Copper-zinc alloy and machinery and equipment using the same
A copper-zinc alloy with specific Zn and Co content forms soft cobalt oxides to address adhesion and seizure issues, improving seizure and wear resistance in sliding members.
Patent Information
- Application Number
- JP2020159535
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-24
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2040-09-24
AI Technical Summary
Copper-zinc alloys used in sliding members like bearings for internal combustion engines face issues with adhesion and seizure due to the formation of hard oxides like alumina and silica, which peel off during sliding, leading to increased shear resistance and potential seizure.
A copper-zinc alloy composition with 44% or more Zn, 0.5% to 3.1% Co, and the balance Cu and unavoidable impurities, where the parent phase is composed of a single β phase, (α+β) phase, or (β+γ) phase, forms soft cobalt oxides that act as a solid lubricant, reducing adhesion and improving seizure resistance.
The alloy enhances seizure resistance and wear resistance by forming soft cobalt oxides that prevent peeling and adhesion, while maintaining mechanical properties and reducing manufacturing costs.
Smart Images

Figure 0007583404000003 
Figure 0007583404000004 
Figure 0007583404000005
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a copper-zinc alloy and a mechanical device using the same. [Background technology]
[0002] Conventionally, copper-zinc alloys have been used for sliding members such as bearings of superchargers for internal combustion engines. For such copper-zinc alloys, copper-zinc alloys containing Cu, Zn, Al, Mn, and Si as main components are used. The copper-zinc alloys containing Al, Mn, Si, and the like have their hardness increased by adding Al, Mn, and Si as alloy components, and also form Mn-Si compounds, and thus improve the wear resistance of the copper-zinc alloy (see Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 3718147 Summary of the Invention [Problem to be solved by the invention]
[0004] However, if the copper-zinc alloy contains Al or Si, Al and Si are more easily oxidized than Cu and Zn, and therefore form oxides made of alumina or silica on the surface of the copper-zinc alloy during sliding, etc. Alumina and silica are hard oxides, and therefore are easily peeled off due to shear resistance during sliding, etc. As a result, adhesion of the copper-zinc alloy occurs, and there is a possibility that the copper-zinc alloy may become seized.
[0005] Therefore, an object of the present disclosure is to provide a copper-zinc alloy capable of improving seizure resistance and a mechanical device using the same. [Means for solving the problem]
[0006] The present disclosure For bearings Copper-zinc alloys are 44 Mass% or more 47% or less by mass of Zn, 0.5% to 3.1% by mass of Co, and the balance being Cu and unavoidable impurities. The matrix is composed of a single β phase. It is characterized by:
[0011] The present disclosure For bearings In the copper-zinc alloy, the Co content may be 1.9 mass % or more and 3.1 mass % or less.
[0012] The mechanical device according to the present disclosure is For bearings Made of copper-zinc alloy The rotor shaft is provided with a bearing and the rotor shaft slides on the bearing, and the bearing is a radial bearing or a thrust bearing. It is characterized by: Effect of the Invention
[0014] According to the copper-zinc alloy having the above-mentioned configuration and the mechanical device using the same, it is possible to improve the seizure resistance. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a diagram illustrating a configuration of a supercharger in an embodiment of the present disclosure. [Diagram 2] FIG. 2 is a schematic diagram for explaining a seizure resistance test method in an embodiment of the present disclosure. [Diagram 3] 4 is a graph showing test results of seizure resistance in an embodiment of the present disclosure. [Figure 4] 1 is a graph showing test results of abrasion resistance in an embodiment of the present disclosure. [Diagram 5] 1 is a graph showing hardness test results in an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The embodiments of the present disclosure will be described in detail below with reference to the drawings. The copper-zinc alloy according to the embodiment of the present disclosure contains 30% by mass or more and 51% by mass or less of Zn (zinc), 0.5% by mass or more and 3.1% by mass or less of Co (cobalt), and the balance is composed of Cu (copper) and unavoidable impurities. Next, the reason for limiting the composition range of each alloy component constituting this copper-zinc alloy will be described.
