Method for manufacturing hollow core fiber and method for manufacturing preform for hollow core fiber

By employing a viscosity profile and doping in the outer cylinder, the method addresses the challenges of precise manufacturing in anti-resonant hollow core fibers, enhancing beam quality and reducing deformation, thus improving manufacturing efficiency.

JP7583784B2Active Publication Date: 2024-11-14HERAEUS QUARZGLAS GMBH & CO KG
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022502576
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-17
Filing Date
2020-07-15
Publication Date
2024-11-14
Estimated Expiration
2040-07-15

AI Technical Summary

Technical Problem

Conventional anti-resonant hollow core fibers face challenges in precise manufacturing due to complex internal geometries and difficulty in achieving uniform wall thickness and precise positioning of anti-resonant elements, leading to poor beam quality and increased deformation during the drawing process.

Method used

The method involves using an outer cylinder with a radial viscosity profile that increases towards the inside, combined with doping to match viscosities of different preform components, ensuring stable and reproducible positioning of anti-resonant elements by minimizing deformation during heat treatment.

Benefits of technology

This approach enables high precision in the structural elements and positioning, reducing optical and mechanical deformations, resulting in improved beam quality and reduced manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583784000003
    Figure 0007583784000003
  • Figure 0007583784000004
    Figure 0007583784000004
  • Figure 0007583784000005
    Figure 0007583784000005
Patent Text Reader

Abstract

A method for manufacturing an antiresonant hollow-core fiber having a hollow core extending along the fiber's longitudinal axis and an inner cladding region containing a plurality of antiresonant elements and surrounding the hollow core is known. The known method includes the steps of providing a cladding tube having an inner bore and a longitudinal axis, with a cladding wall defined by an inner and outer side extending along the longitudinal axis, providing a plurality of antiresonant element preforms, placing the antiresonant element preforms at target positions inside the cladding wall to form primary preforms for the hollow-core fiber having a hollow core region and a cladding region, and drawing the primary preforms to form the hollow-core fiber or further processing the primary preforms to form secondary preforms. Based on this, in order to achieve high precision and accurate positioning of the antiresonant elements in a sufficiently stable and reproducible manner, when further processing the primary preform (1) according to step (c), an outer cylinder is used that has a radial viscosity profile in which the viscosity increases toward the inside of the outer cylinder.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Background technology The present invention relates to a method of making an anti-resonant hollow-core fiber having a hollow core extending along a longitudinal axis of the fiber and a cladding region including a plurality of anti-resonant elements and surrounding the hollow core, the method comprising: (a) providing a primary preform for a hollow-core fiber, the hollow-core fiber including at least one cladding tube having a cladding tube interior bore and a cladding tube longitudinal axis along which extends a cladding tube wall defined by an inner side and an outer side; (b) forming a plurality of precursors or preforms for anti-resonant elements at target locations on the cladding wall; (c) further processing the primary preform into a secondary preform from which a hollow-core fiber is drawn, the further processing including one or more repeated collapsing of additional cladding material in the form of an outer cylinder having an inner side facing the coating tube, an outer side, and an outer cylinder wall located between the inner side and the outer side.

[0002] The present invention further relates to a method for making an anti-resonant hollow-core fiber preform having a hollow core extending along a longitudinal axis of the fiber and a cladding region surrounding the hollow core, the cladding region including a plurality of anti-resonant elements, the method comprising: (a) providing a primary preform for a hollow-core fiber, the hollow-core fiber including at least one cladding tube having a cladding tube interior bore and a cladding tube longitudinal axis along which extends a cladding tube wall defined by an inner side and an outer side; (b) forming a plurality of precursors or preforms for anti-resonant elements at target locations on the cladding wall; (c) further processing the primary preform into a secondary preform for a hollow-core fiber, the further processing including one or more repeated collapses of additional cladding material in the form of an outer cylinder having an inner side facing the coating tube, an outer side, and an outer cylinder wall located between the inner side and the outer side.

[0003] Conventional single-mode optical fibers made from solid materials have a glass core surrounded by a cladding region made of glass with a low refractive index. The propagation of light is based on total internal reflection between the core and cladding regions. However, the interaction of the guided light with the solid material is associated with increased delay times in data transmission and a relatively low damage threshold for energetic radiation.

[0004] These disadvantages are avoided or mitigated by "hollow-core fibers", whose core consists of a vacuum cavity filled with gas or liquid. In hollow-core fibers, the interaction of light with the glass is reduced compared to solid-core fibers. Since the refractive index of the core is smaller than that of the cladding, light propagation by total internal reflection is not possible and light is usually considered to leak from the core into the cladding. Depending on the physical mechanism of light propagation, hollow-core fibers are distinguished into "photonic bandgap fibers" and "antiresonant reflecting fibers".

[0005] In a "photonic bandgap fiber", a hollow core region is surrounded by a cladding that contains a periodic arrangement of small hollow channels. The periodic structure of the hollow channels in the cladding has an effect called "photonic bandgap" in semiconductor technology, which means that light in a certain wavelength range that scatters into the cladding structure cannot spread laterally within the cladding because it interferes constructively in the central cavity based on Bragg reflection.

[0006] In hollow-core fiber embodiments, called "antiresonant hollow-core fibers" (ARHCF), a hollow core region is surrounded by an inner cladding region and is located within so-called "antiresonant elements" (or "antiresonant elements"; abbreviation "AREs"). The walls of the antiresonant elements, evenly distributed around the hollow core, function as an antiresonantly operated Fabry-Perot cavity that can reflect incoming light and pass it through to the fiber core.

