Manufacturing method for iron (Fe)-nickel (Ni) alloy powder
A controlled reduction process using a nucleating agent and complexing agent with hydrazine, along with optional cobalt, addresses the issues of particle size and composition instability in conventional methods, resulting in alloy powder with improved magnetic properties and reduced eddy current loss.
Patent Information
- Application Number
- JP2022557484
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-08-31
- Filing Date
- 2021-10-15
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2041-10-15
AI Technical Summary
Conventional methods for producing iron-nickel alloy powder, such as atomization and gas phase reduction, result in large particle sizes, wide particle size distributions, and unstable composition, leading to high eddy current losses and increased manufacturing costs due to the use of hydrazine as a reducing agent.
A method involving the use of a specific nucleating agent, complexing agent, and controlled reduction reaction with hydrazine, along with optional cobalt addition, to produce iron-nickel alloy powder with improved powder properties, including smaller particle size, uniform distribution, and reduced agglomeration, using water-soluble salts and pH adjustment.
The method produces alloy powder with excellent magnetic properties, high saturation magnetic flux density, and reduced eddy current loss, achieving finer particles with controlled size distribution and lower manufacturing costs.
Smart Images

Figure 0007583298000033 
Figure 0007583298000034 
Figure 0007583298000035
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing iron (Fe)-nickel (Ni) based alloy powder. [Background technology]
[0002] The iron-nickel alloy known as permalloy is a soft magnetic material with high magnetic permeability, and is used for the magnetic cores of magnetic components such as choke coils and inductors. In particular, iron-nickel alloy powder is used as a material for magnetic dust cores (dust cores) obtained by compression molding.
[0003] There are various types of permalloys known, such as 78 permalloy (permalloy A) and 45 permalloy, and they are used according to their magnetic properties and applications. 78 permalloy is an iron-nickel alloy with a nickel content of about 78.5% by mass, and is characterized by high magnetic permeability. 45 permalloy is an iron-nickel alloy with a nickel content of 45% by mass, and is characterized by a slightly lower magnetic permeability but a high saturation magnetic flux density.
[0004] In recent years, mobile devices such as laptops and smartphones have been rapidly miniaturized and improved in performance. In addition, magnetic components such as inductors are required to have improved magnetic properties and to support higher frequencies. To achieve this, materials for powder cores are required to have high magnetic flux density and reduced losses. The main losses are hysteresis loss and eddy current loss. In order to reduce hysteresis loss, it is effective to reduce the coercive force of the alloy powder. On the other hand, in order to reduce eddy current loss, it is effective to apply a thin insulating coating to the particle surface of the alloy powder to reduce the eddy current between the particles, or to refine the alloy powder and narrow the particle size distribution. This is because the presence of coarse particles makes it easier for eddy currents to flow through them, resulting in loss due to Joule heat.
[0005] Conventionally known methods for producing fine alloy powder include dry methods such as atomization, gas phase reduction, and dry reduction. The atomization method is a method in which water or gas is sprayed onto a molten metal to rapidly cool and solidify the molten metal. The gas phase reduction method is a method in which a metal halide in a gas phase state is reduced with hydrogen. The dry reduction method is a method in which a metal oxide is reduced using a reducing agent.
[0006] For example, Patent Document 1 describes that Ni-Fe alloy powder used as a material for noise filters, choke coils, inductors, etc. is produced by a gas phase reduction method (Patent Document 1
[0001] and
[0014] ). Patent Document 1 also discloses that a mixture of NiCl2 and FeCl3 is heated, and the vaporized chloride is brought into contact with hydrogen gas to cause a reduction reaction, thereby producing Ni-Fe alloy fine powder (Patent Document 1
[0016] ). Patent Document 2 also describes that Fe-Ni alloy powder used as a material for electronic components such as choke coils and inductors is produced by reducing oxides of Fe and Ni in a reducing gas (Patent Document 2 claim 1).
[0007] On the other hand, it has been proposed to produce finer alloy powders using a wet method. For example, Patent Document 3 discloses a method for producing nickel-iron alloy nanoparticles, which is characterized by adding a reducing agent such as hydrazine to an aqueous solution containing a nickel salt and an iron salt, and simultaneously reducing the nickel ions and iron ions contained in the aqueous solution to produce nickel-iron alloy nanoparticles (claims 1 to 6 of Patent Document 3). It is also said that this production method can efficiently produce nickel-iron alloy nanoparticles with an average primary particle size of 200 nm or less, which are suitable as a filler for imparting magnetic properties, on an industrial scale at low production costs (
[0015] of Patent Document 3). [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2003-193160 A [Patent Document 2] JP 2012-197474 A [Patent Document 3] JP 2008-024961 A Summary of the Invention [Problem to be solved by the invention]
[0009] Although it has been proposed to produce fine alloy powders by dry and wet methods, the conventional techniques have room for improvement in obtaining alloy powders with excellent powder properties. For example, the average particle size of alloy powders produced by the atomization method is large, at several μm or more, and does not fully meet the demand for finer particles. In addition, the particle size distribution of the obtained alloy powder is wide in the gas-phase reduction method proposed in Patent Document 1. Therefore, the alloy powder contains coarse particles, which is insufficient for reducing eddy current loss. There is also a problem that the composition and particle size of the alloy powder are not stable. The dry reduction method proposed in Patent Document 2 requires high-temperature heating, and therefore has a problem that the obtained alloy powder is easily sintered to form coarse aggregated particles.
[0010] The wet method proposed in Patent Document 3 has the advantage that, unlike the dry method, the reduction reaction proceeds at a low temperature, so that coarse aggregated particles are less likely to be generated. Even if aggregated particles are formed, the bonds between the particles are not strong, so the aggregated particles can be easily broken down. However, the method proposed in Patent Document 3 requires the use of a large amount of hydrazine as a reducing agent. This significantly increases the cost of the reducing agent, making it impractical. In addition, the particle size distribution of the obtained alloy powder was not sufficiently small.
[0011] The present inventors have conducted extensive research in light of the above-mentioned problems. As a result, they have found that, when producing iron-nickel alloy powder by a wet method, it is possible to obtain alloy powder with excellent powder characteristics and magnetic properties by using a specific nucleating agent and complexing agent. They have also found that, when the iron content is high, adding a specific content of cobalt allows the reduction reaction promotion effect and spheroidization promotion effect of cobalt to be used in a very small amount of reducing agent to obtain spherical alloy powder with little aggregation, a smooth surface, and a high saturation magnetic flux density.
[0012] The present invention was completed based on these findings, and an object of the present invention is to provide a method for producing iron-nickel based alloy powder having excellent powder properties and magnetic properties. [Means for solving the problem]
[0013] The present invention includes the following aspects (1) to (32). In this specification, the expression "to" includes both ends of the expression. In other words, "X to Y" is synonymous with "X or more and Y or less."
[0014] (1) A method for producing an iron (Fe)-nickel (Ni) based alloy powder containing at least iron (Fe) and nickel (Ni) as magnetic metals, the method comprising the following steps: A preparation step of preparing a magnetic metal source, a nucleating agent, a complexing agent, a reducing agent, and a pH adjusting agent as starting materials; a crystallization step of preparing a reaction liquid containing the starting material and water, and crystallizing a crystallized powder containing the magnetic metal in the reaction liquid by a reduction reaction; and A recovery step of recovering the crystallized powder from the reaction liquid, The magnetic metal source includes a water-soluble iron salt and a water-soluble nickel salt; the nucleating agent is a water-soluble salt of a metal more noble than nickel; the complexing agent is at least one selected from the group consisting of a hydroxycarboxylic acid, a salt of a hydroxycarboxylic acid, and a derivative of a hydroxycarboxylic acid; the reducing agent is hydrazine (N2H4); The method, wherein the pH adjuster is an alkali hydroxide.
[0015] (2) The method according to (1) above, wherein the water-soluble iron salt is at least one selected from the group consisting of ferrous chloride (FeCl2), ferrous sulfate (FeSO4), and ferrous nitrate (Fe(NO3)2).
[0016] (3) The method according to (1) or (2) above, wherein the water-soluble nickel salt is at least one selected from the group consisting of nickel chloride (NiCl2), nickel sulfate (NiSO4), and nickel nitrate (Ni(NO3)2).
[0017] (4) The method according to any one of the above (1) to (3), wherein the nucleating agent is at least one selected from the group consisting of copper salts, palladium salts, and platinum salts.
[0018] (5) Any of the above methods (1) to (4), wherein the complexing agent is at least one hydroxycarboxylic acid selected from tartaric acid ((CH(OH)COOH)2) and citric acid (C(OH)(CH2COOH)2COOH).
[0019] (6) The method according to any one of the above (1) to (5), wherein the pH adjuster is at least one selected from sodium hydroxide (NaOH) and potassium hydroxide (KOH).
[0020] (7) The magnetic metal further comprises cobalt (Co); The method according to any one of the above (1) to (6), wherein the magnetic metal source further contains a water-soluble cobalt salt.
[0021] (8) In the magnetic metal, the content of iron (Fe) is 60 mol% or more and 85 mol% or less, and the content of cobalt (Co) is 10 mol% or more and 30 mol% or less, The method according to (7) above, wherein the content of the water-soluble iron salt in the magnetic metal source is 60 mol % or more and 85 mol % or less, and the content of the water-soluble cobalt salt in the magnetic metal source is 10 mol % or more and 30 mol % or less.
[0022] (9) The method according to (7) or (8) above, wherein the water-soluble cobalt salt is at least one selected from the group consisting of cobalt chloride (CoCl2), cobalt sulfate (CoSO4), and cobalt nitrate (Co(NO3)2).
[0023] (10) Any of the methods (1) to (9) above, wherein the starting material further contains an amine compound containing two or more primary amino groups (-NH2), one primary amino group (-NH2) and one or more secondary amino groups (-NH-), or two or more secondary amino groups (-NH-) in the molecule.
[0024] (11) The method according to (10) above, wherein the amine compound is at least one of an alkyleneamine and an alkyleneamine derivative.
[0025] (12) The method according to (11) above, wherein the alkyleneamine and / or alkyleneamine derivative has at least a structure represented by the following (A) in which a nitrogen atom of an amino group in the molecule is bonded via a carbon chain having two carbon atoms: [ka]
[0026] (13) The amine compound is at least one alkyleneamine selected from the group consisting of ethylenediamine (H2NC2H4NH2), diethylenetriamine (H2NC2H4NHC2H4NH2), triethylenetetramine (H2N(C2H4NH)2C2H4NH2), tetraethylenepentamine (H2N(C2H4NH)3C2H4NH2), pentaethylenehexamine (H2N(C2H4NH)4C2H4NH2), and propylenediamine (CH3CH(NH2)CH2NH2), and / or tris(2-aminoethyl)amine (N( The method according to any one of (10) to (12), wherein the alkyleneamine derivative is at least one selected from the group consisting of N,N'-diacetic acid (HOOCCHNHCHNHCHCOOH), N-(2-aminoethyl)ethanolamine (HNCHNHCHOH), N-(2-aminoethyl)propanolamine (HNCHNHCHOH), 2,3-diaminopropionic acid (HNCHCH(NH)COOH), ethylenediamine-N,N'-diacetic acid (HOOCCHNHCHNHCHCOOH), and 1,2-cyclohexanediamine (HNCHNH).
[0027] (14) The method according to any one of (10) to (13) above, wherein the amount of the amine compound blended relative to the total amount of the magnetic metal is 0.01 mol % or more and 5.00 mol % or less.
[0028] (15) Any of the methods (1) to (14) above, in which, when preparing a reaction solution in the crystallization step, a metal salt raw material solution in which the magnetic metal source, the nucleating agent, and the complexing agent are dissolved in water, a reducing agent solution in which the reducing agent is dissolved in water, and a pH adjusting solution in which the pH adjusting agent is dissolved in water are each prepared, the metal salt raw material solution and the pH adjusting solution are mixed to form a mixed solution, and the mixed solution and the reducing agent solution are mixed.
[0029] (16) The method according to (15) above, wherein, when preparing the reaction solution, the pH adjusting solution and the reducing agent solution are added successively to the metal salt raw material solution and mixed.
[0030] (17) The method according to (15) or (16) above, wherein the time required for mixing the mixed solution and the reducing agent solution is 1 second or more and 180 seconds or less.
[0031] (18) Any of the methods (1) to (14) above, wherein when preparing a reaction solution in the crystallization step, a metal salt raw material solution in which the magnetic metal source, the nucleating agent, and the complexing agent are dissolved in water, and a reducing agent solution in which the reducing agent and the pH adjuster are dissolved in water are separately prepared, and the metal salt raw material solution and the reducing agent solution are mixed together.
[0032] (19) The method according to (18) above, wherein, when preparing the reaction solution, the reducing agent solution is added to the metal salt raw material solution, or conversely, the metal salt raw material solution is added to the reducing agent solution and mixed.
[0033] (20) The method according to (18) or (19) above, wherein the time required for mixing the metal salt raw material solution and the reducing agent solution is 1 second or more and 180 seconds or less.
[0034] (21) The method according to any one of (1) to (20) above, wherein in the crystallization step, an additional raw material liquid, in which at least one of the water-soluble nickel salt and the water-soluble cobalt salt is dissolved in water, is further added to and mixed with the reaction liquid before the reduction reaction is completed.
[0035] (22) The method according to any one of the above (15) to (21), wherein an amine compound is added to at least one of the metal salt raw material solution, the reducing agent solution, the pH adjusting solution, and the reaction solution.
[0036] (23) Any of the above methods (1) to (22), wherein the temperature of the reaction solution at the start of crystallization of the crystallized powder (reaction initiation temperature) is 40°C or higher and 90°C or lower, and the temperature of the reaction solution maintained during crystallization after the start of crystallization (reaction maintenance temperature) is 60°C or higher and 99°C or lower.
[0037] (24) Any of the above methods (1) to (23), further comprising a crushing step of subjecting the crystallized powder after the recovery step or the crystallized powder during the recovery step to a crushing treatment using collision energy to crush aggregated particles contained in the crystallized powder.
[0038] (25) The method according to (24) above, wherein the crystallized powder after the recovery step is crushed by dry crushing or wet crushing, or the crystallized powder during the recovery step is crushed by wet crushing.
[0039] (26) The method according to (25) above, wherein the dry disintegration is spiral jet disintegration.
[0040] (27) The method according to (25) above, wherein the wet crushing is high-pressure fluid impingement crushing.
[0041] (28) Any of the methods according to (1) to (27) above, further comprising a high-temperature heat treatment step in which the crystallized powder after the recovery step or the crystallized powder during the recovery step is subjected to a heat treatment at a temperature higher than 150°C and not higher than 400°C in an inert atmosphere, a reducing atmosphere, or a vacuum atmosphere, thereby improving the composition uniformity within the particles of the iron (Fe)-nickel (Ni)-based alloy powder.
[0042] (29) Any of the above-mentioned methods (1) to (28), further comprising an insulating coating step of subjecting the crystallized powder obtained through the recovery step to an insulating coating treatment to form an insulating coating layer made of a metal oxide on the particle surfaces of the crystallized powder, thereby improving insulation between particles.
[0043] (30) The method according to (29) above, wherein in the insulating coating step, the crystallized powder is dispersed in a mixed solvent containing water and an organic solvent, a metal alkoxide is added to and mixed with the mixed solvent to prepare a slurry, the metal alkoxide is hydrolyzed and subjected to dehydration condensation polymerization in the slurry to form an insulating coating layer made of a metal oxide on the particle surfaces of the crystallized powder, and then the crystallized powder with the insulating coating layer formed thereon is recovered from the slurry.
[0044] (31) The method according to (30) above, wherein the metal alkoxide is mainly composed of silicon alkoxide (alkyl silicate), and the metal oxide is mainly composed of silicon dioxide (SiO2).
[0045] (32) The method according to (30) or (31) above, wherein the hydrolysis of the metal alkoxide is carried out in the presence of a base catalyst (alkali catalyst). Effect of the Invention
[0046] According to the present invention, there is provided a method for producing an iron-nickel based alloy powder having excellent powder properties and magnetic properties. [Brief description of the drawings]
[0047] [Figure 1] FIG. 2 is a process diagram illustrating the method for producing the alloy powder of the present embodiment. [Diagram 2] FIG. 2 is a process diagram illustrating the preparation of a reaction solution and the production of an alloy powder in the first embodiment. [Diagram 3] FIG. 2 is a process diagram illustrating the preparation of a reaction solution and the production of an alloy powder in the first embodiment. [Figure 4] FIG. 2 is a process diagram illustrating the preparation of a reaction solution and the production of an alloy powder in a second embodiment. [Diagram 5] FIG. 2 is a process diagram illustrating the preparation of a reaction solution and the production of an alloy powder in a second embodiment. [Figure 6] FIG. 11 is a process diagram illustrating the preparation of a reaction solution and the production of an alloy powder in a third embodiment. [Figure 7] FIG. 2 is a graph showing the transition of liquid temperature in a reaction tank during the crystallization step in Example 1. [Figure 8] 1 is a SEM image of the alloy powder obtained in Example 1. [Figure 9] 2 is an SEM image of the alloy powder obtained in Example 2. [Figure 10] 1 shows SEM images of the alloy powder obtained in Example 6 (before and after the spiral jet crushing treatment). [Figure 11]1 shows STEM images and EDS line analysis results of the alloy powder obtained in Example 8 (before and after high-temperature heat treatment). [Figure 12] 1 shows a STEM image and EDS line analysis results of a particle cross section of the alloy powder obtained in Example 9. [Figure 13] 1 is an SEM image of the alloy powder obtained in Example 10. [Figure 14] 1 shows SEM images of the alloy powder obtained in Example 12 (before and after insulating coating treatment). [Figure 15] 1 is an SEM image of the alloy powder obtained in Example 13. [Figure 16] 1 is an SEM image of the alloy powder obtained in Example 14. [Figure 17] 2 is a SEM image of the alloy powder obtained in Comparative Example 1. [Figure 18] 2 is an SEM image of the alloy powder obtained in Comparative Example 2. [Figure 19] 1 is an SEM image of the alloy powder obtained in Comparative Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0048] A specific embodiment of the present invention (hereinafter, referred to as the present embodiment) will be described. Note that the present invention is not limited to the following embodiment, and various modifications are possible without departing from the gist of the present invention.
[0049] <<1. Method of manufacturing iron-nickel alloy powder>> The method for producing the iron (Fe)-nickel (Ni) alloy powder of the present embodiment includes the following steps: a preparation step of preparing a starting material containing a magnetic metal source, a nucleating agent, a complexing agent, a reducing agent, and a pH adjusting agent; a crystallization step of preparing a reaction liquid containing the starting material and water, and crystallizing a crystallized powder containing the magnetic metal in the reaction liquid by a reduction reaction; and a recovery step of recovering the crystallized powder from the resulting reaction liquid. Here, the iron (Fe)-nickel (Ni) alloy powder contains at least iron (Fe) and nickel (Ni) as magnetic metals. The magnetic metal source also contains a water-soluble iron salt and a water-soluble nickel salt. The nucleating agent is a water-soluble salt of a metal more noble than nickel. The complexing agent is at least one selected from the group consisting of hydroxycarboxylic acid, a salt of hydroxycarboxylic acid, and a derivative of hydroxycarboxylic acid. The reducing agent is hydrazine (N2H4).
[0050] The iron (Fe)-nickel (Ni)-based alloy powder (hereinafter, sometimes simply referred to as "alloy powder") of this embodiment contains at least iron (Fe) and nickel (Ni). The alloy powder may also contain cobalt (Co) as necessary. That is, the alloy powder may be an iron-nickel alloy powder containing only iron and nickel, or may be an iron-nickel-cobalt alloy powder containing iron, nickel, and cobalt. Iron, nickel, and cobalt are all magnetic metals that exhibit ferromagnetism. Therefore, iron-nickel alloy powder and iron-nickel-cobalt alloy powder have high saturation magnetic flux density and excellent magnetic properties. In this specification, magnetic metal is a general term for iron, nickel, and cobalt. That is, when the alloy does not contain cobalt, magnetic metal is a general term for iron and nickel, and when the alloy contains cobalt, magnetic metal is a general term for iron, nickel, and cobalt.
[0051] The proportions of iron (Fe), nickel (Ni) and cobalt (Co) contained in the alloy powder of this embodiment are not particularly limited. The amount of iron may be 10 mol% or more and 95 mol% or less, 25 mol% or more and 90 mol% or less, or 40 mol% or more and 80 mol% or less. The amount of nickel may be 5 mol% or more and 90 mol% or less, 10 mol% or more and 75 mol% or less, or 20 mol% or more and 60 mol% or less. The amount of cobalt may be 0 mol% or more and 40 mol% or less, or 5 mol% or more and 20 mol% or less. However, the total amount of iron, nickel and cobalt is 100 mol% or less.
[0052] The alloy powder of this embodiment does not exclude the inclusion of other additive components other than the magnetic metals (Fe, Ni, and Co). Examples of such additive components include copper (Cu) and / or boron (B). However, in order to maximize the effect based on the magnetic metals, the content of the additive components other than the magnetic metals is preferably as small as possible. The content of the components other than the magnetic metals may be 10 mass% or less, 5 mass% or less, 1 mass% or less, or 0 mass%. The alloy powder may contain impurities (unavoidable impurities) that are inevitably mixed in during the manufacturing process. Examples of such inevitable impurities include oxygen (O), carbon (C), chlorine (Cl), and alkaline components (Na, K, etc.). Since the inevitable impurities may cause deterioration of the properties of the alloy powder, it is preferable to minimize the amount of the inevitable impurities. The amount of the inevitable impurities is preferably 5 mass% or less, more preferably 3 mass% or less, for oxygen (O) contained in the oxide film that is inevitably formed on the surface of the alloy powder. On the other hand, the content of carbon (C), chlorine (Cl) and alkali components (Na, K, etc.) is preferably 1 mass% or less, more preferably 0.5 mass% or less, and even more preferably 0.1 mass% or less. The alloy powder may have a composition containing a magnetic metal, with the balance being inevitable impurities.
[0053] The manufacturing method of the alloy powder of this embodiment includes at least a preparation step, a crystallization step, and a recovery step. If necessary, a crushing step or a high-temperature heat treatment step may be provided after or during the recovery step, or an insulating coating step may be provided after the recovery step. FIG. 1 shows an example of a process in the manufacturing method of this embodiment. In FIG. 1, the crushing treatment, the high-temperature heat treatment, and the insulating coating treatment are shown, but these treatments may be provided as necessary and are not essential treatments. In addition, when the crushing treatment, the high-temperature heat treatment, and / or the insulating coating treatment are performed, there is no particular restriction on the order in which these treatments are performed. If anything, it is preferable to perform the crushing treatment after the high-temperature heat treatment. This is because the connection (bond) between the alloy particles strengthened by the high-temperature heat treatment can be reduced or eliminated. In addition, it is preferable to perform the crushing treatment before the insulating coating. This is because the entire surface of each alloy particle in which the connection is reduced or eliminated can be uniformly insulating coated. In contrast, if the alloy particles are in a connected state, an insulating coating layer is not formed at the connection part. Therefore, it is preferable to reduce or eliminate the connection as much as possible before the insulating coating treatment. Details of each step will be described below.
[0054] <Preparation process> In the preparation step, a magnetic metal source, a nucleating agent, a complexing agent, a reducing agent, and a pH adjuster are prepared as starting materials. The magnetic metal source is a raw material of iron and nickel, but may contain a raw material of cobalt if necessary. The starting materials may also contain an amine compound. Each raw material is described below.
[0055] (a) Magnetic metal source The magnetic metal source is a raw material of the magnetic metal, and includes at least a water-soluble iron salt and a water-soluble nickel salt. The iron salt is a raw material (iron source) of the iron component contained in the alloy powder, and is not particularly limited as long as it is an iron salt that is easily soluble in water. Examples of the iron salt include iron chloride, iron sulfate, iron nitrate, or a mixture thereof, which contain divalent and / or trivalent iron ions. The water-soluble iron salt is preferably at least one selected from the group consisting of ferrous chloride (FeCl2), ferrous sulfate (FeSO4), and ferrous nitrate (Fe(NO3)2). The nickel salt is a raw material (nickel source) of the nickel component contained in the alloy powder, and is not particularly limited as long as it is a nickel salt that is easily soluble in water. The water-soluble nickel salt is preferably at least one selected from the group consisting of nickel chloride (NiCl2), nickel sulfate (NiSO4), and nickel nitrate (Ni(NO3)2), and is particularly preferably at least one selected from the group consisting of nickel chloride (NiCl2) and nickel sulfate (NiSO4).
[0056] If necessary, the magnetic metal may further contain cobalt (Co), and the magnetic metal source may further contain a water-soluble cobalt salt. This makes it possible to produce an iron-nickel-cobalt alloy powder. The iron-nickel-cobalt alloy powder, in which part of the iron or nickel is replaced with cobalt, is characterized by a particularly high saturation magnetic flux density.
[0057] The water-soluble cobalt salt has the effect of promoting the reduction reaction during the crystallization of the alloy powder (reduction promotion effect), and this reduction promotion effect is particularly prominent when the content of iron (Fe) in the magnetic metal is as high as 60 mol% or more. Furthermore, the water-soluble cobalt salt also has the effect of making the alloy powder into spherical particles with a smooth surface (spheroidization promotion effect). Therefore, if the content of the water-soluble iron salt in the magnetic metal source is 60 mol% or more and 85 mol% or less, and the content of the water-soluble cobalt salt is 10 mol% or more and 30 mol% or less, it is possible to obtain an iron-nickel-cobalt alloy powder with an extremely large saturation magnetic flux density (for example, 2T (Tesla) or more) and a smooth and spherical surface, even if the amount of hydrazine used as a reducing agent is very small. For example, the content of iron in this alloy powder is 60 mol% or more and 85 mol% or less, and the content of cobalt is 10 mol% or more and 30 mol% or less.
