Method for manufacturing joined body and method for manufacturing insulating circuit board
By using metal foils with specific Young's modulus and thickness values, the method ensures uniform pressure application and prevents foreign matter adhesion, addressing non-uniform bonding and surface roughness issues in power module substrates.
Patent Information
- Application Number
- JP2022510479
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-03-24
- Filing Date
- 2021-03-22
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2041-03-22
AI Technical Summary
Existing methods for bonding metal plates in power module substrates face issues with non-uniform pressure application and foreign matter adhesion due to the use of carbon spacers, leading to poor bonding and surface roughness, which prevents semiconductor mounting.
The use of metal foils with specific Young's modulus and thickness values to uniformly press and heat the laminate, preventing foreign matter adhesion and ensuring even bonding by following the laminate's surface shape.
Achieves high-quality bonding with uniform pressure application and suppresses foreign matter adhesion, resulting in a high-quality bonded body suitable for semiconductor mounting.
Smart Images

Figure 0007582299000003 
Figure 0007582299000004 
Figure 0007582299000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a bonded body made of multiple different metal plates, such as a power module substrate having a two-layer circuit layer, and in particular to a manufacturing method suitable for bonding metal plates together by solid-phase diffusion bonding, and a manufacturing method for an insulated circuit board using the manufacturing method for the bonded body. This application claims priority based on Japanese Patent Application No. 2020-052827, filed on March 24, 2020, the contents of which are incorporated herein by reference. [Background technology]
[0002] A power module substrate (insulating circuit substrate) generally has a structure in which a circuit layer is formed on one surface of a ceramic substrate that serves as an insulating layer, and a heat dissipation layer for heat dissipation is formed on the other surface.
[0003] As an example of such a power module substrate, a power module substrate is disclosed in Patent Document 1. In this power module substrate, metal plates made of aluminum or an aluminum alloy, or copper or a copper alloy, are bonded to both sides of a ceramic substrate via brazing material, thereby forming a circuit layer on one side of the ceramic substrate and a heat dissipation layer on the other side. A heat dissipation plate made of aluminum or an aluminum alloy, or copper or a copper alloy, is bonded to the heat dissipation layer.
[0004] In this power module substrate, the ceramic substrate and the metal plate are bonded by applying pressure and heat to the laminate using a pressure device. At this time, a spacer made of a carbon layer and a graphite layer is interposed between the laminate and the pressure device. In this case, the carbon layer is disposed on the laminate side. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2016-63145 A Summary of the Invention [Problem to be solved by the invention]
[0006] In some cases, the circuit layer of this type of power module substrate has a two-layer structure of aluminum and copper. To manufacture such a joint consisting of multiple different metal plates, a copper plate is joined to an aluminum layer formed on a ceramic substrate by the method described in Patent Document 1 to form a copper layer, but the joining of aluminum and copper may be performed by solid-phase diffusion bonding, which involves applying pressure and heat without using a brazing material.
[0007] In this case, it is necessary to apply pressure more uniformly than in joining via a brazing material, but in the pressing device described in Patent Document 1, the side of the spacer that comes into contact with the laminate is formed from a carbon layer, so displacement due to the application of load when pressing is small. If there are minute irregularities on the surface of the laminate or if it has a high degree of flatness, the pressure may not be applied uniformly, which may result in poor joining.
[0008] Furthermore, if the surface of the spacer that contacts the laminate is formed of a carbon layer, this carbon layer may locally fall off when it is heated and pressurized together with the laminate, and part of the carbon layer may adhere to the surface of the laminate. Even if a soft etching process is performed on the surface of the bonded body to remove this foreign matter, it is not possible to completely remove it, resulting in a problem that semiconductor elements and the like cannot be mounted on the laminate (circuit layer) after bonding.
[0009] On the other hand, if a strong etching process is performed to remove foreign matter, the surface of the laminate after bonding becomes rough, so in this case too, it is not possible to mount a semiconductor element or the like on the circuit layer.