[0007] This fiber technology allows for reduced optical attenuation, a very wide transmission spectrum (even in the ultraviolet or infrared wavelength ranges), and low latency during data transmission.

[0008] Potential applications of hollow-core fibers lie in the fields of high-performance beam control for data transmission, material processing, modal filtering, and nonlinear optics, especially for generating supercontinuums from the extreme ultraviolet to the infrared wavelength range.

[0009] Background technology A drawback of anti-resonant hollow-core fibers is that higher order modes are not automatically suppressed, so they often do not become purely single mode over long transmission distances, resulting in poor quality output beams.

[0010] Francesco Poletti, "Nested antiresonant nodeless hollow core fiber"; Optics Express, Vol. 22, No. 20 (2014); DOI: 10.1364 / OE 22.023807, proposes a fiber design in which the antiresonant element is not formed as a simple single structural element, but is composed of multiple structural elements nested within each other. The nested antiresonant elements are designed in such a way that the higher-order core modes are phase-matched to the cladding modes and suppressed, but the fundamental core mode is not suppressed. This ensures that the fundamental core mode always propagates, making the hollow core fiber effectively single-mode over a limited wavelength band.

[0011] Efficient mode suppression depends on the central wavelength of the propagating light as well as on structural parameters of the fiber design, such as the radius of the hollow core and the diameter difference of the nested ring structures within the anti-resonant element.

[0012] From EP 3136143 A1 an anti-resonant hollow-core fiber (called "hollow-core fiber without band gap") is known, whose core is capable of propagating other modes besides the fundamental mode. For this purpose, the core is surrounded by an inner cladding with "anti-resonant elements" that provide phase matching of the anti-resonant mode and higher modes. The production of hollow-core fibers is carried out by the so-called "stack and draw" method, in which a preform is formed by arranging and fixing the starting elements in an axially parallel collection, and then drawing the preform. Here, a cladding tube with a hexagonal inner cross section is used, to whose inner edge six so-called "ARE preforms" (anti-resonant element preforms) are fixed. The hollow-core fiber is formed by drawing the preform in two stages.

[0013] From International Patent Application 2018 / 169487 A1 a method for manufacturing a preform for an antiresonant hollow core fiber is known, in which a first cladding region is made up of a number of rods and a second cladding region is made up of a number of tubes surrounded by an outer cladding tube. The rods, tubes and cladding tube are joined by a "stack and draw" method to form the preform. Before the preform is drawn, sealing is performed by applying a sealant to the preform ends. As sealant a UV adhesive is used, for example.

[0014] Problem to be solved by the invention Anti-resonant hollow-core fibers, and especially those with nested structural elements, have complex internal geometries that make them difficult to manufacture accurately and reproducibly. This is compounded by the fact that resonance or anti-resonance conditions cannot be met without small dimensional tolerances on the magnitude of the operating wavelength of the propagating light. Deviations from the target shape can be caused during the construction of the fiber preform, but can also occur during the fiber drawing process due to inappropriate deformations that are not to scale.

[0015] In the known "stack and draw" method, a large number of elements must be joined in precise positions. For example, to manufacture a hollow-core fiber of the "NANF" design known from the literature mentioned at the beginning, six anti-resonant element preforms, each consisting of an anti-resonant element outer tube (abbreviated as "ARE outer tube") and an anti-resonant element inner tube (abbreviated as "ARE inner tube") welded to one side of the inner cladding surface of the outer ARE tube, must be attached inside the cladding tube.

[0016] In order to achieve low attenuation values ​​and wide propagation ranges, the azimuthal position of the anti-resonant element inside the cladding tube is also important, in addition to the uniform wall thickness of the anti-resonant element walls, which cannot be easily achieved by the "stack and draw" method. It is an object of the present invention to provide a manufacturing method for achieving anti-resonant hollow-core fibers at low cost, avoiding the limitations of conventional manufacturing methods.

[0017] In particular, it is an object of the present invention to provide a method for producing an antiresonant hollow-core fiber, and a method for producing a preform for an antiresonant hollow-core fiber, which makes it possible to achieve high precision of the structural elements and exact positioning of the antiresonant elements within the fiber in a sufficiently stable and reproducible manner.

[0018] Furthermore, the drawbacks of the conventional "stack and draw" method, in which the required construction precision, in particular the uniform wall thickness and precise positioning of the anti-resonant elements in defined azimuthal positions, are not easily achievable, must be avoided as far as possible.

[0019] Summary of the Invention With regard to the production of antiresonant hollow-core fibers, the above-mentioned problem is solved according to the invention, starting from the method as mentioned at the beginning, in that an outer layer cylinder having a radial viscosity profile with an increasing viscosity towards the inside of the outer layer cylinder is used for further processing the primary preform according to step (c).

[0020] The starting point for the manufacture of an anti-resonant hollow-core fiber is a preform, also referred to herein as the "primary preform", which includes a cladding tube that contains a precursor or preform for forming an anti-resonant element in the hollow-core fiber (herein referred to as the "anti-resonant element" for short). The primary preform can be drawn to form a hollow-core fiber, but is usually further processed to produce a preform, also referred to herein as the "secondary preform", from the primary preform. If necessary, the hollow-core fiber is produced by drawing the secondary preform. Alternatively, the primary or secondary preform is surrounded by an outer cylinder or cylinders, forming a coaxial assembly of components, which is directly drawn to form the hollow-core fiber. In this case, the general term "preform" is to be understood as the name of the component or the coaxial assembly of components from which the hollow-core fiber is finally drawn.