[0058] The water-soluble cobalt salt is not particularly limited as long as it is a cobalt salt that is easily water-soluble. The water-soluble cobalt salt is preferably at least one selected from the group consisting of cobalt chloride (CoCl2), cobalt sulfate (CoSO4), and cobalt nitrate (Co(NO3)2), and more preferably at least one selected from the group consisting of cobalt chloride (CoCl2) and cobalt sulfate (CoSO4).
[0059] (b) Nucleating agent The nucleating agent is a water-soluble salt of a metal more noble than nickel. This nucleating agent (water-soluble salt of a metal more noble than nickel) is preferentially reduced in the reaction solution in the subsequent crystallization step to generate initial nuclei, which act to promote the precipitation of crystallized powder. Here, a metal more noble than nickel is a metal that has a higher potential in an aqueous solution in the standard potential series than nickel. A metal more noble than nickel can also be said to have a smaller tendency to ionize than nickel. Examples of such metals include tin (Sn), lead (Pb), antimony (Sb), bismuth (Bi), copper (Cu), silver (Ag), palladium (Pd), iridium (Ir), platinum (Pt), and gold (Au).
[0060] By using a water-soluble salt of a metal more noble than nickel as a nucleating agent, the formation of crystallized powder in the reaction solution can be controlled in the subsequent crystallization process. For example, by increasing the amount of nucleating agent added, fine crystallized powder can be obtained. That is, in the crystallization process, the ions and complex ions of the magnetic metal contained in the reaction solution are reduced and precipitated to form the crystallized powder. Among magnetic metals, nickel is more noble than iron and cobalt, and has a small tendency to ionize. Therefore, if a water-soluble salt (nucleating agent) of a metal more noble than nickel is contained in the reaction solution, the metal more noble than nickel will be reduced and precipitated before all the magnetic metals. The precipitated metal more noble than nickel acts as an initial nucleus, and these initial nuclei grow to form crystallized powder made of magnetic metal, so the particle size of the crystallized powder can be controlled by the amount of nucleating agent added, which determines the number of initial nuclei.
[0061] The nucleating agent is not particularly limited as long as it is a water-soluble salt of a metal more noble than nickel. However, the nucleating agent is preferably at least one selected from the group consisting of copper salts, palladium salts, and platinum salts. Copper (Cu), palladium (Pd), and platinum (Pt) are particularly noble and have a small tendency to ionize. Therefore, they are particularly effective as nucleating agents. Examples of water-soluble copper salts include, but are not limited to, copper sulfate. Examples of water-soluble palladium salts include, but are not limited to, sodium palladium (II) chloride, ammonium palladium (II) chloride, palladium (II) nitrate, and palladium (II) sulfate. The nucleating agent is particularly preferably a palladium salt. When a palladium salt is used, it becomes possible to control the particle size of the crystallized powder (alloy powder) more finely.
[0062] The amount of the nucleating agent may be adjusted so that the particle size of the final alloy powder is the desired value. For example, the amount of the nucleating agent relative to the total amount of the magnetic metal may be 0.001 mol ppm or more and 5.0 mol ppm or less, or 0.005 mol ppm or more and 2.0 mol ppm or less. By setting the amount of the nucleating agent within this range, an alloy powder having an average particle size of 0.2 μm or more and 0.6 μm or less can be obtained. However, the amount of the nucleating agent is not limited to the above-mentioned range. For example, when producing a fine alloy powder having an average particle size of less than 0.2 μm, the amount of the nucleating agent may be set to more than 5.0 mol ppm.
[0063] (c) Complexing agent The complexing agent is at least one selected from the group consisting of hydroxycarboxylic acids, salts of hydroxycarboxylic acids, and derivatives of hydroxycarboxylic acids. This complexing agent (hydroxycarboxylic acid, etc.) has the effect of making the reaction uniform in the subsequent crystallization step. That is, the magnetic metal component is dissolved in the reaction solution as magnetic metal ions (Fe 2+ , Ni 2+However, the amount of magnetic metal ions dissolved in the reaction solution is extremely small because the reaction solution becomes strongly alkaline due to the pH adjuster (NaOH, etc.). However, when a complexing agent is present, the magnetic metal components can be dissolved in large amounts as complex ions (Fe complex ions, Ni complex ions, etc.). The presence of such complex ions increases the reduction reaction rate, suppresses local uneven distribution of the magnetic metal components, and enables the reaction system to be homogenized. In addition, the complexing agent has the effect of changing the balance of the complex stability of multiple magnetic metal ions in the reaction solution. Therefore, when a complexing agent is present, the reduction reaction of the magnetic metal changes, and the balance between the nucleation rate and the grain growth rate changes. By using a complexing agent (hydroxycarboxylic acid, etc.) specified in this embodiment, the above-mentioned actions work in a composite manner, and the reaction proceeds in a favorable direction, resulting in improved powder properties (particle size, particle size distribution, sphericity, surface properties of particles) of the obtained alloy powder. In addition, the alloy powder with improved powder properties has excellent filling properties and is suitable as a raw material for powder cores. In this regard, the complexing agent (such as hydroxycarboxylic acid) of the present embodiment can be said to have the functions of a reduction reaction accelerator, a spheroidizing accelerator, and a surface smoothing agent. A suitable complexing agent includes at least one hydroxycarboxylic acid selected from tartaric acid ((CH(OH)COOH)2) and citric acid (C(OH)(CH2COOH)2COOH).
[0064] The amount of the complexing agent relative to the total amount of the magnetic metal is preferably 5 mol% or more and 100 mol% or less, more preferably 10 mol% or more and 75 mol% or less, and even more preferably 15 mol% or more and 50 mol% or less. When the amount is 5 mol% or more, the functions of the reduction reaction accelerator, the spheroidization accelerator, and the surface smoothing agent are fully exerted, so that the powder characteristics (particle size, particle size distribution, sphericity, surface properties of particles) of the alloy powder are further improved. In addition, when the amount is 100 mol% or less, the amount of the complexing agent used can be reduced without causing a significant difference in the degree of function expression as a complexing agent, which leads to a reduction in manufacturing costs.
[0065] (d) Reducing agent The reducing agent is hydrazine (N2H4, molecular weight: 32.05). This reducing agent (hydrazine) acts to reduce the magnetic metal ions and complex ions in the reaction solution in the subsequent crystallization process. Hydrazine has the advantage of being highly reducing, and that by-products associated with the reduction reaction are not generated in the reaction solution. It is also easy to obtain high-purity hydrazine with few impurities.
[0066] In addition to anhydrous hydrazine, hydrazine hydrate (N2H4·H2O, molecular weight: 50.06), which is a hydrazine hydrate, is known. Either may be used. For example, commercially available industrial grade 60% by mass hydrazine hydrate can be used as hydrazine hydrate.
[0067] The amount of reducing agent depends greatly on the composition of the iron (Fe)-nickel (Ni) alloy powder, and the greater the content of iron that is difficult to reduce, the more reducing agent is required. In addition to the composition of the alloy powder, it is also affected by the temperature of the reaction solution, or the amount of complexing agent or pH adjuster. For example, when the iron content in the iron-nickel alloy powder is 60 mol% or less, the amount of reducing agent to be mixed with respect to the total amount of magnetic metal is preferably 1.8 to 7.0 in molar ratio, more preferably 2.0 to 6.0 in molar ratio, and even more preferably 2.5 to 5.0 in molar ratio. When the iron content in the iron-nickel alloy powder is more than 60 mol% and 75 mol% or less, the amount of reducing agent to be mixed with respect to the total amount of magnetic metal is preferably 2.5 to 9.0 in molar ratio, more preferably 3.5 to 8.0 in molar ratio. When the iron content of the iron-nickel alloy powder is more than 75 mol% and less than 95 mol%, the amount of the reducing agent to be blended with respect to the total amount of magnetic metal is preferably 3.5 to 10.0 in molar ratio, more preferably 4.5 to 9.0. On the other hand, when producing an iron-nickel-cobalt alloy powder, the amount of the reducing agent to be blended can be significantly reduced compared to the iron-nickel alloy powder due to the action of the water-soluble cobalt salt described above. In particular, the action of the water-soluble cobalt salt is remarkable in the production of an alloy powder with a high iron content. For example, when producing an alloy powder with a composition in which the iron content is 60 mol% to 85 mol% and the cobalt (Co) content is 10 mol% to 30 mol%, the amount of the reducing agent to be blended with respect to the total amount of magnetic metal is preferably 1.0 to 4.0 in molar ratio, more preferably 1.2 to 2.0.
[0068] In either case, when the blending amount is equal to or greater than the lower limit described above, the reduction of the magnetic metal ions and complex ions proceeds sufficiently, and a crystallized powder (alloy powder) without any unreduced substances such as iron hydroxide can be obtained. When the blending amount is equal to or less than the upper limit described above, the amount of the reducing agent (hydrazine) used can be reduced, leading to a reduction in manufacturing costs.
[0069] (e) pH adjuster The pH adjuster is an alkali hydroxide. This pH adjuster (alkali hydroxide) has the effect of strengthening the reduction reaction of hydrazine, which is a reducing agent. In other words, the higher the pH of the reaction solution, the stronger the reducing power of hydrazine. Therefore, by using an alkali hydroxide as a pH adjuster, the reduction reaction of the magnetic metal ions and complex ions in the reaction solution and the accompanying precipitation of crystallized powder are promoted. The type of alkali hydroxide is not particularly limited. However, in terms of availability and price, it is preferable that the pH adjuster contains at least one selected from sodium hydroxide (NaOH) and potassium hydroxide (KOH).
[0070] The amount of pH adjuster (alkali hydroxide) may be adjusted so that the reducing power of the reducing agent (hydrazine) is sufficiently high. Specifically, the pH of the reaction solution at the reaction temperature is preferably 9.5 or higher, more preferably 10 or higher, and even more preferably 10.5 or higher. Therefore, the amount of alkali hydroxide may be adjusted so that the pH falls within this range.
[0071] (f) Amine compounds If necessary, the starting material may further include an amine compound that contains two or more primary amino groups (-NH2), one primary amino group (-NH2) and one or more secondary amino groups (-NH-), or two or more secondary amino groups (-NH-) in the molecule.
[0072] The amine compound has the effect of promoting the reduction reaction in the subsequent crystallization process. In other words, the amine compound functions as a complexing agent and dissolves the magnetic metal ions (Fe 2+ , Ni 2+ It has the function of complexing the metal ions (Fe complex ions, Ni complex ions, etc.) to form complex ions (Fe complex ions, Ni complex ions, etc.). It is believed that the presence of complex ions in the reaction solution causes the reduction reaction to proceed even further.
[0073] Amine compounds also have the effect of suppressing the self-decomposition of hydrazine, which is a reducing agent. In other words, when crystallized powder made of a magnetic metal precipitates in the reaction solution, nickel (Ni) in the magnetic metal acts as a catalyst, which can cause hydrazine to decompose. This is called self-decomposition of hydrazine. This decomposition reaction is shown in the following formula (1), in which hydrazine (N2H4) decomposes into nitrogen (N2) and ammonia (NH3). If such self-decomposition occurs, it is undesirable because it impairs the function of hydrazine as a reducing agent.
[0074]
number
[0075] Adding an amine compound to the mixture liquid makes it possible to suppress the self-decomposition of hydrazine. Although the detailed mechanism is unknown, it is speculated that this is because excessive contact between hydrazine in the reaction liquid and the crystallized powder is prevented. In other words, among the amino groups contained in the amine compound molecules, especially the primary amino group (-NH2) and secondary amino group (-NH-) are strongly adsorbed to the surface of the crystallized powder in the reaction liquid. It is thought that the amine compound molecules cover and protect the crystallized powder, preventing excessive contact between the hydrazine molecules and the crystallized powder, thereby suppressing the self-decomposition of hydrazine. The self-decomposition of hydrazine becomes more noticeable when the content of nickel in the magnetic metal is high, so amine compounds are particularly effective in such cases.
[0076] The amine compound is preferably at least one of an alkyleneamine and an alkyleneamine derivative. The alkyleneamine and / or alkyleneamine derivative preferably has at least the structure represented by the following (A) in which the nitrogen atom of the amino group in the molecule is bonded via a carbon chain having two carbon atoms.
[0077] [ka]
[0078] By using such alkyleneamines or alkyleneamine derivatives as the amine compounds, the effect of suppressing the self-decomposition of hydrazine (reducing agent) can be more effectively exhibited. The reason for this is believed to be that such alkyleneamines or alkyleneamine derivatives contain short carbon chains, which effectively suppress the contact of hydrazine molecules with the crystallized powder. In contrast, when the nitrogen atom of the amino group is bonded via an excessively long carbon chain, the degree of freedom of movement of the carbon chain is large even if the amino group is adsorbed to the crystallized powder. Therefore, it is speculated that the contact between the crystallized powder and hydrazine molecules is not effectively hindered.
[0079] Specific examples of alkyleneamines having the structure represented by (A) above include one or more selected from the group consisting of ethylenediamine (abbreviation: EDA) (H2NC2H4NH2), diethylenetriamine (abbreviation: DETA) (H2NC2H4NHC2H4NH2), triethylenetetramine (abbreviation: TETA) (H2N(C2H4NH)2C2H4NH2), tetraethylenepentamine (abbreviation: TEPA) (H2N(C2H4NH)3C2H4NH2), pentaethylenehexamine (abbreviation: PEHA) (H2N(C2H4NH)4C2H4NH2), and propylenediamine (also known as 1,2-diaminopropane, 1,2-propanediamine) (abbreviation: PDA) (CH3CH(NH2)CH2NH2). Specific examples of the alkyleneamine derivative having the structure represented by (A) above include tris(2-aminoethyl)amine (abbreviation: TAEA) (N(C2H4NH2)3), N-(2-aminoethyl)ethanolamine (also known as 2-(2-aminoethylamino)ethanol (abbreviation: AEEA) (H2NC2H4NHC2H4OH), N-(2-aminoethyl)propanolamine (also known as 2-(2-aminoethylamino)propanol (abbreviation: AEPA) (H2NC2H4NHC 3H6OH), L(or D, DL)-2,3-diaminopropionic acid (also known as 3-amino-L(or D, DL)-alanine) (abbreviated as DAPA) (H2NCH2CH(NH)COOH), ethylenediamine-N,N'-diacetic acid (also known as ethylene-N,N'-diglycine) (abbreviated as EDDA) (HOOCCH2NHC2H4NHCH2COOH), 1,2-cyclohexanediamine (also known as 1,2-diaminocyclohexane) (abbreviated as CHDA) (H2NC6H 10 These alkyleneamines and alkyleneamine derivatives are water-soluble, and among them, ethylenediamine and diethylenetriamine are preferred because they have a relatively strong effect of inhibiting the self-decomposition of hydrazine, and are easily available and inexpensive.
[0080] The structural formulas of ethylenediamine (EDA), diethylenetriamine (DETA), triethylenetetramine (TETA), tetraethylenepentamine (TEPA), pentaethylenehexamine (PEHA), propylenediamine (PDA), tris(2-aminoethyl)amine (TAEA), N-(2-aminoethyl)ethanolamine (AEEA), N-(2-aminoethyl)propanolamine (AEPA), and L (or D, DL)-2,3-diaminopropionic acid (DAPA) are shown in (B) to (M) below.
[0081] [ka]
[0082] [ka]
[0083] [ka]
[0084] [ka]
[0085] [ka]
[0086] [ka]
[0087] [ka]
[0088] [ka]
[0089] [ka]
[0090] [ka]
[0091] [ka]
[0092] [ka]
[0093] The amount of the amine compound to be blended with respect to the total amount of the magnetic metal is preferably 0.00 mol% or more and 5.00 mol% or less, more preferably 0.01 mol% or more and 5.00 mol% or less, and even more preferably 0.03 mol% or more and 5.00 mol% or less. The amount of the amine compound to be blended may be 0.00 mol%, that is, the amine compound may not be blended. However, by making the amount blended 0.01 mol% or more, it is possible to fully exert the effect of suppressing the self-decomposition of hydrazine and the effect of promoting the reduction reaction based on the amine compound. In addition, by making the amount blended 5.00 mol% or less, it is possible to appropriately express the function as a complexing agent. Therefore, it is possible to make the powder characteristics of the alloy powder (particle size, particle size distribution, sphericity, surface properties of the particles) more excellent. If the amount of the amine compound blended exceeds 5.00 mol%, the function as a complexing agent becomes too strong. There is a risk that the particle growth will become abnormal and the powder characteristics of the alloy powder will deteriorate.
[0094] <Crystallization process> In the crystallization process, a reaction liquid containing the prepared starting material and water is prepared, and the magnetic metal-containing crystallized powder is crystallized in the reaction liquid by a reduction reaction. The preparation of the reaction liquid and the crystallization of the crystallized powder are described below. In actual production, the crystallization reaction starts at the same time as the reaction liquid is prepared in most cases, but there is a possibility that the crystallization reaction starts, even if only slightly, during the preparation of the reaction liquid. The crystallization reaction referred to here is a reaction that occurs during the crystallization process. That is, the main reaction is a reduction reaction by hydrazine (such as the formula (6) described below), but it also includes the self-decomposition reaction of hydrazine (the formula (1) described above). Therefore, the term crystallization reaction is used in a broader sense than reduction reaction.
[0095] In the crystallization process, at least one of a plurality of solutions such as a metal salt raw material solution and a reducing agent solution is heated and mixed to prepare a reaction solution, and the reaction solution is heated and stirred in a reaction tank while being kept at a predetermined temperature, and the crystallization reaction proceeds in that state. A general-purpose method can be applied for heating, and for example, a reaction tank (reaction vessel) is placed in a water bath, or a reaction tank with a steam jacket or a reaction tank with a heater is used. The reaction tank (reaction vessel) and the stirring blades for stirring the reaction solution are required to be made of an inert material that is as unlikely to cause nucleation on their surfaces when in contact with the reaction solution from the viewpoint of not interfering with the action of the nucleating agent, and further to have excellent strength and thermal conductivity. To satisfy these requirements, for example, a metal container (e.g., a Teflon (registered trademark)-coated stainless steel container) or a stirring blade (e.g., a Teflon (registered trademark)-coated stainless steel stirring blade) coated with a fluororesin (e.g., PTFE, PFA) is suitable.
[0096] (a) Preparation of reaction solution First, the starting materials, ie, the magnetic metal source, the nucleating agent, the complexing agent, the reducing agent, the pH adjuster, and optionally the amine compound, are dissolved in water as necessary and then mixed to prepare a reaction liquid. It is preferable to use high-purity water for the preparation of this reaction liquid in order to reduce the amount of impurities in the final alloy powder. As high-purity water, pure water with a conductivity of 1 μS / cm or less or ultrapure water with a conductivity of 0.06 μS / cm or less can be used, and among them, it is preferable to use pure water, which is inexpensive and easily available.
[0097] When the starting materials are solid, such as iron salts, nickel salts, cobalt salts, and alkali hydroxides, it is preferable to preliminarily mix and dissolve them in water to form an aqueous solution. The starting materials and water may be mixed by a known method such as stirring and mixing. The procedure for mixing the starting materials and the aqueous solution is not particularly limited as long as the homogeneity of the reaction solution is not impaired. However, from the viewpoint of ensuring the homogeneity of the reaction solution, it is preferable to prepare aqueous solutions containing each starting material separately in advance and mix the prepared aqueous solutions, and it is particularly preferable to prepare the reaction solution according to the first or second embodiment described below.
[0098] In the first embodiment, when preparing a reaction solution in the crystallization step, a metal salt raw material solution in which a magnetic metal source, a nucleating agent, and a complexing agent are dissolved in water, a reducing agent solution in which a reducing agent is dissolved in water, and a pH adjustment solution in which a pH adjustment agent is dissolved in water are prepared, and the metal salt raw material solution and the pH adjustment solution are mixed to prepare a mixed solution, and the resulting mixed solution and the reducing agent solution are mixed. Figures 2 and 3 show process diagrams showing an example of the preparation of the reaction solution and the production of the alloy powder in the first embodiment.
[0099] In the first embodiment, three solutions, a metal salt raw material solution, a reducing agent solution, and a pH adjusting solution, are prepared separately. The metal salt raw material solution is prepared by dissolving a magnetic metal source (water-soluble iron salt, water-soluble nickel salt, etc.), a nucleating agent (a water-soluble salt of a metal more noble than nickel), and a complexing agent (hydroxycarboxylic acid, etc.) in water. The reducing agent solution is prepared by dissolving a reducing agent (hydrazine) in water. The pH adjusting solution is prepared by dissolving a pH adjusting agent (alkali hydroxide) in water. Next, the metal salt raw material solution and the pH adjusting solution are mixed to prepare a mixed solution. At this time, the salt of the magnetic metal (water-soluble iron salt, water-soluble nickel salt, etc.) contained in the metal salt raw material solution reacts with the alkali hydroxide contained in the pH adjusting agent to form a hydroxide of the magnetic metal. The hydroxides are iron hydroxide (Fe(OH)2), nickel hydroxide (Ni(OH)2), cobalt hydroxide (Co(OH)2), iron nickel hydroxide ((Fe, Ni)(OH)2), iron nickel cobalt hydroxide ((Fe, Ni, Co)(OH)2), etc. After that, a reducing agent solution is mixed with the resulting mixed solution to make a reaction solution.
[0100] As a specific preparation procedure for the reaction solution in the first embodiment, it is preferable to sequentially add and mix the pH adjusting solution and the reducing agent solution to the metal salt raw material solution. In the first embodiment using three types of solutions, the metal salt raw material solution, the reducing agent solution, and the pH adjusting solution, the metal salt raw material solution has the largest liquid amount (volume). Therefore, by sequentially adding other solutions to the metal salt raw material solution having a larger liquid amount and mixing them, a more uniform mixed state can be achieved than by adding the metal salt raw material solution to the other solutions, and the reduction reaction can be uniformly promoted in the reaction solution.
[0101] When an amine compound is added, it is sufficient to add the amine compound to at least one of the metal salt raw material solution, the reducing agent solution, and the pH adjusting solution. Alternatively, the amine compound may be added after all of these solutions are mixed. Fig. 2 shows an embodiment in which an amine compound is added to at least one of the metal salt raw material solution, the reducing agent solution, and the pH adjusting solution. Fig. 3 shows an embodiment in which an amine compound is added to a reaction liquid obtained by mixing all of the metal salt raw material solution, the reducing agent solution, and the pH adjusting solution.
[0102] In the first embodiment, a reaction solution is prepared by mixing a reducing agent solution with a mixed solution of a metal salt raw material solution and a pH adjuster, and a reduction reaction proceeds from the time when the reducing agent solution is added. When the reducing agent solution is mixed, the reducing agent (hydrazine) concentration rises sharply locally in a small area where the reducing agent is added. The mixed solution also contains a pH adjuster (alkali hydroxide), and in the initial stage of mixing the reducing agent solution with this mixed solution, the pH of the mixed solution (reaction solution) is still high. As mentioned above, the higher the pH, the stronger the reducing agent (hydrazine) exerts reducing power. Therefore, in the initial stage of mixing the reducing agent solution, the reducing agent concentration and pH become locally high, and nucleation due to the nucleating agent and a reduction reaction that generates crystallized powder occur rapidly. On the other hand, as the reducing agent solution is added, the pH of the mixed solution (reaction solution) gradually decreases. Therefore, in the final stage of mixing the reducing agent solution, the reducing power of the reducing agent is not as strong as in the initial stage, and nucleation and reduction reaction proceed slowly. Therefore, a difference occurs in the reducing power of the reducing agent between the initial stage and the final stage of mixing the reducing solution.
[0103] If the difference in reducing power between the initial stage and the final stage is large, the uniformity of the nucleation reaction and the reduction reaction may decrease, and the powder properties (particle size, surface smoothness, etc.) of the obtained crystallized powder may vary widely. Therefore, it is desirable to reduce the difference in reducing power as much as possible. For this purpose, it is preferable to mix the reducing agent solution as quickly as possible. The time required to mix the reducing agent solution with the mixed solution of the metal salt raw material solution and the pH adjuster (mixing time) is preferably 180 seconds or less, more preferably 120 seconds or less, and even more preferably 60 seconds or less. On the other hand, due to the constraints of the manufacturing equipment, it may be difficult to shorten the mixing time excessively. The mixing time may be 1 second or more, 3 seconds or more, or 5 seconds or more.
[0104] In addition, when mixing the metal salt raw material solution with the pH adjuster solution, if the mixing time is long, the characteristics of the magnetic metal hydroxide formed may vary, which may lead to variations in the powder characteristics of the crystallized powder. The effect is not as great as when mixing the reducing agent solution, but the shorter the mixing time, the better. The time required to mix the pH adjuster (mixing time) is preferably 180 seconds or less, more preferably 120 seconds or less, and even more preferably 80 seconds or less. The mixing time may be 1 second or more, 3 seconds or more, or 5 seconds or more.
[0105] In order to suppress the variation in the powder properties of the crystallized powder, it is also effective to perform stirring and mixing by stirring the reducing agent solution and pH adjuster solution while mixing. Stirring can suppress a sudden increase in the concentration of components in the solution, making it possible to suppress the variation in the properties of the crystallized powder. Stirring and mixing can be performed using a stirring device such as a stirring blade.
[0106] In the second embodiment, when preparing a reaction solution in the crystallization step, a metal salt raw material solution in which a magnetic metal source, a nucleating agent, and a complexing agent are dissolved in water, and a reducing agent solution in which a reducing agent and a pH adjuster are dissolved in water are prepared, and the metal salt raw material solution and the reducing agent solution are mixed. Figures 4 and 5 show process diagrams showing an example of the preparation of the reaction solution and the production of the alloy powder in the second embodiment.
