler is created on a mass basis using a concentrated particle size analyzer (Otsuka Electronics Co., Ltd.'s "FPAR-1000"), and the median diameter is taken as the average particle size.

[0100] When the resin composition contains an organic filler (E), the content of the organic filler (E) is not particularly limited, but is preferably 0.1% by mass or more, more preferably 1% by mass or more, and even more preferably 3% by mass or more, from the viewpoint of remarkably obtaining the desired effect of the present invention, assuming that the resin component in the resin composition is 100% by mass. The upper limit is preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 10% by mass or less. In the resin composition, the component (E) is not intended to be contained uniformly throughout the resin composition, and the content of the component (E) herein means the content relative to the entire resin composition.

[0101] <(F) Flame retardant> The resin composition optionally contains (F) a flame retardant.

[0102] (F) Examples of the flame retardant include organic phosphorus flame retardants, organic nitrogen-containing phosphorus compounds, nitrogen compounds, silicone flame retardants, metal hydroxides, etc. The flame retardants may be used alone or in combination of two or more.

[0103] As the (F) flame retardant, commercially available products may be used, for example, "SPS-100" manufactured by Otsuka Chemical Co., Ltd.; "HCA-HQ-HST" and "HCA-HQ" manufactured by Sankosha Co., Ltd.

[0104] When the resin composition contains a flame retardant (F), the content of the flame retardant (F) is not particularly limited, but is preferably 0.1% by mass or more, more preferably 1% by mass or more, and even more preferably 3% by mass or more, from the viewpoint of significantly obtaining the desired effect of the present invention, assuming that the resin component in the resin composition is 100% by mass. The upper limit is preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 10% by mass or less. In the resin composition, the (F) component is not intended to be contained uniformly throughout the resin composition, and the content of the (F) component herein means the content relative to the entire resin composition.

[0105] <(G) Curing accelerator> The resin composition optionally contains (G) a curing accelerator.

[0106] (G) Examples of the curing accelerator include phosphorus-based curing accelerators, amine-based curing accelerators, imidazole-based curing accelerators, guanidine-based curing accelerators, and metal-based curing accelerators. Among them, phosphorus-based curing accelerators, amine-based curing accelerators, imidazole-based curing accelerators, and metal-based curing accelerators are preferred, and amine-based curing accelerators, imidazole-based curing accelerators, and metal-based curing accelerators are more preferred. The curing accelerator may be used alone or in combination of two or more types.

[0107] Examples of the phosphorus-based curing accelerator include triphenylphosphine, phosphonium borate compounds, tetraphenylphosphonium tetraphenylborate, n-butylphosphonium tetraphenylborate, tetrabutylphosphonium decanoate, (4-methylphenyl)triphenylphosphonium thiocyanate, tetraphenylphosphonium thiocyanate, butyltriphenylphosphonium thiocyanate, and the like, with triphenylphosphine and tetrabutylphosphonium decanoate being preferred.

[0108] Examples of the amine curing accelerator include trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine (DMAP), benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, and 1,8-diazabicyclo(5,4,0)-undecene, with 4-dimethylaminopyridine and 1,8-diazabicyclo(5,4,0)-undecene being preferred.

[0109] Examples of the imidazole curing accelerator include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2, 4-Diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-furan Examples of the imidazole compounds include imidazole compounds such as 2-ethyl-4-methyl-5-hydroxymethylimidazole, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, and 2-phenylimidazoline, as well as adducts of imidazole compounds and epoxy resins. Of these, 2-ethyl-4-methylimidazole and 1-benzyl-2-phenylimidazole are preferred.

[0110] As the imidazole-based curing accelerator, a commercially available product may be used, for example, "P200-H50" manufactured by Mitsubishi Chemical Corporation.

[0111] Examples of the guanidine curing accelerator include dicyandiamide, 1-methylguanidine, 1-ethylguanidine, 1-cyclohexylguanidine, 1-phenylguanidine, 1-(o-tolyl)guanidine, dimethylguanidine, diphenylguanidine, trimethylguanidine, tetramethylguanidine, pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, and 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene. Examples of such biguanide include o-[4.4.0]dec-5-ene, 1-methylbiguanide, 1-ethylbiguanide, 1-n-butylbiguanide, 1-n-octadecylbiguanide, 1,1-dimethylbiguanide, 1,1-diethylbiguanide, 1-cyclohexylbiguanide, 1-allylbiguanide, 1-phenylbiguanide, and 1-(o-tolyl)biguanide. Of these, dicyandiamide and 1,5,7-triazabicyclo[4.4.0]dec-5-ene are preferred.

[0112] Examples of metal-based curing accelerators include organometallic complexes or organometallic salts of metals such as cobalt, copper, zinc, iron, nickel, manganese, and tin. Specific examples of organometallic complexes include organocobalt complexes such as cobalt(II) acetylacetonate and cobalt(III) acetylacetonate, organocopper complexes such as copper(II) acetylacetonate, organozinc complexes such as zinc(II) acetylacetonate, organoiron complexes such as iron(III) acetylacetonate, organonickel complexes such as nickel(II) acetylacetonate, and organomanganese complexes such as manganese(II) acetylacetonate. Examples of organometallic salts include zinc octylate, tin octylate, zinc naphthenate, cobalt naphthenate, tin stearate, and zinc stearate.

[0113] When the resin composition contains the (G) curing accelerator, the content of the (G) curing accelerator is not particularly limited, but when the resin component in the resin composition is taken as 100 mass%, from the viewpoint of significantly obtaining the desired effect of the present invention, it is preferably 0.001 mass% or more, more preferably 0.01 mass% or more, and even more preferably 0.05 mass% or more. The upper limit is preferably 5 mass% or less, more preferably 1 mass% or less, and even more preferably 0.5 mass% or less. In the resin composition, the (G) curing accelerator is not intended to be contained uniformly throughout the resin composition, and the content of the (G) curing accelerator herein means the content relative to the entire resin composition.

[0114] <(H) Other Additives> The resin composition may further contain other additives as optional components other than the above-mentioned components. Examples of such additives include resin additives such as thickeners, defoamers, leveling agents, and adhesion promoters; polymerization initiators, etc. These additives may be used alone or in combination of two or more. The content of each additive can be appropriately set by a person skilled in the art.

