Manufacturing method of electrode plate, manufacturing method of secondary battery, electrode plate and secondary battery
The method for manufacturing electrode plates with a smaller roughness non-laser irradiated surface reduces spatter adhesion, addressing the issue of internal short circuits and maintaining battery performance by minimizing spatter detachment.
Patent Information
- Application Number
- JP2021213044
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-12-27
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2041-12-27
AI Technical Summary
The production of electrode plates with electrode tabs results in the scattering of fine molten metal pieces (spatter) that can adhere to the tab, potentially causing minute internal short circuits in secondary batteries.
A manufacturing method for electrode plates that involves cutting the electrode core with a laser, utilizing a surface with smaller surface roughness as the non-laser irradiated surface to minimize spatter adhesion, particularly using pulsed lasers to reduce spatter attachment to the electrode tab.
The method effectively reduces the number of spatters adhering to the electrode tab, preventing internal short circuits and maintaining battery performance by minimizing spatter detachment within the secondary battery.
Smart Images

Figure 0007583704000002 
Figure 0007583704000003 
Figure 0007583704000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing an electrode plate, a method for manufacturing a secondary battery, an electrode plate, and a secondary battery. [Background technology]
[0002] A secondary battery such as a lithium ion secondary battery includes, for example, an electrode body in which a positive electrode plate and a negative electrode plate face each other via a separator. Hereinafter, these positive electrode plate and negative electrode plate are collectively referred to as "electrode plate". This electrode plate includes, for example, an electrode core body which is a metal foil, and an electrode active material layer applied to the surface of the electrode core body. In manufacturing an electrode plate having such a configuration, first, an electrode active material layer is applied to a large electrode core body to prepare a precursor of the electrode plate (hereinafter referred to as "electrode precursor"). Then, an electrode plate is cut out from the electrode precursor using a laser or the like. In this way, an electrode plate of a desired size can be obtained. Various lasers such as a continuous wave laser (CW laser) and a pulsed laser are used to cut out this electrode plate (see Patent Document 1).
[0003] Incidentally, when constructing a secondary battery, an electrode tab where the electrode core is exposed may be formed on a part of an electrode plate, and the electrode tab may be connected to a conductive member (such as a current collector). When manufacturing an electrode plate having such an electrode tab, first, an area (core exposed area) where no electrode active material layer is provided and where the electrode core is exposed is formed on an electrode precursor. Then, when cutting out an electrode plate from the electrode precursor, a part of the core exposed area is cut out. This makes it possible to manufacture an electrode plate having a part of the core exposed area (electrode tab). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2018-37308 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, in the manufacture of an electrode plate having an electrode tab, when the core exposed region where the metal foil (electrode core) is exposed is cut with a laser, fine molten metal pieces (spatter) may scatter and adhere to the electrode tab of the electrode plate. If a large amount of spatter detaches from the electrode tab inside the secondary battery after construction, there is a risk that the possibility of a small internal short circuit occurring may increase.
[0006] The present invention has been made in consideration of the above-mentioned problems, and has an object to provide a technique for reducing the number of sputter deposits on the electrode tabs of an electrode plate. [Means for solving the problem]
[0007] In order to achieve the above object, a method for manufacturing an electrode plate is disclosed herein.
[0008] The method for manufacturing an electrode plate disclosed herein manufactures an electrode plate including an electrode core that is a metal foil and an electrode active material layer applied to the surface of the electrode core. The method for manufacturing an electrode plate includes a precursor preparation step of preparing an electrode precursor having an active material applied region where an electrode active material layer is applied to the surface of the electrode core and a core exposed region where the electrode core is exposed without the electrode active material layer applied, and a core exposed region cutting step of cutting the core exposed region with a laser to form an electrode tab. In the method for manufacturing an electrode plate disclosed herein, the electrode core has a first surface and a second surface opposite to the first surface and having a smaller surface roughness than the first surface, and in the core exposed region cutting step, a laser is irradiated to the first surface.
[0009] The technology disclosed herein has been developed with the focus on the fact that the difference in surface roughness of each surface of the electrode core has a large effect on the amount of sputter adhesion. Specifically, it has been found that the amount of sputter adhesion on the laser irradiated surface is not easily affected by the surface roughness of the laser irradiated surface. It has also been found that the amount of sputter adhesion on the non-laser irradiated surface is easily affected by the surface roughness of the non-laser irradiated surface, and the larger the surface roughness of the non-laser irradiated surface, the greater the amount of sputter adhesion. In the manufacturing method of the electrode plate disclosed herein, the second surface with the smaller surface roughness is used as the non-laser irradiated surface. This makes it difficult for sputter scattered on the non-laser irradiated surface side of the electrode core to adhere to the non-laser irradiated surface of the electrode core, thereby reducing the number of sputter adhesions to the electrode tab.
[0010] In a preferred embodiment of the electrode plate manufacturing method disclosed herein, the laser is a pulsed laser. A pulsed laser can cut an electrode plate more easily than other lasers (such as a CW laser), but it tends to generate a larger amount of scattered spatter. However, according to the manufacturing method disclosed herein, even if the amount of scattered spatter increases when a pulsed laser is used, the amount of spatter adhering to the electrode tab can be sufficiently reduced.
[0011] In a preferred embodiment of the method for producing an electrode plate disclosed herein, the electrode core contains copper or a copper alloy. Spatters generated from negative electrode cores containing these copper-based materials are highly conductive, and therefore tend to cause a decrease in battery performance due to minute internal short circuits. However, the method for producing an electrode plate disclosed herein can reduce the amount of spatter attached to the electrode tab, and therefore can suitably prevent a decrease in battery performance due to minute internal short circuits even when an electrode core containing a copper-based material is used.
[0012] In a preferred embodiment of the method for producing an electrode plate disclosed herein, the average roughness Sa of the second surface is 0.07 μm or more and 0.25 μm or less. By using an electrode core having a second surface with such small surface roughness, the amount of spatter adhesion can be more suitably reduced.
[0013] In a preferred embodiment of the method for producing an electrode plate disclosed herein, the average roughness Sa of the first surface is 0.1 μm or more and 0.3 μm or less. According to the method for producing an electrode plate disclosed herein, even when an electrode core having such a first surface is used, the amount of sputtering adhering to the electrode core can be reduced.
[0014] In a preferred embodiment of the electrode plate manufacturing method disclosed herein, an active material-imparting region cutting step is further provided in which the active material-imparting region is cut with a laser, and the core-exposed region cutting step and the active material-imparting region cutting step are alternately performed to manufacture an electrode plate having a plurality of electrode tabs protruding from the side edges of the active material-imparting region. This makes it possible to minimize laser cutting of the core-exposed region, which causes a large amount of spatter to scatter on the surface side of the electrode plate, and therefore further reduce the amount of spatter adhering to the electrode tabs.
[0015] As another aspect of the technology disclosed herein, a method for manufacturing a secondary battery is provided. The method for manufacturing a secondary battery is a method for manufacturing a secondary battery having an electrode assembly including a positive electrode plate and a negative electrode plate, and at least one of the positive electrode plate and the negative electrode plate is manufactured using the manufacturing method for the electrode plate having the above-mentioned configuration. This makes it possible to suppress detachment of sputters from the electrode plate inside the manufactured secondary battery, and to prevent a decrease in performance of the secondary battery.
[0016] In a preferred embodiment of the method for producing a secondary battery disclosed herein, the method further includes an electrode body fabrication step of fabricating an electrode body having an electrode tab group in which a plurality of electrode tabs are stacked, and a current collecting member connection step of connecting a current collecting member to one surface of the electrode tab group, and in the current collecting member connection step, the second surface of the electrode core is disposed on the other surface of the electrode tab group to which the current collecting member is not connected. This allows the first surface, which has a larger amount of spatter attached than the second surface, to be enclosed between the electrode tab and the current collecting member (or between the plurality of electrode tabs), thereby more suitably suppressing detachment of the spatter from the electrode plate.
[0017] In addition, an electrode plate is provided as another aspect of the technology disclosed herein. That is, the electrode plate disclosed herein includes an electrode core, which is a foil-shaped metal member, and an electrode active material layer that is applied to the surface of the electrode core and contains an electrode active material. The electrode plate also includes an electrode plate main body portion, which is a region where the electrode active material layer is applied to the surface of the electrode core, and an electrode tab that protrudes from the electrode plate main body portion, has no electrode active material layer applied, and includes an exposed region where the electrode core is exposed. The electrode core of the electrode plate has a first surface and a second surface opposite to the first surface and has a surface roughness smaller than that of the first surface, and the electrode core exposed in the electrode tab has a number of metal particles attached to the second surface that is smaller than the number of metal particles attached to the first surface. The electrode plate disclosed herein is manufactured by the manufacturing method of the electrode plate having the above configuration. This electrode plate has a structural feature in that the number of metal particles (sputtering) attached to the second surface, which has a relatively small surface roughness, is small.
