Emulsion composition containing hydrophobically modified cellulose fibers

The emulsion composition of hydrophobically modified cellulose fibers and an organic compound at 25°C forms a durable and water-resistant membrane, addressing the need for improved durability and water resistance in existing membranes.

JP7583547B2Active Publication Date: 2024-11-14KAO CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020130111
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-13
Filing Date
2020-07-31
Publication Date
2024-11-14
Estimated Expiration
2040-07-31

AI Technical Summary

Technical Problem

Existing membranes containing hydrophobically modified cellulose fibers and oil require improved durability and water resistance.

Method used

An emulsion composition comprising hydrophobically modified cellulose fibers, water, and an organic compound that is liquid at 25°C and 1 atm, which forms a network upon drying, resulting in a durable and water-resistant membrane.

Benefits of technology

The composition produces a membrane with excellent water resistance and durability, suitable for applications requiring synovial properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583547000010
    Figure 0007583547000010
  • Figure 0007583547000011
    Figure 0007583547000011
  • Figure 0007583547000012
    Figure 0007583547000012
Patent Text Reader

Abstract

To provide an aqueous emulsion composition for producing a film having synovial property and high waterproofness or durability.SOLUTION: There is provided an emulsion composition containing the following components (A)-(C): (A) one or more kinds of hydrophobic modified cellulose fiber selected from a group consisting of components (a) and (b), (a) a hydrophobic modified cellulose fiber formed by binding of a silicone compound to a cellulose fiber, and (b) a hydrophobic modified cellulose fiber formed by binding of a hydrocarbon based compound having a total carbon number of 16-40 with a cationic group to an anionic group of an anion modified cellulose fiber; (B) water; and (C) an organic compound which is liquid at 25°C and at 1 atmosphere.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an emulsion composition containing hydrophobically modified cellulose fibers. [Background technology]

[0002] Conventionally, in the field of packaging containers for cosmetics, food, etc., surface films have been developed to prevent adhesion of fluids such as dirt and objects that may come into contact with containers, trays, etc. (e.g., objects filled in the container or packaged with a film, such as cosmetics or food themselves) etc. Recently, films containing hydrophobically modified cellulose fibers and oil have become known. For example, Patent Document 1 discloses a membrane having hydrophobically modified cellulose fibers in which one or more modifying groups selected from anionic groups and hydroxyl groups of cellulose fibers are bonded, and an oil having an SP value of 10 or less. On the other hand, as an emulsion composition, Patent Document 2 describes that a viscous aqueous composition having excellent shape retention, dispersion stability, and salt resistance as well as excellent emulsion stability can be produced by binding a monoamine having an organic value of 300 or less as a salt to anion-modified cellulose fine fibers. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] WO2018 / 164135 [Patent Document 2] JP 2012-126786 A Summary of the Invention [Problem to be solved by the invention]

[0004] The film having hydrophobically modified cellulose fibers and oil described in Patent Document 1 is prepared by dispersing hydrophobically modified cellulose fibers in a solvent and evaporating the solvent from a state in which the oil is dissolved. Such a film shows a certain degree of synovial properties, but further durability is required.

[0005] Moreover, the object of Patent Document 2 is to obtain a viscous water-based composition having excellent emulsion stability, and is not to form a film.

[0006] Accordingly, an object of the present invention is to provide an aqueous emulsion composition and a film for producing a film having excellent water resistance or durability and synovial properties. [Means for solving the problem]

[0007] The present invention relates to the following [1] to [8]. [1] An emulsion composition containing the following components (A) to (C): (A) One or more hydrophobically modified cellulose fibers selected from the group consisting of the following components (a) and (b): (a) Hydrophobically modified cellulose fibers formed by bonding silicone compounds to cellulose fibers (b) Hydrophobically modified cellulose fibers in which a hydrocarbon compound having a total carbon number of 16 to 40 and a cationic group is bonded to the anionic group of an anionically modified cellulose fiber via an ionic bond. (B) Water (C) An organic compound that is liquid at 25°C and 1 atmosphere [2] The emulsion composition according to [1] above, further comprising a component (D) a polyether-modified silicone compound. [3] Component (A-1) anionically modified cellulose fiber, Component (A-2) one or more compounds selected from the group consisting of amino-modified silicones and hydrocarbon-based compounds having cationic groups and a total carbon number of 16 to 40, Component (B) water, and Component (C) An organic compound that is liquid at 25°C and 1 atm A method for producing the emulsion composition according to [1] or [2] above, comprising the step of mixing the above. [4] A method for producing a membrane containing hydrophobically modified cellulose fibers, comprising a step of drying the emulsion composition according to [1] or [2] above. [5] A dry film obtained by drying the emulsion composition according to [1] or [2] above. [6] A coating film obtained by applying the emulsion composition according to [1] or [2] above and then drying it. [7] A biofouling inhibitor, antifouling agent, or anti-snow agent, comprising the emulsion composition according to [1] or [2] above. [8] (A) one or more hydrophobically modified cellulose fibers selected from the group consisting of the following components (a) and (b): (a) Hydrophobically modified cellulose fibers formed by bonding silicone compounds to cellulose fibers (b) a hydrophobically modified cellulose fiber in which a hydrocarbon compound having a total carbon number of 16 to 40 and a cationic group is bonded to an anionic group of the anionically modified cellulose fiber via an ionic bond; and (C) An organic compound that is liquid at 25°C and 1 atmosphere A film having a particulate structure. Effect of the Invention

[0008] By using the aqueous emulsion composition provided by the present invention, a film having excellent water resistance or a film having excellent synovial properties and durability can be produced. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a Cryo-SEM micrograph (25,000x) of the emulsion composition produced in Example 1. [Diagram 2] FIG. 2 is a graph showing the particle size distribution of the emulsion droplets of the emulsion composition produced in Example 1. [Diagram 3] FIG. 3 is a SEM micrograph (8000x) of the dry film of the emulsion composition produced in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] As a result of intensive research by the inventors to solve the above problems, they unexpectedly discovered that by applying an emulsion composition containing hydrophobically modified cellulose fibers, in which a silicone compound or a specific hydrocarbon compound is bonded to cellulose fibers, and water and an organic compound that is liquid at 25°C and 1 atmosphere, onto a substrate and drying it, it is possible to produce a film that is highly water-resistant or durable and exhibits synovial properties, and thus completed the present invention. Although the mechanism by which this effect is exerted is unclear, it is speculated that in the emulsion composition, the hydrophobically modified cellulose fibers form a network in the liquid organic compound at 25°C and 1 atmosphere, and that the network crosslinks and forms a membrane as it dries.

[0011] 1. Emulsified composition The emulsion composition of the present invention contains the following components (A) to (C). <Component (A)> Component (A) is one or more types of hydrophobically modified cellulose fibers selected from the group consisting of (a) and (b) below. (a) Hydrophobically modified cellulose fibers formed by bonding silicone compounds to cellulose fibers (b) Hydrophobically modified cellulose fibers in which a hydrocarbon compound having a total carbon number of 16 to 40 and a cationic group is ionically bonded to the anionic group of the anionically modified cellulose fiber.

[0012] In this specification, hydrophobically modified cellulose fibers are cellulose fibers to which a silicone compound is bonded, or anionically modified cellulose fibers to which a hydrocarbon compound having a total carbon number of 16 to 40 and containing cationic groups is bonded via ionic bonds to the anionic groups of the anionically modified cellulose fibers.

[0013] [Cellulose type I crystal structure and crystallinity] The hydrophobically modified cellulose fiber preferably has a cellulose type I crystal structure due to the use of natural cellulose as a raw material. The crystallinity of the hydrophobically modified cellulose fiber is preferably 10% or more, more preferably 15% or more, and even more preferably 20% or more from the viewpoint of strength development during film formation. Also, from the viewpoint of raw material availability, it is preferably 90% or less, more preferably 85% or less, even more preferably 80% or less, and even more preferably 75% or less. The cellulose type I crystallinity is measured by the method described in the Examples below.

[0014] [Average fiber diameter of hydrophobically modified cellulose fibers] The average fiber diameter of the hydrophobically modified cellulose fiber is preferably 0.1 nm or more, more preferably 1.0 nm or more, and even more preferably 2.0 nm or more from the viewpoint of handling, and is preferably 200 nm or less, more preferably 100 nm or less, and even more preferably 50 nm or less from the viewpoint of strength when formed into a membrane. The average fiber diameter of the hydrophobically modified cellulose fiber is measured by the method described in the Examples below.

[0015] [Modifying group] A preferred embodiment of the hydrophobically modified cellulose fibers of component (a), that is, the hydrophobically modified cellulose fibers formed by bonding a silicone compound to cellulose fibers, has a structure represented by the following general formula (T-Ce).

[0016] [ka]

[0017] (Wherein, X is -CHOH, -CHO-R 1 , -C(=O)OH, -C(=O)OR 1 , -C(=O)-O - H3N + -R 1 and -C(=O)-NH-R 1 is one or more groups selected from the group consisting of 1 is a modifying group, each R is independently a hydrogen atom or a modifying group, R1 and R may be the same or different, and multiple R 1 and at least one of R is a modifying group; and m is an integer of 20 or more and 3,000 or less.

[0018] The modifying group in the hydrophobically modified cellulose fiber in which a silicone compound is bonded to the cellulose fiber is a group derived from the silicone compound, and the modifying group (i.e., R 1 The structure of R) depends on the structure of the silicone compound used. The bonding mode of the modifying group to the cellulose fiber is preferably a covalent bond or an ionic bond. From the viewpoint of ease of production, an ionic bond is preferred, and from the viewpoint of the stability of the film formed, a covalent bond is preferred. Compounds for introducing a modifying group, such as silicone compounds and hydrocarbon compounds having a total carbon number of 16 to 40 and having cationic groups, may be referred to as "modifying compounds" in this specification.

[0019] The bonding sites of the modifying groups in the cellulose fibers include hydroxyl groups and aldehyde groups of the cellulose fibers, and functional groups introduced by chemically modifying the cellulose fibers. The functional groups introduced by chemical modification are preferably anionic groups, more preferably carboxyl groups. As the cellulose fibers, anion-modified cellulose fibers are preferred, and carboxyl group-containing cellulose fibers are more preferred, from the viewpoints of ease of preparation and mild reaction conditions.

[0020] When the bonding site is a hydroxy group of the cellulose fiber, the bonding type is a covalent bond, and examples of the bonding include an ether bond, an ester bond, and a carbonate bond.

[0021] When the bonding site is an anionic group of an anion-modified cellulose fiber, the bonding mode is an ionic bond or a covalent bond. When the bonding mode is an ionic bond, the modifying compound having a cationic group is bonded via electrostatic interaction, and when the bonding mode is a covalent bond, the modifying compound is bonded via an ester bond, an amide bond, or the like, and particularly when the modifying compound is bonded to a carboxy group of a carboxy group-containing cellulose fiber, the modifying compound is bonded via an ester bond, an amide bond, a carbonate bond, a urethane bond, or the like.

[0022] For example, the modifying compound is an amino-modified silicone (hereinafter, "H2N-[alkyl silicone backbone]"), and the cellulose fiber is a carboxyl group-containing cellulose fiber (hereinafter, "[cellulose backbone]-C * (=O)-OH". If the bonding mode is ionic bonding, the hydrophobically modified cellulose fiber is "[cellulose skeleton]-C * (=O)-O - H3N + On the other hand, if the bond type is an amide bond, the hydrophobically modified cellulose fiber will have a structure like "Cellulose backbone -C". * The structure of the modifying group will be "(=O)-NH- [alkyl silicone skeleton]" and the modifying group will be "- [alkyl silicone skeleton]". In this way, the structure of the modifying group will depend on the structure of the modifying compound used. * " refers to the carbon atom at the 6th position of the cellulose structural unit.

[0023] Furthermore, the modifying groups of the hydrophobically modified cellulose fibers of component (b), i.e., the hydrophobically modified cellulose fibers in which a hydrocarbon compound having a cationic group and a total carbon number of 16 to 40 is bonded via ionic bonds to the anionic groups of the anionically modified cellulose fibers, are derived from a hydrocarbon compound having a cationic group and a total carbon number of 16 to 40. In this case, the bonding mode of the modifying group to the anionic groups of the anionically modified cellulose fibers is ionic bonding, and the hydrophobically modified cellulose fibers of component (b) are in a state in which the cationic groups of the modifying groups are adsorbed to the anionic groups on the surface of the cellulose fibers via electrostatic interaction. Hereinafter, the term "modifying group" refers to both groups derived from silicone compounds and groups derived from hydrocarbon compounds having a total of 16 to 40 carbon atoms and containing cationic groups.

