Method for determining mechanochemical state and method for producing mechanochemical fly ash
By measuring electrical conductivity, the method addresses the inefficiencies of conventional methods for determining fly ash activation, allowing for quick and accurate assessment of mechanochemical state for cement-free concrete production.
Patent Information
- Application Number
- JP2020166800
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-01
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-10-01
AI Technical Summary
Conventional methods for determining the mechanochemical state of fly ash are time-consuming and labor-intensive, making it difficult to accurately assess whether fly ash has been activated for use in cement-free concrete production.
A method is developed to determine the mechanochemical state of fly ash by measuring the electrical conductivity (EC) of a suspension, providing a quicker and more efficient alternative to traditional methods such as X-ray diffraction and elution measurements.
This method allows for rapid and accurate determination of the mechanochemical state of fly ash, enabling efficient production without unnecessary prolongation of the treatment process.
Smart Images

Figure 0007582611000001 
Figure 0007582611000002 
Figure 0007582611000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for determining the mechanochemical state of a self-hardening material made from coal ash (fly ash). [Background technology]
[0002] As a conventional technique, a method for producing a self-hardening material using mechanochemically treated fly ash as a raw material has been proposed (Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 6347512 [Non-patent literature]
[0004] [Non-Patent Document 1] Geotechnical Society of Japan "Soil Testing Methods and Commentary" Revision Editorial Committee: Soil Testing Methods and Commentary (First Revised Edition), 2000 Summary of the Invention [Problem to be solved by the invention]
[0005] When mechanochemical treatment is performed using conventional techniques, it is difficult to determine whether the fly ash is in a mechanochemical state.
[0006] In view of the above problems, an object of the present invention is to provide a method for easily determining whether fly ash is in a mechanochemical state. [Means for solving the problem]
[0007] In order to solve the above problems, one aspect of the present invention provides a method for determining whether fly ash is in a mechanochemical state by measuring the electrical conductivity of a suspension of fly ash. Effect of the Invention
[0008] According to the present invention, a method for easily determining whether fly ash is in a mechanochemical state can be provided. [Brief description of the drawings]
[0009] [Figure 1] 1 shows the results of X-ray diffraction analysis of fly ash in Test 1. [Diagram 2] This is the particle size distribution of fly ash in Test 1. [Diagram 3] (a) Al and Si elution amounts in Test 1, and (b) a summary of the test results. [Figure 4] This is the particle size distribution of fly ash in Test 2. [Diagram 5] Chemical composition of fly ash in test 2. [Figure 6] (a) X-ray diffraction analysis results in Test 2, and (b) the relationship between grinding time and peak intensity. [Figure 7] 1 shows the relationship between the grinding time and the amorphous rate in Test 2. [Figure 8] 1 shows the results of grinding time, pH and EC measurements in Test 2. [Figure 9] (a) Measurement results of the grinding time and pH (30 minutes after mixing), and (b) measurement results of the grinding time and EC (30 minutes after mixing) in Test 2. [Figure 10] The relationship between the grinding time and the amount of dissolved Si and dissolved Al in Test 2. [Figure 11] 1 shows (a) the residual electrical conductivity, (b) the decrease rate of the residual electrical conductivity, and (c) a summary of the measured values in Test 2. [Figure 12] The EC residual rate and the reduction rate of the EC residual rate for ash types B to F. [Figure 13] Changes in the EC residual rate of ash types B to F over time. [Figure 14] This is the standard value for ending mechanochemical treatment for each ash type, taking into account a 10% likelihood. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] A method for determining the mechanochemical state of fly ash according to an embodiment of the present invention will be described below with reference to Figs.
[0011] <Summary> Mechanochemical treatment of coal ash (fly ash) is generally carried out by grinding the fly ash in a ball mill or the like. When the fly ash is subjected to the grinding treatment, the ash particles are pulverized, and a mechanochemical phenomenon occurs in which the surface is activated. When this ground ash is mixed with a highly alkaline silicon slurry, it hardens in a short time, so it can be used as cement-free concrete.
[0012] In the process of mechanochemical treatment, it is important in terms of process management and quality control to accurately determine whether the surface of the fly ash has reached an activated mechanochemical state, i.e., whether it has been mechanochemicalized.
[0013] Conventional methods for determining the mechanochemical transformation of fly ash include measuring the change in constituent minerals by X-ray diffraction and the amount of Al and Si dissolved in a highly alkaline solution, but all of these methods require time and effort.
