Method for producing a particulate support material containing elemental silver and elemental ruthenium - Patents.com

A scalable method for producing particulate support materials with elemental silver and ruthenium using a water-insoluble carrier material and hydrazine reduction addresses efficiency issues, enabling diverse applications.

JP7583925B2Active Publication Date: 2024-11-14HERAEUS DEUTSCHLAND GMBH & CO KG
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023519895
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-10-28
Filing Date
2021-02-23
Publication Date
2024-11-14
Estimated Expiration
2041-02-23

AI Technical Summary

Technical Problem

Existing methods for producing particulate support materials with elemental silver and elemental ruthenium are not scalable to manufacturing levels and lack efficiency.

Method used

A method involving successive steps of contacting a water-insoluble particulate carrier material with aqueous solutions containing silver and ruthenium precursors, followed by reduction with hydrazine at a pH greater than 7, to form a free-flowing impregnated material, and subsequent removal of volatile components.

Benefits of technology

Enables the production of a scalable and efficient particulate support material with elemental silver and ruthenium, suitable for various applications including antimicrobial finishes and coatings.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a method for producing a particulate support material having silver and ruthenium, the method comprising the following steps: a) providing a water-insoluble particulate support material and silver and ruthenium precursors dissolved in water; b) contacting the particulate support material with an aqueous precursor solution to form an intermediate; c) contacting the intermediate with an aqueous hydrazine solution having a pH >7-14 to form an agglomerate comprising silver and ruthenium; d) optionally washing the resulting agglomerate; and e) removing water and other possible volatile components from the agglomerate.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an efficient method for producing a particulate support material having elemental silver and elemental ruthenium.

[0002] WO 2007 / 139735 A2 discloses a method for producing nano / microparticles with a core-shell structure. The particles comprise a non-metallic core with a shell of transition metal / precious metal. The transition metal / precious metal is selected from copper, nickel, silver, palladium, platinum, ruthenium, gold, osmium and rhodium. The particles can be produced by providing a solution of transition metal salt / precious metal salt, dispersing nano / microparticles in the salt solution, evaporating the solvent to obtain a slurry containing coated nano / microparticles, adding a reducing agent to the slurry, and drying the slurry.

[0003] WO 2007 / 142579 A1 discloses a polymer matrix comprising an electron donor and metal particles comprising at least one metal selected from the group consisting of palladium, gold, ruthenium, rhodium, osmium, iridium and platinum. The electron donor may be at least one base metal, for example silver. The preparation method disclosed is the sequential deposition of silver and at least one further metal selected from the group consisting of palladium, gold, ruthenium, rhodium, osmium, iridium and platinum. The deposition is carried out in each case from a suspension of the metal particles in question by contacting them with the polymer matrix.

[0004] WO 2009 / 044146(A1) discloses a material comprising metal nanoparticles supported on a porous polysaccharide derivative, the nanoparticles having a diameter of 1-30 nm. The metal of the nanoparticles may be a noble metal. The material may be produced by adding the porous polysaccharide to a solvent, adding a salt of the metal, stirring the mixture at an elevated temperature, and separating the supported nanoparticles from the mixture.

[0005] The object of the present invention was to provide an efficient method that can be scaled up to production level for producing particulate support materials with elemental silver and elemental ruthenium. The support materials thus loaded can be used as additives for antimicrobial finishing in or on a very wide variety of materials and substances, such as metal surfaces, coatings, plasters, moulding compounds, plastics, synthetic resin products, silicone products, foams, textiles, cosmetics, hygiene products and much more.

[0006] This object is achieved by a method for producing a particulate support material comprising elemental silver and elemental ruthenium, the method comprising the following successive steps: a) providing a water-insoluble particulate support material and (i) an aqueous solution A containing a dissolved silver precursor (for brevity, also referred to as simply "aqueous solution A" in the following description and claims) and an aqueous solution B containing a dissolved ruthenium precursor (for brevity, also referred to as simply "aqueous solution B" in the following description and claims), or (ii) an aqueous solution containing both a dissolved silver precursor and a dissolved ruthenium precursor (for brevity, also referred to as simply "aqueous solution C" in the following description and claims); b) contacting the water-insoluble particulate support material with (i) aqueous solution A and aqueous solution B, or preferably (ii) aqueous solution C, to form an intermediate, preferably an intermediate in the form of a free-flowing impregnated particulate material; c) contacting the intermediate with an aqueous solution containing hydrazine having a pH in the range of >7-14, preferably >11-14, to form an agglomerate containing elemental silver and elemental ruthenium; d) optionally washing the mass obtained after completion of step c), and e) removing water and other possible volatile components from the mass obtained after completion of step c) or d).

