Bonded rare earth permanent magnet with high space filling ratio and manufacturing method thereof

The manufacturing method for bonded rare earth permanent magnets with reduced resin content and optimized processing enhances magnetic properties and resource utilization, addressing the performance gap with sintered magnets.

JP7582697B2Active Publication Date: 2024-11-13CHENGDU TO NAN ELECTRONICS
View PDF 20 Cites 0 Cited by

Patent Information

Application Number
JP2023026746
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-09-16
Filing Date
2023-02-22
Publication Date
2024-11-13
Estimated Expiration
2043-02-22

AI Technical Summary

Technical Problem

Bonded rare earth permanent magnets fail to meet the high performance requirements in applications due to lower magnetic properties and economic efficiency compared to sintered magnets, limiting their widespread use.

Method used

A manufacturing method for bonded rare earth permanent magnets with a high space filling rate, utilizing reduced thermosetting resin content, a coupling agent, and a lubricant, along with specific processing conditions, to enhance magnetization effects and structural strength.

Benefits of technology

The method results in bonded magnets with improved magnetic properties and resource utilization, achieving higher density and performance comparable to sintered magnets, thus overcoming the limitations of conventional bonded magnets.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582697000001
    Figure 0007582697000001
  • Figure 0007582697000002
    Figure 0007582697000002
  • Figure 0007582697000003
    Figure 0007582697000003
Patent Text Reader

Abstract

To provide a bond rare earth permanent magnet having a high space packing rate, and a manufacturing method of the same.SOLUTION: A manufacturing method of a rare earth permanent magnet containing a thermosetting resin, a lubricant, a coupling agent and rare earth permanent magnet powder as raw materials includes: mixing rare earth permanent magnet powder, a thermosetting resin, and a solution where a coupling agent is dissolved, stirring the mixture in a sealed state and then drying the mixture, and obtaining a magnet powder complex after crushing; mixing the magnet powder complex and the lubricant, and putting the mixture in a mold, compressing and molding the mixture at predetermined compressive force for holding time of 0.3 to 10 seconds, keeping the compressed powder obtained after mold release at 120-200°C and obtaining a preliminary molding; and fine-machining the preliminary molding. A bond rare earth permanent magnet effectively shortens a fine powder distance in a bong magnet, effectively increases a magnetization effect of fine powder and interaction force after magnetization, greatly improves performance of a compressed and molded bond rare earth permanent magnet, which effectively improves a utilization factor of the rare earth permanent magnet powder.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the technical field of permanent magnets, in particular to a bonded rare earth permanent magnet with high space-filling factor and its manufacturing method. [Background technology]

[0002] In recent years, rare earth permanent magnets such as praseodymium / neodymium iron boron and its lanthanum cerium substitutes, samarium cobalt, etc. have been widely used due to their extremely strong magnetic properties and relative stability. With the demand for high power density and high stability in the electric motor field, from aerospace to wind power generation, home electronic devices, precision machine tools to new energy vehicles, rare earth permanent magnets such as neodymium iron boron and its lanthanum cerium substitutes, samarium cobalt, etc. are being used in an increasingly wide range of fields as magnetic energy components.

[0003] Since their appearance in the 1970s, the manufacturing technology of rare earth permanent magnets has developed rapidly, and according to the technology, they can be divided into sintered rare earth permanent magnets and bonded rare earth permanent magnets, among which those that use organic materials such as resin, plastic, and rubber as the complex-forming medium (also called binder) for rare earth permanent magnet powder are collectively called bonded rare earth permanent magnets (hereinafter referred to as bonded magnets). Since bonded magnets first appeared in Japan in the 1980s, they have been successively derived into compression molded bonded magnets (generally applied to resin composite magnets), injection molded bonded magnets (generally using thermoplastic resins such as nylon, polyformaldehyde, and polyphenylene sulfide as the complex-forming medium), and rolled bonded magnets (generally using modified rubber as the complex-forming medium) according to the binding medium and technology. Since the compression molding is performed using an organic medium complex, high-temperature sintering, deformation due to high temperatures, and post-processing do not occur, so the primary molded products have high dimensional accuracy and are suitable for mass production. This has led to rapid development since mass production began in the 1990s, and with the rapid development of information technology in the late 1990s, bonded rare earth permanent magnets have been widely used in fields such as computer memory drives, computer peripherals, precise vehicle control, and vehicle comfort layout.

[0004] Although bonded rare earth permanent magnets have achieved large-scale mass production, the growth rate of demand has slowed since global usage reached 6,000 tons in 2010, and compared with the global scale of sintered rare earth permanent magnets, bonded rare earth permanent magnets have yet to become the mainstream of permanent magnet materials. At present, the current inventory market size of sintered rare earth permanent magnets globally is more than 200,000 tons per year, while the usage of bonded rare earth permanent magnets is only 10,000 tons per year, gradually deteriorating from less than one-tenth of the sintered market in 2010 to less than one-twentieth of the sintered rare earth permanent magnets in 2021.

