Piercer Plug
Patent Information
- Application Number
- JP2021047593
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-22
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2041-03-22
AI Technical Summary
【0012】 本開示によれば、耐剥離性及び耐摩耗性を損なわずに適切に潤滑性を向上させ、長寿命のピアサープラグを得ることができる。
Smart Images

Figure 0007583271000003 
Figure 0007583271000004 
Figure 0007583271000005
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a piercer plug used in piercing and rolling of seamless steel pipes. [Background technology]
[0002] Conventionally, piercer plugs have been used with a scale coating formed on the surface in order to ensure the heat insulation properties, lubricity, and seizure resistance of the surface (see, for example, JP-B-4-8498, JP-A-4-74848, JP-A-4-270003, JP-B-1-7147, JP-A-63-203205, etc.).
[0003] The scale film gradually wears away with each piercing and rolling. When the scale film is completely worn away and the base metal (plug body) is exposed, melting of the base metal and seizing with the mating material occur. When piercing difficult-to-process materials such as stainless steel, wear of the scale film is significant and it may wear away after just a few passes. Each time this occurs, heat treatment is required to re-form the scale film, but this heat treatment takes several to several tens of hours, which is a problem of low efficiency.
[0004] Japanese Patent No. 4279350 proposes a technique for forming a thermal spray coating made of iron and oxides on the surface of the base metal of a piercer plug. The thermal spray coating has better adhesion to the base metal and wear resistance than a scale coating, and can be formed in a few minutes to a few tens of minutes. Therefore, the thermal spray coating has a longer life than a scale coating, and can be regenerated in a short time even if it wears.
[0005] In Japanese Patent No. 5339016, in a manufacturing method of a plug for piercing and rolling in which a coating is formed on the surface of the base metal of the plug by arc spraying, particles having a lower thermal conductivity than iron oxide (specifically, ZrO 2 It is disclosed to use a cored wire containing solid lubricant particles (specifically BN particles).
[0006] Although not related to piercer plugs, JP 2003-147503 A discloses a bearing in which a thermal spray coating made of a low-melting-point metal (specifically, tin, lead, zinc, etc.) or an alloy thereof and a solid lubricant is formed on the sliding surface of a base material. JP 2013-526655 A also discloses a thermal spray wire for coating the sliding surface of a bearing, which includes an inner layer, a powder material layer surrounding the inner layer, and an outer layer surrounding the powder material layer. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Special Publication No. 4-8498 [Patent Document 2] Japanese Patent Application Publication No. 4-74848 [Patent Document 3] Japanese Patent Application Publication No. 4-270003 [Patent Document 4] Special Publication No. 1-7147 [Patent Document 5] Japanese Patent Publication No. 63-203205 [Patent Document 6] Patent No. 4279350 [Patent Document 7] Patent No. 5339016 [Patent Document 8] JP 2003-147503 A [Patent Document 9] Special Publication No. 2013-526655 Summary of the Invention [Problem to be solved by the invention]
[0008] As described above, the thermal sprayed coating has better adhesion to the base metal, i.e., the plug body, and is more excellent in wear resistance than the scale coating. Therefore, the life of the thermal sprayed coating is longer than that of the scale coating. However, when piercing a low-alloy billet in a relatively low temperature range or when piercing a high-strength billet such as a high-alloy billet, peeling of the coating occurs, and melting and seizing may occur starting from the exposed base metal, damaging the plug body.
[0009] The main properties required for a thermal spray coating to suppress damage to the plug body are lubricity, spalling resistance, and wear resistance. However, it is difficult to satisfy all of these properties at the same time. That is, in an arc spray coating made from iron wire, if the ratio of unoxidized Fe in the coating is increased, the piercing efficiency (≒ lubricity) tends to decrease as shown in Figure 1, but the shear adhesion strength (≒ spalling resistance) of the thermal spray coating improves as shown in Figure 2, and the wear amount decreases, that is, the wear resistance improves, as shown in Figure 3. Also, when the thermal spray coating is melted between the billet and the plug body, the friction coefficient decreases and the lubricity improves, but the more the coating melts, the lower the wear resistance and spalling resistance become. Thus, there is a trade-off relationship between lubricity, spalling resistance, and wear resistance.
