Hexagonal boron nitride powder

The production of high-purity, low-specific surface area hexagonal boron nitride powder with controlled particle size addresses performance issues in mold release and heat dissipation, offering superior mold release and thermal conductivity with reduced impurity contamination.

JP7584434B2Active Publication Date: 2024-11-15DENKA CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021558344
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-11-19
Filing Date
2020-11-12
Publication Date
2024-11-15
Estimated Expiration
2040-11-12

AI Technical Summary

Technical Problem

Existing boron nitride powders face challenges in achieving high purity, low specific surface area, and controlled particle size, which affect their performance as mold release materials and heat dissipation fillers, and are prone to impurity metal contamination.

Method used

The production of hexagonal boron nitride powder with a purity of 98% by mass or more, specific surface area less than 2.0 m^2/g, and controlled average particle size of 2.0 to 35 μm, with low impurity metals like sodium and calcium, achieved through a carbon reduction method under controlled pressure and temperature conditions.

Benefits of technology

The resulting hexagonal boron nitride powder exhibits excellent mold release properties, improved thermal conductivity, and enhanced fillability, making it suitable for diverse applications including mold release materials and heat dissipation fillers with reduced impurity effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007584434000001
    Figure 0007584434000001
  • Figure 0007584434000002
    Figure 0007584434000002
Patent Text Reader

Abstract

One aspect of the present disclosure provides hexagonal boron nitride powder having a purity of at least 98 mass% and a specific surface area of less than 2.0 m2 / g.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to hexagonal boron nitride powder. [Background technology]

[0002] Boron nitride has excellent lubricity, high thermal conductivity, and insulating properties, etc. Therefore, boron nitride is used in various applications such as a solid lubricant, a release agent for molten gas and aluminum, a filler for heat dissipation materials, and a raw material for sintered bodies.

[0003] Boron nitride powder is used as a release agent in the die casting of magnesium, aluminum, aluminum alloys, etc. For example, boron nitride powder is mixed with water together with a dispersant to prepare a slurry, and the slurry is applied to the surface of a die and baked to provide a release layer (e.g., Patent Documents 1 and 2, etc.). As die shapes become increasingly complex and precise, boron nitride powder used as a release agent is required to have better releasability.

[0004] Boron nitride powder is used as a heat dissipation material by improving its crystallinity. Primary particles of boron nitride that have been grown by improving their crystallinity have a scale shape. Therefore, the primary particles of boron nitride have thermal anisotropy derived from the shape. From the viewpoint of reducing the influence of anisotropy, the primary particles may be aggregated and boron nitride may be used as aggregated particles. A technique for producing aggregated particles by controlling the particle size of the primary particles to be small is known (e.g., Patent Document 3). In addition, a technique for producing spherical boron nitride fine particles of submicron size with high sphericity to be used as a filler for heat dissipation materials is known (e.g., Patent Document 4). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Publication No. 55-29506 [Patent Document 2] Japanese Patent Application Publication No. 63-270798 [Patent Document 3] JP 2016-60661 A [Patent Document 4] International Publication No. 2015 / 122379 Summary of the Invention [Problem to be solved by the invention]

[0006] The present disclosure aims to provide a highly versatile hexagonal boron nitride powder. The present disclosure also aims to provide a method for producing the above-mentioned hexagonal boron nitride powder. [Means for solving the problem]

[0007] One aspect of the present disclosure is a sintered body having a purity of 98% by mass or more and a specific surface area of ​​2.0 m 2 The present invention provides a hexagonal boron nitride powder having a molecular weight of less than 1.0 μm / g.

[0008] The hexagonal boron nitride powder is of high purity and has a specific surface area of ​​2.0 m 2 / g, it can be used for various purposes. For example, when used as a release agent, a dense release layer can be formed due to the small specific surface area, and excellent releasability can be exhibited. In addition, for example, when used as a heat dissipation filler, the required properties of the hexagonal boron nitride powder are the same as those of a release agent, and due to its high purity and low specific surface area, it can have excellent filling properties and excellent filler properties. Furthermore, even when used for cosmetic purposes, it can be a suitable raw material with excellent reliability due to its high purity as hexagonal boron nitride and low specific surface area.