[0005] The rapid and steady growth in shipments of sintered praseodymium / neodymium iron boron magnets in recent years explains the rapid increase in application demand for rare earth permanent magnets, which are characterized by their high performance and high power density. Meanwhile, bonded rare earth permanent magnets cannot fully meet this demand. Taking the most commonly used neodymium iron boron magnet as an example, we have developed the highest performance isotropic compression molded bonded neodymium iron boron magnet BH for mass production. max The measured value of BH is about 12 MGOe at the highest, and the best performance for mass production is achieved under the alignment conditions of anisotropic compression molded HDDR magnets. max The highest measured value for bonded NdFeB magnets is around 20 MGOe, whereas the highest performance sintered NdFeB magnets for mass production can reach around 52 MGOe after orientation under good crystallization conditions. Due to the huge difference in magnetic properties, bonded NdFeB magnets cannot meet the high performance requirements of applications.

[0006] In addition, in terms of material utilization and cost, a sintered neodymium iron boron magnet containing 21% neodymium was compared with a compression-molded bonded praseodymium and / or neodymium iron boron magnet with the same neodymium content prepared by the liquid quenching method, and the sintered neodymium iron boron magnet BH was compared under non-orientation conditions. maxThe measured value of bonded rare earth permanent magnets can reach about 24 MGOe, while that of bonded magnets can only reach about 9 MGOe. As a result, in terms of performance applications, the actual cost performance of bonded rare earth permanent magnets is much lower than that of sintered magnets with the same rare earth content. In other words, the difference in the actual utilization rate of rare earth has become a bottleneck restricting the expansion of applications of bonded rare earth permanent magnets, which well explains the difficulties the development of bonded rare earth permanent magnets has faced in recent years. Summary of the Invention [Means for solving the problem]

[0007] SUMMARY OF THE DISCLOSURE In order to solve the above technical problems, the present invention provides a bonded rare earth permanent magnet having a high space filling factor and a manufacturing method thereof.

[0008] The present invention is realized by the following technical means: First, the present invention provides a method for producing a bonded rare earth permanent magnet with a high space filling factor, the raw material of the rare earth permanent magnet contains the following components in mass percentage: 0.1-1.6 wt% thermosetting resin, 0.05-0.8 wt% lubricant, 0-1.0 wt% coupling agent, and the remainder being rare earth permanent magnet powder. The method of manufacturing includes: The crystallized rare earth permanent magnet powder is mixed with a solution in which the thermosetting resin and the coupling agent are dissolved, and the mixture is stirred in a sealed state, dried, and pulverized to obtain a magnet powder complex; mixing the magnet powder complex with the lubricant to obtain clinker; The clinker is placed in a mold at a temperature of 40 to 120°C, preheated, and compressed into a mold. After demolding, a pressed powder is obtained. The pressed powder is kept at 120 to 200°C for 2 to 3 hours to obtain a preform, which is then precision processed.

[0009] Furthermore, the rare earth permanent magnet powder includes at least one of quenched praseodymium and / or neodymium iron boron magnet powder and modified powder containing dysprosium / terbium / cobalt / aluminum, quenched lanthanum iron boron powder, quenched cerium iron boron powder, HDDR permanent magnet powder, samarium cobalt permanent magnet powder, ferrite permanent magnet powder, samarium iron nitrogen permanent magnet powder, and Fe3B-based permanent magnet powder containing Nd.

[0010] Furthermore, in a preferred embodiment of the present invention, the coupling agent comprises one or a mixture of two of a silane and / or a titanate.

[0011] Furthermore, in a preferred embodiment of the present invention, the lubricant comprises graphite and / or stearate; Preferably, the stearate comprises zinc stearate and / or calcium stearate.

[0012] Furthermore, in a preferred embodiment of the present invention, the crystallization treatment is carried out in a high-purity argon atmosphere at 670 to 730° C. for 10 to 20 minutes.

[0013] Furthermore, in a preferred embodiment of the present invention, the rare earth permanent magnet powder has a particle size of 60 to 200 mesh.

[0014] Furthermore, in a preferred embodiment of the present invention, in the step of producing the magnet powder complex, the time for stirring in a sealed state is 40 to 60 minutes.

[0015] Furthermore, in a preferred embodiment of the present invention, the density of the compacted powder is 6.2 to 7.1 g / cm 3 It is.

[0016] Furthermore, in a preferred embodiment of the present invention, the compression force during the compression molding is 12-50 T / cm 2 and the pressure retention time is 0.3 to 10 s.

