Method for treating steelmaking slag and method for predicting expansion ratio of steelmaking slag due to immersion in water

The method of extracting Ca components from steelmaking slag using a solvent and subsequent aging treatment addresses the instability issues of conventional treatments, enhancing stability and preventing expansion in roadbed materials and concrete applications.

JP7582361B2Active Publication Date: 2024-11-13JFE STEEL CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023025702
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-04-20
Filing Date
2023-02-22
Publication Date
2024-11-13
Estimated Expiration
2043-02-22

AI Technical Summary

Technical Problem

Conventional aging treatments for steelmaking slag, such as atmospheric and steam aging, are inadequate in stabilizing the slag and preventing expansion and pulverization due to hydration of free CaO, which can lead to issues in roadbed materials and concrete applications.

Method used

A method involving a contact treatment with a solvent, such as ethylene glycol, to extract Ca components from steelmaking slag, followed by an aging treatment if necessary, to stabilize the slag and predict the water immersion expansion ratio based on the extracted Ca amount.

Benefits of technology

The method effectively stabilizes steelmaking slag by suppressing expansion and pulverization, ensuring its suitability for roadbed materials and concrete applications by removing surface Ca components and predicting hydration risks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582361000003
    Figure 0007582361000003
  • Figure 0007582361000001
    Figure 0007582361000001
  • Figure 0007582361000002
    Figure 0007582361000002
Patent Text Reader

Abstract

To stabilize a steel slag by a treatment different from conventional aging treatments.SOLUTION: The Ca component of steel slag is extracted into a solvent by conducting a contact treatment in which the steel slag is brought into contact with the solvent. When at least one of the estimated f-CaO content and free CaO content in the steel slag exceeds a threshold value, it is preferable to further conduct an aging treatment on the steel slag that has already undergone the contact treatment.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for treating steelmaking slag and a method for predicting the water immersion expansion ratio of steelmaking slag. [Background technology]

[0002] Slag generated in converters, electric furnaces, torpedo cars, etc. (slag generated during the steelmaking process) is called steelmaking slag. In the steelmaking process, a large amount of lime is added to remove phosphorus, silicon, and other elements from the molten iron, and as a result, undissolved lime and lime that crystallizes during cooling remain in the steelmaking slag as free CaO (hereinafter also referred to as "f-CaO"). When f-CaO undergoes a hydration reaction, it becomes Ca(OH)2, expands in volume by approximately twice its size, and is then pulverized. As a result, there is concern that steelmaking slag may deviate from the specified particle size due to pulverization, or may expand after shipping. Applications of steelmaking slag include roadbed material and fine aggregate for concrete, etc. When f-CaO in the steelmaking slag used in these applications hydrates and expands, it can cause the roadbed to bulge and the concrete to crack.

[0003] Therefore, in the past, in order to prevent the steelmaking slag from expanding or powdering after shipment, the steelmaking slag was sometimes subjected to an aging treatment before shipment to stabilize it. Examples of aging treatments include air aging treatments in which steelmaking slag is stored for a long period of time in a slag yard or the like to cause a hydration reaction between the moisture in the air and f-CaO; and steam aging treatments in which water vapor is used to promote the hydration reaction (Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2009-227490 A Summary of the Invention [Problem to be solved by the invention]

[0005] In recent years, there has been a demand for the development of a process for stabilizing steelmaking slag that is different from the conventional aging process. The present invention has been made in consideration of the above points, and has an object to stabilize steelmaking slag by a treatment different from conventional aging treatments. [Means for solving the problem]

[0006] As a result of extensive investigations, the present inventors have found that the above object can be achieved by employing the following configuration, and have completed the present invention.