[0009] The hexagonal boron nitride powder may have a total sodium and calcium content of less than 50 ppm, or may be 30 ppm or less. When the total sodium and calcium content in the hexagonal boron nitride powder is within the above range, it is useful as a release agent for use in the manufacture of electronic materials, for example, since it is possible to further suppress impregnation of impurity metals into products. When the total sodium and calcium content in the hexagonal boron nitride powder is within the above range, it is also useful as a heat dissipation material, since it is possible to further improve thermal conductivity.

[0010] The hexagonal boron nitride powder may have an average primary particle size of 2.0 to 35 μm, or may have an average primary particle size of 9.0 to 30 μm. By having the average primary particle size within the above range, a denser release layer can be formed, making the powder more useful as a release agent. Effect of the Invention

[0011] According to the present disclosure, it is possible to provide a highly versatile hexagonal boron nitride powder. According to the present disclosure, it is also possible to provide a method for producing the above-mentioned hexagonal boron nitride powder.

[0012] According to the present disclosure, for example, it is possible to provide a hexagonal boron nitride powder that is useful as a release agent or the like. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, embodiments of the present disclosure will be described. However, the following embodiments are merely examples for explaining the present disclosure, and are not intended to limit the present disclosure to the following contents.

[0014] In this specification, the numerical range indicated by "XX to △△" means "XX or more and △△ or less" unless otherwise specified. In this specification, "parts" and "%" are based on mass unless otherwise specified. In addition, in this specification, the unit of pressure is gauge pressure, and notations such as "G" or "gage" are omitted unless otherwise specified.

[0015] Unless otherwise specified, the materials exemplified in this specification can be used alone or in combination of two or more. When a plurality of substances corresponding to each component are present in the composition, the content of each component in the composition means the total amount of the plurality of substances present in the composition, unless otherwise specified.

[0016] One embodiment of the hexagonal boron nitride powder has a purity of 98% by mass or more and a specific surface area of ​​2.0 m 2 The hexagonal boron nitride powder can be used for various purposes, such as a solid lubricant, a release agent, a filler for heat dissipation materials, a raw material for cosmetics, and a raw material for sintered bodies.

[0017] The lower limit of the purity of the hexagonal boron nitride powder is 98% by mass or more, but may be, for example, 99% by mass or more. When the purity of the hexagonal boron nitride powder is within the above range, the melting point decrease caused by impurities is suppressed, so that, for example, when used as a release agent, the release property can be sufficiently maintained even when used at high temperatures. The purity of the hexagonal boron nitride powder is measured by the method described in the examples of the present specification.

[0018] The upper limit of the specific surface area of ​​hexagonal boron nitride powder is 2.0 m 2 / g, but for example, 1.5m 2 / g or less, or 0.8m 2 The lower limit of the specific surface area may be, for example, 0.1 m 2 / g or more, 0.2m 2 / g or more, or 0.3m 2 The specific surface area may be adjusted within the above range, for example, 0.1 m 2 / g or more 2.0m 2 / g or less, or 0.2-1.5m 2 The specific surface area of ​​the hexagonal boron nitride powder can be controlled, for example, by adjusting the heating temperature and heating time when the raw material powder is heat-treated to form primary particles.

[0019] In this specification, the specific surface area of ​​the hexagonal boron nitride powder is measured using a measuring device in accordance with JIS Z 8803: 2013. The specific surface area is a value calculated by applying the BET single point method using nitrogen gas.

[0020] The upper limit of the average particle size of the primary particles in the hexagonal boron nitride powder may be, for example, 35 μm or less, 30 μm or less, 25 μm or less, or 20 μm or less. When the upper limit of the average particle size of the primary particles is within the above range, for example, when used as a release material, the adhesion between the mold and the release layer can be further improved. In addition, by reducing the upper limit of the average particle size of the primary particles, the handleability can be improved when used as a filler for a heat dissipation material. The lower limit of the average particle size of the primary particles may be, for example, 2.0 μm or more, 4.0 μm or more, 6.0 μm or more, or 9.0 μm or more. When the lower limit of the average particle size of the primary particles is within the above range, for example, a denser release layer can be formed when used as a release material. The average particle size of the primary particles may be adjusted within the above range, and may be, for example, 2.0 to 35 μm, 2.0 to 30 μm, or 9.0 to 30 μm. The average particle size of the primary particles can be controlled by adjusting, for example, the composition of the raw material powder, the firing time of the raw material powder, and the like.