[0010] The present invention has been made in view of the above circumstances, and aims to produce a good joined body by uniformly pressing the laminate when joining a laminate of a plurality of different metal plates under pressure and heat, and to prevent foreign matter from adhering to the surface of the laminate. Another object of the present invention is to produce an insulated circuit board using the manufacturing method. [Means for solving the problem]
[0011] The method for manufacturing a joined body of the present invention is a method for manufacturing a joined body by heating a laminate of a first plate member and a second plate member while applying pressure to it to produce a joined body, wherein the first plate member includes a first metal plate, a first pressing member having a first metal foil / carbon sheet or a ceramic sheet / graphite sheet laminated in that order is arranged so that the first metal foil is in contact with the surface of the first metal plate, the first metal foil is made of a material that does not react when heated at the contact surface between the first plate member and the first metal foil, and the product of the Young's modulus (GPa) and the thickness (mm) of the first metal foil is 0.6 or more and 100 or less.
[0012] In the present invention, the Young's modulus and thickness are values measured at 25°C.
[0013] By using a first metal foil made of a material that does not react with the surface of the first metal plate of the laminate when heated, when the laminate is pressurized and heated through this first metal foil, it is possible to prevent part of the carbon sheet or ceramic sheet from adhering to the surface of the laminate (first metal plate).
[0014] In addition, the first metal foil deforms due to its ductility so as to absorb minute irregularities on the surface of the laminate and gaps due to flatness, so that a uniform load can be applied to the laminate to produce a bonded body in which the entire surface is evenly bonded. Furthermore, since a soft graphite sheet is disposed on the back surface of the hard carbon or ceramic sheet, the first metal foil can be made to conform to the surface shape of the laminate more easily, thereby improving bondability.
[0015] By setting the product of the Young's modulus (GPa) and thickness (mm) of the first metal foil to be 0.6 or more and 100 or less, the foil can bend locally to conform to the surface shape of the laminate when pressed, and the entire surface of the laminate can be pressed, thereby enabling the plate components to be joined with high precision.
[0016] Furthermore, there is no risk of the first metal foil cracking or parts of the metal foil peeling off and adhering to the laminate when pressure is applied, and a high-quality bonded body with few defects can be produced while suppressing damage to the carbon sheet or ceramic sheet.
[0017] If the product of Young's modulus (GPa) and thickness (mm) exceeds 100, the first metal foil is impaired in its ability to conform to the surface shape of the laminate, resulting in poor bonding. If it is less than 0.6, the metal foil breaks and carbon or ceramics adheres to the surface of the laminate.
[0018] In the present invention, a second pressing member having a second metal foil / carbon sheet or a ceramic sheet / graphite sheet laminated in this order is arranged so that the second metal foil is in contact with the surface of the second plate member, the second metal foil is made of a material that does not react when heated at the contact surface between the second plate member and the second metal foil, and the product of the Young's modulus (GPa) and the thickness (mm) of the second metal foil is preferably 0.6 or more and 100 or less.
[0019] By providing metal foil made of a material that does not react with the surface of the laminate when heated on both sides of the laminate, it is possible to reliably prevent parts of the carbon sheet or ceramic sheet from adhering to the surface of the laminate.
[0020] In the present invention, either the first plate member or the second plate member may be made of copper or a copper alloy, and the other may be made of aluminum or an aluminum alloy.
[0021] Aluminum and copper are generally bonded by solid-state diffusion bonding, and the present invention is particularly effective in bonding them in this solid phase.
[0022] The present invention does not exclude liquid phase bonding using a brazing material. For example, the present invention can be applied to a case where the first plate member is made of a metal plate, the second plate member is made of a ceramic substrate, and they are bonded together using a brazing material.
[0023] The method for manufacturing an insulated circuit board of the present invention is a method for manufacturing an insulated circuit board using the above-mentioned method for manufacturing a bonded body, wherein the first plate member is a first metal plate made of copper or a copper alloy, the second plate member is a ceramic substrate and a second metal plate made of aluminum or an aluminum alloy bonded to one side of the ceramic substrate, the first metal plate is laminated on the second metal plate bonded to the ceramic substrate to form the laminate, and the first metal plate and the second metal plate are solid-state diffusion bonded with the first metal plate in contact with the first metal foil.