[0010] An object of the present disclosure is to provide a piercer plug having a long life and appropriately improved lubrication without compromising peel resistance and wear resistance. [Means for solving the problem]
[0011] A piercer plug according to an embodiment of the present disclosure may include a plug body and a first thermal spray coating formed on a surface of the plug body. The plug body may include a tip portion, a bottom portion rearward of the tip portion, and a rolled portion formed between the tip portion and the bottom portion. The first thermal spray coating may include a tip region formed on the surface of the tip portion, a bottom region formed on the surface of the bottom portion, and a rolled region formed on the surface of the rolled portion. The tip region may be comprised of Fe, O, and impurities. The rolled region may be comprised of Fe, O, W, and impurities. The content of W excluding O in the rolled region may be 4.0 wt % or less. Effect of the Invention
[0012] According to the present disclosure, it is possible to obtain a piercer plug having a long life by appropriately improving lubrication without impairing peel resistance and wear resistance. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a graph showing the measurement results of the drilling efficiency of a thermal spray coating. [Diagram 2] FIG. 2 is a graph showing the measurement results of the adhesion strength of the thermal spray coating. [Diagram 3] FIG. 3 is a graph showing the measurement results of the wear amount of the thermal spray coating. [Figure 4] FIG. 4 is a longitudinal cross-sectional view showing a piercer plug according to one embodiment of the present disclosure. [Diagram 5] FIG. 5 is a diagram showing an example of an apparatus used for forming a thermal spray coating. [Figure 6] FIG. 6 is a diagram showing a cross section of a cored wire. [Figure 7] FIG. 7 is a vertical cross-sectional view showing a modified example of a piercer plug according to the present disclosure. [Figure 8] FIG. 8 is a vertical cross-sectional view showing a modified example of a piercer plug according to the present disclosure. [Figure 9] FIG. 9 is a graph showing the relationship between the W content in the rolled region and the wear rate in Experiment 2. [Figure 10] FIG. 10 is a graph showing the relationship between the W content in the rolled region and the friction coefficient in Experiment 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] As a result of intensive research, the inventors have found that the regions of the thermal spray coating formed on the surface of the plug body that require lubricity, peeling resistance, and wear resistance are not necessarily the same. Specifically, the inventors divided the plug body 2 into the front end portion 21, the rolled portion 22, and the bottom portion 23 with reference to FIG. 4, and examined the required characteristics of the thermal spray coating 3 formed on the surfaces of these three portions. As shown in Table 1, the front end region 31 of the thermal spray coating 3 formed on the surface of the front end portion 21, the rolled region 32 of the thermal spray coating 3 formed on the surface of the rolled portion 22, and the bottom region 33 of the thermal spray coating 3 formed on the surface of the bottom portion 23 were examined. In Table 1, "A" indicates a strongly required characteristic, "B" indicates a required characteristic, and "C" indicates a characteristic that is preferably higher but is not particularly required. As a result, it was found that lubricity is strongly required especially in the rolled region 32, and is not particularly required in the front end region 31 and the bottom region 33. That is, it has been found that it is sufficient to focus on wear resistance and peeling resistance in the tip region 31 and bottom region 33 other than the rolled region 32, and by selectively forming a highly lubricating thermal spray coating 3 in the rolled region 32, a piercer plug 1 with high lubricity and long life can be efficiently obtained. The present invention has been completed based on the above findings. Hereinafter, embodiments of the present disclosure will be described.
[0015] [Table 1]
[0016] A piercer plug according to an embodiment of the present disclosure may include a plug body and a first thermal spray coating formed on a surface of the plug body. The plug body may include a tip portion, a bottom portion rearward of the tip portion, and a rolled portion formed between the tip portion and the bottom portion. The first thermal spray coating may include a tip region formed on the surface of the tip portion, a bottom region formed on the surface of the bottom portion, and a rolled region formed on the surface of the rolled portion. The tip region may be composed of Fe, O, and impurities. The rolled region may be composed of Fe, O, W, and impurities. The content of W excluding O in the rolled region may be 4.0% by weight or less. This sufficiently reduces the wear rate of the rolled region during piercing and rolling of the billet, and the rolled region interposed between the plug body and the billet melts, thereby appropriately improving the lubricity that is strongly required for the rolled region. As a result, a piercer plug with a long life can be obtained.
[0017] The content of W excluding O in the rolled region may be 0.5% by weight or more. This sufficiently reduces the friction coefficient of the rolled region, resulting in a piercer plug with a long life.
[0018] The bottom region may be composed of the same elements as the rolled region. This allows the thermal spray coating to divide the surface region into two regions: the tip region and a region behind the tip region (the rolled region and the bottom region). Even when the surface region is divided into two regions, the lubricity of the region corresponding to the rolled region can be improved, so that a piercer plug with a long life can be obtained.
[0019] The piercer plug may include a second sprayed coating formed between the plug body and the first sprayed coating. The second sprayed coating may be composed of Fe, O, and impurities. Fe oxides have excellent peeling resistance. This improves the adhesion between the surface of the plug body and the first sprayed coating, and makes it possible to suppress peeling of the first sprayed coating. As a result, a piercer plug with a long life can be obtained.
[0020] Hereinafter, the embodiments of the present invention will be described in detail with reference to the drawings. In the drawings, the same or corresponding parts are designated by the same reference numerals and their description will not be repeated. The dimensional ratios between the components shown in each drawing do not necessarily represent the actual dimensional ratios.
[0021] [Piercer plug structure] 4 is a longitudinal sectional view of a piercer plug 1 according to one embodiment of the present invention. The piercer plug 1 includes a plug body 2 and a thermal spray coating 3. The entire plug body 2 is integrally formed of the same material. The material of the plug body 2 may be, for example, carbon steel or stainless steel.
[0022] The plug body 2 has a bullet shape. The cross section of the plug body 2 has a circular shape. The plug body 2 has a front end 2a and a face at the end opposite to the front end 2a, i.e., a rear end face 2b. The plug body 2 has a shape in which the outer diameter increases from the front end 2a to the rear end face 2b of the plug body 2. The boundary between the rear end face 2b of the plug body 2 and the other faces forms a circular ridgeline. A line passing through the centers of the outer circumferential circles of the multiple cross sections of the plug body 2 is the plug axis C. The plug axis C is the traveling direction of the billet during piercing and rolling.
