Raw material composition for refractory bricks, manufacturing method for refractory bricks, and manufacturing method for molten metal container

The refractory brick composition, with controlled alumina, spinel, and magnesia content, addresses cracking and peeling issues by managing expansion and modulus, improving durability for secondary electric furnace smelting ladles.

JP7583294B2Active Publication Date: 2024-11-14SHINAGAWA REFRACTORIES CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2022113006
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-07-14
Publication Date
2024-11-14
Estimated Expiration
2042-07-14

AI Technical Summary

Technical Problem

Existing alumina-magnesia-based refractory bricks face issues of cracking and peeling due to excessive expansion and increased elastic modulus, which are not effectively addressed by existing compositions.

Method used

A refractory brick composition comprising 65% to 85% alumina, 14% to 34% spinel with a particle size of 1 mm or less, 3% or less magnesia with a particle size of 300 μm or less, and a binder, controlling the expansion coefficient and elastic modulus to prevent cracking and peeling.

Benefits of technology

The composition suppresses cracking and peeling, enhancing slag corrosion resistance, slag infiltration resistance, and spalling resistance, making it suitable for use as a lining in secondary electric furnace smelting ladles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583294000001
    Figure 0007583294000001
Patent Text Reader

Abstract

To improve corrosion resistance and slag infiltration resistance of an alumina-magnesia-based refractory brick, and suppress crack or peeling.SOLUTION: The present invention relates to a refractory brick that contains an alumina raw material of 65 mass% or more and 85 mass% or less, 1 mm or less spinel raw material of 14 mass% or more and 34 mass% or less, 300 μm or less magnesia raw material of 3 mass% or less (excluding zero) and a binder of 5 mass% or less (excluding zero), and has a residual dimensional change rate after heating to 1500°C of 0% or more and 0.65% or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a refractory brick suitable for use in linings of molten metal vessels, in particular ladles for secondary refining in electric furnaces. [Background technology]

[0002] Alumina-magnesia refractory bricks are primarily used for lining molten metal vessels, especially ladles for secondary refining in electric furnaces.

[0003] For example, Patent Document 1 discloses "an unfired alumina-magnesia brick having a composition of 80-95% by weight of Al2O3, 2-10% by weight of MgO, 0-10% by weight of SiO2, and 0-3% by weight of unavoidable components, and characterized in that the magnesia raw materials contain 1-5% by weight of electrofused magnesia having a particle size of 3.36-1.0 mm and 5-20% by weight of electrofused spinel having a particle size of 1.0 mm or less."

[0004] Furthermore, Patent Document 2 discloses "a refractory brick which is press-molded and then heat-treated at 100°C to 1,150°C, using an alumina raw material and a magnesia raw material containing 90% by mass or more of fine powder of 0.5 mm or less, the total amount of Al2O3 and MgO being 90% by mass or more, containing 4 to 16% by mass of MgO, 0.5 to 5% by mass of SiO2, 0.3 to 2% by mass of the total amount of Na2O and K2O, and the remainder being unavoidable impurities and Al2O3." [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent Publication No. 2000-272956 [Patent Document 2] Patent Publication No. 2007-145684 Summary of the Invention [Problem to be solved by the invention]

[0006] Patent Document 1 claims that MgO is blended into the coarse grains of 1 mm or more, and that expansion due to spinel formation at high temperatures is used to prevent gaps from opening. However, in this case, the magnesia grain size is large and the amount is large, so the expansion is excessive, causing problems such as cracks and peeling.

[0007] In Patent Document 2, a magnesia raw material containing 90% by mass or more of fine powder of 0.5 mm or less is used as the MgO content in the bricks in order to generate a spinel formation reaction by the reaction between alumina and magnesia, and 4 to 16% by mass of the magnesia raw material is used. In this case, too, the large amount of magnesia causes an increase in the elastic modulus, which causes problems such as cracking and peeling due to thermal spalling.

[0008] The present invention has been proposed in view of the above-mentioned conventional circumstances, and has as its object to provide an alumina-magnesia refractory brick in which the expansion coefficient and elastic modulus are controlled so as to suppress cracking and spalling. [Means for solving the problem]

[0009] The present invention relates to It consists of 65% by mass or more and 85% by mass or less of alumina raw material, 14% by mass or more and 34% by mass or less of spinel raw material with a particle size of 1 mm or less, 3% by mass or less of magnesia raw material with a particle size of 300 μm or less (excluding zero), and a binder component. A raw material composition for refractory bricks.