[0018] In a preferred embodiment of the electrode plate disclosed herein, a plurality of electrode tabs protrude outward from the outer edge of the electrode plate body, and each of the electrode tabs includes an active material layer-applied region where an electrode active material layer is applied to a base portion of the electrode tab adjacent to the electrode plate body. To manufacture an electrode plate having such a configuration, it is necessary to alternately perform a core-exposed region cutting step and an active material-applied region cutting step. As described above, by adopting such a manufacturing process, it is possible to minimize the laser cutting of the core-exposed region, which scatters a large amount of spatter, and therefore the amount of spatter adhering to the electrode tab can be further reduced.
[0019] In a preferred embodiment of the electrode plate disclosed herein, a modified substance fixing region in which a modified substance of the electrode active material layer is fixed on the electrode core is formed on the outer edge of the electrode plate main body, and the width of the modified substance fixing region on the first surface is larger than the width of the modified substance fixing region on the second surface. In the electrode plate disclosed herein, the surface roughness of the first surface of the electrode core is larger than that of the second surface, so that the modified substance of the electrode active material layer that is attached in large amount to the first surface, which is the laser irradiated surface, can be prevented from detaching from the electrode core.
[0020] As another aspect of the technology disclosed herein, a secondary battery is provided. The secondary battery is a secondary battery having an electrode assembly including a positive electrode plate and a negative electrode plate, at least one of the positive electrode plate and the negative electrode plate being an electrode plate having the above-mentioned configuration. This makes it possible to suppress detachment of sputters from the electrode plate inside the secondary battery and to prevent a decrease in performance of the secondary battery due to a minute internal short circuit.
[0021] In a preferred embodiment of the secondary battery disclosed herein, the electrode body includes an electrode tab group in which a plurality of electrode tabs are stacked, a current collecting member is connected to one surface of the electrode tab group, and the second surface of the electrode core is disposed on the other surface of the electrode tab group to which the current collecting member is not connected. This allows the first surface, which has a larger amount of spatter attached thereto than the second surface, to be enclosed between the electrode tab and the current collecting member (or between the plurality of electrode tabs), thereby more suitably suppressing detachment of the spatter from the electrode tab.
[0022] In a preferred embodiment of the secondary battery disclosed herein, the electrode tab group is bent so that the current collecting member and the side surface of the electrode body face each other. [Brief description of the drawings]
[0023] [Figure 1] 4 is a flowchart illustrating a method for manufacturing an electrode plate according to an embodiment. [Diagram 2] FIG. 2 is a plan view illustrating a negative electrode plate manufactured by a method for manufacturing an electrode plate according to an embodiment of the present invention. [Diagram 3] 4A to 4C are plan views illustrating a method for manufacturing an electrode plate according to an embodiment. [Figure 4] 4 is a cross-sectional view taken along line IV-IV in FIG. 3. [Diagram 5] 3 is a cross-sectional view taken along the line VV in FIG. 2. [Figure 6] FIG. 1 is a perspective view illustrating a secondary battery according to an embodiment. [Figure 7] FIG. 7 is a schematic vertical cross-sectional view taken along line VII-VII in FIG. [Figure 8] FIG. 7 is a schematic vertical cross-sectional view taken along line VIII-VIII in FIG. 6. [Figure 9] FIG. 7 is a schematic cross-sectional view taken along line IX-IX in FIG. 6. [Figure 10] FIG. 2 is a perspective view showing a schematic view of an electrode body attached to a sealing plate. [Figure 11] 4 is a perspective view that shows a schematic diagram of an electrode assembly to which a positive electrode second current collecting portion and a negative electrode second current collecting portion are attached. FIG. [Figure 12] FIG. 2 is a perspective view illustrating an electrode assembly of the secondary battery according to one embodiment. [Figure 13] FIG. 2 is a front view showing a schematic diagram of an electrode assembly to which a positive electrode second current collecting portion and a negative electrode second current collecting portion are attached. [Figure 14] 14 is a cross-sectional view taken along the line XIV-XIV in FIG. 13. [Figure 15] 11 is a cross-sectional view showing a schematic diagram of a connection portion between a current collector and an electrode body of a secondary battery according to another embodiment. FIG. [Figure 16] 11A to 11C are cross-sectional views illustrating a conventional method for manufacturing an electrode plate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] Hereinafter, an embodiment of the technology disclosed herein will be described with reference to the drawings. It should be noted that matters other than those specifically mentioned in this specification and necessary for implementing the technology disclosed herein (for example, the general configuration and manufacturing process of a battery) can be understood as design matters for a person skilled in the art based on the conventional technology in the field. The technology disclosed herein can be implemented based on the contents disclosed in this specification and the technical common sense in the field. In this specification, the expression "A to B" indicating a range includes the meaning of A or more and B or less, as well as "preferably greater than A" and "preferably smaller than B".
[0025] In this specification, the term "secondary battery" refers generally to an electricity storage device in which a charge / discharge reaction occurs by the movement of charge carriers between a pair of electrodes (positive and negative electrodes) via an electrolyte. Such secondary batteries include so-called storage batteries such as lithium ion secondary batteries, nickel-metal hydride batteries, and nickel-cadmium batteries, as well as capacitors such as electric double layer capacitors.
[0026] 1. Manufacturing method of electrode plate The method for manufacturing an electrode plate disclosed herein manufactures an electrode plate for a secondary battery. Hereinafter, a method for manufacturing an electrode plate (negative electrode plate) on the negative electrode side of a lithium ion secondary battery will be described as one embodiment of the method for manufacturing an electrode plate disclosed herein. FIG. 1 is a flowchart showing a method for manufacturing an electrode plate according to this embodiment. FIG. 2 is a plan view that typically shows a negative electrode plate manufactured by the method for manufacturing an electrode plate according to this embodiment. FIG. 3 is a plan view that explains the method for manufacturing an electrode plate according to this embodiment. FIG. 4 is a cross-sectional view taken along the line IV-IV in FIG. 3. FIG. 5 is a cross-sectional view taken along the line VV in FIG. 2. In addition, the symbol L in FIGS. 2 to 5 indicates the "longitudinal direction" of the negative electrode plate 20 (or the negative electrode precursor 20A), the symbol S indicates the "transverse direction", and the symbol T indicates the "thickness direction".
[0027] As shown in Fig. 1, the method for manufacturing an electrode plate according to this embodiment includes a precursor preparation step S1, an active material application region cutting step S2, and a core exposed region cutting step S3. This produces a negative electrode plate 20 having a configuration as shown in Fig. 2. Below, an overview of the negative electrode plate 20 to be manufactured will be described, and then each step shown in Fig. 1 will be described.
[0028] (1) Overview of the negative electrode plate As shown in FIG. 2, the negative electrode plate 20 is a long strip-shaped member. The negative electrode plate 20 includes a negative electrode core 22, which is a long metal foil, and a negative electrode active material layer 24 applied to the surface of the negative electrode core 22. The negative electrode active material layer 24 is preferably applied to both sides of the negative electrode core 22 (see FIG. 5). This allows a secondary battery with better battery performance to be constructed. In addition, the negative electrode plate 20 in this embodiment includes two regions, an electrode plate main body portion 20b and a negative electrode tab 22t, in a plan view. The electrode plate main body portion 20b is a region where the negative electrode active material layer 24 is applied to the surface of the negative electrode core 22. On the other hand, the negative electrode tab 22t is a portion protruding from the electrode plate main body portion 20b, and includes an exposed region where the negative electrode active material layer 24 is not applied and the negative electrode core 22 is exposed.
[0029] A plurality of negative electrode tabs 22t protrude outward (upward in the short-side direction S in FIG. 2) from the outer edge 20b1 of the electrode plate main body 20b. These plurality of negative electrode tabs 22t are provided at predetermined intervals in the longitudinal direction L of the negative electrode plate 20. In addition, an active material layer-applied region to which the negative electrode active material layer 24 is applied is formed at the base portion of the negative electrode tab 22t adjacent to the electrode plate main body 20b. As will be described in detail later, the negative electrode plate 20 having such a configuration is manufactured by alternately performing the active material-applied region cutting step S2 and the core-exposed region cutting step S3 multiple times. This makes it possible to minimize the laser cutting of the negative electrode core-exposed region A2 (see FIG. 3) from which a large amount of spatter scatters, and therefore the amount of spatter adhering to the negative electrode tab 22t can be further reduced.