[0021] The cladding material may be added, for example, by collapsing an outer cylinder onto the primary preform, with the coaxial arrangement of the primary preform and the outer cylinder either being stretched or not stretched upon collapsing of the outer cylinder, with or without changing the shape or configuration of the anti-resonant element preform.

[0022] The implementation of one of the thermoforming processes (hereinafter also referred to as "thermal processes") described in step (c) may result in deformations and structural errors of the fiber geometry to be obtained, especially when several thick-walled and fine preform components made of the same material are closely located or in contact with each other.

[0023] This is because the required processing temperature is usually determined by the flat and very thick components, typically the outer cladding region of the preform. Smaller components (e.g. the anti-resonant element preform and its individual structural elements) deform more strongly at the same temperature. During the heat treatment, the preform is heated from the outside to the inside in the heating zone, so that a radial temperature profile with a minimum value in the center of the preform occurs over the preform volume. This can exacerbate the aforementioned deformation problem if fine components are located closer to the heating zone in the radial direction of the preform than less fine components, which is typical for anti-resonant hollow-core fiber preforms.

[0024] The viscosity of single-component glasses, especially silica glasses, can be changed by doping. By using materials with different dopings, and thus by using matched viscosities, structure preservation can be ensured during heat treatment. Doping provides a match of the viscosities of adjacent preform components. In particular, doping can be used to reduce the thermal stability of a component in favor of the stability of the adjacent component.

[0025] However, when an outer layer cylinder is used to cover the primary preform, a step-like viscosity change can occur at the interface between the primary preform and the outer layer cylinder. Such an abrupt change can lead to internal mechanical stresses in the finished (secondary) preform and, in the final hollow-core fiber, that adversely affect both the optical and mechanical properties. Such adverse effects include deviations of optical parameters from the designed properties (deviations of refractive index due to mechanical stress) as well as an increased tendency to break.

[0026] The object of the present invention is to realize the use of differently doped starting materials for the starting cylinder and the cladding in order to suppress deformations, particularly of fine structural elements, during heat treatment, but without this having a detrimental effect on the optical and mechanical properties of the fiber and the preform, thereby achieving a higher precision of the geometry and positioning of the anti-resonant elements in the hollow-core fiber.

[0027] For this purpose, at least the outer layer cylinder, and preferably also the cladding tube, exhibits a dopant concentration gradient towards the common interface, which is achieved in the outer layer cylinder by having a radial viscosity profile in which the viscosity increases towards the inside of the outer layer cylinder.

[0028] This allows the viscosity difference between the outer cylinder and the cladding to be maintained without significant changes at the interface, since this creates a transition zone with adapted viscosity at the interface, which suppresses deformations and contributes to maintaining the structure of the anti-resonant element.

[0029] In a preferred manner, the viscosity in the region inside the outer cylinder has a value η(Z) and the viscosity in the region outside the cladding has a value η(M), and at a measurement temperature of 1250°C the following holds for the viscosity values ​​(when the viscosity is expressed as a logarithmic value in dPa·s): η(M)=η(Z)±0.5 dPa·s, preferably η(M)=η(Z)±0.3 dPa·s.

[0030] Here, the viscosity η(M) at the cladding outer surface lies within the narrowest possible range around the viscosity value η(Z) of the outer cylinder in the region of the inner cladding surface, and more preferably, η(M) is greater than η(Z).

[0031] In addition, the viscosity profile at the outer cylinder wall is the minimum viscosity value η(Z min ) toward the inside of the outer cylinder.

[0032] For example, a radial viscosity profile with a viscosity minimum at the cylinder wall is achieved by introducing into the glass of the outer layer cylinder a dopant which reduces the viscosity of the glass of the outer layer cylinder and can at least partially disappear when heated. Preferably, fluorine, chlorine and / or hydroxyl groups are used here. Preferably, therefore, the outer layer cylinder consists of silica glass and the viscosity profile of the outer layer cylinder is generated by the addition of at least one dopant which reduces the viscosity of the silica glass, the dopant preferably comprising fluorine, chlorine and / or hydroxyl groups.

[0033] It has been found that it is preferable for the silica glass of the outer cylinder to contain fluorine as a dopant at a concentration of 500 to 8000 ppm by weight.

[0034] It has been found to be even more advantageous if the difference between the viscosity minimum and the viscosity of the cladding in the region of the contact surface is large, since this difference is a measure for the viscosity difference between the cladding and the outer cylinder, which is usually desired (except at the contact surface). Therefore, the viscosity minimum η(Z min ) (when viscosity is expressed as a logarithmic value): η(M)-η(Z min )>0.8 dPa s, preferably >1 dPa s.

[0035] In another preferred variation of the method, the cladding has a radial viscosity profile between the outside of the cladding and the inside of the cladding, with the viscosity gradually increasing inwardly.

[0036] It has been found to be advantageous if the cladding is made of silica glass and fluorine is used as a dopant in concentrations of 500-8000 ppm by weight in order to adjust the viscosity gradient within the cladding wall.

[0037] In this relationship, the cladding tube has a viscosity maximum value η(Z max ), and in step (b) at least a part of the anti-resonant element preform or the precursor for the anti-resonant element is present as a tubular anti-resonant element preform, preferably consisting of a plurality of nested structural elements including an outer ARE tube and an inner ARE tube inserted therein, the anti-resonant element preform being made of silica glass, the silica glass of the cladding tube having a maximum viscosity η(M max ) which is at least 0.4 dPa·s higher, preferably at least 0.5 dPa·s higher (when the viscosity is expressed as a logarithmic value).