[0024] The method for producing an insulating circuit board of the present invention is a method for producing an insulating circuit board using the above-mentioned method for producing a bonded body, in which the first plate member is formed by laminating a first metal plate made of copper or a copper alloy and an AlSiC composite material obtained by impregnating a porous body of silicon carbide with a metal mainly composed of aluminum, the second plate member is formed by laminating a ceramic substrate, a second metal plate made of aluminum or an aluminum alloy bonded to both sides of the ceramic substrate, and the first metal plate laminated on one of the second metal plates, the other second metal plate of the second plate member is brought into contact with the first metal plate of the first plate member to laminate the first plate member and the second plate member to form the laminate, and the first metal foil of the first pressing member is brought into contact with the AlSiC composite material of the laminate, and the second metal foil of the pressing member is brought into contact with the surface of the first metal plate of the second plate member with the base, and the first metal plate and the second metal plate, and the first metal plate and the AlSiC composite are simultaneously solid-phase diffusion bonded to each other in a state where the first metal foil of the pressing member is brought into contact with the surface of the first metal plate of the second plate member. Effect of the Invention
[0025] According to the method for manufacturing a bonded body of the present invention, when a stack of multiple different plate members is pressurized and bonded in a heated state, a uniform pressure is applied to the stack to produce a good bonded body and the adhesion of foreign matter to the surface of the stack can be suppressed. [Brief description of the drawings]
[0026] [Figure 1]FIG. 1 is a cross-sectional view showing a power module substrate as an embodiment of a bonded body (insulating circuit board) of the present invention. [Diagram 2] 2A to 2C are cross-sectional views (part 1) illustrating a manufacturing process for the power module substrate in FIG. [Diagram 3] 2 is a cross-sectional view (part 2) showing a manufacturing process of the power module substrate in FIG. [Figure 4] FIG. 4 is a front view of a pressure device used in the manufacturing method of FIGS. 2 and 3. [Diagram 5] FIG. 5 is a cross-sectional view of a spacer used in the pressure device of FIG. [Figure 6] 1 is an SEM image of the surface of the circuit layer of Sample No. 2 in the example. [Figure 7] 1 is an SEM image of the surface of the circuit layer of Sample No. 1 in the examples. [Figure 8] 10A to 10C are cross-sectional views showing a manufacturing process of another power module substrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.
[0028] This embodiment is a power module substrate 1 as an example of an insulating circuit substrate (joint). As shown in Fig. 1, this power module substrate 1 includes a ceramic substrate 10, a circuit layer 20 bonded to one surface of the ceramic substrate 10, and a heat dissipation layer 30 bonded to the other surface of the ceramic substrate 10.
[0029] The ceramic substrate 10 is made of, for example, AlN (aluminum nitride), Si 3 N 4 (Silicon nitride) and other nitride ceramics, or Al 2 O 3 The ceramic substrate 10 may be made of oxide-based ceramics such as alumina, etc. The thickness of the ceramic substrate 10 is set to be 0.2 mm or more and 1.5 mm or less.
[0030] The circuit layer 20 and the heat dissipation layer 30 each have a two-layer structure made of a second metal layer 41 made of aluminum or an aluminum alloy and a first metal layer 42 made of copper or a copper alloy. In other words, in the power module substrate 1, the second metal layer 41 is formed on both sides of the ceramic substrate 10, and the first metal layer 42 is formed on the second metal layer 41.
[0031] The second metal layer 41 can be made of pure aluminum having a purity of 99% by mass or more (for example, pure aluminum in the 1000 series according to the JIS standard, particularly 1N90 (purity of 99.9% by mass or more: so-called 3N aluminum) or 1N99 (purity of 99.99% by mass or more: so-called 4N aluminum), or an aluminum alloy such as an A6063 series. In order to buffer the difference in thermal expansion and contraction between the first metal layer 42 and the ceramic substrate 10, it is preferable to use pure aluminum for the second metal layer 41.
[0032] The first metal layer 42 is preferably made of, for example, copper with a purity of 99.96% by mass or more (oxygen-free copper) or copper with a purity of 99.90% by mass or more (tough pitch copper).
