Method for manufacturing hollow core fiber and method for manufacturing preform for hollow core fiber

The method addresses the challenge of precise manufacturing in anti-resonant hollow core fibers by using oval-shaped preforms and controlled thermal processing, achieving high precision and reproducibility in fiber production with reduced optical attenuation and deformation.

JP7582982B2Active Publication Date: 2024-11-13HERAEUS QUARZGLAS GMBH & CO KG
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2021576503
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-17
Filing Date
2020-07-15
Publication Date
2024-11-13
Estimated Expiration
2040-07-15

AI Technical Summary

Technical Problem

Conventional methods for manufacturing anti-resonant hollow core fibers face challenges in achieving precise structural elements and accurate positioning, particularly due to complex geometries and sensitivity to dimensional tolerances, leading to difficulties in producing fibers with suppressed higher-order modes and consistent single-mode operation.

Method used

A manufacturing method involving the use of primary preforms with tubular anti-resonant elements having an oval cross-sectional shape and controlled thermal processing, combined with precise machining and the application of dopants to reduce viscosity and enhance thermal stability, ensures accurate positioning and reproducible fiber production.

Benefits of technology

This method enables the production of anti-resonant hollow core fibers with improved precision and reproducibility, maintaining single-mode operation over a wide propagation range while reducing optical attenuation and deformation errors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582982000001
    Figure 0007582982000001
  • Figure 0007582982000002
    Figure 0007582982000002
  • Figure 0007582982000003
    Figure 0007582982000003
Patent Text Reader

Abstract

A method for manufacturing an antiresonant hollow-core fiber having a hollow core extending along the fiber's longitudinal axis and an inner cladding region including a plurality of antiresonant elements and surrounding the hollow core is known. The known method includes the steps of providing a cladding tube having an inner bore and a longitudinal axis, a cladding wall defined by an inner and outer sides extending along the longitudinal axis, providing a plurality of antiresonant element preforms, positioning the antiresonant element preforms at target locations inside the cladding wall to form a primary preform having a hollow core region and an inner cladding region, further processing the primary preform to form a secondary preform of the hollow-core fiber, the further processing including drawing, and drawing the secondary preform to form the hollow-core fiber. Starting from this, in order to achieve high precision and accurate positioning of the antiresonant elements in a sufficiently stable and reproducible manner, according to the present invention, after drawing of the primary preform, at least a portion of the former tubular antiresonant element preform of the primary preform is drawn along the longitudinal axis A. L and minor axis A K and having an oval outer cross-sectional shape with an axial length ratio A. L / A K is in the range of 1.01 to 1.27, and the minor axis A K runs radially from the longitudinal axis of the cladding tube.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Background technology The present invention provides a method for making an anti-resonant hollow-core fiber having a hollow core extending along a longitudinal axis of the fiber and a cladding region surrounding the hollow core that includes a number of anti-resonant elements, comprising: (a) providing a cladding tube having an internal cladding bore and a cladding longitudinal axis, the cladding wall being defined by an interior and an exterior and extending along the cladding longitudinal axis; (b) providing a number of tubular anti-resonant element preforms; (c) placing the anti-resonant element preform at a target location inside the cladding wall to form a primary preform having a hollow core region and an inner cladding region; (d) further processing the primary preform into a secondary preform from which a hollow-core fiber is drawn, the further processing steps including drawing and, optionally, (i) Collapse, (ii) collapsing and simultaneously stretching; (iii) Collapse of additional cladding material; (iv) Collapse and subsequent stretching of additional cladding material; (v) collapsing and simultaneously stretching additional cladding material; further processing, which includes performing one or more of the following thermoforming processes once or repeatedly; (e) drawing the secondary preform to form a hollow-core fiber; The present invention relates to a manufacturing method comprising the steps of:

[0002] The present invention further relates to a method for making an anti-resonant hollow-core fiber preform having a hollow core extending along a longitudinal axis of the fiber and a cladding region surrounding the hollow core, the cladding region including a plurality of anti-resonant elements, the method comprising: (a) providing a cladding tube having an internal cladding bore and a cladding longitudinal axis, the cladding wall being defined by an interior and an exterior and extending along the cladding longitudinal axis; (b) providing a number of tubular anti-resonant element preforms; (c) placing the anti-resonant element preform at a target location inside the cladding wall to form a primary preform having a hollow core region and an inner cladding region; (d) further processing the primary preform into a secondary preform for a hollow core fiber, the further processing including drawing and, optionally, (i) Collapse, (ii) collapsing and simultaneous stretching; (iii) Collapse of additional cladding material; (iv) Collapse and subsequent stretching of additional cladding material; (v) collapsing and simultaneously stretching additional cladding material; The thermoforming process may include performing one or more of the following steps once or repeatedly:

[0003] Conventional single-mode optical fibers made from solid materials have a glass core surrounded by a cladding region made of glass with a low refractive index. The propagation of light is based on total internal reflection between the core and cladding regions. However, the interaction of the guided light with the solid material is associated with increased delay times in data transmission and a relatively low damage threshold for energetic radiation.

[0004] These drawbacks are avoided or mitigated by "hollow-core fibers", whose core consists of a vacuum cavity filled with gas or liquid. In hollow-core fibers, the interaction of light with the glass is reduced compared to solid-core fibers. Since the refractive index of the core is smaller than that of the cladding, light propagation by total internal reflection is not possible and light is usually considered to leak from the core into the cladding. Depending on the physical mechanism of light propagation, hollow-core fibers are distinguished into "photonic bandgap fibers" and "antiresonant reflecting fibers".

[0005] In a "photonic bandgap fiber", a hollow core region is surrounded by a cladding that contains a periodic arrangement of small hollow channels. The periodic structure of the hollow channels in the cladding has an effect called "photonic bandgap" in semiconductor technology, which means that light in a certain wavelength range that scatters into the cladding structure cannot spread laterally within the cladding because it interferes constructively in the central cavity based on Bragg reflection.