[0017] Furthermore, in a preferred embodiment of the present invention, the step of heating the pressed powder to obtain a preform in order to further increase the density of the preform comprises: The compressed powder is heated to the softening point of the epoxy, and then evacuated to a vacuum so that the atmospheric pressure in the environment is less than 0.2 atm, and the temperature is kept at 120 to 200° C. for 2 to 3 hours.

[0018] In a further preferred embodiment of the present invention, the method further comprises the step of forming a protective coating on the surface of the preform after precision machining, The protective coating is produced by at least one of the following: application of anti-rust oil, electrophoresis, application of epoxy resin, zinc plating, nickel plating, chrome plating, plastic spraying, and polyparaxylene.

[0019] Secondly, the present invention provides a bonded rare earth permanent magnet having a high space filling factor produced by the above-mentioned production method, and the density of the rare earth permanent magnet is 6.2 to 7.0 g / cm. 3 and Preferably, the rare earth permanent magnet further comprises a protective coating, and the protective coating comprises at least one of anti-rust oil coating, electrophoresis, epoxy resin coating, zinc plating, nickel plating, chrome plating, plastic spraying, and polyparaxylene. Effect of the Invention

[0020] Compared with the existing technology, the present invention has the following technical advantages: Firstly, the present invention uses a compression molding method for manufacturing, and the compression molded bonded rare earth permanent magnet obtained thereby has a high utilization rate of rare earth permanent magnet powder and is likely to exhibit high magnetic properties externally, which further improves the economic efficiency and resource utilization rate of the compression molded bonded rare earth permanent magnet compared to the prior art.

[0021] Secondly, the bonded rare earth permanent magnet provided in the present application has a large inter-domain interaction force, which allows the entire permanent magnet to exhibit high external performance.

[0022] Thirdly, for the compression molded bonded permanent magnets in the bonded magnets, it is usually necessary to ensure that the mass percentage of the thermosetting resin (hereinafter referred to as resin) which is the complexing medium is 1.8-4.0wt% in order to guarantee the necessary structural strength and smooth demolding of the bonded permanent magnets, otherwise the product cannot be molded, and the presence of the resin will greatly limit the further compression of the fine powder distance in the microscopic structure of the bonded permanent magnets. Take the currently most commonly used W-6C epoxy resin as an example, the density of the resin is 1.1g / cm 2 Since the beginning of this century, the density of mass-produced compression molded bonded neodymium iron boron magnets has been stable at 5.6-6.1, which is a large distance from the product density of 7.2 or more of sintered magnets and bonded magnets, and the magnetization effect of the microscopic rare earth magnet powder in the finished magnet and the interaction force after magnetization are greatly reduced, so that the bonded magnet is difficult to achieve high performance compared to sintered magnets with a packed structure. However, the bonded rare earth permanent magnet provided by the present application reduces the volume ratio of the resin binder in the compression molded bonded magnet (about 1-10%), effectively shortening the fine powder distance in the bonded magnet and effectively increasing the magnetization effect of the fine powder and the interaction force after magnetization.

[0023] Hereinafter, the implementation means of the present invention will be described in detail in relation to the embodiments, but the scope of the present invention is not limited thereto. The following embodiments are only used to explain the present invention, and specific conditions not described in the embodiments are carried out according to normal conditions or conditions suggested by the manufacturer, and those skilled in the art will understand that the reagents or equipment used are normal products that can be purchased commercially by those who do not specify the manufacturers.

[0024] The technical means of the specific embodiments of the present invention are as follows: In this embodiment, a method for producing a bonded rare earth permanent magnet having a high space filling rate is provided, and the raw material of the rare earth permanent magnet contains the following components in mass percentage: 0.2-1.6 wt% thermosetting resin, 0.05-0.8 wt% lubricant, 0-1.0 wt% coupling agent, and the balance being rare earth permanent magnet powder. Generally, in the prior art, 1.8-4.0wt% of binder is used, but the density of the resin binder is very low compared to the magnet powder, so the high mass percentage of the resin material results in a high resin volume ratio, which affects the magnetization effect and magnetic properties of the magnet powder particles. In order to ensure the structural strength of the final product, the bonded rare earth permanent magnet provided in the present application significantly reduces the amount of thermosetting resin used as the binder, thereby significantly reducing the volume ratio of thermosetting resin in the rare earth permanent magnet, thereby greatly enhancing the interaction between the magnet powder particles, and further achieving the purpose of strengthening the magnetization effect and magnetic performance of the product. At the same time, the frictional heating of the contact points between the particles is used at the preset temperature of the mold and under extremely high pressure conditions during the molding process, and the chemical activity properties of the resin epoxy group are used to bring it to a microscopic state and create a curing condition to generate a curing crosslink to form a network structure, thereby achieving the purpose of basically maintaining the structural strength of the product preform under the condition of low binder usage.