[0107] In the second embodiment, two solutions, a metal salt raw material solution and a reducing agent solution, are prepared separately. The metal salt raw material solution is prepared by dissolving a magnetic metal source (a water-soluble iron salt, a water-soluble nickel salt, etc.), a nucleating agent (a water-soluble salt of a metal more noble than nickel), and a complexing agent (a hydroxycarboxylic acid, etc.) in water. The reducing agent solution is prepared by dissolving a reducing agent (hydrazine) and a pH adjuster (alkali hydroxide) in water. The metal source raw material solution and the reducing agent solution are then mixed to prepare a reaction solution. The second embodiment differs from the first embodiment in that the reducing agent solution contains a pH adjuster.
[0108] As a specific preparation procedure of the reaction solution in the second embodiment, two methods are possible: adding a reducing agent solution to a metal salt raw material solution and mixing them, or conversely, adding a metal salt raw material solution to a reducing agent solution and mixing them. Unlike the first embodiment, the liquid amount (volume) of the reducing agent solution containing both a reducing agent and a pH adjuster (alkali hydroxide) is at the same level as the liquid amount (volume) of the metal salt raw material solution. Therefore, by adding and mixing one of them to the other, a basically uniform mixed state can be achieved, and a uniform reduction reaction can be promoted in the reaction solution.
[0109] However, under crystallization conditions where the mixing ratio of the reducing agent or pH adjuster (alkali hydroxide) to the metal salt raw material is high, it is preferable to add the metal salt raw material solution to the reducing agent solution and mix them. This is because, from the viewpoint of ensuring the productivity of the crystallization process, it is desirable to maintain the metal salt raw material concentration in the reaction solution at a predetermined level or higher (30 to 40 g / L of metal components). That is, under the above-mentioned crystallization conditions, the liquid amount (volume) of the reducing agent solution is considerably larger than the liquid amount (volume) of the metal salt raw material solution. Therefore, adding and mixing the metal salt raw material solution with a smaller liquid amount (volume) to the reducing agent solution with a larger liquid amount (volume) can realize a uniform mixed state and allow the reduction reaction to proceed uniformly in the reaction solution.
[0110] In the second embodiment, for the same reason as in the first embodiment, the time required to mix the metal salt solution with the reducing agent solution (mixing time) is preferably 180 seconds or less, more preferably 120 seconds or less, and even more preferably 60 seconds or less. The mixing time may be 1 second or more, 3 seconds or more, or 5 seconds or more. It is also effective to mix the reducing agent solution by stirring.
[0111] In the third embodiment, in the crystallization step of the first or second embodiment, an additional raw material liquid is further added to and mixed with the reaction liquid before the reduction reaction is completed. This makes the surface of the crystallized powder rich in nickel and cobalt components. Here, the additional raw material liquid is at least one of the water-soluble nickel salt and the water-soluble cobalt salt described above dissolved in water. A process diagram showing an example of the production of the alloy powder in the third embodiment is shown in FIG. 6.
[0112] In the third embodiment, an additional raw material liquid is prepared in addition to the solution used in the preparation of the reaction liquid in the first embodiment or the second embodiment. This additional raw material liquid is prepared by dissolving at least one of a water-soluble nickel salt and a water-soluble cobalt salt in water. The additional raw material liquid may be added to the reaction liquid in one go, in portions, and / or by dropwise addition. Although not essential, the addition is preferably performed before the reduction reaction is completed. When the reduction reaction is completely completed, the crystallized particles start to form aggregates. Adding the additional raw material liquid at this timing to advance the precipitation of the metal component by the reduction reaction may strengthen the bond between the particles contained in the aggregates.
[0113] Moreover, the third embodiment has an advantage that the amount of the reducing agent used can be reduced compared to the first and second embodiments. Iron ions (or iron hydroxide) are less easily reduced than nickel ions (or nickel hydroxide) and cobalt ions (or cobalt hydroxide). This is because adding an additional raw material liquid containing a nickel component or a cobalt component to the reaction liquid can promote the reduction reaction of the iron ions (or iron hydroxide), which are less easily reduced, toward the end of the crystallization.
[0114] The amount of magnetic metals (Ni, Co) in the additional raw material liquid may be set according to the degree to which the crystallized powder surface is enriched in nickel or cobalt components. However, considering the composition uniformity of the entire particle, it is preferable that the amount is 5 mol% to 50 mol% with respect to the total amount of magnetic metals (Ni, Co) excluding iron in the alloy powder. When the particle surface becomes rich in nickel or cobalt components, the iron component that is likely to form a porous oxide film decreases. Therefore, a dense oxide film is formed and the amount of oxidation of the particle surface is suppressed, so not only is it more stable in the air, but magnetic properties such as saturation magnetic flux density are also improved.
[0115] (b) Crystallization of crystallized powder When the reaction solution is prepared, a reduction reaction occurs in the reaction solution. That is, in the presence of a pH adjuster (alkali hydroxide) and a nucleating agent (a salt of a metal more noble than nickel), the ions and complex ions of the magnetic metal source are reduced by a reducing agent (hydrazine), thereby forming a crystallized powder containing the magnetic metal.
[0116] The reduction reaction in the crystallization process will be explained using reaction formulas. The reduction reactions of iron (Fe), nickel (Ni) and cobalt (Co) are two-electron reactions as shown in the following formulas (2) to (4). On the other hand, the reaction of hydrazine (N2H4) as a reducing agent is a four-electron reaction as shown in the following formula (5).
[0117]
number
number
number
number
[0118] When a magnetic metal chloride (FeCl2, NiCl2, CoCl2) is used as a magnetic metal source and sodium hydroxide (NaOH) is used as a pH adjuster, as shown in the following formula (6), a neutralization reaction occurs between the magnetic metal chloride and sodium hydroxide, producing hydroxides (Fe, Ni, Co)(OH)2, etc.). Then, this hydroxide (Fe, Ni, Co)(OH)2, etc.) is reduced by the action of a reducing agent (hydrazine) to become a crystallized powder. 0.5 moles of reducing agent (hydrazine) are required to reduce 1 mole of magnetic metal (Fe, Ni, Co). Also, as can be seen from the above formula (5), the higher the alkalinity (pH), the higher the reducing power of hydrazine. Therefore, sodium hydroxide used as a pH adjuster also has the effect of promoting the reduction reaction by hydrazine.
[0119]
number
[0120] In the reduction reaction of the above formula (6), the reduction of the ions (or hydroxides) of each element of the magnetic metals (Fe, Ni, Co) proceeds simultaneously to some extent due to co-reduction. Here, co-reduction refers to a phenomenon in which the reduction reaction of one element occurs concomitantly with the reduction reaction of another element. However, as mentioned above, iron ions (or iron hydroxide) are less easily reduced than nickel ions (or nickel hydroxide) and cobalt ions (or cobalt hydroxide). Therefore, at the end of the crystallization reaction, nickel ions (or nickel hydroxide) and cobalt ions (or cobalt hydroxide) tend to be consumed and disappeared in the reduction reaction in the reaction solution, and iron ions (or iron hydroxide) tend to remain. This tendency is particularly noticeable when the iron content is high (for example, the iron content of the alloy powder is over 60 mol%). When such a phenomenon occurs, not only does it take a long time to complete the crystallization reaction (reduction reaction), but a gradient structure with a non-uniform composition is easily formed within the particles. When a gradient structure is formed, the center of the particles of the obtained alloy powder has a composition rich in nickel and cobalt, and the composition becomes richer in iron as it approaches the particle surface.
[0121] In contrast, in the third embodiment described above, the additional raw material liquid is added to the reaction solution during the crystallization reaction to promote the reduction reaction of the iron ions (or iron hydroxide), which are difficult to reduce, toward the end of the crystallization process. This makes it possible to improve the time required for the crystallization reaction (reduction reaction) and the compositional non-uniformity within the obtained alloy powder particles, particularly when the iron content is high.
[0122] The temperature of the reaction solution at the start of crystallization of the crystallized powder (reaction start temperature) is preferably 40°C to 90°C, more preferably 50°C to 80°C, and even more preferably 60°C to 70°C. Here, the reaction solution at the start of crystallization refers to a reaction solution containing the starting material and water immediately after preparation. In addition, the temperature of the reaction solution maintained during crystallization after the start of crystallization (reaction holding temperature) is preferably 60°C to 99°C, more preferably 70°C to 95°C, and even more preferably 80°C to 90°C. In order to adjust the reaction start temperature within a suitable range, it is desirable to preheat at least one of the multiple solutions such as the metal salt raw material solution and the reducing agent solution used in the preparation of the reaction solution. In order to adjust the reaction holding temperature within a suitable range, it is desirable to continue heating the reaction solution after the preparation of the reaction solution.
[0123] From the viewpoint of obtaining crystallized powder with a sharp particle size distribution by making nucleation more uniform, it is preferable to preheat one of the multiple solutions such as the metal salt raw material solution and the reducing agent solution (for example, heated to 70°C) and not preheat the other solution (for example, kept at 25°C), and then add and mix them to prepare a reaction solution at a predetermined temperature (for example, 55°C). In contrast, if both of the two solutions (for example, the metal salt raw material solution and the reducing agent solution) are preheated (for example, heated to 70°C), non-uniform nucleation is likely to occur. That is, when the two solutions are added and mixed, heat is generated by mixing the solutions. Therefore, the added and mixed solution (reaction solution) becomes locally hot (for example, about 78°C) at the start of mixing, and nucleation occurs instantly. The two solutions are added and mixed while nucleation is occurring, and this state is likely to cause non-uniform nucleation.
[0124] Although it is possible to improve the uniformity of nucleation by extremely shortening the addition time of the two solutions or by strongly stirring them, such a method is not necessarily a preferable embodiment. In the method of preparing a reaction solution by preheating only one of the solutions (for example, heating to 70°C) and then adding and mixing the two solutions, the added and mixed solution (reaction solution) is maintained at a low temperature (for example, 55°C) and is not locally heated. Since the timing of nucleation is delayed, nucleation proceeds after the two solutions are well mixed. Therefore, nucleation is likely to occur uniformly. The above is a more preferable example, and does not exclude the case where all of the multiple solutions such as the metal salt raw material solution and the reducing agent solution are preheated. The heating of the solution and its temperature may be set so that the reaction start temperature and the reaction holding temperature are within the ranges described above.
[0125] If the reaction initiation temperature is too low, the nucleation becomes more uniform, but the reduction reaction proceeds slowly, and the heating time required to raise the temperature to the reaction holding temperature at which the reduction reaction can be promoted becomes long. Similarly, if the reaction holding temperature is too low, the reduction reaction proceeds slowly, and the heating time required for crystallization becomes long. In either case, the cycle time required in the crystallization process becomes long, and productivity decreases. In addition, since the self-decomposition of hydrazine proceeds, a large amount of hydrazine is required, and as a result, the production cost increases. If the reaction initiation temperature or reaction holding temperature is high, the reduction reaction is promoted, the cycle time required in the crystallization process is shortened, and the obtained crystallized powder tends to be highly crystallized. However, at the same time, the self-decomposition rate of hydrazine increases. Therefore, if the reaction initiation temperature or reaction holding temperature is too high, not only will the nucleation become non-uniform, but the smoothness of the particle surface will deteriorate due to excessive high crystallization, and the surface irregularities may become large. In addition, if the crystallization is not terminated at an appropriate time, the hydrazine may self-decompose due to the reduction reaction and be consumed preferentially. Therefore, a large amount of hydrazine is required, which may lead to an increase in production costs. By setting the reaction initiation temperature and reaction holding temperature within the above-mentioned preferred ranges, it is possible to produce high-performance alloy powders at low cost while maintaining high productivity.
[0126] <Recovery process> In the recovery step, the crystallized powder is recovered from the reaction solution obtained in the crystallization step. The recovery of the crystallized powder may be performed by a known method. For example, a method of separating the crystallized powder from the reaction solution using a separation device such as a Denver filter, a filter press, a centrifuge, or a decanter may be used. The crystallized powder may be washed during or after solid-liquid separation. The washing may be performed using a washing liquid. High-purity pure water having a conductivity of 1 μS / cm or less may be used as the washing liquid. The washed crystallized powder may be subjected to a drying treatment. The drying treatment may be performed using a general-purpose drying device such as an atmospheric dryer, a hot air dryer, an inert gas atmosphere dryer, a reducing gas atmosphere dryer, or a vacuum dryer at a temperature of 40° C. to 150° C., preferably 50° C. to 120° C. However, from the viewpoint of preventing deterioration of magnetic properties due to excessive oxidation of the crystallized powder during the drying process, it is preferable to use an inert gas atmosphere dryer, a reducing gas atmosphere dryer, or a vacuum dryer rather than an air dryer or a hot air dryer using air.
[0127] In addition, the crystallized powder dried in the closed container of an inert gas atmosphere dryer, a reducing gas atmosphere dryer, or a vacuum dryer has a particle surface that is not oxidized much. Therefore, if the crystallized powder is taken out of the dryer into the air immediately after drying, the particle surface will be rapidly oxidized, and the crystallized powder may burn due to the heat generated by the oxidation reaction. This phenomenon is particularly likely to occur with fine crystallized powder (for example, particle size 0.1 μm or less). Therefore, it is desirable to perform a gradual oxidation treatment on the particle surface of the crystallized powder, which is not oxidized much after drying, by forming a thin oxide film in advance and stabilizing it. As a specific procedure for the gradual oxidation treatment, the temperature of the crystallized powder that has been heated and dried in the closed container of an inert gas atmosphere dryer, a reducing gas atmosphere dryer, or a vacuum dryer is lowered to room temperature to about 40°C, and then a gas with a low oxygen concentration (for example, nitrogen gas or argon gas containing 0.1 to 2 volume% oxygen) is supplied into the closed container, and the particle surface of the crystallized powder is slowly oxidized little by little to form a thin oxide film. The crystallized powder that has been subjected to the gradual oxidation treatment is less susceptible to oxidation and is stable, so there is no risk of it generating heat or burning even if it is left in the air.
[0128] <High-temperature heat treatment process> After the recovery step or during the recovery step, a high-temperature heat treatment step may be provided in which the crystallized powder is subjected to a high-temperature heat treatment. When the high-temperature heat treatment is performed after the recovery step, the high-temperature heat treatment may be performed after the drying treatment. When the high-temperature heat treatment is performed during the recovery step, the high-temperature heat treatment may be performed instead of the drying treatment. The high-temperature heat treatment may be performed at a temperature of more than 150°C and not more than 400°C, preferably 200°C or more and not more than 350°C, in an inert atmosphere, a reducing atmosphere, or a vacuum atmosphere. The high-temperature heat treatment can promote the diffusion of different elements such as Fe and Ni in the iron (Fe)-nickel (Ni)-based alloy particles, thereby improving the composition uniformity within the particles, or adjusting magnetic properties such as magnetic force. If necessary, the above-mentioned gradual oxidation treatment may be performed after the high-temperature heat treatment.
[0129] <Crushing process> If necessary, a crushing step may be provided in which the crystallized powder recovered in the recovery step or the crystallized powder before the drying step is subjected to a crushing treatment during the recovery step. When the alloy particles constituting the crystallized powder are precipitated in the crystallization step, the alloy particles may come into contact with each other and fuse to form aggregated particles. Therefore, the crystallized powder obtained through the crystallization step may contain coarse aggregated particles. As described above, coarse aggregated particles may have eddy currents flowing therethrough, which may increase the loss due to Joule heat or inhibit the packing property of the powder. The aggregated particles can be crushed by providing a crushing step after or during the recovery step. Crushing may be performed using dry crushing such as spiral jet crushing and counter jet mill crushing, wet crushing such as high-pressure fluid collision crushing, or other general-purpose crushing methods. Dry crushing can be applied directly to the crystallized powder recovered in the recovery step as a dry powder. In addition, if the crystallized powder as a dry powder after the recovery step is made into a slurry, wet crushing can be applied to it. Furthermore, if the slurry-like crystallized powder is obtained during the recovery process before drying, wet crushing can be applied as is. In these crushing methods, the collision energy of the particles is utilized to break down the aggregated particles. The collision also smooths the surface during the crushing process, which also helps improve the packing ability of the powder.
[0130] <Insulation coating process> If necessary, an insulating coating step may be provided after the recovery step. In the insulating coating step, the crystallized powder obtained through the recovery step is subjected to an insulating coating treatment to form an insulating coating layer made of a highly resistive metal oxide on the particle surface of the crystallized powder, thereby improving the insulation between the particles. Similar to the increase in loss due to eddy currents in coarse agglomerated particles, in a powder core obtained by compression molding an iron-nickel alloy powder, there is a risk that eddy currents flowing between particles due to contact between the alloy particles will increase. By forming an insulating coating layer, it is possible to suppress the generation of eddy currents due to contact between the alloy particles.
[0131] In the insulating coating process, the crystallized powder is dispersed in a mixed solvent containing water and an organic solvent, and a metal alkoxide is added to and mixed with the mixed solvent to prepare a slurry. In the obtained slurry, the metal alkoxide is hydrolyzed and dehydration polycondensed to form an insulating coating layer on the particle surface of the crystallized powder. Then, the cake-like crystallized powder on which the insulating coating layer is formed is solid-liquid separated from the slurry, and the separated crystallized powder is dried to recover the crystallized powder on which the insulating coating layer made of a highly resistant metal oxide is formed. If necessary, the separated and dried crystallized powder may be subjected to a heat treatment. Since the hydrolysis reaction of the metal alkoxide in the mixed solvent containing water and an organic solvent proceeds very slowly as it is, a small amount of a hydrolysis catalyst such as an acid or a base (alkali) is generally added to promote the reaction. In this embodiment, it is also preferable to add a base catalyst (alkali catalyst).
[0132] As the high-resistance metal oxide, those containing at least one selected from the group consisting of silicon dioxide (SiO2), aluminum oxide (Al2O3), zirconium oxide (ZrO2), and titanium dioxide (TiO2) as a main component are preferable. In particular, those containing silicon dioxide (SiO2) as a main component are particularly preferable because they are inexpensive and have excellent insulating properties.
[0133] In order to obtain such a metal oxide, the metal alkoxide used in the slurry for the insulating coating treatment is selected from alkoxides that can finally form a metal oxide by hydrolysis and dehydration polycondensation. Specifically, those mainly composed of at least one selected from the group consisting of silicon alkoxides (alkyl silicates), aluminum alkoxides (alkyl aluminates), zirconium alkoxides (alkyl zirconates), and titanium alkoxides (alkyl titanates) are preferred, and among them, those mainly composed of silicon alkoxides (alkyl silicates) are particularly preferred. If necessary, a small amount of a component (e.g., boron alkoxide) that is incorporated into the insulating coating layer by hydrolysis or the like when the metal alkoxide is hydrolyzed and dehydration polycondensed to form the insulating coating layer may be added to the above-mentioned metal alkoxide.
[0134] The surface of the insulating coated alloy powder is covered with a highly resistant metal oxide, which is an inorganic substance. If necessary, an organic functional group may be introduced into the surface of the inorganic substance. Specifically, for example, a small amount of a silicon-, titanium-, zirconium-, or aluminum-based coupling agent is added to the metal alkoxide used in the insulating coating treatment, and the organic functional group is incorporated into the metal oxide during hydrolysis and dehydration condensation polymerization of the metal alkoxide. Another method is to surface treat the insulating coated alloy powder with the above-mentioned coupling agent to modify the metal oxide surface with an organic functional group. In either method, the introduction of an organic functional group increases the affinity with the resin, so that the strength of the molded body can be expected to be improved when the insulating coated alloy powder is mixed with a resin binder or the like and molded.
[0135] Specific examples of silicon alkoxides (alkyl silicates) include tetramethoxysilane (also known as tetramethyl orthosilicate, silicon tetramethoxide) (abbreviation: TMOS) (Si(OCH3)4), tetraethoxysilane (also known as tetraethyl orthosilicate, silicon tetraethoxide) (abbreviation: TEOS) (Si(OC2H5)4), tetrapropoxysilane (also known as tetrapropyl orthosilicate, silicon tetrapropoxide) (Si(OC3H7)4), tetrabutoxysilane (also known as tetrabutyl orthosilicate, and silicon tetrapropoxide) (Si(OC3H7)4), Examples of the alkylsilane include one or more selected from the group consisting of tetraethoxysilane (Si(OC4H9)4), tributyl ether (Tetrabutyl ether) (Si(OC4H9)4), etc. Furthermore, alkoxides in which the alkoxyl group of these alkoxides is substituted with another alkoxyl group may be used, or commercially available alkyl silicates as silicate oligomers that have already been polymerized to 4-5 monomers (for example, Ersilicate 40 (trade name), Ersilicate 48 (trade name), Methylsilicate 51 (trade name), etc., manufactured by Colcoat Co., Ltd.) may be used. Among these, tetraethoxysilane (TEOS) is preferred because it is less harmful, easily available, and inexpensive.
[0136] Specific examples of aluminum alkoxides (alkyl aluminates) include one or more selected from aluminum trimethoxide (Al(OCH3)3), aluminum triethoxide (Al(OC2H5)3), aluminum triisopropoxide (Al(O-iso-C3H7)3), aluminum tri-n-butoxide (Al(On-C4H9)3), aluminum tri-sec-butoxide (Al(Os-C4H9)3), aluminum tri-tert-butoxide (Al(Ot-C4H9)3), and the like.
[0137] Specific examples of zirconium alkoxides (alkyl zirconates) include one or more selected from zirconium tetraethoxide (Zr(OC2H5)4), zirconium tetra-n-propoxide (Zr(On-C3H7)4), zirconium tetraisopropoxide (Zr(O-iso-C3H7)4), zirconium tetra-n-butoxide (Zr(On-C4H9)4), zirconium tetra-tert-butoxide (Zr(Ot-C4H9)4), zirconium tetraisobutoxide (Zr(O-iso-C4H9)4), and the like.
[0138] Specific examples of titanium alkoxides (alkyl titanates) include one or more selected from titanium tetramethoxide (Ti(OCH3)4), titanium tetraethoxide (Ti(OC2H5)4), titanium tetraisopropoxide (Ti(O-iso-C3H7)4), titanium tetraisobutoxide (Ti(O-iso-C4H9)4), titanium tetra-n-butoxide (Ti(On-C4H9)4), titanium tetra-tert-butoxide (Ti(Ot-C4H9)4), titanium tetra-sec-butoxide (Ti(Os-C4H9)4), and the like.
[0139] Other metal alkoxides include one or more selected from boron alkoxides (alkyl boronates), such as boron trimethoxide (B(OCH3)3), boron triethoxide (B(OC2H5)3), and boron tri-tert-butoxide (B(Ot-C4H9)3).
[0140] The organic solvent used in the slurry for the insulating coating process is preferably one that forms a mixed solvent with water and dries moderately easily. In other words, it is preferable that the organic solvent has high compatibility with water and a relatively low boiling point (about 60°C to 90°C). In addition, it is preferable that the organic solvent is safe, easy to handle, easily available, and inexpensive. Considering these points, denatured alcohol containing ethyl alcohol as the main component is preferable.
[0141] The hydrolysis reaction and dehydration condensation polymerization reaction of metal alkoxide in the insulating coating process are explained using reaction formulas for the case where silicon alkoxide (Si(OR)4, R: alkyl group) is used as the metal alkoxide.
[0142] In a hydrolysis reaction, in the presence of a base catalyst (alkali catalyst) such as ammonia (NH3), silicon atoms (Si) convert to nucleophilic hydroxy ions (OH - Upon direct attack by the silicon atom, one of the alkoxy groups (-OR) is first hydrolyzed. This reduces the charge on the silicon atom, and the nucleophilic hydroxyl ion (OH - ) becomes increasingly susceptible to attack. As a result, all four alkoxy groups (-OR) are hydrolyzed and converted into silanol groups (Si-OH), as shown in formula (8) below. In this way, when a base catalyst (alkali catalyst) is used, all alkoxy groups (-OR) in the hydrolyzed silicon alkoxide molecules are hydrolyzed, resulting in a state in which completely hydrolyzed molecules (Si(OH)4) and completely unhydrolyzed molecules (Si(OR)4) coexist in the slurry.
[0143]
number
number
[0144] On the other hand, in the presence of an acid catalyst such as nitric acid (HNO3), the protons (H + The protonation of the alkoxy group (-OR) by silanol makes the silicon atom (Si) more susceptible to attack by water (HO). Therefore, one of the alkoxy groups (-OR) is hydrolyzed first to become a silanol group (Si-OH). I will not go into the details here, but when this happens, the charge on the silicon atom and the charge on the oxygen atom (O) decrease, so the proton (H +) is less likely to be attacked. Therefore, the next hydrolysis does not occur immediately, and the alkoxy group (-OR) of other unhydrolyzed silicon alkoxide molecules is more likely to undergo hydrolysis. Thus, when an acid catalyst is used, hydrolysis of the alkoxy group (-OR) proceeds evenly in all silicon alkoxide molecules as shown in the following formula (10). Therefore, there are no completely hydrolyzed molecules or molecules that have not been hydrolyzed at all, and a state where evenly hydrolyzed molecules (Si(OH) X (OR) 4-X ; 0 < x < 4) exists in the slurry.
[0145]
Number
Number
[0146] The dehydration condensation polymerization reaction is a reaction in which the formation of a siloxane bond (Si-O-Si) proceeds by the dehydration condensation polymerization reaction of silanol groups (Si-OH) between hydrolyzed silicon alkoxide molecules as shown in the following formula (11). When this dehydration condensation polymerization reaction proceeds to completion, silicon dioxide (SiO2) is generated as shown in the following formula (12).
[0147]
Number
Number
[0148] Summarizing the above, when the hydrolysis and dehydration condensation polymerization of silicon alkoxide are completed, silicon dioxide (SiO2) and alcohol are produced as shown in the following formula (13). For example, when tetraethoxysilane (TEOS: Si(OR)4, R: C2H5) is used, silicon dioxide (SiO2) and ethyl alcohol (C2H5OH) are produced.
[0149]
Number
[0150] The above formula (13) holds regardless of whether it is a base catalyst (alkali catalyst) or an acid catalyst as long as the silicon alkoxide is hydrolyzed. However, the form of silicon dioxide (SiO2) generated during the progress of dehydration polycondensation is greatly affected by the hydrolysis state by the above-mentioned hydrolysis catalyst.