[0033] The thicknesses of the second metal layer 41 and the first metal layer 42 are not limited, but for example, the second metal layer 41 is 0.1 mm or more and 2.0 mm or less, and the first metal layer 42 is 0.2 mm or more and 5.0 mm or less. The second metal layer 41 and the first metal layer 42 may have the same thickness in the circuit layer 20 and the heat dissipation layer 30, or may have different thicknesses. In the illustrated example, the second metal layer 41 and the first metal layer 42 are denoted by the same reference numerals without distinguishing between the circuit layer 20 and the heat dissipation layer 30.
[0034] A method for manufacturing the power module substrate 1 thus configured will be described.
[0035] First, as shown in FIG. 2, a second metal plate 41a made of aluminum or an aluminum alloy is laminated on both sides of a ceramic substrate 10 via a brazing material 50, and the laminate is pressurized and heated to bond the ceramic substrate 10 and the second metal plate 41a, thereby forming a second metal layer 41 on both sides of the ceramic substrate 10 (first bonding process).
[0036] Next, as shown in FIG. 3, a first metal plate 42a made of copper or a copper alloy is laminated on the second metal layer 41, and the laminate is pressurized and heated to perform solid-state diffusion bonding between the aluminum and copper, thereby forming a first metal layer 42 on the second metal layer 41 (second bonding process).
[0037] In the first bonding step, the second metal plate 41a corresponds to the first plate member of the present invention, and the ceramic substrate 10 corresponds to the second plate member of the present invention. Meanwhile, in the second bonding step, the first metal plate 42a corresponds to the first plate member of the present invention, and the ceramic substrate 10 and the second metal plate 41a (second metal layer 41) bonded to one surface of the ceramic substrate 10 correspond to the second plate member of the present invention.
[0038] In this manufacturing method, a pressure device 110 shown in Fig. 4 is used to pressurize the laminate in the first bonding step and the laminate in the second bonding step. In the following, the laminate in the first bonding step (a laminate made of the ceramic substrate 10 and both second metal plates 41a) and the laminate in the second bonding step (a laminate made of the ceramic substrate 10 on which both second metal layers 41 are formed and the first metal plate 42a) will be described as the laminate S without distinction.
[0039] The pressure applying device 110 comprises a base plate 111, guide posts 112 attached vertically to the four corners of the upper surface of the base plate 111, a fixed plate 113 fixed to the upper ends of the guide posts 112, a pressure plate 114 supported by the guide posts 112 so as to be freely movable up and down between the base plate 111 and the fixed plate 113, and a biasing portion 115 such as a spring provided between the fixed plate 113 and the pressure plate 114 to bias the pressure plate 114 downward.
[0040] The fixed plate 113 and the pressure plate 114 are disposed parallel to the base plate 111, and the laminate S is disposed between the base plate 111 and the pressure plate 114.
[0041] On the sides of the base plate 111 and the pressing plate 114 that come into contact with the laminate S, a spacer 60 is disposed to ensure uniform pressure.
[0042] Each spacer 60 corresponds to the first pressing member and the second pressing member of the present invention, and has a structure in which a graphite sheet 61, a carbon sheet 62, and a metal foil (first metal foil or second metal foil) 63 are laminated in this order, as shown in FIG.
[0043] Graphite sheet 61 is made of a soft graphite material having cushioning properties, and is constructed by laminating multiple thin flake graphite films like mica. It is made by treating natural graphite with acid, forming it into a sheet, and rolling it. This graphite sheet 61 has a bulk density of 0.5 Mg / m 3 More than 1.3Mg / m 3 For example, Asahi Graphite Co., Ltd.'s T-5 (thermal conductivity: 75.4 W / mK, elastic modulus: 11.4 GPa) and Toyo Tanso Co., Ltd.'s graphite sheet PF (compressibility 47%, recovery rate 14%) can be used.