[0017] Zn has the function of improving the mechanical properties of the copper-zinc alloy. The Zn content can be 30% by mass or more and 51% by mass or less. If the Zn content is less than 30% by mass, the mechanical properties of the copper-zinc alloy may be reduced. If the Zn content is more than 51% by mass, the copper-zinc alloy may become embrittled and the mechanical properties may be reduced. By setting the Zn content to 30% by mass or more and 51% by mass or less, the parent phase of the copper-zinc alloy can be an α single phase, an (α+β) phase, a β single phase, or a (β+γ) phase.
[0018] The Zn content may be 30% by mass or more and 31% by mass or less. By setting the Zn content to 30% by mass or more and 31% by mass or less, the parent phase of the copper-zinc alloy can be a single α phase.
[0019] The Zn content may be 40% by mass or more and 51% by mass or less. By making the Zn content 40% by mass or more and 51% by mass or less, the parent phase of the copper-zinc alloy can be the (α+β) phase, the β single phase, or the (β+γ) phase. Since the parent phase of the copper-zinc alloy is composed of the (α+β) phase, the β single phase, or the (β+γ) phase, the wear resistance can be improved more than when the parent phase is composed of the α single phase. In addition, since Zn is less expensive than Cu, the manufacturing cost of the copper-zinc alloy can be reduced by increasing the Zn content.
[0020] The Zn content may be 44% by mass or more and 47% by mass or less. By setting the Zn content to 44% by mass or more and 47% by mass or less, the parent phase of the copper-zinc alloy can be a β single phase. By setting the Zn content in this composition range, the seizure resistance of the copper-zinc alloy can be further improved when Co is added as described later.
[0021] The Zn content may be 50% by mass or more and 51% by mass or less. By making the Zn content 50% by mass or more and 51% by mass or less, the parent phase of the copper-zinc alloy can be a (β+γ) phase. By making the Zn content within this composition range, the parent phase contains a γ phase, so that the wear resistance of the copper-zinc alloy can be improved.
[0022] Co has the function of improving the seizure resistance of the copper-zinc alloy. One of the reasons why Co improves the seizure resistance of the copper-zinc alloy is that it forms soft cobalt oxides (CoO, Co3O4, etc.) on the surface of the copper-zinc alloy during sliding, etc. It is believed that the soft cobalt oxides present on the surface of the copper-zinc alloy in the form of powder or thin film, etc., act like a solid lubricant. This can suppress adhesion due to shear resistance during sliding, etc., and improve the seizure resistance of the copper-zinc alloy.
[0023] More specifically, Co tends to oxidize more easily than Cu and Zn. Therefore, on the surface of the copper-zinc alloy, cobalt is preferentially oxidized during sliding, etc., and cobalt oxide is formed. For example, in the case of a binary copper-zinc alloy, Zn is more easily oxidized than Cu, so zinc oxide (ZnO, etc.) is formed on the surface of the copper-zinc alloy. Zinc oxide is softer than alumina (Al2O3) and silica (SiO2), which will be described later, so it has better seizure resistance than copper-zinc alloys containing Al (aluminum) and Si (silicon), but it has lower seizure resistance than cobalt oxide.
[0024] Furthermore, when the copper-zinc alloy contains Al and Si, Al and Si are more easily oxidized than Cu and Zn, so alumina and silica are formed on the surface of the copper-zinc alloy by selective oxidation. Alumina and silica are harder oxides than cobalt oxide, so they are more likely to peel off due to shear resistance during sliding, etc. As a result, the shear resistance increases and they adhere, causing seizure in the copper-zinc alloy. In contrast, cobalt oxide is softer than alumina and silica, so it is less likely to peel off due to shear resistance during sliding. This suppresses adhesion due to increased shear resistance, improving the seizure resistance of the copper-zinc alloy.