[0007] From another point of view, the process according to the invention can also be understood as a process for providing a particulate support material comprising elemental silver and elemental ruthenium, comprising the successive steps a) to e).

[0008] Steps a) to e) are consecutive steps and may be directly successive steps without intermediate steps.

[0009] In step a) of the method according to the invention, a water-insoluble particulate support material is provided, and (i) said aqueous solutions A and B, or (ii) said aqueous solution C. It is preferred to provide aqueous solution C. It is self-evident to the skilled person that the particulate support material is present in the solid state of matter.

[0010] The support material particles can have a wide variety of particle shapes. For example, they may be irregularly shaped or they may have a defined shape, for example spherical, ellipsoidal, platelet-like or rod-like. The support material particles may be porous and / or have cavities or none of these. They may have a smooth, rough or structured outer surface. The support material particles may have an average particle size (d50) in the range of, for example, 20-100 μm. The term "average particle size" means an average particle size (d50) that can be determined by laser diffraction. Laser diffraction measurements can be performed using a corresponding particle size measuring device, for example a Mastersizer 3000 from Malvern Instruments. The absolute particle sizes are generally 1 μm or more, and they generally do not exceed 1000 μm.

[0011] The water-insoluble particulate carrier material has a more or less large water absorption capacity between the particles and optionally also within the particles, for example within the pores and / or cavities on the particle surface. The water-insoluble particulate carrier material may be water-swellable or even capable of forming a hydrogel with water.

[0012] From the term "water-insoluble carrier material" it is already clear to the skilled person that the water-insoluble actual carrier material is impermeable not only to water but also to the chemicals that come into contact in the method according to the invention, otherwise it cannot in principle perform the function of a carrier material or the function of a water-insoluble carrier material well. It is selected so that it is not attacked, dissolved or its properties as a carrier material are not impaired by water or by the said chemicals or combinations of chemicals. The water-insoluble actual carrier material itself is preferably a non-water-repellent material. It is preferably hydrophilic but in each case water-insoluble as described. The actual carrier material may be a material selected from inorganic or organic substances or materials and in each case may be in the form of particles, for example a powder. For the avoidance of doubt, the carrier material is a silver-free and ruthenium-free material or a silver-free and ruthenium-free material. Examples include glasses, nitrides such as aluminum nitride, titanium nitride, silicon nitride, high melting point oxides such as aluminum oxide, titanium dioxide, for example silica or quartz silicon dioxide, silicates such as sodium aluminum silicate, zirconium silicate, zeolites, plastics such as (meth)acrylic homopolymers and copolymers and polyamides, modified or unmodified naturally occurring polymers such as polysaccharides and polysaccharide derivatives, in particular cellulose and cellulose derivatives, carbon substrates, in particular porous carbon substrates and wood.

[0013] Cellulose powder, especially in the form of linear cellulose fibres, for example having fibre lengths in the range 10 to 1000 μm, is a preferred particulate support material.

[0014] The aqueous solution A provided in step a)(i) contains a dissolved silver precursor and the aqueous solution B, also provided in step a)(i), contains a dissolved ruthenium precursor.

[0015] The term "aqueous solution A" already makes it clear to the skilled person that this is a solution and not, for example, a dispersion, in other words, aqueous solution A typically does not contain undissolved substances, i.e., does not contain any sediment or precipitate. Aqueous solution A is characterized in that, in addition to water as a solvent, it also contains one or more silver(I) compounds dissolved therein. The silver(I) compounds and any desired or undesired substances present in aqueous solution A are typically selected such that aqueous solution A as it is, and preferably also in combination with or in contact with aqueous solution B, does not contain or does not form any sediment or precipitate.

[0016] The term "aqueous solution B" already makes it clear to the skilled person that this is a solution and not, for example, a dispersion, in other words, aqueous solution B typically does not contain undissolved substances, i.e. does not contain any sediment or precipitate. Aqueous solution B is characterized in that, in addition to water as a solvent, it also contains one or more ruthenium compounds dissolved therein. The ruthenium compounds and any desired or undesired substances present in aqueous solution A are typically selected such that aqueous solution B, as it is, and preferably also together with or in contact with aqueous solution A, does not contain or does not form any sediment or precipitate.