[0044] The carbon sheet 62 is made of a heat-resistant hard carbon material and formed into a flat plate shape, and is sintered at a high temperature of about 3000° C. The carbon sheet 62 has a bulk density of 1.6 Mg / m 3 More than 1.9Mg / m 3 The substrate is configured to have a relatively hard and smooth flat surface as follows. For example, G-347 (thermal conductivity: 116 W / mK, elastic modulus: 10.8 GPa) manufactured by Asahi Graphite Co., Ltd. can be used.
[0045] The metal foil 63 corresponds to the first metal foil and the second metal foil of the present invention, and is made of a material that does not react with the surface of the laminate S when heated. When the first metal plates 42a arranged on both sides of the laminate S are made of copper or a copper alloy, it is preferable that the metal foil 63 is made of copper or a copper alloy, or stainless steel. The non-reactive material refers to a material that does not peel off when cooled from the joining temperature to room temperature, and in which no intermetallic compound is formed between the metal foil and the surface of the laminate.
[0046] The thickness of the spacer 60 is not particularly limited, but for example, the graphite sheet 61 is 0.5 mm to 5.0 mm, the carbon sheet 62 is 0.5 mm to 2.0 mm, and the metal foil 63 is 0.005 mm to 0.15 mm.
[0047] As described above, the metal foil 63 can be made of any suitable metal as long as it is a material that does not react with the surface of the laminate S (copper in this case) when heated, but the product of Young's modulus (GPa) and thickness (mm) is set to be 0.6 or more and 100 or less. If the product is less than 0.6, the metal foil 63 will break and carbon will adhere to the surface of the laminate S, and if it exceeds 100, the ability to conform to the surface shape of the laminate S will be impaired, resulting in poor bonding.
[0048] The Young's modulus (GPa) and thickness are values at room temperature (25° C.).
[0049] In this embodiment, the carbon sheet 62 is used, but the present invention is not limited to this, and any material that is hard and does not deform when heated may be used, for example, a ceramic sheet. The ceramic sheet is a sintered body made of various ceramics such as aluminum nitride, silicon nitride, alumina, etc., in a sheet shape. Specifically, for example, the Al 2 O 3 A ceramic sintered sheet can be used. When a ceramic sheet is used, the thickness can be set to 0.3 mm or more and 2.0 mm or less.
[0050] Hereinafter, the first bonding step and the second bonding step using this pressure device 110 will be described in order.
[0051] (First joining process) 2, a second metal plate 41a made of aluminum or an aluminum alloy is laminated on both sides of a ceramic substrate 10 via a brazing material 50 to form a laminate S. As the brazing material 50, an alloy such as an Al-Si based, Al-Ge based, Al-Cu based, Al-Mg based, or Al-Mn based alloy is used.
[0052] 4, the laminate S is pressed in the stacking direction and heated together with the pressurizing device 110 in a vacuum atmosphere, thereby bonding the second metal plate 41a to the ceramic substrate 10 and forming the second metal layer 41 on both sides of the ceramic substrate 10. In this case, since the surface of the laminate S is made of aluminum or an aluminum alloy, the metal foil 63 is made of aluminum foil, aluminum alloy foil, or stainless steel foil.
[0053] The pressure at this time is, for example, 0.1 MPa to 3.4 MPa, the joining temperature is 600° C. to 655° C., and the heating time is 15 minutes to 120 minutes.
[0054] (Second joining process) As shown in FIG. 3, a laminate S is formed by laminating a first metal plate 42a made of copper or a copper alloy on each of second metal layers 41 formed on both sides of a ceramic substrate 10.
[0055] 4, the laminate S is pressed in the stacking direction, and the pressurizing device 110 is heated in a vacuum atmosphere to solid-state diffusion bond the first metal plate 42a to the second metal layer 41, thereby forming the first metal layer 42 on the second metal layer 41. In this case, since the surface of the laminate S is copper or a copper alloy, a copper foil, a copper alloy foil, or a stainless steel foil is used for the metal foil 63.
[0056] The stainless steel foil may be, for example, a foil material of SUS304. Titanium or nickel foil may also be used. In this case, it is preferable to use titanium or nickel foil with a purity of 99% or more.