[0115] In one embodiment, the nitrogen atom content of the resin composition is preferably 1% by mass or more when the resin component in the resin composition is 100% by mass. The nitrogen atom content (mass%) of the resin composition is a numerical value obtained by dividing the mass of the nitrogen atoms contained in the molecules of the amine-based curing accelerator, cyanate ester-based curing agent, etc. by the total mass of the resin component and converting the result into a percentage. In this embodiment, a cured body layer with a gradient type near the conductor layer, or a cured body layer with a combination of a laminar gradient type and a gradient type near the conductor layer can be effectively obtained.

[0116] By making the nitrogen atom content 1% by mass or more relative to the resin component, even if a resin composition with a homogeneous composition is used, the proportion of inorganic filler in the region near the conductor layer decreases during curing, so that smears occurring in via holes can be effectively removed using plasma from N2 gas or O2 gas, which has low inorganic filler removal ability. Here, the decrease in the proportion of inorganic filler in the region near the conductor layer is presumably due to the migration of molecules containing nitrogen atoms to the conductor layer.

[0117] In this embodiment, the nitrogen atom content of the resin composition is more preferably 1.5% by mass or more, further preferably 1.8% by mass or more, and particularly preferably 2% by mass or more, from the viewpoint of ensuring sufficient smear removal, when the resin component in the resin composition is taken as 100% by mass. The upper limit is not particularly limited, but may be, for example, 10% by mass.

[0118] <Resin sheet> The resin composition can be used by coating in the form of a varnish, but from an industrial perspective, it is generally preferred to use the resin composition in the form of a resin sheet containing the resin composition.

[0119] In a preferred embodiment, the resin sheet has a support and a resin composition layer formed on the support. Fig. 4 is a cross-sectional view that typically shows a cross section of a resin sheet 600 having a support 500 and a resin composition layer 400 in one embodiment of the present invention. The inorganic filler content of the resin composition layer 400 is 40 mass% or more. This resin composition layer 400 is provided on the support 500.

[0120] 5 is a cross-sectional view that shows a schematic cross section of the support 500 and the cured body layer 100 when the resin composition layer 400 in FIG. 4 is cured to form the cured body layer 100. In a cross section of the cured body layer 100 perpendicular to a main surface 100D of the cured body layer 100 (here, the surface of the cured body layer 100 opposite to the support 500) when the resin composition layer 400 is cured to form the cured body layer 100, the area of ​​the resin component per unit area in a region 110' at a distance of 0 μm to 1 μm from the main surface 100D of the cured body layer 100 opposite to the support 500 is defined as A.0-1 In addition, the area of ​​the resin component per unit area in the region 120′ at a distance of 1 μm to 2 μm from the main surface 100D is defined as A 1-2 In this case, the cured body layer 100 satisfies the above condition (1).

[0121] Furthermore, in a cross section of the cured body layer 100 perpendicular to the main surface 100D of the cured body layer 100 when the resin composition layer 400 is cured to form the cured body layer 100, the area of ​​the resin component per unit area in a region 130′ at a distance of 0 μm to 0.5 μm from the main surface 100D of the cured body layer 100 on the side opposite to the support 500 is defined as A 0-0.5 In addition, in a cross section of the cured body layer 100 perpendicular to the main surface 100D of the cured body layer 100, the area of ​​the resin component per unit area in a region 140′ at a distance of 0.5 μm to 1 μm from the main surface 100D is defined as A 0.5-1 In this case, it is preferable that the cured body layer 100 satisfies the above condition (2).

[0122] Fig. 6 is a cross-sectional view that shows a cross section of the support 500 and the cured body layer 100 when the resin composition layer 400 in Fig. 4 is cured to form the cured body layer 100. As shown in Fig. 6, in a cross section of the cured body layer 100 perpendicular to the main surface 100D of the cured body layer 100 when the resin composition layer 400 is cured to form the cured body layer 100, the area of ​​the resin component per unit area in a region 150' at a distance of 0.5 μm to d μm from the main surface 100D of the cured body layer 100 on the side opposite to the support 500 is defined as A 0.5-d In addition, in the cross section of the cured body layer 100 perpendicular to the main surface 100D of the cured body layer 100, the area of ​​the resin component per unit area in a region 160′ at a distance of d μm to 0.5D μm from the main surface 100D is defined as A d-0.5D In this case, it is preferable that the cured body layer 100 satisfies the above condition (3).

[0123] The thickness of the resin composition layer is preferably 50 μm or less, more preferably 40 μm or less, from the viewpoint of making the printed wiring board thinner and being able to provide a cured product with excellent insulation even if the cured product of the resin composition is a thin film. The lower limit of the thickness of the resin composition layer is not particularly limited, but can usually be 5 μm or more.

[0124] When a resin composition layer comprising a first layer formed from a first resin composition and a second layer formed from a second resin composition is cured to obtain a layered gradient type cured layer, the thickness of the second layer bonded to the substrate is not limited as long as the desired effects of the present invention are obtained, but is preferably less than 2 μm, more preferably less than 1.5 μm, even more preferably 1 μm, and particularly preferably 0.8 μm.

[0125] Examples of the support include films made of plastic materials, metal foils, and release papers, with films made of plastic materials and metal foils being preferred.

[0126] When a film made of a plastic material is used as the support, examples of the plastic material include polyesters such as polyethylene terephthalate (hereinafter sometimes abbreviated as "PET") and polyethylene naphthalate (hereinafter sometimes abbreviated as "PEN"), polycarbonate (hereinafter sometimes abbreviated as "PC"), acrylics such as polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), polyether sulfide (PES), polyether ketone, polyimide, etc. Among these, polyethylene terephthalate and polyethylene naphthalate are preferred, and inexpensive polyethylene terephthalate is particularly preferred.

[0127] When a metal foil is used as the support, examples of the metal foil include copper foil, aluminum foil, etc., and copper foil is preferred. As the copper foil, a foil made of a single metal, copper, or an alloy of copper and another metal (e.g., tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.) may be used.

[0128] The surface of the support to be bonded to the resin composition layer may be subjected to a matte treatment, a corona treatment, or an antistatic treatment.