[0007] That is, the present invention provides the following [1] to [9]. [1] A method for treating steelmaking slag, comprising subjecting steelmaking slag to a contact treatment in which the steelmaking slag is brought into contact with a solvent, thereby extracting the Ca component of the steelmaking slag into the solvent. [2] A method for treating steelmaking slag as described in [1] above, wherein when at least one of the estimated f-CaO content and the free CaO content of the steelmaking slag exceeds a threshold value, the steelmaking slag that has been subjected to the contact treatment is further subjected to an aging treatment. [3] The method for treating steelmaking slag according to [2] above, wherein the aging treatment is carried out when the estimated f-CaO content of the steelmaking slag exceeds 12.0. [4] The method for treating steelmaking slag according to [2] or [3] above, wherein the aging treatment is carried out when the free CaO content of the steelmaking slag exceeds 8.0 mass%. [5] A method for treating steelmaking slag according to any one of [1] to [4] above, wherein the cooling rate of the steelmaking slag from a molten state to 1000°C is 50°C / h or more. [6] The method for treating steelmaking slag according to any one of [1] to [5] above, wherein the particle size of the steelmaking slag is 53 mm or less. [7] A method for treating steelmaking slag according to any one of [1] to [6] above, wherein the contact treatment is a treatment in which the steelmaking slag is contacted with ethylene glycol at 50°C or higher for 30 minutes or more. [8] A method for treating steelmaking slag described in any one of [2] to [4] above, comprising predicting a water immersion expansion ratio of the steelmaking slag based on the amount of the Ca component extracted into the solvent by the contact treatment, and determining conditions for the aging treatment based on the predicted water immersion expansion ratio. [9] A method for predicting the water immersion expansion ratio of a steelmaking slag, comprising: subjecting the steelmaking slag to a contact treatment in which the steelmaking slag is brought into contact with a solvent, thereby extracting the Ca component of the steelmaking slag into the solvent, and predicting the water immersion expansion ratio of the steelmaking slag based on the amount of the Ca component extracted into the solvent by the contact treatment. Effect of the Invention

[0008] According to the present invention, steelmaking slag can be stabilized by a treatment different from conventional aging treatments. [Brief description of the drawings]

[0009] [Figure 1] 1 is a graph showing the relationship between the amount of Ca extraction and the water immersion expansion ratio. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] [Method of processing steel slag] The method for treating steelmaking slag of the present invention involves subjecting the steelmaking slag to a contact treatment in which the steelmaking slag is brought into contact with a solvent, thereby extracting the Ca component of the steelmaking slag into the solvent. This stabilizes the steelmaking slag (hereinafter simply referred to as "slag"). In other words, the Ca components, including f-CaO, which undergoes a hydration reaction, are extracted into the solvent and removed, thereby suppressing the expansion and powdering of the slag.

[0011] Incidentally, the Ca component that is extracted and removed from the slag by the solvent is mainly the Ca component that is present on the slag surface (the surface where the slag comes into contact with the solvent). However, it is believed that the expansion of the slag progresses as water diffuses through the surface layer of the slag, causing the f-CaO on the slag surface to hydrate and expand, resulting in the repeated initiation and propagation of cracks and the hydration of f-CaO. Therefore, simply by removing the Ca component from the surface of the slag, the expansion of the slag can be substantially suppressed, and ultimately, pulverization can also be suppressed.

[0012] Contact Treatment The contact treatment is a treatment in which the steelmaking slag is brought into contact with a solvent. The method for bringing the slag into contact with the solvent is not particularly limited, and examples thereof include a method in which the slag is immersed in the solvent to bring them into contact with each other. At this time, it is preferable to stir the slag immersed in the solvent because this provides a better effect of the present invention (effect of stabilizing the steelmaking slag and suppressing expansion and powdering), although stirring is not essential.

[0013] The steelmaking slag and the solvent, as well as the conditions for contacting the two, will be described below.

[0014] Steel Slag The steelmaking slag to be subjected to the contact treatment is slag generated in the steelmaking process, and examples thereof include converter slag, electric furnace slag, and torpedo car slag. As described above, steelmaking slag contains free CaO (f-CaO) derived from lime added in the steelmaking process.

[0015] The steelmaking slag is preferably subjected to the contact treatment in its as-used state. The as-used state means a state (almost) the same as when actually used, such as a state where processing such as making the grain size uniform according to the application has been carried out.

[0016] The contact treatment can be performed on any steelmaking slag, but may be performed on a steelmaking slag that satisfies specific requirements by selecting the steelmaking slag. The steelmaking slag to be subjected to the contact treatment is selected, for example, as follows.

[0017] (Estimated amount of f-CaO) Before the contact treatment, the composition of the steelmaking slag is determined by elemental analysis using fluorescent X-rays, and the estimated f-CaO content defined by the following formula (1) is calculated. Estimated f-CaO amount = [T-CaO]-(1.87×[SiO2]+0.70×[Fe2O3]+1.10×[Al2O3]+1.18×[P2O5])...(1) Here, [X] in the above formula (1) is the content (unit: mass%) of component X in the steelmaking slag, and T-CaO is the total CaO.