[0024] The bond amount (mmol / g) and introduction rate (mol%) of the modifying group in the hydrophobically modified cellulose fiber refer to the amount and ratio of the modifying group introduced into the hydrophobically modified cellulose fiber. Specifically, they are measured by the method described in the Examples below. The bond amount and introduction rate of the modifying group can be adjusted by the amount and type of the modifying compound added, the reaction temperature, the reaction time, the solvent, etc.

[0025] The amount of modifying groups bonded to the hydrophobically modified cellulose fiber is preferably 0.1 mmol / g or more, more preferably 0.2 mmol / g or more, and even more preferably 0.5 mmol / g or more from the viewpoint of obtaining a film with improved water resistance and synovial fluid properties, and is preferably 3 mmol / g or less, more preferably 2.5 mmol / g or less, and even more preferably 2 mmol / g or less from the viewpoint of reactivity.

[0026] In addition, the introduction rate of the modifying group in the hydrophobically modified cellulose fiber is preferably 10 mol% or more, more preferably 20 mol% or more, even more preferably 40 mol% or more, and even more preferably 50 mol% or more, from the viewpoint of obtaining a membrane with improved water resistance and synovial fluid properties, and is preferably 99 mol% or less, more preferably 97 mol% or less, even more preferably 95 mol% or less, and even more preferably 90 mol% or less, from the viewpoint of reactivity.

[0027] [Method for producing hydrophobically modified cellulose fibers] The hydrophobically modified cellulose fibers of component (A) can be produced, for example, by a process comprising the steps of: (1) introducing anionic groups into raw cellulose fibers to obtain anionically modified cellulose fibers; and (2) bonding a silicone compound and / or a hydrocarbon compound having a total carbon number of 16 to 40 and having cationic groups to the anionically modified cellulose fibers to obtain hydrophobically modified cellulose fibers.

[0028] As an embodiment of the step (2), Component (A-1) anion-modified cellulose fiber, Component (A-2) One or more compounds selected from the group consisting of amino-modified silicones and hydrocarbon-based compounds having cationic groups and a total carbon number of 16 to 40. Component (B) water, and Component (C) An organic compound that is liquid at 25°C and 1 atm Such an embodiment is the same as the step in the production method of the emulsion composition of the present invention described below, i.e., the step of mixing component (A-1), component (A-2), component (B) and component (C). According to such an embodiment, the hydrophobically modified cellulose fiber and the emulsion composition of the present invention can be produced in the same step, and therefore, this can be said to be a more preferable production method.

[0029] (1) A process for obtaining anionically modified cellulose fibers The anionically modified cellulose fiber used in the present invention can be obtained by subjecting raw cellulose fiber to an oxidation treatment or an anionic group addition treatment to introduce at least one anionic group and thereby anionically modifying the fiber.

[0030] The cellulose fibers to be anionically modified, i.e., the cellulose fibers that are the raw material for hydrophobically modified cellulose fibers and anionically modified cellulose fibers, are preferably natural cellulose fibers from an environmental perspective, and examples of such fibers include wood pulps such as coniferous pulp and broadleaf pulp; cotton pulps such as cotton linters and cotton lint; non-wood pulps such as straw pulp and bagasse pulp; and bacterial cellulose, and these may be used alone or in combination of two or more.

[0031] The average fiber diameter of the raw cellulose fibers is not particularly limited, but from the viewpoints of handling and cost, it is preferably 1 μm or more, and on the other hand, preferably 300 μm or less.

[0032] The average fiber length of the raw cellulose fibers is not particularly limited, but is preferably 100 μm or more and 5,000 μm or less from the viewpoints of availability and cost. The average fiber diameter and average fiber length of the raw cellulose fibers can be measured according to the method described in the Examples below. From the viewpoint of dispersibility, it is preferable to use cellulose fibers having an average fiber length of 1 μm or more and 1,000 μm or less, which are obtained by subjecting the raw cellulose fibers to a short fiber treatment such as alkaline hydrolysis or acid hydrolysis.

[0033] The anionic group to be introduced includes a carboxy group, a sulfonic acid group, or a phosphoric acid group.

[0034] (i) Introducing carboxyl groups as anionic groups into cellulose fibers Methods for introducing carboxyl groups into cellulose fibers include, for example, a method of converting hydroxyl groups of cellulose into carboxyl groups by oxidation, and a method of reacting the hydroxyl groups of cellulose with at least one selected from the group consisting of compounds having a carboxyl group, acid anhydrides of compounds having a carboxyl group, and derivatives thereof.

[0035] The method for oxidizing the hydroxyl groups of the cellulose is not particularly limited, but for example, a method of oxidizing the cellulose by reacting an oxidizing agent such as sodium hypochlorite and a bromide such as sodium bromide with 2,2,6,6-tetramethyl-1-piperidine-N-oxyl (TEMPO) as a catalyst can be applied. For more details, a known method, for example, the method described in JP 2011-140632 A can be referred to.

[0036] By subjecting cellulose fibers to oxidation treatment using TEMPO as a catalyst, the hydroxymethyl group (-CHOH) at the C6 position of the cellulose structural unit is selectively converted to a carboxy group. This method is particularly advantageous in that it has excellent selectivity for the hydroxy group at the C6 position, which is the target of oxidation on the surface of the raw cellulose fiber, and the reaction conditions are mild. Therefore, a preferred embodiment of the anion-modified cellulose fiber in the present invention is a cellulose fiber in which the C6 position of the cellulose structural unit is a carboxy group. In this specification, such a cellulose fiber may be referred to as an "oxidized cellulose fiber". Oxidized cellulose fibers are preferred because they are easier to prepare than other anion-modified cellulose fibers. Therefore, one preferred embodiment of the hydrophobically modified cellulose fiber in the present invention is a hydrophobically modified cellulose fiber in which an amino-modified silicone is bonded to a carboxy group-containing cellulose fiber.

[0037] By further subjecting the oxidized cellulose fibers to a further oxidation treatment or reduction treatment, it is possible to prepare oxidized cellulose fibers from which the remaining aldehyde groups have been removed.

[0038] (ii) In the case of introducing sulfonic acid groups or phosphoric acid groups as anionic groups into cellulose fibers As a method for introducing sulfonic acid groups as anionic groups into cellulose fibers, a method of adding sulfuric acid to cellulose fibers and heating the fibers can be given. Methods for introducing phosphate groups as anionic groups into cellulose fibers include a method of mixing a powder or an aqueous solution of phosphoric acid or a phosphoric acid derivative with dry or wet cellulose fibers, a method of adding an aqueous solution of phosphoric acid or a phosphoric acid derivative to a dispersion of cellulose fibers, etc. When these methods are adopted, in general, after mixing or adding a powder or an aqueous solution of phosphoric acid or a phosphoric acid derivative, a dehydration treatment, a heat treatment, etc. are carried out.

[0039] (iii) Anionically modified cellulose fiber (component (A-1)) Examples of the anionic group contained in the anion-modified cellulose fiber thus obtained include a carboxy group, a sulfonic acid group, and a phosphate group. From the viewpoint of the efficiency of introducing the modifying group into the cellulose fiber, the anionic group is preferably a carboxy group. Examples of the ion (counter ion) that is paired with the anionic group in the anion-modified cellulose fiber include metal ions such as sodium ions, potassium ions, calcium ions, and aluminum ions that are generated in the presence of an alkali during production, and protons that are generated by replacing these metal ions with an acid.

[0040] The anionic group content in the anion-modified cellulose fiber is preferably 0.1 mmol / g or more, more preferably 0.4 mmol / g or more, even more preferably 0.6 mmol / g or more, and even more preferably 0.8 mmol / g or more, from the viewpoint of introducing a modifying group. Also, from the viewpoint of improving the handleability, it is preferably 3 mmol / g or less, more preferably 2 mmol / g or less, and even more preferably 1.8 mmol / g or less. The "anionic group content" means the total amount of anionic groups in the cellulose constituting the cellulose fiber, and is specifically measured by the method described in the Examples below.

[0041] The average fiber diameter of the anionically modified cellulose fiber is preferably 0.1 nm or more, more preferably 1.0 nm or more, and even more preferably 2.0 nm or more from the viewpoint of handling, and is preferably 200 nm or less, more preferably 100 nm or less, and even more preferably 50 nm or less from the viewpoint of strength when formed into a film. The average fiber diameter of the anionically modified cellulose fiber is measured by the method described later in the Examples.

[0042] (2) A process for obtaining hydrophobically modified cellulose fibers The hydrophobically modified cellulose fiber of component (A) can be produced by bonding the anion-modified cellulose fiber described above with one or more compounds selected from the group consisting of amino-modified silicones and hydrocarbon-based compounds having cationic groups and a total carbon number of 16 to 40. As such a production method, a known method, for example, the method described in JP 2015-143336 A, can be used.

[0043] (i) Silicone compounds The silicone compound used as the modifying compound in the present invention may be a commercially available product or may be prepared according to a known method. Only one type of silicone compound may be used, or two or more types may be used.

[0044] Examples of silicone compounds used as modifying compounds in the present invention include amino-modified silicones, epoxy-modified silicones, carboxy-modified silicones, carbinol-modified silicones, hydrogen-modified silicones, etc., and the position of the reactive group may be a side chain or a terminal of the silicone compound. Among these, amino-modified silicones are preferred from the viewpoint of ease of modification.

[0045] (ii) Amino-modified silicone Amino-modified silicone is a silicone compound that has an amino group. The amino-modified silicone has a kinetic viscosity of 10 mm at 25°C. 2 / s or more 20,000mm 2Further, amino-modified silicones having an amino equivalent of 400 g / mol or more and 16,000 g / mol or less are preferred.

[0046] The kinetic viscosity at 25°C can be determined using an Ostwald viscometer. From the viewpoint of synovial properties, it is more preferable to use a viscosity of 20 mm. 2 / s or more, more preferably 50 mm 2 / s or more, and from the viewpoint of handling, 10,000 mm is preferable. 2 / s or less, and more preferably 5,000 mm 2 / s or less.

[0047] In addition, the amino equivalent is preferably 400 g / mol or more, more preferably 600 g / mol or more, and even more preferably 800 g / mol or more from the viewpoint of synovial fluid properties, and is preferably 16,000 g / mol or less, more preferably 14,000 g / mol or less, and even more preferably 12,000 g / mol or less from the viewpoint of ease of binding to anion-modified cellulose fibers. The amino equivalent is the molecular weight per nitrogen atom, and is calculated by amino equivalent (g / mol) = mass average molecular weight / number of nitrogen atoms per molecule. Here, the mass average molecular weight is a value obtained by gel permeation chromatography using polystyrene as a standard substance, and the number of nitrogen atoms can be obtained by elemental analysis.

[0048] A specific example of the amino-modified silicone is a compound represented by the general formula (a1).

[0049] [ka]

[0050] [In the formula, R 1a R represents a group selected from an alkyl group having 1 to 3 carbon atoms, a hydroxy group, an alkoxy group having 1 to 3 carbon atoms, or a hydrogen atom, and is preferably a methyl group or a hydroxy group from the viewpoint of synovial properties. 2ais a group selected from an alkyl group having 1 to 3 carbon atoms, a hydroxyl group, or a hydrogen atom, and from the same viewpoint, is preferably a methyl group or a hydroxyl group. B represents a side chain having at least one amino group, R 3a represents an alkyl group having 1 to 3 carbon atoms or a hydrogen atom. x and y each represent an average degree of polymerization, and are selected so that the kinematic viscosity at 25°C and amino equivalent of the compound fall within the above-mentioned ranges. 1a , R 2a , R 3a may be the same or different, and multiple R 2a may be the same or different.

[0051] In the compound of general formula (a1), from the viewpoint of synovial properties, x is preferably a number of 10 or more and 10,000 or less, more preferably a number of 20 or more and 5,000 or less, and even more preferably a number of 30 or more and 3,000 or less. y is preferably a number of 1 or more and 1,000 or less, more preferably a number of 1 or more and 500 or less, and even more preferably a number of 1 or more and 200 or less. The mass average molecular weight of the compound of general formula (a1) is preferably 2,000 or more and 1,000,000 or less, more preferably 5,000 or more and 100,000 or less, and even more preferably 8,000 or more and 50,000 or less.

[0052] In the general formula (a1), examples of the side chain B having an amino group include the following. -C3H6-NH2 -C3H6-NH-C2H4-NH2 -C3H6-NH-[C2H4-NH] e -C2H4-NH2 -C3H6-NH(CH3) -C3H6-NH-C2H4-NH(CH3) -C3H6-NH-[C2H4-NH] f -C2H4-NH(CH3) -C3H6-N(CH3)2 -C3H6-N(CH3)-C2H4-N(CH3)2 -C3H6-N(CH3)-[C2H4-N(CH3)] g -C2H4-N(CH3)2 -C3H6-NH-cyclo-C5H 11 (where e, f, and g are numbers from 1 to 30.)