[0023] As shown in FIG. 4, the plug body 2 has a front end portion 21, a bottom portion 23 opposite to the front end portion 21, and a rolled portion 22 located between the front end portion 21 and the bottom portion 23. The rolled portion 22 is a rear portion (on the right side in the figure) continuing from the front end portion 21. The bottom portion 23 has a reeling portion 23a and a relief portion 23b. The reeling portion 23a is a rear portion continuing from the rolling portion 22. The relief portion 23b is a rear portion continuing from the reeling portion 23a and is a portion close to the rear end face 2b. The front end portion 21 and the rolled portion 22 are portions that are responsible for most of the wall thickness reduction in piercing-rolling. The bottom portion 23 is a portion that finishes the wall thickness of the hollow blank pipe (also referred to as a shell) in piercing-rolling. In other words, the front end portion 21 is a portion on which a force for piercing the billet mainly acts during piercing-rolling. The rolling section 22 is a section where a force for expanding the diameter of the billet mainly acts during piercing-rolling. The reeling section 23a is a section where a force for uniformizing the wall thickness of the hollow blank produced by piercing or expanding the diameter of the billet or for smoothing the inner circumferential surface of the hollow blank mainly acts during piercing-rolling.
[0024] The outside diameter of the plug body 2 increases from the front to the rear of the plug axis C. That is, the outside diameter of the plug body 2 changes in the direction of the plug axis C. From the front end portion 21 to the rolled portion 22, the rate of change of the outside diameter of the plug body 2 in the direction of the plug axis C decreases from the front end 2a to the reeling portion 23a. That is, in the longitudinal section, the angle θ2 of the tangent of the outer edge line from the front end portion 21 to the rolled portion 22 with respect to the plug axis C decreases from the front end 2a to the reeling portion 23a. The rate of change of the outside diameter of the plug body 2 in the direction of the plug axis C in the reeling portion 23a is equal to or smaller than the minimum value of the rate of change from the front end portion 21 to the rolled portion 22. That is, in the longitudinal section, the angle θ1 of the tangent of the outer edge line of the reeling portion 23a with respect to the plug axis C is equal to or smaller than the minimum value of the angle θ2 of the tangent of the outer edge line from the front end portion 21 to the rolled portion 22 with respect to the plug axis C. In the example shown in FIG. 4, the rate of change of the outer diameter of the reeling portion 23a in the direction of the plug axis C is approximately constant.
[0025] Furthermore, the front end of the rolled portion 22 is preferably located at a position 0.2×D [mm] or less from the front end 2a, where D [mm] is the overall length of the plug body 2 (the dimension of the plug axis C from the front end 2a to the rear end face 2b). The rear end of the rolled portion 22 is preferably located at a position 0.4×D [mm] or more from the front end 2a. In other words, the rolled portion 22 is located between the front end portion 21 and the bottom portion 23, including a range from a position of 0.2×D [mm] to 0.4×D "mm" starting from the front end 2a with respect to the overall length D of the plug body 2.
[0026] The thermal spray coating 3 is formed on the surface of the plug body 2. The thermal spray coating 3 covers the surfaces of the front end portion 21, the rolled portion 22, and the bottom portion 23, except for the rear end face 2b of the plug body 2. That is, as shown in FIG. 4, the thermal spray coating 3 has three regions, namely, a front end region 31 covering the front end portion 21, a rolled region 32 covering the rolled portion 22, and a bottom region 33 covering the bottom portion 23. The three regions are divided into each region and cover the surface of the plug body 2. The constituent elements contained in each of the front end region 31, the rolled region 32, and the bottom region 33 are determined according to the properties (wear resistance, lubricity, and peeling resistance) required for each region. That is, the constituent elements contained in each region differ according to the properties required for each region.
[0027] As shown in Table 1 above, tip region 31 is required to have high wear resistance. Therefore, tip region 31 is made of Fe, O, and impurities. This improves wear resistance. Note that tip region 31 may contain other substances as long as they can improve wear resistance.
[0028] As shown in Table 1 above, the rolling region 32 is required to have a high level of lubricity. Therefore, the rolling region 32 is made of Fe, O, W, and impurities. This allows the melting point of the rolling region 32 to be lower than that of the front end region 31. That is, when the billet is pierced and rolled, the rolling region 32 of the thermal spray coating 3 can be melted in the operating temperature range of the piercer plug 1. During piercing and rolling, the surface temperature of the piercer plug 1 is usually, for example, 850 to 1300°C. It is preferable that the rolling region 32 is determined so as to melt in this temperature range. The rolling region 32 interposed between the plug body 2 and the billet melts, thereby decreasing the coefficient of friction. This allows the lubricity of the rolling region 32 to be improved. Note that the rolling region 32 may be made of Fe, O, one or more elements selected from the group consisting of Na, Si, P, Ca, V, Nb, and W, and impurities, and may contain other substances, as long as the lubricity can be improved.
[0029] As shown in Table 1 above, the bottom region 33 does not have any strongly required properties. However, the bottom region 33 is required to have peeling resistance. Therefore, the constituent elements of the bottom region 33 preferably contain Fe and O. This can improve the peeling resistance of the bottom region 33. Since the bottom region 33 does not have any strongly required properties, the lubricity may be improved as in the modified example described later.