[0018] When contact treatment is performed on slag with a large estimated amount of f-CaO, many voids are generated inside the slag due to the extraction of f-CaO. If steam aging treatment (described later) is further performed in this state, steam passes through these voids, which tends to promote the hydration reaction of the f-CaO present inside the slag. In other words, for slag with a high estimated f-CaO content, if only contact treatment is performed before shipping (without further steam aging treatment), the hydration reaction of the f-CaO present inside the slag may progress after shipping, causing it to expand or powder.

[0019] For this reason, the estimated f-CaO content of steelmaking slag that is subjected to only contact treatment is preferably 13.0 or less, more preferably 12.5 or less, and even more preferably 12.0 or less. If the estimated amount of f-CaO is within the above range, there are few voids inside the slag caused by the extraction of f-CaO. This makes it possible to suppress the hydration reaction (and the associated expansion and powdering) of f-CaO present inside the slag after shipment, even if only the contact treatment is performed before shipment (without further steam aging treatment).

[0020] (Free CaO content) Before the contact treatment, the free CaO content of the steelmaking slag may be directly determined in advance. For the same reasons as above, the free CaO content of steelmaking slag that is subjected to only contact treatment is preferably 10.0 mass % or less, more preferably 9.0 mass % or less, and even more preferably 8.0 mass % or less.

[0021] The free CaO content of steelmaking slag is determined using the ethylene glycol extraction method (slag: 0.1 g, ethylene glycol: 25 mL, extraction temperature: 80°C, extraction time: 30 minutes) in accordance with the method described in Reference 1 below. Reference 1: "Quantitative Determination of Free CaO in Steel Slag by Combined Use of Ethylene Glycol Extraction / ICP Atomic Emission Spectroscopy and Thermogravimetry", Iron and Steel, The Iron and Steel Institute of Japan, 2014, Vol. 100, No. 3, pp. 340-345

[0022] (Cooling rate from molten state to 1000℃) Consider the case where the cooling rate from the molten state to 1000°C (hereinafter simply referred to as the "cooling rate") is low for the slag that is subjected to the contact treatment. In this case, since the crystal size of f-CaO is large, a large amount of f-CaO remains on the slag surface after the contact treatment. In addition, since the crystal size of f-CaO is large, the pore size generated after the contact treatment is large. If a steam aging treatment (described later) is further performed in this state, the area of ​​the inside of the slag that comes into contact with steam increases, which tends to promote the hydration reaction of the f-CaO present inside the slag. In other words, for slag with a low cooling rate, if only contact treatment is performed before shipping (without steam aging treatment), the hydration reaction of f-CaO present inside the slag may progress after shipping, causing the slag to expand or powder.

[0023] For this reason, the cooling rate of the slag to be subjected to the contact treatment is preferably 50° C. / h or more, more preferably 75° C. / h or more, and even more preferably 100° C. / h or more. If the cooling rate is within the above range, the pore size generated after the contact treatment is small. This makes it possible to suppress the hydration reaction (and the associated expansion and powdering) of f-CaO present inside the slag after shipment, even if only the contact treatment is performed before shipment (without further steam aging treatment).

[0024] (particle size) For reasons of excellent handleability during the contact treatment, the particle size of the steelmaking slag to be subjected to the contact treatment is preferably 75 mm or less, more preferably 63 mm or less, and even more preferably 53 mm or less. On the other hand, the lower limit of the particle size of the steelmaking slag to be subjected to the contact treatment is not particularly limited from the viewpoint of handleability. However, when the steel slag is used as a roadbed material or fine aggregate for concrete, the particle size is, for example, 1 mm or more, and preferably 2 mm or more. The particle size is the size of the mesh when the slag is sieved and the mass of the slag that does not pass through the sieve (mass on the sieve) is 0 (zero).

[0025] "solvent" The solvent used in the contact treatment is not particularly limited as long as it is a solvent that can extract Ca components from steelmaking slag, and examples thereof include glycol-based solvents such as ethylene glycol; acidic solvents such as hydrochloric acid; and alkaline solvents such as an aqueous sodium hydroxide solution. Among these, glycol solvents are preferred, and ethylene glycol is more preferred, because they provide better effects for the present invention.