[0057] In this case, the pressure is, for example, from 0.3 MPa to 3.5 MPa, and the heating temperature is from 400° C. to less than 548° C. By maintaining this pressurized and heated state for 5 minutes to 240 minutes, the second metal layer 41 and the first metal plate 42a are solid-phase diffusion bonded together, and the first metal layer 42 is formed on the second metal layer 41.
[0058] As described above, in the pressure application device 110 of this embodiment, a spacer 60 is interposed between the laminate S, in which a first metal plate 42a is laminated on a second metal layer 41, and the base plate 111 and the pressing plate 114, and a metal foil 63 is arranged on the contact surface side of the spacer 60 with the laminate S.
[0059] Since the metal foil 63 is a ductile material, even if the surface of the laminate S is uneven or has low flatness, the metal foil 63 deforms to follow the shape of the surface. Moreover, since the product of the Young's modulus (GPa) and the thickness (mm) of the metal foil 63 is set to 0.6 to 100, the metal foil 63 has excellent deformability as described above.
[0060] Therefore, it is possible to apply a uniform pressure to the entire surface of the laminate S, thereby uniformly bonding the entire surface. In addition, since it is not a brittle material like a carbon sheet, it will not be damaged by pressure, and since it is a material that does not react with the first metal plate 42a provided on the surface of the laminate S, it will not adhere to the first metal plate 42a.
[0061] As described above, by using the pressure device 110 provided with the spacer 60, a high-quality power module substrate (insulating circuit substrate) 1 without bonding defects can be manufactured.
[0062] The present invention is not limited to the configurations of the above-described embodiments, and various modifications can be made without departing from the spirit of the present invention.
[0063] For example, the manufacturing method of the present invention can be applied to the case where a circuit layer having a two-layer structure of an aluminum layer and a copper layer is formed on one surface of a ceramic substrate, and the other surface of the ceramic substrate does not need to have a two-layer heat dissipation layer as in the embodiment. In this case, the spacer in contact with the ceramic substrate 10 does not need to include the metal foil 63.
[0064] In the above embodiment, the surface of the laminate is made of copper or a copper alloy, but it may also be made of aluminum or an aluminum alloy, in which case it is desirable for the metal foil of the spacer to be aluminum, an aluminum alloy, or stainless steel.
[0065] The manufacturing method of the present invention may be applied not only to joining a metal plate made of copper or a copper alloy to a metal plate made of aluminum or an aluminum alloy, but also to joining an AlSiC composite material to copper or a copper alloy.
[0066] AlSiC composites are composites of aluminum and silicon carbide formed by impregnating a porous body made of silicon carbide (SiC) with a metal whose main component is aluminum (Al: pure aluminum or aluminum alloy), and an aluminum coating layer is formed on the surface of the porous body.
[0067] When using this AlSiC composite, as shown in Figure 8, a first metal plate 42a made of copper or a copper alloy is laminated on each second metal layer 41 formed on both sides of a ceramic substrate 10, and a plate-shaped AlSiC composite 70 is laminated on one of the first metal plates 42a to form a laminate.
[0068] By contacting this laminate with the metal foil (first metal foil) 63 of the spacer (first pressing material) 60 on the surface of the AlSiC composite 70 and with the metal foil (second metal foil) 63 of the spacer (second pressing material) 60 on the surface of the first metal plate 42a, and by heating the laminate in a vacuum atmosphere while pressing it in the stacking direction, each second metal layer 41 and the first metal plate 42a, and further the first metal plate 42a and the AlSiC composite 70 can be simultaneously solid-state diffusion bonded.
[0069] In this case, a circuit layer and a heat dissipation layer each consisting of a first metal layer and a second metal layer are formed on a ceramic substrate by the method described in the above embodiment, and an AlSiC composite material is bonded to the first metal layer of the heat dissipation layer as a heat sink to produce an insulated circuit substrate.
[0070] That is, second metal layers are formed on both sides of a ceramic substrate (by a first bonding process), each first metal plate is laminated onto each second metal layer, and an AlSiC composite is laminated onto one of the first metal plates, and the laminate is pressurized and heated to perform solid-state diffusion bonding (second bonding process).