[0151] Silicon alkoxide molecules (Si(OH) X (OR) 4-X ; 0 < x < 4) hydrolyzed evenly by an acid catalyst have unhydrolyzed alkoxy groups (-OR) in the molecule. Therefore, when the dehydration polycondensation of silanol groups (Si-OH) between molecules proceeds, a hydrolyzed polymer polymerized into a linear or branched linear form is generated. When this occurs in the slurry during the insulation coating process, a hydrolyzed polymer of silicon alkoxide is generated on the particle surface composed of iron oxide (FeO) or nickel oxide (NiO) of the crystallized powder. However, since these are polymerized into a linear or branched linear form, they are difficult to densify in the solvent of the slurry, and therefore it is not easy to form a dense insulation coating layer.
[0152] On the other hand, when a base catalyst (alkali catalyst) is used, completely hydrolyzed molecules (Si(OH)4) are present. Therefore, when the dehydration condensation polymerization of silanol groups (Si-OH) between molecules progresses, dense hydrolysis polymers that are polymerized in a block form are generated. Therefore, even in the solvent of the slurry in the insulation coating process, dense hydrolysis polymers of silicon alkoxide are generated on the particle surfaces of the iron oxide (FeO) or nickel oxide (NiO) of the crystallized powder, and as a result, a dense insulation coating layer can be formed. In addition, when a base catalyst (alkali catalyst) is used, there is a possibility that molecules (Si(OR)4) that are not hydrolyzed at all may be present. However, as described later, completely unhydrolyzed molecules that remain in the slurry without being consumed by the insulation coating of the crystallized powder in the insulation coating process and hydrolysis polymers (silica sol) of particulate silicon alkoxide with a very small molecular weight are removed from the system together with the filtrate during the filtration and washing in the insulation coating process. Therefore, it does not affect the insulation coating process.
[0153] For the above reasons, it is preferable to use a base catalyst (alkaline catalyst) rather than an acid catalyst for hydrolysis of metal alkoxide in the insulating coating treatment. In this respect, the preferred catalyst is different from that used when coating is performed by applying a solvent to a substrate. In other words, when used as a binder for a coating liquid that is applied to a substrate and the solvent is dried, rather than coating the particle surface in a solvent, it is preferable to use a polymerized linear or branched linear polymerized by the above-mentioned acid catalyst.
[0154] Regarding the timing of hydrolysis of metal alkoxide in the insulating coating treatment, the embodiment in which the crystallized powder and metal alkoxide are uniformly mixed in the slurry and hydrolyzed by a hydrolysis catalyst has been described. However, this embodiment is not limited to the embodiment in which hydrolysis is performed at this timing. For example, it is possible to prepare a metal oxide sol (silica sol in the case of silicon alkoxide) obtained by hydrolyzing the metal alkoxide in advance with a hydrolysis catalyst, and mix this metal oxide sol with the crystallized powder to make a slurry. If the average molecular weight of the metal oxide sol is small, about 500 to 5000, the timing of hydrolysis of the metal alkoxide hardly has any effect. This is because the particle surface of the crystallized powder is covered with small metal oxide sol particles due to the bond between the iron oxide (FeO) or nickel oxide (NiO) on the surface of the crystallized powder and the hydrolysis group of the metal oxide sol (silanol group (Si-OH) in the case of silicon alkoxide), and then polymerization of the sol particles proceeds.
[0155] In the insulating coating process, from the viewpoint of uniformly forming an insulating coating layer, it is preferable to subject the slurry containing the crystallized powder, water, an organic solvent, a metal alkoxide, and a hydrolysis catalyst to a process such as stirring with a stirring blade of a stirrer or stirring by rotating a container using a dedicated roller. The processing time and processing temperature of the insulating coating process vary depending on the type of metal alkoxide to be applied and the required thickness of the insulating coating layer. For example, metal methoxides generally have a higher hydrolysis rate than metal ethoxides. Therefore, the processing time and processing temperature may be appropriately set and are not particularly limited. For example, the processing time may be several hours to one week, and the processing temperature may be room temperature to 60°C. If the processing temperature is high, such as 40°C to 60°C, the processing speed can be increased to several times that at room temperature.
[0156] The thickness of the insulating coating layer is not generally limited because it depends on the required level of insulation. If necessary, it is preferably 1 nm to 30 nm, more preferably 2 nm to 25 nm, and even more preferably 3 nm to 20 nm. If it is too thick, the insulating property will be saturated while the content ratio of the soft magnetic component will decrease, and magnetic properties such as saturation magnetic flux density will simply deteriorate. If the thickness is within the above range, it is possible to exhibit the insulating function of the insulating coating layer without significantly deteriorating properties such as magnetic properties.
[0157] The crystallized powder in which the insulating coating layer is formed by hydrolysis and dehydration polycondensation of the metal alkoxide is separated from the slurry as a cake-like crystallized powder using a known separation device such as a Denver filter, a filter press, a centrifuge, or a decanter. If necessary, the crystallized powder may be washed during solid-liquid separation. For washing, water, an organic solvent such as a relatively low boiling point alcohol, or a mixture thereof may be used as a washing liquid. As described above, if there is a metal alkoxide or its hydrolysis polymer (a metal oxide sol with unhydrolyzed molecules or a small molecular weight) remaining in the slurry without being consumed by the insulating coating, these are removed from the system together with the filtrate and washing waste liquid during solid-liquid separation and washing.
[0158] The cake-like crystallized powder obtained by solid-liquid separation is dried and, if necessary, heated to recover the crystallized powder on which an insulating coating layer made of a highly resistant metal oxide is formed. There are no particular restrictions on the drying as long as excessive oxidation during drying can be suppressed. However, it is preferable to use a drying device such as an inert gas atmosphere dryer, a reducing gas atmosphere dryer, or a vacuum dryer, and the drying can be performed at a temperature of 40°C to 150°C. The higher the drying temperature, the more the dehydration condensation polymerization of the metal alkoxide hydrolysis polymer constituting the insulating coating layer progresses, resulting in a harder, denser, and more insulating metal oxide. If further improvement is desired, a heat treatment of more than 150°C to 450°C or less may be performed in an inert gas atmosphere, a reducing gas atmosphere, or a vacuum. Since the insulating coating layer has already been formed, it is basically not necessary to perform a gradual oxidation treatment after drying.
[0159] The insulating coating treatment significantly improves the insulating properties of crystallized powder (alloy powder). For example, the compact resistivity (applied pressure: 64 MPa) of iron-nickel alloy powder without insulating coating treatment is usually 0.1 Ω·cm or less. However, when this iron-nickel alloy powder is subjected to insulating coating treatment to form an insulating coating layer made of silicon dioxide (SiO2) with a thickness of about 0.015 μm (15 nm), the compact resistivity increases to 10 6 It is improved to more than Ω·cm.
[0160] In this way, the iron (Fe)-nickel (Ni) alloy powder of this embodiment can be manufactured. The manufacturing method of this embodiment is characterized by using a specific nucleating agent (a water-soluble salt of a metal nobler than nickel) that has the effect of finely refining the alloy powder, and a specific complexing agent (such as hydroxycarboxylic acid) that has the effects of promoting reduction reactions, promoting spheroidization, and smoothing the surface, and this makes it possible to improve the powder characteristics while maintaining the magnetic characteristics of the manufactured alloy powder. Specifically, the average particle size of the manufactured alloy powder can be freely controlled, and a fine alloy powder can be obtained. In addition, the obtained alloy powder has a narrow particle size distribution and a uniform particle size. Furthermore, this alloy powder is spherical and has a smooth surface. Therefore, it has excellent packing properties. In addition, although not limited to this, the amount of hydrazine used can be reduced by using an amine compound that functions as a hydrazine self-decomposition inhibitor and a reduction reaction accelerator. Therefore, it is possible to reduce the manufacturing cost and to improve the powder characteristics of the alloy powder.
[0161] <<2. Iron-nickel alloy powder>> The iron (Fe)-nickel (Ni) alloy powder of this embodiment has a small particle size distribution. In addition, the average particle size of this alloy powder can be freely controlled. Therefore, it is easy to refine the powder and the particle size distribution can be narrowed. In addition, the powder is spherical, has high surface smoothness, and has excellent packing properties. The alloy powder of this embodiment, which has such advantages, can be used for various electronic components such as noise filters, choke coils, inductors, and radio wave absorbers, and is particularly suitable as a material for powder cores for choke coils and inductors.
[0162] The average particle size of the alloy powder is preferably 0.10 μm to 0.60 μm, more preferably 0.10 μm to 0.50 μm. By appropriately increasing the average particle size, it is possible to suppress the deterioration of magnetic properties and the decrease in filling property due to surface oxidation. Also, by appropriately decreasing the average particle size, it is possible to suppress eddy current loss.
[0163] The coefficient of variation (CV value) in the particle size distribution of the alloy powder is preferably 25% or less, more preferably 20% or less, and even more preferably 15% or less. Here, the coefficient of variation is an index of particle size variation, and the smaller the coefficient of variation, the narrower the particle size distribution. By keeping the coefficient of variation small, the number of coarse particles and excessively fine particles with large surface oxidation is reduced, so that it is possible to prevent an increase in eddy current loss while maintaining excellent magnetic properties. The coefficient of variation (CV value) is calculated by determining the average particle size and standard deviation in the number particle size distribution of the alloy powder, and using these according to the following formula (14).
[0164]
number
[0165] The green density of alloy powder depends on the composition and particle size of the alloy powder. When the iron content is high, the specific gravity of the alloy decreases, so the density decreases. When the particle size is small, the particles are less likely to pack together, so the green density also tends to decrease. For an iron-nickel alloy powder with an average particle size of 0.3 μm to 0.5 μm and an iron content of 45 mol% to 60 mol% of iron (Fe), which results in a specific gravity of 8.2 to 8.3, the green density (applied pressure: 100 MPa) is 3.60 g / cm. 3 More than 3.70 g / cm is preferable. 3 In the case of an iron-nickel alloy powder having an average particle size of 0.3 μm to 0.5 μm and a specific gravity of 7.9 to 8.0, in which the iron content is 10 mol % to 20 mol % of iron (Fe), the green density (applied pressure: 100 MPa) is 3.45 g / cm 3 More than 3.55 g / cm is preferable. 3As for the particle size of the alloy powder, when the average particle size is reduced from 0.3 μm to 0.5 μm to about 0.2 μm to 0.25 μm, the green density (applied pressure: 100 MPa) is 0.1 g / cm 3 The degree of magnetic flux density tends to decrease. By increasing the green density, it is possible to produce a green core with excellent magnetic properties (magnetic flux density). The crystallite diameter of the alloy powder is preferably 30 nm or less, more preferably 10 nm or less. By suppressing the crystallite diameter to a moderately small size, it is possible to easily obtain a small coercive force like an amorphous soft magnetic material. The saturation magnetic flux density of the alloy powder is preferably 1 T (tesla) or more, more preferably 1.2 T or more, and even more preferably 1.5 T (tesla) or more. It is even more preferable if it is equal to or higher than the saturation magnetic flux density of pure iron powder (1.95 T to 2.0 T). By increasing the saturation magnetic flux density of the alloy powder, it is possible to increase the magnetic properties (magnetic flux density) of the green core. The coercive force of the alloy powder is preferably 2000 A / m or less, more preferably 1600 A / m or less, and even more preferably 1200 A / m or less. By suppressing the coercive force of the alloy powder, it is possible to prevent an increase in hysteresis loss.
[0166] As mentioned above, iron ions (or iron hydroxide) are less easily reduced than nickel ions (or nickel hydroxide) and cobalt ions (or cobalt hydroxide), so in iron (Fe)-nickel (Ni) alloy powders with a high iron content (for example, alloy powders with an iron content of over 60 mol%), the center of the particle is rich in nickel and cobalt, and the closer to the particle surface, the more iron-rich the composition becomes, so a gradient structure (or core-shell structure) tends to form within the particle. The composition tends to become non-uniform within the particle.
[0167] How does this non-uniform composition within a particle affect the properties of the alloy powder? It does not have a significant effect on magnetic properties (saturation magnetic flux density, coercive force, etc.). For example, saturation magnetic flux density shows a positive correlation with the iron content (the higher the iron content, the higher the saturation magnetic flux density). Therefore, even if the composition becomes non-uniform within a particle, creating areas where the iron content is higher than the average and areas where it is lower than the average, there will also be areas where the saturation magnetic flux density is higher than the average and areas where it is lower than the average, and when averaged across the entire alloy powder, it will be almost the same as if the composition were non-uniform. Also, as for coercive force, the composition dependency in the iron-nickel (-cobalt) system is not that great to begin with, so the degree of non-uniformity in the composition that occurs within a particle will not change it significantly.
[0168] On the other hand, the non-uniform composition within the particles may affect chemical and physical properties such as oxidation resistance and thermal expansion coefficient. As an example of this, with regard to oxidation resistance, for example, if the particle surface has a more iron-rich composition due to the gradient structure, oxidation may progress more easily and oxidation resistance may deteriorate, but if the particle surface can be modified to a nickel-rich composition by the above-mentioned third aspect, oxidation resistance may be improved. Next, regarding the thermal expansion coefficient, unlike the case of saturation magnetic flux density, the thermal expansion coefficient of iron-nickel alloy does not show a positive or negative correlation with the iron content ratio, and is characterized by being very small only when the iron content is around 65 mol% (64 mass%), and an alloy with a low thermal expansion coefficient of this composition is called an Invar alloy (main components are 65 mol% iron and 35 mol% nickel). In the case of this composition, if the composition is non-uniform within the particle, the thermal expansion coefficient will not be small in either the region where the iron content is greater than 65 mol % or the region where it is less than 65 mol %, so when iron (Fe)-nickel (Ni)-based alloy powder is used as Invar alloy powder, it is necessary to homogenize the composition by the above-mentioned high-temperature heat treatment or the like.
[0169] As far as the present inventors know, there is no known method for easily and inexpensively producing iron-nickel alloy powder having such excellent properties. For example, Patent Document 3 discloses a method for producing nickel-iron alloy nanoparticles by a wet method, but this method does not use a nucleating agent made of a water-soluble salt of a metal more noble than nickel, or a complexing agent made of hydroxycarboxylic acid or the like. Therefore, it is presumed that the alloy powder produced by this method has inferior powder characteristics (particle size, particle size distribution, sphericity, particle surface properties). In fact, Patent Document 3 shows a transmission electron microscope photograph of a fine powder as an example sample (Figure 1 of Patent Document 3), and it is estimated from this photograph that the coefficient of variation (CV value) in the particle size distribution of the fine powder is large, about 35%.
[0170] Moreover, in the method of Patent Document 3, which does not use a nucleating agent or a complexing agent, a large amount of reducing agent (hydrazine) must be used to obtain fine alloy powder. In fact, in the example of Patent Document 3, alloy nanoparticles are produced using 16.6 g of nickel chloride hexahydrate, 4.0 g of ferrous chloride tetrahydrate, and 135 g of hydrazine site hydrate as raw materials. Converting from this blending amount, a large amount of hydrazine is blended, about 30 times the total amount of iron and nickel, in molar ratio. In such a method requiring a large amount of hydrazine, the cost of the reducing agent increases significantly, making it impractical. EXAMPLES
[0171] The present invention will be described in more detail with reference to the following examples and comparative examples, but the present invention is not limited to the following examples.
[0172] (1) Preparation of iron-nickel alloy powder [Example 1] In Example 1, an iron-nickel alloy powder (iron-nickel alloy powder) containing 50 mol % of iron (Fe) and 50 mol % of nickel (Ni) was produced according to the procedure shown in Fig. 5. In Example 1, when preparing the reaction solution, a reducing solution at room temperature was added to and mixed with a metal salt raw material solution heated using a water bath.
[0173] <Preparation process> Ferrous chloride tetrahydrate (FeCl2·4H2O, molecular weight: 198.81, reagent manufactured by Wako Pure Chemical Industries, Ltd.) was prepared as a water-soluble iron salt, and nickel chloride hexahydrate (NiCl2·6H2O, molecular weight: 237.69, reagent manufactured by Wako Pure Chemical Industries, Ltd.) was prepared as a water-soluble nickel salt. In addition, ammonium palladium(II) chloride (also known as ammonium tetrachloropalladate(II)) ((NH4)2PdCl4, molecular weight: 284.31, reagent manufactured by Wako Pure Chemical Industries, Ltd.) was prepared as a nucleating agent, trisodium citrate dihydrate (Na3(C3H5O(COO)3)·2H2O, molecular weight: 294.1, reagent manufactured by Wako Pure Chemical Industries, Ltd.) was prepared as a complexing agent, commercial industrial grade 60% by mass hydrazine hydrate (manufactured by Otsuka-MGC Chemical Co., Ltd.) was prepared as a reducing agent, and sodium hydroxide (NaOH, molecular weight: 40.0, reagent manufactured by Wako Pure Chemical Industries, Ltd.) was prepared as a pH adjuster. The 60% by mass hydrazine hydrate was prepared by diluting hydrazine hydrate (N2H4·H2O, molecular weight: 50.06) 1.67 times with pure water. Furthermore, ethylenediamine (EDA; H2NC2H4NH2, molecular weight: 60.1, reagent manufactured by Wako Pure Chemical Industries, Ltd.) was prepared as an amine compound.
[0174] <Crystallization process> (a) Preparation of metal salt source solution A metal salt raw solution containing ferrous chloride tetrahydrate (water-soluble iron salt), nickel chloride hexahydrate (water-soluble nickel salt), palladium (II) chloride ammonium (nucleating agent), trisodium citrate dihydrate (complexing agent) and water was prepared. In this case, in the obtained metal salt raw solution, the amount of palladium (Pd) relative to the total amount of magnetic metals (Fe and Ni) was weighed out to be 0.037 mass ppm (0.02 mol ppm). In addition, the amount of trisodium citrate relative to the total amount of magnetic metals (Fe and Ni) was weighed out to be 0.362 (36.2 mol%) in molar ratio. Specifically, 173.60 g of ferrous chloride tetrahydrate, 207.55 g of nickel chloride hexahydrate, 9.93 μg of palladium (II) chloride ammonium, and 185.9 g of trisodium citrate dihydrate were dissolved in 1200 mL of pure water to prepare the metal salt raw solution.
[0175] (b) Preparation of reducing agent solution A reducing agent solution containing sodium hydroxide (pH adjuster), hydrazine (reducing agent) and water was prepared. At this time, the amount of hydrazine was weighed out so that the molar ratio of the total amount of magnetic metals (Fe and Ni) to the total amount of magnetic metals (Fe and Ni) in the reaction liquid prepared in the subsequent crystallization step was 4.85. The amount of sodium hydroxide was weighed out so that the molar ratio of the total amount of magnetic metals (Fe and Ni) to the total amount of magnetic metals (Fe and Ni) was 4.96. Specifically, 346 g of sodium hydroxide was dissolved in 850 mL of pure water to prepare a sodium hydroxide solution, and 707 g of 60 mass% hydrazine hydrate was added to and mixed with this sodium hydroxide solution to prepare a reducing agent solution.
[0176] (c) Preparation of amine compound solution An amine compound solution containing ethylenediamine (amine compound) and water was prepared. At this time, the amount of ethylenediamine was weighed out so that the molar ratio of the amount of ethylenediamine to the total amount of magnetic metals (Fe and Ni) in the reaction solution prepared in the subsequent crystallization process was a very small amount of 0.01 (1.0 mol%). Specifically, 1.05 g of ethylenediamine was dissolved in 18 mL of pure water to prepare the amine compound solution.
[0177] (d) Preparation of reaction solution and precipitation of crystallized powder The prepared metal salt raw material solution was placed in a Teflon (registered trademark) coated stainless steel container (reaction tank) equipped with stirring blades placed in a water bath and heated while stirring until the liquid temperature reached 70°C. After that, the reducing agent solution with a liquid temperature of 25°C was added to the metal salt raw material solution heated in the water bath for a mixing time of 10 seconds to obtain a reaction liquid with a liquid temperature of 55°C. The concentration of magnetic metals (Fe and Ni) in the reaction liquid was 32.3g / L. This initiated the reduction reaction (crystallization reaction) (reaction start temperature 55°C). As shown in FIG. 7, the temperature of the reaction liquid continued to rise by heating in the water bath after the reaction started, and was kept at a liquid temperature of 70°C after 10 minutes from the start of the reaction (reaction holding temperature 70°C). The color of the reaction liquid was dark green immediately after the start of the reaction (mixing of the reaction liquid), but changed to dark gray after a few minutes. The reason why the color tone turned dark green immediately after the start of the reaction is believed to be because the reaction according to formula (6) above progressed and a coprecipitate of iron hydroxide (Fe(OH)2) and nickel hydroxide (Ni(OH)2) was formed in the reaction solution. Also, the reason why the color tone turned dark gray a few minutes after the start of the reaction is believed to be because nucleation occurred due to the action of the nucleating agent (palladium salt).
[0178] The reduction reaction was allowed to proceed by adding the amine compound solution dropwise to the reaction solution over a period of 10 minutes, from 3 minutes after the start of the reaction, when the color of the reaction solution had changed to dark gray, to 13 minutes after the start of the reaction. This caused iron-nickel crystallized powder to precipitate in the reaction solution. At this point, the reaction solution was black in color, but within 20 minutes after the start of the reaction, the supernatant liquid of the reaction solution became transparent. It is believed that the reduction reaction of the above formula (6) was completed, and all of the iron and nickel components in the reaction solution were reduced to metallic iron and metallic nickel. After the reaction was completed, the reaction solution was a slurry containing iron-nickel crystallized powder.
[0179] <Recovery process> The slurry-like reaction liquid obtained in the crystallization step was subjected to filtration, washing, and solid-liquid separation to recover a cake-like iron-nickel crystallized powder. Filtration and washing were performed using pure water with a conductivity of 1 μS / cm until the conductivity of the filtrate filtered from the slurry was 10 μS / cm or less. The recovered cake-like crystallized powder was dried in a vacuum dryer set at 50°C. The dried crystallized powder was then cooled to 35°C in a vacuum, and nitrogen gas containing 1.0% by volume of oxygen was supplied to the crystallized powder to perform a gradual oxidation treatment. In this way, an iron-nickel alloy powder was obtained. The obtained alloy powder was composed of spherical particles with a smooth surface. The particle size distribution was sharp, and the average particle size was 0.41 μm.
[0180] [Example 2] In Example 2, an iron-nickel alloy powder (iron-nickel-cobalt alloy powder) containing 50 mol % of iron (Fe), 40 mol % of nickel (Ni), and 10 mol % of cobalt (Co) was produced according to the procedure shown in Fig. 3. In Example 2, when preparing a reaction solution, a room temperature pH adjusting solution (alkali hydroxide solution) and then a room temperature reducing agent solution were added to a metal salt raw material solution heated using a water bath, and mixed.
[0181] <Preparation process> The water-soluble iron salt, water-soluble nickel salt, nucleating agent, complexing agent, reducing agent, pH adjuster, and amine compound were prepared in the same manner as in Example 1. In addition, cobalt chloride hexahydrate (CoCl2·6H2O, molecular weight: 237.93, reagent manufactured by Wako Pure Chemical Industries, Ltd.) was prepared as a water-soluble cobalt salt.
[0182] <Crystallization process> (a) Preparation of metal salt source solution A metal salt raw material solution containing ferrous chloride tetrahydrate (water-soluble iron salt), nickel chloride hexahydrate (water-soluble nickel salt), cobalt chloride hexahydrate (water-soluble cobalt salt), palladium (II) ammonium chloride (nucleating agent), trisodium citrate dihydrate (complexing agent) and water was prepared. At this time, in the obtained metal salt raw material solution, the amount of palladium (Pd) was weighed out so that it was 0.037 mass ppm (0.02 mol ppm) with respect to the total amount of magnetic metals (Fe, Ni and Co). In addition, the amount of trisodium citrate was weighed out so that it was 0.362 (36.2 mol%) in molar ratio with respect to the total amount of magnetic metals (Fe, Ni and Co). Specifically, 173.60 g of ferrous chloride tetrahydrate, 166.04 g of nickel chloride hexahydrate, 41.55 g of cobalt chloride hexahydrate, 9.93 μg of palladium (II) ammonium chloride, and 185.9 g of trisodium citrate dihydrate were dissolved in 1200 mL of pure water to prepare a metal salt raw material solution.
[0183] (b) Preparation of reducing agent solution A reducing agent solution containing hydrazine (reducing agent) and water was prepared. At this time, the amount of hydrazine was set so that the molar ratio to the total amount of magnetic metals (Fe, Ni, and Co) in the reaction solution prepared in the subsequent crystallization process was 4.85. Specifically, 707 g of 60 mass% hydrazine hydrate was weighed out to prepare the reducing agent solution.
[0184] (c) Preparation of pH-adjusting solution (alkali hydroxide solution) A pH-adjusted solution (alkali hydroxide solution) containing sodium hydroxide (pH adjuster) and water was prepared. At this time, the amount of sodium hydroxide was weighed out so that the molar ratio of the total amount of magnetic metals (Fe, Ni, and Co) in the reaction solution to be prepared in the subsequent crystallization step would be 4.96. Specifically, 346 g of sodium hydroxide was dissolved in 850 mL of pure water to prepare the pH-adjusted solution.
[0185] (d) Preparation of amine compound solution An amine compound solution containing ethylenediamine (amine compound) and water was prepared. At this time, the ethylenediamine was weighed out so that the molar ratio of the ethylenediamine to the total amount of magnetic metals (Fe, Ni, and Co) in the reaction solution prepared in the subsequent crystallization step was as small as 0.01 (1.0 mol%). Specifically, 1.05 g of ethylenediamine was dissolved in 18 mL of pure water to prepare the amine compound solution.