[0025] Co is a solid solution strengthening element, and has the function of improving the mechanical properties by solid-solubilizing in the parent phase of the copper-zinc alloy. In addition, since Co has a high melting point, it can improve the high-temperature strength of the copper-zinc alloy. For example, in a particle-dispersed copper-zinc alloy strengthened by dispersing hard particles made of intermetallic compounds such as Si or oxides such as alumina, the sliding surface may be damaged due to the falling off of the hard particles during sliding. In contrast, Co enhances the mechanical properties by solid solution strengthening, and therefore can suppress damage to the sliding surface during sliding.
[0026] Co has excellent corrosion resistance, so it can improve the corrosion resistance of the copper-zinc alloy. Depending on the usage environment, the copper-zinc alloy may be exposed to high-temperature engine oil. In such a case, the copper-zinc alloy may react chemically with the sulfur content in the engine oil and corrode to a black color. Since such a black corrosion layer easily peels off, peeling wear or peeled wear pieces may affect the sliding members, etc., causing abnormal wear. Since the copper-zinc alloy contains Co, it can suppress corrosion caused by sulfur content. This makes it possible to improve the wear resistance of the copper-zinc alloy.
[0027] The content of Co is preferably 0.5% by mass or more and 3.1% by mass or less. If the content of Co is less than 0.5% by mass, the amount of cobalt oxide formed during sliding is reduced, and the seizure resistance of the copper-zinc alloy may be reduced. If the content of Co is more than 3.1% by mass, the copper-zinc alloy may be embrittled and its mechanical properties may be reduced. The content of Co may be 1.9% by mass or more and 3.1% by mass or less. If the content of Co is within this composition range, the seizure resistance of the copper-zinc alloy is improved, the specific wear amount is reduced, and the wear resistance can be improved. The content of Co may be 0.5% by mass or more and 1.1% by mass or less. Since Co is expensive, by reducing the content of Co, the seizure resistance of the copper-zinc alloy can be improved and the manufacturing cost of the copper-zinc alloy can be reduced. The content of Co may be 0.5% by mass or more and 2.0% by mass or less. When the Co content is within this range, the increase in hardness due to the addition of Co can be suppressed, so that the seizure resistance of the copper-zinc alloy can be improved, and the embrittlement of the copper-zinc alloy can be further suppressed to further improve the mechanical properties. The Co content may be 1.0 mass%. When the Co content is 1.0 mass%, the seizure resistance of the copper-zinc alloy can be improved, the manufacturing cost of the copper-zinc alloy can be reduced, and the embrittlement of the copper-zinc alloy can be further suppressed to further improve the mechanical properties.
[0028] Co can improve the seizure resistance even when the parent phase of the copper-zinc alloy is composed of any of the metal structures of α single phase, (α + β) phase, β single phase, or (β + γ) phase. The parent phase of the copper-zinc alloy may be composed of (α + β) phase, β single phase, or (β + γ) phase. When the parent phase of the copper-zinc alloy is composed of (α + β) phase, β single phase, or (β + γ) phase, Co can improve the seizure resistance more than when the parent phase is composed of α single phase. Furthermore, when the parent phase of the copper-zinc alloy is composed of β single phase, Co can improve the seizure resistance more than when the parent phase is composed of (α + β) phase or (β + γ) phase. When the parent phase of the copper-zinc alloy contains β phase in this way, the effect of seizure resistance due to the addition of Co tends to be greater.
[0029] The balance of the copper-zinc alloy is composed of Cu and unavoidable impurities. Inevitable impurities are impurities that may be mixed in even if not intentionally added.
[0030] Next, a method for producing a copper-zinc alloy according to an embodiment of the present disclosure will be described. The method for producing a copper-zinc alloy can be performed by casting, extrusion, or the like of a general copper alloy. For example, a Cu raw material, a Zn raw material, and a Co raw material are mixed in a predetermined ratio and melted in a melting furnace such as a low-frequency induction furnace. The molten copper-zinc alloy is then poured into a mold for casting. The casting of the copper-zinc alloy can be performed, for example, by a continuous casting method or the like. The copper-zinc alloy may be extruded after casting. The copper-zinc alloy does not require any particular heat treatment, but may be heat treated as necessary.