[0129] In addition, as the support, a support with a release layer having a release layer on the surface to be bonded to the resin composition layer may be used. The release agent used in the release layer of the support with a release layer may be, for example, one or more release agents selected from the group consisting of alkyd resins, polyolefin resins, urethane resins, and silicone resins. The support with a release layer may be a commercially available product, for example, "SK-1", "AL-5", and "AL-7" manufactured by Lintec Corporation, "Lumirror T60" manufactured by Toray Industries, Inc., "Purex" manufactured by Teijin Limited, and "Unipeel" manufactured by Unitika Limited, which are PET films having a release layer mainly composed of an alkyd resin-based release agent.

[0130] The thickness of the support is not particularly limited, but is preferably in the range of 5 μm to 75 μm, and more preferably in the range of 10 μm to 60 μm. When a support with a release layer is used, it is preferable that the total thickness of the support with a release layer is in the above range.

[0131] In one embodiment, the resin sheet may further include an optional layer as necessary. For example, such an optional layer may be a protective film equivalent to the support provided on the surface of the resin composition layer that is not bonded to the support (i.e., the surface opposite to the support). The thickness of the protective film is not particularly limited, but is, for example, 1 μm to 40 μm. By laminating the protective film, adhesion of dirt and the like to the surface of the resin composition layer and scratches can be suppressed.

[0132] The resin sheet can be produced, for example, by preparing a resin varnish (i.e., a coating liquid containing the resin composition) by dissolving the resin composition in an organic solvent, applying this coating liquid onto a support using a die coater or the like, and then drying it to form a resin composition layer.

[0133] When a first resin composition and a second resin composition are used to obtain a layered gradient type cured body layer, the resin composition layer can be produced by the following step (α). (α) a step of preparing a temporary resin sheet including a support and a first layer by applying a coating liquid including a first resin composition onto a support using a die coater or the like, and drying the applied liquid to form a first layer formed from the first resin composition (hereinafter also referred to as step (α1)), and a step of joining or forming a second layer formed from a second resin composition onto the first layer joined onto the support (hereinafter also referred to as step (α')).

[0134] In one embodiment, step (α') is preferably (α2) a step of applying a coating liquid containing a second resin composition onto the first layer using a die coater or the like, and drying the coating liquid to form a second layer.

[0135] In another embodiment, step (α') preferably includes: (α2') a step of applying a coating liquid containing a second resin composition onto a second support other than the support on which the first layer is formed, using a die coater or the like, and drying the coating liquid to form a second layer formed from the second resin composition, thereby preparing a temporary resin sheet including a second support and the second layer; and (α2'') a step of joining the temporary resin sheet including the first layer and the temporary resin sheet including the second layer.

[0136] Examples of organic solvents include ketones such as acetone, methyl ethyl ketone (MEK), and cyclohexanone; acetates such as ethyl acetate, butyl acetate, cellosolve acetate, propylene glycol monomethyl ether acetate, and carbitol acetate; carbitols such as cellosolve and butyl carbitol; aromatic hydrocarbons such as toluene and xylene; and amide solvents such as dimethylformamide, dimethylacetamide (DMAc), and N-methylpyrrolidone. The organic solvents may be used alone or in combination of two or more.

[0137] Drying may be performed by a known method such as heating or hot air blowing. Drying conditions are not particularly limited, but drying is performed so that the content of organic solvent in the resin composition layer becomes 10 mass % or less, preferably 5 mass % or less. Although it varies depending on the boiling point of the organic solvent in the resin varnish, for example, when a resin varnish containing 30 mass % to 60 mass % of organic solvent is used, the resin composition layer can be formed by drying at 50°C to 150°C for 3 minutes to 10 minutes.

[0138] The resin sheet can be stored in a rolled state. When the resin sheet has a protective film, it can be used by peeling off the protective film.

[0139] The resin sheet can be suitably used for forming an insulating layer of a printed wiring board (for the insulating layer of a printed wiring board), and can be more suitably used for forming an interlayer insulating layer of a printed wiring board (for the interlayer insulating layer of a printed wiring board). In particular, the resin sheet is suitable for insulating layer applications in which plasma treatment with one or more gases selected from the group consisting of O2 gas and N2 gas is applied.

[0140] <Printed wiring board> The printed wiring board has a substrate that includes the above-mentioned cured body layer as an insulating layer and further includes a conductor layer on at least a part of the outermost layer. The cured body layer is usually provided on the surface of the substrate that faces the conductor layer.

[0141] The printed wiring board can be produced, for example, by using the above-mentioned resin sheet by a method including the following steps (A) to (D): (A) a step of laminating a resin sheet including a resin composition layer having an inorganic filler content of 40% by mass or more onto a substrate having a conductor layer in at least a part of its outermost layer, such that the resin composition layer is bonded to the conductor layer side of the substrate; (B) a step of curing the resin composition layer to form a cured body layer; (C) forming a via hole in the cured layer; (D) A step of subjecting the hardened body layer to a plasma treatment with one or more gases selected from the group consisting of O2 gas and N2 gas.

[0142] When producing a printed wiring board, a step (E) of forming a conductor layer may be further carried out.

[0143] These steps (A) to (E) may be carried out according to various methods known to those skilled in the art and used in the manufacture of printed wiring boards. The support may be removed between steps (A) and (B), between steps (B) and (C), between steps (C) and (D), or between steps (D) and (E). If necessary, the formation of the cured body layer and the conductor layer in steps (B) to (E) may be repeated to form a multilayer wiring board.

[0144] Step (A) is a step of laminating a resin sheet onto a substrate such that the resin composition layer is bonded to the conductor layer side of the substrate. Thus, step (A) includes laminating a resin sheet having a support and a resin composition layer formed on the support such that the resin composition layer is bonded to the conductor layer side of the substrate.

[0145] In this specification, the substrate refers to a member that becomes the substrate of a printed wiring board, and examples thereof include a glass epoxy substrate, a metal substrate, a polyester substrate, a polyimide substrate, a BT resin substrate, and a thermosetting polyphenylene ether substrate.

[0146] The board may also have a conductor layer on one or both sides, and the conductor layer may be patterned. A board having a conductor layer (circuit) formed on one or both sides may be called an "inner layer circuit board". In addition, an intermediate product on which a cured body layer and / or a conductor layer is to be formed during the manufacture of a printed wiring board is also included in the "inner layer circuit board" of the present invention. When the printed wiring board is a circuit board with built-in components, an inner layer circuit board with built-in components may be used.