[0186] (e) Preparation of reaction solution and precipitation of crystallized powder The prepared metal salt raw material solution was placed in a Teflon (registered trademark) coated stainless steel container (reaction tank) equipped with stirring blades placed in a water bath and heated while stirring until the liquid temperature reached 70°C. After that, a pH adjusting solution (alkali hydroxide solution) with a liquid temperature of 25°C was added and mixed for a mixing time of 10 seconds to the metal salt raw material solution being heated in the water bath, and further a reducing agent solution with a liquid temperature of 25°C was added and mixed for a mixing time of 10 seconds to obtain a reaction liquid with a liquid temperature of 55°C. The concentration of magnetic metals (Fe, Ni and Co) in the reaction liquid was 32.3g / L. This initiated the reduction reaction (crystallization reaction) (reaction start temperature 55°C). The temperature of the reaction liquid continued to rise by heating with the water bath after the reaction started, and was kept at a liquid temperature of 70°C after 10 minutes from the start of the reaction (reaction holding temperature 70°C). The color of the reaction liquid was dark green immediately after the start of the reaction (mixing of the reaction liquid), but changed to dark gray after a few minutes. The reason why the color tone turned dark green immediately after the start of the reaction is believed to be because the reaction according to the above formula (6) progressed and a coprecipitate of iron hydroxide (Fe(OH)2), nickel hydroxide (Ni(OH)2), and cobalt hydroxide (Co(OH)2) was formed in the reaction solution. Also, the reason why the color tone turned dark gray a few minutes after the start of the reaction is believed to be because nucleation occurred due to the action of the nucleating agent (palladium salt).
[0187] The reduction reaction was carried out by adding the amine compound solution dropwise to the reaction solution for 10 minutes, from 3 minutes to 13 minutes after the start of the reaction when the color of the reaction solution changed to dark gray. As a result, iron-nickel-cobalt crystallized powder precipitated in the reaction solution. At this time, the color of the reaction solution was black, but within 20 minutes after the start of the reaction, the supernatant liquid of the reaction solution became transparent. It is considered that the reduction reaction of the above formula (6) was completed, and all of the iron, nickel, and cobalt components in the reaction solution were reduced to metallic iron, metallic nickel, and metallic cobalt. After the reaction was completed, the reaction solution was a slurry containing iron-nickel-cobalt crystallized powder.
[0188] <Recovery process> The slurry-like reaction liquid obtained in the crystallization step was subjected to filtration, washing, and solid-liquid separation to recover a cake-like iron-nickel-cobalt crystallized powder. Filtration and washing were performed using pure water with a conductivity of 1 μS / cm until the conductivity of the filtrate filtered from the slurry was 10 μS / cm or less. The recovered cake-like crystallized powder was dried in a vacuum dryer set at 50°C. The dried crystallized powder was then cooled to 35°C in a vacuum, and nitrogen gas containing 1.0% by volume of oxygen was supplied to the crystallized powder to perform a gradual oxidation treatment. In this way, an iron-nickel-cobalt alloy powder was obtained. The obtained alloy powder was composed of spherical particles with a smooth surface. The particle size distribution was sharp, and the average particle size was 0.33 μm.
[0189] [Example 3] In Example 3, an iron-nickel alloy powder (iron-nickel alloy powder) containing 50 mol % of iron (Fe) and 50 mol % of nickel (Ni) was produced according to the procedure shown in Fig. 5. In Example 3, when preparing the reaction solution, a reducing solution at room temperature was added to and mixed with a metal salt raw material solution heated using a water bath.
[0190] <Preparation process> The water-soluble iron salt, water-soluble nickel salt, nucleating agent, reducing agent, pH adjuster, and amine compound were prepared in the same manner as in Example 1. Furthermore, tartaric acid ((CH(OH)COOH)2, molecular weight: 150.09, reagent manufactured by Wako Pure Chemical Industries, Ltd.) was prepared as a complexing agent in place of trisodium citrate dihydrate.
[0191] <Crystallization process> (a) Preparation of metal salt source solution A metal salt raw solution containing ferrous chloride tetrahydrate (water-soluble iron salt), nickel chloride hexahydrate (water-soluble nickel salt), palladium (II) chloride ammonium (nucleating agent), tartaric acid (complexing agent) and water was prepared. In this case, in the obtained metal salt raw solution, the amount of palladium (Pd) was weighed out to be 0.037 mass ppm (0.02 mol ppm) with respect to the total amount of magnetic metals (Fe and Ni). Also, the amount of tartaric acid with respect to the total amount of magnetic metals (Fe and Ni) was weighed out to be 0.200 (20.0 mol%) in molar ratio. Specifically, 173.60 g of ferrous chloride tetrahydrate, 207.55 g of nickel chloride hexahydrate, 9.93 μg of palladium (II) chloride ammonium, and 52.4 g of tartaric acid were dissolved in 1200 mL of pure water to prepare the metal salt raw solution.
[0192] (b) Preparation of reducing agent solution A reducing agent solution containing sodium hydroxide (pH adjuster), hydrazine (reducing agent) and water was prepared. At this time, the amount of hydrazine was weighed out so that the molar ratio of the total amount of magnetic metals (Fe and Ni) to the total amount of magnetic metals (Fe and Ni) in the reaction liquid prepared in the subsequent crystallization step was 4.85. The amount of sodium hydroxide was weighed out so that the molar ratio of the total amount of magnetic metals (Fe and Ni) to the total amount of magnetic metals (Fe and Ni) was 4.96. Specifically, 346 g of sodium hydroxide was dissolved in 850 mL of pure water to prepare a sodium hydroxide solution, and 707 g of 60 mass% hydrazine hydrate was added to and mixed with this sodium hydroxide solution to prepare a reducing agent solution.
[0193] (c) Preparation of amine compound solution An amine compound solution was prepared in the same manner as in Example 1.
[0194] (d) Preparation of reaction solution and precipitation of crystallized powder Using the above metal salt raw material solution, reducing agent solution, and amine compound solution, a reaction solution was prepared and a crystallized powder was precipitated in the same manner as in Example 1. The concentration of magnetic metals (Fe and Ni) in the reaction solution was 33.0 g / L.
[0195] <Recovery process> From the slurry-like reaction liquid obtained in the crystallization step, an iron-nickel alloy powder (iron-nickel alloy powder) was produced in the same manner as in Example 1. The obtained alloy powder was composed of spherical particles with smooth surfaces. The particle size distribution was sharp, and the average particle size was 0.40 μm.
[0196] [Example 4] In Example 4, an iron-nickel alloy powder (iron-nickel alloy powder) containing 56 mol % of iron (Fe) and 44 mol % of nickel (Ni) was produced according to the procedure shown in Fig. 5. In Example 4, when preparing the reaction solution, a metal salt raw material solution at room temperature was added to and mixed with a reducing solution heated using a water bath.
[0197] <Preparation process> The same raw materials as those in Example 1 were prepared as the nucleating agent, reducing agent, pH adjuster, complexing agent, and amine compound. In addition, ferrous sulfate heptahydrate (FeSO4·7H2O, molecular weight: 278.05, reagent manufactured by Wako Pure Chemical Industries, Ltd.) was prepared as the water-soluble iron salt instead of ferrous chloride tetrahydrate, and nickel sulfate hexahydrate (NiSO4·6H2O, molecular weight: 262.85, reagent manufactured by Wako Pure Chemical Industries, Ltd.) was prepared as the water-soluble nickel salt instead of nickel chloride hexahydrate.
[0198] <Crystallization process> (a) Preparation of metal salt source solution A metal salt raw solution containing ferrous sulfate heptahydrate (water-soluble iron salt), nickel sulfate hexahydrate (water-soluble nickel salt), palladium (II) chloride ammonium (nucleating agent), trisodium citrate dihydrate (complexing agent) and water was prepared. In this case, in the obtained metal salt raw solution, the amount of palladium (Pd) was weighed out to be 0.37 mass ppm (0.2 mol ppm) with respect to the total amount of magnetic metals (Fe and Ni). Also, the amount of trisodium citrate dihydrate with respect to the total amount of magnetic metals (Fe and Ni) was weighed out to be 0.318 (31.8 mol%) in molar ratio. Specifically, 272.0 g of ferrous sulfate heptahydrate, 202.0 g of nickel sulfate hexahydrate, 99.3 μg of palladium (II) chloride ammonium, and 163.5 g of trisodium citrate dihydrate were dissolved in 950 mL of pure water to prepare the metal salt raw solution.
[0199] (b) Preparation of reducing agent solution A reducing agent solution containing sodium hydroxide (pH adjuster), hydrazine (reducing agent) and water was prepared. At this time, the amount of hydrazine was weighed out so that the molar ratio of the amount of magnetic metals (Fe and Ni) to the total amount of magnetic metals (Fe and Ni) in the reaction liquid prepared in the subsequent crystallization step was 6.41. The amount of sodium hydroxide was weighed out so that the molar ratio of the amount of magnetic metals (Fe and Ni) to the total amount of magnetic metals (Fe and Ni) was 4.67. Specifically, 326 g of sodium hydroxide was dissolved in 800 mL of pure water to prepare a sodium hydroxide solution, and 934 g of 60 mass% hydrazine hydrate was added to and mixed with this sodium hydroxide solution to prepare a reducing agent solution.
[0200] (c) Preparation of amine compound solution An amine compound solution was prepared in the same manner as in Example 1.
[0201] (d) Preparation of reaction solution and precipitation of crystallized powder The prepared reducing agent solution was placed in a Teflon (registered trademark) coated stainless steel container (reaction tank) equipped with stirring blades placed in a water bath and heated while stirring until the liquid temperature reached 70°C. After that, the metal salt raw material solution with a liquid temperature of 25°C was added to the reducing agent solution heated in the water bath for a mixing time of 10 seconds to obtain a reaction liquid with a liquid temperature of 59°C. The concentration of magnetic metals (Fe and Ni) in the reaction liquid was 32.6g / L. This initiated the reduction reaction (crystallization reaction) (reaction start temperature 59°C). The temperature of the reaction liquid continued to rise by heating in the water bath after the reaction started, and was kept at a liquid temperature of 70°C after 10 minutes from the start of the reaction (reaction holding temperature 70°C). The color of the reaction liquid was dark green immediately after the start of the reaction (mixing of the reaction liquid), but changed to dark gray after a few minutes. The reason why the color tone turned dark green immediately after the start of the reaction is believed to be because the reaction according to formula (6) above progressed and a coprecipitate of iron hydroxide (Fe(OH)2) and nickel hydroxide (Ni(OH)2) was formed in the reaction solution. Also, the reason why the color tone turned dark gray a few minutes after the start of the reaction is believed to be because nucleation occurred due to the action of the nucleating agent (palladium salt).
[0202] The reduction reaction was allowed to proceed by adding the amine compound solution dropwise to the reaction solution over a period of 10 minutes, from 3 minutes after the start of the reaction, when the color of the reaction solution had changed to dark gray, to 13 minutes after the start of the reaction. This caused iron-nickel crystallized powder to precipitate in the reaction solution. At this point, the reaction solution was black in color, but within 30 minutes after the start of the reaction, the supernatant liquid of the reaction solution became transparent. It is believed that the reduction reaction of the above formula (6) was completed, and all of the iron and nickel components in the reaction solution were reduced to metallic iron and metallic nickel. After the reaction was completed, the reaction solution was a slurry containing iron-nickel crystallized powder.
[0203] <Recovery process> The slurry-like reaction liquid obtained in the crystallization step was subjected to filtration, washing, and solid-liquid separation to recover a cake-like iron-nickel crystallized powder. Filtration and washing were performed using pure water with a conductivity of 1 μS / cm until the conductivity of the filtrate filtered from the slurry was 10 μS / cm or less. The recovered cake-like crystallized powder was dried in a vacuum dryer set at 50°C. The dried crystallized powder was then cooled to 35°C in a vacuum, and nitrogen gas containing 1.0% by volume of oxygen was supplied to the crystallized powder to perform a gradual oxidation treatment. In this way, an iron-nickel alloy powder was obtained. The obtained alloy powder was composed of spherical particles with a smooth surface. The particle size distribution was sharp, and the average particle size was 0.38 μm.
[0204] [Example 5] In Example 5, an iron-nickel alloy powder (iron-nickel alloy powder) containing 51 mol% iron (Fe) and 49 mol% nickel (Ni) with a nickel-rich surface composition was produced according to the procedure shown in Figure 6. At this time, an additional raw material liquid was added and mixed at the end of the crystallization process. Specifically, first, crystallization of an iron-nickel alloy powder (iron-nickel alloy powder) containing 56 mol% iron (Fe) and 44 mol% nickel (Ni) was carried out in the same manner as in Example 4 except that the amount of hydrazine blended as a reducing agent was different, and then, during this crystallization, a water-soluble nickel salt aqueous solution was added to the reaction solution as an additional raw material liquid and mixed.
[0205] <Preparation process> The same raw materials as those in Example 4 were prepared as the water-soluble iron salt, the water-soluble nickel salt, the nucleating agent, the reducing agent, the pH adjuster, the complexing agent, and the amine compound.
[0206] <Crystallization process> (a) Preparation of metal salt source solution A metal salt raw solution containing ferrous sulfate heptahydrate (water-soluble iron salt), nickel sulfate hexahydrate (water-soluble nickel salt), palladium (II) chloride ammonium (nucleating agent), trisodium citrate dihydrate (complexing agent) and water was prepared. In this case, in the obtained metal salt raw solution, palladium (Pd) was weighed out so that the amount of palladium was 0.37 mass ppm (0.2 mol ppm) relative to the total amount of magnetic metals (Fe and Ni). In addition, trisodium citrate dihydrate was weighed out so that the molar ratio of trisodium citrate dihydrate relative to the total amount of magnetic metals (Fe and Ni) was 0.318 (31.8 mol%). Specifically, 272.0 g of ferrous sulfate heptahydrate, 202.0 g of nickel sulfate hexahydrate, 99.3 μg of palladium (II) chloride ammonium, and 163.5 g of trisodium citrate dihydrate were dissolved in 950 mL of pure water to prepare the metal salt raw solution.
[0207] (b) Preparation of reducing agent solution A reducing agent solution containing sodium hydroxide (pH adjuster), hydrazine (reducing agent) and water was prepared. At this time, in the reaction solution prepared in the subsequent crystallization step, the amount of hydrazine relative to the total amount of magnetic metals (Fe and Ni) at the start of the reaction was weighed out so that the molar ratio was 4.85 (the molar ratio was 4.41 relative to the total amount of magnetic metals (Fe and Ni) at the time of adding the additional raw material liquid). Also, the amount of sodium hydroxide relative to the total amount of magnetic metals (Fe and Ni) at the start of the reaction was weighed out so that the molar ratio was 4.67 (the molar ratio was 4.24 relative to the total amount of magnetic metals (Fe and Ni) at the time of adding the additional raw material liquid). Specifically, 326 g of sodium hydroxide was dissolved in 800 mL of pure water to prepare a sodium hydroxide solution, and 707 g of 60 mass% hydrazine hydrate was added and mixed to this sodium hydroxide solution to prepare a reducing agent solution.
[0208] (c) Preparation of amine compound solution An amine compound solution containing ethylenediamine (amine compound) and water was prepared. At this time, the amount of ethylenediamine was weighed out so that the molar ratio of the amount of ethylenediamine to the total amount of magnetic metals (Fe and Ni) after the addition of the additional raw material liquid was a very small amount of 0.01 (1.0 mol%) in the reaction solution in the subsequent crystallization process. Specifically, 1.16 g of ethylenediamine was dissolved in 18 mL of pure water to prepare the amine compound solution.
[0209] (d) Preparation of additional raw material solution An additional raw material solution containing nickel sulfate hexahydrate (a water-soluble nickel salt) and water was prepared. At this time, the amount of magnetic metal (Ni) in the obtained additional raw material solution was 0.175 moles, and was weighed out so that it was 0.10 times the total amount of magnetic metal (Fe and Ni) in the metal salt raw material solution (1.747 moles). Specifically, 46.0 g of nickel sulfate hexahydrate was dissolved in 200 mL of pure water to prepare the additional raw material solution.
[0210] (e) Preparation of reaction solution and precipitation of crystallized powder The prepared reducing agent solution was placed in a Teflon (registered trademark) coated stainless steel container (reaction tank) with stirring blades installed in a water bath and heated while stirring until the liquid temperature reached 70°C. After that, the metal salt raw material solution with a liquid temperature of 25°C was added to the reducing agent solution heated in the water bath for a mixing time of 10 seconds to obtain a reaction liquid with a liquid temperature of 57°C. The concentration of magnetic metals (Fe and Ni) in the reaction liquid was 35.2g / L. This initiated the reduction reaction (crystallization reaction) (reaction start temperature 57°C). The temperature of the reaction liquid continued to rise by heating in the water bath after the reaction started, and was kept at a liquid temperature of 70°C after 10 minutes from the start of the reaction (reaction holding temperature 70°C). The color of the reaction liquid was dark green immediately after the start of the reaction (mixing of the reaction liquid), but changed to dark gray after a few minutes. The reason why the color tone turned dark green immediately after the start of the reaction is believed to be because the reaction according to formula (6) above progressed and a coprecipitate of iron hydroxide (Fe(OH)2) and nickel hydroxide (Ni(OH)2) was formed in the reaction solution. Also, the reason why the color tone turned dark gray a few minutes after the start of the reaction is believed to be because nucleation occurred due to the action of the nucleating agent (palladium salt).
[0211] The amine compound solution was added dropwise to the reaction solution for 10 minutes from 3 minutes to 13 minutes after the start of the reaction, when the color of the reaction solution changed to dark gray, to proceed with the reduction reaction. As a result, iron-nickel crystallized powder precipitated in the reaction solution. From 11 minutes to 16 minutes after the start of the reaction, the additional raw material solution was added dropwise and mixed little by little to promote the reduction of the iron ions (or iron hydroxide), which are difficult to reduce, and the reduction reaction was proceeded so that the surface of the precipitated iron-nickel crystallized powder had a more nickel-rich composition. The concentration of magnetic metals (Fe and Ni) in the reaction solution after the addition of the additional raw material solution was 32.8 g / L. The color of the reaction solution at this time was black, but the supernatant liquid of the reaction solution became transparent within 30 minutes from the start of the reaction. It is considered that the reduction reaction was completed and all of the iron and nickel components in the reaction solution were reduced to metallic iron and metallic nickel. The reaction solution after the completion of the reaction was a slurry containing iron-nickel crystallized powder.
[0212] <Recovery process> The slurry-like reaction liquid obtained in the crystallization step was subjected to filtration, washing, and solid-liquid separation to recover a cake-like iron-nickel crystallized powder. Filtration and washing were performed using pure water with a conductivity of 1 μS / cm until the conductivity of the filtrate filtered from the slurry was 10 μS / cm or less. The recovered cake-like crystallized powder was dried in a vacuum dryer set at 50°C. The dried crystallized powder was then cooled to 35°C in a vacuum, and nitrogen gas containing 1.0% by volume of oxygen was supplied to the crystallized powder to perform a gradual oxidation treatment. In this way, an iron-nickel alloy powder was obtained. The obtained alloy powder was composed of spherical particles with a smooth surface. The particle size distribution was sharp, and the average particle size was 0.40 μm.
[0213] [Example 6] In Example 6, the crystallized powder obtained in Example 1 was subjected to a spiral jet crushing process, which is a dry crushing process, using a micro jet mill (Japan Pneumatic Co., Ltd., JKE-30) at a crushing gas pressure of 0.5 MPa to produce an iron-nickel alloy powder (iron-nickel alloy powder) containing 50 mol% iron (Fe) and 50 mol% nickel (Ni). The obtained alloy powder had a sharp particle size distribution similar to that of Example 1, and an average particle size of 0.41 μm. In addition, the spiral jet crushing process reduced agglomerated particles, improving packing properties (increasing the green compact density), and reduced surface irregularities, resulting in a powder consisting of spherical particles with a very smooth surface.
[0214] [Example 7] In Example 7, as described below, following the crystallization step, the slurry-like crystallized powder before drying was subjected to a high-pressure fluid collision crushing treatment, which is a wet crushing method, during the recovery step to produce an iron-nickel alloy powder (iron-nickel alloy powder) containing 50 mol % of iron (Fe) and 50 mol % of nickel (Ni).
[0215] <Recovery process (including crushing process)> The slurry-like reaction liquid containing the iron-nickel crystallized powder obtained in the same crystallization step as in Example 1 was filtered and washed, and then a washed crystallized powder slurry with a concentration of 20 mass% of the iron-nickel crystallized powder was prepared using pure water with a conductivity of 1 μS / cm. The above filtration and washing was performed using pure water with a conductivity of 1 μS / cm until the conductivity of the filtrate filtered from the slurry became 10 μS / cm or less. The above washed crystallized powder slurry was subjected to a crushing treatment by passing it through a high-pressure fluid collision crushing device (manufactured by Sugino Machine; pressure: 200 MPa) twice, and then subjected to a solid-liquid separation treatment to recover a cake-like iron-nickel crystallized powder. The recovered cake-like crystallized powder was dried in a vacuum dryer set at 50°C. Then, the dried crystallized powder was cooled to 35°C in a vacuum, and then nitrogen gas containing 1.0 volume% of oxygen was supplied to the crystallized powder to perform a gradual oxidation treatment to obtain an iron-nickel alloy powder. The obtained alloy powder had a sharp particle size distribution and an average particle size of 0.41 μm, similar to that of Example 1. Furthermore, the high-pressure fluid collision disintegration treatment reduced agglomerated particles, improving packing properties (increasing the green compact density), and reduced surface irregularities, resulting in the powder being composed of spherical particles with an extremely smooth surface.
[0216] [Example 8] In Example 8, an iron-nickel alloy powder (iron-nickel alloy powder) containing 65 mol% of iron (Fe) and 35 mol% of nickel (Ni) was produced by subjecting the crystallized powder obtained according to the procedure shown in Fig. 6 to a high-temperature heat treatment. In Example 8, when preparing the reaction solution, the metal salt raw material solution at room temperature was added to and mixed with the reducing solution heated using a water bath.
[0217] <Preparation process> The same raw materials as those in Example 4 were prepared as the water-soluble iron salt, the water-soluble nickel salt, the nucleating agent, the reducing agent, the pH adjuster, the complexing agent, and the amine compound.
[0218] <Crystallization process> (a) Preparation of metal salt source solution A metal salt raw solution containing ferrous sulfate heptahydrate (water-soluble iron salt), nickel sulfate hexahydrate (water-soluble nickel salt), palladium (II) chloride ammonium (nucleating agent), trisodium citrate dihydrate (complexing agent) and water was prepared. In this case, in the obtained metal salt raw solution, palladium (Pd) was weighed out so that the amount of palladium (Pd) was 2.81 mass ppm (1.50 mol ppm) relative to the total amount of magnetic metals (Fe and Ni). In addition, trisodium citrate dihydrate was weighed out so that the molar ratio relative to the total amount of magnetic metals (Fe and Ni) was 0.724 (72.4 mol%). Specifically, 318.1 g of ferrous sulfate heptahydrate, 161.9 g of nickel sulfate hexahydrate, 750.5 μg of palladium (II) chloride ammonium, and 374.7 g of trisodium citrate dihydrate were dissolved in 950 mL of pure water to prepare the metal salt raw solution.
[0219] (b) Preparation of reducing agent solution A reducing agent solution containing sodium hydroxide (pH adjuster), hydrazine (reducing agent) and water was prepared. At this time, in the reaction liquid prepared in the subsequent crystallization step, the amount of hydrazine was weighed out so that the molar ratio relative to the total amount of magnetic metals (Fe and Ni) at the start of the reaction was 8.98. Also, the amount of sodium hydroxide was weighed out so that the molar ratio relative to the total amount of magnetic metals (Fe and Ni) at the start of the reaction was 7.07. Specifically, 497.5 g of sodium hydroxide was dissolved in 1218 mL of pure water to prepare a sodium hydroxide solution, and 1318 g of 60 mass% hydrazine hydrate was added to and mixed with this sodium hydroxide solution to prepare a reducing agent solution.
[0220] (c) Preparation of amine compound solution An amine compound solution containing ethylenediamine (amine compound) and water was prepared. At this time, the amount of ethylenediamine was weighed out so that the molar ratio of the amount of ethylenediamine to the total amount of magnetic metals (Fe and Ni) after the addition of the additional raw material liquid was a very small amount of 0.01 (1.0 mol%) in the reaction solution in the subsequent crystallization process. Specifically, 1.06 g of ethylenediamine was dissolved in 18 mL of pure water to prepare the amine compound solution.
[0221] (d) Preparation of reaction solution and precipitation of crystallized powder The prepared reducing agent solution was placed in a Teflon (registered trademark) coated stainless steel container (reaction tank) equipped with stirring blades placed in a water bath and heated while stirring until the liquid temperature reached 80°C. After that, the metal salt raw material solution with a liquid temperature of 25°C was added to the reducing agent solution heated in the water bath for a mixing time of 10 seconds to obtain a reaction liquid with a liquid temperature of 71°C. The concentration of magnetic metals (Fe and Ni) in the reaction liquid was 25.0 g / L. This initiated the reduction reaction (crystallization reaction) (reaction start temperature 71°C). The temperature of the reaction liquid continued to rise by heating in the water bath after the start of the reaction, and was kept at a liquid temperature of 80°C after 10 minutes from the start of the reaction (reaction holding temperature 80°C). The color of the reaction liquid was dark green immediately after the start of the reaction (mixing of the reaction liquid), but changed to dark gray after a few minutes. The reason why the color tone turned dark green immediately after the start of the reaction is believed to be because the reaction according to formula (6) above progressed and a coprecipitate of iron hydroxide (Fe(OH)2) and nickel hydroxide (Ni(OH)2) was formed in the reaction solution. Also, the reason why the color tone turned dark gray a few minutes after the start of the reaction is believed to be because nucleation occurred due to the action of the nucleating agent (palladium salt).
