Resin composition

The resin composition with an active ester curing agent and balanced epoxy resin and inorganic filler addresses unevenness in insulating layers, enhancing dielectric properties and formability in printed wiring boards.

JP7585603B2Active Publication Date: 2024-11-19AJINOMOTO CO INC
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2019130695
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-07-12
Publication Date
2024-11-19
Estimated Expiration
2039-07-12

AI Technical Summary

Technical Problem

The demand for improved dielectric properties in insulating layers of printed wiring boards has led to increased inorganic filler content, which results in unevenness and non-uniformity of the insulating layer due to substrate unevenness, affecting wiring formability.

Method used

A resin composition incorporating a predetermined active ester curing agent with specific structural units and a balanced ratio of epoxy resin and inorganic filler, suppressing unevenness and enhancing dielectric properties.

Benefits of technology

The resin composition achieves a cured product with excellent dielectric properties and improved flatness, ensuring uniformity and better wiring formability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007585603000033
    Figure 0007585603000033
  • Figure 0007585603000001
    Figure 0007585603000001
  • Figure 0007585603000002
    Figure 0007585603000002
Patent Text Reader

Abstract

To provide a resin composition that can suppress the unevenness occurring in a curing substrate and gives a cured product with excellent dielectric properties.SOLUTION: A resin composition contains (A) an epoxy resin, (B) an active ester curing agent having a specific constitutional unit, and (C) an inorganic filler. The (B) component content is 30 mass% or less when a nonvolatile content in the resin composition is 100 mass%. The (C) component content is 60 mass% or less when the nonvolatile content in the resin composition is 100 mass%.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition. The present invention further relates to a resin sheet, a printed wiring board, and a semiconductor device obtained by using the resin composition. [Background technology]

[0002] 2. Description of the Related Art A known manufacturing technique for printed wiring boards is a build-up method in which insulating layers and conductor layers are alternately stacked.

[0003] As an insulating material for a printed wiring board used in such an insulating layer, for example, Patent Document 1 discloses a resin composition. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2019-6869 A DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]

[0005] In recent years, there has been a demand for further improvement in dielectric properties such as the dielectric constant and dielectric loss tangent of insulating layers, and one possible solution for this purpose is to increase the content of inorganic filler.

[0006] However, as a result of intensive research by the present inventors, it was found that when an insulating layer is formed on a substrate having irregularities using a resin composition having a high content of inorganic filler, the surface of the insulating layer opposite the substrate follows the irregularities of the substrate, reducing the flatness of the insulating layer, and unevenness (unevenness on the insulating layer surface) is likely to occur on the cured substrate. If the cured substrate has irregularities, the composition of the insulating layer becomes non-uniform, which may result in poor wiring formability.

[0007] An object of the present invention is to provide a resin composition that can suppress unevenness occurring on a cured substrate and give a cured product having excellent dielectric properties; a resin sheet containing the resin composition; and a printed wiring board and a semiconductor device that have an insulating layer formed using the resin composition. [Means for solving the problem]

[0008] As a result of extensive investigations into the above problems, the present inventors have found that the above problems can be solved by incorporating a specific active ester curing agent, and have thus completed the present invention.

[0009] That is, the present invention includes the following. [1] (A) epoxy resin, (B) an active ester-based curing agent having a structural unit represented by the following general formula (1) and a structural unit represented by the following general formula (2), (C) a resin composition containing an inorganic filler, The content of the (B) component is 30% by mass or less, based on 100% by mass of the nonvolatile components in the resin composition; A resin composition, wherein the content of the component (C) is 60 mass% or more, based on 100 mass% of the non-volatile components in the resin composition. [ka] (In general formula (1), R 11 each independently represents an optionally substituted aliphatic hydrocarbon group, an optionally substituted aryl group, or an optionally substituted aralkyl group, Z represents an optionally substituted isophthaloyl group, or an optionally substituted naphthalenedicarbonyl group, and n1 represents 0 or an integer of 1 to 3. In general formula (2), R 12 each independently represents an aliphatic hydrocarbon group which may have a substituent, an aryl group which may have a substituent, or an aralkyl group which may have a substituent. n2 represents 0 or an integer of 1 to 3. [2] R in general formula (1) 11 and R in general formula (2)12 each independently represents an aliphatic hydrocarbon group which may have a substituent. [3] The resin composition according to [1] or [2], wherein the aliphatic hydrocarbon group represents an alkyl group having a branched structure. [4] The resin composition according to any one of [1] to [3], wherein the content of the (B) component when the nonvolatile components in the resin composition are taken as 100% by mass is b, and the content of the (C) component when the nonvolatile components in the resin composition are taken as 100% by mass is c, in which b / c is 0.01 or more and 3 or less. [5] The resin composition according to any one of [1] to [4], further comprising (F) a curing agent. [6] The resin composition according to any one of [1] to [5], which is for forming an insulating layer. [7] The resin composition according to any one of [1] to [6], which is for forming an insulating layer for forming a conductor layer. [8] A resin sheet comprising a support and a resin composition layer provided on the support, the resin composition layer comprising the resin composition according to any one of [1] to [7]. [9] A printed wiring board comprising an insulating layer formed from a cured product of the resin composition according to any one of [1] to [7].