[0030] For each member constituting the negative electrode plate 20, materials that can be used in a conventionally known general secondary battery can be used without any particular restrictions. For example, a metal material having a predetermined conductivity is used for the negative electrode core 22. The negative electrode core 22 is preferably made of, for example, copper or a copper alloy. These copper-based materials have suitable conductivity and are inexpensive, and are therefore suitable as materials for the negative electrode core 22. On the other hand, spatter generated from the negative electrode core 22 containing a copper-based material is highly conductive and therefore prone to causing minute internal short circuits. However, according to the manufacturing method of the electrode plate according to this embodiment, it is possible to suppress the spatter generated during laser cutting from adhering to the negative electrode tab 22t. In addition, the negative electrode core 22 may contain a material other than a copper-based material. For example, the negative electrode core 22 may contain a subcomponent such as chromium (Cr). By mixing such a subcomponent with a high melting point into the negative electrode core 22, the amount of spatter scattered during laser cutting can be reduced. The thickness of the negative electrode core 22 is preferably 3 μm to 50 μm, and more preferably 5 μm to 20 μm.
[0031] On the other hand, the negative electrode active material layer 24 is a layer containing a negative electrode active material. A material capable of reversibly absorbing and releasing charge carriers in relation to the positive electrode active material is used for the negative electrode active material. Examples of such negative electrode active materials include carbon materials and silicon-based materials. Examples of carbon materials that can be used include graphite, hard carbon, soft carbon, and amorphous carbon. Also, amorphous carbon-coated graphite, in which the surface of graphite is coated with amorphous carbon, can be used. On the other hand, examples of silicon-based materials include silicon and silicon oxide (silica). Also, the silicon-based material may contain other metal elements (e.g., alkaline earth metals) or their oxides. Also, the negative electrode active material layer 24 may contain additives other than the negative electrode active material. Examples of such additives include binders and thickeners. Specific examples of binders include rubber-based binders such as styrene butadiene rubber (SBR). Also, specific examples of thickeners include carboxymethyl cellulose (CMC). The thickness of the negative electrode active material layer 24 is preferably from 10 μm to 500 μm, more preferably from 30 μm to 400 μm, and further preferably from 50 μm to 300 μm.
[0032] The negative electrode plate 20 having the above-mentioned configuration is manufactured by carrying out a precursor preparation step S1, an active material applied region cutting step S2, and a substrate exposed region cutting step S3 shown in Fig. 1. Each step will be described below.
[0033] (2) Precursor preparation step S1 In this step, an electrode precursor, which is a precursor of an electrode plate, is prepared. The electrode precursor shown in FIG. 3 is a precursor of a negative electrode plate (negative electrode precursor 20A). This negative electrode precursor 20A includes a negative electrode core 22 that is a strip-shaped metal foil. The area of the negative electrode core 22 of this negative electrode precursor 20A is larger than the area of the manufactured negative electrode plate 20 (see FIG. 2). A negative electrode active material layer 24 is applied to the surface of the negative electrode core 22. The negative electrode active material layer 24 is applied to the center of the negative electrode core 22 in the short side direction S so as to extend along the longitudinal direction L. In this specification, the region to which the negative electrode active material layer 24 is applied is referred to as a "negative electrode active material applied region A1". On the other hand, the negative electrode active material layer 24 is not applied to both side edge portions (regions on both outer sides of the negative electrode active material layer 24 in the short side direction S) of the negative electrode precursor 20A, and the negative electrode core 22 is exposed. In this specification, the region where the negative electrode core 22 is exposed is referred to as the "negative electrode core exposed region A2". The means for preparing the negative electrode precursor 20A having the above configuration is not particularly limited, and various conventionally known methods can be adopted without particular limitation. For example, the negative electrode precursor 20A can be prepared by applying a raw material paste containing a negative electrode active material and the like to the surface of the negative electrode core 22 and then drying it. In addition, this process is not particularly limited as long as the negative electrode precursor 20A can be prepared. For example, the negative electrode precursor 20A having the above configuration may be purchased and prepared. Note that the negative electrode precursor is not limited to the structure shown in FIG. 2 as long as it has a negative electrode active material imparted region and a negative electrode core exposed region. For example, the negative electrode precursor may adopt a structure in which the negative electrode core exposed region is formed only on one side edge portion.
[0034] (3) Active material application area cutting step S2 The method for manufacturing an electrode plate according to this embodiment includes an active material-applied region cutting step S2 in which the negative electrode active material-applied region A1 of the negative electrode precursor 20A is cut by a laser. N1 3, the laser is scanned over the negative electrode active material applied region A1 along the side edge portion A1a of the negative electrode active material applied region A1. This makes it possible to more effectively prevent spatter from adhering to the negative electrode plate 20 after manufacture. Specifically, while the negative electrode active material applied region A1 is being laser-cut as in this step, the negative electrode active material layer 24 acts as a wall to block the spatter, so that the spatter is less likely to scatter onto the surface side of the negative electrode plate 20. Meanwhile, in the core-exposed region cutting step S3 (dotted line L in FIG. 3) described later, N2 ), since there is no negative electrode active material layer 24 serving as a wall, spatters tend to scatter to the surface side of the negative electrode plate 20. That is, as shown in FIG. 3, N2 ) and active material application area cutting step S2 (dotted line L N1 ) is alternately performed, laser cutting of the negative electrode substrate exposed region A2 can be kept to a minimum, and the amount of spatter scattering itself can be significantly reduced. In addition, the side edge portion A1a of the negative electrode active material applied region A1 is prone to have a non-uniform thickness of the negative electrode active material layer 24. In contrast, when the active material applied region cutting step S2 is performed, the side edge portion A1a of the negative electrode active material applied region A1 is cut off, which contributes to the manufacture of a negative electrode plate 20 in which the thickness of the negative electrode active material layer 24 is uniform.
[0035] (4) Core exposed area cutting process S3 In the core exposed region cutting step S3, the negative electrode core exposed region A2 of the negative electrode precursor 20A is cut with a laser to form the negative electrode tab 22t. N22, a laser is scanned along the short side direction S of the negative electrode precursor 20A from the negative electrode active material applied region A1 toward the negative electrode core exposed region A2. Then, after the laser is scanned a fixed distance along the longitudinal direction L of the negative electrode precursor 20A in the negative electrode core exposed region A2, the pulsed laser is scanned again along the short side direction S toward the negative electrode active material applied region A1. As a result, a part of the negative electrode core exposed region A2 is cut out in a convex shape to form the negative electrode tab 22t (see FIG. 2). Then, as described above, in the manufacturing method according to this embodiment, the active material applied region cutting step S2 (dotted line L N1 ) and the core exposed region cutting process S3 (dotted line L N2 ) is repeated at regular intervals. This makes it possible to cut out the side edge portion A1a of the negative electrode active material-applied region A1 and to cut out a plurality of negative electrode tabs 22t.
[0036] Here, as shown in FIG. 4, the negative electrode core 22 used in this embodiment has a first surface 22a and a second surface 22b opposite to the first surface 22a and having a smaller surface roughness than the first surface 22a. In the manufacturing method according to this embodiment, in the core exposed region cutting step S3, the second surface 22b having a relatively smaller surface roughness is set as a laser non-irradiated surface, and the first surface 22a is irradiated with the laser L. This makes it possible to reduce the number of spatters Sp adhering to the negative electrode tab 22t of the negative electrode plate 20 after manufacture. Hereinafter, the reason why the manufacturing method of the electrode plate according to this embodiment can reduce the number of spatters is described in comparison with the conventional manufacturing method of the electrode plate (see FIG. 16).
[0037] First, as shown in FIG. 16, in the manufacture of an electrode plate, the second surface 122b, which is the surface on the side with a smaller surface roughness, may become the laser irradiated surface, and the first surface 122a, which is the surface on the side with a larger surface roughness, may become the laser irradiated surface. When the negative electrode core exposed region A2 (negative electrode core 122) is cut by laser in this state, it is presumed that a large amount of spatter Sp adheres to both the first surface 122a and the second surface 122b of the negative electrode core 122 by the following mechanism. First, when the negative electrode core exposed region A2 is irradiated with a laser, the negative electrode core exposed region A2 is slightly bent so that the second surface 122b, which is the laser irradiated surface, becomes concave. Then, the molten negative electrode core 122 scatters as spatter Sp. At this time, since the second surface 122b has a concave shape, it is in a state where the scattered spatter Sp is easily attached. Therefore, the amount of spatter Sp attached is not easily affected by the surface roughness of the second surface 122b. On the other hand, as a result of the bending of the negative electrode core exposed region A2, the first surface 122a has a convex shape, so that the scattered spatter Sp is less likely to adhere to the first surface 122a, but if the surface roughness is large, the scattered spatter Sp is more likely to adhere to the first surface 122a due to the unevenness of the surface. Therefore, if the surface roughness of the first surface 122a, which is the non-laser irradiated surface, is large, the amount of spatter Sp adhering to the negative electrode plate (typically the negative electrode tab 122t) after cutting increases.