[0038] The outer cylinder and the cladding tube consist in the most preferred case of silica glass. The fluorine doping of the additional cladding material provided by the outer cylinder achieves a sufficient reduction in viscosity relative to the silica glass of the cladding tube, even if the silica glass of the cladding tube itself does not contain any dopant. It has proven to be advantageous if the silica glass of the cladding tube has a viscosity at a measuring temperature of 1250°C that is at least 0.5 dPa·s higher, preferably at least 0.6 dPa·s higher, than the silica glass of the additional cladding material. Here and below, the viscosity difference is expressed as the logarithmic viscosity value in dPa·s.

[0039] In an advantageous manner, all preform components of the preform consist of different silica glass qualities, the viscosity of which in a first approximation increases from the outside to the inside. To adjust the viscosity, other dopants besides fluorine may be used, such as Al2O3, nitrogen, chlorine and hydroxyl. However, in the simplest case, it is sufficient that the additional cladding material consists of fluorine-containing silica glass.

[0040] In a further preferred manner, at least a part of the preform for the antiresonant element is present as a tubular antiresonant element preform, which is preferably constructed of multiple structural elements nested together, including an outer ARE tube and an inner ARE tube inserted therein, and the antiresonant element preform consists of silica glass, which has a viscosity at a measurement temperature of 1250°C that is at least 0.4 dPa·s higher, preferably at least 0.5 dPa·s higher, than the silica glass of the cladding tube.

[0041] Here, the silica glass of the ARE outer tube can contain dopants that increase its viscosity, such as nitrogen or Al2O3, but it has proven to be particularly advantageous if the cladding tube is made from silica glass that contains a dopant that reduces the viscosity of the silica glass.

[0042] With regard to high thermal stability of the ARE inner tube when the structural elements are nested, it has proven to be advantageous if at least a part of the ARE inner tube, preferably the entire ARE inner tube, is made from silica glass, which has a viscosity at a measuring temperature of 1250°C that is at least 0.4 dPa·s higher, preferably at least 0.5 dPa·s higher, than the silica glass of the ARE outer tube.

[0043] The cladding tube is preferably produced in a two-stage drawing process without a forming tool in a vertical drawing method. In a first stage, a starting hollow cylinder of glass is mechanically worked to adjust the final dimensions of the starting hollow cylinder. In a first drawing process with a longitudinal axis oriented vertically, the starting cylinder is continuously fed to a heating zone having a first heating zone length, softened in the heating zone in a zone-by-zone manner, and an intermediate cylinder is drawn from the softened zone. In a first drawing process with a longitudinal axis oriented vertically, the starting cylinder is continuously fed to a heating zone having a first heating zone length, softened in the heating zone in a zone-by-zone manner, and an intermediate cylinder is drawn from the softened zone. The cladding tube is obtained by cutting the continuous tube.

[0044] By using preform components that have a relatively low viscosity, especially in the outer cladding region, the method according to the invention allows relatively large preforms to be used for heat treatment.

[0045] In this respect, preferably a secondary preform is formed having an outer diameter in the range of 30-90 mm and / or a primary preform is formed having an outer diameter in the range of 20 mm-70 mm, preferably 30-70 mm.

[0046] The outer diameter of the preform in the range of 30-90 mm is large compared to the current state of the art. With larger preform outer diameters, the absolute shape errors present are scaled down to a greater extent during fiber drawing, so that when using larger preforms, a more precise manufacture of the hollow-core fiber is also essentially achieved. However, at diameters larger than 90 mm, temperature gradients arise in the preform volume during the fiber drawing process, which may lead to deviations in the wall thickness in the anti-resonant elements in the hollow-core fiber. At preform outer diameters shorter than 30 mm, a particularly large contribution by the scaling down of the shape errors is no longer obtained. Furthermore advantageously, primary preforms are formed with an outer diameter in the range of 20-70 mm, preferably in the range of 30-70 mm. This is a relatively large outer diameter. In the prior art, the outer diameter of the primary preforms was usually in the range of 4-6 mm.

[0047] In a preferred variant of the method, forming a preform for the antiresonant element according to step (b) comprises positioning the antiresonant element preform at a target position inside the cladding tube wall, and a positioning template having holding elements for positioning the antiresonant element preform at the target position is used for the positioning.

[0048] The positioning template has, for example, a shaft which projects into the cladding tube inner bore and is provided with retaining elements in the form of a number of radially outwardly directed retaining arms.

[0049] The structurally defined star-shaped arrangement of the holding elements facilitates the exact positioning and fixing of the anti-resonant element preform at each target position, whereby a positioning template is preferably used only in the region of the cladding tube end face, preferably in the region of both cladding tube end faces.

[0050] The accuracy of positioning of the preform on the inner cladding surface of the cladding tube is improved in that the inside of the cladding tube is formed by a machining process, in particular by drilling, milling, grinding, honing and / or polishing.

[0051] In a preferred method, tubular structural elements are provided, at least some of which have a wall thickness in the range of 0.2-2 mm, preferably in the range of 0.25-1 mm, thereby further improving the positioning accuracy of the preform in the cladding tube. In this case, the cladding tube is provided with an outer diameter in the range of 90-250 mm, preferably in the range of 120-200 mm. Each of these components has a length of at least 1 m, which is a relatively voluminous structural element for forming an anti-resonant element. This allows for easy handling. Furthermore, if the cladding tube and the structural element are vertically arranged, and the structural elements are positioned and fixed at their respective upper end faces in the target position, for example by using the above-mentioned sealing or bonding material, the parallelism and vertical alignment of the longitudinal axes of the structural elements are supported by gravity.