[0006] In hollow-core fiber embodiments, called "antiresonant hollow-core fibers" (ARHCF), a hollow core region is surrounded by an inner cladding region and is located within so-called "antiresonant elements" (or "antiresonant elements"; abbreviation "AREs"). The walls of the antiresonant elements, evenly distributed around the hollow core, function as an antiresonantly operated Fabry-Perot cavity that can reflect incoming light and pass it through to the fiber core.

[0007] This fiber technology allows for reduced optical attenuation, a very wide transmission spectrum (even in the ultraviolet or infrared wavelength ranges), and low latency during data transmission.

[0008] Potential applications of hollow-core fibers lie in the fields of high-performance beam control for data transmission, material processing, modal filtering, and nonlinear optics, especially for generating supercontinuums from the extreme ultraviolet to the infrared wavelength range.

[0009] Background technology A drawback of anti-resonant hollow-core fibers is that higher order modes are not automatically suppressed, so they often do not become purely single mode over long transmission distances, resulting in poor quality output beams.

[0010] Francesco Poletti, "Nested antiresonant nodeless hollow core fiber"; Optics Express, Vol. 22, No. 20 (2014); DOI: 10.1364 / OE 22.023807, proposes a fiber design in which the antiresonant element is not formed as a simple single structural element, but is composed of multiple structural elements nested within each other. The nested antiresonant elements are designed in such a way that the higher-order core modes are phase-matched to the cladding modes and suppressed, but the fundamental core mode is not suppressed. This ensures that the fundamental core mode always propagates, making the hollow core fiber effectively single-mode over a limited wavelength band.

[0011] Efficient mode suppression depends on the central wavelength of the propagating light as well as on structural parameters of the fiber design, such as the radius of the hollow core and the diameter difference of the nested ring structures within the anti-resonant element.

[0012] From EP 3136143 A1 an anti-resonant hollow-core fiber (called "hollow-core fiber without band gap") is known, whose core is capable of propagating other modes besides the fundamental mode. For this purpose, the core is surrounded by an inner cladding with "anti-resonant elements" that provide phase matching of the anti-resonant mode and higher modes. The production of hollow-core fibers is carried out by the so-called "stack and draw" method, in which a preform is formed by arranging and fixing the starting elements in an axially parallel collection, and then drawing the preform. Here, a cladding tube with a hexagonal inner cross section is used, to whose inner edge six so-called "ARE preforms" (anti-resonant element preforms) are fixed. The hollow-core fiber is formed by drawing the preform in two stages.

[0013] From International Patent Application 2018 / 169487 A1 a method for manufacturing a preform for an antiresonant hollow core fiber is known, in which a first cladding region is made up of a number of rods and a second cladding region is made up of a number of tubes surrounded by a cladding tube. The rods, tubes and cladding tube are joined by a "stack and draw" method to form the preform. Before drawing the preform, sealing is performed by applying a sealant to the preform ends. As sealant a UV adhesive is used, for example.

[0014] Problem to be solved by the invention Anti-resonant hollow-core fibers, and especially those with nested structural elements, have complex internal geometries that make them difficult to manufacture accurately and reproducibly. This is compounded by the fact that resonance or anti-resonance conditions cannot be met without small dimensional tolerances on the magnitude of the operating wavelength of the propagating light. Deviations from the target shape can be caused during the construction of the fiber preform, but can also occur during the fiber drawing process due to inappropriate deformations that are not to scale.

[0015] In the known "stack and draw" method, a large number of elements have to be joined in precise positions. For example, to manufacture a hollow-core fiber of the "NANF" design known from the literature mentioned at the beginning, six anti-resonant element preforms, each consisting of an anti-resonant element outer tube (abbreviated as "ARE outer tube") and an anti-resonant element inner tube (abbreviated as "ARE inner tube") welded to one side of the inner cladding surface of the ARE outer tube, have to be attached inside the cladding tube.

[0016] In order to achieve low attenuation values ​​and wide propagation ranges, the azimuthal position of the anti-resonant element inside the cladding tube is also important, in addition to the uniform wall thickness of the anti-resonant element walls, which cannot be easily achieved by the "stack and draw" method. It is an object of the present invention to provide a manufacturing method for achieving anti-resonant hollow-core fibers at low cost, avoiding the limitations of conventional manufacturing methods.

[0017] In particular, it is an object of the present invention to provide a method for manufacturing anti-resonant hollow-core fibers and anti-resonant hollow-core fiber preforms, which makes it possible to achieve high precision of the structural elements and exact positioning of the anti-resonant elements within the fiber in a sufficiently stable and reproducible manner.

[0018] Furthermore, the drawbacks of the conventional "stack and draw" method, in which the required construction precision, in particular the uniform wall thickness and precise positioning of the anti-resonant elements in defined azimuthal positions, are not easily achievable, must be avoided as far as possible.

[0019] Summary of the Invention With regard to a method for producing an antiresonant hollow-core fiber, the object is achieved by starting from a method of the type mentioned at the beginning, and in accordance with the invention, by providing a method for producing a hollow-core fiber in which, after the drawing in step (d), at least a part of the original tubular antiresonant element preform of the primary preform has a cross-sectional longitudinal axis A L and cross-sectional minor axis A K and having an oval outer cross-sectional shape with an axial length ratio A. L / A K is in the range of 1.01 to 1.27, and the cross-sectional minor axis A K is solved by passing radially from the longitudinal axis of the cladding tube.