[0026] When ethylene glycol is used as the solvent, the amount of the solvent brought into contact with the slag is, for example, 1.5 L or more, preferably 1.8 L or more, and more preferably 2.0 L or more, per 1 kg of slag. The upper limit is not particularly limited, and is, for example, 3.5 L, preferably 3.0 L, per 1 kg of slag.

[0027] 《Contact temperature》 When ethylene glycol is used as the solvent, the temperature of the solvent brought into contact with the slag (contact temperature) is preferably 50°C or higher, more preferably 60°C or higher, even more preferably 70°C or higher, particularly preferably 85°C or higher, and most preferably 90°C or higher, because this provides better effects of the present invention. The upper limit of the contact temperature is not particularly limited, and is, for example, 100°C.

[0028] Contact Time When ethylene glycol is used as the solvent, the time for which the slag is in contact with the solvent (contact time) is preferably 30 minutes or more, more preferably 35 minutes or more, even more preferably 40 minutes or more, particularly preferably 45 minutes or more, and most preferably 50 minutes or more, because this provides a better effect of the present invention. The upper limit of the contact time is not particularly limited, and is, for example, 100 minutes, preferably 80 minutes.

[0029] When a solvent other than ethylene glycol is used, the contact conditions such as the contact temperature and contact time are appropriately adjusted depending on the solvent.

[0030] Aging Treatment The slag that has been subjected to the contact treatment may further be subjected to an aging treatment. As described above, the Ca components of the slag that are removed by the contact treatment are mainly the Ca components present on the slag surface (the surface where the slag comes into contact with the solvent). If the estimated f-CaO amount and / or free CaO content of the slag is low, even if only contact treatment is performed before shipment (without further steam aging treatment), the occurrence of hydration reaction of f-CaO present inside the slag (and the associated expansion and powdering) after shipment can be suppressed. On the other hand, when the estimated f-CaO content and / or free CaO content of the slag is high, if only contact treatment is performed before shipment (without further steam aging treatment), the hydration reaction of the f-CaO present inside the slag may progress after shipment, causing it to expand or powder. Therefore, when at least one of the estimated f-CaO amount and the free CaO content of the slag exceeds a threshold value, it is preferable to further subject the slag that has been subjected to the contact treatment to an aging treatment. Here, as described above, the threshold value of the estimated f-CaO content is preferably 13.0, more preferably 12.5, and even more preferably 12.0. Similarly, the threshold value of the free CaO content is preferably 10.0 mass%, more preferably 9.0 mass%, and even more preferably 8.0 mass%. This allows the small amount of f-CaO remaining on the surface of the slag after the contact treatment to undergo a hydration reaction, thereby making the effects of the present invention more excellent. The above thresholds are merely examples, and even if the estimated f-CaO amount and / or the free CaO content of the slag is equal to or less than the above thresholds, the slag that has been subjected to the contact treatment may be further subjected to an aging treatment. The aging treatment is preferably a steam aging treatment in which water vapor is used to promote the hydration reaction. The conditions of the steam aging treatment (temperature, pressure, treatment time, etc.) are not particularly limited and may be appropriately adjusted.

[0031] <Prediction of Water Immersion Expansion Ratio> As will be described below, the present inventors have found that there is a correlation between the amount of Ca component extracted from the slag into the solvent (Ca extraction amount) and the water immersion expansion ratio of the slag.

[0032] First, the inventors prepared 10 types of steelmaking slag (slags A to J) with different compositions in an as-used state. Next, the slags A to J were subjected to contact treatment under the same conditions (solvent: ethylene glycol, contact temperature: 70°C, contact time: 40 minutes) to determine the amount of Ca extracted (unit: mg / L). The amount of Ca extracted was determined by quantitative analysis using an ICP emission spectrometer. Furthermore, among slags A to J, slags A to J other than those that had been subjected to contact treatment were subjected to a water immersion expansion test specified in JIS A 5015 to determine the water immersion expansion ratio (unit: %).

[0033] FIG. 1 is a graph showing the relationship between the amount of Ca extraction and the water immersion expansion ratio. As shown in Figure 1, a proportional relationship is observed between the amount of extracted Ca and the water immersion expansion ratio. Specifically, in the graph in Figure 1, a linear approximation is observed: y = 0.0001x + 0.0143 (y: water immersion expansion ratio, x: amount of extracted Ca).