[0052] With regard to the production of a preform for a hollow-core fiber, the above-mentioned problem is solved according to the invention, starting from the method as mentioned at the beginning, in that an outer layer cylinder having a radial viscosity profile with an increasing viscosity towards the inside of the outer layer cylinder is used for further processing the primary preform according to step (c).

[0053] The preform is the starting point for antiresonant hollow-core fiber fabrication. The preform is drawn either directly to draw an antiresonant hollow-core fiber or to form a blank from which the antiresonant hollow-core fiber is subsequently drawn. Fabrication of the preform involves collapsing additional cladding material onto the primary preform using an outer cylinder with a radial viscosity profile that increases toward the inside of the outer cylinder.

[0054] This allows the viscosity difference between the outer cylinder and the cladding tube to be maintained without significant changes in the interface. The procedures for producing the preform are described in detail above in connection with the manufacture of hollow-core fibers, and those descriptions are incorporated herein by reference.

[0055] definition The following are supplementary definitions for the individual steps and terms in the above-mentioned specification. These definitions are part of the present specification. If there is a substantial discrepancy between any of the following definitions and the rest of the specification, the definitions mentioned in the rest of the specification shall prevail.

[0056] anti-resonance element The anti-resonant element may be a simple structural element or a nested structural element of the hollow-core fiber. It has at least two walls with negative curvature (convex) or no curvature (flat, straight) as viewed in the direction of the hollow core. Typically, the anti-resonant element consists of a material transparent to the operating light, such as glass (especially doped or undoped SiO2), plastic (especially polymers), composite materials or crystalline materials.

[0057] Anti-resonant element preform / anti-resonant element pre-stage The anti-resonant element preform is a component or a preform component that becomes an anti-resonant element in a hollow-core fiber mainly by simple drawing in a fiber drawing process. The anti-resonant element pre-stage is a component or a preform component that becomes an anti-resonant element preform or directly an anti-resonant element only by deformation. The anti-resonant element preform can be a simple component or a nested component to which additional positioning aids can be fixed. The anti-resonant element preform is originally present in the primary preform.

[0058] The nested anti-resonant element preform forms an anti-resonant element nested within a hollow-core fiber. It is composed of an outer tube and at least one further structural element disposed within the inner bore of the outer tube. The further structural element may be a further tube that is in contact with the inner cladding surface of the outer tube. The outer tube is also referred to as the "anti-resonant element outer tube" or "ARE outer tube" for short, and the further tube is also referred to as the "anti-resonant element inner tube" or "ARE inner tube" for short, or "nested ARE inner tube".

[0059] In the case where the anti-resonant element preforms are nested multiple times within the inner bore of the nested inner ARE tube, at least one further structural element may be disposed, for example a third tube, which is in contact with the inner cladding surface of the nested inner ARE tube.

[0060] When the anti-resonant element preforms are nested multiple times, a distinction is made between a "nested outer ARE inner tube" and a "nested inner ARE inner tube" as necessary to distinguish between the multiple tubes disposed within the outer ARE tube.

[0061] The term "cross section" in connection with cylindrical anti-resonant element preforms and their cylindrical structural elements always refers to a cross section perpendicular to the respective cylinder longitudinal axis and, unless otherwise specified, refers to a cross section of the external contour of the tubular component (and not a cross section of the internal contour).

[0062] Further processing of the primary preform, in particular by a thermoforming process, can produce intermediate products in which the original anti-resonant element preform is present in a modified shape relative to its initial shape, which modified shape is also referred to herein as the anti-resonant element preform or anti-resonant element pre-stage.

[0063] Preform / Primary preform / Secondary preform / Core preform (Cane) A preform is a component from which an anti-resonant hollow-core fiber is drawn. It can be a primary preform or a secondary preform produced by further processing of a primary preform. A primary preform can be an assembly of at least one cladding tube and a preform or precursor for an anti-resonant element housed therein in a loosely or rigidly fixed manner. Further processing of a primary preform into a secondary preform from which a hollow-core fiber is drawn can be performed by: (i) stretching; (ii) Collapse; (iii) collapsing and simultaneous stretching; (iv) Collapse of additional cladding material; (v) Collapse and subsequent stretching of additional cladding material; (vi) collapsing and simultaneously stretching additional cladding material; The thermoforming process may include performing one or more of the following steps once or repeatedly:

[0064] In the literature, a core preform (English: cane) is a preform obtained by collapsing and / or stretching a primary preform. Usually, the core preform is covered with additional cladding material before or during the drawing of the hollow-core fiber.

[0065] Stretching / Collapse In drawing, the primary preform is stretched to an elongation. This drawing may be performed without simultaneous collapse. The drawing may be performed to scale, so that, for example, the shape and arrangement of the components of the primary preform are reflected in the final drawn product. However, in drawing, the primary preform may not be drawn to size, and the geometry may change.

[0066] Collapsing involves narrowing the internal bore or closing or narrowing the annular gap between the tubular components, and is usually accomplished in parallel with stretching.

[0067] Hollow core / inner cladding region / outer cladding region The assembly consisting of at least one cladding tube and the preform or precursor of the anti-resonant element housed therein in a loosely or rigidly fixed manner is also referred to herein as the "primary preform". This primary preform consists of a hollow core and a cladding region. This cladding region is also referred to as the "internal cladding region" when there is an "external cladding region" formed, for example by collapsing into the assembly, and it is necessary to distinguish between these cladding regions. The names "internal cladding region" and "external cladding region" are also used for the corresponding regions of the hollow-core fiber or intermediate product obtained by further processing of the primary preform.