[0021] In this specification, the average particle size of the primary particles is measured in accordance with ISO 13320:2009 using a particle size distribution analyzer (manufactured by Nikkiso Co., Ltd., product name: MT3300EX). The average particle size obtained by the above measurement is the average particle size based on volume statistics, and the average particle size is the median value (d50). When measuring the particle size distribution, water is used as the solvent for dispersing the aggregates, and hexametaphosphoric acid is used as the dispersant. In this case, the refractive index of water is 1.33, and the refractive index of hexagonal boron nitride powder is 1.80.

[0022] The hexagonal boron nitride powder may have a low content of sodium and calcium. The total content of sodium and calcium may be, for example, less than 50 ppm, 40 ppm or less, 35 ppm or less, 30 ppm or less, 20 ppm or less, or 10 ppm or less. The total content of sodium and calcium may also be below the detection limit of a detection device. When the total content of sodium and calcium is within the above range, for example, when used as a release agent, it is possible to reduce the occurrence of color unevenness due to the influence of impurity metals on the surface of the product and the occurrence of deterioration of insulation properties due to the migration of impurity metals into the product. When the product is an electronic material, the effect of using the above-mentioned hexagonal boron nitride powder is more remarkable. The sodium and calcium content in the hexagonal boron nitride powder can be adjusted, for example, by the composition of the raw material powder and acid washing. In the production of hexagonal boron nitride powder, alkali metals or alkaline earth metals are often used as additives, and among them, sodium and calcium are often used. Therefore, these elements are easily manifested in the hexagonal boron nitride powder. Therefore, it is preferable to reduce the total content of sodium and calcium from the viewpoint of further improving the above-mentioned effects. In addition, while adjusting the total content of sodium and calcium to the above range, the sodium content may be 30 ppm or less, 20 ppm or less, or 10 ppm or less, and the calcium content may be 40 ppm or less, 30 ppm or less, or 20 ppm or less.

[0023] The hexagonal boron nitride powder may contain other metal elements in addition to sodium and calcium depending on the manufacturing method. Examples of other metal elements include manganese, iron, and nickel. The hexagonal boron nitride powder preferably has a low content of other metal elements. The hexagonal boron nitride powder may have a manganese, iron, and nickel content of 20 ppm or less, 10 ppm or less, or 5 ppm or less. The manganese, iron, and nickel contents may also be below the detection limit of a detection device.

[0024] In this specification, the metal content in the hexagonal boron nitride powder is measured by the pressure acid decomposition method of ICP emission spectrometry.

[0025] The hexagonal boron nitride powder may contain agglomerates formed by agglomeration of a plurality of primary particles depending on the manufacturing method, etc. When the hexagonal boron nitride powder contains the agglomerates, the content of the agglomerates may be, for example, 8 mass% or less, 5 mass% or less, 3 mass% or less, or 1.5 mass% or less based on the total amount of the hexagonal boron nitride powder. When the content of the agglomerates is within the above range, for example, when used as a release agent, a release layer with even better uniformity can be formed, and the release property of the release layer can be improved. The hexagonal boron nitride powder preferably does not contain the agglomerates.

[0026] The above-mentioned hexagonal boron nitride powder can be produced, for example, by the following method. One embodiment of the method for producing hexagonal boron nitride powder includes a first step of heat-treating a raw material powder containing a carbon-containing compound and a boron-containing compound in a gas atmosphere containing a compound having a nitrogen atom as a constituent element and under a pressure of 0.25 MPa or more and less than 5.0 MPa at a temperature of 1600°C or more and less than 1850°C to obtain a heat-treated product, and a second step of firing the heat-treated product at a temperature higher than that of the first step to obtain hexagonal boron nitride powder.

[0027] The first step is to produce boron nitride by pressurizing and heating a raw material powder containing a carbon-containing compound and a boron-containing compound in the presence of a compound having a nitrogen atom as a constituent element.

[0028] A carbon-containing compound is a compound having carbon atoms as a constituent element. The carbon-containing compound reacts with a boron-containing compound and a compound having nitrogen atoms as a constituent element to form boron nitride. As the carbon-containing compound, a raw material having high purity and relatively low cost can be used. Examples of such carbon-containing compounds include carbon black and acetylene black.

[0029] A boron-containing compound is a compound having boron as a constituent element. A boron-containing compound is a compound that reacts with a carbon-containing compound and a compound having a nitrogen atom as a constituent element to form boron nitride. As the boron-containing compound, a raw material having high purity and relatively low cost can be used. Examples of such a boron-containing compound include boric acid and boron oxide.