[0038] In contrast, in the manufacturing method according to the present embodiment, as shown in FIG. 4, in the core exposed region cutting step S3, the second surface 22b with a small surface roughness is set as a laser non-irradiated surface, and the first surface 22a is irradiated with the laser L. In other words, the manufacturing method according to the present embodiment includes a step of checking the surface roughness of both surfaces of the negative electrode core 22 and a step of irradiating the first surface 22a with the laser L. This makes it possible to prevent the scattering sputter Sp from being collected by the negative electrode core 22. On the other hand, in the manufacturing method according to the present embodiment, the first surface 22a, which is the surface with a large surface roughness, is disposed on the laser irradiated surface to which the sputter is likely to adhere, regardless of the magnitude of the surface roughness. This makes it possible to manufacture a negative electrode core 22 in which the amount of sputter adhesion on the second surface 22b with a relatively small surface roughness is significantly reduced.
[0039] In addition, as the surface roughness of the second surface 22b of the negative electrode core 22 decreases, the amount of spatter Sp attached to the second surface 22b tends to decrease. From this viewpoint, the maximum height Sz of the second surface 22b is preferably 2.5 μm or less, more preferably 2.0 μm or less, more preferably 1.8 μm or less, and particularly preferably 1.4 μm or less. On the other hand, from the viewpoint of reducing the amount of spatter attachment, the lower limit of the maximum height Sz of the second surface 22b is not particularly limited, and may be 0.7 μm or more, 0.9 μm or more, or 1.0 μm or more. In this specification, the "maximum height Sz" is measured in accordance with ISO25178 and is the sum of the maximum peak height Sp and the maximum valley depth Sv in the surface roughness measurement of the negative electrode core.
[0040] From the viewpoint of reducing the amount of sputter Sp attached to the second surface 22b, the average roughness Sa of the negative electrode core 22 is preferably 0.25 μm or less, more preferably 0.2 μm or less, more preferably 0.18 μm or less, and particularly preferably 0.14 μm or less. On the other hand, the lower limit of the average roughness Sa of the second surface 22b is not particularly limited, and may be 0.07 μm or more, 0.09 μm or more, or 0.1 μm or more. Note that the "average roughness Sa" in this specification is also measured in accordance with ISO25178.
[0041] On the other hand, as described above, since the first surface 22a is a laser irradiated surface, a certain amount of spatter adheres thereto without being affected by the surface roughness. Therefore, from the viewpoint of reducing the amount of spatter adhesion, the surface roughness of the first surface 22a is not particularly limited. For example, the maximum height Sz of the first surface 22a may be 3 μm or less, 2.5 μm or less, or 1.8 μm or less. On the other hand, the lower limit of the maximum height Sz of the first surface 22a may be 1 μm or more, 1.25 μm or more, or 1.5 μm or more. In addition, the average roughness Sa of the first surface 22a may be 0.3 μm or less, 0.25 μm or less, or 0.18 μm or less. In addition, the average roughness Sa of the first surface 22a may be 0.1 μm or more, or 0.14 μm or more.
[0042] The type of laser used in the manufacturing method of the electrode plate disclosed herein is not particularly limited, and any conventionally known laser that can be used to cut the electrode precursor can be used without any particular limitation. Examples of this type of laser include a continuous wave laser (CW laser) and a pulsed laser. Among these, the pulsed laser can apply a large amount of energy in a short time width in a concentrated manner (high peak output), so that the negative electrode precursor 20A can be cut quickly and contribute to improving manufacturing efficiency. On the other hand, the pulsed laser causes a large impact during laser irradiation, which can also cause an increase in the amount of spatter scattering when cutting the negative electrode core 22. However, according to the manufacturing method of this embodiment, even if the amount of spatter scattering increases, the amount of spatter adhesion to the negative electrode tab 22t can be sufficiently reduced, so that the problems caused by using the pulsed laser can be suitably solved.
[0043] In addition, the laser irradiation conditions in the technology disclosed herein are not particularly limited, and are preferably adjusted appropriately depending on the type of laser and the structure of the negative electrode precursor 20A (typically, the thickness and material of the negative electrode active material layer 24 and the negative electrode core 22). As an example, when a pulsed laser is used, it is preferable to reduce the repetition frequency. This reduces the number of laser irradiations, so that the amount of sputtering can be reduced. From this viewpoint, the frequency of the pulsed laser is preferably 1000 KHz or less, and more preferably 800 KHz or less. On the other hand, if the frequency of the pulsed laser is increased, it is possible to apply a large amount of energy in a short time width in a concentrated manner, which can contribute to improving the manufacturing efficiency. From this viewpoint, the frequency of the pulsed laser is preferably 50 KHz or more, and more preferably 80 KHz or more.
[0044] In addition, when a pulse laser is used, the average output is preferably 50 W or more, more preferably 80 W or more, and particularly preferably 95 W or more. As the average output of the pulse laser increases, the cutting of the negative electrode precursor 20A tends to become easier. On the other hand, the average output of the pulse laser is preferably 500 W or less, more preferably 300 W or less, and particularly preferably 285 W or less. As the average output of the pulse laser decreases, the impact during laser irradiation decreases, so the amount of sputtering tends to decrease. In addition, when a pulse laser is used, the pulse width is preferably 30 ns or more, more preferably 50 ns or more, and particularly preferably 60 ns or more. As the pulse width increases, the time for heating the negative electrode precursor 20A increases, so the cutting of the negative electrode precursor 20A tends to become easier. On the other hand, the pulse width of the pulse laser is preferably 300 ns or less, more preferably 200 ns or less, even more preferably 150 ns or less, and particularly preferably 120 ns or less. As the pulse width becomes smaller, the amount of melted negative electrode substrate 22 decreases, and therefore the amount of scattered sputtering tends to decrease.
[0045] Moreover, the spot diameter of the pulse laser is preferably 10 μm to 60 μm, more preferably 20 μm to 50 μm, and further preferably 25 μm to 40 μm. This allows negative electrode plate 20 to be easily cut out from negative electrode precursor 20A. Furthermore, the scanning speed of the pulse laser is preferably 5000 mm / sec or less, and more preferably 3000 mm / sec or less. By slowing down the scanning speed in this manner, cutting defects of negative electrode core 22 can be suppressed. On the other hand, the lower limit of the scanning speed of the pulse laser is not particularly limited, and may be 20 mm / sec or more. From the viewpoint of improving manufacturing efficiency by shortening the cutting time, the lower limit of the scanning speed of the pulse laser is preferably 200 mm / sec or more, and more preferably 500 mm / sec or more.
[0046] (5) Other processes As described above, in the manufacturing method according to the present embodiment, the active material application region cutting step S2 (dotted line L in FIG. 3) N1 ), and a core-exposed region cutting process S3 (dotted line L in FIG. 3 ). N23.) is repeated at regular intervals to cut off the side edge portion A1a of the negative electrode active material application region A1 and form a plurality of negative electrode tabs 22t. N3 As shown in FIG. 2, the center of the negative electrode precursor 20A in the short-side direction S is cut along the long-side direction L. This makes it possible to produce a negative electrode plate 20 in which a negative electrode tab 22t is formed only on one side of the outer edge 20b1 of the electrode plate main body 20b, as shown in FIG. 2. N4 As shown in FIG. 1, negative electrode precursor 20A is cut in short direction S at a predetermined interval in length direction L. This allows negative electrode plate 20 of a desired length to be manufactured. N3 , L N4 In cutting negative electrode precursor 20A along these two-dot chain lines L, a cutting blade, a mold, a cutter, or the like may be used instead of laser cutting. N3 , L N4 The cutting along the line may be appropriately performed according to the shape of the negative electrode plate after production, and is not limited to the technology disclosed herein.
[0047] 2. Structure of the negative electrode plate Next, a detailed structure of the electrode plate (negative electrode plate 20) manufactured by the electrode plate manufacturing method according to this embodiment will be described.
[0048] 2, the negative electrode plate 20 according to this embodiment includes a negative electrode core 22 and a negative electrode active material layer 24. The negative electrode plate 20 also includes an electrode plate main body 20b, which is a region where the negative electrode active material layer 24 is applied to the surface of the negative electrode core 22, and a negative electrode tab 22t, which protrudes from the electrode plate main body 20b, where the negative electrode active material layer 24 is not applied, and includes an exposed region where the negative electrode core 22 is exposed. These have already been described, so duplicated description will be omitted.