[10] A semiconductor device comprising the printed wiring board described in [9]. Effect of the Invention

[0010] According to the present invention, it is possible to provide a resin composition that can suppress unevenness occurring on a cured substrate and give a cured product with excellent dielectric properties; a resin sheet containing the resin composition; a printed wiring board having an insulating layer formed using the resin composition, and a semiconductor device. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a schematic side view showing an example of two test tubes used to determine whether a thermosetting resin is in a liquid state, a semi-solid state, or a solid state. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention will be described in detail below with reference to preferred embodiments. However, the present invention is not limited to the following embodiments and examples, and can be modified and implemented as desired without departing from the scope of the claims of the present invention and their equivalents.

[0013] [Resin composition] The resin composition of the present invention is a resin composition containing (A) an epoxy resin, (B) an active ester-based curing agent having a structural unit represented by the following general formula (1) and a structural unit represented by the following general formula (2), and (C) an inorganic filler, in which the content of the (B) component is 30% by mass or less, when the non-volatile components in the resin composition are taken as 100% by mass, and the content of the (C) component is 60% by mass or more, when the non-volatile components in the resin composition are taken as 100% by mass. In the present invention, by containing a predetermined amount of the (B) component and a predetermined amount of the (C) component, unevenness occurring on the cured substrate can be suppressed, and a cured product with excellent dielectric properties can be obtained. In addition, in the present invention, a cured product with excellent peel strength can usually be obtained. [ka] (In general formula (1), R 11 each independently represents an optionally substituted aliphatic hydrocarbon group, an optionally substituted aryl group, or an optionally substituted aralkyl group, Z represents an optionally substituted isophthaloyl group, or an optionally substituted naphthalenedicarbonyl group, and n1 represents 0 or an integer of 1 to 3. In general formula (2), R 12 each independently represents an aliphatic hydrocarbon group which may have a substituent, an aryl group which may have a substituent, or an aralkyl group which may have a substituent. n2 represents 0 or an integer of 1 to 3.

[0014] The resin composition may further contain optional components in combination with the components (A) to (C). Examples of the optional components include a curing accelerator (D), a thermoplastic resin (E), a curing agent (F), and other additives (G). Each component contained in the resin composition will be described in detail below.

[0015] <(A) Epoxy resin> The resin composition contains an epoxy resin (A) as component (A). Examples of component (A) include bixylenol type epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, bisphenol AF type epoxy resin, dicyclopentadiene type epoxy resin, trisphenol type epoxy resin, naphthol novolac type epoxy resin, phenol novolac type epoxy resin, tert-butyl-catechol type epoxy resin, naphthalene type epoxy resin, naphthol type epoxy resin, anthracene type epoxy resin, glycidylamine type epoxy resin, glycidyl ester type epoxy resin, cresol novolac type epoxy resin, biphenyl type epoxy resin, linear aliphatic epoxy resin, epoxy resin having a butadiene structure, alicyclic epoxy resin, heterocyclic epoxy resin, spiro ring-containing epoxy resin, cyclohexane type epoxy resin, cyclohexane dimethanol type epoxy resin, naphthylene ether type epoxy resin, trimethylol type epoxy resin, tetraphenylethane type epoxy resin, etc. The epoxy resin may be used alone or in combination of two or more kinds.

[0016] The resin composition preferably contains, as component (A), an epoxy resin having two or more epoxy groups in one molecule. From the viewpoint of significantly obtaining the desired effects of the present invention, the ratio of the epoxy resin having two or more epoxy groups in one molecule to 100% by mass of the non-volatile components of component (A) is preferably 50% by mass or more, more preferably 60% by mass or more, and particularly preferably 70% by mass or more.