[0222] The reduction reaction was allowed to proceed by adding the amine compound solution dropwise to the reaction solution over a period of 10 minutes, from 3 minutes after the start of the reaction, when the color of the reaction solution had changed to dark gray, to 13 minutes after the start of the reaction. This caused iron-nickel crystallized powder to precipitate in the reaction solution. At this point, the reaction solution was black in color, but within 40 minutes after the start of the reaction, the supernatant liquid of the reaction solution became transparent. It is believed that the reduction reaction was complete, and all of the iron and nickel components in the reaction solution were reduced to metallic iron and metallic nickel. After the reaction was complete, the reaction solution was a slurry containing iron-nickel crystallized powder.
[0223] <Recovery process> The slurry-like reaction liquid obtained in the crystallization step was subjected to filtration, washing, and solid-liquid separation to recover a cake-like iron-nickel crystallized powder. Filtration and washing were performed using pure water with a conductivity of 1 μS / cm until the conductivity of the filtrate filtered from the slurry was 10 μS / cm or less. The recovered cake-like crystallized powder was dried in a vacuum dryer set at 50°C. The dried crystallized powder was then cooled to 35°C in a vacuum, and nitrogen gas containing 1.0% by volume of oxygen was supplied to the crystallized powder to perform a gradual oxidation treatment.
[0224] <High-temperature heat treatment process> The crystallized powder thus obtained was subjected to a high-temperature heat treatment in which it was heated at 350°C for 60 minutes in a nitrogen atmosphere to produce an iron-nickel alloy powder (iron-nickel alloy powder) containing 65 mol% iron (Fe) and 35 mol% nickel (Ni). The obtained alloy powder had a sharp particle size distribution similar to that of Example 1, and an average particle size of 0.27 μm. Furthermore, the high-temperature heat treatment promoted the diffusion of Fe and Ni within the iron (Fe)-nickel (Ni) alloy particles, improving the composition uniformity within the particles and reducing the characteristic variation within the particles.
[0225] [Example 9] In Example 9, an iron-nickel alloy powder (iron-nickel alloy powder) containing 65 mol% iron (Fe) and 35 mol% nickel (Ni) with a nickel-rich surface composition was produced according to the procedure shown in FIG. 6. In this case, an additional raw material liquid was added and mixed during the crystallization process. Specifically, a metal salt raw material solution at room temperature was added and mixed to a reducing solution heated using a water bath to prepare a reaction solution, and crystallization of an iron-nickel alloy powder (iron-nickel alloy powder) containing 67.4 mol% iron (Fe) and 32.6 mol% nickel (Ni) was first promoted. Then, during this crystallization, a water-soluble nickel salt aqueous solution was added and mixed as an additional raw material liquid to the reaction solution.
[0226] <Preparation process> The same raw materials as those in Example 4 were prepared as the water-soluble iron salt, the water-soluble nickel salt, the nucleating agent, the reducing agent, the pH adjuster, the complexing agent, and the amine compound.
[0227] <Crystallization process> (a) Preparation of metal salt source solution A metal salt raw solution containing ferrous sulfate heptahydrate (water-soluble iron salt), nickel sulfate hexahydrate (water-soluble nickel salt), palladium (II) chloride ammonium (nucleating agent), trisodium citrate dihydrate (complexing agent) and water was prepared. In this case, in the obtained metal salt raw solution, palladium (Pd) was weighed out so that the amount of palladium (Pd) was 0.97 mass ppm (0.52 mol ppm) relative to the total amount of magnetic metals (Fe and Ni). In addition, trisodium citrate dihydrate was weighed out so that the molar ratio relative to the total amount of magnetic metals (Fe and Ni) was 0.750 (75.0 mol%). Specifically, 318.1 g of ferrous sulfate heptahydrate, 145.7 g of nickel sulfate hexahydrate, 250.0 μg of palladium (II) chloride ammonium, and 374.7 g of trisodium citrate dihydrate were dissolved in 500 mL of pure water to prepare the metal salt raw solution.
[0228] (b) Preparation of reducing agent solution A reducing agent solution containing sodium hydroxide (pH adjuster), hydrazine (reducing agent) and water was prepared. At this time, in the reaction solution prepared in the subsequent crystallization step, the amount of hydrazine relative to the total amount of magnetic metals (Fe and Ni) at the start of the reaction was weighed out so that the molar ratio was 7.62 (the molar ratio was 7.36 relative to the total amount of magnetic metals (Fe and Ni) at the time of adding the additional raw material liquid). Also, the amount of sodium hydroxide relative to the total amount of magnetic metals (Fe and Ni) at the start of the reaction was weighed out so that the molar ratio was 7.33 (the molar ratio was 7.07 relative to the total amount of magnetic metals (Fe and Ni) at the time of adding the additional raw material liquid). Specifically, 497.5 g of sodium hydroxide was dissolved in 1218 mL of pure water to prepare a sodium hydroxide solution, and 1080 g of 60 mass% hydrazine hydrate was added to and mixed with this sodium hydroxide solution to prepare a reducing agent solution.
[0229] (c) Preparation of amine compound solution An amine compound solution containing ethylenediamine (amine compound) and water was prepared. At this time, the amount of ethylenediamine was weighed out so that the molar ratio of the amount of ethylenediamine to the total amount of magnetic metals (Fe and Ni) after the addition of the additional raw material liquid was a very small amount of 0.01 (1.0 mol%) in the reaction solution in the subsequent crystallization process. Specifically, 1.06 g of ethylenediamine was dissolved in 18 mL of pure water to prepare the amine compound solution.
[0230] (d) Preparation of additional raw material solution An additional raw material solution containing nickel sulfate hexahydrate (a water-soluble nickel salt) and water was prepared. At this time, the amount of magnetic metal (Ni) in the obtained additional raw material solution was 0.0616 moles, and was weighed out so that it was 0.035 times the total amount of magnetic metal (Fe and Ni) in the metal salt raw material solution (1.760 moles). Specifically, 16.2 g of nickel sulfate hexahydrate was dissolved in 200 mL of pure water to prepare the additional raw material solution.
[0231] (e) Preparation of reaction solution and precipitation of crystallized powder The prepared reducing agent solution was placed in a Teflon (registered trademark) coated stainless steel container (reaction tank) equipped with stirring blades placed in a water bath and heated while stirring until the liquid temperature reached 80°C. After that, the metal salt raw material solution with a liquid temperature of 25°C was added to the reducing agent solution heated in the water bath for a mixing time of 10 seconds to obtain a reaction liquid with a liquid temperature of 75°C. The concentration of magnetic metals (Fe and Ni) in the reaction liquid was 29.1g / L. This initiated the reduction reaction (crystallization reaction) (reaction start temperature 75°C). The temperature of the reaction liquid continued to rise by heating in the water bath after the start of the reaction, and was kept at a liquid temperature of 80°C after 10 minutes from the start of the reaction (reaction holding temperature 80°C). The color of the reaction liquid was dark green immediately after the start of the reaction (mixing of the reaction liquid), but changed to dark gray after a few minutes. The reason why the color tone turned dark green immediately after the start of the reaction is believed to be because the reaction according to formula (6) above progressed and a coprecipitate of iron hydroxide (Fe(OH)2) and nickel hydroxide (Ni(OH)2) was formed in the reaction solution. Also, the reason why the color tone turned dark gray a few minutes after the start of the reaction is believed to be because nucleation occurred due to the action of the nucleating agent (palladium salt).
[0232] The amine compound solution was added dropwise to the reaction solution for 10 minutes from 3 minutes to 13 minutes after the start of the reaction, when the color of the reaction solution changed to dark gray, to proceed with the reduction reaction. As a result, iron-nickel crystallized powder precipitated in the reaction solution. From 25 minutes to 35 minutes after the start of the reaction, the additional raw material solution was added dropwise and mixed little by little to promote the reduction of the iron ions (or iron hydroxide), which are difficult to reduce, and the reduction reaction was proceeded so that the surface of the precipitated iron-nickel crystallized powder had a more nickel-rich composition. The concentration of magnetic metals (Fe and Ni) in the reaction solution after the addition of the additional raw material solution was 28.4 g / L. The color of the reaction solution at this time was black, but the supernatant liquid of the reaction solution became transparent within 40 minutes from the start of the reaction. It is considered that the reduction reaction was completed and all of the iron and nickel components in the reaction solution were reduced to metallic iron and metallic nickel. The reaction solution after the completion of the reaction was a slurry containing iron-nickel crystallized powder.
[0233] <Recovery process> The slurry-like reaction liquid obtained in the crystallization step was subjected to filtration, washing, and solid-liquid separation to recover a cake-like iron-nickel crystallized powder. Filtration and washing were performed using pure water with a conductivity of 1 μS / cm until the conductivity of the filtrate filtered from the slurry was 10 μS / cm or less. The recovered cake-like crystallized powder was dried in a vacuum dryer set at 50°C. The dried crystallized powder was then cooled to 35°C in a vacuum, and nitrogen gas containing 1.0% by volume of oxygen was supplied to the crystallized powder to perform a gradual oxidation treatment. In this way, an iron-nickel alloy powder was obtained. The obtained alloy powder was composed of spherical particles with a smooth surface. The particle size distribution was sharp, and the average particle size was 0.39 μm.
[0234] [Example 10] In Example 10, an iron-nickel alloy powder (iron-nickel alloy powder) containing 80 mol% iron (Fe) and 20 mol% nickel (Ni) with a composition having a large iron content was produced according to the procedure shown in FIG. 6. In this case, an additional raw material liquid was added and mixed during the crystallization process. Specifically, a metal salt raw material solution at room temperature was added and mixed to a reducing solution heated using a water bath to prepare a reaction solution, and crystallization of an iron-nickel alloy powder (iron-nickel alloy powder) containing 83.3 mol% iron (Fe) and 16.7 mol% nickel (Ni) was first promoted. Then, during this crystallization, a water-soluble nickel salt aqueous solution was added and mixed as an additional raw material liquid to the reaction solution.
[0235] <Preparation process> The same raw materials as those in Example 4 were prepared as the water-soluble iron salt, the water-soluble nickel salt, the nucleating agent, the reducing agent, the pH adjuster, the complexing agent, and the amine compound.
[0236] <Crystallization process> (a) Preparation of metal salt source solution A metal salt raw solution containing ferrous sulfate heptahydrate (water-soluble iron salt), nickel sulfate hexahydrate (water-soluble nickel salt), palladium (II) chloride ammonium (nucleating agent), trisodium citrate dihydrate (complexing agent) and water was prepared. In this case, in the obtained metal salt raw solution, the amount of palladium (Pd) was weighed out to be 0.79 mass ppm (0.42 mol ppm) with respect to the total amount of magnetic metals (Fe and Ni). In addition, the amount of trisodium citrate dihydrate with respect to the total amount of magnetic metals (Fe and Ni) was weighed out to be 0.754 (75.4 mol%) in molar ratio. Specifically, 394.3 g of ferrous sulfate heptahydrate, 74.6 g of nickel sulfate hexahydrate, 201.6 μg of palladium (II) chloride ammonium, and 377.5 g of trisodium citrate dihydrate were dissolved in 836 mL of pure water to prepare the metal salt raw solution.
[0237] (b) Preparation of reducing agent solution A reducing agent solution containing sodium hydroxide (pH adjuster), hydrazine (reducing agent) and water was prepared. At this time, in the reaction solution prepared in the subsequent crystallization step, the amount of hydrazine relative to the total amount of magnetic metals (Fe and Ni) at the start of the reaction was weighed out so that the molar ratio was 9.40 (the molar ratio was 9.02 relative to the total amount of magnetic metals (Fe and Ni) at the time of adding the additional raw material liquid). Also, the amount of sodium hydroxide relative to the total amount of magnetic metals (Fe and Ni) at the start of the reaction was weighed out so that the molar ratio was 7.37 (the molar ratio was 7.07 relative to the total amount of magnetic metals (Fe and Ni) at the time of adding the additional raw material liquid). Specifically, 501.3 g of sodium hydroxide was dissolved in 1228 mL of pure water to prepare a sodium hydroxide solution, and 1334 g of 60 mass% hydrazine hydrate was added to and mixed with this sodium hydroxide solution to prepare a reducing agent solution.
[0238] (c) Preparation of amine compound solution An amine compound solution containing ethylenediamine (amine compound) and water was prepared. At this time, the amount of ethylenediamine was weighed out so that the molar ratio of the amount of ethylenediamine to the total amount of magnetic metals (Fe and Ni) after the addition of the additional raw material liquid was a very small amount of 0.01 (1.0 mol%) in the reaction solution in the subsequent crystallization process. Specifically, 1.07 g of ethylenediamine was dissolved in 18 mL of pure water to prepare the amine compound solution.
[0239] (d) Preparation of additional raw material solution An additional raw material solution containing nickel sulfate hexahydrate (a water-soluble nickel salt) and water was prepared. At this time, the amount of magnetic metal (Ni) in the obtained additional raw material solution was 0.0709 mol, and was weighed out so that it was 0.04 times the total amount of magnetic metal (Fe and Ni) in the metal salt raw material solution (1.773 mol). Specifically, 18.64 g of nickel sulfate hexahydrate was dissolved in 200 mL of pure water to prepare the additional raw material solution.
[0240] (e) Preparation of reaction solution and precipitation of crystallized powder The prepared reducing agent solution was placed in a Teflon (registered trademark) coated stainless steel container (reaction tank) equipped with stirring blades placed in a water bath and heated while stirring until the liquid temperature reached 80°C. After that, the metal salt raw material solution with a liquid temperature of 25°C was added to the reducing agent solution heated in the water bath for a mixing time of 10 seconds to obtain a reaction liquid with a liquid temperature of 71°C. The concentration of magnetic metals (Fe and Ni) in the reaction liquid was 24.5g / L. This initiated the reduction reaction (crystallization reaction) (reaction start temperature 71°C). The temperature of the reaction liquid continued to rise by heating in the water bath after the start of the reaction, and was kept at a liquid temperature of 80°C after 10 minutes from the start of the reaction (reaction holding temperature 80°C). The color of the reaction liquid was dark green immediately after the start of the reaction (mixing of the reaction liquid), but changed to dark gray after a few minutes. The reason why the color tone turned dark green immediately after the start of the reaction is believed to be because the reaction according to formula (6) above progressed and a coprecipitate of iron hydroxide (Fe(OH)2) and nickel hydroxide (Ni(OH)2) was formed in the reaction solution. Also, the reason why the color tone turned dark gray a few minutes after the start of the reaction is believed to be because nucleation occurred due to the action of the nucleating agent (palladium salt).
[0241] The amine compound solution was added dropwise to the reaction solution for 10 minutes from 3 minutes to 13 minutes after the start of the reaction, when the color of the reaction solution changed to dark gray, to proceed with the reduction reaction. As a result, iron-nickel crystallized powder precipitated in the reaction solution. From 8 minutes to 18 minutes after the start of the reaction, the additional raw material solution was added dropwise and mixed little by little to promote the reduction of the iron ions (or iron hydroxide), which are difficult to reduce, and the reduction reaction was proceeded so that the surface of the precipitated iron-nickel crystallized powder had a more nickel-rich composition. The concentration of magnetic metals (Fe and Ni) in the reaction solution after the addition of the additional raw material solution was 24.2 g / L. The color of the reaction solution at this time was black, but the supernatant liquid of the reaction solution became transparent within 60 minutes from the start of the reaction. It is considered that the reduction reaction was completed and all of the iron and nickel components in the reaction solution were reduced to metallic iron and metallic nickel. The reaction solution after the reaction was completed was a slurry containing iron-nickel crystallized powder.
[0242] <Recovery process> The slurry-like reaction liquid obtained in the crystallization step was subjected to filtration, washing, and solid-liquid separation to recover a cake-like iron-nickel crystallized powder. Filtration and washing were performed using pure water with a conductivity of 1 μS / cm until the conductivity of the filtrate filtered from the slurry was 10 μS / cm or less. The recovered cake-like crystallized powder was dried in a vacuum dryer set at 50°C. The dried crystallized powder was then cooled to 35°C in a vacuum, and nitrogen gas containing 1.0% by volume of oxygen was supplied to the crystallized powder to perform a gradual oxidation treatment. In this way, an iron-nickel alloy powder was obtained. The obtained alloy powder was composed of spherical particles with a smooth surface. The particle size distribution was sharp, and the average particle size was 0.48 μm.
[0243] [Example 11] In Example 11, an iron-nickel alloy powder (iron-nickel alloy powder) containing 90 mol% iron (Fe) and 10 mol% nickel (Ni) with a composition having a large iron content was produced according to the procedure shown in FIG. 6. In this case, an additional raw material liquid was added and mixed during the crystallization process. Specifically, a metal salt raw material solution at room temperature was added and mixed to a reducing solution heated using a water bath to prepare a reaction solution, and crystallization of an iron-nickel alloy powder (iron-nickel alloy powder) containing 91.8 mol% iron (Fe) and 8.2 mol% nickel (Ni) was first promoted. Then, during this crystallization, a water-soluble nickel salt aqueous solution was added and mixed as an additional raw material liquid to the reaction solution.
[0244] <Preparation process> The same raw materials as those in Example 4 were prepared as the water-soluble iron salt, the water-soluble nickel salt, the nucleating agent, the reducing agent, the pH adjuster, the complexing agent, and the amine compound.
[0245] <Crystallization process> (a) Preparation of metal salt source solution A metal salt raw solution containing ferrous sulfate heptahydrate (water-soluble iron salt), nickel sulfate hexahydrate (water-soluble nickel salt), palladium (II) chloride ammonium (nucleating agent), trisodium citrate dihydrate (complexing agent) and water was prepared. In this case, in the obtained metal salt raw solution, the amount of palladium (Pd) was weighed out so that it was 0.77 mass ppm (0.41 mol ppm) relative to the total amount of magnetic metals (Fe and Ni). In addition, the amount of trisodium citrate dihydrate was weighed out so that it was 0.369 (36.9 mol%) in molar ratio relative to the total amount of magnetic metals (Fe and Ni). Specifically, 446.0 g of ferrous sulfate heptahydrate, 37.5 g of nickel sulfate hexahydrate, 202.6 μg of palladium (II) chloride ammonium, and 189.7 g of trisodium citrate dihydrate were dissolved in 720 mL of pure water to prepare the metal salt raw solution.
[0246] (b) Preparation of reducing agent solution A reducing agent solution containing sodium hydroxide (pH adjuster), hydrazine (reducing agent) and water was prepared. At this time, in the reaction solution prepared in the subsequent crystallization process, the amount of hydrazine relative to the total amount of magnetic metals (Fe and Ni) at the start of the reaction was weighed out so that the molar ratio was 9.15 (the molar ratio was 8.97 relative to the total amount of magnetic metals (Fe and Ni) at the time of adding the additional raw material liquid). Also, the amount of sodium hydroxide relative to the total amount of magnetic metals (Fe and Ni) at the start of the reaction was weighed out so that the molar ratio was 8.29 (the molar ratio was 8.13 relative to the total amount of magnetic metals (Fe and Ni) at the time of adding the additional raw material liquid). Specifically, 579 g of sodium hydroxide was dissolved in 1418 mL of pure water to prepare a sodium hydroxide solution, and 1334 g of 60 mass% hydrazine hydrate was added to and mixed with this sodium hydroxide solution to prepare a reducing agent solution.
[0247] (c) Preparation of amine compound solution An amine compound solution containing ethylenediamine (amine compound) and water was prepared. At this time, the amount of ethylenediamine was weighed out so that the molar ratio of the amount of ethylenediamine to the total amount of magnetic metals (Fe and Ni) after the addition of the additional raw material liquid was a very small amount of 0.01 (1.0 mol%) in the reaction solution in the subsequent crystallization process. Specifically, 1.07 g of ethylenediamine was dissolved in 18 mL of pure water to prepare the amine compound solution.
[0248] (d) Preparation of additional raw material solution An additional raw material solution containing nickel sulfate hexahydrate (a water-soluble nickel salt) and water was prepared. At this time, the amount of magnetic metal (Ni) in the obtained additional raw material solution was 0.0356 moles, and was weighed out so that it was 0.02 times the total amount of magnetic metal (Fe and Ni) in the metal salt raw material solution, which was 1.747 moles. Specifically, 9.37 g of nickel sulfate hexahydrate was dissolved in 100 mL of pure water to prepare the additional raw material solution.
[0249] (e) Preparation of reaction solution and precipitation of crystallized powder The prepared reducing agent solution was placed in a Teflon (registered trademark) coated stainless steel container (reaction tank) equipped with stirring blades placed in a water bath and heated while stirring until the liquid temperature reached 85°C. The metal salt raw material solution with a liquid temperature of 25°C was then added and mixed with the reducing agent solution heated in the water bath for a mixing time of 10 seconds to obtain a reaction liquid with a liquid temperature of 78°C. The concentration of magnetic metals (Fe and Ni) in the reaction liquid was 25.0 g / L. This initiated the reduction reaction (crystallization reaction) (reaction start temperature 78°C). The temperature of the reaction liquid continued to rise by heating in the water bath after the start of the reaction, and was kept at a liquid temperature of 85°C after 10 minutes from the start of the reaction (reaction holding temperature 85°C). The color of the reaction liquid was dark green immediately after the start of the reaction (mixing of the reaction liquid), but changed to dark gray after a few minutes. The reason why the color tone turned dark green immediately after the start of the reaction is believed to be because the reaction according to formula (6) above progressed and a coprecipitate of iron hydroxide (Fe(OH)2) and nickel hydroxide (Ni(OH)2) was formed in the reaction solution. Also, the reason why the color tone turned dark gray a few minutes after the start of the reaction is believed to be because nucleation occurred due to the action of the nucleating agent (palladium salt).
[0250] The amine compound solution was added dropwise to the reaction solution for 10 minutes from 3 minutes to 13 minutes after the start of the reaction, when the color of the reaction solution changed to dark gray, to proceed with the reduction reaction. As a result, iron-nickel crystallized powder precipitated in the reaction solution. From 8 minutes to 18 minutes after the start of the reaction, the additional raw material solution was added dropwise and mixed little by little to promote the reduction of the iron ions (or iron hydroxide), which are difficult to reduce, and the reduction reaction was proceeded so that the surface of the precipitated iron-nickel crystallized powder had a more nickel-rich composition. The concentration of magnetic metals (Fe and Ni) in the reaction solution after the addition of the additional raw material solution was 24.8 g / L. The color of the reaction solution at this time was black, but the supernatant liquid of the reaction solution became transparent within 50 minutes from the start of the reaction. It is considered that the reduction reaction was completed and all of the iron and nickel components in the reaction solution were reduced to metallic iron and metallic nickel. The reaction solution after the reaction was completed was a slurry containing iron-nickel crystallized powder.
[0251] <Recovery process> The slurry-like reaction liquid obtained in the crystallization step was subjected to filtration, washing, and solid-liquid separation to recover a cake-like iron-nickel crystallized powder. Filtration and washing were performed using pure water with a conductivity of 1 μS / cm until the conductivity of the filtrate filtered from the slurry was 10 μS / cm or less. The recovered cake-like crystallized powder was dried in a vacuum dryer set at 50°C. The dried crystallized powder was then cooled to 35°C in a vacuum, and nitrogen gas containing 1.0% by volume of oxygen was supplied to the crystallized powder to perform a gradual oxidation treatment. In this way, an iron-nickel alloy powder was obtained. The obtained alloy powder was composed of spherical particles with a smooth surface. The particle size distribution was sharp, and the average particle size was 0.38 μm.
[0252] [Example 12] In Example 12, an iron-nickel alloy powder (iron-nickel alloy powder) containing 55 mol % of iron (Fe) and 45 mol % of nickel (Ni) and coated with silicon dioxide (SiO2), an insulating metal oxide, was produced by applying an insulating coating treatment to the crystallized powder obtained according to the procedure shown in Figure 5. In Example 12, when preparing the reaction solution, the metal salt raw material solution at room temperature was added to and mixed with the reducing solution heated using a water bath.
[0253] <Preparation process> The same raw materials as those in Example 4 were prepared as the water-soluble iron salt, the water-soluble nickel salt, the nucleating agent, the reducing agent, the pH adjuster, the complexing agent, and the amine compound.
[0254] <Crystallization process> (a) Preparation of metal salt source solution A metal salt raw solution containing ferrous sulfate heptahydrate (water-soluble iron salt), nickel sulfate hexahydrate (water-soluble nickel salt), palladium (II) chloride ammonium (nucleating agent), trisodium citrate dihydrate (complexing agent) and water was prepared. In this case, in the obtained metal salt raw solution, the amount of palladium (Pd) was weighed out to be 0.56 mass ppm (0.3 mol ppm) with respect to the total amount of magnetic metals (Fe and Ni). Also, the amount of trisodium citrate dihydrate with respect to the total amount of magnetic metals (Fe and Ni) was weighed out to be 0.543 (54.3 mol%) in molar ratio. Specifically, 267.7 g of ferrous sulfate heptahydrate, 207.1 g of nickel sulfate hexahydrate, 149.3 μg of palladium (II) chloride ammonium, and 279.6 g of trisodium citrate dihydrate were dissolved in 950 mL of pure water to prepare the metal salt raw solution.
[0255] (b) Preparation of reducing agent solution A reducing agent solution containing sodium hydroxide (pH adjuster), hydrazine (reducing agent) and water was prepared. At this time, in the reaction liquid prepared in the subsequent crystallization step, the amount of hydrazine relative to the total amount of magnetic metals (Fe and Ni) was weighed out so that the molar ratio was 4.85. Also, the amount of sodium hydroxide relative to the total amount of magnetic metals (Fe and Ni) was weighed out so that the molar ratio was 4.95. Specifically, 346 g of sodium hydroxide was dissolved in 848 mL of pure water to prepare a sodium hydroxide solution, and 709 g of 60 mass% hydrazine hydrate was added to and mixed with this sodium hydroxide solution to prepare a reducing agent solution.