[0030] The W content in the rolling region is 4.0% by weight or less. The W content in the rolling region is the W content relative to the total of Fe, W and impurities contained in the rolling region (W / (Fe+W+impurities)×100), that is, the content excluding O (hereinafter, the same applies to the W content in the tip region and the bottom region). As will be described later, when the W content in the rolling region is 4.0% by weight or less, the wear rate of the rolling region can be reduced. As a result, a piercer plug 1 having a long life can be obtained. From the viewpoint of reducing the wear rate of the rolling region, the W content in the rolling region is preferably 4.0% by weight or less, more preferably 3.0% by weight or less, and more preferably 2.4% by weight or less.
[0031] The W content in the rolling region is 0.5% by weight or more. As will be described later, by making the W content in the rolling region 0.5% by weight or more, the friction coefficient of the rolling region can be reduced. As a result, a piercer plug 1 having a long life can be obtained. From the viewpoint of sufficiently reducing the friction coefficient of the rolling region, the W content in the rolling region is preferably 0.5% by weight or more, more preferably 0.8% by weight or more, and even more preferably 1.2% by weight or more.
[0032] Thus, according to the present disclosure, by forming a highly lubricating thermal spray coating 3 (rolled region 32) on the optimal location, i.e., the surface of the rolled portion 22, and appropriately improving the lubricity, it is possible to obtain a piercer plug 1 with excellent lubricity and a long life without impairing the peeling resistance and wear resistance.
[0033] [Piercer plug manufacturing method] The following describes an example of a method for manufacturing the piercer plug 1. The method described below is merely an example, and the method for manufacturing the piercer plug 1 is not limited to this.
[0034] First, prepare the plug body 2. The plug body 2 to be used has a portion including at least a part of the surface excluding the rear end face 2b made of carbon steel or stainless steel.
[0035] A thermal spray coating 3 is formed on the plug body 2. The thermal spray coating 3 can be formed by using an arc spraying apparatus 100 shown in FIG.
[0036] The arc spraying device 100 includes a spray gun 101 and a rotating table 104. The spray gun 101 generates an arc at the tip of continuously supplied spray wires 102 and 103, and sprays molten metal by compressed air.
[0037] In this embodiment, a front end region 31, a rolled region 32 and a bottom region 33 of the thermal sprayed coating 3 are separately formed on the surfaces of the front end portion 21, the rolled portion 22 and the bottom portion 23 of the plug body 2, respectively.
[0038] First, the bottom region 33 of the sprayed coating 3 is formed on the surface of the bottom portion 23. The sprayed wires 102 and 103 used to form the bottom region 33 are not particularly limited, but it is preferable to improve the peeling resistance. For this reason, the sprayed wires 102 and 103 used to form the bottom region 33 are iron wires. The iron wires are arc sprayed to coat the surface of the bottom portion 23 with iron oxide. That is, the constituent elements of the bottom region 33 are Fe and O. This improves the peeling resistance of the bottom region 33.
[0039] Next, the rolled region 32 of the thermal spray coating 3 is formed on the surface of the rolled portion 22 of the plug body 2. The thermal spray wire 102 used to form the rolled region 32 is a so-called cored wire 110. Fig. 6 is a cross-sectional view perpendicular to the axial direction of the cored wire 110. The cored wire 110 includes an iron shell 111 and a filler material 112 enclosed inside the shell 111.
[0040] The filler 112 contains Fe and W. The filler 112 may contain one or more elements selected from the group consisting of Na, Si, P, Ca, V, Nb, and W, which are capable of forming a thermal spray coating having a lower melting point than the tip region 31. The filler 112 may further contain other substances.
[0041] In this embodiment, the cored wire 110 is melted by the thermal spray gun 101 to form the rolled region 32 on the surface of the rolled portion 22. At this time, the above-mentioned substance contained in the filler 112 can make the melting point of the rolled region 32 lower than that of the tip region 31. The substance contained in the filler 112 may be the same substance as the substance in the rolled region 32, or may be a mixture of multiple substances that will become the same compound after thermal spraying.
[0042] The substance contained in the filler 112 is not limited to one or more selected from the group consisting of Na, Si, P, Ca, V, Nb, and W. It can be appropriately determined so that the rolling region 32 can melt in the operating temperature range of the piercer plug 1 during piercing-rolling. More specifically, the surface temperature of the piercer plug 1 during piercing-rolling is usually 850 to 1300°C, such as 1150°C or 1200°C. The rolling region 32 is preferably determined so as to melt in this temperature range.
[0043] The sprayed wire 103 forming the rolling region 32 may be a cored wire 110 having the same configuration as the sprayed wire 102, or may be an ordinary iron wire. The iron wire is, for example, a wire of carbon steel (ordinary steel), and more specifically, a wire containing iron as a main component and carbon, silicon, manganese, impurities, and the like. In the process of forming the rolling region 32 in this embodiment, at least one of the sprayed wires 102 and 103 may be a cored wire 110 containing a substance capable of forming a sprayed coating having a lower melting point than the tip region 31.
[0044] Next, tip region 31 of thermal spray coating 3 is formed on the surface of tip portion 21. Sprayed wires 102 and 103 used to form tip region 31 are iron wires. The iron wires are arc sprayed to coat the surface of tip portion 21 with iron oxide. That is, the constituent elements of tip region 31 are Fe and O. This improves the wear resistance of tip region 31.