[0030] When the boron-containing compound contains boric acid, the above-mentioned production method may include, for example, a step of preparing a raw material powder, which may further include a step of dehydrating the boron-containing compound. By including the step of dehydrating the boron-containing compound, the yield of boron nitride obtained in the first step can be improved.

[0031] The raw material powder may contain other compounds in addition to the carbon-containing compound and the boron-containing compound. Examples of other compounds include boron nitride powder as a nucleating agent. When the raw material powder contains boron nitride powder as a nucleating agent, the average particle size of the synthesized boron nitride powder can be more easily controlled. The raw material powder preferably contains a nucleating agent. When the raw material powder contains a nucleating agent, it becomes easier to adjust the specific surface area of ​​the boron nitride powder, and the specific surface area is preferably 2.0 m. 2 This makes it easier to produce boron nitride powder with a molecular weight of less than 1 / g.

[0032] When using boron nitride powder as a nucleating agent, the content of the boron nitride powder as a nucleating agent may be, for example, 0.05 to 8 parts by mass based on 100 parts by mass of the raw material powder. By setting the lower limit of the content of the nucleating agent to 0.05 parts by mass or more, the effect of including the nucleating agent can be further improved. By setting the upper limit of the content of the nucleating agent to 8 parts by mass or less, the yield of the boron nitride powder can be improved.

[0033] The compound having a nitrogen atom as a constituent element is a compound that reacts with a carbon-containing compound and a boron-containing compound to form boron nitride. Examples of the compound having a nitrogen atom as a constituent element include nitrogen and ammonia. The compound having a nitrogen atom as a constituent element may be supplied in the form of a gas (also called a nitrogen-containing gas). From the viewpoint of promoting the formation of boron nitride by the nitriding reaction and from the viewpoint of reducing costs, the nitrogen-containing gas preferably contains nitrogen gas, and more preferably is nitrogen gas. When a mixed gas of multiple gases is used as the nitrogen-containing gas, the ratio of nitrogen gas in the mixed gas may preferably be 95 volume / volume% or more.

[0034] The first step is carried out under pressure. The lower limit of the pressure in the first step is 0.25 MPa or more, but may be, for example, 0.30 MPa or more, or 0.50 MPa or more. By setting the lower limit of the pressure in the first step within the above range, it is possible to suppress the generation of boron carbide as a by-product, and also to suppress an increase in the specific surface area of ​​the boron nitride powder. The upper limit of the pressure in the first step is less than 5.0 MPa, but may be, for example, 4.0 MPa or less, 3.0 MPa or less, 2.0 MPa or less, 1.0 MPa or less, or less than 1.0 MPa. By setting the upper limit of the pressure in the first step within the above range, it is possible to suppress a decrease in the amount of volatilization of boron oxide and shorten the firing time. The pressure in the first step may be adjusted within the above range, and may be, for example, 0.25 MPa or more and less than 5.0 MPa, 0.25 to 1.0 MPa, or 0.25 MPa or more and less than 1.0 MPa.

[0035] The first step is carried out under heating. The lower limit of the heating temperature in the first step is 1600°C or more, but may be, for example, 1650°C or more, or 1700°C or more. By setting the lower limit of the heating temperature in the first step within the above range, the reaction of the raw material powder can be promoted, and the yield of boron nitride obtained in the first step can be improved. By setting the lower limit of the heating temperature in the first step within the above range, metal elements such as sodium and calcium that may be mixed into the raw material powder (metal elements that will later become impurity metal elements) can be more sufficiently removed from the system. The upper limit of the heating temperature in the first step is, for example, less than 1850°C, but may be, for example, 1800°C or less, or 1750°C or less. By setting the upper limit of the heating temperature in the first step within the above range, the generation of by-products can be sufficiently suppressed. The heating temperature in the first step may be adjusted within the above range, and may be, for example, 1650°C or more and less than 1850°C, or 1650 to 1800°C. In the first step, the temperature increase rate is not particularly limited, but may be, for example, 0.5° C. / min or more.

[0036] The heating time in the first step may be, for example, 2 hours or more, or 3 hours or more. The heating time in the first step may also be, for example, 12 hours or less, 10 hours or less, or 8 hours or less. The heating time in the first step may be adjusted within the above-mentioned range, and may be, for example, 2 to 12 hours, or 2 to 10 hours. In this specification, the heating time means the time during which the temperature of the surrounding environment of the object to be heated is maintained at a predetermined temperature after the temperature reaches the predetermined temperature.