[0014] Therefore, in the following, we propose an alternative method to the conventional one, which is to measure the electrical conductivity (EC) of fly ash.
[0015] <Test 1: Characteristics of mechanochemically treated fly ash> In order to understand the physical and chemical properties of the mechanochemically treated fly ash, a mechanochemical treatment using a ball mill (Test 1) was carried out as follows.
[0016] The mechanochemical treatment was carried out by grinding the fly ash. The fly ash used was ash type A. The grinding device used was a planetary ball mill (Fritsch, P-5).
[0017] The mechanochemical treatment was carried out by placing 500g of balls in a pot for 50g of fly ash and grinding the fly ash for 6 hours. Six types of treatment were carried out by changing the rotation speed of the planetary ball mill in increments of 50 rpm from 150 (rpm, revolutions per minute) to 400 rpm. In this way, in Test 1, the grinding time was kept constant and the rotation speed of the ball mill was changed, so the degree of mechanochemical treatment increased as the rotation speed increased.
[0018] X-ray diffraction analysis and particle size distribution measurements were performed on the ground fly ash and untreated fly ash (raw ash). In addition, the amount of Al and Si (aluminum and silicon) dissolved in alkaline solution, as well as the pH and EC of the ground ash were measured.
[0019] The results of the X-ray diffraction analysis are shown in Figure 1. Peaks of quartz and mullite were detected as crystalline minerals in the fly ash. At a rotation speed of 200 rpm, the quartz peak was smaller than that of the untreated sample, suggesting that the quartz crystal structure had been destroyed. As the rotation speed increased further, the mullite peak became smaller, suggesting that the mullite crystal structure had been destroyed.
[0020] Figure 2 shows the particle size distribution measurement results for raw ash and ground fly ash. A Microtrack-Bell MT3300 EXII particle size distribution analyzer was used for the measurements. Raw ash has a wide distribution shape, with a peak at a particle size of around 70 μm (micrometers). Grinding reduces the particle size, with a peak at a particle size of around 2 μm. Up to a rotation speed of 200 to 350 rpm, the average particle size became smaller with increasing rotation speed, but at 400 rpm the average particle size was larger than at 200 rpm, which is thought to be due to re-agglomeration of the particles.
[0021] When the milled ash comes into contact with a highly alkaline silicon slurry, Al and Si are dissolved from the ash, which then form a hardened body. In other words, it is important that Al and Si are dissolved from the ash in order to form a hardened body. The milled ash was mixed with an alkaline solution, and the concentration of the dissolved elements was measured using an ICP emission spectrometer. The measurement procedure is as follows: 1. Mix 0.2g powder + 20ml (milliliters) of 3M KOH solution 2. React in a shaking bath for 24 hours 3. Ultracentrifugation at 15,000 rpm for 20 minutes 4. Filter the supernatant through a 200 nm hydrophilic PTFE membrane filter. 5. Dilute 30 times with pure water 6. Measurement
[0022] The measurement results for Al and Si are shown in Figure 3(a). The amount of Al dissolved increased with grinding, but the amount dissolved was almost the same at rotation speeds of 150, 200, and 250 rpm. Above 300 rpm, the amount dissolved increased with increasing rotation speed. It is presumed that the amount of Al dissolved increased due to the destruction of the mullite crystal structure.
[0023] The amount of silicon dissolved also increased with grinding, and was almost the same at rotation speeds of 150, 200, and 250 rpm. Above 300 rpm, the amount of silicon dissolved increased with increasing rotation speed. When compared with the results of X-ray diffraction analysis, it was found that up to 250 rpm, the silicon was dissolved mainly from quartz (SiO2), and from 300 rpm, the silicon was dissolved mainly from mullite (Al6O 13 It is presumed to be elution from Si2).
[0024] The pH and EC were measured based on the Geotechnical Society standards "Test Method for pH of Soil Suspension" (JGS0211-2000) and "Test Method for Electrical Conductivity of Soil Suspension" (JGS0212-2000) (Non-Patent Document 1). Specifically, the sample (fly ash) and water were mixed and stirred at a mass ratio of 1:5, and the suspension was left to stand for 30 minutes before measurement. The measurement results after 30 minutes of standing are shown in Figure 3(b). Both the pH and EC decreased significantly from 1 hour to 3 hours after grinding, and then decreased gradually thereafter. The decrease in pH was due to the increase in hydroxide ions OH -A decrease in EC suggests a decrease in the amount of water-soluble ions, and a decrease in EC suggests a decrease in the amount of water-soluble ions, respectively.
