Welding control method, welding control device, welding power source, welding system, program, welding method, and additive manufacturing method

The welding control method addresses the challenge of achieving stable penetration depth and reducing spatter by alternating wire feeding and controlling current in arc welding, enhancing welding quality and efficiency.

JP7582923B2Active Publication Date: 2024-11-13KOBE STEEL LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021152554
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-09-17
Publication Date
2024-11-13
Estimated Expiration
2041-09-17

AI Technical Summary

Technical Problem

Existing arc welding methods struggle to achieve stable penetration depth and reduce spatter, particularly in thick plates and galvanized steel sheets, due to the use of high current densities that lead to increased spatter and decreased welding workability.

Method used

A welding control method that alternately repeats forward and reverse feeding of the welding wire, controlling the welding current based on the tip position and feeding speed, with specific ratios and frequencies to maintain a stable penetration depth and reduce spatter.

Benefits of technology

The method achieves both stable penetration depth and reduced spatter by balancing the welding current and wire feeding, ensuring consistent arc length and droplet detachment, thereby improving welding quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582923000003
    Figure 0007582923000003
  • Figure 0007582923000004
    Figure 0007582923000004
  • Figure 0007582923000005
    Figure 0007582923000005
Patent Text Reader

Abstract

To achieve both a stable penetration depth and reduction in a sputter, in an arc welding method for periodically repeating forward feeding and reverse feeding of a tip of a wire.SOLUTION: A frequency f in a period combining a forward feeding period TP and a reverse feeding period TN is set at 50-150 Hz, a relation between an average current IP-AVE of a current non-suppression period TIP and an average current IB-AVE of a current suppression period TIB is 0.65≤IP-AVE / (IP-AVE+IB-AVE)≤0.90, a wave height Wh of a change width at the tip position of a weld wire is 14-35% a distance between a chip and a base material, a relation between the current non-suppression period TIP and the current suppression period TIB just after the current non-suppression period is 0.30≤TIB / (TIP+TIB)≤0.60, and it is controlled so that a relation between the forward feeding period TP and the reverse feeding period TN is restricted, a relation among the current non-suppression period TIP, the current suppression period TIB is restricted, the forward feeding period TP and the reverse feeding period TN is restricted, and the current non-suppression period TIP occupies a period of 2 / 3 or more the forward feeding period TP.SELECTED DRAWING: Figure 9A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a welding control method, a welding control device, a welding power source, a welding system, a program, a welding method, and an additive manufacturing method in an arc welding method in which forward and reverse feeding of a welding wire is alternately and cyclically repeated. [Background technology]

[0002] In the welding of thick plates, which is mainly used in industries such as steel frames and construction machinery, it is required to ensure a certain penetration depth. In addition, in the welding of galvanized steel plates, which is used in industries such as automobiles, it is required to prevent porosity defects. Such securing of penetration depth and prevention of porosity defects can be achieved by increasing the thermal energy of the arc. For this reason, gas-shielded metal arc welding (GMAW) has been used in the past, which incorporates measures such as increasing the current density of the arc by using a shielding gas with a high potential gradient, such as carbon dioxide gas, or increasing the welding current itself. However, the application of a shielding gas with a high potential gradient and the application of a high welding current increase spatter, and the deterioration of welding workability mainly caused by spatter has been a problem.

[0003] In response to the above problem, Patent Document 1 has an objective of suppressing the generation of spatter even when a large current is passed through a welding wire (hereinafter also referred to as "wire"), which is a consumable electrode, when arc welding is performed by periodically repeating alternating forward and reverse feed.The patent document discloses that when the tip of the wire is fed toward the base metal while periodically switching between periods of forward feed and periods of reverse feed, by using a control means that changes the welding current in accordance with the periodically changing tip position of the wire, it is possible to reduce spatter even in a high current range where efficient welding is possible with high heat input, i.e., a current range where a transfer form other than short-circuit transfer occurs. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2020-49506 A Summary of the Invention [Problem to be solved by the invention]

[0005] As described above, Patent Document 1 discloses a method for reducing spatters in a high current range where efficient welding can be achieved with high heat input, but does not specifically mention penetration depth. In other words, Patent Document 1 does not mention anything about the effect of ensuring a stable penetration depth or preventing porosity defects. In Patent Document 1, in an arc welding method in which forward feed and reverse feed are cyclically repeated, control is performed to prevent short circuits, unlike conventional short circuit transfer methods, but depending on differences in processing conditions such as work conditions and welding position, or disturbances during welding, a short circuit may occur during welding control or the timing of droplet detachment may be shifted, which may result in a failure to obtain a stable penetration depth or an increase in the amount of spatter. For this reason, there is a demand for more precise welding control that can achieve both a stable penetration depth and a spatter reduction effect regardless of the welding environment.

[0006] The present invention has been made in consideration of the above-mentioned problems, and its object is to provide a welding control method, a welding control device, a welding power source, a welding system, a program, a welding method, and an additive manufacturing method that are capable of achieving both a stable penetration depth and a reduction in spatter in an arc welding method in which the welding wire is fed alternately and cyclically between forward and reverse feed. [Means for solving the problem]

[0007] Therefore, the above object of the present invention is achieved by the following configuration [1] relating to a welding control method.

[0008] [1] In gas metal arc welding, the welding current is supplied to the welding wire. A forward feed period T during which the tip of the welding wire moves from the uppermost end, which is the position farthest from the base metal, to the lowermost end, which is the position closest to the base metal. P and a reverse feed period T N While controlling the feed speed of the welding wire so that the welding wire is fed toward the base metal with periodic switching of Based on at least a tip position signal of the welding wire or a feed speed signal of the welding wire, The welding current is kept in a current non-suppression period T IP or current suppression period T IB A welding control method for switching and controlling a welding The positive feeding period T P and the reverse feed period T N The combined period is considered as one cycle, and its frequency f is 50 to 150 Hz. The current non-suppression period T IP The average current I P-AVE and the current suppression period T IB The average current I B-AVE The relationship is 0.65≦I P-AVE / (I P-AVE +I B-AVE )≦0.90, A wave height Wh, which is a change width of the tip position of the welding wire between the uppermost end and the lowermost end, is set to 14 to 35% of a tip-base metal distance of the welding wire, Any of the current non-suppression periods T IP and the current suppression period T immediately thereafter. IB The relationship between these two is 0.30≦T IB / (T IP +T IB )≦0.60, The positive feeding period T P and the reverse feed period T N The relationship is 0.40≦T N / (T P +T N )≦0.70, and, The current non-suppression period T IP , the current suppression period T IB , the positive feeding period T Pand the reverse feed period T N The relationship between N / (T P +T N )}>{T IB / (T IP +T IB )} and The positive feeding period T P The period of 2 / 3 or more of the current non-suppression period T IP A welding control method comprising the steps of:

[0009] The above object of the present invention can be achieved by the following configuration [2] relating to a welding control device.

[0010] [2] In gas metal arc welding, in which welding current is supplied to a welding wire, A forward feed period T during which the tip of the welding wire moves from the uppermost end, which is the position farthest from the base metal, to the lowermost end, which is the position closest to the base metal. P and a reverse feed period T N While controlling the feed speed of the welding wire so that the welding wire is fed toward the base metal with periodic switching of Based on at least a tip position signal of the welding wire or a feed speed signal of the welding wire, The welding current is kept in a current non-suppression period T IP or current suppression period T IB A welding control device for switching and controlling The positive feeding period T P and the reverse feed period T N The combined period is considered as one cycle, and its frequency f is 50 to 150 Hz. The current non-suppression period T IP The average current I P-AVE and the current suppression period T IB The average current I B-AVE The relationship is 0.65≦I P-AVE / (I P-AVE +I B-AVE )≦0.90, A wave height Wh, which is a change width of the tip position of the welding wire between the uppermost end and the lowermost end, is set to 14 to 35% of a tip-base metal distance of the welding wire, Any of the current non-suppression periods T IP and the current suppression period T immediately thereafter. IB The relationship between these two is 0.30≦T IB / (T IP +T IB )≦0.60, The positive feeding period T P and the reverse feed period T N The relationship is 0.40≦T N / (T P +T N )≦0.70, and, The current non-suppression period T IP , the current suppression period T IB , the positive feeding period T P and the reverse feed period T N The relationship between N / (T P +T N )}>{T IB / (T IP +T IB )} and The positive feeding period T P The period of 2 / 3 or more of the current non-suppression period T IP A welding control device having a function of controlling the welding time so that the welding speed is within the predetermined range.

[0011] The above object of the present invention can be achieved by the following configuration [3] relating to a welding power source.

[0012] [3] A welding power source comprising the welding control device described in [2].

[0013] The above object of the present invention can be achieved by the following configuration [4] relating to a welding system.

[0014] [4] A welding system comprising the welding control device described in [2] or the welding power source described in [3].

[0015] The above object of the present invention can be achieved by the following configuration [5] relating to a program.

[0016] [5] In gas metal arc welding, in which welding current is supplied to a welding wire, A forward feed period T during which the tip of the welding wire moves from the uppermost end, which is the position farthest from the base metal, to the lowermost end, which is the position closest to the base metal. P and a reverse feed period T N While controlling the feed speed of the welding wire so that the welding wire is fed toward the base metal with periodic switching of Based on at least a tip position signal of the welding wire or a feed speed signal of the welding wire, The welding current is kept in a current non-suppression period T IP or current suppression period T IB A computer of a welding system including at least a welding control device for switching between and controlling the welding The welding control device, The positive feeding period T P and the reverse feed period T N The combined period is considered as one cycle, and its frequency f is 50 to 150 Hz. The current non-suppression period T IP The average current I P-AVE and the current suppression period T IB The average current I B-AVE The relationship is 0.65≦I P-AVE / (I P-AVE +I B-AVE )≦0.90, A wave height Wh, which is a change width of the tip position of the welding wire between the uppermost end and the lowermost end, is set to 14 to 35% of a tip-base metal distance of the welding wire, Any of the current non-suppression periods T IP and the current suppression period T immediately thereafter. IB The relationship between these two is 0.30≦T IB / (T IP +T IB )≦0.60, The positive feeding period T P and the reverse feed period TN The relationship is 0.40≦T N / (T P +T N )≦0.70, and, The current non-suppression period T IP , the current suppression period T IB , the positive feeding period T P and the reverse feed period T N The relationship between N / (T P +T N )}>{T IB / (T IP +T IB )} and The positive feeding period T P The period of 2 / 3 or more of the current non-suppression period T IP A program characterized by executing a function of controlling the number of

[0017] The above object of the present invention can be achieved by the welding method described below in [6].