[0037] The second step is a step of further heating the heat-treated product containing boron nitride obtained in the first step at high temperature and pressure in the presence of a compound having nitrogen atoms as a constituent element to grow primary particles of boron nitride with enhanced crystallinity (primary particles of hexagonal boron nitride) and decarburize them. The primary particles of hexagonal boron nitride obtained by grain growth have a scale-like shape.

[0038] The second step is carried out under pressure. The pressure in the second step may be the same as or different from that in the first step. The lower limit of the pressure in the second step may be, for example, 0.25 MPa or more, 0.30 MPa or more, or 0.50 MPa or more. By setting the lower limit of the pressure in the second step within the above range, the purity of the obtained hexagonal boron nitride powder can be further improved. The upper limit of the pressure in the second step is not particularly limited, but may be, for example, less than 5.0 MPa, 4.0 MPa or less, 3.0 MPa or less, 2.0 MPa or less, 1.0 MPa or less, or less than 1.0 MPa. By setting the upper limit of the pressure in the second step within the above range, the production cost of the hexagonal boron nitride powder can be further reduced, which is industrially advantageous. The pressure in the second step may be adjusted within the above range, and may be, for example, 0.25 MPa or more and less than 5.0 MPa, 0.25 to 1.0 MPa, or 0.25 MPa or more and less than 1.0 MPa.

[0039] The heating temperature in the second step is set to a higher temperature than that in the first step. The lower limit of the heating temperature in the second step may be, for example, 1850°C or higher, or 1900°C or higher. By setting the lower limit of the heating temperature in the second step within the above range, the purity of hexagonal boron nitride can be further improved, and the growth of primary particles can be promoted, so that the specific surface area of ​​the hexagonal boron nitride powder can be made smaller. The upper limit of the heating temperature in the second step may be, for example, 2050°C or lower, or 2000°C or lower. By setting the upper limit of the heating temperature in the second step within the above range, the yellowing of hexagonal boron nitride can be suppressed. The heating temperature in the second step may be adjusted within the above range, and may be, for example, 1850 to 2050°C, or 1900 to 2025°C.

[0040] The heating time (high-temperature firing time) in the second step may be, for example, 0.5 hours or more, or 1 hour or more. By setting the heating time in the second step within the above range, the purity of hexagonal boron nitride can be further improved and the growth of primary particles can be made more sufficient. The heating time in the second step may also be, for example, 30 hours or less, or 25 hours or less. By setting the heating time in the second step within the above range, hexagonal boron nitride powder can be produced more inexpensively. The heating time in the second step may be adjusted within the above range, and may be, for example, 0.5 to 30 hours, or 0.5 to 25 hours.

[0041] The above-mentioned manufacturing method may have other steps in addition to the first step and the second step. The other steps include, for example, the above-mentioned raw material powder preparation step, the raw material powder dehydration step, and the raw material powder pressure molding step. When the above-mentioned manufacturing method has the raw material powder pressure molding step, the firing can be performed in an environment where the raw material powder is present at a high density, and the yield of boron nitride obtained in the first step can be improved.

[0042] The above-mentioned method for producing hexagonal boron nitride powder can be said to be a method that applies the so-called carbon reduction method. By using the above-mentioned method, it is possible to easily obtain hexagonal boron nitride powder in which the average particle size and specific surface area of ​​the primary particles are adjusted. The primary particles of hexagonal boron nitride obtained tend to be thicker than those obtained by other production methods, and it is presumed that this is the reason why the specific surface area can be easily adjusted.

[0043] Although several embodiments have been described above, the present disclosure is not limited to the above-described embodiments. In addition, the descriptions of the above-described embodiments can be mutually applied. EXAMPLES

[0044] The present disclosure will be described in more detail below using examples and comparative examples. Note that the present disclosure is not limited to the following examples.

[0045] Example 1 [Preparation of hexagonal boron nitride powder] 100 parts by mass of boric acid (manufactured by Kojundo Chemical Laboratory Co., Ltd.) and 25 parts by mass of acetylene black (manufactured by Denka Co., Ltd., grade name: HS100) were mixed using a Henschel mixer to obtain a mixed powder (raw material powder). The obtained mixed powder was placed in a dryer at 250°C and held for 3 hours to dehydrate the boric acid. 200 g of the dehydrated mixed powder was placed in a mold with a diameter of 100Φ in a press molding machine and molded under the conditions of a heating temperature of 200°C and a pressing pressure of 30 MPa. The molded body of the raw material powder thus obtained was used for sintering.