[0147] The conductor material of the conductor layer provided on the substrate is not particularly limited. In a preferred embodiment, the conductor layer contains one or more metals selected from the group consisting of gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin and indium. The conductor layer may be a single metal layer or an alloy layer, and examples of the alloy layer include layers formed from alloys of two or more metals selected from the above group (e.g., nickel-chromium alloy, copper-nickel alloy and copper-titanium alloy). Among them, from the viewpoints of versatility, cost, ease of patterning, etc. of the conductor layer formation, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver or copper, or an alloy layer of a nickel-chromium alloy, a copper-nickel alloy or a copper-titanium alloy is preferred, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver or copper, or an alloy layer of a nickel-chromium alloy is more preferred, and a single metal layer of copper is even more preferred.

[0148] The conductor layer of the substrate may be a single-layer structure or a multi-layer structure in which two or more single metal layers or alloy layers made of different types of metals or alloys are laminated. When the conductor layer has a multi-layer structure, the layer in contact with the cured body layer is preferably a single metal layer of chromium, zinc or titanium, or an alloy layer of a nickel-chromium alloy.

[0149] The thickness of the conductor layer of the substrate depends on the desired design of the printed wiring board, but is generally 1 μm to 35 μm, and preferably 5 μm to 30 μm.

[0150] The lamination of the inner layer circuit board and the resin sheet can be carried out, for example, by thermocompression bonding the resin sheet to the inner layer circuit board from the support side. Examples of the member for thermocompression bonding the resin sheet to the inner layer circuit board (hereinafter also referred to as the "thermocompression bonding member") include a heated metal plate (such as a SUS plate) or a metal roll (SUS roll). It is preferable to press the thermocompression bonding member not directly onto the resin sheet, but via an elastic material such as heat-resistant rubber so that the resin sheet can sufficiently follow the surface irregularities of the inner layer circuit board.

[0151] The lamination of the inner layer circuit board and the resin sheet may be performed by a vacuum lamination method. In the vacuum lamination method, the heat-pressure bonding temperature is preferably in the range of 60°C to 160°C, more preferably in the range of 80°C to 140°C, the heat-pressure bonding pressure is preferably in the range of 0.098MPa to 1.77MPa, more preferably in the range of 0.29MPa to 1.47MPa, and the heat-pressure bonding time is preferably in the range of 20 seconds to 400 seconds, more preferably in the range of 30 seconds to 300 seconds. The lamination is preferably performed under reduced pressure conditions of 26.7hPa or less.

[0152] The lamination can be performed by a commercially available vacuum laminator, such as a vacuum pressure laminator manufactured by Meiki Seisakusho Co., Ltd., a vacuum applicator manufactured by Nikko Materials Co., Ltd., or a batch type vacuum pressure laminator.

[0153] After lamination, the laminated resin sheet may be smoothed under normal pressure (atmospheric pressure), for example, by pressing a thermocompression member from the support side. The pressing conditions for the smoothing treatment may be the same as the thermocompression conditions for the lamination. The smoothing treatment may be performed using a commercially available laminator. The lamination and smoothing treatment may be performed consecutively using the commercially available vacuum laminator.

[0154] Step (B) is a step of curing (for example, thermally curing) the resin composition layer to form a cured layer. The curing conditions for the resin composition layer are not particularly limited, and conditions usually adopted for forming a cured layer of a printed wiring board may be used.

[0155] For example, the thermal curing conditions for the resin composition layer vary depending on the type of resin composition, etc., but the curing temperature is preferably 120° C. to 240° C., more preferably 150° C. to 220° C., and even more preferably 170° C. to 210° C. The curing time is preferably 5 minutes to 120 minutes, more preferably 10 minutes to 100 minutes, and even more preferably 15 minutes to 100 minutes.

[0156] Before the resin composition layer is thermally cured, the resin composition layer may be preheated at a temperature lower than the curing temperature. For example, prior to thermally curing the resin composition layer, the resin composition layer may be preheated at a temperature of 50° C. or more and less than 120° C., preferably 60° C. or more and less than 115° C., more preferably 70° C. or more and less than 110° C. for 5 minutes or more, preferably 5 to 150 minutes, more preferably 15 to 120 minutes, and even more preferably 15 to 100 minutes.

[0157] Step (C) is a step of forming a via hole in the cured layer. The formation of the via hole in step (C) can be performed, for example, using a laser or the like. The size and shape of the hole may be appropriately determined according to the design of the printed wiring board. If the cured layer of the present invention is used, the top diameter of the via hole can be, for example, 15 μm or less. The minimum top diameter of the via hole is not particularly limited, but is preferably 15 μm or less, more preferably 13 μm or less, and even more preferably 11 μm or less.

[0158] Step (D) is a step of subjecting the cured body layer to a plasma treatment with one or more gases selected from the group consisting of O2 gas and N2 gas. The gas used for the plasma treatment is preferably O2 gas. In this step (D), smears are removed. The procedure and conditions of the plasma treatment are not particularly limited, and known procedures and conditions that are usually used when forming a cured body layer of a printed wiring board can be adopted.

[0159] In one embodiment, the arithmetic mean roughness (Ra) of the cured body layer surface after the plasma treatment is preferably 400 nm or less, more preferably 350 nm or less, and even more preferably 300 nm or less. The lower limit is not particularly limited, but it may be preferably 0.5 nm or more, more preferably 1 nm or more, etc. In addition, the root mean square roughness (Rq) of the cured body layer surface after the plasma treatment is preferably 400 nm or less, more preferably 350 nm or less, and even more preferably 300 nm or less. The lower limit is not particularly limited, but it may be preferably 0.5 nm or more, more preferably 1 nm or more, etc. The arithmetic mean roughness (Ra) and root mean square roughness (Rq) of the cured body layer surface can be measured using a non-contact surface roughness meter.

[0160] Step (E) is a step of forming a conductor layer, and a conductor layer is formed on the cured body layer. The conductor material, shape, thickness, etc. used for the conductor layer formed in step (E) may be the same as those of the conductor layer provided on the substrate.

[0161] In one embodiment, the conductor layer may be formed by plating. For example, a conductor layer having a desired wiring pattern can be formed by plating the surface of the conductor layer by a conventionally known technique such as a semi-additive method or a full-additive method, and from the viewpoint of ease of production, it is preferable to form the conductor layer by the semi-additive method. An example of forming the conductor layer by the semi-additive method will be described below.