[0068] The term "inside the tube" is also used as a synonym for "inner cladding surface of the tube," and the term "outside the tube" is also used as a synonym for "outer cladding surface of the tube." The term "internal bore" in reference to a tube does not imply that the internal bore is formed by a drilling operation.

[0069] Cutting processing A mechanical manufacturing method for isolating a workpiece, which means in particular turning, cutting, drilling, sawing, milling or grinding, which results in a longitudinal structure extending in the direction of the cladding tube longitudinal axis, which serves as a positioning aid for the anti-resonant element preform, which is accessible from the inside of the cladding tube and may extend through the entire cladding tube wall to the outside.

[0070] Particle size and particle size distribution The particle size and particle size distribution of SiO2 particles are 50 This value is read from a particle size distribution curve that shows the cumulative amount of SiO2 particles according to their size. The particle size distribution is 10 Value, D 50 Value, D 90 It is often characterized based on the value of D 10 The value indicates the particle size that does not reach 10% of the cumulative amount of SiO2 particles, and correspondingly, D 50Value and D 90 indicates the particle size at which the cumulative amount of SiO2 particles does not reach 50% or 90%. The particle size distribution is detected by scattered light and laser diffraction spectroscopy according to ISO13320.

[0071] Working Example The invention is explained in more detail below on the basis of an embodiment with the aid of the figures, the details of which are shown in the figures. [Brief description of the drawings]

[0072] [Figure 1] Based on a radial cross-section, a tube is shown with a coaxially arranged outer cylinder and primary preform, the primary preform being comprised of a cladding tube with an anti-resonant element preform positioned and secured therein. [Diagram 2] 1 shows a graph of the radial course of fluorine concentration and viscosity in the outer cylinder and the cladding tube. [Diagram 3] FIG. 2 shows a diagram illustrating an ideal radial concentration or viscosity profile of a preform for a hollow core fiber.

[0073] In the production of hollow-core fibers or preforms for hollow-core fibers, a large number of components have to be connected to one another. Furthermore, when carrying out a thermoforming process, it is advantageous to seal gaps and channels present in the preform. As is known from DE 10 2004 054 392 A1, SiO2-based sealants or bonding materials are used for joining or sealing. Here, by wet milling of silica glass powder grains, D approx. 5 μm is produced. 50 value and D of about 23 μm 90 An aqueous slurry is produced containing amorphous SiO2 particles having a particle size distribution characterized by a value of . Amorphous SiO2 particles having a medium particle size of about 5 μm are mixed into the base slurry. The slurry used as a joint material has a solids content of 90% and is composed of at least 99.9% by weight of SiO2.

[0074] FIG. 1 shows a schematic diagram of a tube 1 having a coaxial arrangement of an outer cylinder 2 and a cladding tube 3 having a cladding wall, on whose inner surface anti-resonant element preforms 4 are fixed at predefined azimuthal positions, in this embodiment six preforms 4 being evenly spaced apart, and in another preferred embodiment not shown there being an odd number of preforms.

[0075] The cladding tube 3 has an outer diameter of 27 mm and an inner diameter of 20 mm. The anti-resonant element preform 4 exists as a collection of structural elements, the outer ARE tube 4a and the inner ARE tube 4b nested inside each other. The outer ARE tube 4a has an outer diameter of 6.2 mm and the inner ARE tube 4b has an outer diameter of 2.5 mm. The wall thickness of both structural elements (4a; 4b) is equal and is 0.3 mm. All tubular components 2, 3, 4a, 4b have a length of 700 mm.

[0076] The anti-resonant element preforms 4 are fixed on the inner wall of the cladding tube 3 by means of a SiO2-based bonding material. The bonding material is applied locally to the end region of the end face on the inner cladding surface of the cladding tube, and the anti-resonant element preforms 4 are placed on the bonding material 5 by means of a positioning template in which the holding arms for the individual anti-resonant element preforms 4 are structurally defined and arranged in a star shape. The action of the positioning template is limited here to the region near both ends of the end face of the cladding tube. In this way, a precise and reproducible connection is achieved between the cladding tube 3 and the anti-resonant element preforms 4. For the fixing, it is sufficient to harden the bonding material at a low temperature of below 300 ° C, whereby strong heating of the surrounding area and thus deformation of the anti-resonant element preforms 4 is avoided.

[0077] The primary preform thus obtained is covered by an outer cylinder 2 made of silica glass, which has an outer diameter of 63.4 mm and a wall thickness of 17 mm. The outer cylinder 2 is collapsed onto the cladding tube 3, at the same time the coaxial tube is elongated. For this purpose, the coaxial tube with the cladding tube 3 and the outer cylinder 2 is guided from below with its longitudinal axis oriented vertically into a temperature-controlled heating zone, in which it is softened zone by zone from the upper end of the coaxial tube. The heating zone is maintained at a target temperature of 1580°C with a control accuracy of ±0.1°C. This allows the temperature fluctuations in the thermoforming process to be limited to less than ±0.5°C.

[0078] The secondary preform formed in the collapse and drawing process has an outer diameter of about 50 mm and a cladding wall thickness of 16.6 mm, including the outer and inner cladding. The secondary preform is then drawn to form the antiresonant hollow-core fiber. Beforehand, all the antiresonant element preforms are closed with a sealing or bonding material. The sealing material is applied only to the end face of the antiresonant element preforms, which faces upward during the fiber drawing process. This end face is connected to a holding tube made of silica glass, which is simultaneously used as a gas connection. The holding part is fixed to the outer cylinder 2 and the covering tube 3 by means of a sealing or bonding material.