[0071] In addition, the present invention is not limited to the circuit layer and heat dissipation layer of the power module substrate, but can be applied to combinations of metals that can be bonded in liquid and solid phases, and is particularly effective for combinations of metals that can be bonded in solid phase. The present invention can also be applied to bonding between a metal plate and a plate member other than a metal plate (for example, a ceramic substrate). EXAMPLES
[0072] An evaluation test was carried out to confirm the effect of the present invention. In this test, a second metal plate made of aluminum or an aluminum alloy and a first metal plate made of copper or a copper alloy were laminated and joined. An aluminum alloy (A6063) was used as the second metal plate, and pure copper (C1020) was used as the first metal plate. The metal plate in contact with the spacer was used as the adherend.
[0073] The spacer was a laminated structure of a graphite sheet, a carbon sheet or a ceramic sheet, and a metal foil. For the metal foil, SUS304 was used as stainless steel (SUS), C1020 as copper (Cu), or A6063 as aluminum (Al). The Young's modulus and thickness of each were as shown in Table 1 (values at room temperature (25°C)).
[0074] Graphite sheet (PF-100 manufactured by Toyo Tanso Co., Ltd.), carbon sheet (G-347 manufactured by Asahi Graphite Co., Ltd.), ceramic sheet (Al manufactured by Maruwa Co., Ltd.) 2 O 3 A test was also conducted using a spacer made of a sintered ceramic sheet.
[0075] The laminate of both metal plates was pressurized and heated at a pressure of 1.0 MPa, at a temperature of 500°C, and for a holding time of 30 minutes, and the spacer adhesion, bonding ability (following ability), and shedding (adhesion of foreign matter) to the surface were evaluated.
[0076] (Evaluation of spacer adhesion) Regarding the adhesion of the spacer, after bonding, the spacer was cooled to room temperature, and the metal foil could be manually peeled off from the laminate. Furthermore, the cross sections of the metal foil and the laminate surface were observed under an SEM. If no intermetallic compound was formed between the metal foil and the laminate surface, the spacer was rated as "A", and all other cases were rated as "B".
[0077] (Evaluation of Jointness) Bonding was evaluated using an ultrasonic flaw detector (FINESAT manufactured by Hitachi Power Solutions) to observe the interface between the two metal layers and measure the area to be bonded. The bonding rate was calculated from the area to be bonded (area of the metal layers) before bonding. A bonding rate of 95% or more was given an "A" rating, and a rate of less than 95% was given a "B".
[0078] (Evaluation of surface shedding) After bonding, the spacer was peeled off from the adherend, and the surface of the adherend after 2-3 μm soft etching was observed with SEM-EDX. If no carbon or ceramic components were attached to the pressurized area, it was rated as "A," and if some of the metal foil remained on the adherend, it was rated as "B."
[0079] For soft etching, if the adherend material was Al, a sodium hydroxide solution (concentration: 5% by mass) was used, and the etching was performed for 2 minutes at 50°C. If the adherend material was Cu, ADEKA CL-8 (dilution rate: 20% by volume) was used, and the etching was performed for 2 minutes at room temperature (25°C).
[0080] [Table 1]
[0081] [Table 2]
[0082] As shown in Tables 1 and 2, samples No. 8 to 20, which use metal foil on the spacer surface that does not react with the adherend and have a metal foil Young's modulus x thickness product between 0.6 and 100, show no adhesion to the adherend. Specifically, the SEM image of sample No. 8 shown in Figure 6 shows that no foreign matter is attached to the adherend surface. On the other hand, the SEM image of sample No. 1 shown in Figure 7 shows that foreign matter is attached to the adherend surface.
[0083] In samples Nos. 4 and 6, the product of Young's modulus and thickness of the metal foil was too large, resulting in poor bonding. In samples Nos. 3 and 5, the product of Young's modulus and thickness of the metal foil was too small, resulting in the metal foil breaking and foreign matter being observed at the breakage points.