[0017] Preferably, the aqueous solution C provided in step a)(ii) contains both dissolved silver precursor and dissolved ruthenium precursor. From the term "aqueous solution C", it is already clear to the skilled person that this is a solution, not, for example, a dispersion, in other words, the aqueous solution C does not contain undissolved substances, i.e., does not contain sediments or precipitates. The aqueous solution C is characterized in that, in addition to water as a solvent, it also contains one or more silver(I) compounds dissolved therein and one or more ruthenium compounds dissolved therein. The silver(I) compounds and ruthenium compounds and any desired or undesired substances present in the aqueous solution C are selected so that the aqueous solution C does not contain or form sediments or precipitates.

[0018] The silver precursor and the ruthenium precursor are one or more silver(I) compounds and one or more ruthenium compounds selected from the group consisting of ruthenium(II) compounds, ruthenium(III) compounds and ruthenium(IV) compounds, in particular they are ruthenium(III) compounds.

[0019] Silver(I) compounds and ruthenium compounds that function as silver and ruthenium precursors are compounds that can generate elemental silver or elemental ruthenium from them by the reducing agent hydrazine. Examples include silver acetate, silver nitrate, silver sulfate, ruthenium acetate and ruthenium nitrosyl nitrate. Ruthenium chloride is suitable as a component of aqueous solution B, but is not preferred therein, and it is not suitable as a component of aqueous solution C. A particularly preferred combination of the precursors is the combination of silver nitrate and ruthenium nitrosyl nitrate, both together in aqueous solution C, and the combination of aqueous solution A and aqueous solution B.

[0020] The aqueous solutions A and B provided separately are used in combination in step b), and in this combination, the weight ratio is, for example, in the range of 1 to 2000 parts by weight of silver: 1 part by weight of ruthenium.

[0021] The weight fraction of silver in the aqueous solution A is, for example, in the range of 0.5 to 20 wt % (weight %).

[0022] The weight fraction of ruthenium in aqueous solution B is, for example, in the range of 0.5 to 20 wt %.

[0023] The weight ratio of silver:ruthenium in aqueous solution C is, for example, in the range of 1 to 2000 parts by weight of silver:1 part by weight of ruthenium, with generally a significant predominance of silver. This weight ratio of silver:ruthenium is also found in the process product obtained after completion of step e), i.e. in the particulate support material comprising elemental silver and elemental ruthenium.

[0024] The weight fraction of silver + ruthenium in the aqueous solution C is, for example, in the range of 0.5 to 20 wt %.

[0025] In step b) of the process according to the invention, the water-insoluble particulate support material is contacted with (i) aqueous solutions A and B, or preferably (ii) aqueous solution C, to form an intermediate, preferably an intermediate in the form of a free-flowing impregnated particulate material.

[0026] The intermediate is a mixture of a water-insoluble particulate carrier material with (i) aqueous solutions A and B, or preferably with (ii) aqueous solution C. Depending on the mixing ratio, the intermediate may have different morphologies, for example in the form of a pulp-like, paste-like or dough-like mass, or in the form of a slurry. However, in a preferred embodiment, the intermediate is a free-flowing impregnated particulate material, and step b) is designed accordingly.

[0027] The term "free-flowing impregnated particulate material" as used herein describes material in the form of grains or flakes that have been impregnated with (i) aqueous solutions A and B, or, preferably, (ii) aqueous solution C, each of which grains or flakes may comprise or consist of one or more particles of the original particulate support material. The free-flowing impregnated particulate material is not a liquid, liquid dispersion or suspension; rather, it is a free-flowing material such as a free-flowing powder.