[0018] [6] In gas metal arc welding, in which welding current is supplied to a welding wire, A forward feed period T during which the tip of the welding wire moves from the uppermost end, which is the position farthest from the base metal, to the lowermost end, which is the position closest to the base metal. P and a reverse feed period T N While controlling the feed speed of the welding wire so that the welding wire is fed toward the base metal with periodic switching of Based on at least a tip position signal of the welding wire or a feed speed signal of the welding wire, The welding current is kept in a current non-suppression period T IP or current suppression period T IB A welding method for performing gas metal arc welding while performing welding control by switching to and controlling the welding The positive feeding period T P and the reverse feed period T N The combined period is considered as one cycle, and its frequency f is 50 to 150 Hz. The current non-suppression period T IP The average current I P-AVE and the current suppression period T IB The average current I B-AVE The relationship is 0.65≦I P-AVE / (I P-AVE +I B-AVE )≦0.90, A wave height Wh, which is a change width of the tip position of the welding wire between the uppermost end and the lowermost end, is set to 14 to 35% of a tip-base metal distance of the welding wire, Any of the current non-suppression periods T IP and the current suppression period T immediately thereafter. IB The relationship between these two is 0.30≦T IB / (T IP +T IB )≦0.60, The positive feeding period T P and the reverse feed period T N The relationship is 0.40≦T N / (T P +T N )≦0.70, and, The current non-suppression period T IP , the current suppression period T IB , the positive feeding period T P and the reverse feed period T N The relationship between N / (T P +T N )}>{T IB / (T IP +T IB )} and The positive feeding period T P The period of 2 / 3 or more of the current non-suppression period T IP The welding method is characterized in that the welding control is performed so that the welding current is within the range of 0.5 to 100 .mu.m.

[0019] In addition, the above object of the present invention is achieved by the following configuration [7] relating to an additive manufacturing method.

[0020] [7] In additive manufacturing, gas metal arc welding is used to supply welding current to a welding wire. A forward feed period T during which the tip of the welding wire moves from the uppermost end, which is the position farthest from the base metal, to the lowermost end, which is the position closest to the base metal. P and a reverse feed period T N While controlling the feed speed of the welding wire so that the welding wire is fed toward the base metal with periodic switching of Based on at least a tip position signal of the welding wire or a feed speed signal of the welding wire, The welding current is kept in a current non-suppression period T IP or current suppression period T IB An additive manufacturing method for performing additive manufacturing while performing welding control by switching to and controlling the welding, The positive feeding period T P and the reverse feed period T N The combined period is considered as one cycle, and its frequency f is 50 to 150 Hz. The current non-suppression period T IP The average current I P-AVE and the current suppression period T IB The average current I B-AVE The relationship is 0.65≦I P-AVE / (I P-AVE +I B-AVE )≦0.90, A wave height Wh, which is a change width of the tip position of the welding wire between the uppermost end and the lowermost end, is set to 14 to 35% of a tip-base metal distance of the welding wire, Any of the current non-suppression periods T IP and the current suppression period T immediately thereafter. IB The relationship between these two is 0.30≦T IB / (T IP +T IB )≦0.60, The positive feeding period T P and the reverse feed period T N The relationship is 0.40≦T N / (T P +T N )≦0.70, and, The current non-suppression period T IP , the current suppression period T IB, the positive feeding period T P and the reverse feed period T N The relationship between N / (T P +T N )}>{T IB / (T IP +T IB )} and The positive feeding period T P The period of 2 / 3 or more of the current non-suppression period T IP The additive manufacturing method is characterized in that the welding control is performed so that the welding area is occupied by the welding area. Effect of the Invention

[0021] According to the welding control method, welding control device, welding power source, welding system, program, welding method, and additive manufacturing method of the present invention, it is possible to achieve both a stable penetration depth and reduced spatter in an arc welding method in which the welding wire is fed alternately and cyclically between forward and reverse feed. [Brief description of the drawings]

[0022] [Figure 1] FIG. 1 is a schematic diagram showing an example of the configuration of a welding system according to this embodiment. [Diagram 2] FIG. 2 is a block diagram showing a schematic configuration of a power supply control unit in the welding power supply. [Diagram 3] FIG. 3 is a waveform diagram illustrating the change over time of the wire feed speed FW. [Figure 4] FIG. 4 is a waveform diagram illustrating the change over time in the tip position of the welding wire. [Diagram 5] FIG. 5 is a flowchart illustrating an example of basic control of a welding current in this embodiment. [Figure 6] FIG. 6 is a diagram showing an example of control of the current setting signal Ir that specifies the current value of the welding current. [Figure 7] FIG. 7 is a series of photographs taken by a high-speed camera showing an example of the progress of welding in a conventional short-circuit transfer method, and is a drawing-substitute photograph taken at various times for Test No. 24, which is a reference example described later. [Figure 8] FIG. 8 is a series of photographs taken by a high-speed camera showing an example of the progress of welding in this embodiment, and is a drawing-substitute photograph taken at each elapsed time for Test No. 8, which is an example described later. [Figure 9A] FIG. 9A is a diagram showing the relationship between the wire feed speed FW, the wire tip position, and the welding current set value, for illustrating the setting of the end position of the welding current set value IP1 and the end position of the welding current set value IP2. [Figure 9B] FIG. 9B is a diagram showing the relationship between the wire feed speed FW, the wire tip position, and the welding current set value, for explaining the setting of the end position of the current suppression period TIB. [Figure 10] FIG. 10 is a diagram showing the relationship between the number of short circuits and the penetration depth. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, embodiments of a welding control method, a welding control device, a welding power source, a welding system, a program, a welding method, and an additive manufacturing method according to the present invention will be described in detail with reference to the drawings.

[0024] It should be noted that this embodiment is an example of a case where a welding robot is used, and the welding control method according to the present invention is not limited to the configuration of this embodiment. For example, the welding control method of the present invention may be applied to an automatic welding device using a cart, or to a portable small welding robot. In addition, this embodiment uses a gas metal arc welding method using a pulse waveform. Furthermore, in this embodiment, a gas metal arc welding method to which the welding control method according to the present invention is applied is described, but the welding control method according to the present invention can also be similarly applied to an additive manufacturing method that applies gas metal arc welding.

[0025] In addition, the method for measuring welding behavior according to the present invention is useful not only for welding but also for additive manufacturing technology using GMAW, specifically, for metal additive manufacturing (WAAM: Wire and Arc Additive Manufacturing). The term additive manufacturing may be used broadly as the term additive manufacturing or rapid prototyping, but in the present invention, the term additive manufacturing is used uniformly. When the method according to the present invention is used for additive manufacturing technology, "welding" can be rephrased as "deposition," "additive manufacturing," or "additive manufacturing." For example, when treated as welding, it becomes "welding behavior," but when the present invention is used as additive manufacturing, it can be rephrased as "deposition behavior," or when treated as welding, it becomes "welding system," but when the present invention is used as additive manufacturing, it can be rephrased as "additive manufacturing system."

[0026] <Welding system overview> 1 is a schematic diagram showing an example of the configuration of a welding system according to this embodiment. Welding system 50 includes welding robot 110, welding control device 120, a feeding device (not shown) that feeds welding wire 100, welding power source 140, and controller 150.

[0027] Welding power source 140 is connected to welding robot 110 via a positive power cable (not shown) so as to pass current through welding wire 100, which is a consumable electrode, and is connected to workpiece (hereinafter also referred to as "base material") 200 via a negative power cable (not shown). This connection is for the case where welding is performed with reverse polarity; when welding is performed with positive polarity, the polarity of welding power source 140 can be reversed.

[0028] Furthermore, welding power source 140 and a feeder for feeding welding wire 100 are connected by a signal line, so that the feed speed of the welding wire can be controlled.

[0029] The welding robot 110 is equipped with a welding torch 111 as an end effector. The welding torch 111 has an energization mechanism, i.e., a welding tip, that energizes the welding wire 100. An arc is generated from the tip of the welding wire 100 when energized from the welding tip, and the generated heat welds the workpiece 200 that is the object of welding. The welding tip is also generally referred to as a contact tip.

[0030] Furthermore, the welding torch 111 includes a shielding gas nozzle that serves as a mechanism for ejecting the shielding gas. The shielding gas may have a gas composition that takes the form of globule transition due to the characteristics of the control used in this embodiment, and specifically, it is preferable that the shielding gas contains at least one gas among carbon dioxide gas, nitrogen gas, hydrogen gas, and oxygen gas, which have a high potential gradient. From the viewpoint of versatility, it is more preferable to use carbon dioxide gas alone, and in the case of a mixed gas with argon gas (hereinafter also referred to as "Ar gas"), it is more preferable to use a system in which at least one gas among carbon dioxide gas, nitrogen gas, hydrogen gas, and oxygen gas is contained and a gas other than Ar gas is mixed in a total of 5 to 50 volume %. The shielding gas is supplied from a shielding gas supply device (not shown).

[0031] The welding wire 100 used in this embodiment is not particularly limited, and for example, either a solid wire that does not contain flux or a flux-cored wire that contains flux may be used. The material of the welding wire 100 is also not limited, and for example, the material may be mild steel, stainless steel, aluminum, or titanium, and the wire surface may be plated with Cu or the like. Furthermore, the diameter of the welding wire 100 is also not limited. In this embodiment, the upper limit of the diameter is preferably 1.6 mm, and the lower limit is preferably 0.8 mm.

[0032] In addition, in this embodiment, the specific configuration of the workpiece 200 is not particularly important, and the processing conditions such as the joint shape, welding position, and groove shape are also not particularly important.

[0033] Welding controller 120 mainly controls the operation of welding robot 110. Welding controller 120 holds teaching data that predetermines the operation pattern, welding start position, welding end position, welding conditions, weaving operation, etc. of welding robot 110, and instructs welding robot 110 on these data to control the operation of welding robot 110. Welding controller 120 also provides welding conditions such as welding current, welding voltage, and feed speed during welding work to welding power source 140 in accordance with the teaching data. As shown in FIG. 1, welding system 50 of the present embodiment has a configuration in which welding control device 120 is independent from welding power source 140. However, welding control device 120 may be provided within welding power source 140.

[0034] Controller 150 is connected to welding control device 120, and creates or displays a program for operating welding robot 110, inputs teaching data, and provides the data to welding control device 120. Controller 150 also has a function for manually operating welding robot 110. Note that the connection between controller 150 and welding control device 120 may be wired or wireless.

[0035] In response to a command from welding control device 120, welding power source 140 supplies power to welding wire 100 and workpiece 200, thereby generating an arc between welding wire 100 and workpiece 200. In response to a command from welding control device 120, welding power source 140 also outputs a signal to a feeder (not shown) for controlling the speed at which welding wire 100 is fed.

[0036] <Functional configuration of welding power source> Next, the functional configuration of welding power supply 140 according to this embodiment will be described in detail with reference to Fig. 2. Fig. 2 is a block diagram showing a schematic configuration of a power supply control unit in welding power supply 140. The control system portion of welding power source 140 is executed, for example, through the execution of a program by welding control device 120 or a computer (not shown). The control system of the welding power source 140 includes a current setting unit 36. In addition to a function of setting various current values ​​that define the welding current flowing through the welding wire 100, the current setting unit 36 ​​in this embodiment has a function of setting the start and end times of a period during which the current value of the welding current is suppressed by a current suppression period setting unit 36A, and a function of obtaining information on the tip position of the welding wire 100 by a wire tip position conversion unit 36B. In addition, the current non-suppression period T IP Various condition settings, for example, the rising section T U or falling section T D The current setting points and the like are included in the function of setting various current values ​​that define the welding current in the current setting unit 36.