[0031] The copper-zinc alloy according to the embodiment of the present disclosure can exhibit seizure resistance when used as a sliding member that slides against a sliding member in a mechanical device having a sliding part such as a rotating machine. The copper-zinc alloy is preferably used as a sliding member that slides at a high speed such as high speed rotation (e.g., 100 m / s or more). When the sliding member slides at a low speed (e.g., 10 m / s or less), seizure of the sliding member is considered to be mainly caused by softening of the sliding member due to temperature rise during sliding. For this reason, when the sliding member slides at a low speed, the seizure resistance tends to mainly depend on the hardness of the copper-zinc alloy that forms the sliding member. On the other hand, when the sliding member slides at a high speed, the seizure resistance of the sliding member is considered to depend on the oxide formed on the surface of the sliding member due to temperature rise during sliding. For this reason, when the sliding member slides at high speed, at least in the initial stage of sliding, the softening of the sliding member has almost no effect on seizure, and there tends to be a low correlation between seizure resistance and the hardness of the copper-zinc alloy.
[0032] Such a mechanical device having a sliding part that slides at high speed is, for example, a turbocharger for a vehicle such as an automobile or a ship. The sliding member and the sliding member are incorporated in the turbocharger, the sliding member being a rotor shaft, and the sliding member can be at least one of a radial bearing and a thrust bearing. FIG. 1 is a diagram showing a configuration of a turbocharger 10. The turbocharger 10 includes a turbine impeller 12 and a compressor impeller 14. The turbine impeller 12 and the compressor impeller 14 are connected by a rotor shaft 16. The rotor shaft 16 can be made of, for example, chrome molybdenum steel such as SCM435. The turbocharger 10 includes a radial bearing 18 and a thrust bearing 20 that slide against the rotor shaft 16. The radial bearing 18 is provided on the turbine impeller 12 side and the compressor impeller 14 side. The radial bearing 18 can be made of, for example, a floating metal. A thrust collar 22 is provided on the compressor impeller 14 side of the rotor shaft 16. The thrust bearings 20 are provided on the front and rear sides of the thrust collar 22 in the rotor axial direction. The radial bearing 18 and the thrust bearing 20 may be exposed to a high-temperature environment of approximately 150°C to 350°C.
[0033] The copper-zinc alloy according to the embodiment of the present disclosure can be used for at least one of the radial bearing 18 and the thrust bearing 20. That is, the copper-zinc alloy may be used for the radial bearing 18, may be used for the thrust bearing 20, or may be used for both the radial bearing 18 and the thrust bearing 20. The rotor shaft 16 corresponds to the slidable member, and the radial bearing 18 and the thrust bearing 20 correspond to the sliding members.
[0034] In the case of a sliding member that slides at high speed, such as the radial bearing 18 and the thrust bearing 20 of the turbocharger 10, the oxide formed on the sliding surface of the sliding member can be made a relatively soft cobalt oxide, thereby improving the seizure resistance. More specifically, in the case of a binary copper-zinc alloy, an oxide of Zn is formed on the sliding surface, which reduces the seizure resistance. In the case of a copper-zinc alloy containing Al, Al is preferentially oxidized to form alumina on the sliding surface. Since alumina is a hard oxide, the alumina formed on the sliding surface during sliding is easily peeled off due to shear resistance, which makes seizure more likely to occur. In addition, in the case of a sliding member such as the rotor shaft 16 formed of chromium-molybdenum steel such as SCM435, Cr is contained in an amount of about 0.90 mass% to 1.20 mass%, so adhesive wear with the alumina formed on the sliding surface is more likely to occur.
[0035] In the case where manganese silicide, which is a hard particle, is dispersed in the matrix by adding Mn and Si to the copper-zinc alloy, Si is preferentially oxidized to form silica on the sliding surface. Since silica is a hard oxide, the silica formed on the sliding surface during sliding tends to peel off, and seizure tends to occur. In contrast, by using the copper-zinc alloy according to the embodiment of the present disclosure for at least one of the radial bearing 18 and the thrust bearing 20, cobalt oxide, which is softer than alumina, is formed on the sliding surface, and seizure resistance can be improved.