[0017] Epoxy resins include epoxy resins that are liquid at a temperature of 20° C. (hereinafter sometimes referred to as "liquid epoxy resins") and epoxy resins that are solid at a temperature of 20° C. (hereinafter sometimes referred to as "solid epoxy resins"). The resin composition may contain only a liquid epoxy resin, only a solid epoxy resin, or a combination of a liquid epoxy resin and a solid epoxy resin as component (A), but from the viewpoint of significantly obtaining the desired effects of the present invention, it is preferable to contain only a solid epoxy resin.

[0018] As the solid epoxy resin, a solid epoxy resin having three or more epoxy groups in one molecule is preferable, and an aromatic solid epoxy resin having three or more epoxy groups in one molecule is more preferable.

[0019] As the solid epoxy resin, bixylenol type epoxy resin, naphthalene type epoxy resin, naphthalene type tetrafunctional epoxy resin, cresol novolac type epoxy resin, dicyclopentadiene type epoxy resin, trisphenol type epoxy resin, naphthol type epoxy resin, biphenyl type epoxy resin, naphthylene ether type epoxy resin, anthracene type epoxy resin, bisphenol A type epoxy resin, bisphenol AF type epoxy resin, and tetraphenylethane type epoxy resin are preferred, and naphthalene type epoxy resin is more preferred.

[0020] Specific examples of solid epoxy resins include "HP4032H" (naphthalene type epoxy resin) manufactured by DIC Corporation; "HP-4700" and "HP-4710" (naphthalene type tetrafunctional epoxy resins) manufactured by DIC Corporation; "N-690" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "N-695" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "HP-7200", "HP-7200HH", and "HP-7200H" (dicyclopentadiene type epoxy resin) manufactured by DIC Corporation. anthradiene type epoxy resins); "EXA-7311", "EXA-7311-G3", "EXA-7311-G4", "EXA-7311-G4S", and "HP6000" (naphthylene ether type epoxy resins) manufactured by DIC; "EPPN-502H" (trisphenol type epoxy resins) manufactured by Nippon Kayaku; "NC7000L" (naphthol novolac type epoxy resins) manufactured by Nippon Kayaku; "NC3000H", "NC3000", and "NC 3000L, "NC3100" (biphenyl type epoxy resin); "ESN475V" (naphthol type epoxy resin) manufactured by Nippon Steel & Sumitomo Metal Chemical Co., Ltd.; "ESN485" (naphthol novolac type epoxy resin) manufactured by Nippon Steel & Sumitomo Metal Chemical Co., Ltd.; "YX4000H", "YX4000", "YL6121" (biphenyl type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "YX4000HK" (bixylenol type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "YX8" manufactured by Mitsubishi Chemical Co., Ltd. Examples of epoxy resins include "800" (anthracene type epoxy resin), "PG-100" and "CG-500" manufactured by Osaka Gas Chemicals, "YL7760" (bisphenol AF type epoxy resin) manufactured by Mitsubishi Chemical, "YL7800" (fluorene type epoxy resin) manufactured by Mitsubishi Chemical, "jER1010" (solid bisphenol A type epoxy resin) manufactured by Mitsubishi Chemical, and "jER1031S" (tetraphenylethane type epoxy resin) manufactured by Mitsubishi Chemical. These may be used alone or in combination of two or more.

[0021] The liquid epoxy resin is preferably a liquid epoxy resin having two or more epoxy groups in one molecule.

[0022] As the liquid epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AF type epoxy resin, naphthalene type epoxy resin, glycidyl ester type epoxy resin, glycidyl amine type epoxy resin, phenol novolac type epoxy resin, alicyclic epoxy resin having an ester skeleton, cyclohexane type epoxy resin, cyclohexane dimethanol type epoxy resin, glycidyl amine type epoxy resin, and epoxy resin having a butadiene structure are preferred, and bisphenol A type epoxy resin and bisphenol F type epoxy resin are more preferred.

[0023] Specific examples of liquid epoxy resins include "HP4032", "HP4032D", and "HP4032SS" (naphthalene type epoxy resins) manufactured by DIC Corporation; "828US", "jER828EL", "825", and "Epikote 828EL" (bisphenol A type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER807" and "1750" (bisphenol F type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER152" (phenol novolac type epoxy resin) manufactured by Mitsubishi Chemical Corporation; and "630" and "630LSD" (glycidylamine type epoxy resins) manufactured by Mitsubishi Chemical Corporation. epoxy resin); "ZX1059" manufactured by Nippon Steel & Sumitomo Metal Chemical Co., Ltd. (a mixture of bisphenol A type epoxy resin and bisphenol F type epoxy resin); "EX-721" manufactured by Nagase ChemteX Corporation (glycidyl ester type epoxy resin); "Celloxide 2021P" manufactured by Daicel Corporation (alicyclic epoxy resin having an ester skeleton); "PB-3600" manufactured by Daicel Corporation (epoxy resin having a butadiene structure); "ZX1658" and "ZX1658GS" (liquid 1,4-glycidylcyclohexane type epoxy resin) manufactured by Nippon Steel & Sumitomo Metal Chemical Co., Ltd. may be used alone or in combination of two or more types.