[0079] In the fiber drawing process, the secondary preform is guided from above with its longitudinal axis oriented vertically into a temperature-controlled heating zone, where it is softened zone by zone from the bottom end. At the same time, gas is supplied to the core region (hollow core), creating an internal pressure of 4 mbar in the core region. The heating zone is maintained at a target temperature of 2080°C with a control accuracy of ±0.1°C. This allows the temperature fluctuations during the thermoforming process to be kept below ±0.5°C.

[0080] By drawing the preform to form a hollow-core fiber, the absolute geometric errors present are scaled down so that in the hollow-core fiber, the maximum deviation in wall thickness of the antiresonant element obtained from the antiresonant element preform is less than 3.5% (based on the average wall thickness).

[0081] The small wall thickness deviations are due on the one hand to the use of a comparatively large secondary preform and the associated scaling down of the originally existing absolute geometric deviations, and on the other hand to the comparatively low processing temperatures during the thermoforming process (drawing and collapsing). The comparatively low process temperatures are also due to the fact that the outer cylinder 2 and the cladding tube 3 are made of fluorine-doped silica glass. These components are areal and very thick components in their coaxial arrangement 1, which decisively influence the process temperature. By doping the areal and very thick components of the secondary preform with fluorine, the required process temperature can be reduced, which indirectly improves the relative stiffness and thermal stability of the inner antiresonant element preform 4 by exposing it to a lower temperature during the thermoforming process.

[0082] Table 1 below summarizes the material description of the coaxially arranged components or components of the secondary preform.

[0083] [Table 1]

[0084] The fluorine-doped silica glass tubes (2;3) have a fluorine concentration profile with a maximum value in the center of the tube wall. The data for the fluorine concentration of the silica glass given in the "Material" column of Table 1 are average values.

[0085] The graph in Figure 2 shows the cladding C F Regarding (M), the outer cylinder CF (Z) shows the fluorine concentration profile C (unit: weight ppm) measured at “1250°C” and the viscosity profile η (unit: lg dPa s) along the radial position coordinate (position P (unit: mm)) calculated from the concentration profile with respect to the temperature at 1250°C.

[0086] The fluorine concentration profile in silica glass is determined by infrared spectroscopy. The viscosity is scaled with the fluorine concentration for a given temperature and is calculated from the reference value for undoped silica glass (η = 11.8 dPa s, corresponding to 100%) according to the following formula: Viscosity test at 1250℃: 12% (±2%) per weight percent fluorine

[0087] Table 2 gives viscosity values ​​for the fluorine content of commercial silica glass qualities (for a measurement temperature of 1250° C.).

[0088] [Table 2]

[0089] Figure 2 shows that the viscosity of the outer cylinder η(Z) is lower than that of the cladding tube η(M). In the two silica glass tubes, the viscosity at the center of the tube has a minimum, which is about 10 11.45 dPa·s, and the outer cylinder has a viscosity of about 10 10.65 Therefore, the minimum viscosity difference (unit lg dPa s) is about 0.80 dPa s. The viscosity of the cladding in the outer region of the cladding (about 10 11.5 The difference between the viscosity at the outer cylinder and the viscosity minimum at the outer cylinder is approximately 0.85 (unit: lg dPa s).

[0090] In the preform, the outer cladding surface of the cladding and the inner cladding surface of the outer layer cylinder form a common interface. The local locations of the interface plotted in the viscosity profile are indicated by two boxes "K" in the graph. At these locations, the following values ​​for the viscosity of the outer layer cylinder and the cladding occur: Cladding tube: approx. 11.5 lg(dPa s) Outer cylinder: approx. 11.15 lg (dPa s) The viscosity difference in the region of the contact surface is therefore approximately 0.35 dPa·s (units lgd Pa·s).

[0091] The structural elements (4a; 4b) of the antiresonant element preform (4) are made of undoped silica glass and have a thickness of about 10 11.8 It has a viscosity of dPa·s.

[0092] FIG. 3 shows the idealized form of the radial dopant concentration profile across the wall of the secondary preform. On the y-axis is the fluorine concentration C versus the position coordinate P (relative units). F (relative units) are plotted. At the interface “K”, the dopant concentration C of the fluorine-doped silica glass originating from the outer cylinder is F (Z) is the concentration of fluorine-doped silica glass, C, that is derived from the cladding tube. F (M). Therefore, the corresponding viscosity profiles of the cladding tube and the outer cylinder show the same viscosity on both sides at the contact surface K.

Claims

1. 1. A method for making an anti-resonant hollow-core fiber having a hollow core extending along a longitudinal axis of the fiber and an inner cladding region surrounding the hollow core, the inner cladding region including a plurality of anti-resonant elements, comprising: (a) providing a primary preform (1) for a hollow-core fiber, said hollow-core fiber including at least one cladding tube (3) having a cladding tube inner bore and a cladding tube longitudinal axis along which extends a cladding tube wall defined by an inner side and an outer side; (b) forming a plurality of precursors or preforms (4) for anti-resonant elements at targeted locations on the cladding wall; (c) further processing the primary preform (1) into a secondary preform from which the hollow-core fiber is drawn, the further processing including one or more repeated collapses of additional cladding material in the form of an outer cylinder (2), the outer cylinder (2) having an inner side facing the cladding tube (3), an outer side, and an outer cylinder wall located between the inner side and the outer side; A manufacturing method comprising:

4. A method according to claim 3, wherein for further processing the primary preform (1) according to step (c), the outer layer cylinder (2) is used, which has a radial viscosity profile in which the viscosity at the outer layer cylinder wall increases from a viscosity minimum η(Z min ) towards the inside of the outer layer cylinder.