[0046] The molded body was placed in a carbon atmosphere furnace, and the temperature was increased to 1800°C at a rate of 5°C / min in a nitrogen atmosphere pressurized to 0.8 MPa, and the molded body was heat-treated by holding at 1800°C for 3 hours (first step). Thereafter, the temperature in the carbon atmosphere furnace was further increased to 2000°C at a rate of 5°C / min, and the molded body was heat-treated by holding at 2000°C for 7 hours (second step). The loosely aggregated boron nitride after firing was crushed in a Henschel mixer and passed through a sieve with a mesh size of 75 μm to obtain a powder that had passed through the sieve. In this way, a hexagonal boron nitride powder was prepared.

[0047] [Properties of hexagonal boron nitride powder] The hexagonal boron nitride powder obtained as described above was measured for purity, specific surface area, average particle size of primary particles, and total calcium and sodium content in the powder. Specifically, the measurements were performed by the methods described below. The results are shown in Table 1.

[0048] <Purity of hexagonal boron nitride powder> The purity of the hexagonal boron nitride powder was determined by the following method. Specifically, the sample was first decomposed with an alkali using sodium hydroxide, and ammonia was distilled from the decomposition liquid by steam distillation and collected in an aqueous solution of boric acid. The collected liquid was titrated with a normal sulfuric acid solution to determine the content of nitrogen atoms (N) in the sample. The content of hexagonal boron nitride (hBN) in the sample was then determined based on the following formula (1), and the purity of the hexagonal boron nitride powder was calculated.

[0049] Hexagonal boron nitride (hBN) content in sample [mass%] = nitrogen atom (N) content [mass%] × 1.772 (1)

[0050] The formula weight of hexagonal boron nitride was 24.818 g / mol, and the atomic weight of the nitrogen atom was 14.006 g / mol.

[0051] <Specific surface area of ​​hexagonal boron nitride powder> The specific surface area of ​​the hexagonal boron nitride powder containing aggregates of primary particles was measured using a measuring device in accordance with the method described in JIS Z 8803: 2013. The specific surface area was calculated by applying the BET single point method using nitrogen gas.

[0052] <Average particle size of primary particles: Median diameter (d50)> The average particle size of the primary particles in the hexagonal boron nitride powder was measured. The average particle size of the primary particles of hexagonal boron nitride was measured using a particle size distribution analyzer (manufactured by Nikkiso Co., Ltd., product name: MT3300EX) in accordance with the method described in ISO 13320:2009. The average particle size obtained is the average particle size based on volume statistics and is the median value (d50). When measuring the particle size distribution, water was used as the solvent for dispersing the aggregates, and hexametaphosphoric acid was used as the dispersant. In this case, the refractive index of water was 1.33, and the refractive index of the hexagonal boron nitride powder was 1.80.

[0053] <Total content of calcium and sodium in hexagonal boron nitride powder> The calcium and sodium contents in the hexagonal boron nitride powder were measured by the pressure acid decomposition method of ICP emission spectrometry. The total content was the sum of calcium and sodium. In Tables 1 and 2, "ND" indicates that the measured element was below the detection limit.

[0054] [Evaluation of hexagonal boron nitride powder as a release agent] The hexagonal boron nitride powder obtained as described above was evaluated as a release agent (evaluation of release properties). First, a molded body to be coated with the release agent was prepared as follows. The oxygen content was 1.0% and the specific surface area was 10 m. 2 2.5 mol% of yttria was added to silicon nitride powder of 1.0 g / g, and methanol was added and wet mixed in a wet ball mill for 5 hours to obtain a mixture. The mixture obtained was filtered, and the collected matter was dried to obtain a mixed powder. The mixed powder was filled into a mold, molded at a molding pressure of 20 MPa, and then CIP molded at a molding pressure of 200 MPa to prepare a plate-shaped molded body (5 mm x 50 mm x 50 mm).

[0055] Next, the hexagonal boron nitride powder obtained as described above was dispersed in a normal hexane solution to prepare a slurry with a concentration of 1% by mass. The prepared slurry was applied to both sides of the above-mentioned molded body to a thickness of 10 μm, and dried to prepare a substrate provided with a release layer. 30 substrates were prepared in the same manner, and a block was prepared by stacking 30 substrates. The block was placed in an electric furnace having a carbon heater and fired for 6 hours under conditions of 1900° C. and 0.9 MPa. The peeled surfaces of the substrates after firing were visually observed, and the releasability was evaluated according to the following criteria. A means that the releasability is the best.