[0049] Moreover, each of the negative electrode tabs 22t of the negative electrode plate 20 according to this embodiment includes an active material layer applied region in which the negative electrode active material layer 24 is applied to the base portion of the negative electrode tab 22t adjacent to the plate body portion 20b. This active material layer applied region is formed by manufacturing the negative electrode plate 20 by repeating the active material applied region cutting step S2 and the core exposed region cutting step S3 as described above. In addition, although not shown, in the negative electrode plate 20 according to this embodiment, a modified material fixed region in which a modified material of the negative electrode active material layer 24 is fixed on the negative electrode core 22 may be formed on the outer edge portion 20b1 of the plate body portion 20b. This modified material fixed region may be formed by blowing off a part of the negative electrode active material layer 24 by the impact of the laser in the active material applied region cutting step S2 and thermally modifying the negative electrode active material layer 24 by the heat of the laser. As described above, in this embodiment, the first surface (the surface of the negative electrode core 22 on the side where the surface roughness is relatively rough) of the negative electrode precursor 20A is the laser irradiated surface, and therefore, in the manufactured negative electrode plate 20, the width of the modified substance adhered region on the first surface can be larger than the width of the modified substance adhered region on the second surface. In this embodiment, the surface roughness of the first surface 22a (laser irradiated surface) of the negative electrode core 22 is larger than that of the second surface 22b (laser non-irradiated surface), and therefore, an effect is also exhibited that the modified substance adhered in large amounts to the first surface 22a is less likely to detach from the negative electrode core 22. In addition, the thickness of the modified substance layer in the modified substance adhered region is preferably smaller than the thickness of the negative electrode active material layer 24.
[0050] As shown in FIG. 5, the negative electrode core 22 of the negative electrode plate 20 according to this embodiment has a first surface 22a with a relatively large surface roughness and a second surface 22b with a relatively small surface roughness. As described above, in the manufacturing method according to this embodiment, laser cutting is performed so that the second surface 22b with a relatively small surface roughness becomes the laser non-irradiated surface. Therefore, in the negative electrode tab 22t (exposed negative electrode core 22) of the negative electrode plate 20 after manufacturing, the number of metal particles (spatter) attached to the second surface 22b is smaller than the number of metal particles attached to the first surface 22a. By using such a negative electrode plate 20, it is possible to prevent the spatter from coming off inside the secondary battery and causing a minute internal short circuit.
[0051] The specific number of metal particles (sputters) attached on each surface of the negative electrode tab 22t is not particularly limited. For example, the number of sputters attached on the first surface 22a is 20 particles / cm. 2 More than 25 pieces / cm is acceptable. 2 More than 30 pieces / cm is acceptable. 2 On the other hand, the number of sputter deposits on the first surface 22a is 200 / cm 2 Less than 150 pieces / cm is preferable. 2 Less than 100 pieces / cm is more preferable. 2 More preferably, 80 pieces / cm 2 On the other hand, the number of sputter deposits on the second surface 22b is 0 / cm 2 (no spatter attached) is acceptable, 1 piece / cm 2 More than 2 pieces / cm is acceptable. 2 On the other hand, the number of sputter deposits on the second surface 22b is 50 / cm 2 Less than 45 pieces / cm is preferable. 2 Less than 40 pieces / cm is more preferable. 2 The following is particularly preferred. The sputter adhesion ratio of the second surface 22b to the first surface 22a is preferably 1 / 2 or less, more preferably 1 / 3 or less, even more preferably 1 / 4 or less, and particularly preferably 1 / 5 or less. The "number of sputter adhesions" is the number of metal particles with a particle diameter of 5 μm or more confirmed by microscopic observation. The shape of the sputter is not limited to spherical, and may be elliptical, rod-like, needle-like, plate-like, etc. When such non-spherical sputters are confirmed, the number of metal particles with a maximum particle diameter of 5 μm or more, which is the largest dimension, is counted as the number of sputter adhesions.
[0052] 3. Secondary battery Next, a secondary battery produced using the negative electrode plate 20 according to this embodiment will be described. FIG. 6 is a perspective view showing the secondary battery according to this embodiment. FIG. 7 is a schematic longitudinal sectional view taken along line VII-VII in FIG. 6. FIG. 8 is a schematic longitudinal sectional view taken along line VIII-VIII in FIG. 6. FIG. 9 is a schematic transverse sectional view taken along line IX-IX in FIG. 6. FIG. 10 is a perspective view showing an electrode body attached to a sealing plate. FIG. 11 is a perspective view showing an electrode body to which a positive electrode second current collector and a negative electrode second current collector are attached. FIG. 12 is a perspective view showing an electrode body of a secondary battery according to this embodiment. FIG. 13 is a front view showing an electrode body to which a positive electrode second current collector and a negative electrode second current collector are attached. FIG. 14 is a cross-sectional view taken along line XIV-XIV in FIG. 13. 6 to 14, the symbol X indicates the "thickness direction" of the secondary battery 100, the symbol Y indicates the "width direction", and the symbol Z indicates the "up-down direction". In the thickness direction X, F indicates the "front", and Rr indicates the "rear". In the width direction Y, L indicates the "left", and R indicates the "right". In the up-down direction Z, U indicates the "up" and "D" indicates the "down". However, these directions are determined for the convenience of explanation, and are not intended to limit the installation form of the secondary battery 100.
[0053] As shown in Figs. 6 to 9, the secondary battery 100 according to this embodiment includes an electrode assembly 40, a battery case 50, a positive electrode terminal 60, a negative electrode terminal 65, a positive electrode current collector 70, and a negative electrode current collector 75. Although not shown, the battery case 50 of the secondary battery 100 also contains a non-aqueous electrolyte in addition to the electrode assembly 40. The non-aqueous electrolyte is prepared by dissolving a supporting salt in a non-aqueous solvent. Examples of the non-aqueous solvent include carbonate-based solvents such as ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate. Examples of the supporting salt include fluorine-containing lithium salts such as LiPF6.
[0054] (1) Battery case The battery case 50 is a housing that houses the electrode assembly 40. The battery case 50 in this embodiment has a flat, bottomed rectangular parallelepiped (rectangular) outer shape. The material of the battery case 50 may be the same as that conventionally used, and is not particularly limited. The battery case 50 is preferably made of metal, and more preferably made of, for example, aluminum, an aluminum alloy, iron, an iron alloy, or the like. The battery case 50 includes an exterior body 52 and a sealing plate 54.
[0055] The exterior body 52 is a flat, bottomed, rectangular container having an opening 52h on the upper surface. As shown in FIG. 6, the exterior body 52 includes a bottom wall 52a having a substantially rectangular shape in plan view, a pair of long side walls 52b extending in the vertical direction Z from the long side of the bottom wall 52a, and a pair of short side walls 52c extending in the vertical direction Z from the short side of the bottom wall 52a. On the other hand, the sealing plate 54 is a substantially rectangular plate-like member in plan view that closes the opening 52h of the exterior body 52. The outer periphery of the sealing plate 54 is joined (for example, welded) to the outer periphery of the opening 52h of the exterior body 52. This produces a battery case 50 whose inside is hermetically sealed (closed). The sealing plate 54 is also provided with a liquid injection hole 55 and a gas exhaust valve 57. The liquid injection hole 55 is provided for injecting a nonaqueous electrolyte into the battery case 50 after the exterior body 52 and the sealing plate 54 are joined together. After the nonaqueous electrolyte is injected into the secondary battery 100, the injection hole 55 is sealed with a sealing member 56. The gas exhaust valve 57 is a thin-walled portion designed to break (open) at a predetermined pressure to exhaust the gas inside the battery case 50 when a large amount of gas is generated inside the battery case 50.
[0056] (2) Electrode terminal A positive electrode terminal 60 is attached to one end (left side in Figs. 6 and 7) of the sealing plate 54 in the long side direction Y of the secondary battery 100. The positive electrode terminal 60 is connected to a plate-shaped positive electrode external conductive member 62 on the outside of the battery case 50. Meanwhile, a negative electrode terminal 65 is attached to the other end (right side in Figs. 6 and 7) of the sealing plate 54 in the long side direction Y of the secondary battery 100. A plate-shaped negative electrode external conductive member 67 is also attached to the negative electrode terminal 65. These external conductive members (positive electrode external conductive member 62 and negative electrode external conductive member 67) are connected to other secondary batteries and external devices via external connection members (bus bars, etc.). The external conductive members are preferably made of a metal with excellent conductivity (aluminum, aluminum alloy, copper, copper alloy, etc.).