[0024] When a liquid epoxy resin and a solid epoxy resin are used in combination as the component (A), the ratio by mass (liquid epoxy resin:solid epoxy resin) is preferably 1:1 to 1:20, more preferably 1:1.5 to 1:15, and particularly preferably 1:2 to 1:10. When the ratio by mass of the liquid epoxy resin and the solid epoxy resin is within such a range, the desired effects of the present invention can be significantly obtained. Furthermore, when used in the form of a resin sheet, appropriate adhesion is usually obtained. Furthermore, when used in the form of a resin sheet, sufficient flexibility is usually obtained, and handling is improved. Furthermore, a cured product having sufficient breaking strength can usually be obtained.

[0025] The epoxy equivalent of the (A) component is preferably 50 g / eq. to 5000 g / eq., more preferably 50 g / eq. to 3000 g / eq., even more preferably 80 g / eq. to 2000 g / eq., and even more preferably 110 g / eq. to 1000 g / eq. When it is in this range, the crosslink density of the cured product of the resin composition layer is sufficient, and an insulating layer with small surface roughness can be obtained. The epoxy equivalent is the mass of an epoxy resin containing one equivalent of epoxy groups. This epoxy equivalent can be measured according to JIS K7236.

[0026] The weight average molecular weight (Mw) of the component (A) is preferably 100 to 5,000, more preferably 250 to 3,000, and even more preferably 400 to 1,500, from the viewpoint of significantly achieving the desired effects of the present invention. The weight average molecular weight of the resin can be measured by gel permeation chromatography (GPC) as a polystyrene-equivalent value.

[0027] The content of the (A) component is preferably 1% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more, based on 100% by mass of the non-volatile components in the resin composition, from the viewpoint of obtaining an insulating layer exhibiting good mechanical strength and insulating reliability. The upper limit of the epoxy resin content is preferably 30% by mass or less, more preferably 25% by mass or less, and particularly preferably 20% by mass or less, based on the viewpoint of significantly obtaining the desired effects of the present invention. In the present invention, the content of each component in the resin composition is the value based on 100% by mass of the non-volatile components in the resin composition, unless otherwise specified.

[0028] <(B) Active ester-based curing agent having a structural unit represented by general formula (1) and a structural unit represented by general formula (2)> The resin composition contains, as component (B), an active ester-based curing agent having a structural unit represented by general formula (1) and a structural unit represented by the following general formula (2): By including a predetermined amount of component (B) in the resin composition, it is possible to obtain a cured product having excellent dielectric properties.

[0029] [ka] (In general formula (1), R 11 each independently represents an optionally substituted aliphatic hydrocarbon group, an optionally substituted aryl group, or an optionally substituted aralkyl group, Z represents an optionally substituted isophthaloyl group, or an optionally substituted naphthalenedicarbonyl group, and n1 represents 0 or an integer of 1 to 3. In general formula (2), R 12 each independently represents an aliphatic hydrocarbon group which may have a substituent, an aryl group which may have a substituent, or an aralkyl group which may have a substituent. n2 represents 0 or an integer of 1 to 3.

[0030] R in general formula (1) 11Examples of the aliphatic hydrocarbon group represented by the formula (1) which may have a substituent include an alkyl group and an alkenyl group, with an alkyl group being preferred. The aliphatic hydrocarbon group preferably has 1 to 20 carbon atoms, more preferably has 1 to 15 carbon atoms, and even more preferably has 1 to 10 carbon atoms, or 1 to 8 or 1 to 5 carbon atoms. The aliphatic hydrocarbon group preferably has a branched structure, and more preferably has an alkyl group having a branched structure or an alkenyl group having a branched structure.

[0031] Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, a s-butyl group, an isobutyl group, a t-butyl group, an n-pentyl group, an isopentyl group, a neopentyl group, a t-pentyl group, a neopentyl group, a 1,2-dimethylpropyl group, an n-hexyl group, an isohexyl group, a t-octyl group, an n-nonyl group, a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, a cyclooctyl group, and a cyclononyl group. Among these, alkyl groups having a branched structure such as an isopropyl group, a s-butyl group, an isobutyl group, a t-butyl group, an isopentyl group, a neopentyl group, a t-pentyl group, and a t-octyl group are preferred.