[0036] As described above, the copper-zinc alloy having the above-mentioned configuration contains 30% by mass or more and 51% by mass or less of Zn, 0.5% by mass or more and 3.1% by mass or less of Co, with the remainder being Cu and unavoidable impurities, and since a relatively soft cobalt oxide is formed on the surface of the copper-zinc alloy, the seizure resistance can be improved.
[0037] The copper-zinc alloy having the above-described configuration contains 30% by mass or more and 31% by mass or less of Zn, 0.5% by mass or more and 3.1% by mass or less of Co, with the remainder being Cu and unavoidable impurities, and the parent phase of the copper-zinc alloy is composed of a single α phase, thereby improving the seizure resistance.
[0038] The copper-zinc alloy having the above-described configuration contains 40% by mass or more and 51% by mass or less of Zn, 0.5% by mass or more and 3.1% by mass or less of Co, with the remainder being Cu and unavoidable impurities, and the parent phase of the copper-zinc alloy is composed of the (α+β) phase, single β phase or (β+γ) phase, thereby enabling the improvement of wear resistance as well as seizure resistance.
[0039] According to the copper-zinc alloy having the above-mentioned composition, the alloy contains 44% by mass or more and 47% by mass or less of Zn, 0.5% by mass or more and 3.1% by mass or less of Co, with the remainder being Cu and unavoidable impurities, and the parent phase of the copper-zinc alloy is composed of a single β phase, thereby further improving the seizure resistance.
[0040] The copper-zinc alloy having the above-described configuration contains 50% by mass or more and 51% by mass or less of Zn, 0.5% by mass or more and 3.1% by mass or less of Co, with the remainder being Cu and unavoidable impurities, and the parent phase of the copper-zinc alloy is composed of the (β+γ) phase, thereby enabling the improvement of both seizure resistance and wear resistance.
[0041] The copper-zinc alloy having the above-described composition contains 30% by mass or more and 51% by mass or less of Zn, 1.9% by mass or more and 3.1% by mass or less of Co, with the remainder being Cu and unavoidable impurities, thereby improving both the seizure resistance and the wear resistance.
[0042] According to the mechanical device having the above-described configuration, the sliding member made of the copper-zinc alloy having the above-described configuration is provided so as to slide against the slidable member, thereby improving the seizure resistance of the sliding member and making it possible to suppress seizure between the sliding member and the slidable member. EXAMPLES
[0043] The copper-zinc alloy was evaluated for seizure resistance, wear resistance, hardness, and metal structure. Table 1 shows the alloy composition of the copper-zinc alloy. Table 2 shows the evaluation results of the seizure resistance, wear resistance, hardness, and metal structure of the copper-zinc alloy.
[0044] [Table 1]
[0045] [Table 2]
[0046] First, the copper-zinc alloy will be described. The copper-zinc alloys of Examples 1 to 7 contain 30% by mass or more and 51% by mass or less of Zn, 0.5% by mass or more and 3.1% by mass or less of Co, and the remainder is composed of Cu and unavoidable impurities. The copper-zinc alloys of Examples 1 to 4 have a constant Zn content of about 45% by mass and a Co content of 0.5% by mass or more and 3.1% by mass or less. The copper-zinc alloys of Examples 5 to 7 have a constant Co content of about 1% by mass and a Zn content of 30% by mass or more and 51% by mass or less.
[0047] The copper-zinc alloy of Comparative Example 1 contained 30 mass% Zn, 3.5 mass% Al, 2 mass% Ni, 1 mass% Ti, and the balance was composed of Cu and unavoidable impurities. The copper-zinc alloy of Comparative Example 2 contained 46.8 mass% Zn, 1.95 mass% Mn, and 0.62 mass% Si, and the balance was composed of Cu and unavoidable impurities. The copper-zinc alloy of Comparative Example 3 contained 29.8 mass% Zn, and the balance was composed of Cu and unavoidable impurities. The copper-zinc alloy of Comparative Example 4 contained 44.3 mass% Zn, and the balance was composed of Cu and unavoidable impurities. The copper-zinc alloy of Comparative Example 5 contained 45.6 mass% Zn, 0.24 mass% Co, and the balance was composed of Cu and unavoidable impurities. The copper-zinc alloys of Examples 1 to 7 and Comparative Examples 1 to 5 shown in Table 1 were produced by casting.