[0037] In this embodiment, the welding current is IP and current suppression period T IB The welding current is alternately repeated in a pulse waveform. IP The set current value Ip (hereinafter also referred to as the "peak current Ip") and the current suppression period T IB A set current value Ib (hereinafter also referred to as "base current Ib") for the current suppression period T is set. A steady-state current Ia for reset control of the droplet detachment timing, which will be described later, may also be set. In this embodiment, the welding current is basically controlled by two values, the peak current Ip and the base current Ib. Therefore, the time t1 at which the period during which the current value is suppressed starts represents the time at which the base current Ib starts, i.e., the base current start time. Furthermore, the time t2 at which the period during which the current value is suppressed ends represents the time at which the base current Ib ends, i.e., the base current end time. Note that the current non-suppression period T IP The time when the peak current starts is called the peak current start time, and the current non-suppression period T IP may be referred to as the peak current end time.

[0038] The main power supply circuit of welding power supply 140 is composed of a three-phase AC power supply (hereinafter also referred to as the “AC power supply”) 1, a primary side rectifier 2, a smoothing capacitor 3, a switching element 4, a transformer 5, a secondary side rectifier 6, and a reactor 7.

[0039] AC power input from an AC power source 1 is full-wave rectified by a primary side rectifier 2, and further smoothed by a smoothing capacitor 3 to be converted into DC power. Next, the DC power is converted into high-frequency AC power by inverter control using a switching element 4, and then converted into secondary power via a transformer 5. The AC output of the transformer 5 is full-wave rectified by a secondary side rectifier 6, and further smoothed by a reactor 7. The output current of the reactor 7 is provided to a welding tip 8 as an output from the main power supply circuit, and is passed through a welding wire 100 serving as a consumable electrode.

[0040] The welding wire 100 is fed by the feed motor 24 and the feed device 130, and an arc 9 is generated between the welding wire 100 and the base material 200. In this embodiment, the feed motor 24 moves the tip of the welding wire 100 toward the base material 200 during a forward feed period T P and a reverse feed period T during which the tip of the welding wire 100 moves in a direction opposite to the direction in which the base material 200 is located. N The welding wire 100 is fed so that the welding direction is periodically switched between the welding direction and the welding direction. The "tip of the welding wire" here generally refers to the tip of the wire when ignoring the presence of droplets hanging from the tip of the wire. In other words, the wire melted by the arc is considered to have immediately transferred to the base metal. As described later, the position is determined by the speed difference between the wire feed speed and the wire melting speed.

[0041] The feeding of the welding wire 100 by the feed motor 24 is controlled by a control signal Fc from the feed drive unit 23. The average value of the feed speed is approximately the same as the melting speed. In this embodiment, the feeding of the welding wire 100 by the feed motor 24 is also controlled by the welding power source 140.

[0042] The current setting unit 36 ​​is provided with a voltage setting signal Vr, which is a target value of the voltage applied between the welding tip 8 and the base material 200, from the voltage setting unit 34. The voltage setting signal Vr here is also provided to the voltage comparison unit 35, and is compared with the voltage detection signal Vo detected by the voltage detection unit 32. The voltage detection signal Vo is an actual measurement value. The voltage comparison unit 35 amplifies the difference between the voltage setting signal Vr and the voltage detection signal Vo, and outputs it to the current setting unit 36 ​​as a voltage error amplified signal Va. The current setting unit 36 ​​controls the welding current so that the length of the arc 9 (hereinafter also referred to as "arc length") is constant. That is, the current setting unit 36 ​​executes constant voltage control through the control of the welding current.

[0043] The current setting unit 36 ​​resets the value of the peak current Ip, the value of the base current Ib, the period for which the peak current Ip is provided, or the magnitude of the value of the peak current Ip and the value of the base current Ib based on the voltage setting signal Vr and the voltage error amplification signal Va, and outputs a current setting signal Ir to the current error amplification unit 37 according to the reset period or the magnitude of the reset value.

[0044] The current error amplifier 37 amplifies the difference between the current setting signal Ir given as a target value and the current detection signal Io detected by the current detector 31, and outputs it as a current error amplified signal Ed to the inverter driver 30. The inverter driver 30 corrects the drive signal Ec of the switching element 4 using the current error amplified signal Ed.

[0045] A detachment detection signal Drl, which is a signal for detecting detachment of a droplet from the tip of the welding wire 100, is also input to the current setting unit 36. The detachment detection signal Drl is output from the detachment detection unit 33. The detachment detection unit 33 monitors a change in the voltage detection signal Vo output by the voltage detection unit 32, and detects detachment of a droplet from the welding wire 100 from the change. The detachment detection unit 33 is an example of a detection means.

[0046] The detachment detection unit 33 here detects the detachment of a droplet by, for example, comparing a value obtained by differentiating or second-order differentiating the voltage detection signal Vo with a detection threshold value. The detection threshold value is stored in advance in a storage unit (not shown). The detachment detection unit 33 may generate the detachment detection signal Drl based on a change in resistance value calculated from the voltage detection signal Vo and the current detection signal Io, which are actual measured values.

[0047] The current setting unit 36 ​​is also provided with an average feed speed Fave of the welding wire 100 being fed. The average feed speed Fave is output by the average feed speed setting unit 20 based on teaching data stored in a storage unit (not shown). In other words, the average feed speed Fave may be referred to as a set value (command value) of the feed speed. The current setting unit 36 ​​determines the values ​​of the peak current Ip, the base current Ib, the time t1 when the base current Ib starts, and the time t2 when the base current Ib ends, based on the given average feed rate Fave.

[0048] 2, the average feed speed Fave is input to the current setting unit 36, but the signal input to the current setting unit 36 ​​may use a value related to the average feed speed Fave as a set value, replacing the average feed speed Fave. For example, if a database of average feed speeds Fave and average current values ​​that enable optimal welding for the average feed speeds Fave is stored in a storage unit (not shown), the average current value may be used as a set value, replacing the average feed speed Fave.

[0049] The average feed speed Fave is also given to the amplitude feed speed setting unit 21 and the feed speed command setting unit 22. The amplitude feed speed setting unit 21 here determines the values ​​of the amplitude Wf ​​and the period Tf based on the input average feed speed Fave. The amplitude feed refers to a feeding method in which a forward feed period, which is a period in which the feed speed is higher than the average feed speed Fave, and a reverse feed period, which is a period in which the feed speed is lower than the average feed speed Fave, alternately appear. The period in which the feed speed is lower than the average feed speed Fave refers to a period less than the average feed speed Fave, and includes a negative feed speed, that is, a speed in which the wire tip moves in the opposite direction to the position of the base material 200. The amplitude Wf ​​gives the change width for the average feed speed Fave, and the period Tf gives the time of the amplitude change, which is a repetition unit. The amplitude feed speed setting unit 21 generates and outputs an amplitude feed speed Ff according to the determined amplitude Wf ​​and period Tf or frequency f values.

[0050] The feed speed command setting unit 22 outputs a feed speed command signal Fw based on the amplitude feed speed Ff and the average feed speed Fave. In the present embodiment, the feed speed command signal Fw is expressed by the following equation. Fw=Ff+Fave...Equation (1)

[0051] However, the feed speed command signal Fw expressed by the formula (1) is applied only when the detachment of a droplet from the tip of the welding wire 100 is detected within an expected period. When the detachment of a droplet is not detected within the expected period, the feed speed command setting unit 22 may switch the feed speed command signal Fw to feed control at a constant speed. For example, the feed speed command setting unit 22 switches the feed speed command signal Fw to feeding at an average feed speed Fave. The switch from feeding at the average feed speed Fave to the feed control expressed by the formula (1) is determined according to the timing at which the detachment of a droplet is detected. A specific control example will be described later. The feed speed command setting unit 22 detects, based on a separation detection signal Drl given from a separation detection unit 33, at which phase of the amplitude feeding the separation has occurred.

[0052] The feed speed command signal Fw is output to a phase shift detection unit 26, a feed error amplification unit 28, and a current setting unit . The feed error amplifier 28 amplifies the difference between the feed speed command signal Fw, which is the target speed, and the feed speed detection signal Fo, which is the actual measured feed speed of the welding wire 100 by the feed motor 24, and outputs a speed error amplified signal Fd, in which the error has been corrected, to the feed drive unit 23. The feed driver 23 generates a control signal Fc based on the speed error amplified signal Fd and provides the control signal Fc to the feed motor 24. The feed speed converter 25 converts the amount of rotation of the feed motor 24, etc. into a feed speed detection signal Fo of the welding wire 100. The phase shift detector 26 in this embodiment compares the feed speed command signal Fw with the feed speed detection signal Fo, which is a measured value, and outputs the phase shift time Tθd. The phase shift detector 26 may obtain the phase shift time Tθd by measuring the feed operation of the feed motor 24 when parameters that define the amplitude feed, such as the period Tf, the amplitude Wf, and the average feed speed Fave, are varied.

[0053] The phase shift time Tθd is provided to a wire tip position conversion unit 36B of the current setting unit 36. The wire tip position conversion unit 36B calculates the tip position of the welding wire 100 with respect to the base material 200 as a reference plane based on the feed speed command signal Fw and the phase shift time Tθd, and provides information on the calculated tip position to the current suppression period setting unit 36A. Here, the current suppression period setting unit 36A sets a period during which the welding current is suppressed, i.e., a period during which the current setting signal Ir is controlled to the base current Ib, based on information on the tip position of the welding wire 100 or based on information on the tip position of the welding wire 100 and the feed speed command signal Fw. Here, the current setting unit 36 ​​is an example of a control means that changes the welding current depending on the tip position of the welding wire 100.

[0054] <Basic control of welding current based on information on the tip position of the welding wire or on the feed speed command signal Fw> An example of control of the welding current by the welding power source 140 based on the information on the tip position of the welding wire 100 or the feed speed command signal Fw will be described below. The control of the welding current is realized by the current setting unit 36 ​​constituting the welding power source 140. As described above, the current setting unit 36 ​​in this embodiment realizes the control through the execution of a program.

[0055] The current setting unit 36 ​​in this embodiment controls switching of the current value of the welding current based on information on the tip position of the welding wire 100 and a feed speed command signal Fw for the welding wire 100. Therefore, prior to describing the control of the welding current, a description will be given of changes over time in the feed speed command signal Fw and changes over time in the tip position of the welding wire 100.

[0056] FIG. 3 is a waveform diagram illustrating the change over time of the feed speed command signal Fw. The horizontal axis is time (phase) and the vertical axis is the wire feed speed. The vertical axis is expressed in meters per minute or revolutions. In FIG. 3, a speed higher than the average feed speed Fave is represented as "forward feed", and a speed lower than the average feed speed Fave is represented as "reverse feed". In this embodiment, the feed speed command signal Fw changes in a sine wave shape defined by a period Tf and an amplitude Wf. In the following, the period during which the feed speed is higher than the average feed speed Fave is referred to as the forward feed period T. P On the other hand, the period during which the feed rate is smaller than the average feed rate Fave is called the reverse feed period T N For ease of explanation, the first half of each period will be called the "early period" and the second half the "late period." Here, the average feed speed F can be regarded as the wire melting speed F. In the following, as shown in FIG. P and the reverse feeding period T N The amplitude feed that is periodically repeated is sometimes called the "initial condition".