[0034] Therefore, in advance, in the same manner as described above, the amount of Ca extraction and the water immersion expansion ratio are determined for a plurality of types (for example, three or more types) of slags having different compositions under the same conditions, and a relational expression between the two is determined. Then, the target slag is subjected to contact treatment, and the water immersion expansion ratio is predicted based on the obtained amount of Ca extracted and using a previously determined relationship equation.

[0035] The conditions for the aging treatment may then be determined based on the predicted water immersion expansion ratio. For example, if the predicted water immersion expansion ratio is small, it may be possible to determine to shorten the processing time of the aging treatment.

[0036] The entity that executes the prediction of the water immersion expansion ratio and the determination of the conditions for the aging treatment is not particularly limited. For example, the prediction may be executed by an information processing device such as a personal computer in response to the operation of an operator who performs the contact treatment. EXAMPLES

[0037] The present invention will be specifically described below with reference to examples, although the present invention is not limited to the examples described below.

[0038] [Test 1] <Steel slag> Steelmaking slag (maximum particle size: 53 mm) shown in Table 1 below was prepared.

[0039] Contact Treatment The prepared steelmaking slag was immersed in ethylene glycol as a solvent and subjected to a contact treatment under the conditions (contact temperature and contact time) shown in Table 1 below. In the contact treatment, 2 L of solvent was used per 1 kg of steelmaking slag.

[0040] <Powdering rate> The slag was passed through a sieve with 2.36 mm mesh, and the mass of the slag that did not pass through the sieve (slag 1) was determined. Next, slag 1 was subjected to steam aging treatment (temperature: 100°C, pressure: atmospheric pressure, treatment time: 48 hours), and then passed through a sieve with 2.36 mm openings to determine the mass of the slag that passed through the sieve (slag 2). The mass ratio of slag 2 to slag 1 was calculated as the powdering rate (unit: mass %). Such a powdering rate was determined for both the steelmaking slag before the contact treatment and the steelmaking slag after the contact treatment. In Table 1 below, the dusting rate was recorded as "very low" when it was less than 1% by mass, "low" when it was 1% or more but less than 5% by mass, "medium" when it was 5% or more but less than 50% by mass, and "high" when it was 50% or more by mass.

[0041] [Table 1]

[0042] <Summary of evaluation results> As shown in Table 1 above, Examples 18 to 23, which did not satisfy the following (1a) or (2a), had a "high" powdering rate after the contact treatment. In contrast, in Examples 1 to 17, which satisfied the following (1a) and (2a), the powdering rate after the contact treatment was "very low," "low," or "medium." Examples 1 to 23 satisfy the following (3a) and (4a). (1a) The estimated f-CaO content of the slag is 13.0% or less, or the free CaO content of the slag is 10.0% or less by mass. (2a) The slag cooling rate is 50°C / h or more. (3a) The contact temperature is 50°C or higher. (4a) The contact time is 30 minutes or more.

[0043] Furthermore, looking at Examples 1 to 17, Examples 1 to 3 and 12 to 16, which did not satisfy any of the following (1b) to (4b), had a "medium" powdering rate after the contact treatment. In contrast, in Examples 4 to 11 and 17, which satisfied all of the following (1b) to (4b), the powdering rate after the contact treatment was "very low" or "low." (1b) The estimated f-CaO content of the slag is 12.0% or less, or the free CaO content of the slag is 8.0% or less by mass. (2b) The slag cooling rate is 100°C / h or more. (3b) The contact temperature is 60°C or higher. (4d) The contact time is 40 minutes or more.

[0044] Among Examples 4 to 11 and 17, Example 11, in which the contact temperature was 85°C or higher and the contact time was 40 minutes or longer, and Example 17, in which the contact temperature was 80°C or higher and the contact time was 45 minutes or longer, had an "extremely low" powdering rate after contact treatment.

[0045] [Test 2] <Prediction of Water Immersion Expansion Ratio> Next, the water immersion expansion ratio was predicted using the relational expression y=0.0001x+0.0143 (y: water immersion expansion ratio, x: Ca extraction amount) derived from the graph in FIG. 1 described above.