[0028] The free flowability of the free-flowing impregnated particulate material can be investigated by rotational powder analysis. For this purpose, a cylindrical measuring drum can be filled with a predefined volume of the free-flowing impregnated particulate material. The measuring drum has a predefined diameter and a predefined depth. The measuring drum rotates around a horizontally oriented cylindrical axis at a predefined constant speed. One of the two end faces of the cylinder, which together enclose the free-flowing impregnated particulate material filled in the cylindrical measuring drum, is transparent. Before the start of the measurement, the measuring drum is rotated for 60 seconds. In the actual measurement, images of the free-flowing impregnated particulate material are then taken during the rotation using a camera along the axis of rotation of the measuring drum at a high frame rate, for example 5 to 15 images per second. The camera parameters can be selected so that the highest possible contrast is obtained at the material-air interface. During the rotation of the measuring drum, the free-flowing impregnated particulate material is carried against gravity to a certain height and then falls to the bottom of the drum. The fall occurs in a sliding (discontinuous) manner, also called an avalanche. The measurement is terminated when a statistically relevant number of avalanches, for example 200-400 avalanche slides, have been recorded. The camera images of the free-flowing impregnated particulate material are subsequently evaluated by digital image analysis. In rotational powder analysis, the "avalanche angle" and the time interval between two avalanches ("avalanche time") can be determined as parameters characteristic of free flow. The avalanche angle is the angle of the material surface when the avalanche falls and therefore represents a measure of the height to which the free-flowing impregnated particulate material piles up before this pile collapses in the manner of an avalanche. The time interval between two avalanches corresponds to the time elapsed between the occurrence of two avalanches. A suitable tool for carrying out said rotational powder analysis and for determining the avalanche angle and the time interval between two avalanches is the Revolution Powder Analyzer manufactured by PS Prozesstechnik GmbH, Neuhausstrasse 36, CH-4057 Basel. The operating instructions and recommendations included with the instrument must be followed. Typically, the measurements are carried out at room temperature or at 20 °C.The free-flowing impregnated particulate material formed in step b) of the method according to the invention may have an avalanche angle in the range of 40 to 80 degrees, determined using a test amount of 100 mL of the free-flowing impregnated particulate material, using the apparatus at 0.5 rpm and using a cylinder having an internal depth of 35 mm and an internal diameter of 100 mm, in which the time interval between two avalanches may for example be in the range of 2 to 5 seconds, which may represent another characteristic of the free flowability of the free-flowing impregnated particulate material.

[0029] The particulate support material can be added to aqueous solution A and / or aqueous solution B, or vice versa. Sequential, alternating or simultaneous addition of aqueous solutions A and B to the particulate support material charged first is preferred. Generally, mixing is performed during and also after the addition, e.g. by stirring.

[0030] In the preferred case of working with aqueous solution C, the particulate support material may be added to aqueous solution C, or vice versa. Here, it is preferred that aqueous solution C is added to the particulate support material which is initially charged. Generally, mixing is performed during and also after the addition, for example by stirring.

[0031] In a preferred embodiment of the formation of an intermediate in the form of a free-flowing impregnated particulate material, it is important that step b) is carried out in such a way that, after completion of step b), neither a pulp-like, paste-like or dough-like mass nor a slurry results, but rather a free-flowing impregnated particulate material is formed in the form of a macroscopically homogeneous product. The free flowability of the free-flowing impregnated particulate material may depend, for example, on its particle size, the surface properties of the particles, and the content of the particles in aqueous solution A+aqueous solution B or aqueous solution C.

[0032] When carrying out step b), it is appropriate to allow sufficient time for mixing of the particulate support material with (i) aqueous solution A and aqueous solution B, or (ii) aqueous solution C. For example, it is appropriate to mix, in particular stir, for a sufficient time after the addition is completed. In the case of the preferred embodiment of the formation of an intermediate in the form of a free-flowing impregnated particulate material, it is appropriate to mix until the mixed material is homogeneous, in particular visually homogeneous, when viewed macroscopically. The actual addition may be carried out, for example, as a metered addition with mixing. Generally applicable time information regarding the metered addition rate and the mixing time cannot be specified here, since it depends on the relevant batch size and the type of ingredients to be mixed, in particular the type of particulate support material.

[0033] When step b) is carried out according to the preferred embodiment, the volumes of (i) aqueous solutions A and B or (ii) aqueous solution C can be selected according to the relevant concentrations of the amount of particulate support material to be contacted therewith and its absorption behavior for the aqueous solutions. Such a procedure can contribute to the fact that in the subsequent step c), elemental silver and elemental ruthenium can be deposited as completely as possible in and / or attached to the particulate support material. If too large volumes are selected, the above-mentioned less preferred or even undesirable pulps, doughs, pastes or slurries will result instead of the preferred intermediate form of a free-flowing impregnated particulate material. The skilled person can easily determine the absorption behavior of the relevant particulate support material for the corresponding aqueous solutions in the application of laboratory experiments and can therefore determine the upper limit of the number of liters of aqueous solution per kilogram of particulate support material without any loss of free flowability. Generally applicable information on the absorption behavior of the particulate support material for (i) aqueous solutions A and B or (ii) aqueous solution C cannot be produced here, since it depends on the nature of the components to be mixed, and in particular on the nature of the particulate support material.

[0034] Preferably, the successive steps b) and c) are direct successive steps without any intermediate step, in particular without any removal of water therebetween from the intermediate, which is preferably present in the form of a free-flowing impregnated particulate material.