[0057] 4 is a waveform diagram illustrating a change over time in the tip position (hereinafter also referred to as the "wire tip position") of the welding wire 100. The horizontal axis represents time (phase), and the vertical axis represents the distance (height) from the surface of the base material 200 in the normal upward direction. However, in FIG. 4, the position (height) when the welding wire 100 is fed at the maximum or minimum feed speed is taken as the reference distance, and distances greater than the reference distance are represented as positive values, and distances smaller than the reference distance are represented as negative values.

[0058] 4, the time points corresponding to the position where the tip of the welding wire 100 is closest to the base metal surface (hereinafter also referred to as the "bottom end") are indicated by T0 and T4, and the time point corresponding to the position where the tip of the welding wire 100 is farthest from the base metal surface (hereinafter also referred to as the "top end") is indicated by T2. The apex here is an example of the top end.

[0059] As shown in FIG. 4, the period during which the tip position of the welding wire 100 approaches the base metal surface over time, specifically, the period during which the tip position of the welding wire 100 moves from the uppermost end to the lowermost end, is called the “normal feeding period T P ", and the period during which the tip position of the welding wire 100 moves away from the base metal surface over time, specifically, the period during which the tip position of the welding wire 100 moves from the bottom end to the top end, is called the "reverse feeding period T N "

[0060] Also, time points corresponding to the reference distance are designated as T1 and T3. T1 is an intermediate time point from the bottom end, where the tip position of the welding wire 100 is closest to the base metal surface, to the top end, where the tip position is furthest from the base metal surface. Meanwhile, T3 is an intermediate time point from the top end to the bottom end. As shown in Fig. 4, the change in width from the reference distance to the top end or the change in width from the reference distance to the bottom end is the "amplitude Wf," and the change in width from the top end to the bottom end is the "wave height Wh."

[0061] 3 and 4, the feed speed of the welding wire 100 when the tip of the welding wire 100 is located at the uppermost or lowermost end is set to a predetermined average feed speed Fave. This allows the wire melting rate and the wire feed speed to be balanced even if the wire feed speed changes periodically, and the arc length becomes approximately constant, making it possible to continue stable welding.

[0062] FIG. 5 is a flow chart for explaining an example of basic control of the welding current in this embodiment. The control shown in FIG. 5 is executed by the current setting unit 36 ​​described in FIG. 2. The symbol S in the figure indicates a step. The control shown in FIG. 5 corresponds to one period of change in the tip position of the welding wire 100. For this reason, in FIG. 5, the state at time T when time T is point T0 is set as step 1. The current setting unit 36 ​​in this embodiment calculates the tip position of the welding wire 100 to control the current setting signal Ir. The average feed speed Fave is equivalent to the wire melting speed Fm. Therefore, the tip position of the welding wire 100 can be obtained by integrating the difference between the feed speed command signal Fw and the wire melting speed Fm (≈Fave). Therefore, the current setting unit 36 ​​sets the tip position of the welding wire 100 based on the following equation. Wire tip position = ∫(Fw-Fave) dt Equation (2) The change in tip position calculated by equation (2) corresponds to FIG.

[0063] 2 is used to feed the welding wire 100, a phase shift may occur between the command and the actual feed speed, i.e., the feed speed detection signal Fo. Therefore, the current setting unit 36 ​​corrects the base current start time t1 calculated according to the tip position of the welding wire 100 calculated from the average feed speed Fave and the feed speed command signal Fw, using the phase shift time Tθd provided by the phase shift detection unit 26. Specifically, the value of the base current start time t1 is reset as shown in the following equation. t1=t1+Tθd Equation (3)

[0064] Similarly, the current setting unit 36 ​​corrects the base current end time t2 calculated from the average feed speed Fave and the feed speed command signal Fw, using the phase shift time Tθd. t2=t2+Tθd...Equation (4) Here, the case where the base current start time t1 and the base current end time t2 are controlled from the viewpoint of the feed speed has been described, but the same is true from the viewpoint of position control.

[0065] 6 is a diagram showing an example of control of a current setting signal Ir that specifies a current value of a welding current. The horizontal axis represents time, and the vertical axis represents a current detection signal Io. Time points T0, T1, T2, T3, and T4 in the diagram correspond to time points T0, T1, T2, T3, and T4 in FIG. 4, respectively. The time points T0, T1, T2, T3, and T4 here are determined from the tip position of the welding wire 100, which is calculated from the average feed speed Fave and the feed speed command signal Fw.

[0066] As shown in FIG. 6, the base current start time t1 is the time T0 when the tip of the welding wire 100 is at the lowest position, that is, the positive feed period T P From the reverse feed period T N In Fig. 6, the maximum value of the base current start time t1 is represented as t1'.

[0067] Returning now to the description of Fig. 5, as shown in step 2, when the tip position of the welding wire 100 reaches the lowest end, i.e., time T0, the current setting unit 36 ​​judges whether or not the time T at which measurement started from time T0 is equal to or longer than the base current start time t1. While the judgment result in step 2 is negative (False), as shown in step 3, the current setting unit 36 ​​continues to output the peak current Ip as the current setting signal Ir. This period is called the current non-suppression period T in Fig. 6. IP Corresponds to.

[0068] 5, when the determination result in step 2 becomes positive (True), the current setting unit 36 ​​starts outputting the base current Ib as the current setting signal Ir as shown in step 4. As described above, when the switching to the base current Ib starts, the feeding of the welding wire 100 has already ended during the reverse feed period T N , and the tip of welding wire 100 begins to move in a direction away from the base metal surface.

[0069] The molten metal droplet near the time T0 when the tip of the welding wire 100 is at the lowest end is located near the molten pool, and therefore the arc length is short. NThat is, the tip of the welding wire 100 moves as if it is being pulled up. An inertial force acts on the entire grown droplet in the forward feeding direction, i.e., in the direction approaching the base material 200, while the welding wire 100 moves in the reverse direction, i.e., in the direction away from the base material 200, so that the droplet changes to a more suspended shape, and detachment is further promoted.

[0070] Moreover, by switching the welding current to the base current Ib during the period when separation is predicted, the arc reaction force can be reduced more than during the period when the peak current Ip is supplied. As a result, the force lifting the droplet becomes even weaker, making it even more likely for the droplet to become suspended. In this way, during the current suppression period T IB During this process, by detaching the droplets from the tip of the welding wire 100, it is expected that spatter will be reduced.

[0071] Returning to the explanation of FIG. 5, as shown in step 5, the current setting unit 36, which has switched the current setting signal Ir to the base current Ib, judges whether or not the time T is equal to or longer than the base current end time t2. In FIG. 6, the maximum value of the base current end time t2 is indicated as t2'. While the judgment result in step 5 is negative (False), as shown in step 4, the current setting unit 36 ​​outputs the base current Ib as the current setting signal Ir. After the supply of the base current Ib is started, the tip of the welding wire 100 moves so as to be pulled up to the apex, i.e., the position where the tip is farthest from the base material 200, while droplets are detached.

[0072] After the droplet is detached, the supply period of the base current Ib, i.e., the current suppression period T IB The period during which the peak current Ip is supplied, i.e., the current non-suppression period T IP Therefore, it is desirable to end the supply of the base current Ib between the times T1 and T2.

[0073] When the determination result in step 5 becomes positive (True), the current setting unit 36 ​​starts outputting the peak current Ip as the current setting signal Ir, as shown in step 6. Next, as shown in step 7, the current setting unit 36 ​​determines whether the time T, at which measurement started from time T0, has reached time T4. While the determination result in step 7 is negative (False), the current setting unit 36 ​​outputs the peak current Ip as the current setting signal Ir, as shown in step 6. On the other hand, when the determination result in step 7 becomes positive (True), the current setting unit 36 ​​returns to step 1. Through the above control, the current setting signal Ir becomes a pulse waveform that periodically repeats the peak current Ip and the base current Ib.

[0074] <Method of controlling droplet detachment> The above description is the basic control of the welding current by the welding power source 140 based on the information on the tip position of the welding wire 100 or the feed speed command signal Fw. In actual welding, there is a possibility that separation does not occur as expected depending on the welding environment, such as the welding conditions and disturbances. In this embodiment, the value of the frequency f, the peak current Ip, i.e., the current non-suppression period T IP The set current, base current Ib, i.e., the current suppression period T IB Set current, current non-suppression period T IP (which may also be called the "peak current period"), the current suppression period T IB (which may be referred to as the "base current period"), the positive feed period T P , reverse feed period T N By controlling each of the above under the conditions described in detail below, droplet detachment can be controlled with higher accuracy.

[0075] In addition, the current non-suppression period T IP Set current or current suppression period T IB The set current is not limited to a constant current value, and the set value may be changed within each period. IP Overall or current suppression period T IB As an index of the total heat energy, the current non-suppression period T IP or current suppression period T IBThe average current of the current non-suppression period T IP The average current of P-AVE " and the current suppression period T IB The average current of B-AVE " is displayed.

[0076] Each control element will now be described in detail.

[0077] (Frequency f: 50~150Hz) Positive feed period T P and the reverse feeding period T N The combined period of these is regarded as one cycle, and the frequency f is controlled in order to prevent short circuits by stably separating or dripping the droplets formed at the tip of the welding wire. This frequency f is set in the range of 50 to 150 Hz as a condition described later, that is, a condition for forming an optimal droplet size while maintaining the penetration depth. When the frequency f is below 50Hz, excessively large droplets are formed at the tip of the wire, but the inertial force acting on the droplets is insufficient, so the large droplets tend to come into contact with the molten pool and are difficult to separate from. As a result, short circuits increase, which in turn increases spatter and makes it difficult to obtain a stable penetration depth.

[0078] On the other hand, when the frequency f exceeds 150 Hz, the size of the droplet formed at the wire tip does not grow to the optimal size, and the inertial force is insufficient, so the current suppression period T IB As a result, droplets can detach at unintended times, causing short circuits and spattering. Therefore, the frequency f is specified to be in the range of 50 to 150 Hz, preferably 60 to 130 Hz, and more preferably 70 to 120 Hz.

[0079] The droplet size suitable for the above-mentioned frequency f is 1.7 to 5.0 mm in average volume. 3The droplet size here means the size of the droplet just before it separates, and examples of the method include a method of calculating the volume from the melting speed Fm, a method of taking pictures from one or more directions with a visual sensor, and a method of calculating the volume based on the obtained two-dimensional images, etc. The average volume before separation is 1.7 to 5.0 mm 3 Within this range, it is possible to more effectively suppress short circuits, and it is possible to effectively reduce spatters and obtain a stable penetration depth.

[0080] (0.65≦I P-AVE / (I P-AVE +I B-AVE )≦0.90) Current non-suppression period T IP The average current I P-AVE and current suppression period T IB The average current I B-AVE I for the sum of P-AVE The ratio of I P-AVE / (I P-AVE +I B-AVE ) is in the range of 0.65 to 0.90. When the above ratio falls below 0.65, the current non-suppression period T IP In the current suppression period T IB In the current non-suppression period T, it becomes difficult for the droplets to separate due to inertial force alone, so the timing of separation is shifted and a short circuit is likely to occur. This short circuit causes spattering and makes it difficult to obtain a stable penetration depth. IP In this case, the thermal energy tends to be small, and therefore the penetration depth in particular becomes shallow.