[0084] In sample No. 7, an intermetallic compound was confirmed by SEM observation of the Cu / Al cross section, and a failure occurred in the spacer adhering to the adherend. [Industrial Applicability]
[0085] When a stack of multiple different plate members is pressed and bonded in a heated state, a uniform pressure is applied to the stack to produce a good bonded body and the adhesion of foreign matter to the surface of the stack can be suppressed. [Explanation of symbols]
[0086] 1 Power module substrate (joint) (insulated circuit board) 10 Ceramic substrate (second plate member) 20 circuit layers 30 Heat dissipation layer 41 Second metal layer (second plate member) 41a Second metal plate (first plate member / second plate member) 42 First metal layer 42a First metal plate (first plate member) 50 Brazing material 60 Spacer (first pressing member and second pressing member) 61 Graphite Sheet 62 Carbon Sheet 63 Metal foil (first metal foil and second metal foil) 70 AlSiC composite 110 Pressurizing device
Claims
1. A method for producing a bonded body by heating a laminate of a first plate member and a second plate member while applying pressure thereto, comprising the steps of: the first plate member includes a first metal plate; a first pressing member having a first metal foil / carbon sheet or a ceramic sheet / graphite sheet laminated in this order is disposed on a surface of the first metal plate such that the first metal foil is in contact with the surface of the first metal plate; the first metal foil is made of a material that does not react when heated at a contact surface between the first plate member and the first metal foil; A method for producing a bonded body, wherein the product of Young's modulus (GPa) and thickness (mm) of the first metal foil is 0.6 or more and 100 or less.
2. a second pressing member having a second metal foil / carbon sheet or a ceramic sheet / graphite sheet laminated in this order is disposed so that the second metal foil is in contact with a surface of the second plate member; the second metal foil is made of a material that does not react when heated at a contact surface between the second plate member and the second metal foil, 2. The method for producing a joint body according to claim 1, wherein the product of Young's modulus (GPa) and thickness (mm) of the second metal foil is 0.6 or more and 100 or less.
3. 3. The method for manufacturing a joined body according to claim 1, wherein one of the first plate member and the second plate member is made of copper or a copper alloy, and the other is made of aluminum or an aluminum alloy.
4. A method for producing an insulating circuit board using the method for producing a bonded body according to any one of claims 1 to 3, comprising the steps of: The first plate member is a first metal plate made of copper or a copper alloy, the second plate member includes a ceramic substrate and a second metal plate made of aluminum or an aluminum alloy bonded to one surface of the ceramic substrate; A method for manufacturing an insulated circuit board, comprising stacking the first metal plate on the second metal plate joined to the ceramic substrate to form the laminate, and solid-state diffusion bonding the first metal plate and the second metal plate in a state in which the first metal foil is in contact with the first metal plate.
5. A method for producing an insulating circuit board using the method for producing a bonded body according to claim 2, comprising the steps of: The first plate member is formed by laminating a first metal plate made of copper or a copper alloy and an AlSiC composite material obtained by impregnating a porous body of silicon carbide with a metal mainly composed of aluminum, The second plate member includes a ceramic substrate, a second metal plate made of aluminum or an aluminum alloy bonded to both sides of the ceramic substrate, and the first metal plate laminated on one of the second metal plates, the other second metal plate of the second plate member is brought into contact with the first metal plate of the first plate member, thereby stacking the first plate member and the second plate member to form the laminate; A method for manufacturing an insulated circuit board, characterized in that the first metal plate and the second metal plate, and the first metal plate and the AlSiC composite are simultaneously solid-state diffusion bonded together while the first metal foil of the first pressing member is brought into contact with the AlSiC composite and the second metal foil of the second pressing member is brought into contact with a surface of the first metal plate of the second plate member.
Citation Information
Patent Citations
Substrate for semiconductor device, manufacturing method for the same and semiconductor device
JP2001135752A
Manufacturing apparatus and manufacturing method of substrate for power module with heatsink
JP2016063145A
Manufacturing method of substrate for power module with heat sink
JP2016072563A
Manufacturing method of conjugate, manufacturing method of insulation circuit board, and manufacturing method of insulation circuit board with heat sink
JP2018157116A
Method of manufacturing bonded body for insulating circuit board, and bonded body for insulating circuit board
WO2019188885A1