Boron nitride particles and manufacturing method thereof

By introducing gases at specific angles into a reactor to control particle size variation, the method produces boron nitride particles with enhanced thermal conductivity for effective heat dissipation in electronic components.

JP7584439B2Active Publication Date: 2024-11-15DENKA CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021562573
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-06
Filing Date
2020-11-20
Publication Date
2024-11-15
Estimated Expiration
2040-11-20

AI Technical Summary

Technical Problem

Existing boron nitride particles used as fillers in electronic components exhibit significant variations in particle size, which affect their effectiveness in heat dissipation and insulation properties.

Method used

A manufacturing method involving separate introduction of a first gas containing boric acid ester and a second gas containing ammonia into a reactor at specific angles to reduce particle size variation, followed by heating steps to produce boron nitride particles with controlled size and shape.

Benefits of technology

The method achieves boron nitride particles with small variations in particle size and improved thermal conductivity, suitable for heat dissipation applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007584439000002
    Figure 0007584439000002
  • Figure 0007584439000003
    Figure 0007584439000003
  • Figure 0007584439000001
    Figure 0007584439000001
Patent Text Reader

Abstract

An aspect of the present invention is a method for manufacturing boron nitride particles, comprising a reaction step for introducing a first gas including a boric acid ester and a second gas including ammonia each separately into a cylindrical reactor from one end surface of the reactor and reacting the boric acid ester and the ammonia at a temperature of 750°C or higher in the reactor to obtain a boron nitride particle precursor, and a heating step for heating the boron nitride particle precursor to a temperature of 1000°C or higher to obtain boron nitride particles, wherein, in the reaction step, the first gas is introduced into the reactor so that a side surface of the reactor is positioned on an extension line that is in a first direction in which the first gas is introduced into the reactor, and the second gas is introduced into the reactor so that the side surface of the reactor is positioned on an extension line that is in a second direction in which the second gas is introduced into the reactor.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to boron nitride particles and a method for producing the same. [Background technology]

[0002] In electronic components such as transistors, thyristors, and CPUs, efficient dissipation of heat generated during use is an important issue. For this reason, heat dissipation materials with high thermal conductivity are used together with such electronic components. Meanwhile, boron nitride particles have high thermal conductivity and high insulation properties, so they are widely used as a filler in heat dissipation materials.

[0003] For example, when boron nitride particles are used as a filler for primary sealing of electronic components, boron nitride particles having a relatively small particle size are suitable so that the boron nitride particles can enter narrow gaps around the electronic components. For example, Patent Document 1 discloses spherical boron nitride microparticles characterized by an average particle size of 0.01 to 1.0 μm, an orientation index of 1 to 15, a boron nitride purity of 98.0 mass% or more, and an average circularity of 0.80 or more, and a method for producing the same. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2015 / 122379 Summary of the Invention [Problem to be solved by the invention]

[0005] According to the investigations of the present inventors, when boron nitride particles are used as a filler in the primary sealing of electronic components as described above, it is important that the boron nitride particles not only have a small average particle size, but also that the variation in particle size is small.

[0006] Therefore, an object of one aspect of the present invention is to obtain boron nitride particles having small variation in particle size. [Means for solving the problem]

[0007] As a result of investigations conducted by the present inventors, it was found that in a manufacturing method for obtaining boron nitride particles from a boric acid ester and ammonia, the method of introducing a gas containing a boric acid ester and ammonia containing gas into a reactor is important in order to reduce variation in particle size of the obtained boron nitride particles.

[0008] One aspect of the present invention is a method for producing boron nitride particles, comprising: a reaction step in which a first gas containing a borate ester and a second gas containing ammonia are separately introduced into a cylindrical reactor from one end face of the reactor, and the borate ester and ammonia are reacted in the reactor at 750°C or higher to obtain a precursor of boron nitride particles; and a heating step in which the precursor of the boron nitride particles is heated at 1000°C or higher to obtain boron nitride particles, wherein in the reaction step, the first gas is introduced into the reactor so that the side of the reactor is located on an extension of a first direction in which the first gas is introduced into the reactor, and the second gas is introduced into the reactor so that the side of the reactor is located on an extension of a second direction in which the second gas is introduced into the reactor.