[0081] On the other hand, when the above ratio exceeds 0.90, the current non-suppression period T IPIn this process, as the droplet size becomes excessively large, the arc pressure applied to the droplet (hereinafter, also referred to as "arc reaction force" when referring to the arc pressure on the droplet) becomes excessive, causing the droplet pushed up to detach in a direction different from the molten pool, which makes it easier for large spatter to occur. In addition, arc interruption and long-term short circuiting are also more likely to occur, which causes spatter and makes it impossible to obtain a stable penetration depth. Therefore, I P-AVE / (I P-AVE +I B-AVE ) is specified to be in the range of 0.65 to 0.90, and preferably in the range of 0.70 to 0.85.

[0082] (Wave height Wh: 14~35% of tip-base metal distance) 4, the wave height Wh, which is the variation in the tip position of the welding wire 100 between the uppermost end and the lowermost end, is set in the range of 14 to 35% of the tip-base metal distance. For example, when the tip-base metal distance is 25 mm, the wave height Wh should be set in the range of 3.75 mm to 8.75 mm. If the above-mentioned wave height Wh is outside the range of 14 to 35% of the tip-base metal distance, it becomes impossible to prevent a short circuit. Note that the "reference distance" that is the reference position for the wave height Wh and the amplitude Wf ​​may be set arbitrarily.

[0083] (0.30≦T IB / (T IP +T IB )≦0.60) Any current non-suppression period T IP and the current suppression period T immediately after IB The current suppression period T IB The ratio of T IB / (T IP +T IB ) is in the range of 0.30 to 0.60. When the above ratio falls below 0.30, the current suppression period T IB In the current non-suppression period T IPThe arc reaction force causes the material to easily come off, which increases the risk of short circuits and spattering, making it difficult to obtain a stable penetration depth.

[0084] On the other hand, if the above ratio exceeds 0.60, the electromagnetic pinch force is insufficient, and the current suppression period T IB As a result, droplets can detach at unintended times, causing short circuits and spattering. Therefore, T IB / (T IP +T IB ) is specified to be in the range of 0.30 to 0.60, preferably 0.31 to 0.58, and more preferably 0.31 to 0.52.

[0085] (0.40≦T N / (T P +T N )≦0.70) Positive feed period T P and the reverse feeding period T N The reverse feed period T for the sum of N The ratio of T N / (T P +T N ) is in the range of 0.40 to 0.70. If the ratio is less than 0.40, the time required for droplet detachment cannot be obtained, and the current suppression period T IB As a result, droplets can detach at unintended times, causing short circuits and spattering.

[0086] On the other hand, when the above ratio exceeds 0.70, the droplet formed at the wire tip becomes thin and elongated, and the reverse feed period T N Short circuits are likely to occur before T N / (T P +T N ) is specified in the range of 0.40 to 0.70.

[0087] {T N / (T P +T N )}>{TIB / (T IP +T IB )} Positive feed period T p and the reverse feeding period T N The reverse feed period T for the sum of N The ratio of {T N / (T P +T N )} and the current non-suppression period T IP and current suppression period T IB The current suppression period T for the sum of IB The ratio of {T IB / (T IP +T IB )} is expressed as {T N / (T P +T N )}>{T IB / (T IP +T IB )}. {T N / (T P +T N )} has a value of {T IB / (T IP +T IB ) value, the arc force at the time when the tip of the wire approaches the molten pool before reverse feed occurs is insufficient, and the penetration depth becomes shallow.

[0088] In other words, if there is sufficient arc pressure before and after the wire tip is at the lowest end, even if the average arc length is short, a buried arc state without short circuit can be achieved and sufficient penetration depth can be obtained. However, as described above, the timing before and after the wire tip is at the lowest end is longer than the current suppression period T IB If this is the case, sufficient arc pressure cannot be obtained, so that the droplets are likely to come into contact with the molten pool and short-circuit, and as a result, sufficient penetration depth cannot be obtained. The buried arc refers to a state in which the wire sinks into the molten pool due to strong arc pressure, generating an arc. Generally, the higher the welding current, the stronger the arc pressure.

[0089] (positive feeding period T P The period of more than 2 / 3 of the current is the non-suppression period TIP (occupying The period of at least 2 / 3 of the period during which the tip of the welding wire 100 moves from the uppermost end to the lowermost end is defined as the current non-suppression period T IP Here, the period during which the wire tip position moves from the top to the bottom is the normal feeding period T P Refers to...

[0090] Here, explanation will be given with reference to Fig. 7 and Fig. 8. Fig. 7 is a series of photographs taken by a high-speed camera showing an example of the progress of welding in a conventional short-circuit transfer method, together with the advancement or retreat of the welding wire, the current non-suppression period, and the current suppression period, and is a drawing substitute photograph for each elapsed time for Test No. 24, which is a reference example described later. Fig. 8 is a series of photographs taken by a high-speed camera showing an example of the progress of welding in this embodiment, together with the advancement or retreat of the welding wire, the current non-suppression period, and the current suppression period, and is a drawing substitute photograph for each elapsed time for Test No. 8, which is an example described later. As shown in FIG. 7, in the conventional short-circuit transfer type wire feed control, the forward feed period T P is approximately 8.4ms from 0ms to 8.4ms, whereas the normal feeding period T P During the non-suppression period T IP Since the period from 0 ms to 2.4 ms is approximately 2.4 ms, the normal feeding period T P During the non-suppression period T IP It can be seen that the proportion of is less than half. In this way, in the conventional short-circuit transfer type wire feed control, P During the non-suppression period T IP By controlling the ratio to less than half, low-spatter welding is possible, but as a result, the arc pressure does not act on the molten pool, resulting in a shallow penetration depth.

[0091] On the other hand, as shown in FIG. 8, in the wire feed control according to the present embodiment, the normal feed period T P is approximately 8.4ms from 0ms to 8.4ms, while the normal feeding period T PDuring the non-suppression period T IP is about 7.2 ms from 0 ms to about 7.2 ms, and the normal feeding period T P During the non-suppression period T IP It can be seen that the proportion of In this way, in the wire feed control according to the present embodiment, the normal feed period T P During the non-suppression period T IP By controlling the ratio to 2 / 3 or more, sufficient arc pressure is provided to dig into the molten pool as the wire tip approaches the molten pool, resulting in a deep penetration depth.

[0092] Next, preferred conditions in this embodiment will be described in detail.

[0093] As shown in FIG. 9A, the current non-suppression period T IP is the current suppression period T during which the base current changes to a predetermined current value. IB The immediately following rising section T U , the current changes from a predetermined current value to the base current during the current suppression period T IB The previous falling edge T D , and the rising section T U and the falling section T D Current control section other than T C It is preferable to separately control the current.

[0094] This rising section T U is a current non-suppression period T IP The ratio of the rising section T U / current non-suppression period T IP It is preferable that the value of "(T ) × 100%)" is 20% or less. U The welding current value rises sharply as shown in FIG. 9A, in other words, during the current non-suppression period T IP Rising section T U The ratio may be as close to 0% as possible.

[0095] In addition, the falling section T D is the current non-suppression period T IP The ratio of the falling edge period T D / current non-suppression period T IP It is preferable that the value of "(T )×100%)" is 20% or less. D The welding current value falls sharply as shown in FIG. 9A, in other words, during the current non-suppression period T IP Falling period T D The ratio may be as close to 0% as possible. In addition, the rising section T U or falling section T D may each change linearly, curvedly or stepwise, or may be a combination of these.

[0096] Next, as shown in FIG. 9A, the current control section T C It is preferable to provide at least two welding current set values ​​in the first welding current set value I. P1 and the second welding current setting value I P2 Let us assume that.

[0097] When the uppermost end position of the welding wire 100 is set as 0 deg, the first welding current setting value I P1 As the timing for setting the first welding current setting value I P1 It is preferable to set the end position of the range of the first welding current setting value I to a range of 20 degrees or less. P1 By setting the end position of the range to 20 deg or less, the oscillation of the droplet that has begun to form can be suppressed, and more stable detachment can be maintained.

[0098] In addition, when the uppermost end position of the welding wire 100 is set as 0 deg, the second welding current setting value I P2 As the timing for setting the second welding current setting value I P2It is preferable to set the end position of the second welding current setting value I in the range of 135 to 220 degrees. P2 By setting the end position of the range between 135 and 220 deg, the arc pressure can be effectively applied to the molten pool, making it possible to obtain a stable penetration depth.

[0099] Furthermore, as shown in FIG. 9B, the welding current setting value I P2 The end of the range is the current control section T C The welding current setting value I P2 When the end position of the range is Xdeg, the current suppression period T IB It is preferable to set the end position of the current suppression period T in the range of (X+100) to (X+220) deg. IB By setting the end position of in the range of (X+100)~(X+220)deg, the current suppression period T IB This is preferable from the viewpoint of stabilizing droplet detachment since the timing when the most inertial force acts is included within the period.

[0100] First welding current setting I P1 The welding current set in is preferably in the range of 250 to 600 A, and the second welding current set value I P2 The welding current set in the first welding current setting value I is preferably in the range of 300 to 650 A. P1 and the second welding current setting value I P2 By setting the set currents in the above ranges, the first welding current set value I P1 and the second welding current setting value I P2 By providing the above, the effect obtained can be further improved. In addition, the second welding current setting value I P2 The welding current set by is the first welding current setting value I P1 This will always be a larger value than the welding current set by

[0101] Current control section T C , in detail, the first welding current set value I P1 and the second welding current setting value I P2During this period, it is preferable to set the external characteristic of the welding power source. More specifically, by setting the external characteristic of the welding power source within the range of 0.05 V to 20 V / 100 A, the arc length is controlled to be approximately constant by changing the welding current even when the extension length changes during welding.

[0102] Current non-suppression period T IP The average current I P-AVE The current suppression period T IB The average current I B-AVE In terms of adjusting the droplet size, the current non-suppression period T IP The current suppression period T IB From the viewpoint of adjusting the droplet size, it is preferable that the duration is in the range of 2.0 to 9.0 ms. In addition, the normal feeding period T P and reverse feed period T N The preferred range of is the above-mentioned frequency f and {T N / (T P +T N )} is a period calculated from the respective specified ranges. EXAMPLES

[0103] The present invention will be described in more detail below with reference to examples. The present invention is not limited to these examples, and can be modified within the scope of the invention, and all such modifications are within the technical scope of the invention.

[0104] [1. Preliminary Examination] First, prior to the main test described below, a preliminary test was carried out to examine the relationship between the number of short circuits and the penetration depth. Fig. 10 is a diagram showing the relationship between the number of short circuits and the penetration depth. The upper photograph in Fig. 10 is a cross-sectional photograph of a welded portion when welding was performed under welding conditions of a welding current of 309 A, a welding voltage of 36.7 V, and a welding speed of 50 cm / min, with the number of short circuits being 97.7 times / second. The lower photograph in Fig. 10 is a cross-sectional photograph of a welded portion when welding was performed under welding conditions of a welding current of 307 A, a welding voltage of 36.8 V, and a welding speed of 50 cm / min, with the number of short circuits being 9.6 times / second.

[0105] As is clear from these cross-sectional photographs, a correlation is observed between the number of short circuits and the penetration depth, and it can be seen that the lower test example, which has a significantly lower number of short circuits, has a deeper penetration of the weld. It was also visually confirmed that the fewer the number of short circuits, the less spatter is generated. In other words, it is believed that a smaller number of short circuits leads to a stable penetration depth and reduced spatter. For these reasons, in the following tests, the number of short circuits will be used to determine whether a stable penetration depth and reduced spatter have been achieved.