[0045] In order to separately form the front end region 31, the rolled region 32, and the bottom region 33, the regions that are not to be arc sprayed may be masked. Also, the spray angle of the spray gun 101 may be relatively changed so that the molten metal is sprayed onto a predetermined region, thereby changing the region to be sprayed as appropriate. In other words, the method is not limited as long as the sprayed coating 3 can be formed separately for each surface layer region on the surfaces of the front end portion, the rolled portion, and the bottom portion of the plug body 2.
[0046] It should be noted that the longer the spraying distance, the higher the ratio of oxides in the thermal spray coating 3. This is because oxidation of the metal sprayed from the tip of the thermal spray gun 101 progresses in accordance with the spraying distance. The spraying distance is not limited to this, but is, for example, 100 to 1400 mm. In addition, by spraying while gradually increasing the spraying distance, it is possible to increase the ratio of metal components in the vicinity of the plug body 2 and increase the ratio of oxides toward the surface.
[0047] While rotating the plug body 2 about its axis by the turntable 104, thermal spraying is continued until the surface layer region of the thermal spray coating 3 reaches a predetermined thickness. The thickness of the surface layer region is, but is not limited to, 200 to 3000 μm, for example.
[0048] After the thermal spray coating 3 is formed, it is preferable to carry out a heat treatment for diffusion. This allows the plug body 2 and the thermal spray coating 3 to be more closely attached to each other. The heat treatment for diffusion is, for example, performed at 700 to 1200°C for 5 minutes or more. The time for the heat treatment is more preferably 10 minutes or more. The temperature for the heat treatment is more preferably a temperature lower than the melting point of a material capable of forming a thermal spray coating having a lower melting point than the tip region 31 described above. For example, the temperature for the heat treatment can be 1100°C or lower, more preferably 1000°C or higher. The temperature for the heat treatment may also be 800°C or higher, more preferably 900°C or higher.
[0049] Thus, according to the manufacturing method of the piercer plug 1 of the present disclosure, by separately forming each of the tip region 31, the rolled region 32, and the bottom region 33, it is possible to efficiently obtain a piercer plug 1 having excellent lubricity and a long life without impairing the peel resistance and wear resistance.
[0050] [Variations] In the above embodiment, the surface region of the thermal spray coating 3 is divided into three regions (the tip region 31, the rolled region 32, and the bottom region 33), but as shown in FIG. 7, it may be divided into two regions, the tip region 31 and a region behind the tip region 31 (one region including the rolled region 32 and the bottom region 33). Hereinafter, these two regions may be collectively referred to as the body region. In this case, the thermal spray coating 3 is formed so as to improve the wear resistance of the tip region 31 and improve the lubricity of the region behind the tip region 31. This improves the lubricity of the region corresponding to the rolled region 32, so that a piercer plug 1 with high lubricity can be obtained without impairing the peel resistance and the wear resistance. In addition, since it is only necessary to divide the surface region into two, the work of forming the thermal spray coating in each region can be simplified. The surface region of the thermal spray coating 3 may be divided into four or more regions. Even when the surface region is divided into a plurality of regions, the process of forming each region at a position corresponding to the surface of the plug body 2 is the same as the above-mentioned process of forming the surface region. That is, the surface layer region is formed by arc spraying each divided region.
[0051] 8, a thermal sprayed coating 4 of the thermal sprayed coating 3 may be formed between the plug body 2 and the thermal sprayed coating 3. As shown in the figure, the thermal sprayed coating 4 can be divided into three regions at positions corresponding to the respective regions of the thermal sprayed coating 3. The thermal sprayed coating 4 may be one region, or may be divided into two or more regions. The thermal sprayed coating 4 is preferably composed of Fe and O. This can improve the adhesion between the surface of the plug body 2 and the thermal sprayed coating 3 and suppress peeling of the thermal sprayed coating 3, thereby making it possible to obtain a piercer plug 1 with a longer life.
[0052] The thermal sprayed coating 4 can be formed on the surface of the plug body 2 by using an arc spraying apparatus 100, similarly to the thermal sprayed coating 4. After the thermal sprayed coating 4 is formed on the surface of the plug body 2, the thermal sprayed coating 3 is formed on the surface of the thermal sprayed coating 4. The process of forming the thermal sprayed coating 4 is similar to the process of forming the thermal sprayed coating 3 described above, and therefore a detailed description thereof will be omitted.
[0053] In this way, the thermal sprayed coating 3 can be formed by dividing the regions not only in the direction of the plug axis C of the plug body 2 but also in the film thickness direction of the thermal sprayed coating 3. This makes it possible to more appropriately form the thermal sprayed coating 3 according to the characteristics required for each portion of the plug body 2 (the front edge portion 21, the rolled portion 22, and the bottom portion 23). EXAMPLES
[0054] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0055] (Experiment 1) In experiment 1, a thermal spray coating was formed on the surface of a plug body by arc spraying using multiple types of wires (thermal spray wire rods), and a billet piercing test was performed. The plug body used in this test was made of an iron-based alloy. As shown in Table 2, a plug body was used in which the maximum diameter in the longitudinal section of the plug body was 70 mm and the total length of the plug axial center was 230 mm, or a plug body in which the maximum diameter in the longitudinal section of the plug body was 57 mm and the total length of the plug axial center was 120 mm. On the surfaces of these plug bodies, thermal spray coatings were formed in the tip region, the rolled region, and the bottom region by arc spraying. In this case, the thickness of the tip region was 1200 to 1500 μm, the thickness of the rolled region was 500 μm, and the thickness of the bottom region was 300 μm.