[0056] A: All of the substrates separated naturally, and no black spots due to impurities were found on the peeled surfaces of the substrates. B: All of the substrates naturally separated from each other, and a few black spots due to impurities were observed on the peeled surfaces of the substrates. C: The substrates were not released from each other, or black spots due to impurities were observed on the peeled surface of the substrate.

[0057] Example 2 In Example 2, hexagonal boron nitride powder was produced in the same manner as in Example 1, except that the heating temperature in the second step was 1900° C. The evaluation results of the hexagonal boron nitride powder of Example 2 are shown in Table 1.

[0058] Example 3 In Example 3, hexagonal boron nitride powder was produced in the same manner as in Example 1, except that the pressure in the first step and the second step was 0.3 MPa. The evaluation results of the hexagonal boron nitride powder of Example 3 are shown in Table 1.

[0059] Example 4 In Example 4, hexagonal boron nitride powder was produced in the same manner as in Example 1, except that 1 part by mass of hexagonal boron nitride (manufactured by Denka Company Ltd., grade name: GP) was further added as a nucleating agent to the raw material powder of Example 1. The evaluation results of the hexagonal boron nitride powder of Example 4 are shown in Table 1.

[0060] Example 5 In Example 5, hexagonal boron nitride powder was produced in the same manner as in Example 1, except that the hexagonal boron nitride powder obtained in Example 1 was further jet milled using a jet mill (manufactured by Daiichi Jitsugyo Co., Ltd., product name: PJM-80) under a milling pressure of 0.2 MPa. The evaluation results of the hexagonal boron nitride powder of Example 5 are shown in Table 1.

[0061] Example 6 In Example 6, hexagonal boron nitride powder was produced in the same manner as in Example 1, except that 10 parts by mass of hexagonal boron nitride (manufactured by Denka Co., Ltd., grade name: SGP) was further blended as a nucleating agent to the raw material powder of Example 1, and the heating time in the second step was 40 hours. The evaluation results of the hexagonal boron nitride powder of Example 6 are shown in Table 1.

[0062] Comparative Example 1 A commercially available hexagonal boron nitride powder was used as Comparative Example 1. The evaluation results of the hexagonal boron nitride powder of Comparative Example 1 are shown in Table 2.

[0063] Comparative Example 2 In Comparative Example 2, hexagonal boron nitride powder was produced in the same manner as in Example 1, except that the heating temperature in the second step was changed from 2000° C. to 1800° C. The evaluation results of the hexagonal boron nitride powder of Comparative Example 2 are shown in Table 2.

[0064] Comparative Example 3 In Comparative Example 3, hexagonal boron nitride powder was produced in the same manner as in Example 1, except that the pressure in the first and second steps was 0.2 MPa. The evaluation results of the hexagonal boron nitride powder of Comparative Example 3 are shown in Table 2. Note that under the production conditions of Comparative Example 3, the degree of contamination inside the furnace was greater than that of Example 1.

[0065] [Table 1]

[0066] [Table 2] [Industrial Applicability]

[0067] According to the present disclosure, it is possible to provide a highly versatile hexagonal boron nitride powder. According to the present disclosure, it is also possible to provide a method for producing the above-mentioned hexagonal boron nitride powder.

Claims

1. The purity is 98% by mass or more, and the specific surface area is 2.0 m 2 / g or less, A hexagonal boron nitride powder having a total sodium and calcium content of less than 50 ppm.

2. 2. The hexagonal boron nitride powder according to claim 1, wherein the total content of sodium and calcium is 30 ppm or less.

3. The hexagonal boron nitride powder according to claim 1 or 2, wherein the average particle size of the primary particles is 2.0 to 35 μm.

4. The hexagonal boron nitride powder according to any one of claims 1 to 3, wherein the average particle size of the primary particles is 9.0 to 30 µm.

Citation Information

Patent Citations

  • Highhtemperature mold releaser composition for diecasting of aluminum and its usage

    JP1980029506A

  • Lubricating mold release agent

    JP1988270798A

  • Hexagonal boron nitride and manufacturing method thereof

    JP2010047450A

  • Boron nitride powder and method for producing the same

    JP2016060661A

  • Hexagonal boron nitride powder

    JP2018043899A