[0009] The angle between the extension direction extending from one end face to the other end face of the reactor and the first direction is defined as θ 1 When this is done, tanθ 1 The angle between the extension direction extending from one end face to the other end face of the reactor and the second direction is defined as θ 2 When this is done, tanθ 2 may be 1.2 or greater.

[0010] Another aspect of the present invention is boron nitride particles having an average particle size of 1 μm or less and a difference between the 10% cumulative particle size and the 100% cumulative particle size of 5 μm or less in a volume-based particle size distribution.

[0011] The average circularity of the boron nitride particles may be greater than or equal to 0.8.

[0012] Another aspect of the present invention is a resin composition containing a resin and the above-mentioned boron nitride particles. Effect of the Invention

[0013] According to one aspect of the present invention, boron nitride particles having small variation in particle size can be obtained. [Brief description of the drawings]

[0014] [Figure 1] FIG. 2 is a perspective view showing an example of a reactor used in the method for producing boron nitride particles according to an embodiment. [Diagram 2] 1(a) is a side view of the reactor as viewed from the first inlet pipe side, and FIG. 1(b) is a side view of the reactor as viewed from the second inlet pipe side. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] One embodiment of the present invention is a method for producing boron nitride particles, comprising a reaction step of reacting a boric acid ester with ammonia at 750°C or higher to obtain a precursor of boron nitride particles, and a heating step of heating the precursor of the boron nitride particles at 1000°C or higher to obtain boron nitride particles.

[0016] In the reaction step, a first gas containing a borate ester and a second gas containing ammonia are separately introduced into a reactor.

[0017] Fig. 1 is a perspective view showing an example of a reactor. As shown in Fig. 1, the reactor 1 is, for example, cylindrical with both ends open (both end faces are opening faces), and has an internal space S located between one end face 1a and the other end face 1b. The length of the reactor 1 may be, for example, 1000 mm or more and 1600 mm or less. The inner diameter of the reactor 1 may be, for example, 30 mm or more and 100 mm or less.

[0018] Both ends of the reactor 1 are held by the holding member 2 so that the outside of the reactor 1 and the internal space S can be isolated (so that the internal space S can be a closed system as necessary). The reactor 1 is installed so that the heating part H is located in a resistance heating furnace (not shown) in order to heat only a part (hereinafter referred to as the "heating part") H between both end faces 1a and 1b. The length of the heating part H (the length in the longitudinal direction of the reactor 1) may be, for example, 500 mm or more and 900 mm or less. By heating the heating part H of the reactor 1, the boric acid ester and ammonia react in the heating part H. The temperature of the heating part H may be, for example, 750°C or more and 1500°C or less.

[0019] A first inlet pipe 3 and a second inlet pipe 4 are separately attached to one end surface 1a of the reactor 1 so that gas can be introduced from the outside of the reactor 1 into the internal space S. Fig. 2(a) is a side view of the reactor 1 seen from the first inlet pipe 3 side. Fig. 2(b) is a side view of the reactor 1 seen from the second inlet pipe 4 side.

[0020] 1 and 2(a), the first introduction pipe 3 has, for example, a cylindrical shape with a tip bent in a predetermined direction. The first introduction pipe 3 is introduced from the outside of the reactor 1 into the internal space S so as to extend approximately parallel to the extension direction D extending from one end face 1a to the other end face 1b of the reactor 1 (extension direction extending from the one end face 1a toward the other end face 1b), and the angle between the extension direction D of the reactor 1 and the position in the internal space S at a distance of, for example, 10 to 40 mm from the one end face 1a is θ 1 The bending direction d1 of the first introduction tube 3 is defined as a direction perpendicular to the tip surface 3a of the first introduction tube 3.

[0021] 1 and 2(b), the second introduction pipe 4 has, for example, a cylindrical shape with a tip bent in a predetermined direction. The second introduction pipe 4 is introduced from the outside of the reactor 1 into the internal space S so as to extend approximately parallel to the extension direction D of the reactor 1, and in the internal space S, at a position, for example, 10 to 40 mm away from one end face 1a, the angle formed with the extension direction D of the reactor 1 is θ 2 The bending direction d1 of the second introduction tube 4 is defined as a direction perpendicular to the tip surface 4a of the second introduction tube 4.