[0056] The thermal spray coating was applied separately to the tip region, the rolled region, and the bottom region using an Fe wire or an Fe-W cored wire. The composition of the filler of the Fe-W cored wire was adjusted so that the W content after the thermal spray coating was 0 to 10.5% by weight. Hereinafter, the thermal spray coating applied using the Fe wire will be referred to as the Fe wire thermal spray coating, and the thermal spray coating applied using the Fe-W cored wire will be referred to as the Fe-W thermal spray coating. As shown in Table 2, the melting point of the Fe wire thermal spray coating is 1370°C, and the melting point of the Fe-W wire thermal spray coating is 1120°C. That is, the Fe-W thermal spray coating can have a lower melting point than the Fe wire thermal spray coating.
[0057] Using various piercer plugs prepared in this manner, piercing and rolling of SUS304 billets heated to 1200°C or 1150°C was carried out. Piercing was repeated until each piercer plug was damaged and unusable, and the number of billets that could be pierced and rolled before each piercer plug became unusable was compared as the "life number of passes." The results are shown in Table 2. In Table 2 below, Test Nos. 5, 6, 9, 10 and 11 are examples, and Test Nos. 1, 2, 3, 4, 7, 8, 12, 13, 14, 15 and 16 are comparative examples.
[0058] [Table 2]
[0059] In Test No. 1, a piercer plug in which an Fe wire sprayed coating was applied to all of the tip region, rolling region, and bottom region was used to pierce a SUS304 billet at 1200°C. As a result, after three passes, the sprayed coating in the rolling region wore away and peeled off, exposing the plug body. In this case, it is presumed that there is a risk of the plug body being melted down. This is thought to be due to poor lubricity in the rolling region. In the remarks column of Table 2, "wear to meltdown in rolling region" refers to the case in which the plug body was exposed and there was a risk of the plug body being melted down.
[0060] In Test No. 2, a piercer plug having an Fe-W wire-sprayed coating with a W content of 2.4 wt% applied to the tip region and an Fe wire-sprayed coating applied to the rolled region and bottom region was used to pierce a SUS304 billet at 1,200°C. As a result, as in Test No. 1, after three passes, the sprayed coating in the rolled region wore away and peeled off, exposing the plug body.
[0061] In Test No. 3, a piercer plug in which an Fe-W wire sprayed coating, each with a W content of 2.4 wt%, was applied to the tip region and rolled region, and an Fe wire sprayed coating was applied to the bottom region, was used to pierce a SUS304 billet at 1200°C. As a result, the life was longer than that of the piercer plugs in Test Nos. 1 and 2, but the sprayed coating in the tip region was lost and melted after four passes.
[0062] In test No. 4, a piercer plug in which an Fe-W wire spray coating, each with a W content of 2.4 wt%, was applied to the tip region, rolling region, and bottom region, was used to pierce a SUS304 billet at 1200°C. As a result, as in test No. 3, the spray coating in the tip region was lost and dissolved after four passes.
[0063] In test No. 5, a piercer plug with an Fe wire spray coating on the tip and bottom regions and an Fe-W wire spray coating with a W content of 2.4 wt% on the rolled region was used to pierce a SUS304 billet at 1200°C. As a result, the spray coating was not damaged even after piercing for up to eight passes, and the life was extended.
[0064] In test No. 6, a piercer plug with an Fe wire sprayed coating on the tip region and an Fe-W wire sprayed coating with a W content of 2.4 wt% on the rolling region and bottom region was used to pierce a SUS304 billet at 1200°C. As a result, as in test No. 5, the sprayed coating was not damaged even with piercing up to eight passes, and the life was extended.
[0065] In Test No. 7, a piercer plug in which an Fe wire sprayed coating was applied to the tip region and the rolled region and an Fe-W wire sprayed coating with a W content of 2.4 wt% was applied to the bottom region was used to pierce a SUS304 billet at 1,200°C. As a result, as in Test No. 1, after three passes, the sprayed coating in the rolled region wore away and peeled off, exposing the plug body.
[0066] In Test No. 8, the size of the piercer plug was different from that of Test No. 0.1 (the same was true for the following Test Nos. 9 to 16), and a piercer plug in which an Fe wire sprayed coating was applied to all of the tip region, rolling region, and bottom region was used to pierce a SUS304 billet at 1,150°C. As a result, as in Test No. 0.1, after three passes, the sprayed coating in the rolling region wore away and peeled off, exposing the plug body.
[0067] In test No. 9, a piercer plug with an Fe wire spray coating on the tip region and an Fe-W wire spray coating with a W content of 0.6 wt% on the rolling region and bottom region was used to pierce a SUS304 billet at 1150°C. As a result, the spray coating was not damaged even after piercing for up to five passes, and the life was relatively long.