[0162] First, a plating seed layer is formed on the surface of a conductor layer by electroless plating. Next, a mask pattern is formed on the formed plating seed layer to expose a part of the plating seed layer corresponding to a desired wiring pattern. After a metal layer is formed on the exposed plating seed layer by electrolytic plating, the mask pattern is removed. Thereafter, unnecessary plating seed layer is removed by etching or the like to form a conductor layer having a desired wiring pattern.

[0163] In other embodiments, the conductor layer may be formed using a metal foil.

[0164] <Semiconductor device> The semiconductor device of the present invention includes the printed wiring board of the present invention. The semiconductor device of the present invention can be manufactured by using the printed wiring board of the present invention.

[0165] Examples of the semiconductor device include various semiconductor devices used in electric appliances (eg, computers, mobile phones, digital cameras, televisions, etc.) and vehicles (eg, motorcycles, automobiles, trains, ships, aircraft, etc.).

[0166] The semiconductor device of the present invention can be manufactured by mounting a component (semiconductor chip) on a conductive portion of a printed wiring board. The "conductive portion" refers to a portion of a printed wiring board that transmits an electric signal, and the portion may be either on the surface or embedded. The semiconductor chip is not particularly limited as long as it is an electric circuit element made of semiconductor material.

[0167] The method of mounting a semiconductor chip when manufacturing a semiconductor device is not particularly limited as long as the semiconductor chip functions effectively, but specific examples include a wire bonding mounting method, a flip chip mounting method, a bumpless buildup layer (BBUL) mounting method, an anisotropic conductive film (ACF) mounting method, a non-conductive film (NCF) mounting method, etc. Here, the "bumpless buildup layer (BBUL) mounting method" refers to "a mounting method in which a semiconductor chip is directly embedded in a recess in a printed wiring board and the semiconductor chip is connected to the wiring on the printed wiring board." EXAMPLES

[0168] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples. In the following description, unless otherwise specified, "parts" and "%" mean "parts by mass" and "% by mass", respectively.

[0169] <Measurement and evaluation method> First, the measurement and evaluation methods used in the physical property evaluation in this specification will be described.

[0170] [Preparation of substrate for measurement and evaluation] (1) Surface preparation for inner layer circuit boards A glass cloth-based epoxy resin double-sided copper-clad laminate (copper foil thickness 3 μm, substrate thickness 0.15 mm, Mitsubishi Gas Chemical Company's "HL832NSF LCA", 255 × 340 mm size) with a circuit formed thereon was prepared as an inner layer circuit board. Both sides of the inner layer circuit board were treated with an organic coating on the copper surface using MEC's ​​"FlatBOND-FT".

[0171] (2) Lamination of resin sheets The protective film was peeled off from the resin sheets 1 to 5 prepared in each of the following Examples and Comparative Examples. The resin sheets with the exposed resin composition layer were laminated on both sides of the inner layer circuit board using a batch type vacuum pressure laminator (Nichigo-Morton's two-stage build-up laminator "CVP700") so that the resin composition layer was bonded to the inner layer circuit board. The lamination was performed by reducing the pressure for 30 seconds to 13 hPa or less, and then pressing at 100°C and a pressure of 0.74 MPa for 30 seconds. The laminated resin sheets were then heat pressed at atmospheric pressure, 100°C, and a pressure of 0.5 MPa for 60 seconds to smooth them.

[0172] (3) Curing of the resin composition layer After laminating the resin sheets, the resin composition layers were heat-cured to form cured layers on both sides of the inner layer circuit board. At that time, the resin composition layers were heat-cured with the support attached.

[0173] The resin composition layer was thermally cured at 130°C (after being placed in a 130°C oven) for 30 minutes, and then at 175°C (after being transferred to a 175°C oven) for 30 minutes. Thereafter, the substrate was taken out into a room temperature atmosphere, and the support was peeled off. This substrate was designated evaluation substrate A. The thickness of the cured layer in evaluation substrate A was 10 μm.

[0174] (4) Formation of via holes using a UV-YAG laser Using a UV-YAG laser processing machine ("LU-2L212 / M50L" manufactured by Via Mechanics Co., Ltd.), small diameter via holes were formed in the cured layer under the following conditions. Power 0.08W, number of shots 25, target top diameter 10μm

[0175] (5) Desmearing After the via holes were formed, the inner layer circuit board on which the hardened layer was formed was treated for 5 minutes using a vacuum plasma etching device (100-E PLASMA SYSTEM manufactured by Tepla) under conditions of 100% O2 gas and a vacuum degree of 100 Pa. This board was designated as evaluation board B.

[0176] (6) Formation of the conductor layer A conductor layer was formed on the exposed surface of the cured layer. A titanium layer (30 nm thick) and then a copper layer (300 nm thick) were formed on evaluation board B using a sputtering device (Canon Anelva's "E-400S"). The obtained board was heated at 150°C for 30 minutes to perform an annealing treatment, and then an etching resist was formed according to the semi-additive method. After pattern formation by exposure and development, copper sulfate electrolytic plating was performed to form a conductor layer with a thickness of 25 μm. After the conductor pattern was formed, the board was heated at 200°C for 60 minutes to perform an annealing treatment. The obtained printed wiring board is called evaluation board C.

[0177] [Measurement of resin area ratio] For evaluation substrate A, a cross section was cut so that the cross section of the cured layer perpendicular to the support surface was exposed, and the cross section was observed with a scanning electron microscope (SEM) using a focused ion beam / scanning ion microscope (SII NanoTechnology Corp., "SMI3050SE"), and the SEM observation image was saved as an image. Using image analysis software (National Institutes of Health, "ImageJ"), the resin part was colored black and the inorganic filler part other than the resin was colored white for a certain distance a (μm) to b (μm) and for a certain distance b (μm) to c (μm) from the boundary between the support and the cured layer in a width of 7.5 μm, and the area A' of the resin part was calculated as the number of pixels in the black part for each region. a-b and A'b-c Derive the area A of the resin component per unit area corresponding to conditions (1) to (3) a-b / A b-c was calculated according to the following formula. A a-b / A b-c =k(A' a-b / A' b-c )

[0178] Here, k represents the coefficient that satisfies k=|cb| / |ba|. Condition (1)A 0-1 / A 1-2 Then, a = 0, b = 1, c = 2, and condition (2)A 0-0.5 / A 0.5-1 Then, a = 0, b = 0.5, c = 1. Condition (3)A 0.5-d / A d-0.5D For (a), d was set to 1 μm. The thickness D of the hardened layer of the evaluation substrate A was 10 μm. Therefore, under condition (3)A 0.5-d / A d-0.5D So, a=0.5, b=1, and c=5.