[0025] In order to improve the friction between particles and between the particles and the mold wall during the compression process of magnet powder complex particles under microscopic conditions, we properly add lubricants suitable for powder compression in the preparation process of clinker, which is also favorable for the smooth release of the compressed powder.

[0026] In addition, in order to further improve the binding strength between the thermosetting resin and the magnet powder surface, a coupling agent containing silane and / or titanate can be added according to the type of resin. From the viewpoint of performance, it is preferable to use titanate as a coupling agent, which is easy to form a uniformly applied binder layer on the surface of the magnet powder fine particles, and further optimizes the performance of the product. From the viewpoint of strength, it is preferable to use a silane coupling agent, which contributes to cost reduction, and silane forms an S-shaped staggered structure on the surface of the magnet powder fine particles, which is favorable to increasing the structural strength of the product.

[0027] More preferably, the thermosetting resin and coupling agent used in the preferred embodiment of the present invention are commercially available W-6C / W-6D bonded rare earth permanent magnet epoxy resin (containing coupling agent) products, in which the ratio of thermosetting resin to coupling agent is about 3:1. Since the required ratio of coupling agent varies greatly depending on the type of thermosetting resin, it is necessary to select the type according to the specific application type and determine the optimal ratio.

[0028] Furthermore, the lubricant includes graphite or stearate. Graphite micropowder lubricant is used, and graphite micropowder is a commonly used lubricant, and its conductive properties can effectively improve the problem of poor conductivity during subsequent electrophoretic surface treatment due to the increase in interparticle resistance caused by resin encapsulation. When stearate is used as lubricant, since it is the same organic compound, the stearate lubricant has better binding force on the surface of the magnet powder complex, and the subsequent structural strength of the product is better. Preferably, the stearate includes zinc stearate and calcium stearate.

[0029] Preferably, the composition contains the following components in mass percentages: 0.2-1.6 wt% thermosetting resin, 0.05-0.8 wt% lubricant, 0-1.0 wt% coupling agent, and the remainder rare earth permanent magnet powder. Within these ranges, the mass percentages of the resin and lubricant can be appropriately adjusted based on the structural and application characteristics of the product.

[0030] Furthermore, the rare earth permanent magnet powder includes at least one of quenched praseodymium / neodymium iron boron magnet powder, neodymium iron boron magnet powder containing dysprosium, quenched lanthanum (cerium) iron boron powder, HDDR permanent magnet powder, samarium cobalt permanent magnet powder, ferrite permanent magnet powder, samarium iron nitrogen permanent magnet powder, and Fe3B-based permanent magnet powder containing Nd.

[0031] Preferably, in order to improve the coercive force of the magnet, when the magnet powder is selected as quenched praseodymium and / or neodymium iron boron magnet powder, it is preferable to adopt magnet powder containing Dy / Tb-PrNd-Fe-B, Dy / Tb-Hx phases; similarly, when the magnet powder is selected as quenched praseodymium and / or neodymium iron boron magnet powder, modified powder containing one or two of Co / Al-PrNd-Fe-B is preferentially selected to improve the heat resistance of the magnet.

[0032] It should be explained that the quenched praseodymium and / or neodymium iron boron magnet powder is a quenched praseodymium and / or neodymium iron boron magnet powder product with the basic phase structure of R2Fe14B, and the experiment in this application is assumed to adopt the commercial quenched praseodymium and / or neodymium iron boron magnet powder or equivalent magnet powder manufactured by Magnequench, USA, which is collectively called MQP permanent magnet powder in the industry. That is, the quenched permanent magnet powder includes ordinary quenched praseodymium and / or neodymium iron boron magnet powder, quenched lanthanum / cerium iron boron powder, and quenched praseodymium and / or neodymium iron boron magnet powder including Dy / Tb-PrNd-Fe-B, Dy / Tb-Hx, Co / Al-PrNd-Fe-B, HDDR permanent magnet powder is the general name for neodymium iron boron magnet powder with anisotropic characteristics produced by hydrogen destruction method in the industry.

[0033] The method for producing the bonded rare earth permanent magnet having a high space-filling factor includes the following steps: In step S1, the crystallized rare earth permanent magnet powder is mixed with a solution in which the thermosetting resin and the coupling agent are organically dissolved, and the mixture is stirred in a sealed state, dried, and then pulverized to obtain a magnet powder complex.

[0034] Furthermore, the crystallization conditions are 670-730°C for 10-20 minutes (preferably 690-710°C for 13-18 minutes) in an argon atmosphere. The crystallized rare earth permanent magnet powder is crushed to a particle size of 80-120 mesh (preferably 100 mesh).