[0022] The above angle θ 1 is an angle at which the side surface (side surface along the extending direction D; the same applies below) 1c of the reactor 1 is located on the extension line of the bending direction d1 of the first inlet pipe 3 (the extension line of the bending direction d1 of the first inlet pipe 3 intersects with the side surface 1c of the reactor 1). Similarly, the above angle θ 2 is an angle such that the side surface (side surface along the extending direction D) 1c of the reactor 1 is located on an extension line of the bending direction d2 of the second inlet pipe 4 (the extension line of the bending direction d2 of the second inlet pipe 4 intersects with the side surface 1c of the reactor 1).

[0023] In the reaction step, a first gas containing a borate ester is introduced from the outside of the reactor 1 into the internal space S through a first introduction pipe 3, and a second gas containing ammonia is introduced from the outside of the reactor 1 into the internal space S through a second introduction pipe 4 separately from the first gas.

[0024] The first gas is obtained, for example, by passing an inert gas through a liquid borate ester. In this case, the first gas is a gas consisting of a borate ester and an inert gas. The borate ester may be, for example, an alkyl borate ester, preferably trimethyl borate. Examples of the inert gas include rare gases such as helium, neon, and argon, and nitrogen gas. The second gas is, for example, a gas consisting of ammonia.

[0025] The molar ratio of the amount of ammonia introduced to the amount of borate ester introduced (ammonia / borate ester) may be, for example, 1 or more and 10 or less.

[0026] The boric acid ester and ammonia introduced into the reactor 1 react in the heated reactor 1 to generate a precursor (white powder) of boron nitride particles. Some of the generated precursor of boron nitride particles adheres to the inside of the reactor 1, but most of the precursor of boron nitride particles is sent to a recovery container (not shown) attached to the other end surface 1b side of the reactor 1 by an inert gas or unreacted ammonia gas and collected. The reaction time for reacting the boric acid ester and ammonia is preferably within 30 seconds from the viewpoint of easily reducing the particle size of the obtained boron nitride particles. The reaction time is the time that the boric acid ester and ammonia remain in the heating section H of the reactor 1, and can be adjusted by the gas flow rate when the first gas and the second gas are introduced and the length of the heating section H.

[0027] In the reaction process described above, the first inlet pipe 3 is arranged at the angle θ 1 Since the first gas is bent in the bending direction d1, the angle between the first gas and the extension direction D of the reactor 1 is θ 1 Similarly, the second introduction pipe 4 is introduced in the first introduction direction (first direction) d1 at an angle θ 2 Since the second gas is bent in the bending direction d2, the angle between the extension direction D of the reactor 1 and the second gas is also θ 2 The gas is introduced in a second introduction direction (second direction) d2 such that the gas is introduced in a direction perpendicular to the first introduction pipe 3. That is, the side surface 1c of the reactor 1 is located on an extension line of the introduction direction d1 of the first gas and on an extension line of the introduction direction d2 of the second gas. The first introduction direction d1 is defined as a direction perpendicular to the tip surface 3a of the first introduction pipe 3, similar to the bending direction d1 of the first introduction pipe 3. The second introduction direction d2 is defined as a direction perpendicular to the tip surface 4a of the second introduction pipe 4, similar to the bending direction d2 of the second introduction pipe 4.

[0028] In this way, by introducing the first gas in the first introduction direction d1 and the second gas in the second introduction direction d2, the variation in particle size of the obtained boron nitride particles can be reduced. Although the reason is not clear, it is presumed that the reason is that by introducing the first gas and the second gas in the first introduction direction d1 and the second introduction direction d2, respectively, the first gas and the second gas advance inside the reactor 1 at an angle to the extension direction D of the reactor 1 while colliding with the side surface 1c of the reactor 1, and therefore the first gas and the second gas are more likely to be mixed uniformly with each other than, for example, when the first gas and the second gas are introduced parallel to the extension direction D of the reactor 1.

[0029] Angle θ 1 and θ 2 From the viewpoint of further reducing the variation in particle size of the obtained boron nitride particles, the angle θ is preferably 50° or more, more preferably 60° or more, further preferably 65° or more, and particularly preferably 70° or more. 1 and θ 2 Each of the angles θ is less than 90°, and may be, for example, less than or equal to 80°. 1 and θ 2 About tanθ 1 and tan θ 2 From the viewpoint of further reducing the variation in particle size of the obtained boron nitride particles, tan θ is preferably 1.2 or more, more preferably 1.7 or more, even more preferably 2.1 or more, and particularly preferably 2.7 or more. 1 and tan θ 2 may each be, for example, 11.4 or less.