[0053] The amino-modified silicone used in the present invention can be produced, for example, by hydrolyzing an organoalkoxysilane represented by general formula (a2) with an excess of water, heating the resulting hydrolysate with dimethylcyclopolysiloxane in the presence of a basic catalyst such as sodium hydroxide at 80 to 110°C to cause an equilibrium reaction, and then neutralizing the basic catalyst with an acid when the reaction mixture reaches the desired viscosity (see JP-A-53-98499). H2N(CH2)2NH(CH2)3Si(CH3)(OCH3)2(a2)

[0054] In addition, from the viewpoint of obtaining a film having high water resistance, the amino-modified silicone is preferably at least one selected from the group consisting of monoamino-modified silicones having one amino group in one side chain B and diamino-modified silicones having two amino groups in one side chain B, and more preferably at least one selected from the group consisting of compounds in which the side chain B having an amino group is represented by -C3H6-NH2 [hereinafter referred to as component (a1-1)] and compounds in which the side chain B having an amino group is represented by -C3H6-NH-C2H4-NH2 [hereinafter referred to as component (a1-2)].

[0055] Examples of the amino-modified silicones in the present invention that are useful from the viewpoint of performance include TSF4703 (kinetic viscosity: 1000, amino equivalent: 1600) and TSF4708 (kinetic viscosity: 1000, amino equivalent: 2800) manufactured by Momentive Performance Materials, Inc., and SS-3551 (kinetic viscosity: 1000, amino equivalent: 1700), SF8457C (kinetic viscosity: 1200, amino equivalent: 1800), SF8417 (kinetic viscosity: 1200, amino equivalent: 1700), SF8452C (kinetic viscosity: 600, amino equivalent: 6400), BY16-209 (kinetic viscosity: 500, amino equivalent: 1800), and BY16-892 (kinetic viscosity: 1500, amino equivalent: 2000), BY16-898 (kinematic viscosity: 2000, amino equivalent: 2900), FZ-3760 (kinematic viscosity: 220, amino equivalent: 1600), BY16-213 (kinematic viscosity: 55, amino equivalent: 2700), KF-8002 (kinematic viscosity: 1100, amino equivalent: 1700) manufactured by Shin-Etsu Chemical Co., Ltd. Preferred are KF-8004 (kinematic viscosity: 800, amino equivalent: 1500), KF-8005 (kinematic viscosity: 1200, amino equivalent: 11000), KF-867 (kinematic viscosity: 1300, amino equivalent: 1700), KF-864 (kinematic viscosity: 1700, amino equivalent: 3800), and KF-859 (kinematic viscosity: 60, amino equivalent: 6000). In parentheses, kinematic viscosity is the value measured at 25°C (unit: mm 2 / s) and the unit of amino equivalent is g / mol.

[0056] As the (a1-1) component, BY16-213 (kinetic viscosity: 55, amino equivalent: 2700) and BY16-853U (kinetic viscosity: 14, amino equivalent: 450) are more preferable.

[0057] As the (a1-2) component, SF8417 (kinetic viscosity: 1200, amino equivalent: 1700), BY16-209 (kinetic viscosity: 500, amino equivalent: 1800), FZ-3760 (kinetic viscosity: 220, amino equivalent: 1600), SF8452C (kinetic viscosity: 600, amino equivalent: 6400), KF-8002 (kinetic viscosity: 1100, amino equivalent: 1700), and SS-3551 (kinetic viscosity: 1000, amino equivalent: 1700) are more preferable.

[0058] The silicone compound may have a substituent. Examples of the substituent include alkoxy groups having 1 to 6 carbon atoms, such as a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, a butoxy group, an isobutoxy group, a sec-butoxy group, a tert-butoxy group, a pentyloxy group, an isopentyloxy group, and a hexyloxy group; a methoxycarbonyl group, an ethoxycarbonyl group, a propoxycarbonyl group, an isopropoxycarbonyl group, a butoxycarbonyl group, an isobutoxycarbonyl group, a sec-butoxycarbonyl group, and the like. Examples of the alkoxy group include alkoxy-carbonyl groups having 1 to 6 carbon atoms, such as a carboxyl group, a tert-butoxycarbonyl group, a pentyloxycarbonyl group, or an isopentyloxycarbonyl group; halogen atoms such as a fluorine atom, a chlorine atom, a bromine atom, or an iodine atom; acyl groups having 1 to 6 carbon atoms, such as an acetyl group or a propionyl group; aralkyl groups; aralkyloxy groups; alkylamino groups having 1 to 6 carbon atoms; and dialkylamino groups having an alkyl group with 1 to 6 carbon atoms.

[0059] (iii) Hydrocarbon compounds having a total of 16 or more carbon atoms and containing cationic groups In the present invention, the hydrocarbon-based compound having a total carbon number of 16 or more and having a cationic group is one in which one or more hydrocarbon groups are bonded to one cationic group. The total carbon number of the hydrocarbon-based compound having a cationic group is 16 or more, more preferably 18 or more, from the viewpoint of obtaining a membrane having high water resistance, and is preferably 40 or less, more preferably 30 or less, and even more preferably 26 or less, from the viewpoint of handling.

[0060] A hydrocarbon compound having a cationic group is a compound in which the hydrocarbon group is directly bonded to a nitrogen atom or a phosphorus atom via a covalent bond when the cationic group is a primary amine, secondary amine, tertiary amine, quaternary ammonium, phosphonium, etc. A compound in which the cationic group is bonded to at least one of the nitrogen atom or the carbon atom of the functional group via a covalent bond when the cationic group is an amidine, guanidine, etc. A compound in which at least one hydrocarbon group is bonded to any position of the ring structure via a covalent bond when the cationic group is an imidazolium, pyridinium, imidazoline, etc. The hydrocarbon compound having a cationic group is more preferably one that does not contain an oxyalkylene group.

[0061] (hydrocarbon group) Examples of the hydrocarbon group in the hydrocarbon compound include a chain saturated hydrocarbon group, a chain unsaturated hydrocarbon group, a cyclic saturated hydrocarbon group, and an aromatic hydrocarbon group. From the viewpoint of availability, the number of carbon atoms in the hydrocarbon group is preferably 1 or more, more preferably 2 or more, and even more preferably 3 or more, and from the same viewpoint, it is preferably 40 or less, more preferably 30 or less, and even more preferably 24 or less. The number of carbon atoms in the hydrocarbon group means the number of carbon atoms in one hydrocarbon group, unless otherwise specified.

[0062] Specific examples of chain saturated hydrocarbon groups include methyl, ethyl, propyl, isopropyl, butyl, sec-butyl, tert-butyl, isobutyl, pentyl, tert-pentyl, isopentyl, hexyl, isohexyl, heptyl, octyl, 2-ethylhexyl, nonyl, decyl, dodecyl, tridecyl, tetradecyl, octadecyl, docosyl, and octacosanyl groups.

[0063] Specific examples of the chain unsaturated hydrocarbon group include, for example, ethenyl, propenyl, butenyl, isobutenyl, isoprenyl, pentenyl, hexenyl, heptenyl, octenyl, nonenyl, decenyl, dodecenyl, tridecenyl, tetradecenyl, and octadecenyl groups.

[0064] Specific examples of cyclic saturated hydrocarbon groups include cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, cyclononyl, cyclodecyl, cyclododecyl, cyclotridecyl, cyclotetradecyl, and cyclooctadecyl groups.

[0065] The aromatic hydrocarbon group is, for example, selected from the group consisting of an aryl group and an aralkyl group. In the aryl group and the aralkyl group, the aromatic ring itself may be substituted or unsubstituted.

[0066] Examples of the aryl group include a phenyl group, a naphthyl group, an anthryl group, a phenanthryl group, a biphenyl group, a triphenyl group, a terphenyl group, and groups in which these groups are substituted with the substituents described below.

[0067] Examples of the aralkyl group include a benzyl group, a phenethyl group, a phenylpropyl group, a phenylpentyl group, a phenylhexyl group, a phenylheptyl group, a phenyloctyl group, and groups in which the aromatic group of these groups is further substituted with a substituent.

[0068] The above-mentioned hydrocarbon compounds may further have some hydrogen atoms substituted with, for example, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, a hydroxyl group, a methoxy group, an ethoxy group, a carboxyl group, an aldehyde group, a ketone group, a thiol group, etc.

[0069] The hydrocarbon compound having a cationic group is preferably a hydrocarbon compound having an amino group such as a primary amine, a secondary amine, a tertiary amine, or a quaternary ammonium (referred to as "hydrocarbon amine" in this specification). Specific examples of such hydrocarbon amines are preferably hexadecylamine, stearylamine, oleylamine, dioctylamine, didecylamine, didodecylamine, trihexylamine, trioctylamine, tetrabutylammonium salt, tetrahexylammonium salt, dimethyldioctylammonium salt, dimethyldidecylammonium salt, trimethylhexadecylammonium salt, and the like.

[0070] (3) Microfabrication process By micronizing the cellulose at any stage of the method for producing hydrophobically modified cellulose fibers, it is possible to micronize the cellulose from the micrometer scale to the nanometer scale. By reducing the average fiber diameter to the nanometer size, the strength during film formation is improved, so it is preferable to further carry out a micronization treatment step.

[0071] A known dispersing machine is preferably used as the device used in the micronization treatment. For example, a disintegrator, a beater, a low-pressure homogenizer, a high-pressure homogenizer, a grinder, a cutter mill, a ball mill, a jet mill, a single-screw extruder, a twin-screw extruder, an ultrasonic agitator, a household juicer mixer, etc. can be used. In addition, the solid content of the reaction product fiber in the micronization treatment is preferably 50 mass% or less.

[0072] <Ingredient (B)> The component (B) in the present invention is water. Component (B) serves as a solvent in the production of hydrophobically modified cellulose fibers and as one of the components of the emulsion composition of the present invention.

[0073] <Component (C)> The component (C) in the present invention is an organic compound that is liquid at 25° C. and 1 atm. The component (C) may be a solvent used in the production of hydrophobically modified cellulose fibers. The solubility in water of an organic compound that is liquid at 25°C and 1 atmospheric pressure is preferably 10 g or less, and more preferably 1 g or less, per 100 g of water at 25°C. From the viewpoint of obtaining a film with improved water resistance and synovial fluid properties, the molecular weight of component (C) is preferably 100,000 or less, more preferably 50,000 or less, and even more preferably 10,000 or less, and from the same viewpoint, it is preferably 100 or more, more preferably 200 or more.

[0074] Component (C) in the present invention specifically includes an oil, an organic solvent, a polymerizable monomer, a prepolymer, etc. Component (C) in the present invention is preferably an oil, and examples of the oil, from the viewpoint of obtaining a film having improved water resistance and synovial properties, include one or more selected from the group consisting of alcohol, ester oil, hydrocarbon oil, silicone oil, ether oil, oils and fats, fluorine-based inert liquids, and fatty acids, and preferably one or more selected from the group consisting of ester oil, silicone oil, ether oil, oils and fats, and fluorine-based inert liquids, and more preferably silicone oil, esther oil, etc. Te More preferably, the oil is at least one selected from the group consisting of silicone oil and / or ether oil. Te More preferred is ethyl oil.

[0075] Examples of ester oils include monoester oils, diester oils, and triester oils. Specific examples include aliphatic or aromatic monocarboxylic acid or dicarboxylic acid esters having 2 to 18 carbon atoms, such as isopropyl myristate, octyldodecyl myristate, myristyl myristate, 2-hexyldecyl myristate, isopropyl palmitate, glycerin tri-2-ethylhexanoate, and glycerin triisostearate.

[0076] Examples of silicone oils include dimethylpolysiloxane, methylpolysiloxane, methylphenylpolysiloxane, octamethylcyclotetrasiloxane, and decamethylcyclopentasiloxane. Examples of fats and oils include vegetable oils such as soybean oil, coconut oil, linseed oil, cottonseed oil, rapeseed oil, and castor oil, and animal oils.

[0077] From the viewpoint of obtaining a film having improved water resistance and synovial fluid resistance, the compound of component (C) preferably has an SP value of 10 or less, more preferably 9.5 or less, even more preferably 9.0 or less, and even more preferably 8.5 or less, and from the same viewpoint, preferably has an SP value of 6.0 or more, more preferably 6.5 or more.

[0078] In this specification, the SP value is the solubility parameter calculated by the Fedors method (unit: (cal / cm 3 ) 1 / 2 ) and are described in, for example, reference books such as "SP Value Basics, Applications and Calculation Methods" (Joho Kikansha, 2005) and Polymer Handbook Third Edition (A Wiley-Interscience publication, 1989).