[0035] In step c) of the process according to the invention, the intermediate obtained after completion of step b), or the preferred free-flowing impregnated particulate material, is contacted with an aqueous solution having a pH in the range of >7-14, preferably >11-14, and comprising hydrazine (for brevity, also referred to as simply "aqueous hydrazine solution" in the following description and claims) to form an agglomerate comprising elemental silver and elemental ruthenium.

[0036] The pH of the aqueous hydrazine solution is particularly preferably in the range of 12-14.

[0037] The basic pH of the aqueous hydrazine solution can be adjusted with a strong base, in particular with a corresponding amount of an alkali metal hydroxide, especially sodium hydroxide or potassium hydroxide.

[0038] In preparing the aqueous hydrazine solution, hydrazine can be added as such, more precisely as hydrazine hydrate, or as a hydrazinium salt, for example hydrazinium chloride or, preferably, hydrazinium sulfate, from which it is released by means of a strong base.

[0039] The hydrazine concentration of the aqueous hydrazine solution is, for example, in the range of about 0.1 to 5 wt %, typically in the range of 0.2 to 1 wt %.

[0040] Generally, the aqueous hydrazine solution does not contain any other components than water, hydrazine, and a base. When the hydrazine is derived from a hydrazinium salt, the corresponding salt formed from the base and the hydrazinium salt is also included.

[0041] One mole of the reducing agent hydrazine can deliver 4 moles of electrons with a reducing effect, thus releasing 1 mole of N2 upon reduction. Thus, for example, 1 mole of Ag+ To reduce Ru, 0.25 moles of hydrazine are required, and 1 mole of Ru 3+ To reduce this, 0.75 moles of hydrazine are required.

[0042] The aqueous hydrazine solution is contacted with the intermediate or free-flowing, impregnated particulate material in an amount equal to or greater than the stoichiometrically required amount to completely reduce the silver and ruthenium precursors contained therein, but preferably in an amount up to 110% of the amount stoichiometrically required.

[0043] In this case, the aqueous hydrazine solution may be added to the intermediate or to the free-flowing impregnated particulate material, or vice versa. It is preferred to add the aqueous hydrazine solution to the intermediate introduced first or to the free-flowing impregnated particulate material introduced first. The addition can be carried out, for example, at a temperature in the range of 15-50° C. The reduction of the silver and ruthenium precursors to elemental silver and elemental ruthenium occurs directly on contact with hydrazine. The reduction of the silver and ruthenium precursors occurs simultaneously. During the addition, and preferably also after the end of the addition, mixing is usually carried out, for example by kneading and / or stirring, for example up to 1 hour after the end of the addition. Generally, the end of the reduction can be recognized by the fact that nitrogen is no longer released.

[0044] The method can be carried out so that the mass containing elemental silver and elemental ruthenium formed in step c) is a suspension or slurry. However, the method can also be carried out so that the mass containing elemental silver and elemental ruthenium formed in step c) contains only a small amount of free liquid, or even no free liquid at all, for example, for this purpose, one can work with an aqueous hydrazine solution with a volume adjusted according to the concentration. "No free liquid" means that the mass containing elemental silver and elemental ruthenium does not undergo phase separation in the sense that a separate aqueous phase forms as a supernatant above the mass containing elemental silver and elemental ruthenium, even after 10 minutes, at rest.

[0045] In an optional but preferred step d) of the process according to the invention, the agglomerates containing elemental silver and elemental ruthenium obtained after completion of step c) may be washed, in particular by washing with water, in order to remove water-soluble components such as base, any excess hydrazine and other water-soluble components.

[0046] In step e) of the process according to the invention, water and any other volatile components present are removed from the mass obtained after completing step c) or from the washed mass obtained after completing step d).

[0047] The removal of water can take place in the sense of substantially complete removal of water or in the sense of removal of water until a desired residual water content is reached. For this purpose, most of the water may first be removed by conventional methods such as squeezing, pressure filtration, straining, centrifugation or other methods acting in a similar manner, before drying, optionally assisted by reduced pressure, at a temperature in the range of, for example, 20 to 150° C.