[0057] (3) Electrode current collector In the secondary battery 100, a plurality of electrode bodies 40 (three in the figure) are accommodated inside the battery case 50. The positive electrode terminal 60 is connected to each of the plurality of electrode bodies 40 via a positive electrode current collector 70 accommodated inside the battery case 50. Specifically, the positive electrode current collector 70 that connects the positive electrode terminal 60 and the electrode body 40 is accommodated inside the battery case 50. As shown in FIG. 7, the positive electrode current collector 70 includes a positive electrode first current collector 71 that is a plate-shaped conductive member extending along the inner side surface of the sealing plate 54, and a plurality of positive electrode second current collectors 72 that are plate-shaped conductive members extending along the up-down direction Z. The lower end 60c of the positive electrode terminal 60 extends toward the inside of the battery case 50 through the terminal insertion hole 58 of the sealing plate 54 and is connected to the positive electrode first current collector 71 (see FIG. 7). On the other hand, the positive electrode second current collecting part 72 is connected to the positive electrode tab group 42 of the electrode body 40. The connection between the positive electrode second current collecting part 72 and the positive electrode tab group 42 is made by ultrasonic welding, resistance welding, laser welding, or the like, and a first joint part 72a is formed at the connection part (see FIG. 13). In consideration of the jointability with the positive electrode tab group 42, the positive electrode second current collecting part 72 is preferably made of the same material (e.g., aluminum, aluminum alloy, etc.) as the positive electrode core body 12. As shown in FIG. 9, the positive electrode tab group 42 of the electrode body 40 is bent so that the positive electrode second current collecting part 72 and one side surface 40a of the electrode body 40 face each other. As a result, the upper end part of the positive electrode second current collecting part 72 and the positive electrode first current collecting part 71 are electrically connected.
[0058] On the other hand, the negative electrode terminal 65 is connected to each of the plurality of electrode bodies 40 via a negative electrode current collector 75 housed in the battery case 50. The connection structure on the negative electrode side is substantially the same as the connection structure on the positive electrode side described above. Specifically, the negative electrode current collector 75 includes a negative electrode first current collector 76 which is a plate-shaped conductive member extending along the inner side surface of the sealing plate 54, and a plurality of negative electrode second current collectors 77 which are plate-shaped conductive members extending along the up-down direction Z. The lower end 65c of the negative electrode terminal 65 extends into the battery case 50 through the terminal insertion hole 59 and is connected to the negative electrode first current collector 76 (see FIG. 7). The negative electrode second current collector 77 is connected to the negative electrode tab group 44 of the electrode body 40. For the connection between the negative electrode second current collector 77 and the negative electrode tab group 44, ultrasonic bonding, resistance welding, laser welding, or the like is preferably used. A second joint portion 77a is formed at the connection portion between the negative electrode second current collecting portion 77 and the negative electrode tab group 44 (see FIG. 13). In consideration of the joint with the negative electrode tab group 44, the negative electrode second current collecting portion 77 is preferably made of the same material (e.g., copper, copper alloy, etc.) as the negative electrode core 22. The negative electrode tab group 44 is bent so that the negative electrode second current collecting portion 77 and the other side surface 40b of the electrode body 40 face each other (see FIG. 9). This electrically connects the upper end portion of the negative electrode second current collecting portion 77 and the negative electrode first current collecting portion 76.
[0059] (4) Insulating materials In addition, in the secondary battery 100 according to this embodiment, various insulating members are attached to prevent electrical conduction between the electrode body 40 and the battery case 50. Specifically, an external insulating member 92 is interposed between the positive electrode external conductive member 62 (negative electrode external conductive member 67) and the outer surface of the sealing plate 54 (see FIG. 6). This can prevent the positive electrode external conductive member 62 and the negative electrode external conductive member 67 from being electrically connected to the sealing plate 54. Also, a gasket 90 is attached to each of the terminal insertion holes 58, 59 of the sealing plate 54 (see FIG. 7). This can prevent the positive electrode terminal 60 (or the negative electrode terminal 65) inserted into the terminal insertion holes 58, 59 from being electrically connected to the sealing plate 54. Also, an internal insulating member 94 is disposed between the positive electrode first current collecting portion 71 (or the negative electrode first current collecting portion 76) and the inner surface of the sealing plate 54. The internal insulating member 94 includes a plate-shaped base portion 94a interposed between the positive electrode first current collecting portion 71 (or the negative electrode first current collecting portion 76) and the inner surface of the sealing plate 54. This can prevent the positive electrode first current collecting portion 71 or the negative electrode first current collecting portion 76 from being electrically connected to the sealing plate 54. Furthermore, the internal insulating member 94 includes a protruding portion 94b protruding from the inner surface of the sealing plate 54 toward the electrode body 40. This can restrict the movement of the electrode body 40 in the vertical direction Z, and can prevent the electrode body 40 and the sealing plate 54 from coming into direct contact with each other. In addition, the electrode body 40 is accommodated inside the battery case 50 while being covered with an electrode body holder 98 (see FIG. 8) made of an insulating resin sheet. This can prevent the electrode body 40 and the exterior body 52 from coming into direct contact with each other. The material of each of the insulating members described above is not particularly limited as long as it has a predetermined insulating property. As an example, synthetic resin materials such as polyolefin resins (eg, polypropylene (PP), polyethylene (PE)), fluorine resins (eg, perfluoroalkoxyalkane (PFA), polytetrafluoroethylene (PTFE)), etc. can be used.
[0060] (5) Electrode body The electrode body includes a positive electrode plate 10 and a negative electrode plate 20. As shown in FIG. 12, the electrode body 40 in this embodiment is a wound electrode body. In such a wound electrode body, a pair of electrode plates (positive electrode plate 10, negative electrode plate 20) are wound in a state in which they face each other with a separator 30 interposed therebetween. When producing this electrode body 40, first, a laminate is formed by laminating a long strip-shaped positive electrode plate 10 and a long strip-shaped negative electrode plate 20 with a long strip-shaped separator 30 interposed therebetween. Then, after this laminate is wound in the longitudinal direction, a stop tape 38 (see FIG. 13) is attached to the end portion 30a of the separator 30 arranged on the outermost periphery. Hereinafter, each member constituting the electrode body 40 will be described.
[0061] (a) Separator First, the separator 30 is a sheet-like member having a function of preventing contact between the positive electrode plate 10 and the negative electrode plate 20 and allowing charge carriers to pass through. An example of such a separator 30 is a resin sheet having a plurality of fine holes formed therein through which charge carriers can pass. Such a resin sheet preferably includes a resin layer made of a polyolefin resin (e.g., polyethylene (PE), polypropylene (PP)). In addition, a heat-resistant layer containing an inorganic filler such as alumina, boehmite, aluminum hydroxide, or titania may be formed on the surface of the resin sheet.
[0062] (b) Positive electrode plate The positive electrode plate 10 includes a positive electrode core 12, which is a foil-shaped metal member, a positive electrode active material layer 14 provided on the surface of the positive electrode core 12, and a protective layer 16 provided on the surface of the positive electrode core 12 so as to be adjacent to the side edge portion 10a of the positive electrode plate 10. A metal material having a predetermined electrical conductivity is used for the positive electrode core 12. For example, aluminum, an aluminum alloy, stainless steel, etc. may be used for the positive electrode core 12. In addition, a plurality of positive electrode tabs 12t protruding toward the outside in the short direction S (the left side in FIG. 12) are provided at a predetermined interval in the longitudinal direction L of the positive electrode plate 10 on the side edge portion 10a of the positive electrode plate 10. The positive electrode tabs 12t are not provided with the positive electrode active material layer 14 or the protective layer 16, and are an area where the positive electrode core 12 is exposed. Then, in the electrode body 40 after winding, a positive electrode tab group 42 is formed in which a plurality of positive electrode tabs 12t are stacked. As described above, the positive electrode tab group 42 is connected to the positive electrode second current collecting portion 72 (see FIG. 13). From the viewpoint of battery performance, the positive electrode active material layer 14 and the protective layer 16 are preferably provided on both sides of the positive electrode core 12. The protective layer 16 may be provided so that a part of it covers the side edge portion of the positive electrode active material layer 14. The materials for the positive electrode active material layer 14 and the protective layer 16 can be any conventionally known material that can be used in general secondary batteries (for example, lithium ion secondary batteries) without any particular restrictions, and detailed description thereof will be omitted as they do not limit the technology disclosed herein.
[0063] (c) Negative electrode plate On the other hand, the negative electrode plate 20 according to the present embodiment is used in this secondary battery 100. As described above, in the manufacturing method of the electrode plate according to the present embodiment, when cutting the negative electrode core exposed region A2 (negative electrode core 22) of the negative electrode precursor 20A, the second surface 22b having a relatively small surface roughness is used as the laser non-irradiated surface, and the first surface 22a having a relatively large surface roughness is used as the laser irradiated surface. Therefore, in the manufactured negative electrode plate 20, the amount of spatter attached to the negative electrode tab 22t is reduced. By using such a negative electrode plate 20, it is possible to prevent the spatter from detaching from the negative electrode tab 22t inside the secondary battery 100 and causing a small internal short circuit.