[0079] Examples of oils having an SP value of 10 or less that can be used in the present invention include oleic acid (SP value: 9.2), D-limonene (SP value: 9.4), PEG400 (SP value: 9.4), dimethyl succinate (SP value: 9.9), neopentyl glycol dicaprate (SP value: 8.9), hexyl laurate (SP value: 8.6), isopropyl laurate (SP value: 8.5), isopropyl myristate (SP value: 8.5), isopropyl palmitate (SP value: 8.5), isopropyl oleate (SP value: 8.6), hexadecane (SP value: 8.0), olive oil (SP value: 9.3), jojoba oil (SP value: 8.6), squalane (SP value: 7.9), liquid paraffin (SP value: 7.9), fluorine. Inert liquid (e.g., Fluorinert FC-40 (manufactured by 3M, SP value: 6.1), Fluorinert FC-43 (manufactured by 3M, SP value: 6.1), Fluorinert FC-72 (manufactured by 3M, SP value: 6.1), Fluorinert FC-770 (manufactured by 3M, SP value: 6.1)), silicone oil (e.g., KF96-1cs (manufactured by Shin-Etsu Chemical Co., Ltd., SP value: 7 .3), KF-96-10cs (manufactured by Shin-Etsu Chemical Co., Ltd., SP value: 7.3), KF-96-50cs (manufactured by Shin-Etsu Chemical Co., Ltd., SP value: 7.3), KF-96-100cs (manufactured by Shin-Etsu Chemical Co., Ltd., SP value: 7.3), KF-96-1000cs (manufactured by Shin-Etsu Chemical Co., Ltd., SP value: 7.3), KF-96H-10,000cs (manufactured by Shin-Etsu Chemical Co., Ltd., SP value: 7.3), etc.

[0080] <Ingredient (D)> The emulsion composition of the present invention may contain a polyether-modified silicone compound as component (D). By blending such component (D) in the emulsion composition, a film with improved water resistance and synovial fluid properties can be obtained, and the durability of the obtained film can be improved. One example of component (D) is a compound having a methyl silicone chain as the main chain and a polyoxyethylene group as the side chain, and specifically, a compound represented by the following general formula can be mentioned.

[0081] [ka]

[0082] (In the formula, R 1 is a methylene group, an ethylene group, or a trimethylene group, and R 2 represents an alkyl group having 1 to 4 carbon atoms, m represents an integer of 0 to 50, n represents an integer of 1 to 10, p represents an integer of 1 to 50, and q represents an integer of 0 to 50. 1 (C2H4O) p (C3H6O) q R 2 In the group represented by (C2H4O) p and (CHO) q can be random or block.)

[0083] From the viewpoint of the durability of the film obtained by drying the emulsion composition, the HLB value of the polyether-modified silicone compound is preferably within a specific range, specifically, preferably 1 or more, more preferably 5 or more, even more preferably 10 or more, and preferably 18 or less, more preferably 16 or less.

[0084] When two or more polyether-modified silicones with different HLB values ​​are used, the weighted average HLB value should be within the above range. The HLB value is an index that represents the balance between hydrophilicity and lipophilicity, and in the present invention refers to the value calculated by the following Griffin formula: HLB value = 20 × total molecular weight of hydrophilic groups / molecular weight

[0085] The kinematic viscosity of the polyether-modified silicone compound at 25°C is preferably within a specific range from the viewpoint of the durability of the film obtained by drying the emulsion composition. 2 / s or more, preferably 5 mm 2 / s or more, preferably 1000 mm 2 / s or less, preferably 500 mm 2 / s or less, more preferably 200 mm 2 / s or less.

[0086] Polyether-modified silicone compounds that can be preferably used as component (D) are commercially available, and examples of commercially available products include "KF-615A", "KF-640", "KF-642", "KF-643", "KF-644", "KF-351A", "KF-354L", "KF-355A", "KF-6011", "KF-6012", "KF-6015", "KF-6016", "KF-6017", "KF-6020", and "KF-6043" manufactured by Shin-Etsu Chemical Co., Ltd. (all trade names). From the viewpoint of the durability of the film obtained by drying the emulsion composition, "KF-640", "KF-642", "KF-643", "KF-351A", "KF-354L", "KF-355A", and the like can be preferably used. Commercially available products having a structure not corresponding to the above general formula (for example, "KF-6028" and "KF-6038" (both trade names) manufactured by Shin-Etsu Chemical Co., Ltd.) can also be used as component (D).

[0087] <Polymer compounds> The emulsion composition of the present invention may further contain a polymer compound. From the viewpoint of obtaining a membrane having high water resistance, such a polymer compound is preferably one or more selected from the group consisting of the following polymer compound (X) and polymer compound (Y), and more preferably the polymer compound (X). Polymer compound (X): A polymer compound having an ester group, an amide group, a urethane group, an amino group, an ether group, or a carbonate group in the main chain (however, a polymer compound that falls under either component (A-1) or component (D) is not considered to be a polymer compound (X)). Polymer compound (Y): Methacrylic or acrylic polymer having an ester group or amide group in the side chain

[0088] The mass average molecular weight of the polymer compound is preferably 1,000 or more from the viewpoint of obtaining a membrane having high water resistance, and from the same viewpoint, is preferably 500,000 or less.

[0089] [High molecular compound (X)] Examples of the polymer compound (X) having an ester group in the main chain include condensates of dicarboxylic acids such as adipic acid, sebacic acid, dodecanedioic acid, phthalic acid, isophthalic acid, terephthalic acid, succinic acid, and alkenylsuccinic acid with diols such as ethylene glycol, propylene glycol, and butanediol, and condensates of compounds having both a hydroxyl group and a carboxyl group in one molecule, such as glycolic acid and lactic acid.

[0090] Examples of the polymer compound (X) having an amide group in the main chain include condensates of dicarboxylic acids such as adipic acid, sebacic acid, dodecanedioic acid, phthalic acid, isophthalic acid, terephthalic acid, succinic acid, and alkenylsuccinic acid with diamines such as aliphatic diamines such as ethylenediamine, hexamethylenediamine, and propylenediamine.

[0091] Examples of the polymer compound (X) having a urethane group in the main chain include polymers of diisocyanates such as triresin diisocyanate, diphenyl isocyanate, xylylene diisocyanate, and hexamethylene diisocyanate with diols such as ethylene glycol, propylene glycol, and butanediol.

[0092] Examples of the polymer compound (X) having an amino group in the main chain include polymers of alkylimines such as ethyleneimine, propyleneimine, butyleneimine, dimethylethyleneimine, pentyleneimine, and hexyleneimine.

[0093] Examples of the polymer compound (X) having an ether group in the main chain include polymers of alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide, and polymers of formaldehyde.

[0094] Examples of the polymer compound (X) having a carbonate group in the main chain include condensation products of polyols such as 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(4-hydroxyphenyl)butane, and 1,1-bis(4-hydroxyphenyl)cyclohexane with phosgene.

[0095] [High molecular compound (Y)] Examples of the polymer compound (Y), that is, a methacrylic or acrylic polymer having an ester group or an amide group in the side chain, include polyalkyl(meth)acrylates such as polymethyl(meth)acrylate, polyethyl(meth)acrylate, and polybutyl(meth)acrylate, and poly(meth)acrylamides such as poly(meth)acrylamide, poly N-methyl(meth)acrylamide, poly N,N-dimethyl(meth)acrylamide, and poly N-phenyl(meth)acrylamide.

[0096] <Other ingredients> In addition to the above-mentioned components, the emulsion composition of the present invention may contain plasticizers, crystal nucleating agents, fillers (inorganic fillers, organic fillers), hydrolysis inhibitors, flame retardants, antioxidants, lubricants such as hydrocarbon waxes and anionic surfactants, UV absorbers, antistatic agents, antifogging agents, light stabilizers, pigments, antifungal agents, antibacterial agents, foaming agents, surfactants; starches, polysaccharides such as alginic acid; natural proteins such as gelatin, glue, and casein; inorganic compounds such as tannins, zeolites, ceramics, and metal powders; fragrances; flow regulators; leveling agents; conductive agents; UV dispersants; and deodorants, within the range that does not impair the effects of the present invention. Similarly, other polymeric materials and other compositions may be added within the range that does not impair the effects of the present invention.

[0097] <Properties of the emulsion composition> The emulsion composition of the present invention is a composition in an emulsified state that contains the above-mentioned components (A), (B) and (C) as essential components. The emulsification in the present invention is a state in which a mechanical force is applied to a mixture of water and an organic compound that is liquid at 25°C and 1 atm, and one liquid droplet is finely dispersed in the other liquid. Either an o / w type emulsion or a w / o type emulsion may be used, but an o / w type emulsion is preferred.

[0098] The content of component (A) in the emulsion composition or at the time of mixing is, from the viewpoint of emulsifying power, preferably 0.02 mass% or more, more preferably 0.05 mass% or more, and even more preferably 0.1 mass% or more, while, from the viewpoint of handleability, it is preferably 15 mass% or less, more preferably 10 mass% or less, and even more preferably 5 mass% or less.

[0099] The content of component (B) in the emulsion composition or at the time of mixing is preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more, from the viewpoint of maintaining the emulsified state, and is preferably 98% by mass or less, from the viewpoint of the effective amount.

[0100] The content of component (C) in the emulsion composition or at the time of mixing is, from the viewpoint of maintaining the emulsified state, preferably 0.1 mass % or more, more preferably 0.5 mass % or more, and even more preferably 1 mass % or more, while, from the viewpoint of solution viscosity and handleability, it is preferably 70 mass % or less, more preferably 60 mass % or less, and even more preferably 50 mass % or less.

[0101] The mass ratio (A / C) of component (A) to component (C) in the emulsion composition or when mixed is preferably 0.0001 or more, more preferably 0.001 or more, even more preferably 0.004 or more, even more preferably 0.01 or more, and even more preferably 0.04 or more, from the viewpoint of obtaining a film with improved water resistance and synovial fluid properties, and from the viewpoint of film formability, it is preferably 20 or less, more preferably 10 or less, even more preferably 5 or less, even more preferably 3 or less, and even more preferably 2 or less. From these viewpoints, it is preferably 0.0001 or more and 20 or less, more preferably 0.001 or more and 10 or less, even more preferably 0.004 or more and 5 or less, even more preferably 0.01 or more and 3 or less, and even more preferably 0.04 or more and 2 or less.

[0102] When component (D) is used, the content of component (D) in the emulsion composition or at the time of mixing is preferably 0.01 mass % or more, more preferably 0.05 mass % or more, and even more preferably 0.1 mass % or more, from the viewpoint of film durability, while it is preferably 5 mass % or less, more preferably 2 mass % or less, and even more preferably 1 mass % or less, from the viewpoint of suppressing an increase in the viscosity of the composition.

[0103] When the emulsion composition of the present invention contains the polymer compound, the content of the polymer compound in the emulsion composition is preferably 0.1 mass % or more, and more preferably 0.5 mass % or more, from the viewpoint of film durability, while it is preferably 20 mass % or less, more preferably 10 mass % or less, and even more preferably 5 mass % or less, from the viewpoint of suppressing an increase in the viscosity of the composition.

[0104] The viscosity of the emulsion composition is not particularly limited, but from the viewpoint of handling, the viscosity at 25°C is preferably 0.5 mPa·s or more, more preferably 0.8 mPa·s or more, and even more preferably 1 mPa·s or more, and from the same viewpoint, the viscosity is preferably 30 Pa·s or less, more preferably 20 Pa·s or less, and even more preferably 10 Pa·s or less. The viscosity here is measured using a Brookfield viscometer with an appropriate rotor suited to the viscosity range of each sample at 25°C and a rotation speed of 60 rpm after stirring for 1 minute.

[0105] The average particle size of the emulsion droplets in the emulsion composition, as measured by SEM observation described below, is preferably 10 nm or more, more preferably 50 nm or more, and even more preferably 100 nm or more, from the viewpoint of improving water resistance, synovial fluid resistance, and their durability, and from the same viewpoint, is preferably 2000 nm or less, more preferably 1000 nm or less, even more preferably 700 nm or less, and even more preferably 500 nm or less, preferably 10 nm or more and 2000 nm or less, more preferably 50 nm or more and 1000 nm or less, and even more preferably 100 nm or more and 500 nm or less.

[0106] 2. Method for producing emulsion composition The method for producing the emulsion composition of the present invention includes a step of mixing the above-mentioned components (A), (B), (C), etc. Here, an organic compound that is liquid at 25°C and 1 atmospheric pressure may be mixed with the aqueous dispersion of hydrophobically modified cellulose fibers, or the organic compound dispersion of hydrophobically modified cellulose fibers may be mixed with water.