[0030] In the heating step, the precursor of the boron nitride particles obtained in the reaction step is heated at 1000°C or higher to obtain boron nitride particles. The heating step may include, for example, a first heating step in which the precursor of the boron nitride particles is heated at 1000 to 1600°C to obtain a first precursor, a second heating step in which the first precursor is heated at 1000 to 1600°C to obtain a second precursor, and a third heating step in which the second precursor is heated at 1800 to 2200°C to obtain boron nitride particles. In this case, after the end of the first heating step, the environmental temperature in which the first precursor is placed is temporarily lowered to room temperature (10 to 30°C) before the start of the second heating step. In another embodiment, in the heating step, the first heating step may be omitted, and the second heating step and the third heating step may be performed.

[0031] In the first heating step, the precursor of boron nitride particles obtained in the reaction step is placed in another reaction tube (e.g., an alumina tube) installed in a resistance heating furnace, and nitrogen gas and ammonia gas are introduced separately into the reaction tube. The gas introduced at this time may be only ammonia gas. The flow rates of nitrogen gas and ammonia gas may be appropriately adjusted so that the reaction time is a desired value. For example, the higher the flow rates of nitrogen gas and ammonia gas, the shorter the reaction time.

[0032] Next, the reaction tube is heated to 1000 to 1600° C. The heating time may be, for example, 1 hour or more and 10 hours or less, thereby obtaining the first precursor.

[0033] After the first heating step is completed, the power supply to the resistance heating furnace is turned off, the introduction of nitrogen gas and ammonia gas is stopped, and the temperature inside the reaction tube is lowered to room temperature (10 to 30° C.), and the first precursor is allowed to stand still. The time for standing still may be, for example, 0.5 hours or more and may be 96 hours or less.

[0034] In the second heating step, nitrogen gas and ammonia gas are introduced into the reaction tube again, and the reaction tube is heated again to 1000 to 1600°C. Examples of the flow rates of nitrogen gas and ammonia gas and the heating time may be the same as those described in the first heating step. The conditions of the first heating step and the second heating step may be the same or different from each other. This results in the second precursor.

[0035] In the third heating step, the second precursor obtained in the second heating step is placed in a boron nitride crucible and heated to 1800 to 2200°C in a nitrogen atmosphere in an induction heating furnace. The heating time may be, for example, 0.5 hours or more and 10 hours or less. This produces boron nitride particles.

[0036] The above-described manufacturing method can provide boron nitride particles having, for example, a mean particle size of 1 μm or less and a difference between the 10% cumulative particle size and the 100% cumulative particle size of 10 μm or less in a volumetric particle size distribution. That is, another embodiment of the present invention provides boron nitride particles having a mean particle size of 1 μm or less and a difference (D100-D10) between the 10% cumulative particle size (D10) and the 100% cumulative particle size (D100) of 10 μm or less in a volumetric particle size distribution.

[0037] The average particle size of the boron nitride particles may be preferably 0.9 μm or less, 0.8 μm or less, or 0.7 μm or less from the viewpoint of reducing the dielectric constant of a heat dissipation member containing the boron nitride particles (hereinafter also simply referred to as "heat dissipation member"). The average particle size of the boron nitride particles may be preferably 0.01 μm or more, 0.05 μm or more, 0.1 μm or more, 0.2 μm or more, 0.3 μm or more, or 0.4 μm or more from the viewpoint of suppressing an increase in viscosity when the boron nitride particles are mixed with a resin.

[0038] From the viewpoint of reducing the dielectric constant of the heat dissipation member and suppressing the variation in particle size, which is more suitable for primary sealing of electronic components, the D100-D10 of the boron nitride particles may be preferably 5 μm or less, 4 μm or less, or 3 μm or less. The D100-D10 of the boron nitride particles may be, for example, 0.5 μm or more, 0.8 μm or more, or 1 μm or more.