[0179] In addition, when measuring the resin area ratio, the binarization threshold was set so that the value of (number of pixels in the inorganic filler part) / (total number of pixels in the cross section of the cross-sectional sample) × 100 was within the range of ±3 of the volume percentage value of the inorganic filler in the cross-sectional sample, and the conditions were calibrated.

[0180] [Evaluation of smear removal] The periphery of the bottom of the via hole of evaluation substrate B was observed by SEM, and the maximum smear length from the wall surface of the bottom of the via hole was measured from the obtained image. The smear removability was evaluated according to the following criteria. Evaluation criteria: ○: Maximum smear length is less than 2 μm ×: Maximum smear length is 2 μm or more

[0181] [Measurement of adhesion strength (peel strength) between the cured layer and the conductor layer] The peel strength between the cured layer and the conductor layer was measured for evaluation substrate C in accordance with JIS C6481. Specifically, a cut was made in the conductor layer of evaluation substrate C, measuring 10 mm in width and 100 mm in length, one end of the cut was peeled off and held with a gripper, and the load when 35 mm was peeled off in the vertical direction at a speed of 50 mm / min at room temperature was measured to determine the peel strength (kgf / cm). A tensile tester ("AC-50C-SL" manufactured by TSE) was used for the measurement.

[0182] Varnishes of resin compositions 1 to 4 used in the following examples and comparative examples were prepared as follows.

[0183] [Preparation of varnish of resin composition 1] Ten parts of a bisphenol A type epoxy resin ("828US" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent: approximately 180), 20 parts of a bixylenol type epoxy resin ("YX4000H" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent: approximately 190), 10 parts of a biphenyl type epoxy resin ("NC3000L" manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent: approximately 269), 2 parts of a phosphazene resin ("SPS-100" manufactured by Otsuka Chemical Co., Ltd.), and 10 parts of a phenoxy resin ("YX7553BH30" manufactured by Mitsubishi Chemical Corporation, a 1:1 solution of MEK and cyclohexanone with a solid content of 30% by mass) were dissolved in 60 parts of MEK and 20 parts of toluene by heating with stirring. After cooling to room temperature, 30 parts of an active ester-based curing agent (DIC Corporation's "HPC-8000-65T", active group equivalent of about 223, toluene solution with a solid content of 65% by mass), 8 parts of a phenol-based curing agent (DIC Corporation's "LA-3018-50P", active group equivalent of about 151, 2-methoxypropanol solution with a solid content of 50% by mass), 6 parts of a benzoxazine compound (JFE Chemical Corporation's "ODA-BOZ", MEK solution with a solid content of 50% by mass), 4 parts of a curing accelerator (4-dimethylaminopyridine (DMAP), MEK solution with a solid content of 5% by mass), and spherical silica (Denka Corporation's "UFP-30", average particle size 0.3 μm, specific surface area 30.9 m) were added. 2 ) were mixed and uniformly dispersed in a high-speed rotary mixer, and then filtered through a cartridge filter ("SHP020" manufactured by ROKITECHNO) to prepare a varnish of resin composition 1.

[0184] [Preparation of varnish of resin composition 2] Ten parts of a bisphenol A type epoxy resin ("828US" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent approximately 180), 20 parts of a bixylenol type epoxy resin ("YX4000H" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent approximately 190), 10 parts of a biphenyl type epoxy resin ("NC3000L" manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent approximately 269), and 50 parts of a phenoxy resin ("YX7553BH30" manufactured by Mitsubishi Chemical Corporation, a 1:1 solution of MEK and cyclohexanone with a solid content of 30 mass %) were heated and dissolved in 60 parts of MEK and 20 parts of toluene with stirring. After cooling to room temperature, 30 parts of an active ester-based curing agent (DIC Corporation's "HPC-8000-65T", active group equivalent of about 223, toluene solution with solid content of 65% by mass), 8 parts of a phenol-based curing agent (DIC Corporation's "LA-3018-50P", active group equivalent of about 151, 2-methoxypropanol solution with solid content of 50% by mass), 6 parts of a benzoxazine compound (JFE Chemical Corporation's "ODA-BOZ", MEK solution with solid content of 50% by mass), and 4 parts of a curing accelerator (4-dimethylaminopyridine (DMAP), MEK solution with solid content of 5% by mass) were mixed to prepare a varnish of resin composition 2.

[0185] [Preparation of varnish of resin composition 3] Ten parts of a naphthylene ether type epoxy resin (DIC Corporation's "HP6000", epoxy equivalent approximately 250), 10 parts of a liquid naphthalene type epoxy resin (DIC Corporation's "HP4032SS", epoxy equivalent approximately 144), and 10 parts of a bixylenol type epoxy resin (Mitsubishi Chemical Corporation's "YX4000H", epoxy equivalent approximately 185) were heated and dissolved with stirring in 10 parts of MEK, 10 parts of cyclohexanone, and 40 parts of solvent naphtha. After cooling to room temperature, 16 parts of a bisphenol A dicyanate prepolymer ("BA230S75" manufactured by Lonza Japan, cyanate equivalent of about 232, MEK solution with non-volatile content of 75% by mass) and 6 parts of a phenol novolac type multifunctional cyanate ester resin ("PT30" manufactured by Lonza Japan, cyanate equivalent of about 124, MEK solution with non-volatile content of 80% by mass) were mixed with stirring, and further The mixture consisted of 12 parts of an active ester curing agent (DIC Corporation's "HPC-8000-65T," active group equivalent of approximately 223, a toluene solution with a solid content of 65% by mass), 2 parts of a 1% by mass MEK solution of 4-dimethylaminopyridine (DMAP) as a curing accelerator, 4.5 parts of a 1% by mass MEK solution of cobalt (III) acetylacetonate (Tokyo Chemical Industry Co., Ltd.), and spherical silica (Admatechs Corporation's "SOC2," surface-treated with aminosilane, average particle size 0.5 μm, specific surface area 5.9 m). 2 A varnish of resin composition 3 was prepared by mixing 140 parts of 10-(2,5-dihydroxyphenyl)-10-hydro-9-oxa-10-phosphaphenanthrene-10-oxide ("HCA-HQ-HST" manufactured by Sankosha) as a flame retardant, 4 parts of 10-(2,5-dihydroxyphenyl)-10-hydro-9-oxa-10-phosphaphenanthrene-10-oxide (manufactured by Sankosha), and 2 parts of Staphyloid (manufactured by Ganz Kasei Co., Ltd., AC3816N) as rubber particles, and dispersing the mixture uniformly using a high-speed rotating mixer. The mixture was then filtered using a cartridge filter ("SHP050" manufactured by ROKITECHNO Co., Ltd.). The nitrogen atom content of resin composition 3 was 2.02% by mass.