[0020] The starting point for the manufacture of an anti-resonant hollow-core fiber is again a preform, referred to as a "primary preform". The manufacture of the primary preform typically includes the attachment and connection of an anti-resonant element preform and a cladding tube. The primary preform can be drawn to form a hollow-core fiber, but is typically further processed to produce a preform, referred to here as a "secondary preform". If necessary, the hollow-core fiber is produced by drawing this secondary preform. Alternatively, the primary or secondary preform is surrounded by one or more outer cylinders, forming a coaxial assembly of components, which is directly drawn to form the hollow-core fiber. In this case, the general term "preform" is to be understood as the name of the component or coaxial assembly of components from which the hollow-core fiber is finally drawn.

[0021] The cladding material may be added, for example, by collapsing an outer cylinder onto the primary or secondary preform, and the coaxial arrangement of the preform and outer cylinder may or may not be stretched upon collapse of the outer cylinder, with the antiresonant element preform either changing its shape or configuration or remaining unchanged.

[0022] The production of the secondary preform involves multiple steps in which the initial elements of the hollow-core fiber are produced and positioned relative to one another, and at least one hot forming process. Since each initial element has a certain deviation from its target shape, and each positioning and deformation step inevitably introduces shape deviations, the finished preform will have absolute shape errors. Especially in the hot forming of glass, even small deviations from the optimal heating zone temperature profile, which is usually cylindrically symmetric, can lead to undesirable and non-reproducible deformations. Such deformations are also due to the pressure and temperature conditions during the drawing or fiber drawing process and are very difficult to avoid.

[0023] The method according to the present invention is aimed at compensating for the deforming effects of such pressure and temperature conditions during the drawing and fiber drawing processes.

[0024] For this purpose, the drawing of the primary preform is performed in such a way that, after completion of the drawing process, at least a portion of the original tubular and round in cross-section of the primary preform's anti-resonant element preform has an oval outer cross-sectional shape.

[0025] In drawing the primary preform, additional cladding material may or may not be applied, and the result of the drawing process is a secondary preform or another semi-finished product, which must be further processed as required to become a secondary preform.

[0026] It has been found to be advantageous if most, and preferably all, of the structural elements of the original primary preform are originally round, but are changed in shape during the drawing process, so that after the drawing process they have a non-circular, oval, optimally elliptical cross-sectional shape, since further shape changes occur during the subsequent fiber drawing process, resulting in the cavities with oval radial cross-sections being transformed into cavities with round radial cross-sections.

[0027] It has been found that the ellipticity of the cross-sectional shape of the stretched structural element, which is favorable for this correction, is described by the major and minor axes (in the cross section). Major axis A in the cross section L and the minor axis A of the cross section K The ratio of is in the range of 1.01 to 1.27. What is important here is the orientation of the oval on the inner cladding surface of the original cladding tube. That is, the cross-sectional minor axis A K passes through the radial direction, and the cross-sectional major axis A L is oriented tangentially to the original inner cladding surface.

[0028] The anti-resonant element preform may consist of a structural element, for example a simple tube element, or of several structural elements, for example nested within each other, forming in the simplest case an outer ARE tube, into which an inner ARE tube is inserted.

[0029] In a particularly preferred method relating to an anti-resonant element preform consisting of a simple tubular structural element, the tubular element has an oval, preferably elliptical, outer cross-sectional shape and an axial length ratio A L / A K is in the range of 1.07 to 1.27.

[0030] Another particularly preferred method involves an anti-resonant element preform constructed from a plurality of nested structural elements, including at least one outer ARE tube and at least one inner ARE tube running within the outer ARE tube parallel to the longitudinal axis of the outer ARE tube.

[0031] In such an anti-resonant element preform, the inner ARE tube is fixed inside the outer ARE tube wall. If the contact area between the inner and outer ARE tubes is too small, surface tension during the hot forming process can cause delamination and decentering of the inner ARE tube inside the outer ARE tube. To counter this, the outer ARE tube has an oval, preferably elliptical, outer cross-sectional shape with an axial length ratio A L / A K is in the range of 1.07 to 1.27, the ARE inner tube has an oval, preferably elliptical, outer cross-sectional shape, and the axial length ratio A L / A K It has been found to be advantageous if is in the range of 1.01 to 1.05.

[0032] The relatively large ellipticity of the ARE outer tube increases the contact area with the inner capillary.

[0033] The primary preform before stretching preferably has an outer diameter in the range of 20 to 70 mm, particularly preferably in the range of 30 to 70 mm.

[0034] This is because the larger the diameter, the slower the tracking speed during stretching, and therefore the longer each axial portion of the preform is exposed to the high temperature of the heating zone. However, if the tracking speed during stretching is too slow, the structural elements of the anti-resonance element preform will be deformed. Therefore, the diameter of the primary preform is preferably 70 mm or less. Also, the diameter of the primary preform is preferably 20 mm or more, and particularly preferably 30 mm or more. This is because it has been found that if the diameter is smaller than this, the thermal inertia of the preform is too small to adjust the temperature change in the heating zone.

[0035] In a preferred method, during drawing, the primary preform is continuously fed into the heating zone at an infeed speed, softened in zones within the heating zone, and withdrawn from the heating zone at a withdrawal speed.

[0036] If the feed rate is too high, a temperature gradient may occur in the primary preform, which may result in different stretching properties of the antiresonant element preforms distributed in different radial positions therein. If the feed rate is too low, undesirable deformations of the antiresonant element preforms may occur. As a good compromise, it has been found to be advantageous to set the feed rate so that the throughput is at least 0.8 g / min, preferably in the range of 0.8 g / min to 85 g / min, particularly preferably in the range of 3.3 g / min to 85 g / min, and the average residence time in the heating zone is at least not more than 25 minutes, preferably in the range of 5 to 25 minutes.

[0037] The temperature of the heating zone during the thermoforming process should be as constant as possible, therefore advantageously temperature controlled heater elements are used during the thermoforming process according to step (d) whereby the target temperature is maintained with an accuracy of + / - 0.1°C.