[0048] As a direct product of the method according to the invention, i.e. after completion of step e), a particulate material or support material with elemental silver and elemental ruthenium is obtained. Depending on the nature of the particulate support material initially used, silver and ruthenium can be present on the inner surface (in the pores and / or cavities) and / or on the outer surface of the initial silver-free and ruthenium-free support material particles, for example forming continuous or discontinuous layers and / or small silver or ruthenium particles. In this case, silver and ruthenium are not present in the form of an alloy, but are rather randomly distributed. It is clear to the skilled person that silver and ruthenium can contain species of silver other than elemental metallic silver and species of ruthenium other than elemental metallic ruthenium on their surface, for example the corresponding oxides, halides and / or sulfides. Such species can be formed during the method according to the invention is carried out or thereafter, for example during storage, use or further processing of the process product. The silver+ruthenium weight fraction of the process product may vary within wide limits, for example within the range of 0.1-50 wt%, preferably 1-40 wt%, while the process product may have a silver:ruthenium weight ratio in the range of, for example, 1-2000 parts by weight of silver:1 part by weight of ruthenium. After reading the disclosure herein, the skilled person will understand which variable parameters and which possibilities for modification are applicable to them when carrying out the process according to the invention in order to produce a process product having the desired silver+ruthenium weight fraction at the desired silver:ruthenium weight ratio in the desired batch size, for example on a single ton scale. Using the example of a preferred method of carrying out the process using aqueous solution C, such variable parameters are in particular: The type and amount of particulate support material used in step b), the volume of aqueous solution C used in step b), weight ratio of silver:ruthenium in solution C, The weight fraction of silver + ruthenium in aqueous solution C, and Residual moisture in the process product obtained after completion of step e) is mentioned.

[0049] Thus, the first step for the skilled person is to first select the type of particulate support material and to determine the target values ​​for the silver and ruthenium contents in the final product. The skilled person then determines the batch size and selects the corresponding amounts of particulate support material that will have elemental silver and elemental ruthenium according to the procedure according to the invention. Once these selections are made, the other variable parameters can be defined accordingly and the method according to the invention can be carried out with aqueous solution C. Similar considerations apply when carrying out the method with aqueous solutions A and B.

[0050] For example, when cellulose powder is used as the particulate support material, the method according to the invention can be used to produce cellulose powders with elemental silver and elemental ruthenium weight fractions in the range of, for example, 0.1-50 wt%, preferably 1-40 wt%, silver+ruthenium, with batch sizes in the range of, for example, up to 5 tonnes, effectively with a silver:ruthenium weight ratio in the range of, for example, 1-2000 parts by weight silver:1 part by weight ruthenium.

[0051] The invention also relates to the products produced by the process according to the invention, and their use as additives for the antimicrobial finishing of metal surfaces, coatings, plasters, moulding compounds, plastics in the form of plastic films, plastic parts or plastic fibres, synthetic resin products, ion exchange resins, silicone products, cellulosic products, foams, textiles, cosmetics, hygiene products and many other articles. The cellulosic products can be selected, for example, from the group consisting of paper products, paperboard, wood fibre products and cellulose acetate, and the plastics can be selected, for example, from the group consisting of ABS plastics, PVC (polyvinyl chloride), polylactic acid, PU (polyurethane), poly(meth)acrylate, PC (polycarbonate), polysiloxanes, phenol formaldehyde resins, melamine formaldehyde resins, polyesters, polyamides, polyethers, polyolefins, polystyrenes, hybrid polymers thereof and mixtures thereof.

[0052] Example 1 (Preparation of a cellulose powder with 18.3 wt% elemental silver and 0.2 wt% elemental ruthenium): 132.45 g of an aqueous silver nitrate solution (silver content 36.24 wt%, 445 mmol Ag) and 2.60 g of an aqueous ruthenium nitrosyl nitrate solution (ruthenium content 19.0 wt%, 4.9 mmol Ru) were added to 364.5 g of demineralized water, and the thus obtained aqueous precursor solution was mixed homogeneously with 211.2 g of cellulose powder (Vitacel® L-600, J. Rettenmaier and Soehne GmbH&Co KG) to obtain an orange free-flowing impregnated particulate material. Rotational powder analysis was performed on 100 mL of this material using a Revolution Powder Analyzer from PS Prozesstechnik GmbH (Neuhausstrasse 36, CH-4057 Basel) at 0.5 rpm, a cylinder with an internal depth of 35 mm and an internal diameter of 100 mm, at 20° C., and 300 avalanches were recorded at a frame rate of 10 images / s. The avalanche angle thus determined was 75 degrees and the time interval between two avalanches was 3.6 seconds. 705 mL of an aqueous hydrazine solution with a pH of 14 [3.68 g (115 mmol) of hydrazine and 71.82 g of 32 wt% sodium hydroxide solution (575 mmol of NaOH), the remainder being water] was added to the free-flowing impregnated particulate material at room temperature with stirring at a metered addition rate of 30 mL / min. Over time, a black homogeneous pulp was formed which became increasingly easier to stir. After completion of the metered addition, stirring was continued for 30 min until nitrogen evolution could no longer be observed. The material was subsequently filtered off, washed with a total of 1000 mL of water and dried in a drying cabinet at 105 °C / 300 mbar to a residual moisture content of 15 wt%. The silver content of the final product (based on 0 wt% residual moisture) was determined to be 18.3 wt% and the ruthenium content was 0.19 wt% by ICP-OES.