[0025] The EC decreased as the rotation speed increased. Specifically, the EC decreased significantly up to 200 rpm, and a considerable decrease was also observed between 250 and 300 rpm. The decrease was not so great above 300 rpm.
[0026] As summarized in Figure 3(b), the boundary between rotation speeds of 250 and 300 rpm was set, and the following characteristics were apparent at rotation speeds above this threshold. The powder color turned black. The crystal peak of mullite has decreased significantly. The amount of Al and Si dissolved in highly alkaline solutions began to increase. -EC has significantly decreased
[0027] As shown in Figures 3(a) and (b), the amount of Al and Si dissolved increases at speeds of 300 rpm and above. In all test results at speeds of 300 rpm and above, it can be seen that the fly ash was mechanochemically converted.
[0028] It can also be seen that EC decreases as the amount of Al and Si dissolved increases as the fly ash becomes mechanochemical. Judging from the fact that the change point at which the amount of Al and Si dissolved from the fly ash starts to increase almost coincides with the change point of EC, it is thought that EC can be an indicator for determining whether the fly ash has become mechanochemical, i.e., whether it has reached a mechanochemical state.
[0029] <Test 2: Relationship between EC and mechanochemical reaction> In order to investigate the relationship between EC and the state of fly ash, particularly the relationship with treatment time, in more detail, the following test (Test 2) was conducted.
[0030] In this test, the rotation speed was kept constant and the grinding time was changed to investigate the relationship between the amount of Al and Si eluted and EC. Specifically, the coal ash used was ash type A, and a planetary ball mill (Fritsch, P-5) was used for the grinding process, with the rotation speed kept constant at 300 rpm. Five treatment times were used: 1, 3, 6, 12, and 24 hours (test names: MC-1h, MC-3h, MC-6h, MC-12h, MC-24h).
[0031] The raw ash was yellowish gray, but after one hour of grinding it darkened and turned blackish gray after three hours of further grinding.
[0032] The particle size distribution was measured using a laser diffraction particle size distribution analyzer (Microtrac MT3000II). The results are shown in Figure 4. The raw ash had a peak near a particle size of 40 μm, but after grinding, the particles were refined and a peak was observed at a particle size of 2 to 3 μm. In MC-3h, a peak also appeared near a particle size of 40 μm, and the particle size distribution began to show two peaks. In MC-24h, the peak near a particle size of 40 μm became larger, suggesting that the finely ground powder had aggregated.
[0033] The chemical composition of the raw ash and the ground fly ash was determined using a wavelength dispersive X-ray fluorescence analyzer (Shimadzu XRF-1800). Figure 5 shows the proportion of each element by grinding time. The chemical composition was approximately 61% silicon, approximately 22% aluminum, followed by 6% iron, 4% calcium, and approximately 1% titanium, potassium, and sodium. Magnesium was 1.15% for the raw ash, while it increased slightly to about 1.5% after 1 to 24 hours of grinding. The main chemical composition ratios of the raw ash and MC-1h to MC-24h were almost the same, with almost no change due to the grinding process.
[0034] The X-ray diffraction patterns of the raw ash and the milled ash are shown in Figure 6(a). An X-ray diffraction analyzer (Rigaku SmartLab) was used for the analysis. As shown in Figure 6(a), quartz and mullite were detected as crystalline minerals. It can be seen that the milling process reduced the peak intensity at all processing times (Figure 6(b)).
[0035] The proportion of amorphous matter was calculated based on the quantitative analysis results. The relationship between the grinding time and the proportion of amorphous matter is shown in Figure 7. The amorphous matter proportion of the raw ash was 69%, but increased to 77% for MC-3h, and then the amorphous matter proportion gradually increased.
[0036] The pH and EC were measured according to the Geotechnical Society's standards "pH test method for soil suspension" (JGS0211-2000) and "Electrical conductivity test method for soil suspension" (JGS0212-2000) (Non-Patent Document 1). Specifically, as in Test 1, the sample (fly ash) and water were mixed and stirred in a mass ratio of 1:5, and the suspension was left to stand for 30 minutes or 1 hour, after which the measurements were taken.
[0037] The measurement results of the suspension are shown in Figures 8 and 9. Both the pH and EC decreased significantly from 1 hour to 3 hours after grinding, and then decreased gradually thereafter. The decrease in pH was due to the increase in hydroxide ions (OH - A decrease in EC suggests a decrease in the amount of water-soluble ions, and a decrease in EC suggests a decrease in the amount of water-soluble ions, respectively.