[0035] Preferably, the crystallization step includes crushing the alloy strip after strip casting under an argon positive pressure environment, placing the resulting coarse material in a crystallization furnace, evacuating the furnace, crystallizing the material at 670-730°C for 10-20 minutes under an argon positive pressure of 0.3, cooling the material, and crushing it to 80-120 mesh in an argon atmosphere to produce a powder.

[0036] More preferably, before the crystallization step, the alloy strip after melting is placed in a strip casting apparatus after low-temperature drying, and then the apparatus is evacuated and filled with argon to a positive pressure of 0.1-0.5, and strip casting is started at a wheel speed of 20-23 meters per second.

[0037] In addition, in this step, step S1 may be carried out by directly using a commercially available powder such as the commercialized neodymium iron boron magnet powder of MQP1-7.

[0038] Furthermore, in the organic solution in which the thermosetting resin is dissolved, the solvent is an organic solvent such as acetone, chloroform, ethyl acetate, etc., and preferably, the solvent is acetone.

[0039] Furthermore, the stirring time in a sealed state is 40 to 60 minutes, preferably 45 to 55 minutes. The purpose of stirring in a sealed state is to prevent the organic solvent from volatilizing too quickly during stirring and to ensure sufficient infiltration of the thermosetting resin solution and the magnet powder particles.

[0040] Preferably, the process for producing the magnet powder complex comprises: 0.1~1.6wt% of commercial thermosetting resin (e.g. W-6C or W-6D epoxy resin) is dissolved in acetone, and then crystallized rare earth permanent magnet powder is mixed in. The mixture is stirred for 40~60min in a sealed state to mix uniformly, and then spread out and dried for 12~36h until the acetone dries. The mixture is then pulverized to 80~120 mesh using a wheel-type Banbury mixer, and sieved.

[0041] Step S2: mixing the magnet powder complex with a lubricant to obtain clinker;

[0042] In step S3, the clinker is placed in a mold having a temperature of 40 to 120°C, preheated, and compressed. After demolding, a pressed powder is obtained. The pressed powder is kept at 120 to 200°C for 2 to 3 hours to obtain a preform, which is then precision processed.

[0043] The temperature of the mold is preheated to 40-120°C (preferably 60-100°C) mainly because the thermosetting resin has a softening point. If the temperature is higher than the softening point, the resin wrapped around the outside of the rare earth permanent magnet powder particles will soften, and the fluidity and filling property of the magnet powder will further increase. For example, the softening point of W-6C or W-6D resin material is 60°C (the temperature range selected here is an empirical value). Similarly, if the set temperature is higher than 120°C, the resin will liquefy, causing adhesion to the mold, making it difficult to release. Here, the corresponding temperature range should be adjusted according to the type of binder selected.

[0044] Furthermore, during the compression molding process, the unit compression force is 12-50T / cm 2 The pressure retention time is 0.3 to 10 s.

[0045] Furthermore, the density of the pressed powder is 6.2 to 7.1 g / cm 3 , preferably 6.4 to 7.0 g / cm 3Depending on the unit compression force and the preheating temperature of the mold, the pressed powder will have different density states. In theory, the higher the density, the better. However, if the density is too high, it will be difficult to release from the mold. Therefore, the density of the pressed powder is set to 6.2-7.1g / cm3. 3 was controlled.

[0046] Furthermore, in the process of heating the pressed powder to obtain a preform, the pressed powder is heated to the softening point of the epoxy, then evacuated to make the atmospheric pressure in the environment less than 0.2 atm (or directly baked in a vacuum oven), and then kept at 120 to 200°C for 2 to 3 hours to harden.

[0047] Specifically, in step S3, the clinker is compressed, molded, and released to produce a magnet of the desired geometric shape, which is divided into three steps: compression stage, pressure holding stage, and demolding stage. Here, the compression stage is The process in which the clinker is compressed from a loose state into a desired geometric shape in the cavity is called the compression stage. The magnet powder particles have extremely high hardness and irregular shapes, and form a loose state body of clinker after the clinker fills the cavity. During the upper and lower die compression process of the die, as the loose state clinker is constantly compressed, the frictional forces between the magnet powder particles and between the clinker and the cavity wall are constantly increasing. The frictional force on the compression surface close to the cavity wall and the downward pressure of the upper die constitute a shear force. According to Bernoulli's theorem, the surface density value of the compressed preform close to the cavity wall is higher than that of the inside of the compressed preform. This results in a compressive stress from the outside to the inside of the compressed preform, and most of the required compressive force is used to overcome the mutual friction force of the magnet powder particles and the friction force of the friction surface with the mold during mold compression and demolding, until the maximum value of the upper and lower mold pressure setting is reached and balanced, the upper and lower molds stop compression, at this time the friction force within the magnet powder is equal to the upper and lower mold pressure, after holding pressure for the required time, the clinker powder is compressed in the space formed by the mold master, the upper and lower molds and the core mold to form a compressed preform constituting a magnet part, and the next mold demolding stage needs to be completed in order to obtain the required molded preform of the magnet part.