[0032] Examples of alkenyl groups include vinyl groups, allyl groups, propenyl groups, isopropenyl groups, 1-propenyl groups, 1-butenyl groups, 2-butenyl groups, 3-butenyl groups, 1-hexenyl groups, 2-hexenyl groups, 3-hexenyl groups, 4-hexenyl groups, 5-hexenyl groups, 1-octenyl groups, 2-octenyl groups, and 1-undecenyl groups.

[0033] R in general formula (1) 11Examples of the aryl group which may have a substituent represented by include an aryl group having 6 to 30 carbon atoms, preferably an aryl group having 6 to 20 carbon atoms, and more preferably an aryl group having 6 to 10 carbon atoms. Examples of such aryl groups include those obtained by removing one hydrogen atom from monocyclic aromatic compounds such as phenyl group, tolyl group, furanyl group, pyrrolyl group, thiophene group, imidazolyl group, pyrazolyl group, oxazolyl group, isoxazolyl group, thiazolyl group, isothiazolyl group, pyridinyl group, pyrimidinyl group, pyridazinyl group, pyrazinyl group, triazinyl group, etc.; those obtained by removing one hydrogen atom from condensed ring aromatic compounds such as naphthyl group, anthracenyl group, phenalenyl group, phenanthrenyl group, quinolinyl group, isoquinolinyl group, quinazolinyl group, phthalazinyl group, pteridinyl group, coumarinyl group, indole group, benzimidazolyl group, benzofuranyl group, acridinyl group, etc.; and the like.

[0034] R in general formula (1) 11 Examples of the aralkyl group which may have a substituent represented by include an aralkyl group having 7 to 30 carbon atoms, preferably an aralkyl group having 7 to 20 carbon atoms, and more preferably an aralkyl group having 7 to 10 carbon atoms. Examples of such aralkyl groups include benzyl group, phenethyl group, phenylpropyl group, etc.

[0035] R in general formula (1) 11 The aliphatic hydrocarbon group, aryl group, and aralkyl group represented by may have a substituent. Examples of the substituent include halogen atom, -OH, -O-C 1-6 alkyl group, -N(C 1-10 alkyl group)2, C 1-10 alkyl group, C 6-10 aryl group, -NH2, -CN, -C(O)O-C 1-10 alkyl group, -COOH, -C(O)H, -NO2, etc. Here, the term "C p-q " (p and q are positive integers and p < q) means that the number of carbon atoms of the organic group described immediately after this term is p to q. For example, "C 1-10The expression "alkyl group" refers to an alkyl group having 1 to 10 carbon atoms. These substituents may be bonded to each other to form a ring, and the ring structure also includes a spiro ring and a fused ring.

[0036] R in general formula (1) 11 As the alkyl group, an aliphatic hydrocarbon group which may have a substituent is preferable, an alkyl group is more preferable, and an alkyl group having a branched structure is even more preferable.

[0037] Z in the general formula (1) represents an isophthaloyl group which may have a substituent, or a naphthalenedicarbonyl group which may have a substituent, and is preferably an isophthaloyl group. The isophthaloyl group and the naphthalenedicarbonyl group represented by Z in the general formula (1) may have a substituent. As the substituent, R 11 The substituents are the same as those that may be possessed by the aliphatic hydrocarbon group represented by the formula (1). Note that the isophthaloyl group is a structure represented by the formula (α), and the naphthalene dicarbonyl group is a group in which two carbonyl groups are bonded to a naphthalene ring, and is a structure represented by the formula (β). In the following formulas, "*" represents a bond. [ka]

[0038] In the general formula (1), n1 represents 0 or an integer of 1 to 3, preferably 1 or 2, and more preferably 1. 11 is preferably bonded to the para position relative to "-OZ-" in general formula (1).

[0039] R in general formula (2) 12 R in general formula (1) 11 In addition, n2 in the general formula (2) is the same as n1 in the general formula (1). In the general formula (2), R 12 is preferably bonded at the para position relative to "-O-" in general formula (2).

[0040] The structural unit represented by general formula (1) has three bonds. The structural unit represented by general formula (2) has three bonds. The bond represented by * in the structural unit represented by general formula (1) is preferably bonded to the bond represented by * in the structural unit represented by general formula (2).