[0010] The present invention also relates to a method for producing a refractory brick, the refractory brick being obtained by molding and drying the raw material composition for a refractory brick, and the refractory brick being obtained by heating at 1500° C., the residual dimensional change rate of which is 0% or more and 0.65% or less. manufacturing It is possible. Effect of the Invention

[0011] In alumina-magnesia refractory bricks, cracking and spalling can be suppressed by controlling the expansion coefficient and elastic modulus. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] As described above, the refractory brick of the present invention is composed of 65% by mass or more and 85% by mass or less of an alumina raw material, 14% by mass or more and 34% by mass or less of a spinel raw material having a particle size of 1 mm or less, 3% by mass or less (excluding zero) of a magnesia raw material having a particle size of 300 μm or less, and a binder component.

[0013] This will be explained in more detail below.

[0014] <Alumina raw material> The alumina raw material is a raw material that becomes the base material. The amount of the alumina raw material used is 65 mass% or more and 85 mass% or less. If the amount of the alumina raw material used is less than 65 mass%, the MgO content becomes relatively high and the thermal expansion coefficient becomes large, and if it exceeds 85 mass%, the MgO content becomes relatively low and the slag corrosion resistance and slag infiltration resistance decrease.

[0015] The particle size of the alumina raw material is not particularly limited, and can be a particle size composition that provides the known closest packing, for example, 15 mass% of particle sizes 5-3 mm, 33 mass% of particle sizes 3-1 mm, 13 mass% of particle sizes 1 mm or less, and 12 mass% of particle sizes 45 μm or less.

[0016] The type of alumina raw material that can be used includes known electrofused alumina, sintered alumina, alumina shale, etc. The purity of the alumina raw material is preferably 90 mass % or more in terms of Al2O3, since this improves corrosion resistance.

[0017] <Spinel raw material> The spinel raw material can be a known aluminum magnesium spinel (MgAl2O4). In addition to the stoichiometric composition (MgO:Al2O3=28:72), the spinel composition can also be one with more Al2O3 than the stoichiometric composition or one with more MgO than the stoichiometric composition. Using one close to the stoichiometric composition (MgO:Al2O3=28:72) is preferable because it makes it easier to control the expansion coefficient and elastic modulus.

[0018] The particle size of the spinel raw material must be 1mm or less, and the amount used must be between 14% and 34% by mass. If the particle size of the spinel raw material is greater than 1mm, the spinel will be unevenly distributed in the brick structure, reducing slag corrosion resistance. On the other hand, if the particle size of the spinel raw material is less than 1mm, the spinel raw material will be uniformly dispersed, improving slag corrosion resistance. If the amount of spinel raw material used is less than 14%, the MgO component will be relatively small, reducing slag corrosion resistance and slag infiltration resistance. If the amount of spinel used is more than 34%, the MgO component will be relatively large, increasing the thermal expansion coefficient and reducing spalling resistance.

[0019] <Magnesia raw material> The magnesia raw material may be any of known electrofused magnesia, seawater magnesia, and natural magnesia. The purity of MgO is preferably 90% by mass or more. The particle size of the magnesia raw material is 300 μm or less, and more preferably 65 μm or less. If the particle size of the magnesia raw material is larger than 300 μm, the thermal expansion coefficient increases and the spalling resistance decreases.

[0020] The amount of magnesia raw material used is 3 mass % or less (excluding zero). If the amount of magnesia raw material used exceeds 3 mass %, the thermal expansion coefficient increases and spalling resistance decreases.

[0021] <Binder> The binder may be any binder that is applicable to known refractory bricks, such as sodium silicate, phenol resin, phosphate, etc. The amount of binder used is preferably 5% by mass or less based on the total amount of the alumina raw material, magnesia raw material, and spinel raw material. EXAMPLES

[0022] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. The alumina raw material was electrofused alumina with a particle size of 5 mm or less and a purity of 99% by mass. The spinel raw material was electrofused spinel with a particle size of 1 mm or less and an Al2O3:MgO mass ratio of 72:28. The magnesia raw material was electrofused magnesia with a purity of 95% by mass and a particle size of 500 μm or less, 300 μm or less, or 65 μm or less.

[0023] Liquid sodium silicate was used as a binder, and was added in an amount of 2.5% by mass in terms of outer percentage, assuming that the total amount of the alumina raw material, the spinel raw material, and the magnesia raw material was 100% by mass.

[0024] A refractory raw material mixture was prepared according to the blending ratio in Table 1, and pressed and molded at 177 MPa using a friction press. The molded product was then dried at 180°C for 12 hours using a hot air dryer to produce a refractory brick.

[0025] Each of the prepared refractory brick samples was evaluated for residual dimensional change rate, elastic modulus, slag corrosion resistance, slag infiltration resistance, and heat spalling resistance.

[0026] The residual dimensional change rate was measured according to JIS R2208. The test temperature was 1500°C, and the atmosphere was air. The residual dimensional change rate is preferably 0% or more and 0.65% or less. If the residual dimensional change rate is 0% or more, joint opening is suppressed, and if it is 0.65% or less, cracks and peeling are reduced.