[0048] In this process, the unit pressure of the upper and lower molds during the magnet molding process is 17.0 to 50.0 tons / cm 2 That is, the working pressure was 1.7GPa~5.0GPa. Depending on the size of the powder particles, there is a large difference in the energy consumed to compress the clinker from a loose state to the required density in the cavity. Taking the general rule as an example, for 100 mesh clinker, the experimental data shows that when the compression pressure is higher than 1.7GPa, the density of the preformed body of the product is 6.40 or more, and when the compression pressure value is higher than 3.0GPa, the density value is 6.8 or more.

[0049] Step S4: After the preform is precisely machined, a protective coating is formed on the surface, and the protective coating is formed by at least one of epoxy coating, anti-rust oil coating, electrophoresis, epoxy resin coating, zinc plating, nickel plating, chrome plating, plastic spraying, and polyparaxylene.

[0050] In addition, when the rare earth permanent magnet powder is samarium cobalt permanent magnet powder and ferrite permanent magnet powder, the material itself is not easily corroded, so there is no need to manufacture a protective coating. When using other permanent magnet powders, such as quenched neodymium iron boron magnet powder, quenched neodymium iron boron magnet powder containing dysprosium / terbium / cobalt / aluminum, quenched lanthanum iron boron powder, quenched cerium iron boron powder, HDDR permanent magnet powder, samarium iron nitrogen permanent magnet powder, Fe3B system permanent magnet powder containing Nd, etc., it is necessary to manufacture a protective coating on the surface of the obtained permanent magnet to prevent the surface of the permanent magnet from corroding.

[0051] Hereinafter, specific embodiments of the present invention will be described in detail. It should be understood that the specific embodiments described herein are only used for the purpose of illustrating and explaining the present invention, and are not used to limit the present invention.

[0052] (Embodiment 1) The present embodiment provides a bonded rare earth permanent magnet with high space-filling factor, the manufacturing method of which includes: (1) Producing powder: Commercially available MQP1-7 quenched neodymium iron boron magnet powder is used to produce rare earth permanent magnet powder.

[0053] (2) To produce clinker, 1.2wt% W-6C epoxy resin is dissolved in acetone, and then the crystallized rare earth permanent magnet powder is mixed in. The mixture is stirred for 50min in a sealed state to mix evenly, and then the mixture is spread out and dried for 24h until the acetone dries. The mixture is crushed to 100 mesh size using a wheel-type Banbury mixer, and sieved to obtain a magnet powder complex. The magnet powder complex is mixed with 0.15wt% zinc stearate to obtain clinker.

[0054] (3) Compress the product. Preheat the mold to 60°C through the oil guide groove built into the mold, fill the above-mentioned clinker, adjust the preheating time of the clinker according to the size of the product, and after the clinker is fully preheated, the unit compression force is 25T / cm 2 After 5s of pressure retention and demolding, the density is 6.5g / cm 3 The pressed powder is then kept at 160°C for 2.5 hours to harden it to its final strength, resulting in a preform.

[0055] (4) Post-processing of products: After the product preform is produced, further machining methods such as grinding or wire cutting are used to obtain a precision preform of the final product according to the customer's drawing requirements. The product precision preform is then painted (painted, electrophoretic, etc.) to produce a work-in-progress, and finally a magnetizing device is used to produce a finished magnetic part that meets the customer's needs.

[0056] (Embodiment 2) The present embodiment provides a bonded rare earth permanent magnet with high space-filling factor, the manufacturing method of which includes: (1) Producing powder: Commercially available MQP1-7 quenched neodymium iron boron magnet powder is used to produce rare earth permanent magnet powder.

[0057] (2) To produce clinker, 0.5wt% of W-6D epoxy resin (containing coupling agent) is dissolved in acetone, and then the crystallized rare earth permanent magnet powder is mixed in. The mixture is stirred for 40min in a sealed state to mix evenly, and then the mixture is spread out and dried for 36h until the acetone dries. The mixture is crushed to 120 mesh size using a wheel-type Banbury mixer, and sieved to obtain a magnet powder complex. The magnet powder complex is mixed with 0.2wt% of calcium stearate to obtain a clinker.