[0038] This allows limiting temperature fluctuations in the heating zone to less than + / - 0.5°C.

[0039] A high drawing rate during drawing is desirable to avoid absolute shape errors, but a large drawing rate also leads to a correspondingly large deformation process and material movement, which can easily cause undesired deformations of the fine structural elements of the antiresonant element preform.

[0040] As a good compromise, it has proven advantageous to set the drawing ratio during drawing to a value lying in the range 1.05-10, preferably in the range 1.05-5.

[0041] In a preferred method variation, the positioning of the anti-resonant element preform and / or the drawing of the primary preform and / or the drawing of the hollow-core fiber includes a fastening and / or sealing step using an encapsulant or bonding material containing amorphous SiO2 particles.

[0042] The sealing or bonding material used for sealing or fastening contains amorphous SiO2 particles, for example, incorporated in a dispersion. This material is applied between the surfaces to be joined or sealed and is usually in the form of a paste when used. Drying at low temperatures removes the dispersion partially or completely and hardens the material. The sealing or bonding material, and especially the hardened SiO2-containing sealing or bonding material obtained after drying, meets the requirements for fastening and compaction. The temperature required for drying is 300 °C or less, which helps to maintain the dimensional stability of the preform and avoids adverse effects due to heat. Heating to high temperatures, for example around 800 °C, during drawing of the preform into a hollow-core fiber, leads to further thermal solidification of the sealing or bonding material, which is also suitable for forming frosted or clear glass. This occurs by sintering or vitrification, where sintering to frosted glass requires a relatively lower temperature and / or shorter heating time than vitrification to full transparency. The sealing or bonding material can therefore be fully compacted by heating and can be vitrified by heating in a thermoforming process.

[0043] During the thermoforming process, the sealing or bonding material will not decompose and will release almost no impurities, therefore it is characterized by temperature stability and purity during the thermoforming process, and avoids deformation due to different thermal expansion coefficients.

[0044] Sealing and bonding materials may also be advantageously used to seal the open ends of the antiresonant element preform and / or the annular gaps between the individual structural and / or tubular elements of the antiresonant element preform during drawing of the primary preform and / or drawing of the hollow-core fiber.

[0045] In this manner, individual components of the primary preform and / or secondary preform may be subjected to different internal pressures during the drawing or fiber drawing process.

[0046] The positioning accuracy of the preform on the inner cladding surface of the cladding tube is further improved by finishing the inside of the cladding tube and / or the outside of the cladding tube and / or the inside of the outer ARE tube and / or the outside of the outer ARE tube by machining, in particular by drilling, sawing, milling, grinding, honing and / or polishing.

[0047] These processing techniques provide more precise and extremely fine structures than other known deformation techniques that use heat and pressure, and avoid surface contamination by forming tools such as nozzles, presses or casting dies.

[0048] This machining also preferably includes structuring the inside of the cladding tube in the target location area of ​​the anti-resonant element preform, so that the anti-resonant element preform is provided with longitudinal structures extending towards the cladding tube longitudinal axis, for example longitudinal slots and / or longitudinal grooves running parallel to the cladding tube longitudinal axis, which are preferably finished by drilling, sawing, milling, cutting or grinding.

[0049] The longitudinal structures extending along the cladding tube longitudinal axis are used as positioning aids for the anti-resonance element preform, which facilitates placing the anti-resonance element preform in a defined position inside the cladding tube.

[0050] The positioning accuracy of the preform on the inner cladding surface of the cladding tube is improved if the upper end face of the structural element is positioned at the target position using a positioning template.

[0051] The positioning template has, for example, a shaft projecting into the cladding tube inner bore, on which are provided holding elements in the form of radially outwardly pointing holding arms.

[0052] The star-shaped arrangement of the structurally determined holding elements facilitates accurate positioning of the anti-resonant element preforms in the respective target positions and fixing them, for example by the above-mentioned sealing or bonding material, with the positioning template preferably being used only in the area of ​​the cladding tube front, preferably in the area of ​​both cladding tube fronts.

[0053] It has further been demonstrated that it is advantageous to heat and soften multiple components of the preform made of silica glass together during drawing of the primary preform according to step (d) and / or during drawing of the hollow-core fiber according to step (e), wherein the silica glass of at least some of the preform components contains at least one dopant that reduces the viscosity of the silica glass.

[0054] The components of the primary preform include a cladding tube and an anti-resonant element preform disposed therein, and the secondary preform includes additional cladding material, which is provided, for example, in the form of an outer cylinder or cylinders, and collapsed onto the primary preform.

[0055] As dopants for reducing the viscosity of silica glass, preferably fluorine, chlorine and / or hydroxyl groups are used.

[0056] Dopants can avoid or reduce stress by allowing the adjustment of the thermal expansion coefficient of adjacent preform components. Dopants can also be used to reduce the thermal stability of one component and increase the stability of an adjacent component.

[0057] For example, it has proven to be advantageous if, at a measuring temperature of 1250°C, the silica glass of the cladding tube has a viscosity at least 0.5 dPa·s higher than the silica glass of the additionally installed cladding material, preferably at least 0.6 dPa·s higher (viscosity expressed as logarithmic value in dPa·s).

[0058] In particular, with regard to the low optical attenuation and wide optical transmission bandwidth of hollow-core fibers, it has proven to be particularly advantageous if the anti-resonant elements are arranged in odd symmetry around the hollow core.