[0041] The component (B) preferably has a structure represented by the following general formula (1-1). [ka] (In general formula (1-1), R 13 and R 14 each independently represents an aliphatic hydrocarbon group which may have a substituent, an aryl group which may have a substituent, or an aralkyl group which may have a substituent; Z 1 represents an isophthaloyl group which may have a substituent, or a naphthalene dicarbonyl group which may have a substituent. n3 and n4 each independently represent an integer of 0 or 1 to 3. * represents a bond.)

[0042] R in general formula (1-1) 13 and R 14 R in general formula (1) 11 The same as Z in the general formula (1-1). 1 is the same as Z in general formula (1). n3 and n4 in general formula (1-1) are the same as n1 in general formula (1).

[0043] The terminal of component (B) may have a structure resulting from a reaction between a phenolic hydroxyl group-containing compound having an aliphatic hydrocarbon group, an aryl group, or an aralkyl group and an aromatic polycarboxylic acid or an acid halide thereof. Specifically, component (B) preferably has the following structure (1-2) at the terminal. [ka] (In formula (1-2), R 15 R in general formula (1) 11 is the same as Z 2is the same as Z in general formula (1). n5 is the same as n1 in general formula (1), and * represents a bond.

[0044] The component (B) may be a mixture of an active ester curing agent having a structural unit represented by general formula (1) and a structural unit represented by general formula (2), and an active ester curing agent represented by the following general formula (3). [ka] (In general formula (3), R 1 each independently represents an aliphatic hydrocarbon group which may have a substituent, an aryl group which may have a substituent, or an aralkyl group which may have a substituent; Z 3 represents a phenylene group which may have a substituent or a naphthylene group which may have a substituent. Each n independently represents 0 or an integer of 1 to 5.

[0045] R in general formula (3) 1 R in general formula (1) 11 The same as Z in the general formula (3). 3 is the same as Z in general formula (1). n in general formula (3) is the same as n1 in general formula (1).

[0046] When the (B) component contains an active ester-based curing agent represented by general formula (3), the content thereof is preferably less than 40%, more preferably 35% or less, and even more preferably 30% or less, based on 100% of the (B) component, from the viewpoint of obtaining the effects of the present invention prominently. The lower limit is not particularly limited, but may be 0.5% or more.

[0047] When the (B) component contains an active ester-based curing agent represented by general formula (3), the content of the active ester-based curing agent having the structural unit represented by general formula (1) and the structural unit represented by general formula (2) is preferably more than 60%, more preferably 65% ​​or more, and even more preferably 70% or more, based on 100% of the (B) component, from the viewpoint of obtaining the effects of the present invention significantly. The lower limit is not particularly limited, but may be 99.5% or less, for example.

[0048] The (B) component may be synthesized by a known method. For example, it can be synthesized using a phenolic hydroxyl group-containing compound having an aliphatic hydrocarbon group, an aryl group, or an aralkyl group, a phenolic resin having a molecular structure in which a phenolic compound having one or more aliphatic hydrocarbon groups, an aryl group, or an aralkyl group on an aromatic ring is connected with a methylene group, and an aromatic polycarboxylic acid or an acid halide thereof as reaction raw materials. The specific synthesis of the (B) component can be performed by the method described in, for example, WO 2018 / 008412 and WO 2018 / 008415.

[0049] The component (B) may be a commercially available product, such as "EXB8500-65T" manufactured by DIC Corporation.

[0050] The ratio of the amount of the (A) component to the (B) component is the ratio of [total number of epoxy groups in the (A) component]:[total number of reactive groups in the (B) component], and is preferably in the range of 1:0.01 to 1:20, more preferably 1:0.1 to 1:10, and even more preferably 1:0.5 to 1:5. Here, the "number of epoxy groups in the (A) component" refers to the total value obtained by dividing the mass of the non-volatile component of the (A) component present in the resin composition by the epoxy equivalent. In addition, the "number of active groups in the (B) component" refers to the total value obtained by dividing the mass of the non-volatile component of the (B) component present in the resin composition by the active group equivalent. By setting the ratio of the amount of the (A) component to the (B) component within this range, a cured product with better dielectric properties can be obtained.

[0051] The content of component (B) is 30% by mass or less, preferably 28% by mass or less, and more preferably 25% by mass or less, based on 100% by mass of the non-volatile components in the resin composition, from the viewpoint of suppressing unevenness on the cured substrate. Also, the content of component (B) is preferably 1% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more, based on 100% by mass of the non-volatile components in the resin composition, from the viewpoint of obtaining a cured product with excellent dielectric properties.

[0052] <(C) Inorganic filler> The resin composition contains an inorganic filler as component (C). By using the inorganic filler, the dielectric properties and insulating performance of the cured product of the resin composition can be improved.