[0256] (c) Preparation of amine compound solution An amine compound solution containing ethylenediamine (amine compound) and water was prepared. At this time, the amount of ethylenediamine was weighed out so that the molar ratio of the amount of ethylenediamine to the total amount of magnetic metals (Fe and Ni) after the addition of the additional raw material liquid was a very small amount of 0.01 (1.0 mol%) in the reaction solution in the subsequent crystallization process. Specifically, 1.05 g of ethylenediamine was dissolved in 18 mL of pure water to prepare the amine compound solution.
[0257] (d) Preparation of reaction solution and precipitation of crystallized powder The prepared reducing agent solution was placed in a Teflon (registered trademark) coated stainless steel container (reaction tank) equipped with stirring blades placed in a water bath and heated while stirring until the liquid temperature reached 70°C. After that, the metal salt raw material solution with a liquid temperature of 25°C was added to the reducing agent solution heated in the water bath for a mixing time of 10 seconds to obtain a reaction liquid with a liquid temperature of 59°C. The concentration of magnetic metals (Fe and Ni) in the reaction liquid was 33.9g / L. This initiated the reduction reaction (crystallization reaction) (reaction start temperature 59°C). The temperature of the reaction liquid continued to rise by heating in the water bath after the reaction started, and was kept at a liquid temperature of 70°C after 10 minutes from the start of the reaction (reaction holding temperature 70°C). The color of the reaction liquid was dark green immediately after the start of the reaction (mixing of the reaction liquid), but changed to dark gray after a few minutes. The reason why the color tone turned dark green immediately after the start of the reaction is believed to be because the reaction according to formula (6) above progressed and a coprecipitate of iron hydroxide (Fe(OH)2) and nickel hydroxide (Ni(OH)2) was formed in the reaction solution. Also, the reason why the color tone turned dark gray a few minutes after the start of the reaction is believed to be because nucleation occurred due to the action of the nucleating agent (palladium salt).
[0258] The reduction reaction was allowed to proceed by adding the amine compound solution dropwise to the reaction solution over a period of 10 minutes, from 3 minutes after the start of the reaction, when the color of the reaction solution had changed to dark gray, to 13 minutes after the start of the reaction. This caused iron-nickel crystallized powder to precipitate in the reaction solution. At this point, the reaction solution was black in color, but within 30 minutes after the start of the reaction, the supernatant liquid of the reaction solution became transparent. It is believed that the reduction reaction of the above formula (6) was completed, and all of the iron and nickel components in the reaction solution were reduced to metallic iron and metallic nickel. After the reaction was completed, the reaction solution was a slurry containing iron-nickel crystallized powder.
[0259] <Recovery process> The slurry-like reaction liquid obtained in the crystallization step was subjected to filtration, washing, and solid-liquid separation to recover a cake-like iron-nickel crystallized powder. Filtration and washing were performed using pure water with a conductivity of 1 μS / cm until the conductivity of the filtrate filtered from the slurry was 10 μS / cm or less. The recovered cake-like crystallized powder was dried in a vacuum dryer set at 50°C. The dried crystallized powder was then cooled to 35°C in a vacuum, and nitrogen gas containing 1.0% by volume of oxygen was supplied to the crystallized powder to perform a gradual oxidation treatment. In this way, a crystallized powder (iron-nickel alloy powder) was obtained as a dry powder. The obtained crystallized powder (alloy powder) was composed of spherical particles with a smooth surface. The particle size distribution was sharp, and the average particle size was 0.39 μm.
[0260] <Insulation coating process> 50.0 g of the crystallized powder (alloy powder) obtained in the above recovery process was placed in a polypropylene sealed container, and 7.0 g of pure water and 50.0 g of ethyl alcohol (C2H5OH, molecular weight: 46.07, reagent manufactured by Wako Pure Chemical Industries, Ltd.) were added to disperse the crystallized powder (alloy powder) in a mixed solvent of water and ethyl alcohol. Then, 9.8 g of tetraethoxysilane (also known as tetraethyl orthosilicate, tetraethyl silicate) (abbreviation: TEOS) (Si(OC2H5)4, molecular weight: 208.33, reagent manufactured by Wako Pure Chemical Industries, Ltd.) was added as a silicon alkoxide and mixed thoroughly, and 2.4 g of 1 mass% ammonia water was added as a base catalyst (alkali catalyst) for hydrolysis of the silicon alkoxide while stirring to obtain a uniform slurry. The 1% by mass ammonia water was prepared by diluting 28-30% by mass ammonia water (NH3, molecular weight: 17.03, reagent manufactured by Wako Pure Chemical Industries, Ltd.) with pure water. The crystallized powder (alloy powder), water, ethyl alcohol, tetraethoxysilane, and 1% by mass ammonia water were all used at room temperature, and addition and mixing were also all performed at room temperature.
[0261] The above slurry containing the crystallized powder (alloy powder), water, ethyl alcohol, tetraethoxysilane, and ammonia was kept at 40°C for 2 days in a rotating polypropylene sealed container, and hydrolysis and dehydration condensation polymerization of tetraethoxysilane were carried out while stirring the slurry, forming an insulating coating layer mainly composed of a hydrolysis polymer of tetraethoxysilane (composition of silicon dioxide (SiO2) containing a small amount of silanol groups (Si-OH)) on the particle surface of the crystallized powder (alloy powder). After this, the slurry was subjected to filtration washing and solid-liquid separation treatment to recover a cake-like crystallized powder (alloy powder). The filtration washing was performed first using ethanol containing 50 mass% pure water, and then using ethanol. Note that the hydrolysis polymer of tetraethoxysilane remaining in the slurry without being consumed in the insulating coating on the particle surface of the crystallized powder (alloy powder) is a particle (silica sol) with a very small molecular weight, and is removed as a filtrate during filtration washing, so it does not remain in the recovered cake-like crystallized powder (alloy powder).
[0262] The collected cake-like crystallized powder (alloy powder) was dried in a vacuum dryer at 50°C, and then heated in a vacuum at 150°C for 2 hours. This heat treatment caused the hydrolysis polymer of tetraethoxysilane that constituted the insulating coating layer to undergo further dehydration condensation polymerization, turning it into harder and denser silicon dioxide (SiO2), further improving the insulating properties of the insulating coating layer. This type of insulating coating treatment resulted in the production of iron-nickel alloy powder with an insulating coating layer made of highly resistive silicon dioxide (SiO2) formed on the particle surface. The obtained alloy powder was composed of spherical particles with a smooth surface. The particle size distribution was sharp, with an average particle size of 0.42 μm, and the thickness of the insulating coating layer was estimated to be approximately 0.015 μm (approximately 15 nm). In addition, the insulating coating treatment caused the green resistivity (applied pressure: 64 MPa) to exceed the measurement range (>10), up from 0.04 Ω·cm before the insulating coating treatment. 7 The electrical conductivity increased significantly to 100Ω·cm.
[0263] [Example 13] In Example 13, an iron-nickel alloy powder (iron-nickel-cobalt alloy powder) containing 80 mol % of iron (Fe), 10 mol % of nickel (Ni) and 10 mol % of cobalt (Co) was produced according to the procedure shown in Fig. 5. In Example 13, when preparing the reaction solution, a room temperature metal salt raw material solution was added to and mixed with a reducing solution heated using a water bath.
[0264] <Preparation process> The water-soluble iron salt, water-soluble nickel salt, nucleating agent, complexing agent, reducing agent, pH adjuster, and amine compound were prepared in the same manner as in Example 4. In addition, cobalt sulfate heptahydrate (CoSO4·7H2O, molecular weight: 281.103, reagent manufactured by Wako Pure Chemical Industries, Ltd.) was prepared as a water-soluble cobalt salt.
[0265] <Crystallization process> (a) Preparation of metal salt source solution A metal salt raw material solution containing ferrous sulfate heptahydrate (water-soluble iron salt), nickel sulfate hexahydrate (water-soluble nickel salt), cobalt sulfate heptahydrate (water-soluble cobalt salt), palladium (II) ammonium chloride (nucleating agent), trisodium citrate dihydrate (complexing agent) and water was prepared. At this time, in the obtained metal salt raw material solution, the amount of palladium (Pd) was weighed out so that it was 0.38 mass ppm (0.2 mol ppm) with respect to the total amount of magnetic metals (Fe, Ni and Co). In addition, the amount of trisodium citrate was weighed out so that it was 0.362 (36.2 mol%) with respect to the total amount of magnetic metals (Fe, Ni and Co) in molar ratio. Specifically, 394.1 g of ferrous sulfate heptahydrate, 46.6 g of nickel sulfate hexahydrate, 49.8 g of cobalt sulfate heptahydrate, 100.8 μg of palladium (II) ammonium chloride, and 188.7 g of trisodium citrate dihydrate were dissolved in 1000 mL of pure water to prepare a metal salt raw material solution.
[0266] (b) Preparation of reducing agent solution A reducing agent solution containing sodium hydroxide (pH adjuster), hydrazine (reducing agent) and water was prepared. At this time, the amount of hydrazine was weighed out so that the molar ratio of the total amount of magnetic metals (Fe, Ni and Co) to the total amount of magnetic metals (Fe, Ni and Co) in the reaction liquid prepared in the subsequent crystallization step was 3.65. The amount of sodium hydroxide was weighed out so that the molar ratio of the total amount of magnetic metals (Fe, Ni and Co) was 7.07. Specifically, 501 g of sodium hydroxide was dissolved in 1227 mL of pure water to prepare a sodium hydroxide solution, and 540 g of 60 mass% hydrazine hydrate was added to and mixed with this sodium hydroxide solution to prepare a reducing agent solution.
[0267] (d) Preparation of amine compound solution An amine compound solution containing ethylenediamine (amine compound) and water was prepared. At this time, the ethylenediamine was weighed out so that the molar ratio of the ethylenediamine to the total amount of magnetic metals (Fe, Ni, and Co) in the reaction solution prepared in the subsequent crystallization process was a very small amount of 0.01 (1.0 mol%). Specifically, 1.07 g of ethylenediamine was dissolved in 18 mL of pure water to prepare the amine compound solution.
[0268] (e) Preparation of reaction solution and precipitation of crystallized powder The prepared metal salt raw material solution was placed in a Teflon (registered trademark) coated stainless steel container (reaction tank) equipped with stirring blades placed in a water bath and heated while stirring until the liquid temperature reached 85°C. The metal salt raw material solution with a liquid temperature of 25°C was then added to the reducing agent solution heated in the water bath for a mixing time of 10 seconds to obtain a reaction liquid with a liquid temperature of 70°C. The concentration of magnetic metals (Fe, Ni and Co) in the reaction liquid was 31.2g / L. This initiated the reduction reaction (crystallization reaction) (reaction start temperature 70°C). The temperature of the reaction liquid continued to rise by heating in the water bath after the reaction started, and was kept at a liquid temperature of 85°C after 10 minutes from the start of the reaction (reaction holding temperature 85°C). The color of the reaction liquid was dark green immediately after the start of the reaction (mixing of the reaction liquid), but changed to dark gray after a few minutes. The reason why the color tone turned dark green immediately after the start of the reaction is believed to be because the reaction according to the above formula (6) progressed and a coprecipitate of iron hydroxide (Fe(OH)2), nickel hydroxide (Ni(OH)2), and cobalt hydroxide (Co(OH)2) was formed in the reaction solution. Also, the reason why the color tone turned dark gray a few minutes after the start of the reaction is believed to be because nucleation occurred due to the action of the nucleating agent (palladium salt).
[0269] The reduction reaction was carried out by adding the amine compound solution dropwise to the reaction solution for 10 minutes, from 3 minutes to 13 minutes after the start of the reaction when the color of the reaction solution changed to dark gray. As a result, iron-nickel-cobalt crystallized powder precipitated in the reaction solution. At this time, the color of the reaction solution was black, but within 40 minutes after the start of the reaction, the supernatant liquid of the reaction solution became transparent. It is considered that the reduction reaction of the above formula (6) was completed, and all of the iron, nickel, and cobalt components in the reaction solution were reduced to metallic iron, metallic nickel, and metallic cobalt. After the reaction was completed, the reaction solution was a slurry containing iron-nickel-cobalt crystallized powder.
[0270] <Recovery process> The slurry-like reaction liquid obtained in the crystallization step was subjected to filtration, washing, and solid-liquid separation to recover a cake-like iron-nickel-cobalt crystallized powder. Filtration and washing were performed using pure water with a conductivity of 1 μS / cm until the conductivity of the filtrate filtered from the slurry was 10 μS / cm or less. The recovered cake-like crystallized powder was dried in a vacuum dryer set at 50°C. The dried crystallized powder was then cooled to 35°C in a vacuum, and nitrogen gas containing 1.0% by volume of oxygen was supplied to the crystallized powder to perform a gradual oxidation treatment. In this way, an iron-nickel-cobalt alloy powder was obtained. The obtained alloy powder was composed of spherical particles with a smooth surface. The particle size distribution was sharp, and the average particle size was 0.42 μm.
[0271] [Example 14] In Example 14, an iron-nickel alloy powder (iron-nickel-cobalt alloy powder) containing 70 mol % of iron (Fe), 10 mol % of nickel (Ni), and 20 mol % of cobalt (Co) was produced according to the procedure shown in Fig. 5. In Example 14, when preparing the reaction solution, a room temperature metal salt raw material solution was added to and mixed with a reducing solution heated using a water bath.
[0272] <Preparation process> The same raw materials as those in Example 13 were prepared as the water-soluble iron salt, the water-soluble nickel salt, the water-soluble cobalt salt, the nucleating agent, the complexing agent, the reducing agent, the pH adjuster, and the amine compound.
[0273] <Crystallization process> (a) Preparation of metal salt source solution A metal salt raw material solution containing ferrous sulfate heptahydrate (water-soluble iron salt), nickel sulfate hexahydrate (water-soluble nickel salt), cobalt sulfate heptahydrate (water-soluble cobalt salt), palladium (II) ammonium chloride (nucleating agent), trisodium citrate dihydrate (complexing agent) and water was prepared. At this time, in the obtained metal salt raw material solution, the amount of palladium (Pd) was weighed out so that it was 0.38 mass ppm (0.2 mol ppm) with respect to the total amount of magnetic metals (Fe, Ni and Co). In addition, the amount of trisodium citrate was weighed out so that it was 0.362 (36.2 mol%) with respect to the total amount of magnetic metals (Fe, Ni and Co) in molar ratio. Specifically, 343.0 g of ferrous sulfate heptahydrate, 46.3 g of nickel sulfate hexahydrate, 99.1 g of cobalt sulfate heptahydrate, 100.2 μg of palladium (II) ammonium chloride, and 187.6 g of trisodium citrate dihydrate were dissolved in 1100 mL of pure water to prepare a metal salt raw material solution.
[0274] (b) Preparation of reducing agent solution A reducing agent solution containing sodium hydroxide (pH adjuster), hydrazine (reducing agent) and water was prepared. At this time, the amount of hydrazine was weighed out so that the molar ratio of the total amount of magnetic metals (Fe, Ni and Co) to the total amount of magnetic metals (Fe, Ni and Co) in the reaction liquid prepared in the subsequent crystallization step was 1.46. The amount of sodium hydroxide was weighed out so that the molar ratio of the total amount of magnetic metals (Fe, Ni and Co) was 7.07. Specifically, 499 g of sodium hydroxide was dissolved in 1221 mL of pure water to prepare a sodium hydroxide solution, and 215 g of 60 mass% hydrazine hydrate was added to and mixed with this sodium hydroxide solution to prepare a reducing agent solution.
[0275] (d) Preparation of amine compound solution An amine compound solution containing ethylenediamine (amine compound) and water was prepared. At this time, the ethylenediamine was weighed out so that the molar ratio of the ethylenediamine to the total amount of magnetic metals (Fe, Ni, and Co) in the reaction solution prepared in the subsequent crystallization process was a very small amount of 0.01 (1.0 mol%). Specifically, 1.06 g of ethylenediamine was dissolved in 18 mL of pure water to prepare the amine compound solution.
[0276] (e) Preparation of reaction solution and precipitation of crystallized powder The prepared metal salt raw material solution was placed in a Teflon (registered trademark) coated stainless steel container (reaction tank) equipped with stirring blades placed in a water bath and heated while stirring until the liquid temperature reached 85°C. The metal salt raw material solution with a liquid temperature of 25°C was then added to the reducing agent solution heated in the water bath for a mixing time of 10 seconds to obtain a reaction liquid with a liquid temperature of 67°C. The concentration of magnetic metals (Fe, Ni and Co) in the reaction liquid was 33.7g / L. This initiated the reduction reaction (crystallization reaction) (reaction start temperature 67°C). The temperature of the reaction liquid continued to rise by heating in the water bath after the start of the reaction, and was kept at a liquid temperature of 85°C after 10 minutes from the start of the reaction (reaction holding temperature 85°C). The color of the reaction liquid was dark green immediately after the start of the reaction (mixing of the reaction liquid), but changed to dark gray after a few minutes. The reason why the color tone turned dark green immediately after the start of the reaction is believed to be because the reaction according to the above formula (6) progressed and a coprecipitate of iron hydroxide (Fe(OH)2), nickel hydroxide (Ni(OH)2), and cobalt hydroxide (Co(OH)2) was formed in the reaction solution. Also, the reason why the color tone turned dark gray a few minutes after the start of the reaction is believed to be because nucleation occurred due to the action of the nucleating agent (palladium salt).
[0277] The reduction reaction was carried out by adding the amine compound solution dropwise to the reaction solution for 10 minutes, from 3 minutes to 13 minutes after the start of the reaction when the color of the reaction solution changed to dark gray. As a result, iron-nickel-cobalt crystallized powder precipitated in the reaction solution. At this time, the color of the reaction solution was black, but within 40 minutes after the start of the reaction, the supernatant liquid of the reaction solution became transparent. It is considered that the reduction reaction of the above formula (6) was completed, and all of the iron, nickel, and cobalt components in the reaction solution were reduced to metallic iron, metallic nickel, and metallic cobalt. After the reaction was completed, the reaction solution was a slurry containing iron-nickel-cobalt crystallized powder.
[0278] <Recovery process> The slurry-like reaction liquid obtained in the crystallization step was subjected to filtration, washing, and solid-liquid separation to recover a cake-like iron-nickel-cobalt crystallized powder. Filtration and washing were performed using pure water with a conductivity of 1 μS / cm until the conductivity of the filtrate filtered from the slurry was 10 μS / cm or less. The recovered cake-like crystallized powder was dried in a vacuum dryer set at 50°C. The dried crystallized powder was then cooled to 35°C in a vacuum, and nitrogen gas containing 1.0% by volume of oxygen was supplied to the crystallized powder to perform a gradual oxidation treatment. In this way, an iron-nickel-cobalt alloy powder was obtained. The obtained alloy powder was composed of spherical particles with a smooth surface. The particle size distribution was sharp, and the average particle size was 0.40 μm.
[0279] [Example 15] In Example 15, an iron-nickel alloy powder (iron-nickel-cobalt alloy powder) containing 65 mol % of iron (Fe), 10 mol % of nickel (Ni), and 25 mol % of cobalt (Co) was produced according to the procedure shown in Fig. 5. In Example 15, when preparing the reaction solution, a room temperature metal salt raw material solution was added to and mixed with a reducing solution heated using a water bath.
[0280] <Preparation process> The same raw materials as those in Example 13 were prepared as the water-soluble iron salt, the water-soluble nickel salt, the water-soluble cobalt salt, the nucleating agent, the complexing agent, the reducing agent, the pH adjuster, and the amine compound.
[0281] <Crystallization process> (a) Preparation of metal salt source solution A metal salt raw material solution containing ferrous sulfate heptahydrate (water-soluble iron salt), nickel sulfate hexahydrate (water-soluble nickel salt), cobalt sulfate heptahydrate (water-soluble cobalt salt), palladium (II) ammonium chloride (nucleating agent), trisodium citrate dihydrate (complexing agent) and water was prepared. At this time, in the obtained metal salt raw material solution, the amount of palladium (Pd) was weighed out so that it was 0.37 mass ppm (0.2 mol ppm) with respect to the total amount of magnetic metals (Fe, Ni and Co). In addition, the amount of trisodium citrate was weighed out so that it was 0.362 (36.2 mol%) with respect to the total amount of magnetic metals (Fe, Ni and Co) in molar ratio. Specifically, 317.6 g of ferrous sulfate heptahydrate, 46.2 g of nickel sulfate hexahydrate, 123.5 g of cobalt sulfate heptahydrate, 100.0 μg of palladium (II) ammonium chloride, and 187.1 g of trisodium citrate dihydrate were dissolved in 1100 mL of pure water to prepare a metal salt raw material solution.
[0282] (b) Preparation of reducing agent solution A reducing agent solution containing sodium hydroxide (pH adjuster), hydrazine (reducing agent) and water was prepared. At this time, the amount of hydrazine was weighed out so that the molar ratio of the total amount of magnetic metals (Fe, Ni and Co) to the total amount of magnetic metals (Fe, Ni and Co) in the reaction liquid prepared in the subsequent crystallization step was 1.47. The amount of sodium hydroxide was weighed out so that the molar ratio of the total amount of magnetic metals (Fe, Ni and Co) was 7.07. Specifically, 497 g of sodium hydroxide was dissolved in 1216 mL of pure water to prepare a sodium hydroxide solution, and 215 g of 60 mass% hydrazine hydrate was added to and mixed with this sodium hydroxide solution to prepare a reducing agent solution.
[0283] (d) Preparation of amine compound solution An amine compound solution containing ethylenediamine (amine compound) and water was prepared. At this time, the ethylenediamine was weighed out so that the molar ratio of the ethylenediamine to the total amount of magnetic metals (Fe, Ni, and Co) in the reaction solution prepared in the subsequent crystallization process was a very small amount of 0.01 (1.0 mol%). Specifically, 1.06 g of ethylenediamine was dissolved in 18 mL of pure water to prepare the amine compound solution.
[0284] (e) Preparation of reaction solution and precipitation of crystallized powder The prepared metal salt raw material solution was placed in a Teflon (registered trademark) coated stainless steel container (reaction tank) equipped with stirring blades placed in a water bath and heated while stirring until the liquid temperature reached 85°C. The metal salt raw material solution with a liquid temperature of 25°C was then added to the reducing agent solution heated in the water bath for a mixing time of 10 seconds to obtain a reaction liquid with a liquid temperature of 67°C. The concentration of magnetic metals (Fe, Ni and Co) in the reaction liquid was 33.7g / L. This initiated the reduction reaction (crystallization reaction) (reaction start temperature 67°C). The temperature of the reaction liquid continued to rise by heating in the water bath after the start of the reaction, and was kept at a liquid temperature of 85°C after 10 minutes from the start of the reaction (reaction holding temperature 85°C). The color of the reaction liquid was dark green immediately after the start of the reaction (mixing of the reaction liquid), but changed to dark gray after a few minutes. The reason why the color tone turned dark green immediately after the start of the reaction is believed to be because the reaction according to the above formula (6) progressed and a coprecipitate of iron hydroxide (Fe(OH)2), nickel hydroxide (Ni(OH)2), and cobalt hydroxide (Co(OH)2) was formed in the reaction solution. Also, the reason why the color tone turned dark gray a few minutes after the start of the reaction is believed to be because nucleation occurred due to the action of the nucleating agent (palladium salt).
[0285] The reduction reaction was carried out by adding the amine compound solution dropwise to the reaction solution for 10 minutes, from 3 minutes to 13 minutes after the start of the reaction when the color of the reaction solution changed to dark gray. As a result, iron-nickel-cobalt crystallized powder precipitated in the reaction solution. At this time, the color of the reaction solution was black, but within 30 minutes after the start of the reaction, the supernatant liquid of the reaction solution became transparent. It is considered that the reduction reaction of the above formula (6) was completed, and all of the iron, nickel, and cobalt components in the reaction solution were reduced to metallic iron, metallic nickel, and metallic cobalt. After the reaction was completed, the reaction solution was a slurry containing iron-nickel-cobalt crystallized powder.
[0286] <Recovery process> The slurry-like reaction liquid obtained in the crystallization step was subjected to filtration, washing, and solid-liquid separation to recover a cake-like iron-nickel-cobalt crystallized powder. Filtration and washing were performed using pure water with a conductivity of 1 μS / cm until the conductivity of the filtrate filtered from the slurry was 10 μS / cm or less. The recovered cake-like crystallized powder was dried in a vacuum dryer set at 50°C. The dried crystallized powder was then cooled to 35°C in a vacuum, and nitrogen gas containing 1.0% by volume of oxygen was supplied to the crystallized powder to perform a gradual oxidation treatment. In this way, an iron-nickel-cobalt alloy powder was obtained. The obtained alloy powder was composed of spherical particles with a smooth surface. The particle size distribution was sharp, and the average particle size was 0.42 μm.
[0287] [Comparative Example 1] In Comparative Example 1, palladium (II) ammonium chloride (nucleating agent) was not added when preparing the metal salt raw material solution. Otherwise, the reaction solution was prepared and the crystallized powder was precipitated in the same manner as in Example 1, and an iron-nickel alloy powder (iron-nickel alloy powder) containing 50 mol% iron (Fe) and 50 mol% nickel (Ni) was produced. The concentration of magnetic metals (Fe and Ni) in the reaction solution was 32.3 g / L. The obtained alloy powder was composed of spherical particles, and the surfaces of these particles were uneven. The particle size distribution was sharp, and the average particle size was 0.65 μm.
[0288] [Comparative Example 2] In Comparative Example 2, trisodium citrate dihydrate (complexing agent) was not added when preparing the metal salt raw material solution. Otherwise, the reaction solution was prepared and the crystallized powder was precipitated in the same manner as in Example 1, and an iron-nickel alloy powder (iron-nickel alloy powder) containing 50 mol% iron (Fe) and 50 mol% nickel (Ni) was produced. The concentration of magnetic metals (Fe and Ni) in the reaction solution was 33.3 g / L. The obtained alloy powder was composed of irregularly shaped particles, and the surfaces of these particles were uneven. The particle size distribution was broad, and the average particle size was 0.26 μm.