[0059] In a preferred method, tubular structural elements are provided, at least some of which have a wall thickness in the range of 0.2-2 mm, preferably in the range of 0.25-1 mm, thereby further improving the positioning accuracy of the preform in the cladding tube. The cladding tube is then provided with an outer diameter in the range of 90-250 mm, preferably in the range of 120-200 mm. These components each have a length of at least 1 m, which is a relatively voluminous structural element for forming an anti-resonant element. This allows for easy handling. Furthermore, if the cladding tube and the structural element are arranged vertically, and the structural elements are positioned and fixed at their respective upper end faces in their target positions, for example by using the above-mentioned sealing or bonding material, and additionally or alternatively by using the above-mentioned positioning template, the parallelism and vertical alignment of the longitudinal axes of the structural elements are supported by gravity.

[0060] The above-stated technical problem with regard to the method for producing a hollow-core fiber preform can be solved by starting from a method of the type mentioned at the beginning, in accordance with the present invention, in that after the drawing in step (d), at least a part of the original tubular anti-resonator element preform of the primary preform has a cross-sectional longitudinal axis A L and cross-sectional minor axis A K and having an oval outer cross-sectional shape with an axial length ratio A. L / A K is in the range of 1.01 to 1.27, and the cross-sectional minor axis A K is solved by passing radially from the longitudinal axis of the cladding tube.

[0061] In drawing the primary preform, additional cladding material is applied or no additional cladding material is applied. The result of the drawing process is a secondary preform or another semi-finished product in the form of a drawn primary preform, which, if necessary, needs to be further processed into a secondary preform. In both cases, the drawn primary preform is characterized in that at least a part of the antiresonant element preform has an oval cross-sectional shape, which is suitable for counteracting deformations that may occur when drawing the secondary preform into a hollow-core fiber, on the one hand, and on the other hand, for enlarging the contact area between the nested structural elements, thereby further increasing the mechanical stability. This method allows for a precise production of hollow-core fibers.

[0062] The procedures for manufacturing the preform are described in detail above in connection with the manufacture of hollow-core fibers, and those descriptions are incorporated herein by reference.

[0063] definition The following are supplementary definitions for the individual steps and terms in the above-mentioned specification. These definitions are part of the present specification. If there is a substantial discrepancy between any of the following definitions and the rest of the specification, the definitions mentioned in the rest of the specification shall prevail.

[0064] anti-resonance element The anti-resonant element may be a simple structural element or a nested structural element of the hollow-core fiber. It has at least two walls with negative curvature (convex) or no curvature (flat, straight) as viewed in the direction of the hollow core. Typically, the anti-resonant element consists of a material transparent to the operating light, such as glass (especially doped or undoped SiO2), plastic (especially polymers), composite materials or crystalline materials.

[0065] Anti-resonant element preform / anti-resonant element pre-stage The anti-resonant element preform is a component or a preform component that becomes an anti-resonant element in a hollow-core fiber mainly by simple drawing in a fiber drawing process. The anti-resonant element pre-stage is a component or a preform component that becomes an anti-resonant element preform or directly an anti-resonant element only by deformation. The anti-resonant element preform can be a simple component or a nested component to which additional positioning aids can be fixed. The anti-resonant element preform is originally present in the primary preform.

[0066] The nested anti-resonant element preform forms an anti-resonant element nested within a hollow-core fiber. It is composed of an outer tube and at least one further structural element disposed within the inner bore of the outer tube. The further structural element may be a further tube that is in contact with the inner cladding surface of the outer tube. The outer tube is also referred to as the "anti-resonant element outer tube" or "ARE outer tube" for short, and the further tube is also referred to as the "anti-resonant element inner tube" or "ARE inner tube" for short, or "nested ARE inner tube".

[0067] In the case where the anti-resonant element preforms are nested multiple times within the inner bore of the nested inner ARE tube, at least one further structural element may be disposed, for example a third tube, which is in contact with the inner cladding surface of the nested inner ARE tube.

[0068] When the anti-resonant element preforms are nested multiple times, a distinction is made between a "nested outer ARE inner tube" and a "nested inner ARE inner tube" as necessary to distinguish between the multiple tubes disposed within the outer ARE tube.

[0069] The term "cross section" in connection with cylindrical anti-resonant element preforms and their cylindrical structural elements always refers to a cross section perpendicular to the respective cylinder longitudinal axis and, unless otherwise specified, refers to a cross section of the external contour of the tubular component (and not a cross section of the internal contour).

[0070] Further processing of the primary preform, in particular by a thermoforming process, can produce intermediate products in which the original anti-resonant element preform is present in a modified shape relative to its initial shape, which modified shape is also referred to herein as the anti-resonant element preform or anti-resonant element pre-stage.

[0071] Preform / Primary preform / Secondary preform / Core preform (Cane) A preform is a component from which an anti-resonant hollow-core fiber is drawn. It can be a primary preform or a secondary preform produced by further processing of a primary preform. A primary preform can be an assembly of at least one cladding tube and a preform or precursor for an anti-resonant element housed therein in a loosely or rigidly fixed manner. Further processing of a primary preform into a secondary preform from which a hollow-core fiber is drawn can be performed by: (i) stretching; (ii) Collapse; (iii) collapsing and simultaneous stretching; (iv) Collapse of additional cladding material; (v) Collapse and subsequent stretching of additional cladding material; (vi) collapsing and simultaneously stretching additional cladding material; The thermoforming process may include performing one or more of the following steps once or repeatedly:

[0072] In the literature, a core preform (English: cane) is a preform obtained by collapsing and / or stretching a primary preform. Usually, the core preform is covered with additional cladding material before or during the drawing of the hollow-core fiber.

[0073] Stretching / Collapse In drawing, the primary preform is stretched to an elongation. This drawing may be performed without simultaneous collapse. The drawing may be performed to scale, so that, for example, the shape and arrangement of the components of the primary preform are reflected in the final drawn product. However, in drawing, the primary preform may not be drawn to size, and the geometry may change.