2. 2. The method according to claim 1, characterized in that the viscosity in the region inside the outer cylinder has a value η(Z) and the viscosity in the region outside the cladding has a viscosity η(M), and at a measurement temperature of 1250°C the following holds true for the viscosity values ​​(when the viscosity is expressed as a logarithmic value in dPa.s): η(M)=η(Z)±0.5 dPa.s.

3. The method described in claim 2, characterized in that the following holds for the viscosity value (when the viscosity is expressed as a logarithmic value in units of dPa.s): η(M) = η(Z) ± 0.3 dPa.s.

4. The minimum viscosity value η(Z min ) (when viscosity is expressed as a logarithmic value): η(M) - η(Z min 2. The method according to claim 1, wherein the following holds true: 1.) > 0.8 dPa·s.

5. The method according to claim 4, wherein the minimum viscosity η(Z min ) at a measurement temperature of 1250° C. satisfies (when the viscosity is expressed as a logarithmic value): η(M)−η(Z min )>1 dPa·s.

6. 2. The method of claim 1, wherein the cladding tube (3) has a radial viscosity profile in which the viscosity gradually increases inward between the cladding tube outside and the cladding tube inside.

7. The cladding tube (3) has a maximum viscosity η(M max ), and in step (b), at least a portion of the anti-resonant element preform (4) or the precursor to the anti-resonant element is present as a tubular anti-resonant element preform (4), the anti-resonant element preform (4) is made of silica glass, and the silica glass has a maximum viscosity η (M max 7. The method of claim 6, wherein the viscosity of the mixture is at least 0.4 dPa·s higher than that of the mixture.

8. The method described in claim 7, characterized in that at least a portion of the antiresonant element preform (4) or a precursor to the antiresonant element exists as a tubular antiresonant element preform (4), and the tubular antiresonant element preform (4) is composed of a plurality of structural elements nested together, including an ARE outer tube (4a) and an ARE inner tube (4b) inserted therein.

9. 9. The method according to claim 1, wherein the outer layer cylinder (2) is made of silica glass and the viscosity profile of the outer layer cylinder (2) is produced by the addition of at least one dopant that reduces the viscosity of silica glass.

10. The method of claim 9, wherein the dopant contains fluorine, chlorine and / or hydroxyl groups.

11. 9. The method according to claim 1, wherein the cladding tube (3) is made of silica glass and the viscosity profile of the cladding tube (3) is produced by the addition of at least one dopant that reduces the viscosity of silica glass.

12. The method according to claim 10, characterized in that the silica glass of the outer cylinder (2) and of the cladding tube (3) contains fluorine as a dopant in a concentration of 500 to 8000 ppm by weight.

13. 9. The method according to claim 1, wherein the cladding tube (3) is produced in a two-stage drawing process without a forming tool in a vertical wire drawing method, in a first stage a starting hollow cylinder of glass is mechanically worked to adjust the final dimensions of the starting hollow cylinder, in a first drawing process with a longitudinal axis oriented in a vertical direction, the starting hollow cylinder is continuously fed into a first heating zone having a first heating zone length, softened in the heating zone in a zone-by-zone manner and an intermediate cylinder is drawn from the softened zone, and in a second drawing process with a longitudinal axis oriented in a vertical direction, the intermediate cylinder is continuously fed into a second heating zone having a second shorter heating zone length, softened in the second heating zone in a zone-by-zone manner and a continuous tube is drawn from the softened zone, and the cladding tube (3) is obtained by cutting the continuous tube.

14. 9. The method according to any one of claims 1 to 8, characterized in that a secondary preform is formed having an outer diameter in the range of 30 to 90 mm and / or a primary preform (1) is formed having an outer diameter in the range of 20 mm to 70 mm.

15. 9. The method according to claim 1, wherein forming a preform for an antiresonant element by step (b) comprises placing the antiresonant element preform (4) at a target position inside the cladding tube wall, characterized in that a positioning template having holding elements for positioning the antiresonant element preform (4) at the target position is used for the positioning.

16. 1. A method for making a preform for an anti-resonant hollow-core fiber having a hollow core extending along a longitudinal axis of the fiber and an inner cladding region including a plurality of anti-resonant elements and surrounding the hollow core, comprising: (a) providing a primary preform (1) for said hollow-core fiber, said hollow-core fiber including at least one cladding tube (3) having a cladding tube inner bore and a cladding tube longitudinal axis along which extends a cladding tube wall defined by an inner side and an outer side; (b) forming a plurality of precursors or preforms (4) for anti-resonant elements at targeted locations on the cladding wall; (c) further processing the primary preform (1) into a secondary preform for the hollow-core fiber, the further processing comprising one or more repeated collapses of additional cladding material in the form of an outer cylinder (2), the outer cylinder (2) having an inner side facing the cladding tube (3), an outer cylinder outer side, and an outer cylinder wall located between the inner side and the outer side; A manufacturing method comprising:

4. A method according to claim 3, wherein for further processing the primary preform (1) according to step (c), the outer layer cylinder (2) is used, which has a radial viscosity profile in which the viscosity at the outer layer cylinder wall increases from a viscosity minimum η(Z min ) towards the inside of the outer layer cylinder.

Citation Information

Patent Citations

  • Optical flow measurement hollow fiber, method for its production and its use

    DE102014011041A1

  • Glass preform for optical fiber and optical fiber

    JP2002053344A

  • Method of producing optical fiber preform

    JP2002284541A

  • Method for manufacturing optical fiber preform

    JP2003226539A

  • Method for manufacturing optical fiber

    JP2018150184A