[0053] Example 2 (Preparation of a cellulose powder having 10.9 wt% elemental silver and 0.2 wt% elemental ruthenium): 97.96 g of an aqueous solution of silver nitrate (silver content 36.24 wt%, 329 mmol Ag) and 3.68 g of an aqueous solution of ruthenium nitrosyl nitrate (ruthenium content 19.0 wt%, 6.9 mmol Ru) were added to 554.9 g of demineralized water, and the thus obtained aqueous precursor solution was mixed homogeneously with 299.2 g of cellulose powder (Vitacel® L-600, J. Rettenmaier and Soehne GmbH&Co KG) to obtain an orange free-flowing impregnated particulate material. Rotational powder analysis was performed on 100 mL of this material with a Revolution Powder Analyzer from PS Prozesstechnik GmbH (Neuhausstrasse 36, CH-4057 Basel) at 0.5 rpm, using a cylinder with an internal depth of 35 mm and an internal diameter of 100 mm, at 20° C., with a frame rate of 10 images / s, and 300 avalanches were recorded. The avalanche angle thus determined was 68 degrees and the time interval between two avalanches was 3.0 seconds. To the free-flowing impregnated particulate material, 999.9 mL of an aqueous hydrazine solution with a pH of 13.8 [2.80 g (88 mmol) hydrazine and 54.66 g of 32 wt% sodium hydroxide solution (437 mmol NaOH), the remainder water] was added at room temperature with stirring at a metered addition rate of 30 mL / min. Over time, a black homogeneous pulp was formed which became increasingly easier to stir. After completion of the metered addition, stirring was continued for 30 min until nitrogen evolution could no longer be observed. The material was subsequently filtered off, washed with a total of 1000 mL water and dried in a drying cabinet at 105 °C / 300 mbar to a residual moisture content of 15 wt%. The silver content of the final product (based on 0 wt% residual moisture) was determined to be 10.88 wt% and the ruthenium content was 0.21 wt% by ICP-OES.

[0054] Example 3 (Preparation of a cellulose powder having 18.9 wt% elemental silver and 1.0 wt% elemental ruthenium): 75.6 g (445 mmol) of silver nitrate solid and 13.94 g of ruthenium nitrosyl nitrate solution (ruthenium content 19.0 wt%, 26.2 mmol of Ru) were dissolved in 416.8 g of demineralized water, and the thus obtained aqueous precursor solution was mixed homogeneously with 211.2 g of cellulose powder (Vitacel® L-600, J. Rettenmaier and Soehne GmbH&Co KG) to obtain an orange free-flowing impregnated particulate material. Rotational powder analysis was performed on 100 mL of this material using a Revolution Powder Analyzer from PS Prozesstechnik GmbH (Neuhausstrasse 36, CH-4057 Basel) at 0.5 rpm, a cylinder with an internal depth of 35 mm and an internal diameter of 100 mm, at 20° C., and 300 avalanches were recorded at a frame rate of 10 images / s. The avalanche angle thus determined was 73 degrees and the time interval between two avalanches was 3.5 seconds. 705 mL of an aqueous hydrazine solution with a pH of 13.9 [4.19 g (131 mmol) hydrazine and 81.81 g of 32 wt% sodium hydroxide solution (654.51 mmol NaOH), the remainder water] was added to the free-flowing impregnated particulate material at room temperature with stirring at a metered addition rate of 30 mL / min. Over time, a black homogeneous pulp was formed which became increasingly easier to stir. After completion of the metered addition, stirring was continued for 30 min until nitrogen evolution could no longer be observed. The material was subsequently filtered off, washed with a total of 1000 mL water and dried in a drying cabinet at 105 °C / 300 mbar to a residual moisture content of 15 wt%. The silver content of the final product (based on 0 wt% residual moisture) was determined to be 18.9 wt% and the ruthenium content was 1.0 wt% by ICP-OES.