[0074] Collapsing involves narrowing the internal bore or closing or narrowing the annular gap between the tubular components, and is usually accomplished in parallel with stretching.

[0075] Hollow core / inner cladding region / outer cladding region The assembly consisting of at least one cladding tube and the preform or precursor of the anti-resonant element housed therein in a loosely or rigidly fixed manner is also referred to herein as the "primary preform". This primary preform consists of a hollow core and a cladding region. This cladding region is also referred to as the "internal cladding region" when there is an "external cladding region" formed, for example by collapsing into the assembly, and it is necessary to distinguish between these cladding regions. The names "internal cladding region" and "external cladding region" are also used for the corresponding regions of the hollow-core fiber or intermediate product obtained by further processing of the primary preform.

[0076] The term "inside the tube" is also used as a synonym for "inner cladding surface of the tube," and the term "outside the tube" is also used as a synonym for "outer cladding surface of the tube." The term "internal bore" in reference to a tube does not imply that the internal bore is formed by a drilling operation.

[0077] Cutting processing A mechanical manufacturing method for isolating a workpiece, which means in particular turning, cutting, drilling, sawing, milling or grinding, which results in a longitudinal structure extending in the direction of the cladding tube longitudinal axis, which serves as a positioning aid for the anti-resonant element preform, which is accessible from the inside of the cladding tube and may extend through the entire cladding tube wall to the outside.

[0078] Particle size and particle size distribution The particle size and particle size distribution of SiO2 particles are 50 This value is read from a particle size distribution curve that shows the cumulative amount of SiO2 particles according to their size. The particle size distribution is 10 Value, D 50 Value, D 90 It is often characterized based on the value of D 10 The value indicates the particle size that does not reach 10% of the cumulative amount of SiO2 particles, and correspondingly, D 50 Value and D 90 indicates the particle size at which the cumulative amount of SiO2 particles does not reach 50% or 90%. The particle size distribution is detected by scattered light and laser diffraction spectroscopy according to ISO13320.

[0079] Working Example The present invention will be described in detail below based on embodiments with reference to the drawings. [Brief description of the drawings]

[0080] [Figure 1] FIG. 2 is a cross-sectional view of a primary preform for producing a secondary preform for a hollow core fiber, comprising a cladding tube and an anti-resonant element preform positioned and secured therein. [Diagram 2] 1 is a cross-sectional photograph of a secondary preform comprising a preformed anti-resonant element preform. [Diagram 3] FIG. 1 illustrates the processing steps from primary preform to anti-resonant hollow-core fiber. [Figure 4] 13 is a diagram for explaining the force ratio when heating and processing nested anti-resonant elements. FIG.

[0081] In the production of hollow-core fibers or preforms for hollow-core fibers, a large number of components have to be connected to one another. Furthermore, when carrying out a thermoforming process, it is advantageous to seal gaps and channels present in the preform. As is known from DE 10 2004 054 392 A1, SiO2-based sealants or bonding materials are used for joining or sealing. Here, by wet milling of silica glass powder particles, D 50 Value is about 5 μm and D 90 An aqueous slurry is produced containing amorphous SiO2 particles having a particle size distribution characterized by a mean particle size of about 23 μm. Amorphous SiO2 particles having a medium particle size of about 5 μm are mixed into this base slurry. The slurry used as a joint material has a solids content of 90% and is composed of at least 99.9% by weight of SiO2.

[0082] FIG. 1 shows a diagram of a primary preform 3 comprising a cladding tube 1 and a cladding tube wall 2, inside of which anti-resonant element preforms 4 are fixed at predefined azimuthal positions at equal intervals, in this embodiment there are six preforms 4, and in another preferred embodiment not shown there is an odd number of preforms.

[0083] The cladding tube 1 is made of silica glass and has a length of 1000 mm, an outer diameter of 27 mm and an inner diameter of 20 mm. The anti-resonant element preform 4 exists as a collection of nested structural elements consisting of an outer ARE tube 4a and an inner ARE tube 4b. The outer diameter of the outer ARE tube 4a is 6.2 mm and the outer diameter of the inner ARE tube 4b is 2.5 mm. The wall thickness of both structural elements (4a; 4b) is the same, 0.3 mm. The length of the outer ARE tube 4a and the inner ARE tube 4b is the same as the cladding tube length.

[0084] The cladding tube 1 is produced by a two-stage drawing process in a vertical drawing method without forming tools. In the first stage, an initial hollow cylinder made of glass is mechanically processed to set the final dimensions of the initial hollow cylinder. According to the final dimensions, the outer diameter is 90 mm and the diameter ratio of the outer diameter to the inner diameter is 2.5. In the first drawing process with a vertically oriented longitudinal axis, the initial cylinder is continuously fed into a heating zone with a heating zone length of 200 mm, in which it is softened in zones, from which an intermediate cylinder is drawn. In the second drawing process with a vertically oriented longitudinal axis, this intermediate cylinder is continuously fed into another heating zone with a heating zone length of 100 mm, in which it is softened in zones, from which a tubular string is drawn. The length of this tubular string is shortened to obtain the cladding tube.

[0085] The anti-resonant element preform 4 is fixed to the inside of the cladding tube 1 by means of a SiO2 based bonding material 5.

[0086] The bonding material 5 is applied locally to the end face area of ​​the cladding inner cladding surface and the anti-resonant element preforms are placed thereon using a positioning template in which a star-shaped arrangement of holding arms for the individual anti-resonant element preforms 4 is structurally set up, the positioning template being restricted to the area around both cladding end faces.

[0087] This method results in an accurate and reproducible connection between the cladding tube 1 and the anti-resonant element preform 4. The joining material 5 for fixing can be cured at a low temperature of less than 300° C., so that strong heating of the surrounding area and the resulting deformation of the anti-resonant element preform 4 are avoided.