[0046] Specifically, first, multiple types of steelmaking slag were prepared. The prepared slag was subjected to contact treatment under the same conditions as when the above relational expression was obtained, and the amount of Ca extracted (unit: mg / L) was obtained. Next, based on the amount of Ca extracted obtained, the water immersion expansion ratio (unit: %) was predicted using the above relational expression. Hereinafter, this is also referred to as "water immersion expansion ratio (predicted)". The results are shown in Table 2 below.

[0047] Furthermore, the prepared slag was subjected to steam aging treatment until the actually measured water immersion expansion ratio (hereinafter also referred to as "water immersion expansion ratio (actual measurement)") became equal to or less than a certain value. At this time, in Examples 24 to 26, slags having similar but lower water immersion expansion ratios (predicted) were grouped together and subjected to steam aging treatment. On the other hand, in Examples 27 to 28, slags having different water immersion expansion ratios (predicted) were grouped together and subjected to steam aging treatment.

[0048] Further, in Table 2 below, the time difference from the processing time of the steam aging treatment carried out in actual operation (in Table 2 below, simply indicated as "time difference") is shown. In actual operation, the processing time of the steam aging treatment is set to be longer so that even slag containing a very large amount of f-CaO can be stabilized.

[0049] [Table 2]

[0050] <Summary of evaluation results> In Examples 24 to 26, slags with similar but lower water immersion expansion ratios (predicted) were grouped together and subjected to steam aging treatment. As a result, the "time difference" was -72 hours, and the time until the water immersion expansion ratio (actual measurement) fell below a certain value was shortened. On the other hand, in Examples 27 to 28, steam aging was performed according to the slag with a higher water immersion expansion ratio (predicted). Therefore, the "time difference" was 0 hours, and the time until the water immersion expansion ratio (actual measurement) reached a certain value or less could not be shortened.

Claims

1. The steelmaking slag is subjected to a contact treatment in which the steelmaking slag is brought into contact with a solvent, thereby extracting Ca components of the steelmaking slag into the solvent; The solvent is a glycol solvent, The cooling rate of the steelmaking slag from a molten state to 1000 ° C. is 50 ° C. / h or more, The estimated f-CaO content of the steelmaking slag is 13.0% or less, or the free CaO content of the steelmaking slag is 10.0% by mass or less; A method for treating steelmaking slag, wherein the contact treatment is a treatment in which the steelmaking slag is contacted with the solvent at 50°C or higher for 30 minutes or more.

2. The method for treating steelmaking slag according to claim 1, further comprising subjecting the steelmaking slag that has been subjected to the contact treatment to an aging treatment when at least one of the estimated f-CaO amount and the free CaO content of the steelmaking slag exceeds a threshold value.

3. The method for treating steelmaking slag according to claim 2, wherein the aging treatment is carried out when the estimated f-CaO content of the steelmaking slag exceeds 12.

0.

4. The method for treating steelmaking slag according to claim 2, wherein the aging treatment is carried out when the steelmaking slag has a free CaO content of more than 8.0 mass%.

5. A method for treating steelmaking slag according to any one of claims 1 to 4, wherein the particle size of the steelmaking slag is 53 mm or less.

6. The method for treating steelmaking slag according to any one of claims 1 to 4, wherein the glycol-based solvent is ethylene glycol.

7. A water immersion expansion ratio of the steelmaking slag is predicted based on the amount of the Ca component extracted into the solvent by the contact treatment; The method for treating steelmaking slag according to any one of claims 2 to 4, wherein conditions for the aging treatment are determined based on the predicted water immersion expansion ratio.

8. A method for predicting the water immersion expansion ratio of steelmaking slag, comprising the steps of: The method for treating steelmaking slag according to any one of claims 1 to 4, comprising the steps of: subjecting the steelmaking slag to a contact treatment in which the steelmaking slag is brought into contact with a solvent, thereby extracting the Ca component of the steelmaking slag into the solvent; A method for predicting the water immersion expansion ratio of a steelmaking slag, comprising predicting the water immersion expansion ratio of the steelmaking slag based on the amount of the Ca component extracted into the solvent by the contact treatment.

Citation Information

Patent Citations

  • Discrimination of steel slag expansivity

    JP1986117138A

  • Modification of converter slag

    JP1994256045A

  • Quantification method of solid solution component in free lime

    JP2007240302A

  • Method of treating slag

    JP2009227490A

  • Modified steel slag and manufacturing method

    JP2011213543A