[0039] The average particle size and D100-D10 of the boron nitride particles are measured by the following procedure. Using distilled water as a dispersion medium for dispersing boron nitride particles and sodium hexametaphosphate as a dispersant, a 0.125% by mass aqueous solution of sodium hexametaphosphate is prepared. Boron nitride particles are added to this aqueous solution at a ratio of 0.1 g / 80 mL, and ultrasonic dispersion is performed once for 1 minute and 30 seconds at AMPLITUDE (amplitude) 80% using an ultrasonic homogenizer (e.g., manufactured by Nippon Seiki Seisakusho, product name: US-300E) to prepare a dispersion of boron nitride particles. The dispersion is taken while stirring at 60 rpm, and the volume-based particle size distribution is measured using a laser diffraction scattering particle size distribution measuring device (e.g., manufactured by Beckman Coulter, product name: LS-13 320). At this time, the refractive index of water is 1.33, and the refractive index of boron nitride particles is 1.7. From the measurement results, the average particle size is calculated as the particle size (median size, d50) at 50% of the cumulative value of the cumulative particle size distribution, and D100-D10 is calculated as the particle size D10 at 10% of the cumulative value of the cumulative particle size distribution minus the particle size D10 at 10% of the cumulative value.

[0040] The boron nitride particles preferably have a spherical or nearly spherical shape in order to improve the filling property when producing a heat dissipation member and to make the properties of the heat dissipation member isotropic (thermal conductivity, dielectric constant, etc.) From the same viewpoint, the average circularity of the boron nitride particles may preferably be 0.8 or more, 0.82 or more, 0.84 or more, 0.86 or more, or 0.88 or more.

[0041] The average circularity of the boron nitride particles is measured by the following procedure. The image of the boron nitride particle taken with a scanning electron microscope (SEM) (magnification: 10,000 times, image resolution: 1280 x 1024 pixels) is analyzed using image analysis software (e.g., MacView, manufactured by Mountec Co., Ltd.) to calculate the projected area (S) and perimeter (L) of the boron nitride particle. The projected area (S) and perimeter (L) are used to calculate the following formula: Circularity = 4πS / L 2 The circularity is calculated according to the following formula: The average circularity is defined as the average circularity obtained for 100 randomly selected boron nitride particles.

[0042] The boron nitride particles described above are suitable for use in, for example, heat dissipation members. By using the above-mentioned boron nitride particles, a heat dissipation member with a low dielectric constant can be obtained. When the boron nitride particles are used in a heat dissipation member, they are used as a resin composition mixed with, for example, a resin. That is, another embodiment of the present invention is a resin composition containing a resin and the above-mentioned boron nitride particles.

[0043] The content of the above-mentioned boron nitride particles, based on the total volume of the resin composition, is preferably 30 vol. % or more, more preferably 40 vol. % or more, and even more preferably 50 vol. % or more, from the viewpoint of improving the thermal conductivity of the resin composition and making it easier to obtain excellent heat dissipation performance, and is preferably 85 vol. % or less, more preferably 80 vol. % or less, and even more preferably 70 vol. % or less, from the viewpoint of suppressing the generation of voids during molding and the deterioration of insulation and mechanical strength.

[0044] Examples of resins include epoxy resins, silicone resins, silicone rubber, acrylic resins, phenolic resins, melamine resins, urea resins, unsaturated polyesters, fluororesins, polyolefins (polyethylene, etc.), polyimides, polyamideimides, polyetherimides, polybutylene terephthalate, polyethylene terephthalate, polyphenylene ether, polyphenylene sulfide, wholly aromatic polyesters, polysulfones, liquid crystal polymers, polyethersulfones, polycarbonates, maleimide-modified resins, ABS (acrylonitrile-butadiene-styrene) resins, AAS (acrylonitrile-acrylic rubber-styrene) resins, and AES (acrylonitrile-ethylene-propylene-diene rubber-styrene) resins.

[0045] The resin content may be 15 vol.% or more, 20 vol.% or more, or 30 vol.% or more, and may be 70 vol.% or less, 60 vol.% or less, or 50 vol.% or less, based on the total volume of the resin composition.

[0046] The resin composition may further contain a curing agent that cures the resin. The curing agent is appropriately selected depending on the type of resin. For example, when the resin is an epoxy resin, the curing agent may be a phenol novolac compound, an acid anhydride, an amino compound, or an imidazole compound. The content of the curing agent may be, for example, 0.5 parts by mass or more or 1.0 parts by mass or more, and 15 parts by mass or less or 10 parts by mass or less, relative to 100 parts by mass of the resin.