[0048] The metal structure of each copper-zinc alloy was observed by an optical microscope. Table 2 shows the results of the metal structure observation of the parent phase of each copper-zinc alloy. The copper-zinc alloys of Comparative Examples 2, 4, and 5 were composed of a β single phase. The copper-zinc alloy of Comparative Example 3 was composed of an α single phase. The copper-zinc alloys of Examples 1 to 4 were composed of a β single phase. The copper-zinc alloy of Example 5 was composed of an α single phase. The copper-zinc alloy of Example 6 was composed of an (α+β) phase. The copper-zinc alloy of Example 7 was composed of a (β+γ) phase.
[0049] The seizure resistance of each copper-zinc alloy was evaluated. First, the method for evaluating seizure resistance will be described. A high-speed bearing friction test device was used as the test device. Figure 2 is a schematic diagram for explaining the seizure resistance test method. As shown in Figure 2, a thrust collar was placed opposite the test bearing, and a thrust load was applied. The test bearing was a hollow disk-shaped test piece. The test bearings were arranged at four locations in the circumferential direction of the holder. The bearing load was applied from the back of the test bearing by a hydraulic cylinder, and the load was increased stepwise.
[0050] A sudden increase in temperature and torque during the test was judged to be seizure, and the bearing surface pressure at the time of seizure was calculated and taken as the seizure surface pressure. The bearing surface pressure was increased by 0.03 MPa every three minutes. Engine oil (SAE10W-30) was used as the lubricant. Chrome molybdenum steel (SCM435) was used for the thrust collar material. The shaft rotation speed was approximately 25,000 rpm (outer diameter peripheral speed approximately 130 m / s). The seizure surface pressure of each copper-zinc alloy was calculated as the average of four test bearings.
[0051] Next, the results of the seizure resistance test will be described. Figure 3 is a graph showing the results of the seizure resistance test. In the graph of Figure 3, the horizontal axis represents each copper-zinc alloy, and the vertical axis represents the seizure surface pressure, and the seizure surface pressure of each copper-zinc alloy is shown in a bar graph. The higher the seizure surface pressure, the more excellent the seizure resistance. Table 2 shows the values of the seizure surface pressure of each copper-zinc alloy.
[0052] The seizure surface pressure of the copper-zinc alloys of Comparative Examples 1 to 5 was 0.5 MPa for Comparative Example 1, 1.0 MPa for Comparative Example 2, 1.5 MPa for Comparative Example 3, 1.6 MPa for Comparative Example 4, and 0.9 MPa for Comparative Example 5. In contrast, the seizure surface pressure of the copper-zinc alloys of Examples 1 to 7 was 2.8 MPa for Example 1, 3.1 MPa for Example 2, 2.6 MPa for Example 3, 2.9 MPa for Example 4, 2.3 MPa for Example 5, 2.4 MPa for Example 6, and 2.5 MPa for Example 7.
[0053] From these results, it was clear that the copper-zinc alloys of Examples 1 to 7 had better seizure resistance than the copper-zinc alloys of Comparative Examples 1 to 5. When Al or Si was contained, such as in the copper-zinc alloys of Comparative Examples 1 and 2, the seizure surface pressure was reduced and the seizure resistance was reduced. Also, even in the case of a binary copper-zinc alloy, such as in the copper-zinc alloys of Comparative Examples 3 and 4, the seizure surface pressure was reduced and the seizure resistance was reduced compared to the copper-zinc alloys of Examples 1 to 7.