[0027] The elastic modulus was determined by the grind sonic method, which calculates the natural frequency generated by impacting the test piece using a MK5 made by JWLEMMENS-ELEKTONIKA. It is preferable that the elastic modulus is 80 GPa or less, since spalling resistance is improved.

[0028] The slag corrosion resistance and slag infiltration resistance were evaluated by the lining corrosion method using a high-frequency induction furnace. The sample firebricks were lined in a high-frequency induction furnace, steel was melted in the furnace and kept at 1600℃, and slag with a composition of CaO:SiO2=6:4 was poured onto the surface of the molten steel. The test lasted for 5 hours, with the slag replaced every hour.

[0029] The slag corrosion resistance was calculated from the difference between the thickness of the sample before the test and the thickness of the sample after the test (slag erosion thickness). The slag infiltration resistance was calculated from the thickness of the infiltrated layer (slag erosion thickness) in the cross-sectional photograph after the test. For both the slag erosion thickness and the slag infiltration thickness, the smaller the numbers, the higher the corrosion resistance and infiltration resistance.

[0030] Thermal spalling resistance was evaluated based on the change in elastic modulus due to rapid heating and cooling. In other words, the fewer cracks that occur due to the thermal shock of rapid heating and cooling, the smaller the decrease in elastic modulus before and after the test, and the better the spalling resistance, the better. The test method was the molten iron immersion method. Test pieces measuring 40 mm x 40 mm x 230 mm were prepared, and the elastic modulus was measured before the test.

[0031] The test piece is immersed in molten iron at 1700°C for 1 minute, and then cooled naturally. After cooling, the elastic modulus after the test is measured. The rate of change in elastic modulus is calculated from the elastic modulus before the test and the elastic modulus after the test, as shown in the following formula (1).

[0032] Change in elastic modulus = (elastic modulus before test - elastic modulus after test) / elastic modulus before test × 100 (1)

[0033] The composition of each example shown in Table 1 is a refractory brick containing 65% by mass or more and 85% by mass or less of alumina raw material, 14% by mass or more and 35% by mass or less of spinel raw material having a particle size of 1 mm or less, 3% by mass or less (excluding zero) of magnesia raw material having a particle size of 300 μm or less, and 5% by mass or less (excluding zero) of binder.

[0034] [Table 1]

[0035] In Examples 1-5, the amounts of the alumina raw material, spinel raw material, and magnesia raw material were changed within the range of the present invention. In Comparative Examples 1 and 2, the amounts of the alumina raw material and spinel raw material were outside the range of the present invention. In Comparative Examples 3 and 4, the amounts of the magnesia raw material were outside the range of the present invention. In Comparative Example 5, the particle size of the magnesia raw material was outside the range of the present invention.

[0036] In Examples 1-5, the rate of change in elastic modulus is 39.8 to 49.4%, and compared with Comparative Examples 1, 4 and 5, the spalling resistance is excellent.

[0037] In Examples 1-5, the slag corrosion thickness was 2.3 to 2.8 mm, and compared with Comparative Example 2, the slag corrosion resistance was superior.

[0038] In Examples 1-5, the slag infiltration thickness was 0.9 to 1.8 mm, and compared with Comparative Example 1, the slag infiltration resistance was superior.

[0039] In Examples 1 to 5, the residual dimensional change rate is 0.08 to 0.57%, whereas in Comparative Example 3 it is less than 0%, and in Comparative Examples 4 and 5 it exceeds 0.65%.

[0040] As described above, according to the present invention, it is possible to realize a refractory brick that has improved slag erosion resistance, slag infiltration resistance, and spalling resistance. The refractory brick can be used, for example, as a lining brick for an electric furnace secondary smelting ladle, thereby improving durability.

Claims

1. A raw material composition for a refractory brick, comprising: 65% by mass or more and 85% by mass or less of an alumina raw material; 14% by mass or more and 34% by mass or less of a spinel raw material having a particle size of 1 mm or less; 3% by mass or less (excluding zero) of a magnesia raw material having a particle size of 300 μm or less; and 5% by mass or less (excluding zero) of a binder, expressed by outer percentage based on the total amount of the alumina raw material, the spinel raw material, and the magnesia raw material.

2. A method for producing a refractory brick, comprising molding and drying the raw material composition for a refractory brick according to claim 1, the refractory brick having a residual dimensional change rate of 0% to 0.65% after heating at 1500°C.

3. A method for producing a molten metal container lined with the refractory brick obtained according to claim 2.

Citation Information

Patent Citations

  • Monolithic alumina-spinel refractory

    JP1989087577A

  • Tuyere refractory material for ladle-refining process

    JP1999314965A

  • Unburned alumina-magnesia-based brick

    JP2000272956A

  • Refractory brick

    JP2007145684A

  • Steel tapping port sleeve

    JP2019143181A