[0289] [Comparative Example 3] In Comparative Example 3, when preparing the metal salt raw material solution, palladium (II) ammonium chloride (nucleating agent) and trisodium citrate dihydrate (complexing agent) were not mixed. When preparing the reducing agent solution, a large amount of hydrazine (reducing agent) was mixed. Otherwise, an iron-nickel alloy powder (iron-nickel alloy powder) was produced in the same manner as in Example 1. The metal salt raw material solution and the reducing agent solution were prepared as shown below.
[0290] (a) Preparation of metal salt source solution A metal salt raw material solution containing ferrous chloride tetrahydrate (water-soluble iron salt), nickel chloride hexahydrate (water-soluble nickel salt), and water was prepared. Specifically, 173.60 g of ferrous chloride tetrahydrate and 207.55 g of nickel chloride hexahydrate were dissolved in 1200 mL of pure water to prepare the metal salt raw material solution.
[0291] (b) Preparation of reducing agent solution A reducing agent solution containing sodium hydroxide (pH adjuster), hydrazine (reducing agent) and water was prepared. At this time, the amount of hydrazine was weighed out so that the molar ratio of the amount of magnetic metal (Fe and Ni) to the total amount of magnetic metal was 19.4 in the reaction solution prepared in the subsequent crystallization process. The amount of sodium hydroxide was weighed out so that the molar ratio of the amount of magnetic metal (Fe and Ni) to the amount of magnetic metal was 4.96. Specifically, 346 g of sodium hydroxide was dissolved in 850 mL of pure water to prepare a sodium hydroxide solution, and 2828 g of 60 mass% hydrazine hydrate was added and mixed to prepare a reducing agent solution. The reducing agent solution was heated to a liquid temperature of 37°C before use so that the reaction start temperature was 55°C when the reducing agent solution was added and mixed with the metal salt raw material solution.
[0292] The obtained alloy powder was composed of spherical particles with relatively smooth surfaces. The particle size distribution was broad, and the average particle size was 0.22 μm.
[0293] The production conditions of the alloy powders of Examples 1 to 15 and Comparative Examples 1 to 3 are summarized in Table 1.
[0294] [Table 1]
[0295] (2) Evaluation of iron-nickel alloy powder The iron-nickel alloy powders obtained in Examples 1 to 15 and Comparative Examples 1 to 3 were evaluated for various properties as follows.
[0296] <Composition analysis> X-ray diffraction (XRD) measurements were performed using an X-ray diffractometer, and the presence or absence of alloy powder generation was confirmed from the obtained XRD data.
[0297] <Analysis of metal impurities> The impurity content was analyzed. The oxygen content was measured by the inert gas fusion method using an oxygen analyzer (LECO Corporation, TC436), and the carbon and sulfur content was measured by the combustion method using a carbon-sulfur analyzer (LECO Corporation, CS600). The chlorine content was measured using an X-ray fluorescence analyzer (Spectris, Magix), and the silicon and sodium contents were measured using an ICP emission spectrometer (Agilent Technologies, 5100).
[0298] <Particle size (average particle size, coefficient of variation)> The alloy powder was observed with a scanning electron microscope (SEM; JEOL Ltd., JSM-7100F) (magnification: 5000 to 80000 times). The observed images (SEM images) were analyzed, and the average particle size and standard deviation of the particle size were calculated from the number average. Furthermore, the coefficient of variation (CV value) was calculated according to the following formula (14) to determine the particle size (average particle size, coefficient of variation) of the alloy powder.
[0299]
number
[0300] <Intraparticle composition analysis> The alloy powder embedded in the resin was processed into a thin film of about 100 nm using a focused ion beam (FIB) device, and the cross section of the alloy particles in the processed sample was observed with a scanning transmission electron microscope (STEM; Hitachi High-Technologies Corporation, HD-2300A). The observation was performed at a magnification of 100,000 to 200,000 times. The composition distribution in the alloy particles was determined by line analysis using an energy dispersive x-ray spectroscopy (EDS) device. In this case, the composition was calculated from the detection count of the characteristic X-ray (K line) of the measured element.
[0301] <Crystallite diameter> The alloy powder was analyzed by X-ray diffraction (XRD) and the crystallite size was evaluated based on the Scherrer formula from the half-width of the (111) X-ray diffraction peak. The XRD measurement conditions were the same as those for the composition analysis. The crystallite size indicates the degree of crystallization, and the larger the crystallite size, the higher the crystallinity.
[0302] <Compressed powder density> The green density of the alloy powder was evaluated. Specifically, about 0.3 g of the alloy powder was filled into a cylindrical hole (inner diameter 5 mm) of a die. Then, the alloy powder was molded into a pellet shape with a diameter of 5 mm and a height of 3 to 4 mm at a pressure of 100 MPa using a press. The mass and height of the obtained pellet were measured at room temperature, and the green density was calculated.
[0303] <Compressed powder resistivity> The compact resistivity of the alloy powder was measured using a powder resistivity measurement system (Mitsubishi Chemical Analytech, MCP-PD51) to evaluate the electrical conductivity (insulation). Specifically, approximately 4 g of alloy powder was filled into the cylindrical sample chamber of the device, and a pressure of 64 MPa was applied using a press machine attached to the device to obtain the compact resistivity (unit: Ω·cm).
[0304] <Magnetic properties (saturation magnetic flux density, coercive force)> Measurements were performed using a vibrating sample magnetometer (VSM) to evaluate the magnetic properties (saturation magnetic flux density (T: Tesla), coercive force (A / m)) of the alloy powder. The values of saturation magnetic flux density and coercive force were calculated from the BH curve (magnetic hysteresis curve) obtained by the measurement. Note that the magnetic properties of the alloy powder obtained in Comparative Example 2 were not measured because its shape was distorted and it could not be applied to elements such as inductors.
[0305] (3) Evaluation results The evaluation results obtained for Examples 1 to 15 and Comparative Examples 1 to 3 are summarized in Table 2. SEM images of the alloy powders obtained in Examples 1, 2, 10, 13, and 14 are shown in Figs. 8, 9, 13, 15, and 16, respectively, and SEM images of the alloy powder obtained in Example 6 are shown in Figs. 10(a) and 10(b). Here, Fig. 10(a) is an SEM image of the alloy powder before the spiral jet crushing treatment, and Fig. 10(b) is an SEM image of the alloy powder after the spiral jet crushing treatment. In addition, STEM images and EDS line analysis results of the particle cross sections of the alloy powders obtained in Examples 8 and 9 are shown in Figs. 11(a), (b), and 12, respectively. Here, Fig. 11(a) is an STEM image and EDS line analysis results of the particle cross sections of the alloy powder before the high-temperature heat treatment, and Fig. 11(b) is an STEM image and EDS line analysis results of the particle cross sections of the alloy powder after the high-temperature heat treatment. Figures 14(a) and 14(b) show SEM images of the alloy powder obtained in Example 12. Figure 14(a) shows an SEM image of the alloy powder before the insulating coating treatment, and Figure 14(b) shows an SEM image of the alloy powder after the insulating coating treatment. Figures 17 to 19 show SEM images of the alloy powders obtained in Comparative Examples 1 to 3, respectively.
[0306] In Example 1, Example 3, and Comparative Examples 1 to 3, iron-nickel alloy powder was produced by setting the reaction start temperature in the crystallization step at 55°C and the reaction holding temperature at 70°C. In Example 1 and Example 3, which used extremely small amounts of specific nucleating agents and complexing agents, the amount of hydrazine used as a reducing agent was small, but the obtained alloy powder had a fine average particle size of 0.40 to 0.41 μm, a small CV value, and a sharp particle size distribution. In addition, the alloy powder was spherical and had a smooth surface.
[0307] On the other hand, in Comparative Example 1, in which no nucleating agent was used, the obtained alloy powder had a large average particle size of 0.65 μm, compared with Examples 1 and 3, and it was difficult to refine the powder. In addition, although the powder was spherical, the surface irregularities were large. In Comparative Example 2, in which no complexing agent was used, the obtained alloy powder had a fine average particle size of 0.26 μm, but the CV value was large and the particle size distribution was wide. Furthermore, the alloy powder had a large surface irregularity and was irregular in shape. In Comparative Example 3, in which no nucleating agent or complexing agent was used and a large amount of reducing agent (hydrazine) was added, the obtained alloy powder was a spherical powder with a relatively smooth surface. This is considered to be due to the fact that the reduction reaction was strongly activated by adding a large amount of hydrazine. In addition, the obtained alloy powder had a fine average particle size of 0.22 μm. However, the CV value was large and the particle size distribution was wide.
[0308] Example 2 is an example in which iron-nickel-cobalt alloy powder was produced using a specific nucleating agent and complexing agent, with the reaction start temperature in the crystallization process set to 55°C and the reaction holding temperature set to 70°C. Despite the small amount of hydrazine used as a reducing agent, the obtained alloy powder had a fine average particle size of about 0.3 μm and a sharp particle size distribution. The alloy powder also had a smooth surface and was spherical. The saturation magnetization of the alloy powder was also high.
[0309] In Example 5, an additional raw material liquid containing a water-soluble nickel salt was added to the reaction liquid during crystallization to produce an iron-nickel alloy powder containing 51 mol% iron (Fe) and 49 mol% nickel (Ni) with a nickel-rich surface composition. A dense oxide film was formed due to the nickel-rich surface composition, suppressing the amount of oxidation on the particle surface. Therefore, this alloy powder is not only more stable in the air, but also has excellent magnetic properties such as saturation magnetic flux density.
[0310] Example 6 is an example in which a crystallized powder obtained as a dry powder through a crystallization process and a recovery process is subjected to a spiral jet crushing process to produce a spherical iron-nickel alloy powder with a very smooth surface. Example 7 is an example in which a high-pressure fluid collision crushing process is performed on a slurry-like crystallized powder during the recovery process after the crystallization process to produce a spherical iron-nickel alloy powder with a very smooth surface. In addition to having a smooth surface, these alloy powders also have reduced agglomerated particles. As a result, the packing property is improved (the green compact density is increased). Furthermore, the reduction in agglomerated particles is expected to improve eddy current loss through particles.
[0311] Example 8 is an example of the production of an iron-nickel alloy powder containing 65 mol% iron (Fe) and 35 mol% nickel (Ni) with improved composition uniformity within the particles by subjecting the crystallized powder obtained in the crystallization process to a high-temperature heat treatment at a reaction start temperature of 71°C and a reaction holding temperature of 80°C. As is clear from Figure 11(b), this alloy powder has a uniform composition (65 mol% iron and 35 mol% nickel) within the particles, and is expected to be used not only as a soft magnetic material but also as a low thermal expansion material (Invar alloy).
[0312] In Example 9, an additional raw material solution containing a water-soluble nickel salt was added to the reaction solution during crystallization to produce an iron-nickel alloy powder containing 65 mol% iron (Fe) and 35 mol% nickel (Ni) with a nickel-rich surface composition. As is clear from FIG. 12, a nickel-rich layer with a thickness of about 10 to 15 nm is formed on the particle surface, and a dense oxide film is formed due to this nickel-rich surface composition, suppressing the amount of oxidation on the particle surface. Therefore, this alloy powder is not only more stable in the air, but also has excellent magnetic properties such as saturation magnetic flux density.
[0313] In Examples 10 and 11, an additional raw material solution containing a water-soluble nickel salt was added to the reaction solution during crystallization to promote the reduction of iron ions (or iron hydroxide) that are difficult to reduce, while the particle surface has a more nickel-rich composition. The iron content is as high as 80 mol% to 90 mol%, and the composition is close to pure iron. However, even with a relatively small amount of hydrazine used as a reducing agent, reduction failure does not occur, and a smooth-surfaced, spherical alloy powder with an average particle size of about 0.4 to 0.5 μm and a sharp particle size distribution was obtained. The saturation magnetization of the alloy powder was as high as that of pure iron powder (1.95 T to 2.0 T).
[0314] In comparison with Examples 1-7, in Examples 8-11, the green density of the obtained iron-nickel alloy powder is smaller. However, the true density of the iron-nickel alloy powders of Examples 1 to 7 (iron-nickel alloy powder containing 56 to 50 mol% Fe and 44 to 50 mol% Ni, and iron-nickel-cobalt alloy powder containing 50 mol% Fe, 40 mol% Ni, and 10 mol% Co) is 8.2 to 8.25, whereas the true density of the iron-nickel alloy powders of Examples 8 and 9 (iron-nickel alloy powder containing 65 mol% Fe and 35 mol% Ni) is 8.1, the true density of the iron-nickel alloy powder of Example 10 (iron-nickel alloy powder containing 80 mol% Fe and 20 mol% Ni) is 8.0, and the true density of the iron-nickel alloy powder of Example 11 (iron-nickel alloy powder containing 90 mol% Fe and 10 mol% Ni) is 7.9. Considering that the true density of the iron-nickel alloy powder decreases as the iron content increases, it can be seen that the green compact density of each Example is good.
[0315] Example 12 is an example of producing an iron-nickel alloy powder in which the particle surfaces are coated with highly resistive silicon dioxide (SiO2) by applying an insulating coating treatment to the crystallized powder obtained as a dry powder through the crystallization process and the recovery process. This alloy powder has significantly improved insulation between particles (significantly increased powder compact resistivity), and is therefore expected to improve eddy current loss between particles.
[0316] Examples 13 to 15 are examples of producing iron-nickel alloy powders with a cobalt content of 10 mol% to 25 mol% and a high iron content of 65 mol% to 80 mol% by adding a water-soluble iron salt, a water-soluble nickel salt, and a water-soluble cobalt salt to the magnetic metal source to promote the reduction of iron ions (or iron hydroxide) that are difficult to reduce. Specifically, these are examples of producing iron-nickel-cobalt alloy powders containing Fe 80 mol%, Ni 10 mol% and Co 10 mol%, iron-nickel-cobalt alloy powders containing Fe 70 mol%, Ni 10 mol% and Co 20 mol%, and iron-nickel-cobalt alloy powders containing Fe 65 mol%, Ni 10 mol% and Co 25 mol%. Although the composition has a high iron content of 65 mol% to 80 mol%, the reduction reaction promotion effect of the addition of cobalt allows the spherical alloy powders to be obtained without reduction failure even with a very small amount of hydrazine used as a reducing agent. The alloy powder had a fine average particle size of about 0.4 μm, a sharp particle size distribution, and a smooth surface. The saturation magnetization of the alloy powder was equal to or higher than that of pure iron powder (1.95 T to 2.0 T).
[0317] Furthermore, the true specific gravity of the iron-nickel alloy powders (iron-nickel-cobalt alloy powders) obtained in Examples 13 to 15 was estimated to be about 8.0 to 8.1, and the green density of all of them was large and good. This is believed to be because the reduction reaction was completed before the aggregation of particles progressed due to the reduction reaction promotion effect of the addition of cobalt, and as a result, the aggregation of particles during crystallization was suppressed. In addition, it is believed that the improvement in the packing property of the particles is also related to the promotion of spheroidization, which is another effect of the addition of cobalt.
[0318] [Table 2]
Claims
1. A method for producing an iron (Fe)-nickel (Ni) based alloy powder containing at least iron (Fe) and nickel (Ni) as magnetic metals, the method comprising the following steps: A preparation step of preparing a magnetic metal source, a nucleating agent, a complexing agent, a reducing agent, and a pH adjusting agent as starting materials; a crystallization step of preparing a reaction liquid containing the starting material and water, and crystallizing a crystallized powder containing the magnetic metal in the reaction liquid by a reduction reaction; and A recovery step of recovering the crystallized powder from the reaction liquid, The magnetic metal source includes a water-soluble iron salt and a water-soluble nickel salt; the nucleating agent is a water-soluble salt of a metal more noble than nickel; the complexing agent is at least one selected from the group consisting of a hydroxycarboxylic acid, a salt of a hydroxycarboxylic acid, and a derivative of a hydroxycarboxylic acid; The reducing agent is hydrazine (N 2 H 4 ) and The pH adjuster is an alkali hydroxide, When preparing a reaction solution in the crystallization step, a metal salt raw material solution in which the magnetic metal source, the nucleating agent, and the complexing agent are dissolved in water is prepared; a reducing agent solution obtained by dissolving the reducing agent in water; A pH adjusting solution obtained by dissolving the pH adjuster in water; and mixing the metal salt raw material solution and the pH adjusted solution to obtain a mixed solution. mixing the mixed solution with the reducing agent solution; method.
2. A method for producing an iron (Fe)-nickel (Ni) based alloy powder containing at least iron (Fe) and nickel (Ni) as magnetic metals, the method comprising the following steps: A preparation step of preparing a magnetic metal source, a nucleating agent, a complexing agent, a reducing agent, and a pH adjusting agent as starting materials; a crystallization step of preparing a reaction liquid containing the starting material and water, and crystallizing a crystallized powder containing the magnetic metal in the reaction liquid by a reduction reaction; and A recovery step of recovering the crystallized powder from the reaction liquid, The magnetic metal source includes a water-soluble iron salt and a water-soluble nickel salt; the nucleating agent is a water-soluble salt of a metal more noble than nickel; the complexing agent is at least one selected from the group consisting of a hydroxycarboxylic acid, a salt of a hydroxycarboxylic acid, and a derivative of a hydroxycarboxylic acid; The reducing agent is hydrazine (N 2 H 4 ) and The pH adjuster is an alkali hydroxide, When preparing a reaction solution in the crystallization step, a metal salt raw material solution in which the magnetic metal source, the nucleating agent, and the complexing agent are dissolved in water, and a reducing agent solution in which the reducing agent and the pH adjuster are dissolved in water are prepared, and the metal salt raw material solution and the reducing agent solution are mixed. method.
3. The water-soluble iron salt is ferrous chloride (FeCl 2 ), ferrous sulfate (FeSO 4 ), and ferrous nitrate (Fe(NO 3 ) 2 The method according to claim 1 or 2, wherein the at least one selected from the group consisting of:
4. The water-soluble nickel salt is nickel chloride (NiCl 2 ), nickel sulfate (NiSO 4 ), and nickel nitrate (Ni(NO 3 ) 2 The method according to any one of claims 1 to 3, wherein the compound is at least one selected from the group consisting of:
5. The method according to any one of claims 1 to 4, wherein the nucleating agent is at least one selected from the group consisting of copper salts, palladium salts, and platinum salts.
6. The complexing agent is tartaric acid ((CH(OH)COOH) 2 ) and citric acid (C(OH)(CH 2 COOH) 2 The method according to any one of claims 1 to 5, wherein the hydroxycarboxylic acid is at least one selected from the group consisting of hydroxycarboxylic acids, hydroxycarboxylic acids (COOH), ... and hydroxycarboxylic acids (COOH).
7. The method according to any one of claims 1 to 6, wherein the pH adjuster is at least one selected from sodium hydroxide (NaOH) and potassium hydroxide (KOH).
8. The magnetic metal further comprises cobalt (Co); The method of any one of claims 1 to 7, wherein the magnetic metal source further comprises a water-soluble cobalt salt.
9. In the magnetic metal, the content of iron (Fe) is 60 mol% or more and 85 mol% or less, and the content of cobalt (Co) is 10 mol% or more and 30 mol% or less, 9. The method according to claim 8, wherein the magnetic metal source has a water-soluble iron salt content of 60 mol % or more and 85 mol % or less, and a water-soluble cobalt salt content of 10 mol % or more and 30 mol % or less.
10. The water-soluble cobalt salt is cobalt chloride (CoCl 2 ), cobalt sulfate (CoSO 4 ), and cobalt nitrate (Co(NO 3 ) 2 The method according to claim 8 or 9, wherein the at least one selected from the group consisting of
11. The starting material contains two or more primary amino groups (-NH 2 ), one primary amino group (-NH 2 11. The method according to claim 1, further comprising the step of: providing an amine compound having one or more secondary amino groups (-NH-) or two or more secondary amino groups (-NH-) in the molecule.
12. The method of claim 11, wherein the amine compound is at least one of an alkylene amine and an alkylene amine derivative.
13. The method according to claim 12, wherein the alkyleneamine and / or alkyleneamine derivative has at least a structure represented by the following (A) in which a nitrogen atom of an amino group in the molecule is bonded via a carbon chain having two carbon atoms: 【Chemistry 1】
14. The amine compound is ethylenediamine (H 2 N.C. 2 H 4 N.H. 2 ), diethylenetriamine (H 2 N.C. 2 H 4 N.H.C. 2 H 4 N.H. 2 ), triethylenetetramine (H 2 N (C 2 H 4 N.H. 2 C 2 H 4 N.H. 2 ), tetraethylenepentamine (H 2 N (C 2 H 4 N.H. 3 C 2 H 4 N.H. 2 ), pentaethylenehexamine (H 2 N (C 2 H 4 N.H. 4 C 2 H 4 N.H. 2 ), and propylenediamine (CH 3 CH(NH 2 ) CH 2 N.H. 2 At least one alkyleneamine selected from the group consisting of tris(2-aminoethyl)amine (N(C 2 H 4 N.H. 2 ) 3 ), N-(2-aminoethyl)ethanolamine (H 2 N.C. 2 H 4 N.H.C. 2 H 4 OH), N-(2-aminoethyl)propanolamine (H 2 N.C. 2 H 4 N.H.C. 3 H 6 OH), 2,3-diaminopropionic acid (H 2 NCH 2 CH(NH)COOH), ethylenediamine-N,N'-diacetic acid (HOOCCH 2 N.H.C. 2 H 4 N.H.C.H. 2 COOH), and 1,2-cyclohexanediamine (H 2 N.C. 6 H10NH 2 The method according to any one of claims 11 to 13, wherein the alkyleneamine derivative is at least one selected from the group consisting of:
15. The method according to any one of claims 11 to 14, wherein the amount of the amine compound is 0.01 mol % or more and 5.00 mol % or less relative to the total amount of the magnetic metal.
16. The method according to claim 1 , wherein, when preparing the reaction solution, the pH adjusting solution and the reducing agent solution are added to and mixed with the metal salt raw material solution in that order.
17. The method according to claim 1 or 16, wherein the time required for mixing the mixed solution and the reducing agent solution is 1 second or more and 180 seconds or less.
18. The method according to claim 2 , wherein, when preparing the reaction solution, the reducing agent solution is added to the metal salt raw material solution, or conversely, the metal salt raw material solution is added to the reducing agent solution and mixed.
19. 20. The method according to claim 2 or 18, wherein the time required for mixing the metal salt source solution and the reducing agent solution is 1 second or more and 180 seconds or less.
20. The method according to any one of claims 1 to 19, wherein in the crystallization step, an additional raw material liquid in which at least one of the water-soluble nickel salt and the water-soluble cobalt salt is dissolved in water is further added to the reaction liquid and mixed before the reduction reaction is completed.
21. The method according to claim 1 , wherein an amine compound is added to at least one of the metal salt raw material solution, the reducing agent solution, the pH adjusting solution, and the reaction solution.
22. The method according to claim 2, wherein an amine compound is added to at least one of the metal salt raw material solution, the reducing agent solution, and the reaction solution.
23. The method according to any one of claims 1 to 22, wherein the temperature of the reaction solution at the start of crystallization of the crystallized powder (reaction initiation temperature) is 40°C or higher and 90°C or lower, and the temperature of the reaction solution maintained during crystallization after the start of crystallization (reaction maintenance temperature) is 60°C or higher and 99°C or lower.
24. The method according to any one of claims 1 to 23, further comprising a crushing step in which the crystallized powder after the recovery step or the crystallized powder during the recovery step is subjected to a crushing treatment using collision energy to crush aggregated particles contained in the crystallized powder.
25. The method according to claim 24, wherein the crystallized powder after the recovery step is crushed by dry crushing or wet crushing, or the crystallized powder during the recovery step is crushed by wet crushing.
26. 26. The method of claim 25, wherein the dry milling is spiral jet milling.
27. 26. The method of claim 25, wherein the wet grinding is high pressure fluid impingement grinding.
28. The method according to any one of claims 1 to 27, further comprising a high-temperature heat treatment step in which the crystallized powder after the recovery step or the crystallized powder during the recovery step is subjected to a heat treatment at a temperature higher than 150 ° C. and not higher than 400 ° C. in an inert atmosphere, a reducing atmosphere, or a vacuum atmosphere, thereby improving the composition uniformity within the particles of the iron (Fe)-nickel (Ni)-based alloy powder.
29. The method according to any one of claims 1 to 28, further comprising an insulating coating step of subjecting the crystallized powder obtained through the recovery step to an insulating coating treatment to form an insulating coating layer made of a metal oxide on the particle surfaces of the crystallized powder, thereby improving insulation between particles.
30. 30. The method according to claim 29, wherein in the insulating coating step, the crystallized powder is dispersed in a mixed solvent containing water and an organic solvent, a metal alkoxide is further added to and mixed with the mixed solvent to prepare a slurry, the metal alkoxide is hydrolyzed and subjected to dehydration condensation polymerization in the slurry to form an insulating coating layer made of a metal oxide on the particle surfaces of the crystallized powder, and then the crystallized powder with the insulating coating layer formed thereon is recovered from the slurry.
31. The metal alkoxide is mainly composed of silicon alkoxide (alkyl silicate), and the metal oxide is silicon dioxide (SiO 2 31. The method of claim 30, wherein the main component is
32. The method according to claim 30 or 31, wherein the hydrolysis of the metal alkoxide is carried out in the presence of a base catalyst (alkali catalyst).
Citation Information
Patent Citations
Preparation method for superfine spherical nickel-iron alloy powder
CN108274020A
Production of composite grain
JP1995076702A
Production of multilayer coating-coated powder
JP1998259401A
Ni-fe alloy powder
JP2003193160A
Method for manufacturing nickel-iron alloy nanoparticle, and nickel-iron alloy nanoparticle
JP2008024961A