[0068] In test No. 0.10, a piercer plug with an Fe wire spray coating on the tip region and an Fe-W wire spray coating with a W content of 1.2 wt% on the rolling region and bottom region was used to pierce a SUS304 billet at 1150°C. As a result, the spray coating was not damaged even after piercing for up to seven passes, and the life was extended.
[0069] In test No. 11, a piercer plug with an Fe wire spray coating on the tip region and an Fe-W wire spray coating with a W content of 2.4 wt% on the rolling region and bottom region was used to pierce a SUS304 billet at 1150°C. As a result, the spray coating was not damaged in piercing up to seven passes, and the life was extended.
[0070] In Test No. 12, a piercer plug having an Fe wire sprayed coating applied to the tip region and an Fe-W wire sprayed coating with a W content of 4.9 wt% applied to the rolled region and bottom region was used to pierce a SUS304 billet at 1,150°C. As a result, after three passes, the sprayed coating in the rolled region wore away and peeled off, exposing the plug body.
[0071] In Test No. 13, a piercer plug having an Fe wire sprayed coating applied to the tip region and an Fe-W wire sprayed coating with a W content of 10.5 wt% applied to the rolled region and bottom region was used to pierce a SUS304 billet at 1,150°C. As a result, after two passes, the sprayed coating in the rolled region wore away and peeled off, exposing the plug body.
[0072] In Test No. 14, a piercer plug having an Fe-W wire-sprayed coating with a W content of 0.6 wt% applied to the tip region and an Fe wire-sprayed coating applied to the rolled region and bottom region was used to pierce a SUS304 billet at 1,150°C. As a result, after three passes, the sprayed coating in the rolled region wore away and peeled off, exposing the plug body.
[0073] In Test No. 15, a piercer plug having an Fe-W wire-sprayed coating with a W content of 1.2 wt% applied to the tip region and an Fe wire-sprayed coating applied to the rolled region and bottom region was used to pierce a SUS304 billet at 1,150°C. As a result, after three passes, the sprayed coating in the rolled region wore away and peeled off, exposing the plug body.
[0074] In Test No. 16, a piercer plug having an Fe-W wire-sprayed coating with a W content of 2.4 wt% in the tip region and an Fe wire-sprayed coating in the rolled region and bottom region was used to pierce a SUS304 billet at 1,150°C. As a result, after three passes, the sprayed coating in the rolled region wore away and peeled off, exposing the plug body.
[0075] As a result of Test Nos. 1 to 16, the number of life passes was relatively large in Test Nos. 5, 6, 9, 10, and 11. In other words, the life of the piercer plug could be extended. In particular, the number of life passes was 7 to 8 in Test Nos. 5, 6, 10, and 11, and the life of the piercer plug could be extended dramatically compared to the other tests. As shown by the results of Test Nos. 5 and 6, it was confirmed that the number of life passes is not affected whether the bottom region is an Fe thermal spray coating or an Fe-W thermal spray coating, and that the life of the piercer plug is also extended when the body region is an Fe-W thermal spray coating.
[0076] On the other hand, in Test Nos. 12 and 13, the rolling region was a Fe-W spray coating, but the number of life passes was relatively low at 3 and 2. This is thought to be because the W content was relatively high at 4.9% by weight and 10.5% by weight, which promoted melting of the rolling region and caused the rolling region to wear heavily. In other words, it is thought that during piercing rolling, the wear progression due to the coating melting in the rolling region was greater than the wear reduction associated with the reduction in shear stress due to the lubricating effect of the coating melting. Therefore, the W content in the rolling region is preferably 4.0% by weight or less. In addition, in Test No. 11, where the W content is 2.4% by weight, the number of life passes was high at 7, so the W content in the rolling region is preferably 3.0% by weight or less, more preferably 2.4% by weight or less.
[0077] In addition, comparing Test Nos. 8, 9, and 10, the number of passes in life was 5 by setting the W content to 0.6% by weight in Test No. 9, which was higher than that in Test No. 8, and the number of passes in life was 7 by setting the W content to 1.2% by weight in Test No. 10, which was higher than that in Test No. 8. This is considered to be because the wear progression due to the film melting in the rolling region during piercing and rolling was smaller than the wear reduction associated with the reduction in shear stress due to the lubricating effect of the film melting. That is, the W content in the rolling region is preferably 0.5% by weight or more, preferably 0.8% by weight or more, and more preferably 1.2% by weight or more. The W content in the rolling region was further examined in the following Experiments 2 and 3 from the viewpoints of wear rate and wear coefficient.
[0078] (Test 2) In experiment 2, the relationship between the W content in the tip region, the rolling region, and the bottom region and the wear rate of each region was evaluated. Specifically, piercer plugs having the same shape as No. 8 to No. 16 in experiment 1 were used, and piercer plugs with the W content in the thermal spray coating in the entire region including the tip region and the rolling region of 0.0 wt%, 0.6 wt%, 1.2 wt%, 2.4 wt%, 4.9 wt%, and 10.5 wt% were manufactured. In each of these piercer plugs, piercing was performed in only one pass under the same piercing conditions as No. 8 to No. 16 in experiment 1, and the wear rate per pass was evaluated by measuring the reduction in the thickness of the tip region and the rolling region before and after piercing. Experiment 2 will be described with reference to the graph in FIG. 9. In FIG. 9, the body region refers to the rolling region and the bottom region as described above. As shown in the graph in FIG. 9, the wear rate of the tip region gradually increases as the W content increases.