[0107] Alternatively, the method for producing the emulsion composition of the present invention may include a method including a step of mixing components (A-1), (A-2), (B), and (C), and this method is more preferable because the step of obtaining the hydrophobically modified cellulose fiber and the step of obtaining the emulsion composition can be achieved in one step. There is no restriction on the mixing order in this method. For example, components (A-1), (A-2), and (B) may be mixed and then mixed with component (C), or components (A-1), (A-2), and (C) may be mixed and then mixed with component (B). A production method including a step of mixing component (A-1) and component (A-2) in the presence of component (B) and component (C) is preferred. Therefore, a preferred embodiment of the emulsion composition of the present invention contains components (A-1), (A-2), (B), and (C). In this case, the content of component (A) is the total content of components (A-1) and (A-2).

[0108] When component (D) is added, component (D) may be mixed together with these raw materials, or component (D) may be added to an emulsion composition obtained using these raw materials.

[0109] By mixing the components, emulsification occurs, and an emulsion composition is obtained. For such mixing, a magnetic stirrer, a mechanical stirrer, a homomixer, a vacuum emulsifier, a low-pressure homogenizer, a high-pressure homogenizer, a grinder, a cutter mill, a ball mill, a jet mill, a single-screw extruder, a twin-screw extruder, an ultrasonic agitator, a home juicer mixer, or the like can be used. The mixing may be performed by combining two or more types of operations.

[0110] The temperature and time during mixing of the components are not particularly limited, but are preferably within the temperature range of 5 to 50° C. and the time preferably within the range of 1 minute to 3 hours, for example.

[0111] The preferred range of the content of each component when mixed is the same as the preferred range of the content of each component in the emulsion composition of the present invention described above.

[0112] When using component (A-1) and component (A-2) instead of component (A), the upper and lower limit of the preferred content of component (A) is preferably the upper and lower limit of the total amount of both components. Here, the blending ratio of component (A-1) to component (A-2) is preferably 0.1 equivalent or more, more preferably 0.3 equivalent or more, and even more preferably 0.5 equivalent or more, relative to the anionic group of component (A-1), from the viewpoint of synovial property and its durability, while from the viewpoint of stability of emulsion composition, it is preferably 3 equivalent or less, more preferably 2 equivalent or less, and even more preferably 1.5 equivalent or less.

[0113] Alternatively, the ratio ([total number of moles of component (A-2) / [number of moles of anionic groups of component (A-1)]) of [the total number of moles of [the number of moles of amino groups of the amino-modified silicone] and [the number of moles of hydrocarbon-based compounds having a total carbon number of 16 to 40 and having cationic groups] of component (A-2) to [the number of moles of anionic groups of component (A-1)]] is preferably 0.1 or more, more preferably 0.3 or more, and even more preferably 0.5 or more from the viewpoint of obtaining a film having improved water resistance, synovial fluid properties, and durability, and is preferably 3 or less, more preferably 2 or less, and even more preferably 1.5 or less from the viewpoint of film formability. The number of moles of anionic groups of anion-modified cellulose fiber can be obtained by multiplying the amount (g) of anion-modified cellulose fiber used by the anionic group content (mmol / g), and the number of moles of amino groups of amino-modified silicone can be obtained by dividing the amount (g) of amino-modified silicone used by the amino equivalent (g / mol).

[0114] In addition, the mass ratio (A-2 / C) of component (A-2) to component (C) is preferably 0.0001 or more, more preferably 0.001 or more, even more preferably 0.004 or more, even more preferably 0.01 or more, and even more preferably 0.04 or more from the viewpoint of obtaining a film with improved water resistance, synovial fluid resistance, and durability, and is preferably 20 or less, more preferably 10 or less, even more preferably 5 or less, even more preferably 3 or less, and even more preferably 2 or less from the viewpoint of film formability. From these viewpoints, it is preferably 0.0001 or more and 20 or less, more preferably 0.001 or more and 10 or less, even more preferably 0.004 or more and 5 or less, even more preferably 0.01 or more and 3 or less, and even more preferably 0.04 or more and 2 or less.

[0115] 3. Method for producing a membrane containing hydrophobically modified cellulose fibers The method for producing a membrane containing hydrophobically modified cellulose fibers of the present invention includes a step of drying the emulsion composition of the present invention or the emulsion composition obtained by the method for producing an emulsion composition of the present invention.

[0116] Specifically, the emulsion composition is applied to a substrate, for example, a solid surface made of glass, resin, metal, ceramics, concrete, wood, stone, fiber, etc., or to skin, hair, etc. Examples of application methods include, but are not limited to, application methods using an applicator, bar coder, spin coater, etc., brush application, hand application, spraying, dip coating, etc.

[0117] The thickness of the coating film of the emulsion composition on a substrate is preferably 10 μm or more, more preferably 20 μm or more, and even more preferably 30 μm or more from the viewpoint of film durability, and is preferably 2000 μm or less, more preferably 1500 μm or less from the viewpoint of coatability.

[0118] The coating film of the emulsion composition is then dried to obtain a coating film. The drying conditions may be under reduced pressure or normal pressure, and the temperature range is preferably 15° C. to 75° C. The drying time is preferably 1 hour to 24 hours.

[0119] 4. Dried film of emulsion composition It is preferable that the dried film of the emulsion composition of the present invention obtained by the above-mentioned production method exhibits the synovial surface properties shown in the literature (Technology of Super Water-Repellent, Super Oil-Repellent, and Synovial Surfaces / Publisher: Hiroshi Motoki / Publisher: Science & Technology Co., Ltd. / Published on January 28, 2016).

[0120] The synovial surface property can be measured, for example, by the method described in the "Sliding Angle Measurement Test" in the Examples below. The smaller the sliding angle value, the higher the synovial property of the membrane.

[0121] The film of the present invention further improves the durability of the film by containing the above-mentioned polyether-modified silicone compound.

[0122] The thickness of the film of the present invention is not particularly limited, and from the viewpoint of film durability, it is preferably 1 μm or more, more preferably 3 μm or more, and even more preferably 5 μm or more, and from the viewpoint of economic efficiency, it is preferably 2000 μm or less, more preferably 1200 μm or less, more preferably 500 μm or less, and even more preferably 200 μm or less. The thickness of the film can be adjusted to a desired value by setting the coating thickness using a coating tool such as an applicator or adjusting the ratio of the medium. The thickness of the film can be measured according to the method described in the Examples below.

[0123] The film of the present invention is preferable because the higher the smoothness, the higher the synovial property.Specifically, the arithmetic mean roughness of the film immediately after production is preferably 0.3 μm or more, more preferably 0.5 μm or more, and even more preferably 0.8 μm or more from the viewpoint of cost-effectiveness, while it is preferably 40 μm or less, more preferably 35 μm or less, and even more preferably 30 μm or less from the viewpoint of adhesion suppression.The arithmetic mean roughness of the film can be measured according to the method described in the examples below.

[0124] The film of the present invention is preferably durable.The durability of film can be evaluated by, for example, the degree of increase in arithmetic mean roughness of film after contacting with water for a certain period of time or the presence or absence of synovial property.Specifically, according to the test method specified in the "synovial property durability test" in the following examples, if the arithmetic mean roughness of film after 5 minutes of dropping is less than twice the roughness before dropping, and the film after 5 minutes of dropping retains synovial property, the film can be evaluated as having high durability.

[0125] The amount of hydrophobically modified cellulose fiber in the film of the present invention is preferably 1% by mass or more, more preferably 10% by mass or more, from the viewpoint of the durability of the film, and is preferably 65% ​​by mass or less, more preferably 36% by mass or less, and even more preferably 16% by mass or less, from the viewpoint of the synovial properties of the film. The amount of hydrophobically modified cellulose fiber in the film can be determined taking into consideration the amount of volatile components (e.g., water and some oils) in the emulsion composition. The preferred ranges of the amounts of the components (C) and (D) in the membrane of the present invention also correspond to the preferred ranges of the amounts thereof in the emulsion composition.

[0126] The membrane of the present invention may contain optional components that do not impair the effects of the present invention. The content of these optional components in the membrane is preferably 0.1% by mass or more, more preferably 0.2% by mass or more, and even more preferably 0.5% by mass or more, and is preferably 20% by mass or less, more preferably 15% by mass or less, and even more preferably 10% by mass or less.

[0127] By applying the film of the present invention to a solid surface, the solid surface can be modified to a synovial surface. The film of the present invention is not only excellent in synovial properties, but also has excellent durability of the film itself, so that the effect can be maintained for a long time, and therefore it can be suitably used for various purposes, for example, as a packaging material for daily necessities, cosmetics, home appliances, etc., as an interior material for packaging containers such as blister packs, trays, and lunch box lids, food containers, industrial trays and transport pipes used for transporting and protecting industrial parts, and further as a covering material for roofs, walls of buildings, ship bottoms, electric wires, etc. This makes it possible to provide an anti-fouling film that suppresses the adhesion of dust, etc., an anti-snow film that suppresses the adhesion of snow and ice, etc., a water-repellent film, etc., and a coating material for roofs, walls of buildings, ship bottoms, electric wires, etc. rawIt can be suitably used as a biofouling prevention film or the like that inhibits the adhesion of organisms.

[0128] The emulsion composition of the present invention is useful as a biofouling inhibitor, an antifouling agent, and an anti-snow agent. By applying the emulsion composition of the present invention to the above-mentioned solid surfaces, it can be used as a method for inhibiting biofouling, an antifouling method, and an anti-snow method.

[0129] The film of the present invention can be obtained by drying the emulsion composition of the present invention, for example. (A) one or more hydrophobically modified cellulose fibers selected from the group consisting of the following components (a) and (b): (a) Hydrophobically modified cellulose fibers formed by bonding silicone compounds to cellulose fibers (b) a hydrophobically modified cellulose fiber in which a hydrocarbon compound having a total carbon number of 16 to 40 and a cationic group is bonded to an anionic group of the anionically modified cellulose fiber via an ionic bond; and (C) An organic compound that is liquid at 25°C and 1 atmosphere. and has a particulate structure.

[0130] It is believed that the cellulose fibers forming the emulsion particles form a networked particulate structure by removing the water from the emulsion composition through drying, and that the durability is improved by incorporating at least a portion of the (C) component into the particulate structure.

[0131] The maximum length of the particle is preferably 10 to 2000 nm, more preferably 50 to 1000 nm, from the viewpoint of improving water resistance, synovial fluid resistance and durability by SEM observation. The maximum length means the maximum length among length, width and height when the particle is assumed to be contained in the smallest rectangular parallelepiped. The preferred numerical ranges and aspects of each component of the membrane are the same as the preferred numerical ranges and aspects in the above-mentioned emulsion composition. EXAMPLES

[0132] The present invention will be specifically described below by showing examples etc. Note that the following examples are merely illustrative of the present invention and are not intended to limit the present invention in any way.

[0133] [Average fiber diameter, average fiber length, and average aspect ratio of anionically modified cellulose fibers and hydrophobically modified cellulose fibers] Water is added to the cellulose fibers to be measured to prepare a dispersion with a content of 0.0001% by mass. The dispersion is dropped onto mica and dried to prepare an observation sample, and the fiber height (difference in height between where the fibers are present and where they are not present) of the cellulose fibers in the observation sample is measured using an atomic force microscope (AFM) (Nanoscope II Tapping mode AFM manufactured by Digital Instrument; the probe used is Point Probe (NCH) manufactured by Nanosensors). At that time, 100 or more cellulose fibers are extracted from a microscope image in which the cellulose fibers can be confirmed, and the average fiber diameter is calculated from the fiber height. The average fiber length is calculated from the distance in the fiber direction. The average aspect ratio is calculated from the average fiber length / average fiber diameter. The height analyzed in the image by AFM can be considered as the fiber diameter.

[0134] [Average fiber diameter and average fiber length of raw cellulose fibers] Deionized water is added to the cellulose fibers to be measured to prepare a dispersion with a content of 0.01% by mass. The dispersion is measured using a wet dispersion type image analysis particle size distribution meter (manufactured by Jusco International, product name: IF-3200) under the following conditions: front lens: 2x, telecentric zoom lens: 1x, image resolution: 0.835 μm / pixel, syringe inner diameter: 6515 μm, spacer thickness: 500 μm, image recognition mode: ghost, threshold: 8, analysis sample amount: 1 mL, sampling: 15%. 100 or more cellulose fibers are measured, and the average ISO fiber diameter and average ISO fiber length are calculated as the average fiber diameter and average fiber length, respectively.