[0064] By winding a laminate including the positive electrode plate 10, the negative electrode plate 20, and the separator 30 configured as described above, an electrode body 40 having a core portion 46 in which the positive electrode active material layer 14 and the negative electrode active material layer 24 face each other via the separator 30 is formed (see FIG. 13). Then, as shown in FIGS. 12 and 13, in the electrode body 40 after winding, a negative electrode tab group 44 in which a plurality of negative electrode tabs 22t are laminated is formed. In this embodiment, the interval between the negative electrode tabs 22t in the longitudinal direction L of the negative electrode plate 20 is set so that one negative electrode tab 22t is laminated each time the negative electrode plate 20 is wound once. As a result, in the electrode body 40 after winding, as shown in FIG. 14, the first surface 22a of the negative electrode tab 22t (negative electrode core 22) is arranged on one surface 44a of the negative electrode tab group 44, and the second surface 22b of the negative electrode tab 22t (negative electrode core 22) is arranged on the other surface 44b. When such a negative electrode tab 22t is formed, it is preferable to connect the negative electrode second current collecting part 77 to the surface 44a on which the first surface 22a of the negative electrode core 22 is arranged, and to arrange the second surface 22b of the negative electrode core 22 (negative electrode tab 22t) on the other surface 44b not connected to the negative electrode second current collecting part 77. This makes it possible to encapsulate the first surface 22a, which has a large amount of spatter attached, between the negative electrode tab 22t and the negative electrode second current collecting part 77 (or between a plurality of negative electrode tabs 22t), so that detachment of the spatter from the negative electrode plate 20 can be more suitably suppressed. The technology disclosed herein does not limit the position of the first surface 22a of the negative electrode tab 22t in the negative electrode tab group 44. According to the technology disclosed herein, the total amount of spatter adhering to the negative electrode tab 22t can be reduced, and therefore even when the first surface 22a is disposed on the other surface 44b that is not connected to the negative electrode second current collecting portion 77, the amount of spatter detached from the negative electrode tab 22t can be reduced compared to the conventional technology.
[0065] 4. Other embodiments An embodiment of the technology disclosed herein has been described above. Note that the above embodiment shows an example to which the technology disclosed herein is applied, and does not limit the technology disclosed herein.
[0066] For example, in the above-mentioned embodiment, the target of the technology disclosed herein is a negative electrode plate. However, the target of the technology disclosed herein is not limited to a negative electrode plate, and may be a positive electrode plate. Even when such a positive electrode plate is the manufacturing target, the number of sputters adhering to the electrode plate (positive electrode plate) after manufacturing can be reduced.
[0067] The structure of the electrode body is not a factor that limits the technology disclosed herein. For example, the electrode body 40 in the above-mentioned embodiment adopts a configuration in which one negative electrode tab 22t is laminated each time the negative electrode plate 20 is wound once. However, the configuration of the electrode body is not particularly limited, and a configuration in which two negative electrode tabs are laminated each time the negative electrode plate is wound once can also be adopted. In this case, as shown in FIG. 15, it is preferable to adjust the winding direction of the negative electrode plate 20 so that the first surface 22a of the negative electrode tab 22t (negative electrode core body 22) is disposed on the inside in the width direction Y. This allows the first surface 22a, which has a large amount of sputter adhesion, to be enclosed between the negative electrode tabs 22t.
[0068] In the above-mentioned embodiment, a wound electrode body is used as the electrode body. However, the electrode body is not limited to a wound electrode body as long as it includes a positive electrode plate and a negative electrode plate. Another example of the structure of the electrode body is a laminated electrode body in which a plurality of positive electrode plates and negative electrode plates are sequentially laminated with a separator interposed therebetween. To manufacture a negative electrode plate for this type of laminated electrode body, a two-dot chain line L in FIG. N4 It is advisable to perform cutting along the short direction S as shown in for each negative electrode tab 22t. Although detailed explanation is omitted, the positive electrode plate is also produced in the same manner. Then, multiple positive electrode plates and multiple negative electrode plates are sequentially laminated with separators interposed therebetween so that the positive electrode tabs are laminated in the same position and the negative electrode tabs of the negative electrode plates are laminated in the same position. In this way, a laminated electrode body can be produced.
[0069] Moreover, the above-mentioned embodiment is directed to a high-capacity secondary battery 100 in which three electrode bodies 40 are housed inside a battery case 50. However, the number of electrode bodies housed in one battery case is not particularly limited, and may be two or more (plural), or may be one. Furthermore, the secondary battery 100 according to the above-mentioned embodiment is a lithium-ion secondary battery in which lithium ions are charge carriers. However, the secondary battery disclosed herein is not limited to a lithium-ion secondary battery. In the manufacturing process of other secondary batteries (such as nickel-metal hydride batteries), a process of cutting the active material-imparted region and the core-exposed region of the electrode precursor with a laser is also present, and therefore the technology disclosed herein can be applied without particular limitations.
[0070] Moreover, the secondary battery 100 according to the above embodiment is a non-aqueous electrolyte secondary battery using a non-aqueous electrolyte as an electrolyte. However, the technology disclosed herein can also be applied to batteries other than non-aqueous electrolyte secondary batteries. Another example of the structure of a secondary battery is an all-solid-state battery. In this all-solid-state battery, a solid electrolyte layer formed from a solid electrolyte in a sheet shape is used as a separator interposed between a positive electrode plate and a negative electrode plate. In this all-solid-state battery, the separator and the electrolyte are integrated and contained inside the electrode body, so that leakage of the electrolyte can be prevented. In the manufacturing process of this type of all-solid-state battery, a process of cutting the core-exposed region of the electrode precursor with a laser is present, so that the technology disclosed herein can be applied without any particular restrictions.
[0071] [Test example] Test examples relating to the present invention will be described below. Note that the contents of the test examples described below are not intended to limit the present invention.
[0072] 1. Sample Preparation Example 1 In Example 1, a negative electrode for a lithium ion secondary battery was manufactured by laser cutting the negative electrode active material-imparted region and the core-exposed region of the negative electrode precursor. First, a negative electrode precursor was prepared in which a negative electrode active material layer of 80 μm was imparted to both sides of a negative electrode core (copper foil) of 8 μm in thickness. The negative electrode active material layer of this negative electrode precursor contains a negative electrode active material, a thickener, and a binder in a ratio of 98.3:0.7:1.0. Note that graphite was used as the negative electrode active material, carboxymethyl cellulose (CMC) was used as the thickener, and styrene butadiene rubber (SBR) was used as the binder. Next, a negative electrode plate was cut out from the negative electrode precursor under specified conditions. Specifically, in Example 1, a pulse laser was used with a pulse width of 120 ns, a power of 35%, an output of 105 W, and a frequency of 300 kHz. In Example 1, the surface having a relatively smaller surface roughness was used as the laser non-irradiated surface, and the surface having a relatively larger surface roughness was used as the laser irradiated surface to cut out the negative electrode plate.
[0073] Comparative Example 1 In Comparative Example 1, a negative electrode plate was produced under the same conditions as in Example 1, except that when cutting out a negative electrode plate from the negative electrode precursor, the surface on the side having a relatively smaller surface roughness was used as the laser irradiated surface.
[0074] (Example 2, Comparative Example 2) In Example 2, a negative electrode plate was cut out under the same conditions as in Example 1, except that the pulse width of the pulse laser was set to 120 ns, the power to 95%, the output to 285 W, and the frequency to 300 kHz. In Comparative Example 2, a negative electrode plate was produced under the same conditions as in Example 2, except that the surface with a relatively small surface roughness was used as the laser irradiated surface.
[0075] (Example 3, Comparative Example 3) In Example 3, a negative electrode plate was cut out under the same conditions as in Example 1, except that the pulse width of the pulse laser was set to 120 ns, the power to 95%, the output to 95 W, and the frequency to 100 kHz. In Comparative Example 3, a negative electrode plate was produced under the same conditions as in Example 3, except that the surface with a relatively small surface roughness was used as the laser irradiated surface.
[0076] (Example 4, Comparative Example 4) In Example 4, a negative electrode plate was cut out under the same conditions as in Example 1, except that the pulse width of the pulse laser was set to 60 ns, the power to 35%, the output to 105 W, and the frequency to 750 kHz. In Comparative Example 4, a negative electrode plate was produced under the same conditions as in Example 4, except that the surface with a relatively small surface roughness was used as the laser irradiated surface.
[0077] (Example 5, Comparative Example 5) In Example 5, a negative electrode plate was cut out under the same conditions as in Example 1, except that the pulse width of the pulse laser was set to 60 ns, the power to 95%, the output to 114 W, and the frequency to 300 kHz. In Comparative Example 5, a negative electrode plate was produced under the same conditions as in Example 5, except that the surface having a relatively small surface roughness was used as the laser irradiated surface.
[0078] 2.Evaluation Test (1) Measurement of surface roughness In this test, before cutting out the negative electrode plate by laser cutting, the surface roughness of the laser irradiated surface of the exposed core area (exposed negative electrode core) and the surface on the opposite side were measured. Specifically, the maximum height Sz and average roughness Sa of both sides of the negative electrode core were measured in accordance with ISO25178. The measurement results are shown in Table 1.