[0053] As the material of the inorganic filler, an inorganic compound is used. Examples of the material of the inorganic filler include silica, alumina, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium zirconate titanate, barium zirconate, calcium zirconate, zirconium phosphate, and zirconium tungstate phosphate. Among these, silica is particularly suitable. Examples of silica include amorphous silica, fused silica, crystalline silica, synthetic silica, and hollow silica. Moreover, as the silica, spherical silica is preferable. (C) The inorganic filler may be used alone or in combination of two or more types.

[0054] Examples of commercially available products of component (C) include "UFP-30" manufactured by Denka Company; "SP60-05" and "SP507-05" manufactured by Nippon Steel & Sumitomo Metal Materials Co., Ltd.; "YC100C", "YA050C", "YA050C-MJE", and "YA010C" manufactured by Admatechs Co., Ltd.; "Silfill NSS-3N", "Silfill NSS-4N", and "Silfill NSS-5N" manufactured by Tokuyama Corporation; and "SC2500SQ", "SO-C4", "SO-C2", and "SO-C1" manufactured by Admatechs Co., Ltd.

[0055] The specific surface area of ​​component (C) is preferably 1 m 2 / g or more, more preferably 2m 2 / g or more, particularly preferably 3m 2 / g or more. There is no particular upper limit, but it is preferably 60m 2 / g or less, 50m 2 / g or less or 40m 2 The specific surface area is determined by adsorbing nitrogen gas onto the surface of a sample using a specific surface area measuring device (Macsorb HM-1210 manufactured by Mountec Co., Ltd.) according to the BET method, and calculating the specific surface area using the BET multipoint method.

[0056] From the viewpoint of significantly obtaining the desired effects of the present invention, the average particle size of component (C) is preferably 0.01 μm or more, more preferably 0.05 μm or more, and particularly preferably 0.1 μm or more, and is preferably 5 μm or less, more preferably 2 μm or less, and even more preferably 1 μm or less.

[0057] The average particle size of component (C) can be measured by a laser diffraction / scattering method based on the Mie scattering theory. Specifically, a particle size distribution of the inorganic filler is created on a volume basis using a laser diffraction / scattering particle size distribution measuring device, and the median diameter is used as the average particle size. The measurement sample can be prepared by weighing 100 mg of inorganic filler and 10 g of methyl ethyl ketone into a vial and dispersing the mixture by ultrasonic waves for 10 minutes. The measurement sample is measured using a laser diffraction particle size distribution measuring device with blue and red light wavelengths as the light source, and the volume-based particle size distribution of component (C) is measured using a flow cell method, and the average particle size can be calculated as the median diameter from the particle size distribution obtained. An example of a laser diffraction particle size distribution measuring device is the "LA-960" manufactured by Horiba, Ltd.

[0058] From the viewpoint of improving moisture resistance and dispersibility, it is preferable that the (C) component is treated with a surface treatment agent. Examples of the surface treatment agent include vinylsilane coupling agents, (meth)acrylic coupling agents, fluorine-containing silane coupling agents, aminosilane coupling agents, epoxysilane coupling agents, mercaptosilane coupling agents, silane coupling agents, alkoxysilanes, organosilazane compounds, and titanate coupling agents. Among them, from the viewpoint of obtaining the effects of the present invention remarkably, vinylsilane coupling agents, (meth)acrylic coupling agents, and aminosilane coupling agents are preferred. Moreover, the surface treatment agent may be used alone or in any combination of two or more types.

[0059] Commercially available surface treatment agents include, for example, Shin-Etsu Chemical Co., Ltd.'s "KBM1003" (vinyltriethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM503" (3-methacryloxypropyltriethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM403" (3-glycidoxypropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM803" (3-mercaptopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBE903" (3-aminopropyltriethoxysilane), ... Examples of such silane coupling agents include Shin-Etsu Chemical Co., Ltd.'s "KBM573" (N-phenyl-3-aminopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "SZ-31" (hexamethyldisilazane), Shin-Etsu Chemical Co., Ltd.'s "KBM103" (phenyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM-4803" (long-chain epoxy-type silane coupling agent), and Shin-Etsu Chemical Co., Ltd.'s "KBM-7103" (3,3,3-trifluoropropyltrimethoxysilane).