[0038] The amount of eluted Si and Al was measured using the same procedure as in Test 1. As shown in Fig. 10, the amount of eluted Si increased rapidly after 1 hour of grinding (MC-1h), reached a maximum after 12 hours (MC-12h), and then slightly decreased after 24 hours (MC-24h).
[0039] The concentration of Al also increased rapidly after 1 hour of grinding (MC-1h), reached a maximum after 12 hours (MC-12h), and then decreased slightly after 24 hours (MC-24h). This trend was similar to that of Si.
[0040] The amount of eluted Si and Al increased rapidly in MC-1h. This is because, as shown by the X-ray diffraction analysis mentioned above, the elution amounts of quartz (SiO2) and mullite (Al6O 13 The peak of Si2) dropped sharply, which is presumably because the crystal structure of these materials collapsed and Si and Al became more easily eluted in the alkaline solution. The fact that the amount of elution of both Si and Al after 6 hours of grinding was slightly lower is thought to be related to the fact that the second peak after 6 hours in the particle size analysis mentioned above became slightly smaller.
[0041] The amounts of eluted Si and Al both increased significantly after 1 hour of grinding, reaching their peak after 3 hours. The tendency for peak strength to decrease also showed the same characteristics of mechanochemical fly ash as confirmed in Test 1. The color of the fly ash also turned dark gray after 3 hours. From this, it can be concluded that when using the Fritsch P-5 ball mill grinding device, ash type A reaches a mechanochemical state after 3 hours of processing at 300 rpm.
[0042] In response to the decrease in the amount of eluted Si and Al, EC decreased significantly after 1 hour of grinding, and converged to a constant value after 3 hours. It can be seen that EC decreases during the mechanochemical treatment process. In addition, when fly ash is mechanochemicalized, the rate of decrease in EC decreases, and EC converges to a constant value.
[0043] The time change in EC, the ratio to the EC of the raw ash (EC residual rate), and the rate of decrease in the EC residual rate per hour (decrease rate of the EC residual rate) are shown in Figure 11. In Figure 11(c), the decrease rate of the EC residual rate is shown as the rate of change over time from the previous measurement point to that point. As mentioned above, the decrease rate of the EC residual rate is very small after 3 hours, which indicates that the fly ash has become mechanochemical and the decrease in EC has almost converged after 3 hours of treatment.
[0044] As shown by the shaded area in Figure 11(c), the EC residual rate after 3 hours of grinding treatment, when the fly ash was in a mechanochemical state, was 8.8%. In addition, the rate of decrease in the EC residual rate after 1 to 3 hours of treatment was 5.13% / h (hour), whereas the rate of decrease in the EC residual rate after 3 to 6 hours of treatment dropped to 0.28% / h.
[0045] To summarize these results, it is possible to use the convergence of the EC residual rate below a certain level as the standard for determining whether fly ash has reached a mechanochemical state. Specifically, the EC residual rate at which the EC residual rate decrease rate converges can be used as the standard value used to determine whether mechanochemicalization has occurred or to terminate the mechanochemical treatment.
[0046] When using the results of Test 2, the rate of decrease in the EC residual rate from 3 to 6 hours of treatment converges to 2% / h or less, so it is possible to set the EC residual rate at 3 hours of treatment as the standard value. Since the EC residual rate at 3 hours of treatment is 8.8%, the standard value for the end of mechanochemical treatment will be an EC residual rate of 8.8%.
[0047] Considering that excessive mechanochemical treatment can have a negative effect, a certain degree of likelihood can be added to the above criteria. Using the results of Test 2, the EC residual rate after 3 hours of treatment is 8.8%, so adding a 10% likelihood to this EC residual rate of 8.8% to account for measurement errors, etc., it can be considered that the standard value for the end of treatment is an EC residual rate of 9.7%.
[0048] When such a standard value is used, when mechanochemical treatment is performed on fly ash of ash type A, the treatment should be terminated when the EC residual rate falls to 9.7% or less.
[0049] <Confirmation of condition settings> The physical and chemical properties of coal ash vary depending on the origin of the raw coal and the combustion method of the boiler. Therefore, the knowledge gained from the results of Test 2 was applied to different ash types, specific numerical values for the standard values were set, and their validity was confirmed.
[0050] In order to establish standards for judging mechanochemical conversion even when other ash types are used, a mechanochemical treatment similar to that in Test 2 (ball mill grinding treatment, 300 rpm) was carried out using fly ash other than ash type A, and the measurement results of EC, etc. were compared. Five types of fly ash were used: ash types B to F.