[0106] [2. Actual Test] Next, in order to confirm the effect of the welding control method according to the present invention, tests were carried out on the following examples and comparative examples.

[0107] <Common welding conditions> The common welding conditions were as follows: Welding wire: Mild steel solid wire Base material: SS400 (general structural rolled steel JIS G 3101:2004) Welding wire welding speed: 40cm / min Welding method: Bead-on-plate

[0108] <Evaluation method> As explained in [1. Preliminary Test] above, since there is thought to be a correlation between the number of short circuits and whether stable penetration depth and reduction in spatter have been achieved, stable penetration depth and reduction in spatter were evaluated based on the number of short circuits. In this test, a short circuit count of 5.0 times / second or less was rated A (excellent), a short circuit count of more than 5.0 times / second and less than 10.0 times / second was rated B (good), and a short circuit count of more than 10.0 times / second was rated C (poor).

[0109] The test results are shown in Tables 1 and 2, together with the welding conditions other than the common test conditions.

[0110] [Table 1]

[0111] [Table 2]

[0112] As shown in Tables 1 and 2, Tests No. 1 to No. 10 are examples that satisfy all the requirements of the present invention, and the number of short circuits was very small. This indicates that the penetration depth is deep and the amount of spatter generation is small. On the other hand, Tests No. 11 to No. 23 are comparative examples that do not satisfy at least some of the requirements of the present invention, and the number of short circuits was very large in all cases. This indicates that the penetration depth is shallow and the amount of spatter generation is large. In Table 1, "frequency f (Hz)", "(wave height Wh / tip-base metal distance) x 100 (%)", and "I P-AVE / (I P-AVE +I B-AVE )," "T IB / (T IP +T IB )," "T N +(T P +T N )," "{T N / (T P +T N )}>{T IB / (T IP+T IB )}", values ​​that do not satisfy the scope of the present invention are underlined. Test No. 24 in Table 1 is a reference example of the feeding process by the conventional short-circuit transfer method described above with reference to FIG. 8, and the normal feeding period T P The period of more than 2 / 3 of the current is the non-suppression period T IP This is an example that does not satisfy the condition that the occupancy is

[0113] Each test is discussed in detail below.

[0114] Test No. 1, which is an embodiment of the present invention, satisfies all of the requirements of the present invention, but in particular, since the frequency f was 60 Hz and fell within the range of 50 to 150 Hz, an inertial force acted on the tip of the wire, resulting in a small number of short circuits and a rating of B.

[0115] Test No. 2, which is an embodiment of the present invention, satisfies all of the requirements of the present invention, but in particular, since the frequency f was 130 Hz and fell within the range of 50 to 150 Hz, an inertial force acted on the tip of the wire, resulting in a small number of short circuits and an A rating.

[0116] Test No. 3, which is an embodiment of the present invention, satisfies all of the requirements of the present invention, but in particular, {(wave height Wh / tip-base metal distance) x 100} is 15%, which satisfies the range of 14 to 35%, so that inertial forces act on the tip of the wire, the number of short circuits is low, and the test was rated B.

[0117] Test No. 4, which is an embodiment of the present invention, satisfies all of the requirements of the present invention, but in particular, {(wave height Wh / tip-base metal distance) x 100} was 32%, which satisfies the range of 14 to 35%, so that an inertial force acts on the tip of the wire, the number of short circuits was low, and the test was rated A.

[0118] The embodiment, Test No. 5, satisfies all the requirements of the present invention, but in particular, P-AVE / (I P-AVE +IB-AVE )} was 0.67, which satisfies the range of 0.65 to 0.90, so the droplet size was appropriate, the electromagnetic pinch force worked effectively, the number of short circuits was low, and the evaluation was B.

[0119] The embodiment, Test No. 6, satisfies all the requirements of the present invention, but in particular, P-AVE / (I P-AVE +I B-AVE )} was 0.88, which satisfies the range of 0.65 to 0.90, so the droplet size was appropriate, the electromagnetic pinch force worked effectively, the number of short circuits was low, and the evaluation was B.

[0120] The embodiment, Test No. 7, satisfies all the requirements of the present invention, but in particular, IB / (T IP +T IB )} was 0.31, which satisfies the range of 0.30 to 0.60, so the droplet size was appropriate, the electromagnetic pinch force worked effectively, the number of short circuits was low, and the evaluation was A.

[0121] The embodiment, Test No. 8, satisfies all the requirements of the present invention, but in particular, IB / (T IP +T IB )} was 0.58, which satisfies the range of 0.30 to 0.60, so the droplet size was appropriate, the electromagnetic pinch force worked effectively, the number of short circuits was low, and the evaluation was B.

[0122] The embodiment, Test No. 9, satisfies all the requirements of the present invention, but in particular, N +(T P +T N )} was 0.40, which satisfies the range of 0.40 to 0.70, so that the inertial force acts effectively on the tip of the wire, the number of short circuits was reduced, and the wire was rated A.

[0123] The embodiment, Test No. 10, satisfies all the requirements of the present invention, but in particular, {T N +(TP +T N )} was 0.70, which satisfies the range of 0.40 to 0.70, so that the inertial force acts effectively on the wire tip, the number of short circuits was reduced, and the wire was rated A.

[0124] On the other hand, in the comparative example, Test No. 11, the frequency f was 45 Hz, which is below the range specified in the present invention, so the inertial force acting on the wire tip was insufficient and the droplets could not detach, resulting in a high number of short circuits and a rating of C.

[0125] In the comparative example, Test No. 12, the frequency f was 155 Hz, which exceeded the range specified in the present invention. As a result, the droplet size was too small, the inertial force acting on the wire tip was insufficient, and the droplets could not be detached. As a result, the number of short circuits was high and the test was rated C.

[0126] In the comparative example, Test No. 13, {(wave height Wh / tip-base metal distance) × 100} was 13%, which is below the range specified in the present invention. As a result, the inertial force acting on the wire tip was insufficient and the droplets could not detach, resulting in a high number of short circuits and a rating of C.

[0127] In the comparative example, Test No. 14, {(wave height Wh / tip-base metal distance) × 100} was 38%, which exceeded the range specified in the present invention. As a result, even with a normal arc length, the number of short circuits increased, and the number of short circuits was high, resulting in a rating of C.

[0128] In the comparative example, Test No. 15, {(wave height Wh / tip-base metal distance)×100} was 13%, which is below the range specified in the present invention. Therefore, the inertial force acting on the wire tip was insufficient, and the droplet could not be detached. IB / (T IP +T IB )} is 0.22, which is below the range defined in the present invention. IB In the current non-suppression period T IPThe joint was subject to the arc reaction force and was prone to detachment, and the number of short circuits increased. As a result, spatter increased and a stable penetration depth could not be obtained, resulting in a high number of short circuits and a rating of C.

[0129] In the comparative example, Test No. 16, {(wave height Wh / tip-base metal distance)×100} was 40%, which is beyond the range specified by the present invention. Therefore, even with a normal arc length, short circuits increased. IB / (T IP +T IB )} is 0.14, which is below the range defined in the present invention. IB In the current non-suppression period T IP The joint was subject to the arc reaction force and was prone to detachment, and the number of short circuits increased. As a result, spatter increased and a stable penetration depth could not be obtained, resulting in a high number of short circuits and a rating of C.

[0130] Test No. 17, which is a comparative example, is P-AVE / (I P-AVE +I B-AVE )} is 0.60, which is below the range specified in the present invention, so the electromagnetic pinch force acting on the droplet is also small. N / (T P +T N )}<{T IB / (T IP +T IB )}, which does not satisfy the conditions stipulated in the present invention, the arc force was insufficient when the tip of the wire approached the molten pool before reverse feeding occurred, making it prone to short circuits and resulting in shallow penetration depth. As a result, there were many short circuits and the material was rated C.

[0131] Test No. 18, which is a comparative example, is P-AVE / (I P-AVE +I B-AVE )} was 0.91, which exceeded the range specified in the present invention. Therefore, the droplet size was large, the droplets were repelled and detached due to the arc reaction force, and arc interruption and long-term short circuits occurred. As a result, the number of short circuits was high and the specimen was rated C.

[0132] Test No. 19, which is a comparative example, is {T IB / (T IP +T IB )} is 0.29, which is below the range defined in the present invention. IB In the current non-suppression period T IP The joint was easily detached due to the arc reaction force, the number of short circuits increased, spatter increased, and a stable penetration depth could not be obtained, resulting in a high number of short circuits and a rating of C.

[0133] Test No. 20, which is a comparative example, is {T IB / (T IP +T IB )} is 0.64, which is beyond the range specified in the present invention, so the electromagnetic pinch force is insufficient, and the current suppression period T IB In the welding process, stable detachment was not possible, and droplets were detached at unintended times, causing short circuits and spattering. N / (T P +T N )}<{T IB / (T IP +T IB )}, which does not satisfy the conditions stipulated in the present invention, the arc force was insufficient when the tip of the wire approached the molten pool before reverse feeding occurred, making it prone to short circuits and resulting in a shallow penetration depth. As a result, there were many short circuits and the material was rated C.

[0134] Test No. 21, which is a comparative example, is {T N +(T P +T N )} is 0.35, which is below the range specified in the present invention, so that a sufficient time required for droplet detachment cannot be obtained, and the current suppression period T IB In the welding process, stable detachment was not possible, and droplets were detached at unintended times, causing short circuits and spattering. N / (T P +T N )}<{T IB / (T IP +TIB )}, which does not satisfy the conditions stipulated in the present invention, the arc force was insufficient when the tip of the wire approached the molten pool before reverse feeding occurred, making it prone to short circuits and resulting in shallow penetration depth. As a result, there were many short circuits and the material was rated C.

[0135] Test No. 22, which is a comparative example, is {T N +(T P +T N )} was 0.75, which exceeded the range specified in the present invention. Therefore, the droplets formed at the tip of the wire became thin and stretched, making it easier for short circuits to occur before the reverse feed period began, and the penetration was shallow, resulting in a large number of short circuits and a rating of C.

[0136] Test No. 23, which is a comparative example, is {T N / (T P +T N )}<{T IB / (T IP +T IB )}, which does not satisfy the conditions stipulated in the present invention, the arc force was insufficient when the tip of the wire approached the molten pool before reverse feeding occurred, making it prone to short circuits and resulting in shallow penetration depth. As a result, there were many short circuits and the material was rated C.

[0137] The present invention is not limited to the above-described embodiment and examples, and can be modified, improved, etc. as appropriate.