[0088] The primary preform 3 is covered with an outer cylinder of silica glass which is collapsed onto the cladding tube 1 while the tube assembly is stretched to form the secondary preform. The outer diameter of the outer cylinder is 63.4 mm and the wall thickness is 17 mm.

[0089] In the collapse and stretch process, with the longitudinal axis oriented vertically, the coaxial arrangement of the cladding tube 1 and the outer cylinder is fed from below into a temperature-controlled heating zone in which it is softened zone by zone starting from the top end of the arrangement.

[0090] The heating zone is kept at a target temperature of 1600°C with a control accuracy of + / - 0.1°C. This allows limiting temperature fluctuations in the heating zone to less than + / - 0.5°C.

[0091] The collapsing and stretching process imparts an oval external cross-sectional shape to the original tubular anti-resonant element preform 4 of the primary preform 3 by generating and maintaining the same internal pressure in the hollow core region and in the tubular anti-resonant element preform 4. Figure 4 shows the ratio of the forces generated. In both the hollow core region 40 and the internal bore of the ARE inner tube 4b, the ambient pressure p a The inner ARE tube 4b is considered stable during stretching when there is a positive pressure of 2.36 mbar inside the cavity of the inner ARE tube 4b (relative to the pressure on its outside). In the absence of internal pressure, the forces shown by the directional arrow F act on the upper apex "S". The normal force F N1 and the resulting normal force F on the side of the inner pipe wall of the ARE N2 The ratio is 1.07 to 1.27 (1.07 <F N1 / F N2 <1.27). As a result of this force ratio, the inner ARE tube 4b becomes oval upon stretching, approximately elliptical, with the major axis of the ellipse running tangential to the wall of the outer ARE tube 4a and the minor axis running perpendicular thereto.

[0092] Correspondingly, when observing the ARE outer tube 4a, the axial length ratio A L / A K The external cross-sectional shape of the oval, characterized by L / A K <1.27).

[0093] ​The secondary preform thus formed by the collapse and stretch process has an outer diameter of about 50 mm and a cladding wall thickness of 16.6 mm, consisting of the outer cladding and the inner cladding. The photograph in Figure 2 shows the secondary preform 32 thus produced, with the deformed anti-resonant element preform 35 and, in particular, the outer ARE tube formed into an oval. Similarly, the inner ARE tube is measurably deformed into an oval, but the deformation is so slight that it is not visually discernible in Figure 2.

[0094] The secondary preform is drawn to form an anti-resonant hollow-core fiber. For that purpose, all structural elements of the previous anti-resonant element preform, i.e. the outer ARE tube 4a and the inner ARE tube 4b, are encapsulated with the encapsulant or bonding material mentioned above. In this case, the encapsulant is applied only to the front side of the anti-resonant element preform, which faces upwards during the fiber drawing process.

[0095] This same front is then connected to a holding tube made of silica glass, which also serves as a gas connection. This holder is fixed to the outer cylinder and the cladding tube by means of a sealing or bonding material 5. For the fiber drawing process, the secondary preform, with its longitudinal axis oriented vertically, is fed from above into a temperature-controlled heating zone, in which it is softened zone by zone, starting from the bottom end. The heating zone is kept at a target temperature of about 2100 °C with a control accuracy of + / - 0.1 °C. This allows the temperature fluctuations in the heating zone to be limited to less than + / - 0.5 °C. At the same time, gas is fed into the core region (hollow core) and the internal pressure in the core region is set to 4 mbar.

[0096] The fiber drawing process performed in this manner results in the oval cross-sectional shape of the original structural elements of the antiresonant element preform becoming round, resulting in an antiresonant hollow-core fiber with a round cross-sectional shape and with the antiresonant elements embedded in it.

[0097] FIG. 3 illustrates the process steps. A primary preform 31 having a round cross-section of the anti-resonant element preform 34 is stretched and collapsed 37 to produce an oval cross-sectional shape (minor axis A K and cross-sectional major axis A L A secondary preform 32 is formed comprising a drawn anti-resonant element preform 35 (denoted by ) which is drawn in a fiber drawing process 38 to form an anti-resonant hollow-core fiber 33 including an anti-resonant element 36 having a round cross-sectional shape.

Claims

1. 1. A method for making an anti-resonant hollow-core fiber (33) having a hollow core extending along a longitudinal axis of the fiber and an inner cladding region including a plurality of anti-resonant elements and surrounding the hollow core, comprising: (a) providing a cladding tube (1) having an internal cladding bore and a cladding longitudinal axis, the cladding tube wall (2) being defined by an inner and outer side and extending along said cladding longitudinal axis; (b) providing a plurality of tubular anti-resonant element preforms (4; 34); (c) placing said tubular anti-resonant element preform (4; 34) at a target location inside said cladding tube wall (2) to form a primary preform (3; 31) having a hollow core region and an inner cladding region; (d) further processing the primary preform (3; 31) into a secondary preform (32) from which said anti-resonant hollow-core fiber (33) is drawn, said further processing comprising drawing and, optionally (i) Collapse, (ii) collapsing and simultaneously stretching; (iii) Collapse of additional cladding material; (iv) collapse of additional cladding material followed by stretching; (v) collapsing and simultaneously stretching additional cladding material; further processing, which includes performing one or more of the following thermoforming processes once or repeatedly: (e) drawing the secondary preform (32) into the anti-resonant hollow-core fiber (33), After stretching according to step (d), at least a portion of the original tubular anti-resonant element preform (4; 34) has a cross-sectional major axis A L and cross-sectional minor axis A K and an oval outer cross-sectional shape having an axial length ratio A. L / A K is in the range of 1.01 to 1.27, and the cross-sectional minor axis A K runs radially from the longitudinal axis of the cladding tube, During drawing, said primary preform (3; 31) is continuously fed into a heating zone at an infeed rate, softened in zones therein, and withdrawn from said heating zone at a withdrawal rate, said infeed rate being set so as to provide a throughput of at least 0.8 g / min and such that the average residence time in said heating zone is in the range of 5 to 25 minutes, characterised in that for the stretching of the primary preform (3; 31) a temperature-controlled heating zone is used in which the target temperature is maintained with an accuracy of + / - 0.1 ° C. method.