[0051] The test results are shown in Figures 12 and 13. In Figure 12, the rate of decrease in the EC residual rate when it became 2% / h or less is underlined, and the rate of decrease in the EC residual rate when it converged is shaded.
[0052] 12 and 13, it can be seen that for all ash types, as with ash type A, the EC residual rate decrease rate fell to 2% / h or less after 3 or 6 hours, and the EC residual rate converged. Referring particularly to Fig. 13, it can be seen that for all ash types, when the EC residual rate decrease rate fell to 2% / h or less, the graph bends significantly, and the electrical conductivity value and residual rate converge. The maximum EC residual rate at convergence was 28.9% (ash type F, 3 hours of treatment).
[0053] Considering the test results of ash type A in Tests 1 and 2 and the test results of ash types B to F, it can be seen that the standard value for judging mechanochemical formation can be set as "the EC residual rate when the reduction rate of the EC residual rate falls to a predetermined value or less." However, taking into account the test results of ash type F, it is preferable to set the upper limit of this standard value at 30%.
[0054] Based on the test results for ash type A and ash types B to F, the above-mentioned "predetermined value" for determining the rate of decrease in the EC residual rate can be set to 2% / h in a grinding process at 300 rpm using a ball mill.
[0055] This standard value may take the likelihood into consideration. Figure 14 shows the standard values that were set by obtaining the EC residual rate for each ash type when the rate of decrease in the EC residual rate falls to 2% / h or less, and then adding a likelihood of 10%.
[0056] As an example, consider a case where mechanochemical treatment is performed on fly ash of ash type B using the reference values in Figure 14. In this case, sampling is performed each time during the mechanochemical treatment process to measure the EC. When the EC residual rate falls to 16.2% or less, it is determined that the fly ash has been mechanochemically converted, and the mechanochemical treatment can be terminated.
[0057] By adopting such a method, there is no risk of extending the treatment time more than necessary, and therefore it is possible to efficiently mechanochemically convert fly ash.
[0058] <Effects> In the above embodiment, a method for determining whether the fly ash is in a mechanochemical state is used by measuring the electrical conductivity of a suspension of the fly ash.
[0059] By using the above method, it is possible to easily and quickly determine whether or not fly ash is in a mechanochemical state, compared to conventional methods such as measuring changes in constituent minerals by X-ray diffraction or the amount of Al and Si dissolved in a highly alkaline solution.
[0060] In the above embodiment, a method is used in which the fly ash is judged to be in a mechanochemical state when the residual rate of electrical conductivity is equal to or less than a reference value. This reference value is set as the residual rate of electrical conductivity when the reduction rate of the residual rate of electrical conductivity reaches a predetermined value or less in the process of carrying out mechanochemical treatment on the fly ash. This predetermined value is, for example, 2% / hour.
[0061] By using such a reference value, it becomes possible to accurately determine whether or not a mechanochemical state is present.
[0062] In the above embodiment, a method for producing mechanochemically converted fly ash is proposed, which includes a treatment step of performing mechanochemical treatment on fly ash and a determination step of determining whether the fly ash has reached a mechanochemical state, and the treatment step is terminated when it is determined in the determination step that the mechanochemical state has been reached.
[0063] By using such a method, it is possible to efficiently produce mechanochemical fly ash without extending the mechanochemical treatment time more than necessary.
Claims
1. The electrical conductivity of the fly ash suspension was measured. The method determines that the fly ash is in a mechanochemical state when the residual rate of the electrical conductivity is equal to or lower than a reference value.
2. The method according to claim 1 , wherein the reference value is set based on the remaining ratio when a rate of decrease in the remaining ratio becomes equal to or less than a predetermined value during the process of performing the mechanochemical treatment on the fly ash.
3. The method according to claim 1 or 2, wherein the reference value is 30% or less.
4. A treatment step of performing a mechanochemical treatment on the fly ash; and determining whether the fly ash has reached a mechanochemical state using the method according to any one of claims 1 to 3; A method for producing mechanochemical fly ash, the treatment step being terminated when it is determined in the determination step that a mechanochemical state has been reached.
Citation Information
Patent Citations
Tapping screw
JP1988047512A
Production of hydraulic powder
JP1999310442A
Treatment method for flying ash
JP2006281055A
Fly ash treatment method
JP2007245007A
Method of predicting activity index of fly ash for concrete
JP2012047587A