[0079] On the other hand, the wear rate of the body region, i.e., the rolling region and the bottom region, was 126 μm / pass when the W content was 0.0 wt%, 88 μm / pass when it was 0.6 wt%, 50 μm / pass when it was 1.2 wt%, 65 μm / pass when it was 2.4 wt%, 128 μm / pass when it was 4.9 wt%, and 200 μm / pass when it was 10.5 wt%. Thus, the wear rate of the body region gradually slowed down until the W content was 1.2 wt%, and then gradually increased. Then, when the W content was 4.9 wt%, the wear rate of the body region was 128 μm / pass, which was almost the same as when the W content was 0 wt%. As a result, it was found that the wear rate in the rolling region was slower than when the W content was 0 wt% if the W content was at least 4.0 wt% or less, and the wear rate was the slowest when the W content was 1.2 wt%. Furthermore, since the wear rate is almost the same when the W content is 2.4% by weight as when it is 1.2% by weight, it is considered that the wear rate of the trunk region can be appropriately slowed by setting the W content to 2.4% by weight or less, more preferably, by setting the W content to 4.0% by weight or less, preferably 3.0% by weight or less, more preferably 2.4% by weight or less, from the viewpoint of wear rate, it was found that the wear rate of the rolled region can be appropriately reduced, that is, a piercer plug with a long life can be obtained, compared to when the W content in the rolled region is 0.0% by weight.
[0080] (Test 3) In addition to the above-mentioned Test 2, in Experiment 3, the relationship between the friction coefficient of the thermal spray coating and the W content was evaluated. Specifically, a high-temperature friction tester (manufactured by Yonekura Seisakusho Co., Ltd.) was used to evaluate the friction coefficient of the Fe-W wire thermal spray coating according to the W content. A cored wire (Fe-W cored wire) was produced in which a filler 112, which is a mixed powder containing Fe and W, was enclosed inside an Fe outer shell 111, and a thermal spray coating with a W content of 0 to 14 wt % was produced to a thickness of 500 μm on the surface of the test piece by arc spraying. The melting temperature of the thermal spray coating containing W was 1120°C, as in each test of Experiment 1. The test piece on which this coating was sprayed and a steel test piece heated to a predetermined temperature (1150°C or 1200°C) were brought into contact with each other at a surface pressure of 80 MPa and rotated and slid at a speed of 0.25 m / sec. The friction coefficient was derived from the friction force measured at the sliding distance of 5 m. The results are described with reference to FIG. 10. The W content shown on the horizontal axis of the graph was measured by chemically analyzing the thermal spray coating. As shown in the graph of FIG. 10, when the W content in the thermal spray coating is 0.5% by weight, the friction coefficient is significantly reduced by heating at a melting temperature of 1120° C. or higher, compared to when the content is 0.0% by weight. When the W content is 1.2% by weight or higher, the friction coefficient is significantly reduced compared to when the content is 0.0% by weight. Thereafter, the friction coefficient gradually decreases as the W content increases. Therefore, it was found that the friction coefficient can be effectively reduced by setting the W content to 0.5% by weight or higher, preferably 0.8% by weight or higher, and more preferably 1.2% by weight or higher, and the lubricating effect in the rolling region can be obtained more effectively, that is, a piercer plug with a longer life can be obtained.
[0081] From the results of Experiments 1 to 3 above, it was confirmed that the W content in the rolled region should be 4.0 wt % or less, preferably 3.0 wt % or less, and more preferably 2.4 wt % or less from the viewpoint of wear rate, and should be 0.5 wt % or more, preferably 0.8 wt % or more, and more preferably 1.2 wt % or more from the viewpoint of friction coefficient. [Explanation of symbols]
[0082] 1 Piercer Plug 2 Plug body 2a tip 2b Rear end surface 21 Tip 22 Rolling Section 23 Bottom 3 Thermal spray coating 31 Tip area 32 Rolling Area 33 Bottom area 4 Thermal spray coating C Plug shaft center
Claims
1. The plug body, a first thermal spray coating formed on a surface of the plug body, the plug body includes a front end portion, a bottom portion rearward of the front end portion, and a rolled portion formed between the front end portion and the bottom portion, the first thermal spray coating includes a tip region formed on a surface of the tip portion, a bottom region formed on a surface of the bottom portion, and a rolled region formed on a surface of the rolled portion, the tip region comprises Fe, O, and impurities; The rolling region is composed of Fe, O, W, and impurities, a content of W excluding O in the rolled region is 4.0% by weight or less.
2. 2. The piercer plug of claim 1, a W content excluding O in the rolled region is 0.5 wt % or more.
3. The piercer plug according to claim 1 or 2, the bottom region being composed of the same elements as the rolled region.
4. The piercer plug according to any one of claims 1 to 3, further comprising: a second thermal sprayed coating formed between the plug body and the first thermal sprayed coating, The second thermal spray coating comprises Fe, O, and impurities.
Citation Information
Patent Citations
Seamless steel tube piercing plug and preparation method thereof
CN112474808A
Mandrel for cold and / or hot rolling metal articles - has alternating high-strength antiwear and antifriction surfaces
DE4112614A1
Holder
JP1978039016A
Plug for piercer
JP1988203205A
Data processing device
JP1989007147A