[0054] Comparing the copper-zinc alloys of Examples 1 to 4 and Comparative Example 5, the copper-zinc alloy of Comparative Example 5 had a greater decrease in seizure surface pressure than the copper-zinc alloys of Examples 1 to 4. Also, the copper-zinc alloy of Comparative Example 5 had a smaller seizure surface pressure than the copper-zinc alloy of Comparative Example 4. From this, it was found that the Co content is preferably 0.5 mass% or more and 3.1 mass% or less.
[0055] Comparing the copper-zinc alloys of Examples 2, 5 to 7, the copper-zinc alloys of Examples 2, 6, and 7 had a higher seizure surface pressure than the copper-zinc alloy of Example 5. It was found that Co can improve the seizure resistance of the copper-zinc alloy when the parent phase of the copper-zinc alloy is composed of (α+β) phase, β single phase, or (β+γ) phase, more than when the parent phase is composed of α single phase. This revealed that the Zn content should be 40 mass% or more and 51 mass% or less.
[0056] Comparing the copper-zinc alloys of Examples 2, 6, and 7, the copper-zinc alloy of Example 2 had a higher seizure surface pressure than the copper-zinc alloys of Examples 6 and 7. It was found that Co can improve the seizure resistance of the copper-zinc alloy when the parent phase of the copper-zinc alloy is composed of a single β phase, more than when the parent phase is composed of an (α+β) phase or a (β+γ) phase. This revealed that the Zn content should be 44 to 47% by mass.
[0057] When comparing the copper-zinc alloys of Comparative Examples 3 and 4, the copper-zinc alloy of Comparative Example 4 had a slightly higher seizure surface pressure than the copper-zinc alloy of Comparative Example 3. On the other hand, when comparing the copper-zinc alloys of Examples 2 and 5, the copper-zinc alloy of Example 2 had a higher seizure surface pressure than the copper-zinc alloy of Example 5. More specifically, the seizure surface pressure of the copper-zinc alloy of Example 5 was about 1.5 times that of the copper-zinc alloy of Comparative Example 3. On the other hand, the seizure surface pressure of the copper-zinc alloy of Example 2 was about 1.9 times that of the copper-zinc alloy of Comparative Example 4. From this, it is considered that when the parent phase of the copper-zinc alloy contains a β phase, the effect of the addition of Co on seizure resistance is greater.
[0058] The wear resistance of each copper-zinc alloy was evaluated. The wear resistance was measured at room temperature by a pin-on-ring test using a Hayama-type wear tester, with the specific wear rate being measured. The dimensions of the test piece were 5 mm x 5 mm x 25 mm. The mating material was SCM435 material adjusted to a hardness of HRC50. The pin-on-ring test was performed without lubricant and with a surface pressure of 392 N / cm. 2 The peripheral speed was 1.0 m / sec and the travel distance was 2 km.
[0059] Next, the test results of wear resistance will be explained. Figure 4 is a graph showing the test results of wear resistance. In the graph of Figure 4, the horizontal axis indicates each copper-zinc alloy, the vertical axis indicates the specific wear rate, and the bar graph shows the specific wear rate of each copper-zinc alloy. Table 2 shows the numerical values of the specific wear rate of each copper-zinc alloy.
[0060] The specific wear rate of the copper-zinc alloys in Examples 1 to 7 is 6.00×10 -8 (mm 2 / N), and Example 2 is 6.80 × 10 -8 (mm 2 / N), and Example 3 is 6.10 × 10 -8 (mm 2 / N), and Example 4 is 4.63 × 10 -8 (mm 2 / N), and Example 5 is 8.91 × 10 -8 (mm 2 / N), and Example 6 is 5.02 × 10 -8 (mm 2 / N), and Example 7 is 3.07 × 10 -8 (mm 2 / N).
[0061] Comparing the copper-zinc alloys of Examples 1 to 7, the copper-zinc alloy of Example 5 had a larger specific wear rate than the copper-zinc alloys of the other Examples. It was found that when the parent phase of the copper-zinc alloy is composed of (α+β) phase, β single phase, or (β+γ) phase, the wear resistance can be improved more than when the parent phase is composed of α single phase. From this, it was found that the Zn content should be 40 mass% or more and 51 mass% or less in order to improve the wear resistance as well as the seizure resistance.