[0186] [Preparation of varnish of resin composition 4] A varnish of resin composition 4 was prepared in the same manner as resin composition 3, except that in resin composition 3, 16 parts of bisphenol A dicyanate prepolymer ("BA230S75" manufactured by Lonza Japan, cyanate equivalent of about 232, MEK solution with non-volatile content of 75% by mass) was changed to 8 parts, and 6 parts of phenol novolac type polyfunctional cyanate ester resin ("PT30" manufactured by Lonza Japan, cyanate equivalent of about 124, MEK solution with non-volatile content of 80% by mass) was changed to 1 part. The nitrogen atom content of resin composition 3 is 0.88% by mass.

[0187] <Example 1: Preparation of resin sheet 1> A PET film ("AL5" manufactured by Lintec Corporation) having a thickness of 38 μm was prepared as a support. A varnish of resin composition 1 was uniformly applied onto the support using a die coater, and the coating film was dried at 80 to 120 ° C. (average 100 ° C.) for 3 minutes to form a first layer (thickness 9.5 μm) formed of resin composition 1 on the support. Next, a varnish of resin composition 2 was uniformly applied onto the first layer using a die coater so that the total thickness of the resin composition layer after drying was 10 μm, and the coating film was dried at 80 ° C. for 1 minute, and the smooth surface side of a polypropylene cover film ("Alphan MA-411" manufactured by Oji F-Tex Co., Ltd.) having a thickness of 15 μm was bonded to the resin surface to produce a resin sheet 1 having a configuration of support (38 μm PET film) / resin composition layer 1 / resin composition layer 2 / protective film (MA-411).

[0188] <Example 2: Preparation of resin sheet 2> A PET film ("AL5" manufactured by Lintec Corporation) having a thickness of 38 μm was prepared as a support. The varnish of the resin composition 1 was uniformly applied onto the support by a die coater, and the coating film was dried at 80 to 120 ° C. (average 100 ° C.) for 3 minutes to prepare a resin sheet d having a layer of the resin composition 1 (thickness 9.5 μm). Next, a support of a PET film ("AL5" manufactured by Lintec Corporation) having a thickness of 25 μm was prepared, and the varnish of the resin composition 2 was uniformly applied by a die coater, and the coating film was dried at 80 ° C. for 1 minute to prepare a resin sheet e having a layer of the resin composition 2 (thickness 0.5 μm). Next, using a hot roll, the resin sheet d and the resin sheet e were overlapped to prepare a resin sheet 2 so as to have a configuration of the support (38 μm PET film) / resin composition layer 1 / resin composition layer 2 / support (25 μm release PET: peeled off before lamination as a protective film).

[0189] <Example 3: Preparation of resin sheet 3> A 38 μm thick PET film ("AL5" manufactured by Lintec Corporation) was prepared as a support. A varnish of the resin composition 3 was uniformly applied onto the support using a die coater, the applied film was dried at 80 to 120°C (average 100°C) for 3 minutes, and the smooth surface side of a 15 μm thick polypropylene cover film ("Alphan MA-411" manufactured by Oji F-Tex Co., Ltd.) was attached to the resin surface to produce a resin sheet 3 having a structure of support (38 μm PET film) / resin composition layer 3 (thickness 10 μm) / protective film (MA-411).

[0190] <Comparative Example 1: Preparation of Resin Sheet 4> Resin sheet 4 was produced in the same manner as resin sheet 3, except that resin composition 1 was used instead of the varnish.

[0191] <Comparative Example 2: Preparation of Resin Sheet 5> Resin sheet 5 was produced in the same manner as resin sheet 3, except that the varnish was changed to resin composition 4.

[0192] The evaluation results of the examples and comparative examples are shown in Table 1.

[0193] [Table 1]

[0194] The above results show that a cured layer in which conditions (1) to (3) satisfy the specified ranges maintains high peel strength and is excellent in smear removal properties by plasma treatment using N2 gas or O2 gas. [Explanation of symbols]

[0195] 100 Cured body layer 100D Main surface of hardened layer 110 Area where the distance from the conductor layer is between 0 μm and 1 μm 110' Region from 0 μm to 1 μm away from the main surface of the cured body layer on the opposite side to the support 120 Area where the distance from the conductor layer is between 1 μm and 2 μm 120' Region at a distance of 1 μm to 2 μm from the main surface of the cured body layer on the side opposite to the support 130 Area where the distance from the conductor layer is between 0 μm and 0.5 μm 130' Region at a distance of 0 μm to 0.5 μm from the main surface of the cured body layer on the side opposite to the support 140 Area with distance from conductor layer between 0.5μm and 1μm 140' Region at a distance of 0.5 μm to 1 μm from the main surface of the cured body layer on the side opposite to the support 150 Area where the distance from the conductor layer is between 0.5μm and dμm 150' Region from 0.5 μm to d μm away from the main surface of the cured body layer on the side opposite to the support 160 Area where the distance from the conductor layer is between dμm and 0.5Dμm 160' Region where the distance from the main surface of the cured body layer on the opposite side to the support is from dμm to 0.5Dμm 200 Substrates Conductor layer side of 210U board 210 Conductor layer 300 Beer Hall Side of 300S via hole 310 Smear 320 Bottom of via hole 400 Resin composition layer 500 support 600 Resin Sheet

Claims

1. A resin sheet laminated on a substrate having a conductor layer on at least a portion of an outermost layer, such that a resin composition layer is bonded to a surface of the substrate on the conductor layer side, The resin sheet has a support and a resin composition layer having an inorganic filler content of 40% by mass or more, the support has a release layer on a surface to be bonded to the resin composition layer, The nitrogen atom content of the resin composition is 1.0% by mass or more when the resin component in the resin composition is 100% by mass, When the resin composition layer is cured to form a cured body layer, in a cross section of the cured body layer perpendicular to the main surface of the cured body layer, the area of ​​the resin component per unit area in a region from 0 μm to 1 μm away from the main surface of the cured body layer on the side opposite to the support, which is bonded to a surface of the conductor layer side of a substrate having a conductor layer in at least a part of the outermost layer, is represented by A. 0-1 The area of ​​the resin component per unit area in the region from 1 μm to 2 μm is A 1-2 In this case, A 0-1 / A 1-2 > A resin sheet that satisfies 1.