[0135] [Anionic Group Content of Anionically Modified Cellulose Fibers and Hydrophobically Modified Cellulose Fibers] A 100 mL beaker is filled with 0.5 g of cellulose fiber to be measured, and deionized water or a 2 / 1 mixed solvent of methanol / water is added to make a total of 55 mL. 5 mL of 0.01 M aqueous sodium chloride solution is added to the beaker to prepare a dispersion. The dispersion is stirred until the cellulose fiber to be measured is sufficiently dispersed. 0.1 M hydrochloric acid is added to the dispersion to adjust the pH to 2.5 to 3, and an automatic titration device (manufactured by DKK-TOA Corporation, product name "AUT-701") is used to drop 0.05 M aqueous sodium hydroxide solution into the dispersion with a waiting time of 60 seconds, and the conductivity and pH value are measured every minute. The measurement is continued until the pH becomes about 11, and a conductivity curve is obtained. The sodium hydroxide titration amount is determined from the conductivity curve, and the anionic group content of the cellulose fiber to be measured is calculated using the following formula. Anionic group content (mmol / g) = [sodium hydroxide titration amount × sodium hydroxide aqueous solution concentration (0.05M)] / [mass of cellulose fiber to be measured (0.5g)]

[0136] [Aldehyde group content of oxidized cellulose fiber] The carboxyl group content of the oxidized cellulose fiber to be measured is measured by the method for measuring the anionic group content described above. Separately, 100 g of the aqueous dispersion of the oxidized cellulose fiber to be measured (solid content 1.0% by mass), 100 g of acetate buffer (pH 4.8), 0.33 g of 2-methyl-2-butene, and 0.45 g of sodium chlorite are added to a beaker and stirred at 25°C for 16 hours to oxidize the aldehyde groups remaining in the oxidized cellulose fiber. After the reaction is complete, the fiber is washed with deionized water to obtain cellulose fiber with the aldehyde groups oxidized. The reaction solution is freeze-dried, and the carboxyl group content of the resulting dried product is measured using the above-mentioned method for measuring anionic group content, and the "carboxyl group content of the oxidized oxidized cellulose fiber" is calculated. Next, the aldehyde group content of the oxidized cellulose fiber to be measured is calculated using Equation 1.

[0137] Aldehyde group content (mmol / g) = (carboxyl group content of oxidized cellulose fiber after oxidation treatment) - (carboxyl group content of oxidized cellulose fiber to be measured) Equation 1

[0138] [Solid content in dispersion] The measurement is performed using a halogen moisture meter (Shimadzu Corporation; product name "MOC-120H") The measurement is performed every 30 seconds for 1 g of sample at a constant temperature of 150°C, and the value at which the mass loss is 0.1% or less of the initial amount of the sample is regarded as the solid content.

[0139] [Confirmation of crystal structure in hydrophobically modified cellulose fibers] The crystal structure of the hydrophobically modified cellulose fiber is confirmed by measurement under the following conditions using an X-ray diffractometer (MiniFlexII, manufactured by Rigaku Corporation). The measurement conditions were as follows: X-ray source: Cu / Kα-radiation, tube voltage: 30 kv, tube current: 15 mA, measurement range: diffraction angle 2θ = 5 to 45°, X-ray scan speed: 10° / min. The measurement sample had an area of ​​320 mm 2 The cellulose is compressed into a pellet having a thickness of 1 mm. The degree of crystallinity of the cellulose I crystal structure is calculated from the obtained X-ray diffraction intensity according to the following formula A.

[0140] <Formula A> Cellulose type I crystallinity (%) = [(I 22.6 -I 18.5 ) / I 22.6 ] x 100 [In the formula, I 22.6 is the diffraction intensity of the lattice plane (002 plane) (diffraction angle 2θ = 22.6°) in X-ray diffraction, I 18.5 indicates the diffraction intensity of the amorphous part (diffraction angle 2θ = 18.5°).

[0141] On the other hand, when the degree of crystallinity obtained by the above formula A is 35% or less, from the viewpoint of improving calculation accuracy, it is preferable to calculate based on the following formula B in accordance with the description on pages 199-200 of the "Wood Science Experiment Manual" (edited by the Japan Wood Research Society; published in April 2000). Therefore, when the crystallinity obtained by the above formula A is 35% or less, the value calculated based on the following formula B can be used as the crystallinity.

[0142] <Formula B> Cellulose type I crystallinity (%) = [A c / (A c +A a )] x 100 [In the ceremony, A c is the sum of the peak areas of the lattice planes (002 plane) (diffraction angle 2θ = 22.6°), (011 plane) (diffraction angle 2θ = 15.1°), and (0-11 plane) (diffraction angle 2θ = 16.2°) in X-ray diffraction, A a indicates the peak area of ​​the amorphous portion (diffraction angle 2θ = 18.5°), and each peak area is determined by fitting the obtained X-ray diffraction chart with a Gaussian function.

[0143] [Cellulose fiber (equivalent amount) in hydrophobically modified cellulose fiber] The amount of cellulose fiber (converted amount) in the hydrophobically modified cellulose fiber is measured by the following method. (1) When one type of "modifying compound" is added The amount of cellulose fiber (equivalent amount) is calculated by the following formula C. <Formula C> Amount of cellulose fiber (equivalent amount) (g) = mass of hydrophobically modified cellulose fiber (g) / [1 + molecular weight of modifying compound (g / mol) × bond amount of modifying group (mmol / g) × 0.001] (2) When two or more types of "modifying compounds" are added The amount of cellulose fiber (converted amount) is calculated taking into consideration the molar ratio of each compound (that is, the molar ratio when the total molar amount of the compounds added is taken as 1).

[0144] [Measurement of Viscosity of Emulsion Composition] Using a B-type viscometer (Toki Sangyo TVB-10) with a No. 1 rotor, measure the viscosity after 1 minute at 25°C and a rotation speed of 60 RPM.

[0145] [Observation of emulsion composition by Cryo-SEM] The observation of the emulsion composition by cryo-SEM is performed using a field emission scanning electron microscope Scios DualBeam manufactured by FEI. The observation is performed while gradually sublimating the water from the frozen emulsion composition. The observation is performed at an accelerating voltage of 2 kV and a magnification of 25,000 times.

[0146] [Measurement of emulsion droplet size using laser diffraction method] The particle size of the emulsion droplets is measured by laser diffraction using an LA-960 manufactured by Horiba, Ltd. Measurement conditions: Add water to the measurement cell, and measure the volume particle size distribution and volume median particle size (D 50 The relative refractive index is 1.20, the temperature is 25°C, the circulation pump is ON, the circulation speed is 5, and the stirring speed is 5.

[0147] [Preparation of anionically modified cellulose fibers] Preparation Example 1 Bleached coniferous kraft pulp (West Fraser, product name: Hinton) was used as the raw material for natural cellulose fibers. A commercial product (ALDRICH, free radical, 98% by mass) was used as TEMPO. Commercially available products were used for sodium hypochlorite, sodium bromide, and sodium hydroxide.

[0148] First, 10 g of the bleached kraft pulp fiber and 990 g of deionized water were weighed into a 2L PP beaker equipped with a mechanical stirrer and stirring blades, and after stirring at 25 ° C and 100 rpm for 30 minutes, 0.13 g of TEMPO, 1.3 g of sodium bromide, and 35.5 g of 10.5 mass% sodium hypochlorite aqueous solution were added in this order to the 10 g of pulp fiber. Using pH stat titration with an automatic titration device (manufactured by Toa DKK Corporation, product name: AUT-701), 0.5 M sodium hydroxide aqueous solution was dropped to maintain the pH at 10.5. After reaction at 25 ° C for 120 minutes at a stirring speed of 100 rpm, the drop of sodium hydroxide aqueous solution was stopped to obtain a suspension of anion-modified cellulose fiber.

[0149] The suspension of the anion-modified cellulose fiber was adjusted to pH 2 with 0.01M hydrochloric acid, and then thoroughly washed with deionized water until the electrical conductivity of the filtrate measured with a compact electrical conductivity meter (HORIBA, LAQUAtwin EC-33B) was 200μs / cm or less, and then dehydrated to obtain anion-modified cellulose fiber. The carboxyl group content of this anion-modified cellulose fiber was 1.50mmol / g, and the aldehyde group content was 0.23mmol / g.

[0150] Preparation Example 2 (Production of fine anion-modified cellulose fibers) Deionized water was added to the anion-modified cellulose fiber finally obtained in Preparation Example 1 to prepare 100 g of a suspension (solid content 2.0% by mass). A 0.5 M aqueous sodium hydroxide solution was added to adjust the pH to 8, and deionized water was added to make a total of 200 g. This suspension was subjected to a micronization treatment three times at 150 MPa using a high-pressure homogenizer (manufactured by Yoshida Kikai Co., Ltd., product name: Nanovater L-ES) to obtain a micronized anion-modified cellulose fiber dispersion (solid content 1.0% by mass). The counter ion of the carboxyl group of this micronized anion-modified cellulose fiber was a sodium ion. This micronized anion-modified cellulose fiber is abbreviated as "TCNF (Na type)".

[0151] Preparation Example 3 (Production of fine anion-modified cellulose fibers by reduction treatment of aldehyde groups) 182 g of the fine anion-modified cellulose fiber dispersion (solid content 1.0% by mass) obtained in Preparation Example 2 was weighed out, and deionized water was added to make a total of 400 g. 1.2 mL of 0.1 M sodium hydroxide aqueous solution and 120 mg of sodium borohydride were added thereto, and the mixture was stirred at 25°C for 4 hours. Next, 9 mL of 1 M hydrochloric acid was added to carry out protonation. After the reaction was completed, the mixture was filtered, and the resulting cake was washed six times with deionized water to remove salts and hydrochloric acid, to obtain a fine anion-modified cellulose fiber dispersion (solid content 0.9% by mass) in which the aldehyde groups had been reduced. The carboxyl group content of the obtained cellulose fiber was 1.50 mmol / g, and the aldehyde group content was 0.02 mmol / g. The carboxyl group of this fine anion-modified cellulose fiber was in the free acid form (COOH), and is abbreviated as "TCNF (H type)". The average fiber diameter of this fine anion-modified cellulose fiber was 3.3 nm, and the average fiber length was 600 nm.

[0152] [Preparation of hydrophobically modified cellulose fiber and emulsion composition] Example 1 In a beaker, 66.7 g of the fine anion-modified cellulose fiber dispersion obtained in Preparation Example 3 (solid content 0.9% by mass), 12.0 g of silicone oil 1, and 1.53 g of amino-modified silicone 1 (corresponding to 1 equivalent weight relative to the carboxyl group of the anion-modified cellulose fiber) were mixed, and deionized water was added thereto to make a total of 100 g. This solution was stirred with a mechanical stirrer for 5 minutes, and then processed with a high-pressure homogenizer (manufactured by Yoshida Kikai Co., Ltd., product name: Nanovaita L-ES) at 150 MPa for 10 passes to obtain an emulsion composition containing hydrophobically modified cellulose fiber in which amino-modified silicone is linked to anion-modified cellulose fiber via ionic bonds. The obtained composition was a cloudy liquid, and oil droplets were observed to be dispersed in water by observation with an optical microscope and Cryo-SEM, so that it was determined to be an emulsion composition. FIG. 1 shows a micrograph (25,000 times) of the emulsion composition produced in Example 1 by Cryo-SEM. Furthermore, measurement by laser diffraction revealed that the average particle size of the emulsion composition was 300 nm. Figure 2 shows a graph showing the particle size distribution of the emulsion droplets of the emulsion composition obtained by laser diffraction.

[0153] Example 2 An emulsion composition was obtained in the same manner as in Example 1, except that the amount of silicone oil was 1.2 g. The emulsion composition contained hydrophobically modified cellulose fibers in which amino-modified silicone was bonded to anion-modified cellulose fibers via ionic bonds.

[0154] Example 3 Except for using silicone oil 2 instead of silicone oil 1, the same procedure as in Example 1 was repeated to obtain an emulsion composition containing hydrophobically modified cellulose fibers in which amino-modified silicone was linked to anionically modified cellulose fibers via ionic bonds.

[0155] Example 4 An emulsion composition was obtained in the same manner as in Example 1, except that isopropyl myristate was used instead of silicone oil, containing hydrophobically modified cellulose fibers in which amino-modified silicone was linked to anionically modified cellulose fibers via ionic bonds.

[0156] Example 5 An emulsion composition was obtained in the same manner as in Example 1, except that amino-modified silicone 2 was used in place of amino-modified silicone 1 in an amount equivalent to the same amount. The emulsion composition included hydrophobically modified cellulose fibers in which amino-modified silicone was linked to anion-modified cellulose fibers via ionic bonds.

[0157] Example 6 An emulsion composition was obtained containing hydrophobically modified cellulose fibers in which amino-modified silicone was bonded to anion-modified cellulose fibers via ionic bonds in the same manner as in Example 1, except that the amount of amino-modified silicone was 0.77 g (corresponding to 0.5 equivalents relative to the carboxy groups of the anion-modified cellulose fibers).