[0062] Comparing the copper-zinc alloys of Examples 2, 5 to 7, the copper-zinc alloy of Example 7 had a smaller specific wear rate than the copper-zinc alloys of the other Examples. It was found that when the parent phase of the copper-zinc alloy is composed of the (β+γ) phase, the wear resistance can be improved more than when the parent phase is composed of the α single phase, the (α+β) phase, or the β single phase. The reason for this is thought to be that the wear resistance is improved by the inclusion of the γ phase in the parent phase of the copper-zinc alloy. From this, it was revealed that in order to improve the wear resistance together with the seizure resistance, the Zn content should be 50 mass% or more and 51 mass% or less.
[0063] Comparing the copper-zinc alloys of Examples 1 to 4, the copper-zinc alloys of Examples 3 and 4 tended to have a smaller specific wear rate than the copper-zinc alloys of Examples 1 and 2. This shows that in order to improve both the seizure resistance and the wear resistance, it is preferable to set the Co content to 1.9 mass % or more and 3.1 mass % or less.
[0064] The hardness of each copper-zinc alloy was evaluated. The hardness of each copper-zinc alloy was measured at room temperature as the Brinell hardness HBW (10 / 500). A 10 mm diameter cemented carbide indenter was used. The test load was 500 kgf. Next, the hardness test results will be explained. FIG. 5 is a graph showing the hardness test results. In the graph of FIG. 5, the horizontal axis shows each copper-zinc alloy, the vertical axis shows the Brinell hardness HBW (10 / 500), and the Brinell hardness of each copper-zinc alloy is shown in a bar graph. Table 2 shows the Brinell hardness values of each copper-zinc alloy.
[0065] The Brinell hardness of the copper-zinc alloy of Comparative Example 4 was 100. In contrast, the Brinell hardness of the copper-zinc alloys of Examples 1 to 4 was 90 in Example 1, 100 in Example 2, 102 in Example 3, and 122 in Example 4. Since the Brinell hardness of the copper-zinc alloy of Example 4 was higher than that of the copper-zinc alloys of Comparative Example 4 and Examples 1 to 3, it was found that when the Co content is greater than 3.1 mass%, the copper-zinc alloy may become embrittled and the mechanical properties may deteriorate. In addition, since the Brinell hardness of the copper-zinc alloys of Examples 1 to 3 is approximately the same as that of the copper-zinc alloy of Comparative Example 4, it was found that when the Co content is 0.5 mass% or more and 2.0 mass% or less, the increase in hardness due to the addition of Co can be suppressed, and therefore the embrittlement of the copper-zinc alloy can be further suppressed to further improve the mechanical properties. [Explanation of symbols]
[0066] 10. Turbocharger 12 Turbine impeller 14 Compressor impeller 16 Rotor shaft 18 Radial bearings 20 Thrust bearing 22 Thrust collar
Claims
1. A copper-zinc alloy for bearings, comprising 44% by mass or more and 47% by mass or less of Zn, 0.5% by mass or more and 3.1% by mass or less of Co, the remainder being Cu and unavoidable impurities, and the parent phase being composed of a single β phase.
2. The copper-zinc alloy for bearings according to claim 1, A copper-zinc alloy for bearings, characterized in that the Co content is 1.9 mass % or more and 3.1 mass % or less.
3. A bearing made of the copper-zinc alloy for bearings according to any one of claims 1 to 2; a rotor shaft that slides on the bearing, The mechanical device, wherein the bearing is a radial bearing or a thrust bearing.
Citation Information
Patent Citations
Metal wire, manufacturing method thereof and tire
CN107824630A
Electrode wire for electric discharge machining
JP1984050141A
Sliding material with flame sprayed film
JP1995048665A
turbocharger for internal combustion engines
JP3718147B2
Powder-metallurgy of cobalt containing brass alloys
US4139378A