[0138] As described above, the present specification discloses the following:

[0139] (1) In gas metal arc welding, in which a welding current is supplied to a welding wire, A forward feed period T during which the tip of the welding wire moves from the uppermost end, which is the position farthest from the base metal, to the lowermost end, which is the position closest to the base metal. P and a reverse feed period T NWhile controlling the feed speed of the welding wire so that the welding wire is fed toward the base metal with periodic switching of Based on at least a tip position signal of the welding wire or a feed speed signal of the welding wire, The welding current is kept in a current non-suppression period T IP or current suppression period T IB A welding control method for switching and controlling a welding The positive feeding period T P and the reverse feed period T N The combined period is considered as one cycle, and its frequency f is 50 to 150 Hz. The current non-suppression period T IP The average current I P-AVE and the current suppression period T IB The average current I B-AVE The relationship is 0.65≦I P-AVE / (I P-AVE +I B-AVE )≦0.90, A wave height Wh, which is a change width of the tip position of the welding wire between the uppermost end and the lowermost end, is set to 14 to 35% of a tip-base metal distance of the welding wire, Any of the current non-suppression periods T IP and the current suppression period T immediately thereafter. IB The relationship between these two is 0.30≦T IB / (T IP +T IB )≦0.60, The positive feeding period T P and the reverse feed period T N The relationship is 0.40≦T N / (T P +T N )≦0.70, and, The current non-suppression period T IP , the current suppression period T IB , the positive feeding period T P and the reverse feed period T N The relationship between N / (T P +T N )}>{T IB / (T IP +T IB)} and The positive feeding period T P The period of 2 / 3 or more of the current non-suppression period T IP A welding control method comprising the steps of: According to this configuration, in an arc welding method in which forward and reverse feeding of the tip of the wire is cyclically repeated, it is possible to achieve both a stable penetration depth and a reduction in spatter.

[0140] (2) The welding control method according to (1), wherein the feed speed of the welding wire when the tip of the welding wire is located at the uppermost end or the lowermost end is set to a predetermined average feed speed. With this configuration, even if the wire feed speed changes periodically, the wire melting rate and the wire feed speed are balanced, the arc length remains roughly constant, and stable welding can be continued.

[0141] (3) The current non-suppression period T IP is the current suppression period T IB The rising section immediately after, the current suppression period T IB The current control section T other than the immediately preceding falling section, the rising section, and the falling section C It consists of: The rising section is the current non-suppression period T IP 20% or less of the current non-suppression period T IP The welding control method according to claim 1 or 2, wherein the welding speed is 20% or less. According to this configuration, the rising section T U In the falling section T D In this way, it is possible to achieve droplet size adjustment before reverse feed takes place.

[0142] (4) Current control section T C At least two welding current settings I P1 , I P2 having When the uppermost end position of the welding wire is set as a reference at 0 deg, The welding current setting value I P1 Set the end position of the range to within 20 deg. The welding current setting value I P2 The welding control method according to (3), wherein the end position of the range is set in the range of 135 to 220 degrees. According to this configuration, the first welding current set value I P1 By setting the end position of the range to 20 degrees or less, the oscillation of the droplets that have started to form can be suppressed, and more stable detachment can be maintained. In addition, the second welding current setting value I P2 By setting the end position of the range between 135 and 220 deg, the arc pressure can be effectively applied to the molten pool, making it possible to obtain a stable penetration depth.

[0143] (5) The welding current setting value I P2 The end of the range is the current control section T C The terminus of The welding current setting value I P2 If the end position of the range is Xdeg, The current suppression period T IB The welding control method according to (4), wherein the end position of the welding is set within a range of (X+100) to (X+220) degrees. According to this configuration, the current suppression period T IB The timing when the most inertial force is exerted is included within the period, which makes it possible to stabilize droplet detachment.

[0144] (6) The welding current setting value I P1 The set current is 250 to 600A. The welding current setting value I P2 The welding control method according to (4) or (5), wherein the set current is 300 to 650 A. According to this configuration, the first welding current set value I P1 and the second welding current setting value I P2 By providing the above, the effect obtained can be further enhanced.

[0145] (7) The current control section T C In the welding control method according to any one of (4) to (6), an external characteristic of the welding power source is provided. According to this configuration, even if the extension length changes during welding, the arc length can be controlled to be approximately constant by changing the welding current.

[0146] (8) The average volume of the droplet detached from the tip of the welding wire is 1.7 to 5.0 mm 3 The welding control method according to any one of (1) to (7), According to this configuration, it is possible to more effectively suppress short circuits, reduce spatters, and achieve a stable high penetration depth.

[0147] (9) In gas metal arc welding, in which a welding current is supplied to a welding wire, A forward feed period T during which the tip of the welding wire moves from the uppermost end, which is the position farthest from the base metal, to the lowermost end, which is the position closest to the base metal. P and a reverse feed period T N While controlling the feed speed of the welding wire so that the welding wire is fed toward the base metal with periodic switching of Based on at least a tip position signal of the welding wire or a feed speed signal of the welding wire, The welding current is kept in a current non-suppression period T IP or current suppression period T IB A welding control device for switching and controlling The positive feeding period T P and the reverse feed period T N The combined period is considered as one cycle, and its frequency f is 50 to 150 Hz. The current non-suppression period T IP The average current I P-AVE and the current suppression period T IB The average current I B-AVE The relationship is 0.65≦I P-AVE / (I P-AVE +I B-AVE)≦0.90, A wave height Wh, which is a change width of the tip position of the welding wire between the uppermost end and the lowermost end, is set to 14 to 35% of a tip-base metal distance of the welding wire, Any of the current non-suppression periods T IP and the current suppression period T immediately thereafter. IB The relationship between these two is 0.30≦T IB / (T IP +T IB )≦0.60, The positive feeding period T P and the reverse feed period T N The relationship is 0.40≦T N / (T P +T N )≦0.70, and, The current non-suppression period T IP , the current suppression period T IB , the positive feeding period T P and the reverse feed period T N The relationship between N / (T P +T N )}>{T IB / (T IP +T IB )} and The positive feeding period T P The period of 2 / 3 or more of the current non-suppression period T IP A welding control device having a function of controlling the welding time so that the welding speed is within the predetermined range. According to this configuration, in an arc welding method in which forward and reverse feeding of the tip of the wire is cyclically repeated, it is possible to achieve both a stable penetration depth and a reduction in spatter.

[0148] (10) A welding power source equipped with the welding control device described in (9). According to this configuration, in an arc welding method in which forward and reverse feeding of the tip of the wire is cyclically repeated, it is possible to achieve both a stable penetration depth and a reduction in spatter.

[0149] (11) A welding system comprising the welding control device according to (9) or the welding power source according to (10). According to this configuration, in an arc welding method in which forward and reverse feeding of the tip of the wire is cyclically repeated, it is possible to achieve both a stable penetration depth and a reduction in spatter.

[0150] (12) In gas metal arc welding, in which a welding current is supplied to a welding wire, A forward feed period T during which the tip of the welding wire moves from the uppermost end, which is the position farthest from the base metal, to the lowermost end, which is the position closest to the base metal. P and a reverse feed period T N While controlling the feed speed of the welding wire so that the welding wire is fed toward the base metal with periodic switching of Based on at least a tip position signal of the welding wire or a feed speed signal of the welding wire, The welding current is kept in a current non-suppression period T IP or current suppression period T IB A computer of a welding system including at least a welding control device for switching between and controlling the welding The welding control device, The positive feeding period T P and the reverse feed period T N The combined period is considered as one cycle, and its frequency f is 50 to 150 Hz. The current non-suppression period T IP The average current I P-AVE and the current suppression period T IB The average current I B-AVE The relationship is 0.65≦I P-AVE / (I P-AVE +I B-AVE )≦0.90, A wave height Wh, which is a change width of the tip position of the welding wire between the uppermost end and the lowermost end, is set to 14 to 35% of a tip-base metal distance of the welding wire, Any of the current non-suppression periods T IP and the current suppression period T immediately thereafter. IB The relationship between these two is 0.30≦T IB / (T IP +T IB )≦0.60, The positive feeding period T P and the reverse feed period T N The relationship is 0.40≦T N / (T P +T N )≦0.70, and, The current non-suppression period T IP , the current suppression period T IB , the positive feeding period T P and the reverse feed period T N The relationship between N / (T P +T N )}>{T IB / (T IP +T IB )} and The positive feeding period T P The period of 2 / 3 or more of the current non-suppression period T IP A program characterized by executing a function of controlling the number of According to this configuration, in an arc welding method in which forward and reverse feeding of the tip of the wire is cyclically repeated, it is possible to achieve both a stable penetration depth and a reduction in spatter.

[0151] (13) In gas metal arc welding, in which a welding current is supplied to a welding wire, A forward feed period T during which the tip of the welding wire moves from the uppermost end, which is the position farthest from the base metal, to the lowermost end, which is the position closest to the base metal. P and a reverse feed period T N While controlling the feed speed of the welding wire so that the welding wire is fed toward the base metal with periodic switching of Based on at least a tip position signal of the welding wire or a feed speed signal of the welding wire, The welding current is kept in a current non-suppression period T IP or current suppression period T IB A welding method for performing gas metal arc welding while performing welding control by switching to and controlling the welding The positive feeding period T P and the reverse feed period TN The combined period is considered as one cycle, and its frequency f is 50 to 150 Hz. The current non-suppression period T IP The average current I P-AVE and the current suppression period T IB The average current I B-AVE The relationship is 0.65≦I P-AVE / (I P-AVE +I B-AVE )≦0.90, A wave height Wh, which is a change width of the tip position of the welding wire between the uppermost end and the lowermost end, is set to 14 to 35% of a tip-base metal distance of the welding wire, Any of the current non-suppression periods T IP and the current suppression period T immediately thereafter. IB The relationship between these two is 0.30≦T IB / (T IP +T IB )≦0.60, The positive feeding period T P and the reverse feed period T N The relationship is 0.40≦T N / (T P +T N )≦0.70, and, The current non-suppression period T IP , the current suppression period T IB , the positive feeding period T P and the reverse feed period T N The relationship between N / (T P +T N )}>{T IB / (T IP +T IB )} and The positive feeding period T P The period of 2 / 3 or more of the current non-suppression period T IP The welding method is characterized in that the welding control is performed so that the welding current is within the range of 0.5 to 100 .mu.m. According to this configuration, in an arc welding method in which forward and reverse feeding of the tip of the wire is cyclically repeated, it is possible to achieve both a stable penetration depth and a reduction in spatter.