[0047] The resin composition may further contain boron nitride particles other than the above-mentioned boron nitride particles (for example, known boron nitride particles such as chunky boron nitride particles formed by agglomeration of scaly primary particles). EXAMPLES

[0048] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to the following examples.

[0049] [Production Example 1] Boron nitride particles were prepared by the following procedure. First, in the reaction step, a cylindrical reactor (quartz tube, reactor length: 1300 mm, inner diameter of reactor: 75 mm, length of part located in resistance heating furnace: 800 mm) as shown in FIG. 1 was installed in a resistance heating furnace and heated to 1150°C. Meanwhile, a first gas obtained by passing nitrogen gas through trimethyl borate was introduced into the reactor from the first introduction tube. Meanwhile, ammonia gas was directly introduced into the reactor. The first introduction tube and the second introduction tube were arranged in the inner space of the reactor at a position 25 mm away from one end face of the reactor, with an angle of θ 1 and θ 2 In other words, the angles between the first gas introduction direction and the extension direction of the reactor and the second gas introduction direction are θ 1 and θ 2 The first gas and the second gas were introduced so that θ 1 and θ 2 are tanθ 1 and tan θ 2 The angle was set so that the value shown in Table 1 was obtained.

[0050] The molar ratio of the amount of ammonia introduced to the amount of trimethyl borate introduced (ammonia / trimethyl borate) was set to 4.5. This caused trimethyl borate and ammonia to react with each other to obtain a precursor of boron nitride particles (white powder). The reaction time was set to 10 seconds.

[0051] In the heating step, the precursor of boron nitride particles obtained in the reaction step was placed in another reaction tube (alumina tube) installed in a resistance heating furnace, and nitrogen gas and ammonia gas were introduced into the reaction tube at flow rates of 10 L / min and 15 L / min, respectively. The reaction tube was then heated at 1500°C for 2.5 hours. This resulted in the production of a first precursor (first heating step).

[0052] Next, the power to the resistance heating furnace was turned off, the introduction of the nitrogen gas and the ammonia gas was stopped, and the temperature inside the reaction tube was lowered to 25° C., and the first precursor was left to stand for 2 hours.

[0053] Next, nitrogen gas and ammonia gas were introduced and the inside of the reaction tube was heated under the same conditions as in the first heating step, thereby obtaining a second precursor (second heating step).

[0054] Subsequently, the second precursor obtained in the second heating step was placed in a boron nitride crucible and heated in an induction heating furnace in a nitrogen atmosphere at 2000° C. for 5 hours, thereby obtaining boron nitride particles.

[0055] [Manufacturing Examples 2 and 3] The introduction direction of the first gas and the introduction direction of the second gas are defined as tanθ 1 and tan θ 2 The angle θ such that the value shown in Table 1 is obtained. 1 and θ 2 Boron nitride particles were produced in the same manner as in Production Example 1, except that the above-mentioned conditions were changed to the above.

[0056] For each of the obtained boron nitride particles, the average particle size, the difference between the 10% cumulative particle size and the 100% cumulative particle size (D100-D10), and the average circularity were measured by the following methods. The results are shown in Table 1.

[0057] (Average particle size and D100-D10) Distilled water was used as a dispersion medium for dispersing boron nitride particles, and sodium hexametaphosphate was used as a dispersant to prepare a 0.125% by mass aqueous solution of sodium hexametaphosphate. Boron nitride particles were added to this aqueous solution at a ratio of 0.1 g / 80 mL, and ultrasonic dispersion was performed once for 1 minute and 30 seconds at AMPLITUDE (amplitude) 80% using an ultrasonic homogenizer (manufactured by Nippon Seiki Seisakusho, product name: US-300E) to prepare a dispersion of boron nitride particles. The dispersion was taken while stirring at 60 rpm, and the volume-based particle size distribution was measured using a laser diffraction scattering particle size distribution measuring device (manufactured by Beckman Coulter, product name: LS-13 320). At this time, 1.33 was used as the refractive index of water, and 1.7 was used as the refractive index of boron nitride particles. From the measurement results, the average particle size was calculated as the particle size (median size, d50) at 50% of the cumulative value of the cumulative particle size distribution, and D100-D10 was calculated as the particle size D10 at 10% of the cumulative value of the cumulative particle size distribution minus the particle size D10 at 10% of the cumulative value.