[0158] Example 7 In a beaker, 22.2 g (solid content 0.9 mass%) of the fine anion-modified cellulose fiber dispersion obtained in Preparation Example 3, 40.0 g of the silicone oil 1, and 0.51 g (corresponding to 1 equivalent weight relative to the carboxyl groups of the anion-modified cellulose fiber) of the amino-modified silicone 1 were mixed, and deionized water was added thereto to make a total of 100 g. The same process as in Example 1 was then carried out to obtain an emulsion composition containing hydrophobically modified cellulose fibers in which the amino-modified silicone was linked to the anion-modified cellulose fibers via ionic bonds.

[0159] Example 8 100 g of the emulsion composition obtained in Example 1 was weighed into a beaker, and 10.2 g of polyether-modified silicone was added thereto and stirred at 25° C. for 30 minutes to obtain an emulsion composition.

[0160] Example 9 In a beaker, 66.7 g of the fine anion-modified cellulose fiber dispersion obtained in Preparation Example 3 (solid content 0.9% by mass) and 1.53 g of amino-modified silicone 1 were mixed, and deionized water was added to make a total of 88 g. This solution was stirred with a mechanical stirrer for 5 minutes, and then treated with a high-pressure homogenizer (manufactured by Yoshida Kikai Co., Ltd., product name: Nanovaita L-ES) at 150 MPa for 5 passes to obtain an aqueous dispersion of hydrophobically modified cellulose fibers in which amino-modified silicone was linked to anion-modified cellulose fibers via ionic bonds. 12.0 g of silicone oil 1 was added to the obtained aqueous dispersion, and the emulsion composition was obtained by treating with a high-pressure homogenizer (manufactured by Yoshida Kikai Co., Ltd., product name: Nanovaita L-ES) at 150 MPa for 5 passes.

[0161] Example 10 An emulsion composition was obtained in the same manner as in Example 1, except that the amount of silicone oil was 0.6 g. The emulsion composition contained hydrophobically modified cellulose fibers in which amino-modified silicone was bonded to anion-modified cellulose fibers via ionic bonds.

[0162] Example 11 In a beaker, 8.9 g of the fine anion-modified cellulose fiber dispersion obtained in Preparation Example 3 (solid content 0.9 mass%), 40.0 g of the silicone oil 1, and 0.20 g of the amino-modified silicone 1 (corresponding to 1 equivalent weight relative to the carboxyl groups of the anion-modified cellulose fiber) were mixed, and deionized water was added thereto to make a total of 100 g. The same process as in Example 1 was then carried out to obtain an emulsion composition containing hydrophobically modified cellulose fibers in which the amino-modified silicone was linked to the anion-modified cellulose fiber via an ionic bond.

[0163] Example 12 An emulsion composition containing hydrophobically modified cellulose fibers in which oleylamine was linked to anion-modified cellulose fibers via ionic bonds was obtained in the same manner as in Example 1, except that an equivalent amount of oleylamine (manufactured by Wako Pure Chemical Industries, Ltd.) was used instead of amino-modified silicone 1. Further, 0.2 g of polyether-modified silicone 1 was added, and the mixture was stirred at 25°C for 30 minutes to obtain an emulsion composition.

[0164] Example 13 200 mg of 4-(4,6-dimethoxy-1,3,5-triazin-2-yl)-4-methylmorpholinium chloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added to 20 g of the emulsion composition obtained in Example 1, and the mixture was stirred at room temperature (25° C.) for 24 hours. Next, the solution was placed in a dialysis membrane (Spectra Corporation, Spectra-Por, MWCO: 10 kDa) and purified by dialysis against deionized water at room temperature (25° C.) for 48 hours, to obtain an emulsion composition containing hydrophobically modified cellulose fibers to which amino-modified silicone was bonded via amide bonds.

[0165] Comparative Example 1 In a beaker, 60.0 g of the fine anion-modified cellulose fiber dispersion obtained in Preparation Example 2 (solid content 1.0% by mass) and 12.0 g of the silicone oil 1 were mixed, and deionized water was added thereto to make a total of 100 g. The solution was stirred with a mechanical stirrer for 5 minutes, and then treated with a high-pressure homogenizer (manufactured by Yoshida Kikai Co., Ltd., product name: Nanovaita L-ES) at 150 MPa for 10 passes to obtain an emulsion composition containing anion-modified cellulose fiber.

[0166] Comparative Example 2 In a beaker, 66.6 g of the fine anion-modified cellulose fiber dispersion obtained in Preparation Example 3 (solid content 0.9% by mass) and 12.0 g of the silicone oil 1 were mixed, and deionized water was added thereto to make a total of 100 g. The solution was stirred with a mechanical stirrer for 5 minutes, and then treated with a high-pressure homogenizer (manufactured by Yoshida Kikai Co., Ltd., product name: Nanovaita L-ES) at 150 MPa for 10 passes to obtain an emulsion composition containing anion-modified cellulose fiber.

[0167] Comparative Example 3 An emulsion composition was obtained in the same manner as in Example 1, except that polyetheramine 1 was used instead of amino-modified silicone 1, comprising hydrophobically modified cellulose fibers in which polyetheramine was linked to anionically modified cellulose fibers via ionic bonds.

[0168] Comparative Example 4 An emulsion composition was obtained in the same manner as in Example 1, except that octylamine (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used instead of amino-modified silicone 1, to obtain an emulsion composition containing hydrophobically modified cellulose fibers in which octylamine was linked to anion-modified cellulose fibers via ionic bonds.

[0169] Comparative Example 5 An emulsion composition was obtained in the same manner as in Example 1, except that triethylamine (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used instead of amino-modified silicone 1, thereby obtaining an emulsion composition containing hydrophobically modified cellulose fibers in which triethylamine was linked to anionically modified cellulose fibers via ionic bonds.

[0170] Comparative Example 6 The fine anion-modified cellulose fiber dispersion obtained in Preparation Example 3 was repeatedly washed with isopropyl alcohol to perform solvent replacement. The dispersion was diluted with isopropyl alcohol until the solid content was 0.5 mass%, and 100 g of this dispersion was weighed into a beaker. Next, 0.51 g of amino-modified silicone 1 (equivalent to 0.4 equivalents to the carboxyl group of the fine anion-modified cellulose fiber) was mixed with this dispersion, and the solution was stirred with a mechanical stirrer for 5 minutes, and then treated with a high-pressure homogenizer (manufactured by Yoshida Kikai Co., Ltd., product name: Nanovaita L-ES) at 150 MPa for 5 passes to obtain an isopropyl alcohol dispersion of hydrophobically modified cellulose fiber in which amino-modified silicone was linked to anion-modified cellulose fiber via ionic bonds. Further, 10.0 g of squalane was added to this dispersion and stirred at 25° C. for 30 minutes to obtain a coating liquid. This coating liquid was not an emulsion composition like those in the above-mentioned Examples and Comparative Examples, and instead contained squalane dissolved in isopropyl alcohol and hydrophobically modified cellulose fibers dispersed in isopropyl alcohol.

[0171] Details of representative components used in the examples are summarized below. [Modification compound] Amino-modified silicone 1: "SS-3551" manufactured by Dow Toray Co., Ltd., kinematic viscosity: 1,000, amino equivalent: 1,700 Amino-modified silicone 2: "SF-8452C" manufactured by Dow Toray Co., Ltd., kinematic viscosity: 600, amino equivalent: 6,400 Oleylamine: Fujifilm Wako Pure Chemical Industries, Ltd., amino equivalent: 267.5, total carbon number: 18 Polyetheramine 1: Huntsman "M-2070", amino equivalent: 2,000 [Component (C)] Silicone oil 1: Shin-Etsu Chemical Co., Ltd. "KF-96-10cs", SP value: 7.3 Isopropyl myristate: Fujifilm Wako Pure Chemical Industries, Ltd., SP value: 8.5 Silicone oil 2: Shin-Etsu Chemical Co., Ltd. "KF-96H-10,000cs", SP value: 7.3 Silicone oil 3: Shin-Etsu Chemical Co., Ltd. "KF-96-100cs", SP value: 7.3 Silicone oil 4: Shin-Etsu Chemical Co., Ltd. "KF-96-3000cs", SP value: 7.3 Squalane: Fujifilm Wako Pure Chemical Industries, SP value: 7.9 [Component (D)] Polyether modified silicone 1: Shin-Etsu Chemical Co., Ltd. "KF-640", HLB: 14

[0172] [Measurement of Stability of Emulsion Composition] The emulsion compositions prepared in Examples 1 to 13 and Comparative Examples 1 to 6 were weighed into 30 mL glass vials and left at 25° C. for one week. In all samples except for Example 9, no creaming or coalescence was observed, and high emulsion stability was demonstrated. On the other hand, creaming was observed in the sample of Example 9 two days after preparation. This shows that the emulsion compositions of Examples 1 to 8 and 10 to 13 have superior temporal stability of the emulsion system to the emulsion composition of Example 9.

[0173] Comparing Example 1 and Example 9, it was shown that mixing cellulose fibers and a silicone-based compound in the presence of both a liquid organic compound and water at 25°C and 1 atmosphere, i.e., producing hydrophobically modified cellulose fibers in the presence of both of these components, resulted in a more stable emulsion composition.

[0174] [Preparation of dry film] The emulsion compositions prepared in Examples 1 to 13 and Comparative Examples 1 to 2, 4, 5, and 6, and the coating liquid prepared in Comparative Example 3 were each applied in an amount of 2 mL onto separate glass substrates (Micro Slide Glass S2112, manufactured by MATSUNAMI Co., Ltd.) and spread over the entire area of ​​the slide glass. The films were then dried for 24 hours at 1 atmosphere, 25°C, and a humidity of about 40% RH to prepare films. The thickness of the film in Example 1 was measured by the following measurement method and was found to be 90 μm. In addition, the cross section of the dry film produced using the emulsion composition obtained in Example 1 was observed using an SEM by the method described below. As a result, it was found that the dry film had a particulate structure. Figure 3 shows an SEM micrograph (8000x) of the cross section of the dry film.

[0175] [Measurement of film thickness] The thickness of the film after drying was measured using a laser microscope (Keyence, VK-9710) under the following measurement conditions: objective lens: 10x, light intensity: 3%, brightness: 1548, Z pitch: 0.5μm. A part of the film was scraped off with a metal spatula, and the sample with the exposed glass substrate was measured. The height of the glass substrate and the height of the part with the film were measured using the built-in image processing software, and the thickness of the film was calculated by taking the difference between them.

[0176] [Observation of the cross-sectional structure of the membrane] The dried film was frozen with liquid nitrogen and cut with a knife to expose the cross section. After the sample was returned to room temperature (25°C), it was subjected to osmium deposition treatment and the cross section was observed using a FEI field emission scanning electron microscope Scios DualBeam. Observation was performed at an accelerating voltage of 5 kV and a magnification of 8000 times.

[0177] [Measurement of arithmetic mean roughness of film] The arithmetic mean roughness of the surface of the dried films of Examples 1 and 8 and Comparative Example 6 prepared as described above was measured. The arithmetic mean roughness of the film was measured under the following measurement conditions using a laser microscope (Keyence Corporation, VK-9710). The measurement conditions were objective lens: 10x, light amount: 3%, brightness: 1548, Z pitch: 0.5 μm. The arithmetic mean roughness was measured at five points using the built-in image processing software, and the average value was used.

[0178] [Measurement of Water Resistance of Dry Film] The dried films of Examples 1 to 13 and Comparative Examples 1 to 6 were prepared as described above. After wiping off the oil floating on the surface of the dried film, the glass plate was immersed in a 300 mL beaker filled with water, and the swelling degree of the dried film after 5 minutes and 30 minutes was calculated by the following formula E. In addition, when the dried film collapsed and dispersed in water, "collapse" was recorded instead of the swelling degree. The results are shown in the table below.

[0179] <Formula E> Swelling degree [%] = [{[Mass after immersion] - [Mass of glass plate before coating]} ÷ {[Mass before immersion] - [Mass of glass plate before coating]} - 1] x 100 Mass after immersion: Mass of the glass substrate after the glass substrate and the dried film formed on the substrate are immersed for a specified period of time. Mass before immersion: Mass of the glass substrate and the dry film formed on the substrate before immersing the glass substrate in water

[0180] [Slide angle measurement test] The dried films of Examples 1 to 13 and Comparative Examples 1 to 6 prepared as described above were placed horizontally, and 8 μL of water droplets (23° C.) were dropped onto each film at 23° C. using a fully automatic contact angle meter (Kyowa Interface Science Co., Ltd., FAMAS), and left to stand for 1 second. Next, the film surface was tilted to 85° at a speed of 1° / s, and the angle at which the droplet began to slide was measured. The measurement results are shown in the table below. However, if the droplet did not slide down even when tilted to 85°, the water droplet sliding angle was recorded as "85 or more". The smaller the value of the water droplet sliding angle, the higher the synovial property of the film.