[0152] (14) In additive manufacturing using gas metal arc welding, which supplies welding current to a welding wire, A forward feed period T during which the tip of the welding wire moves from the uppermost end, which is the position farthest from the base metal, to the lowermost end, which is the position closest to the base metal. P and a reverse feed period T N While controlling the feed speed of the welding wire so that the welding wire is fed toward the base metal with periodic switching of Based on at least a tip position signal of the welding wire or a feed speed signal of the welding wire, The welding current is kept in a current non-suppression period T IP or current suppression period T IB An additive manufacturing method for performing additive manufacturing while performing welding control by switching to and controlling the welding, The positive feeding period T P and the reverse feed period T N The combined period is considered as one cycle, and its frequency f is 50 to 150 Hz. The current non-suppression period T IP The average current I P-AVE and the current suppression period T IB The average current I B-AVE The relationship is 0.65≦I P-AVE / (I P-AVE +I B-AVE )≦0.90, A wave height Wh, which is a change width of the tip position of the welding wire between the uppermost end and the lowermost end, is set to 14 to 35% of a tip-base metal distance of the welding wire, Any of the current non-suppression periods T IP and the current suppression period T immediately thereafter. IB The relationship between these two is 0.30≦T IB / (T IP +T IB )≦0.60, The positive feeding period T P and the reverse feed period T N The relationship is 0.40≦T N / (T P +T N )≦0.70, and, The current non-suppression period T IP , the current suppression period T IB , the positive feeding period T P and the reverse feed period T N The relationship between N / (T P +T N )}>{T IB / (T IP +T IB )} and The positive feeding period T P The period of 2 / 3 or more of the current non-suppression period T IP The additive manufacturing method is characterized in that the welding control is performed so that the welding area is occupied by the welding area. According to this configuration, in an additive manufacturing method using an arc welding method in which forward and reverse feeding of the tip of the wire is cyclically repeated, it is possible to achieve both a stable penetration depth and reduced spatter. [Explanation of symbols]

[0153] 50 Welding System 100 Welding Wire 110 Welding Robot 111 Welding torch 120 Welding control device 140 Welding power source 150 Controller 200 Workpiece (base material) f frequency Fave Average feed speed Fw Feed speed command signal (feed speed signal) I B-AVE Current suppression period T IB Average current of I P-AVE Current non-suppression period T IP Average current of I P1 First welding current setting I P2 Second welding current setting T C Current Control Section T D Falling section T IB Current suppression period T IP Non-current suppression period T N Reverse feeding period T P Forward feeding period T U Rise interval Wh wave height

Claims

1. In gas metal arc welding, in which a welding current is supplied to a welding wire, A forward feed period T is a period during which the tip of the welding wire moves from the uppermost end, which is the position farthest from the base metal, to the lowermost end, which is the position closest to the base metal. P and a reverse feed period T N While controlling the feed speed of the welding wire so that the welding wire is fed toward the base metal with periodic switching of Based on at least a tip position signal of the welding wire or a feed speed signal of the welding wire, The welding current is maintained for a current non-suppression period T IP or current suppression period T IB A welding control method for switching and controlling a welding The normal feeding period T P and the reverse feed period T N The combined period is one period, and the frequency f is 50 to 150 Hz. The current non-suppression period T IP The average current I P-AVE and the current suppression period T IB The average current I B-AVE The relationship is 0.65≦I P-AVE / (I P-AVE +I B-AVE )≦0.90, a wave height Wh, which is a change width of the tip position of the welding wire between the uppermost end and the lowermost end, is set to 14 to 35% of a tip-base metal distance of the welding wire; Any current non-suppression period T IP and the current suppression period T IB The relationship is 0.30≦T IB / (T IP +T IB )≦0.60, The normal feeding period T P and the reverse feed period T N The relationship is 0.40≦T N / (T P +T N )≦0.70, and, The current non-suppression period T IP , the current suppression period T IB , the positive feeding period T P and the reverse feed period T N The relationship between N / (T P +T N ) 〉 {T IB / (T IP +T IB ) and The normal feeding period T P The current non-suppression period T IP A welding control method comprising the steps of:

2. 2. The welding control method according to claim 1, wherein a feed speed of the welding wire when the tip of the welding wire is located at the uppermost end or the lowermost end is set to a predetermined average feed speed.

3. The current non-suppression period T IP is the current suppression period T IB The immediately following rising section T U , the current suppression period T IB The previous falling section T D , and the rising section T U and the falling interval T D Current control section T other than C It consists of: The rising section T U is the current non-suppression period T IP 20% or less of the falling interval T D is the current non-suppression period T IP The welding control method according to claim 1 or 2, wherein the welding speed is 20% or less.

4. The current control section T C At least two welding current setting values ​​I P1 , I P2 having When the uppermost end position of the welding wire is set as a reference and set to 0 deg, The welding current setting value I P1The end position of the range is set to a range of 20 deg or less, The welding current setting value I P2 The welding control method according to claim 3, wherein the end position of the range is set in the range of 135 to 220 deg.

5. The welding current setting value I P2 The end of the range is the current control section T C The terminus of The welding current setting value I P2 When the end position of the range is X deg, The current suppression period T IB The welding control method according to claim 4, wherein the end position of the welding is set in a range of (X+100) to (X+220) degrees.

6. The welding current setting value I P1 The set current is 250 to 600 A. The welding current setting value I P2 The welding control method according to claim 4 or 5, wherein the set current is 300 to 650 A.

7. The current control section T C The welding control method according to any one of claims 4 to 6, further comprising providing an external characteristic of the welding power source.

8. The average volume of the droplet detached from the tip of the welding wire is 1.7 to 5.0 mm 3 The welding control method according to any one of claims 1 to 7,

9. In gas metal arc welding, in which a welding current is supplied to a welding wire, A forward feed period T is a period during which the tip of the welding wire moves from the uppermost end, which is the position farthest from the base metal, to the lowermost end, which is the position closest to the base metal. P and a reverse feed period T N While controlling the feed speed of the welding wire so that the welding wire is fed toward the base metal with periodic switching of Based on at least a tip position signal of the welding wire or a feed speed signal of the welding wire, The welding current is maintained for a current non-suppression period T IP or current suppression period T IB A welding control device for switching and controlling The normal feeding period T P and the reverse feed period T N The combined period is one period, and the frequency f is 50 to 150 Hz. The current non-suppression period T IP The average current I P-AVE and the current suppression period T IB The average current I B-AVE The relationship is 0.65≦I P-AVE / (I P-AVE +I B-AVE )≦0.90, a wave height Wh, which is a change width of the tip position of the welding wire between the uppermost end and the lowermost end, is set to 14 to 35% of a tip-base metal distance of the welding wire; Any current non-suppression period T IP and the current suppression period T IB The relationship is 0.30≦T IB / (T IP +T IB )≦0.60, The normal feeding period T P and the reverse feed period T N The relationship is 0.40≦T N / (T P +T N )≦0.70, and, The current non-suppression period T IP , the current suppression period T IB , the positive feeding period T P and the reverse feed period T N The relationship between N / (T P +T N ) 〉 {T IB / (T IP +T IB ) and The normal feeding period T P The current non-suppression period T IPA welding control device having a function of controlling the welding time so that the welding speed is within the predetermined range.

10. A welding power source comprising the welding control device according to claim 9.

11. A welding system comprising the welding control device according to claim 9 or the welding power source according to claim 10.

12. In gas metal arc welding, in which a welding current is supplied to a welding wire, A forward feed period T is a period during which the tip of the welding wire moves from the uppermost end, which is the position farthest from the base metal, to the lowermost end, which is the position closest to the base metal. P and a reverse feed period T N While controlling the feed speed of the welding wire so that the welding wire is fed toward the base metal with periodic switching of Based on at least a tip position signal of the welding wire or a feed speed signal of the welding wire, The welding current is maintained for a current non-suppression period T IP or current suppression period T IB A computer of a welding system including at least a welding control device for switching between and controlling the welding The welding control device, The normal feeding period T P and the reverse feed period T N The combined period is one period, and the frequency f is 50 to 150 Hz. The current non-suppression period T IP The average current I P-AVE and the current suppression period T IB The average current I B-AVE The relationship is 0.65≦I P-AVE / (I P-AVE +I B-AVE )≦0.90, a wave height Wh, which is a change width of the tip position of the welding wire between the uppermost end and the lowermost end, is set to 14 to 35% of a tip-base metal distance of the welding wire; Any current non-suppression period T IPand the current suppression period T IB The relationship is 0.30≦T IB / (T IP +T IB )≦0.60, The normal feeding period T P and the reverse feed period T N The relationship is 0.40≦T N / (T P +T N )≦0.70, and, The current non-suppression period T IP , the current suppression period T IB , the positive feeding period T P and the reverse feed period T N The relationship between N / (T P +T N ) 〉 {T IB / (T IP +T IB ) and The normal feeding period T P The current non-suppression period T IP A program characterized by executing a function of controlling the number of

13. In gas metal arc welding, in which a welding current is supplied to a welding wire, A forward feed period T is a period during which the tip of the welding wire moves from the uppermost end, which is the position farthest from the base metal, to the lowermost end, which is the position closest to the base metal. P and a reverse feed period T N While controlling the feed speed of the welding wire so that the welding wire is fed toward the base metal with periodic switching of Based on at least a tip position signal of the welding wire or a feed speed signal of the welding wire, The welding current is maintained for a current non-suppression period T IP or current suppression period T IB A welding method for performing gas metal arc welding while performing welding control by switching to and controlling the welding The normal feeding period T Pand the reverse feed period T N The combined period is one period, and the frequency f is 50 to 150 Hz. The current non-suppression period T IP The average current I P-AVE and the current suppression period T IB The average current I B-AVE The relationship is 0.65≦I P-AVE / (I P-AVE +I B-AVE )≦0.90, a wave height Wh, which is a change width of the tip position of the welding wire between the uppermost end and the lowermost end, is set to 14 to 35% of a tip-base metal distance of the welding wire; Any current non-suppression period T IP and the current suppression period T IB The relationship is 0.30≦T IB / (T IP +T IB )≦0.60, The normal feeding period T P and the reverse feed period T N The relationship is 0.40≦T N / (T P +T N )≦0.70, and, The current non-suppression period T IP , the current suppression period T IB , the positive feeding period T P and the reverse feed period T N The relationship between N / (T P +T N ) 〉 {T IB / (T IP +T IB ) and The normal feeding period T P The current non-suppression period T IP The welding method is characterized in that the welding control is performed so that the welding current is within the range of 0.5 to 100 .mu.m.

14. In additive manufacturing, gas metal arc welding is used to supply welding current to a welding wire. A forward feed period T is a period during which the tip of the welding wire moves from the uppermost end, which is the position farthest from the base metal, to the lowermost end, which is the position closest to the base metal. P and a reverse feed period T N While controlling the feed speed of the welding wire so that the welding wire is fed toward the base metal with periodic switching of Based on at least a tip position signal of the welding wire or a feed speed signal of the welding wire, The welding current is maintained for a current non-suppression period T IP or current suppression period T IB An additive manufacturing method for performing additive manufacturing while performing welding control by switching to and controlling the welding, The normal feeding period T P and the reverse feed period T N The combined period is one period, and the frequency f is 50 to 150 Hz. The current non-suppression period T IP The average current I P-AVE and the current suppression period T IB The average current I B-AVE The relationship is 0.65≦I P-AVE / (I P-AVE +I B-AVE )≦0.90, a wave height Wh, which is a change width of the tip position of the welding wire between the uppermost end and the lowermost end, is set to 14 to 35% of a tip-base metal distance of the welding wire; Any current non-suppression period T IP and the current suppression period T IB The relationship is 0.30≦T IB / (T IP +T IB )≦0.60, The normal feeding period T P and the reverse feed period T N The relationship is 0.40≦T N / (T P +T N )≦0.70, and, The current non-suppression period T IP , the current suppression period T IB , the positive feeding period T P and the reverse feed period T N The relationship between N / (T P +T N ) 〉 {T IB / (T IP +T IB ) and The normal feeding period T P The current non-suppression period T IP The additive manufacturing method is characterized in that the welding control is performed so that the welding area is occupied by the welding area.

Citation Information

Patent Citations

  • Consumable electrode type pulse arc welding method

    JP1985180675A

  • Cold metal transfer welding method and welding equipment

    JP2008542027A

  • Pulsed arc welding control method

    JP2014083553A

  • Welding power source, welding system, control method of welding power source, and program

    JP2020049506A

  • Welding power source, welding system, welding power source control method, and program

    WO2020067074A1