[0058] (Average circularity) First, the projected area (S) and perimeter (L) of the boron nitride particle were calculated by image analysis using image analysis software (e.g., MacView, manufactured by Mountec Co., Ltd.) for an image of the boron nitride particle (magnification: 10,000 times, image resolution: 1280 x 1024 pixels) taken using a scanning electron microscope (SEM). Next, the projected area (S) and perimeter (L) were calculated using the following formula: Circularity = 4πS / L 2 The circularity was determined according to the following formula: The average value of the circularities determined for 100 randomly selected boron nitride particles was calculated as the average circularity.

[0059] The dielectric constant of each of the obtained boron nitride particles was measured by the following method. The results are shown in Table 1. The boron nitride particles were mixed with polyethylene (product name "Novatec HY540" manufactured by Japan Polyethylene Co., Ltd.) in an amount such that the boron nitride particles constituted 20 volume % and then formed into a sheet having a thickness of 0.2 mm. The mixing and sheet forming were carried out using a twin-screw extruder at a temperature of 180°C. The obtained sheet was measured using a cavity resonator method measuring device at a frequency of 36 GHz and a temperature of 25°C to determine the dielectric constant of the sheet.

[0060] [Table 1] [Explanation of symbols]

[0061] 1...reactor, 1a...one end face of reactor, 1b...other end face of reactor, 1c...side face of reactor, 2...holding member, 3...first inlet tube, 3a...tip face of first inlet tube, 4...second inlet tube, 4a...tip face of second inlet tube, D...extension direction of reactor, S...internal space of reactor, d1...inlet direction of first gas, d2...inlet direction of second gas.

Claims

1. a reaction step of separately introducing a first gas containing a borate ester and a second gas containing ammonia into a cylindrical reactor from one end surface of the reactor, and reacting the borate ester and the ammonia at 750° C. or higher in the reactor to obtain a precursor of boron nitride particles; a heating step of heating the precursor of the boron nitride particles at 1000° C. or higher to obtain boron nitride particles; A method for producing boron nitride particles comprising: in the reaction step, the first gas is introduced into the reactor such that a side surface of the reactor is located on an extension line of a first direction in which the first gas is introduced into the reactor, and the second gas is introduced into the reactor such that a side surface of the reactor is located on an extension line of a second direction in which the second gas is introduced into the reactor.

2. The angle between the extension direction extending from the one end surface to the other end surface of the reactor and the first direction is defined as θ 1 When this is done, tan θ 1 The method according to claim 1 , wherein the β-

3. The angle between the extension direction extending from the one end surface to the other end surface of the reactor and the second direction is defined as θ 2 When this is done, tan θ 2 The method according to claim 1 or 2, wherein the ratio is 1.2 or more.

4. Boron nitride particles having an average particle diameter of 0.4 μm or more and 0.7 μm or less, and a difference between a 10% cumulative particle diameter and a 100% cumulative particle diameter of 1 μm or more and 3 μm or less, in a volume-based particle size distribution.

5. 5. The boron nitride particles according to claim 4, having an average circularity of 0.8 or more.

6. A resin composition comprising a resin and the boron nitride particles according to claim 4 or 5.

7. A resin composition containing a resin and the boron nitride particles described in claim 4 or 5 (excluding a resin composition containing scaly boron nitride particles having an average particle size of 3 μm or more and 40 μm or less, and spherical boron nitride particles having an average particle size of 0.05 μm or more and 1 μm or less, wherein the orientation index calculated from X-ray diffraction of the scaly boron nitride particles is 15 to 70, the content of the scaly boron nitride particles in the entire resin composition is 3 vol% to 75 vol%, the content of the spherical boron nitride particles in the entire resin composition is 0.3 vol% to 30 vol%, and the proportion of spherical boron nitride particles having a particle size of 2 μm or more in the entire spherical boron nitride particles is 1% or less).

Citation Information

Patent Citations

  • Method and an apparatus for high pressure gas phase preparation of boron nitride spherical powder

    CN107161960A

  • Boron nitride powder of turbostratic structure and its production

    JP1998203807A

  • NANO spherical particle having composite structure, powder and method for producing the same

    JP2008038163A

  • Boron nitride spherical nanoparticle and method of producing the same

    JP2010180066A

  • Electrically insulating composite material, method of making this material and method of using said material as an electrical insulator

    JP2016531972A