[0181] [Table 1-1]

[0182] [Table 1-2]

[0183] [Table 2]

[0184] The following was found from the above table. It was found that the film obtained by drying the emulsion composition described in the present invention exhibits synovial properties. Considering the composition of Example 1 and the composition of Example 6, it was found that Example 1, which has a higher degree of silicone group introduction as a modification group, has better synovial properties. Considering the composition of Example 1, the composition of Example 2, and the composition of Example 7, it was found that the synovial properties tend to decrease as the amount of organic compound that is liquid at 25°C and 1 atmospheric pressure relative to the hydrophobically modified cellulose fiber increases, that is, as the A / C ratio decreases.

[0185] [Synovial durability test] In order to examine the durability of the films produced in Examples 1, 8, and Comparative Example 6, the substrates on which these films were formed, as prepared in the above-mentioned [Preparation of Dry Film], were held horizontally, and water was continuously dripped onto the substrate from a height of 40 cm at a flow rate of 50 mL / sec. The arithmetic mean roughness and synovial properties of the film were measured at three points: before dripping, after dripping for 5 minutes, and after dripping for 20 minutes. The arithmetic mean roughness of the film was measured by the above-mentioned method. Regarding synovial properties, the substrate was held at an angle of 15° to the horizontal direction, and a 10 μL water droplet was placed on it. If the water droplet slid down, it was judged to have synovial properties, and if it did not slide down, it was judged to have no synovial properties.

[0186] [Table 3]

[0187] The following was found from Table 3 above. It was found that the films obtained by drying the emulsion compositions of Examples 1 and 8 have better durability than the film obtained by drying the coating liquid of Comparative Example 6, because the film roughness after continuous water dripping is suppressed and the synovial properties are maintained. Furthermore, it was found that the film obtained by drying the emulsion composition of Example 8, which further contains a polyether-modified silicone compound, has better durability.

[0188] Example 14 An emulsion composition was obtained in the same manner as in Example 1, except that the amount of silicone oil 1 was 6 g. The emulsion composition included hydrophobically modified cellulose fibers in which amino-modified silicone 1 was bonded to anion-modified cellulose fibers via ionic bonds.

[0189] Example 15 100 g of the emulsion composition obtained in Example 14 was weighed into a beaker, 10.2 g of polyether-modified silicone was added thereto, and the mixture was stirred at 25° C. for 30 minutes to obtain an emulsion composition.

[0190] Example 16 An emulsion composition was obtained containing hydrophobically modified cellulose fibers in which amino-modified silicone 1 was linked to anion-modified cellulose fibers via ionic bonds in the same manner as in Example 14, except that silicone oil 2 was used instead of silicone oil 1.

[0191] Test Example 1 <Outdoor aquatic organism adhesion test> The emulsion compositions prepared in Examples 14 to 16 were applied in an amount of 1.5 mL onto a SUS304 substrate (L50 mm × W50 mm × T3 mm) and dried for 24 hours at 1 atm, 25°C, and a humidity of approximately 40% RH to prepare a film. An untreated SUS304 substrate measuring L50 mm × W50 mm × T3 mm was used as Comparative Example 7. The above-mentioned substrates were connected with chains and placed in seawater near Shimotsu Port in Wakayama Prefecture so that the depth was 2 m below the water surface at low tide, and an immersion test in seawater was conducted for three months. After one month and three months of immersion, the degree of adhesion of crustaceans and algae to the substrate was visually evaluated. The evaluation criteria are as follows. The smaller the value, the higher the effect of inhibiting adhesion of aquatic organisms.

[0192] 1: A state in which the adhesion of aquatic organisms is 2% or less of the substrate surface area. 2: A state in which aquatic organisms are attached to more than 2% and less than 10% of the area of ​​the substrate surface. 3: A state in which aquatic organisms are attached to more than 10% but less than 20% of the surface area of ​​the substrate. 4: A state in which aquatic organisms are attached to more than 20% but less than 30% of the surface area of ​​the substrate. 5: A state in which aquatic organisms are attached to more than 30% but less than 50% of the area of ​​the substrate surface. 6: A state in which aquatic organisms are attached to more than 50% but less than 80% of the area of ​​the substrate surface. 7: A state in which aquatic organisms are attached to more than 80% of the substrate surface area.

[0193] Test Example 2 <Adherent aquatic organism removal test> In the above Test Example 1, the removability of aquatic organisms attached to the substrate after one month and three months of immersion was evaluated according to the following criteria. Note that low pressure here refers to a weak pressure, such as that sprayed from a washing bottle. The smaller the value, the easier it is to remove aquatic organisms.

[0194] 1: Can be easily removed with low pressure water flush. 2: Requires rinsing and scrubbing. 3: Requires use of tools (removed in one scraping operation). 4: Requires multiple cutting operations with tools or cannot be removed. The above results are shown in Table 4.

[0195] [Table 4]

[0196] From Table 4, it was found that the film formed using the emulsion composition of the present invention has an effect of suppressing the adhesion of aquatic organisms themselves, and also has good removability of attached aquatic organisms. In particular, it was found that the film formed using the emulsion composition of Example 15 has excellent effects of suppressing the adhesion of aquatic organisms and of removing them, and that such effects can be maintained for a long period of time of 3 months.

[0197] Example 17 An emulsion composition was obtained in the same manner as in Example 1, except that silicone oil 3 was used instead of silicone oil 1, and 1.91 g (corresponding to 1.25 equivalents relative to the carboxyl groups of the anion-modified cellulose fibers) of amino-modified silicone 1 was used.

[0198] Example 18 100 g of the emulsion composition obtained in Example 17 was weighed into a beaker, 10.2 g of polyether-modified silicone was added thereto, and the mixture was stirred at 25° C. for 30 minutes to obtain an emulsion composition.

[0199] Example 19 An emulsion composition was obtained in the same manner as in Example 18, except that the amount of silicone oil was 4.0 g.

[0200] Example 20 An emulsion composition was obtained in the same manner as in Example 18, except that silicone oil 1 was used instead of silicone oil 3.

[0201] Example 21 An emulsion composition was obtained in the same manner as in Example 18, except that silicone oil 4 was used instead of silicone oil 3.

[0202] [Preparation of dry film] The emulsion compositions prepared in Examples 17 to 21 were each applied in an amount of 2.4 mL onto separate glass substrates (10 cm x 10 cm x 5 mm thick) and spread over the entire surface of the glass substrate. The substrates were then dried for 24 hours at 1 atmosphere, 25°C, and a humidity of approximately 40% RH to prepare films. The thickness of the film of Example 17 was measured by the following measurement method and found to be 20 μm.

[0203] Comparative Examples 8 to 9 In Comparative Example 8, a glass substrate itself was used. In Comparative Example 9, a commercially available anti-snow paint, "Kansai Paint's Easy Snow Paint," was spread with a brush on the same glass substrate as that used in Example 1, and dried for 24 hours at 1 atmosphere, 25°C, and a humidity of about 40% RH. The paint thickness was 20 μm.

[0204] Test example: <Ice crushing slipperiness evaluation test> Each of the substrates in Examples 17 to 21 and Comparative Examples 8 to 9 was fixed to a 45° inclined table with double-sided tape (Scotch super strong double-sided tape, super multi-purpose, width 12 mm, manufactured by 3M). Then, in a room with an air temperature of 2°C, crushed ice was dropped onto the surface of each substrate using an electric ice scraper (DTY19, manufactured by Doshisha Co., Ltd.), and the ice sliding property was evaluated according to the following criteria. The higher the value, the better the ice sliding property. The specific gravity of the crushed ice was 0.49 g / cm. 3 It was.

[0205] 5: More than 90% of the ice has slid away. 4: More than 80% but less than 90% of the ice has slid down. 3: More than 50% but less than 80% of the ice has slid down. 2: More than 20% but less than 50% of the ice slid down. 1: Less than 20% of the ice slid off.

[0206] Test example <Snow sliding evaluation test> The sliding properties were evaluated in the low temperature testing chamber (1°C) at MTS Snow and Ice Research Institute Co., Ltd. A 1 cm x 2 cm x 2 mm thick stainless steel piece was attached to the back of each of the substrates of Examples 17 to 21 and Comparative Examples 8 to 9 with double-sided tape (Scotch super strong double-sided tape, super multi-purpose, width 12 mm, manufactured by 3M), and the substrate was placed on a fixed stand equipped with a magnet so that the substrate was at a 90° angle. Next, artificial snow was blown onto the front of the substrate at a wind speed of 5 m / s for 30 minutes, and the snow sliding properties were evaluated according to the following criteria. The higher the value, the better the snow sliding properties. The specific gravity of the artificial snow was 0.29 g / cm 3 It was.

[0207] 5: Skiing within 10 minutes. Skiing within 4:15 minutes. 3: Skiing within 20 minutes. Skiing within 2:30 minutes. Did not ski within the 1:30 minute test time.

[0208] [Table 5]

[0209] From Table 5, it was found that the film obtained by drying the emulsion composition of the present invention is less likely to retain water droplets and more likely to allow ice and snow to slide off than a glass substrate alone (Comparative Example 8) or a commercially available anti-snow paint (Comparative Example 9). Therefore, it was found that the film obtained by drying the emulsion composition of the present invention exhibits excellent performance as an anti-stain film and anti-snow film. Unexpectedly, snow and ice slid off even under low-temperature conditions of 1 to 2°C, so it is clear that the anti-snow film of the present invention has high usefulness. [Industrial Applicability]

[0210] The emulsion composition of the present invention can form a film with synovial properties, and therefore can be used in the fields of coatings for various surfaces, such as ships and bridges, and cosmetics.

Claims

1. An emulsion composition comprising the following components (A) to (C): (A) One or more hydrophobically modified cellulose fibers selected from the group consisting of the following components (a) and (b): (a) Hydrophobically modified cellulose fibers formed by bonding silicone compounds to cellulose fibers (b) Hydrophobically modified cellulose fibers in which a hydrocarbon compound having a total carbon number of 16 to 40 and a cationic group is bonded to the anionic group of an anionically modified cellulose fiber via an ionic bond. (B) Water (C) An organic compound that has a solubility of 1 g or less per 100 g of water at 25°C and is liquid at 25°C and 1 atmosphere.

2. 2. The emulsion composition according to claim 1, wherein the component (C) contains an oil, and the oil is at least one selected from the group consisting of ester oils, hydrocarbon oils, silicone oils, ether oils, fats and oils, and fluorine-based inert liquids.

3. 3. The emulsion composition according to claim 1, wherein the component (a) is a hydrophobically modified cellulose fiber obtained by bonding a silicone compound to an anionically modified cellulose fiber.

4. The emulsion composition according to any one of claims 1 to 3, wherein component (a) is a hydrophobically modified cellulose fiber in which an amino-modified silicone is bonded to a carboxy group of a carboxy group-containing cellulose fiber via an ionic bond or an amide bond.

5. The emulsion composition according to any one of claims 1 to 4, wherein component (b) is a hydrophobically modified cellulose fiber in which a hydrocarbon compound having an amino group and a total carbon number of 16 to 40 is bonded via an ionic bond to a carboxy group of a carboxy group-containing cellulose fiber.

6. The emulsion composition according to any one of claims 1 to 5, wherein the mass ratio (A / C) of component (A) to component (C) is 0.0001 or more and 20 or less.

7. The emulsion composition according to any one of claims 1 to 6, further comprising a component (D) a polyether-modified silicone compound.

8. Component (A-1) anion-modified cellulose fiber, Component (A-2) one or more compounds selected from the group consisting of amino-modified silicones and hydrocarbon-based compounds having cationic groups and a total carbon number of 16 to 40, Component (B) water, and Component (C) is an organic compound that has a solubility of 1 g or less per 100 g of water at 25°C and is liquid at 25°C and 1 atmosphere. The emulsion composition according to any one of claims 1 to 7, comprising:

9. Component (A-1) anion-modified cellulose fiber, Component (A-2) one or more compounds selected from the group consisting of amino-modified silicones and hydrocarbon-based compounds having cationic groups and a total carbon number of 16 to 40, Component (B) water, and Component (C) is an organic compound that has a solubility of 1 g or less per 100 g of water at 25°C and is liquid at 25°C and 1 atmosphere. The method for producing the emulsion composition according to claim 8, comprising the step of mixing the above ingredients.

10. A method for producing a membrane containing hydrophobically modified cellulose fibers, comprising a step of drying the emulsion composition according to any one of claims 1 to 8.

11. A biofouling inhibitor comprising the emulsion composition according to any one of claims 1 to 8.

12. An antifouling agent comprising the emulsion composition according to any one of claims 1 to 8.

13. A snow prevention agent comprising the emulsion composition according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Viscous aqueous composition, method for producing the same and cellulose fiber used therefor

    JP2012126786A

  • Skin cosmetic

    JP2017014116A

  • Lubricant composition

    JP2018044095A

  • Film comprising hydrophobized cellulose fibers and oil

    WO2018164135A1