[0058] (3) Compress the product. Preheat the mold to 120°C through the oil guide groove built into the mold, fill the above-mentioned clinker, adjust the preheating time of the clinker according to the size of the product, and after the clinker is fully preheated, the unit compression force is 40T / cm 2 After 0.3s of pressure retention and demolding, the density was 6.2g / cm 3 The pressed powder can be produced by heating it to 120℃ in a vacuum oven and keeping it at that temperature for 3 hours, so that the product can be cured and crosslinked in a near vacuum environment, and the density and performance of the product preform can be further improved.

[0059] (4) Post-processing of products: After the product preform is produced, further machining methods such as grinding or wire cutting are used to obtain a precision preform of the final product according to the customer's drawing requirements. The product precision preform is then painted (painted, electrophoretic, etc.) to produce a work-in-progress, and finally a magnetizing device is used to produce a finished magnetic part that meets the customer's needs.

[0060] (Embodiment 3) The present embodiment provides a bonded rare earth permanent magnet with high space-filling factor, the manufacturing method of which includes: (1) Producing powder: Commercially available MQP1-7 quenched neodymium iron boron magnet powder is used to produce rare earth permanent magnet powder.

[0061] (2) To produce clinker, 1.65wt% W-6C epoxy resin (including coupling agent) is dissolved in acetone, and then the crystallized rare earth permanent magnet powder is mixed in. The mixture is mixed uniformly in a sealed mixer for 60 minutes, and then the mixture is spread out and dried for 12 hours until the acetone dries. The mixture is crushed to 80 mesh size by a wheel-type Banbury mixer, and sieved to obtain a magnet powder complex. The magnet powder complex is mixed with 0.05wt% calcium stearate to obtain a clinker.

[0062] (3) Compress the product. Preheat the mold to 40℃ through the oil guide groove built into the mold, fill the above-mentioned clinker, adjust the preheating time of the clinker according to the size of the product, and after the clinker is fully preheated, the unit compression force is 12T / cm 2 After 10.0s of pressure retention and demolding, the density was 6.8g / cm 3 The pressed powder can be placed in an oven and heated to the softening point of the epoxy resin, then the pressure in the oven is reduced to below 0.2 atm, and the product is then heated to 200°C and kept at that temperature for 2 hours, allowing the product to be cured and crosslinked in an almost vacuum environment, further improving the density and performance of the product preform.

[0063] (4) Post-processing of products: After the product preform is produced, further machining methods such as grinding or wire cutting are used to obtain a precision preform of the final product according to the customer's drawing requirements. The product precision preform is then painted (painted, electrophoretic, etc.) to produce a work-in-progress, and finally a magnetizing device is used to produce a finished magnetic part that meets the customer's needs.

[0064] In order to demonstrate that the rare earth permanent magnets provided in the present application have high density and magnetic properties, the following comparative experiments were carried out. All of the following experiments were carried out after preparing the commercial powder MQP1-7 as the raw material powder.

[0065] (Experimental Example 1) The effect of thermosetting resin content on the performance of rare earth permanent magnets is as follows: Based on the content of thermosetting resin (using W-6C epoxy resin) listed in Table 1, the manufacturing method provided in the first embodiment is used to manufacture rare earth permanent magnets, and the density and BH performance of the manufactured products are detected. Br (residual magnetism), Hcb (coercive force), Hcj (intrinsic coercive force), BH max (including maximum energy product). The results are shown in Table 1. (Table 1) Effect of thermosetting resin content on rare earth permanent magnet performance

[0066] [Table 1]

[0067] (Experimental Example 2) The effect of lubricant content on the performance of rare earth permanent magnets is as follows: Based on the content of lubricant (zinc stearate) listed in Table 2, the manufacturing method provided in embodiment 1 is used to manufacture rare earth permanent magnets, and the density and BH performance of the manufactured products are detected. Br (residual magnetism), Hcb (coercive force), Hcj (intrinsic coercive force), BH max (including maximum energy product). The results are shown in Table 2. (Table 2) Effect of lubricant content on the performance of rare earth permanent magnets

[0068] [Table 2]

[0069] (Experimental Example 3) The effect of unit compression pressure on the performance of rare earth permanent magnets is as follows: The manufacturing method provided in embodiment 1 is used to compress the clinker according to the unit compression pressure listed in Table 3 to manufacture rare earth permanent magnets, and the density and BH performance of the manufactured product are detected, and the Br (residual magnetism), Hcb (coercive force), Hcj (intrinsic coercive force), BH max (including maximum energy product). The results are shown in Table 3. (Table 3) Effect of unit compression pressure on the performance of rare earth permanent magnets

[0070] [Table 3]

[0071] (Experimental Example 4) The effect of compression temperature on the performance of rare earth permanent magnets is as follows: The manufacturing method provided in embodiment 1 is used to compress the clinker according to the compression temperature listed in Table 4 to manufacture a rare earth permanent magnet, and the density and BH performance of the manufactured product are detected, and the Br (residual magnetism), Hcb (coercive force), Hcj (intrinsic coercive force), BH max (including maximum energy product). The results are shown in Table 4. (Table 4) Effect of compression temperature on the performance of rare earth permanent magnets

[0072] [Table 4]

[0073] Finally, it is to be understood that the above is merely a preferred embodiment of the present invention, and is not used to limit the scope of protection of the present invention. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principle of the present invention should be included in the scope of protection of the present invention.