[0079] (2) Measurement of spatter adhesion In this test, the number of spatters adhering to the negative electrode tab of the negative electrode plate after laser cutting was measured. Specifically, adhesive tape was attached to the top and bottom surfaces of the negative electrode tab, and the spatters adhering to the negative electrode tab were collected by peeling off the adhesive tape. The adhesive tape was attached to an area of 3.7 cm2 on each side. 2The adhesive tape was then attached with a backing paper and observed under a microscope to measure the number of spatter deposits on the laser irradiated surface and non-laser irradiated surface of the negative electrode tab of each example. The number of spatter deposits was measured by performing image analysis on micrographs of the adhesive tape taken with an optical microscope (Keyence Corporation, model: VHX-6000) and counting the number of metal particles of 5 μm or more. The detailed conditions for photographing and image analysis are as follows. The measurement results are shown in Table 1. The number of spatter deposits in Table 1 is the number per unit area (particles / cm 2 ) is shown.
[0080] [Shooting conditions] Magnification: 200x Shooting mode: Image stitching Image color adjustment: R=1.65, G=1.00, B=2.22 Ring lighting: 180 (1160 lux) Stage-light distance: 67mm Shutter speed: 33.00ms
[0081] [Analysis conditions (automatic area measurement)] Hue: 0~45, 240~255 Saturation: 35~255 Separation degree: 100
[0082] [Table 1]
[0083] As shown in Table 1, when Example 1 is compared with Comparative Example 1, the number of spatters attached to the negative electrode tab is reduced in Example 1. Then, when the number of spatters attached to each of the laser irradiated surface and the laser non-irradiated surface is confirmed, the number of spatters attached to the laser non-irradiated surface is particularly significantly reduced in Example 1, in which the surface with the smaller surface roughness is the laser non-irradiated surface, compared to Comparative Example 1. In addition, a similar tendency was confirmed in the comparison between Examples 2 to 5 and Comparative Examples 2 to 6. From this, it was found that the number of spatters attached to the electrode plate after manufacture can be reduced by making the surface with the smaller surface roughness the laser non-irradiated surface and the surface with the larger surface roughness the laser irradiated surface.
[0084] Although the present invention has been described in detail above, the above description is merely illustrative, and the technology disclosed herein includes various modifications and variations of the above-described specific examples. [Explanation of symbols]
[0085] 10 Positive electrode plate 20 Negative plate 20A negative electrode precursor 22 Negative electrode core 22t negative electrode tab 24 Negative electrode active material layer 30 Separator 40 Electrode body 50 Battery case 60 Positive terminal 65 Negative terminal 70 Positive electrode current collector 75 Negative electrode current collector 100 Secondary battery A1 Negative electrode active material application area A2 Negative electrode core exposed area S1 Precursor preparation process S2 Active material application area cutting process S3 Core exposed area cutting process
Claims
1. A method for producing an electrode plate including an electrode core made of a metal foil and an electrode active material layer provided on a surface of the electrode core, comprising the steps of: a precursor preparation step of preparing an electrode precursor having an active material applied region in which the electrode active material layer is applied to a surface of the electrode core, and a core exposed region in which the electrode active material layer is not applied and the electrode core is exposed; a core exposed region cutting step of cutting the core exposed region with a laser to form an electrode tab; Equipped with the electrode core has a first surface and a second surface opposite to the first surface, the second surface having a surface roughness smaller than that of the first surface; A method for manufacturing an electrode plate, wherein the first surface is irradiated with the laser in the core exposed region cutting step.
2. The method for manufacturing an electrode plate according to claim 1 , wherein the laser is a pulsed laser.
3. The method for manufacturing an electrode plate according to claim 1 or 2, wherein the electrode core contains copper or a copper alloy.
4. The method for manufacturing an electrode plate according to any one of claims 1 to 3, wherein the average roughness Sa of the second surface is 0.07 µm or more and 0.25 µm or less.
5. The method for manufacturing an electrode plate according to any one of claims 1 to 4, wherein the average roughness Sa of the first surface is 0.1 µm or more and 0.3 µm or less.
6. further comprising an active material-application region cutting step of cutting the active material-application region with a laser; The method for manufacturing an electrode plate according to any one of claims 1 to 5, wherein the electrode plate is manufactured in which a plurality of the electrode tabs protrude from side edges of the active material-imparting region by alternately performing the core-exposed region cutting step and the active material-imparting region cutting step.
7. A method for manufacturing a secondary battery having an electrode assembly including a positive electrode plate and a negative electrode plate, comprising the steps of: A method for producing a secondary battery, comprising the steps of: producing at least one of the positive electrode plate and the negative electrode plate by using the method for producing an electrode plate according to any one of claims 1 to 6.
8. an electrode assembly fabrication step of fabricating an electrode assembly having an electrode tab group in which a plurality of the electrode tabs are stacked; a current collecting member connecting step of connecting a current collecting member to one surface of the electrode tab group; Further equipped with The method for manufacturing a secondary battery according to claim 7 , wherein in the current collecting member connecting step, the second surface of the electrode core body is disposed on the other surface of the electrode tab group to which the current collecting member is not connected.
9. An electrode plate comprising an electrode core which is a foil-shaped metal member, and an electrode active material layer provided on a surface of the electrode core, an electrode plate main body portion which is a region where the electrode active material layer is applied to the surface of the electrode core; an electrode tab including an exposed region protruding from the electrode plate main body portion, to which the electrode active material layer is not applied and in which the electrode core is exposed; Equipped with the electrode core has a first surface and a second surface opposite to the first surface, the second surface having a surface roughness smaller than that of the first surface; the electrode core exposed at the electrode tab has a number of metal particles attached to the second surface thereof that is smaller than the number of metal particles attached to the first surface thereof; The number of the metal particles attached on the first surface is 80 particles / cm 2 or less, and the number of the metal particles attached on the second surface is 40 particles / cm 2 or less. 2 Below is the electrode plate.
10. An electrode plate comprising an electrode core which is a foil-shaped metal member, and an electrode active material layer provided on a surface of the electrode core, an electrode plate main body portion which is a region where the electrode active material layer is applied to the surface of the electrode core; an electrode tab including an exposed region protruding from the electrode plate main body portion, to which the electrode active material layer is not applied and in which the electrode core is exposed; Equipped with the electrode core has a first surface and a second surface opposite to the first surface, the second surface having a surface roughness smaller than that of the first surface; the electrode core exposed at the electrode tab has a number of metal particles attached to the second surface thereof that is smaller than the number of metal particles attached to the first surface thereof; An electrode plate, wherein the number of the metal particles attached on the first surface is 80 particles / cm 2 or less, and the ratio of the number of the metal particles attached on the second surface to the number of the metal particles attached on the first surface is ½ or less.
11. An electrode plate comprising an electrode core which is a foil-shaped metal member, and an electrode active material layer provided on a surface of the electrode core, an electrode plate main body portion which is a region where the electrode active material layer is applied to the surface of the electrode core; an electrode tab including an exposed region protruding from the electrode plate main body portion, to which the electrode active material layer is not applied and in which the electrode core is exposed; Equipped with the electrode core has a first surface and a second surface opposite to the first surface, the second surface having a surface roughness smaller than that of the first surface; the electrode core exposed at the electrode tab has a number of metal particles attached to the second surface thereof that is smaller than the number of metal particles attached to the first surface thereof; An electrode plate in which a modified substance adhesion region is formed at the outer edge portion of the electrode plate main body portion, in which a modified substance of the electrode active material layer is adhered to the electrode core, and the width of the modified substance adhesion region on the first surface is larger than the width of the modified substance adhesion region on the second surface.
12. The electrode tabs protrude outward from the outer edge of the electrode plate body, The electrode plate according to claim 9 , wherein each of the electrode tabs includes an active material layer application region, in which the electrode active material layer is applied, at a base portion of the electrode tab adjacent to the electrode plate body portion.
13. A secondary battery having an electrode assembly including a positive electrode plate and a negative electrode plate, A secondary battery, wherein at least one of the positive electrode plate and the negative electrode plate is the electrode plate according to any one of claims 9 to 12.
14. The electrode body includes an electrode tab group in which a plurality of the electrode tabs are stacked, 14. The secondary battery according to claim 13, wherein a current collecting member is connected to one surface of the electrode tab group, and the second surface of the electrode core is disposed on the other surface of the electrode tab group to which the current collecting member is not connected.
15. The secondary battery according to claim 14 , wherein the electrode tab group is bent so that the current collecting member faces a side surface of the electrode body.
Citation Information
Patent Citations
Secondary battery
JP2015069938A
Secondary battery, and method of manufacturing the same
JP2016033912A
Method of manufacturing secondary battery electrode and method of manufacturing secondary battery
JP2018037296A
Secondary battery electrode and method of manufacturing the same, and secondary battery and method of manufacturing the same