Claims

1. A method for producing a particulate support material comprising elemental silver and elemental ruthenium, comprising the following successive steps: a) providing a water-insoluble particulate support material and (i) an aqueous solution A containing a dissolved silver precursor and an aqueous solution B containing a dissolved ruthenium precursor, or (ii) an aqueous solution C containing both a dissolved silver precursor and a dissolved ruthenium precursor; b) contacting the water-insoluble particulate support material with (i) aqueous solution A and aqueous solution B, or (ii) aqueous solution C to form an intermediate; c) contacting the intermediate with an aqueous solution having a pH in the range of 7 to 14 and comprising hydrazine to form an agglomerate comprising elemental silver and elemental ruthenium; d) optionally washing the mass obtained after completion of step c), and e) removing water and other possible volatile components from the mass obtained after completion of step c) or d).

2. The method of claim 1 , wherein the intermediate is a free-flowing impregnated particulate material.

3. 3. The method of claim 2, wherein the free-flowing impregnated particulate material has the form of grains or flakes impregnated with (i) aqueous solution A and aqueous solution B, or (ii) aqueous solution C.

4. 4. The method of claim 2 or 3, wherein the free-flowing, impregnated particulate material has an avalanche angle in the range of 40 to 80 degrees as determined by rotational powder analysis on 100 mL of the free-flowing, impregnated particulate material at 20° C. using a Revolution Powder Analyzer from PS Prozesstechnik GmbH at 0.5 rpm, using a cylinder having an internal depth of 35 mm and an internal diameter of 100 mm.

5. The method of claim 4, wherein the free-flowing impregnated particulate material is further characterized in that the time interval between two avalanches is in the range of 2 to 5 seconds.

6. A method according to any one of claims 1 to 5, wherein the water-insoluble particulate carrier material is water-swellable or capable of forming a hydrogel.

7. 6. The method according to any one of claims 1 to 5, wherein the material of the water-insoluble particulate support material is selected from the group consisting of glasses, nitrides, oxides, silicates, plastics, modified or unmodified naturally occurring polymers, carbon substrates and wood.

8. A method according to any one of claims 1 to 5, wherein the water-insoluble particulate carrier material is a cellulose powder.

9. 9. The method of any one of claims 1 to 8, wherein the silver and ruthenium precursors are one or more silver(I) compounds and one or more ruthenium compounds selected from the group consisting of ruthenium(II) compounds, ruthenium(III) compounds and ruthenium(IV) compounds.

10. 10. The method according to claim 1, wherein the weight ratio of silver:ruthenium in the combination of aqueous solution A and aqueous solution B or in aqueous solution C used in step b) is in the range of 1-2000 parts by weight of silver:1 part by weight of ruthenium.

11. 11. The method according to claim 1, wherein the weight fraction of silver + ruthenium in said aqueous solution C is in the range of 0.5 to 20 wt. %.

12. The method according to any one of claims 1 to 11, wherein the hydrazine concentration of the aqueous hydrazine solution is in the range of 0.1 to 5 wt%.

13. The method according to any one of claims 1 to 12, wherein the aqueous hydrazine solution is contacted with the intermediate in an amount equal to or greater than the stoichiometric amount required to completely reduce the silver and ruthenium precursors contained in the intermediate.

14. 14. Use of a particulate support material with elemental silver and elemental ruthenium produced by the method according to any one of claims 1 to 13 as an additive for the antimicrobial finishing of metal surfaces, coatings, plasters, moulding compounds, plastics in the form of plastic films, plastic parts or plastic fibres, synthetic resin products, ion exchange resins, silicone products, cellulosic products, foams, textiles, cosmetics and hygiene products.

15. 15. The use according to claim 14, wherein the cellulosic product is selected from the group consisting of paper products, paperboard, wood fiber products and cellulose acetate.

16. 15. The use according to claim 14, wherein the plastic is selected from the group consisting of ABS plastic, PVC, polylactic acid, PU, ​​poly(meth)acrylate, PC, polysiloxane, phenol formaldehyde resin, melamine formaldehyde resin, polyester, polyamide, polyether, polyolefin, polystyrene, hybrid polymers thereof, and mixtures thereof.

Citation Information

Patent Citations

  • Composition for forming electrode, and method for forming electrode by using the composition

    JP2015117434A

  • Production method of antimicrobial agent and production method of photocatalyst composite material

    JP2017125058A

  • Core shell particle and use thereof

    JP2020158864A

  • Method for manufacturing metal particles with core-shell structure and metal particles with core-shell structure manufactured using the same

    KR1020150142276A

  • Multicomponent solid solution microparticles and method for producing same, and catalyst

    US20200001370A1