Claims

1. Density: 6.2 to 7.0 g / cm 3 A method for producing a bonded rare earth permanent magnet, The raw material of the rare earth permanent magnet contains the following components in mass percentage: 0.1 to 1.6 wt% thermosetting resin, 0.05 to 0.8 wt% lubricant, 0.1 to 1 wt% coupling agent, and the remainder is rare earth permanent magnet powder. The density is 6.2 to 7.0 g / cm 3 The method for producing a bonded rare earth permanent magnet is as follows: The crystallized rare earth permanent magnet powder is mixed with the solution in which the thermosetting resin and the coupling agent are dissolved, and the mixture is stirred in a sealed state, dried for 12 to 36 hours, and then pulverized to 80 to 120 mesh using a wheel-type Banbury mixer to obtain a magnet powder complex. mixing the magnet powder complex with the lubricant to obtain a clinker; The clinker is placed in a mold preheated to a temperature of 40 to 120 ° C., the clinker is preheated to 40 to 120 ° C., and then compression molded. After demolding, a pressed powder is obtained. The pressed powder is kept at 120 to 200 ° C. for 1 to 3 hours, and then cured and crosslinked to obtain a preform, which is then precision processed. Here, the density of the preform is 6.2 to 7.1 g / cm 3 and In the compression molding process, the compression force is 26 to 50 T / cm 2 , pressure holding time is 0.3 to 10 seconds, The conditions for the crystallization treatment of the rare earth permanent magnet powder are as follows: after strip casting, the alloy strip is roughly crushed under a positive argon pressure environment, the material obtained is placed in a crystallization furnace, and further crystallized in an argon atmosphere at 670 to 730°C for 10 to 20 minutes.

2. The rare earth permanent magnet powder has a density of 6.2 to 7.0 g / cm according to claim 1, characterized in that it contains at least one of the following: quenched praseodymium and / or neodymium iron boron magnet powder, modified powder containing any one of four elements: dysprosium, terbium, cobalt, and aluminum, quenched lanthanum iron boron powder, quenched cerium iron boron powder, HDDR permanent magnet powder, samarium cobalt permanent magnet powder, samarium iron nitrogen permanent magnet powder, and Fe3B-based permanent magnet powder containing Nd. 3 A method for producing a bonded rare earth permanent magnet.

3. The lubricant comprises graphite and / or stearates and salt-based compounds; The stearate salt comprises zinc stearate and / or calcium stearate. 3 A method for producing a bonded rare earth permanent magnet.

4. The grain size of the crystallized rare earth permanent magnet powder is 60-200 mesh. The density is 6.2-7.0 g / cm 3 A method for producing a bonded rare earth permanent magnet.

5. The density of the magnet powder complex according to claim 1 is 6.2 to 7.0 g / cm3, wherein the time for stirring in a sealed state is 40 to 60 min in the process for producing the magnet powder complex. 3 A method for producing a bonded rare earth permanent magnet.

6. The step of heating the compressed powder to obtain a preform includes the following steps: 3 A method for producing a bonded rare earth permanent magnet. The compressed powder is heated to the softening point of the epoxy, and then the pressure in the environment is reduced to less than 0.2 atm by vacuuming, and the temperature is kept at 120-200°C for 2-3 hours.

7. The density of the preform is 6.2 to 7.0 g / cm3 according to claim 1, further comprising a step of forming a protective coating on the surface after precision machining of the preform. 3 A method for producing a bonded rare earth permanent magnet. The protective coating is produced by at least one of the following: application of anti-rust oil, electrophoresis, application of epoxy resin, zinc plating, nickel plating, chrome plating, plastic spraying, and polyparaxylylene.

Citation Information

Patent Citations

  • Method for preparing powder for bound rare-earth permanent-magnet by quasi-compression method

    CN101145418A

  • Neodymium-iron-boron bonded magnet, preparation method thereof and motor

    CN114420397A

  • Ferromagnetic resin composite

    JP1987264602A

  • Rare-earth-iron based resin-bonded magnet

    JP1989245502A

  • Resin bond magnet

    JP1991074810A