2. At least a portion of said tubular anti-resonant element preform (4; 34) is made up of a plurality of mutually nested structural elements (4a; 4b), comprising at least one outer ARE tube (4a) and at least one inner ARE tube (4b) running parallel to the longitudinal axis of said outer ARE tube (4a), said outer ARE tube (4a) having an oval external cross-sectional shape and an axial length ratio A L / A K is in the range of 1.07 to 1.27, and the ARE inner tube (4b) has an oval outer cross-sectional shape and an axial length ratio A L / A K The method of claim 1, wherein is in the range of 1.01 to 1.

05.

3. 2. A method according to claim 1, characterized in that the primary preform (3; 31) has an outer diameter in the range 20 to 70 mm.

4. 2. The method of claim 1, wherein the feed rate is set so that the throughput is in the range of 0.8 g / min to 85 g / min.

5. 5. The method of claim 4, wherein the feed rate is set so that the throughput is in the range of 3.3 g / min to 85 g / min.

6. 2. The method according to claim 1, characterized in that the drawing ratio during drawing is set to a value in the range of 1.05 to 10.

7. The tubular anti-resonator element preform (4) is fixed by amorphous SiO 2 The method according to any one of claims 1 to 6, characterized in that it is carried out using a sealing or bonding material (5) that comprises particles.

8. The method according to claim 2 or any one of claims 3 to 6 which depend on claim 2, characterized in that during the stretching of the primary preform (3; 31), the open ends of the tubular anti-resonance element preform (4) and / or the annular gaps between the individual structural elements (4a; 4b) and / or tube elements of the tubular anti-resonance element preform (4) are sealed by a sealing or bonding material (5).

9. The method according to any one of claims 1 to 6, characterized in that the inside of the cladding tube is provided by machining with longitudinal structures in the area of ​​the target location, which extend towards the cladding tube longitudinal axis.

10. Method according to any one of the preceding claims, characterized in that the tubular anti-resonant element preform (4; 34) is positioned at the target location by means of a positioning template.

11. The method according to claim 10, characterized in that the positioning template is applied in the area of ​​the cladding face.

12. 7. The method according to claim 1, characterized in that during drawing of the primary preform (3; 31) according to step (d) and / or during drawing of the anti-resonant hollow-core fiber (33) according to step (e), several components of the preform made of silica glass are also heated together to soften, the silica glass of at least some of the preform components comprising at least one dopant that reduces the viscosity of the silica glass.

13. 13. The method of claim 12, wherein additional cladding material is collapsed pursuant to step (d), and the silica glass of the cladding tube has a viscosity at least 0.5 dPa·s higher than the silica glass of the additionally attached cladding material at a measurement temperature of 1250°C (viscosity expressed in dPa·s as a logarithmic value).

14. 7. The method according to any one of claims 1 to 6, characterized in that the positioning of the tubular anti-resonant element preform (4; 34) at the target position inside the cladding tube wall (2) and / or the drawing of the anti-resonant hollow-core fiber (33) pursuant to step (d) comprises a fixing and / or sealing step using a sealing or bonding material (5) containing amorphous SiO2 particles.

15. 1. A method for making an anti-resonant hollow-core fiber preform (32) having a hollow core extending along a longitudinal axis of the fiber and an inner cladding region including a plurality of anti-resonant elements and surrounding the hollow core, comprising: (a) providing a cladding tube (1) having an internal cladding bore and a cladding longitudinal axis, the cladding tube wall (2) being defined by an inner and outer side and extending along said cladding longitudinal axis; (b) providing a plurality of tubular anti-resonant element preforms (4); (c) placing said tubular anti-resonant element preform (4; 34) at a target location inside said cladding tube wall (2) to form a primary preform (3; 31) having a hollow core region and an inner cladding region; (d) further processing said primary preform (3; 31) into a secondary preform (32) for said anti-resonant hollow-core fiber, said further processing comprising drawing and, optionally, (i) Collapse, (ii) collapsing and simultaneously stretching; (iii) Collapse of additional cladding material; (iv) collapse of additional cladding material followed by stretching; (v) collapsing and simultaneously stretching additional cladding material; further processing, which includes performing one or more of the following thermoforming processes once or repeatedly: In a manufacturing method comprising: After the elongation according to step (d), at least a portion of the original tubular anti-resonant element preform (4; 34) has an oval outer cross-sectional shape with a cross-sectional major axis AL and a cross-sectional minor axis AK, the axis length ratio AL / AK being in the range of 1.01 to 1.27, the cross-sectional minor axis AK running in a radial direction from the longitudinal axis of the cladding tube, During drawing, said primary preform (3; 31) is continuously fed into a heating zone at an infeed rate, softened in zones therein, and withdrawn from said heating zone at a withdrawal rate, said infeed rate being set so as to provide a throughput of at least 0.8 g / min and such that the average residence time in said heating zone is in the range of 5 to 25 minutes, characterised in that for the stretching of the primary preform (3; 31) a temperature-controlled heating zone is used in which the target temperature is maintained with an accuracy of + / - 0.1 ° C. method.

Citation Information

Patent Citations

  • Method for manufacturing optical fiber

    JP2018150184A

  • An Optical Fiber And Method For Making An Optical Fiber

    US20050226578A1

  • Antiresonant hollow core preforms and optical fibres and methods of fabrication

    WO2019053412A1