1.

2. In the cross section, the area of ​​the resin component per unit area in a region from 0 μm to 0.5 μm from the main surface of the cured body layer on the side opposite to the support, which is bonded to the surface of the conductor layer side of a substrate having a conductor layer in at least a part of the outermost layer, is represented by A 0-0.5 The area of ​​the resin component per unit area in the region from 0.5 μm to 1 μm is A 0.5-1 In this case, A 0-0.5 / A 0.5-1 The resin sheet according to claim 1, wherein the resin sheet satisfies > 1.

1.

3. In the cross section, the area of ​​the resin component per unit area in a region from 0.5 μm to d μm from the main surface of the cured body layer on the side opposite to the support, which is bonded to the surface of the conductor layer side of a substrate having a conductor layer in at least a part of the outermost layer, is represented by A 0.5-d The area of ​​the resin component per unit area in the region from d μm to 0.5D μm is A d-0.5D In this case, 0.9≦A 0.5-d / A d-0.5D 3. The resin sheet according to claim 1 or 2, wherein d is a number satisfying 0.5<d<0.5D, and D is a thickness of the cured body layer.

4. The resin sheet according to any one of claims 1 to 3, wherein the resin composition layer contains an epoxy resin.

5. The resin composition layer comprises a first layer formed of a first resin composition and a second layer formed of a second resin composition having a composition different from the first resin composition. The resin sheet according to any one of claims 1 to 4.

6. The resin sheet according to claim 5 , wherein the second layer has a thickness of less than 2 μm, and the first layer is bonded to the support.

7. The resin sheet according to claim 5 or 6, wherein the second resin composition has an inorganic filler content of less than 20 mass%, and the first layer is bonded to the support.

8. (A) a step of laminating a resin sheet including a resin composition layer having an inorganic filler content of 40% by mass or more onto a substrate having a conductor layer in at least a part of an outermost layer such that the resin composition layer is bonded to a surface of the substrate on the conductor layer side; (B) curing the resin composition layer to form a cured layer; and (C) Step of forming via holes in the cured body layer A method for producing a printed wiring board comprising: In a cross section of the cured body layer perpendicular to the main surface of the cured body layer, the area of ​​the resin component per unit area in a region at a distance of 0 μm to 1 μm from the conductor layer is defined as A. 0-1 The area of ​​the resin component per unit area in the region from 1 μm to 2 μm is A 1-2 In this case, A 0-1 / A 1-2 A method for manufacturing a printed wiring board that satisfies 1.

1.

9. In the cross section, the area of ​​the resin component per unit area in the region from 0 μm to 0.5 μm away from the conductor layer is defined as A 0-0.5 The area of ​​the resin component per unit area in the region from 0.5 μm to 1 μm is A 0.5-1 In this case, A 0-0.5 / A 0.5-1 The method for producing a printed wiring board according to claim 8 , wherein the ratio of the first to the second components is 1.0 to 1.

1.

10. In the cross section, the area of ​​the resin component per unit area in the region from 0.5 μm to d μm away from the conductor layer is defined as A 0.5-d The area of ​​the resin component per unit area in the region from d μm to 0.5D μm is A d-0.5D In this case, 0.9≦A 0.5-d / A d-0.5D 10. The method for producing a printed wiring board according to claim 8, wherein d is a number that satisfies 0.5<d<0.5D, and D is a thickness of the cured body layer.

11. The method for producing a printed wiring board according to any one of claims 8 to 10, wherein the resin composition layer contains an epoxy resin.

12. The method for producing a printed wiring board according to any one of claims 8 to 11, wherein the resin composition layer comprises a first layer formed of a first resin composition and a second layer formed of a second resin composition having a composition different from that of the first resin composition.

13. The method for producing a printed wiring board according to claim 12 , wherein the second layer has a thickness of less than 2 μm, and the second layer is bonded to the substrate in step (A).

14. The method for producing a printed wiring board according to claim 12 or 13, wherein the second resin composition has an inorganic filler content of less than 20 mass%, and the second layer is bonded to the substrate in step (A).

15. The method for manufacturing a printed wiring board according to any one of claims 8 to 14, wherein the top diameter of the via hole is 15 µm or less.

16. The method for producing a printed wiring board according to any one of claims 8 to 15, wherein the step (A) includes laminating a resin sheet having a support and the resin composition layer formed on the support such that the resin composition layer is bonded to a surface of the substrate on the conductor layer side.

17. (A) a step of laminating a resin sheet including a resin composition layer having an inorganic filler content of 40% by mass or more onto a substrate having a conductor layer in at least a part of an outermost layer such that the resin composition layer is bonded to a surface of the substrate on the conductor layer side; (B) curing the resin composition layer to form a cured layer; and (C) Step of forming via holes in the cured body layer A method for producing a cured body layer comprising: In a cross section of the cured body layer perpendicular to the main surface of the cured body layer, the area of ​​the resin component per unit area in a region at a distance of 0 μm to 1 μm from the conductor layer is defined as A. 0-1 The area of ​​the resin component per unit area in the region from 1 μm to 2 μm is A 1-2 In this case, A 0-1 / A 1-2 A method for producing a cured body layer, which satisfies the above requirement.

18. 18. The method for producing a cured body layer according to claim 17, wherein step (A) comprises laminating a resin sheet having a support and the resin composition layer formed on the support such that the resin composition layer is bonded to a surface of the substrate on the conductor layer side.

Citation Information

Patent Citations

  • Manufacturing method of printed wiring board

    JP2007273615A

  • Cured body, laminate, printed circuit board and semiconductor device

    JP2014062230A

  • Resin sheet with support

    JP2015150885A

  • Adhesive sheet with protection film

    JP2016020480A

  • Adhesive film for multilayer printed wiring board

    JP2017147421A