[0060] The degree of surface treatment with the surface treatment agent is preferably within a predetermined range from the viewpoint of improving the dispersibility of the inorganic filler. Specifically, 100 parts by mass of the inorganic filler is preferably surface-treated with 0.2 parts by mass to 5 parts by mass of the surface treatment agent, more preferably 0.2 parts by mass to 3 parts by mass, and even more preferably 0.3 parts by mass to 2 parts by mass.

[0061] The degree of surface treatment with the surface treatment agent can be evaluated by the amount of carbon per unit surface area of ​​the inorganic filler. From the viewpoint of improving the dispersibility of the inorganic filler, the amount of carbon per unit surface area of ​​the inorganic filler is set to 0.02 mg / m 2 More than 0.1 mg / m is preferable. 2 More preferably, 0.2 mg / m or more 2 On the other hand, from the viewpoint of suppressing an increase in the melt viscosity of the resin varnish and the melt viscosity in the form of a sheet, it is more preferable that the content is 1 mg / m 2 Less than 0.8 mg / m is preferred. 2 Less than 0.5 mg / m is more preferable. 2 The following is even more preferred:

[0062] The amount of carbon per unit surface area of ​​the inorganic filler can be measured after the surface-treated inorganic filler is washed with a solvent (e.g., methyl ethyl ketone (MEK)). Specifically, a sufficient amount of MEK as a solvent is added to the inorganic filler that has been surface-treated with a surface treatment agent, and ultrasonic cleaning is performed at 25°C for 5 minutes. After removing the supernatant and drying the solid content, the amount of carbon per unit surface area of ​​the inorganic filler can be measured using a carbon analyzer. The carbon analyzer that can be used is the "EMIA-320V" manufactured by Horiba, Ltd.

[0063] By including a predetermined amount of the (B) component in the resin composition, unevenness in the cured substrate is suppressed even if the (C) component is included in a large amount. The present invention has a technical significance in that unevenness in the cured substrate is suppressed even if the (C) component content is large, and furthermore, the dielectric properties are excellent. The content of the (C) component is 60% by mass or more, preferably 61% by mass or more, more preferably 62% by mass or more, and is preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 80% by mass or less, assuming that the non-volatile components in the resin composition are 100% by mass.

[0064] When the content of the (B) component when the nonvolatile components in the resin composition are taken as 100% by mass is b, and the content of the (C) component when the nonvolatile components in the resin composition are taken as 100% by mass is c, b / c is preferably 0.01 or more, more preferably 0.05 or more, even more preferably 0.1 or 0.2 or more, and is preferably 3 or less, more preferably 1 or less, and even more preferably 0.5 or less. By adjusting b / c to be within this range, unevenness occurring on the cured substrate can be suppressed, and a cured product with excellent dielectric properties can be obtained.

[0065] <(D) Curing accelerator> In addition to the above-mentioned components, the resin composition may further contain a curing accelerator as an optional component (D). By including the component (D), it becomes possible to further accelerate the polymerization by heat.

[0066] Examples of the component (D) include phosphorus-based curing accelerators, amine-based curing accelerators, imidazole-based curing accelerators, guanidine-based curing accelerators, metal-based curing accelerators, etc. The component (D) may be used alone or in combination of two or more types.

[0067] Examples of the phosphorus-based curing accelerator include triphenylphosphine, phosphonium borate compounds, tetraphenylphosphonium tetraphenylborate, n-butylphosphonium tetraphenylborate, tetrabutylphosphonium decanoate, (4-methylphenyl)triphenylphosphonium thiocyanate, tetraphenylphosphonium thiocyanate, butyltriphenylphosphonium thiocyanate, and the like, with triphenylphosphine and tetrabutylphosphonium decanoate being preferred.

[0068] Examples of the amine curing accelerator include trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, and 1,8-diazabicyclo(5,4,0)-undecene, with 4-dimethylaminopyridine and 1,8-diazabicyclo(5,4,0)-undecene being preferred.

[0069] Examples of the imidazole curing accelerator include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2, 4-Diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-furan Examples of the imidazole compounds include imidazole compounds such as 2-ethyl-4-methyl-5-hydroxymethylimidazole, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, and 2-phenylimidazoline, as well as adducts of imidazole compounds and epoxy resins. Of these, 2-ethyl-4-methylimidazole and 1-benzyl-2-phenylimidazole are preferred.

[0070] As the imidazole-based curing accelerator, a commercially available product may be used, for example, "P200-H50" manufactured by Mitsubishi Chemical Corporation.

[0071] Examples of the guanidine curing accelerator include dicyandiamide, 1-methylguanidine, 1-ethylguanidine, 1-cyclohexylguanidine, 1-phenylguanidine, 1-(o-tolyl)guanidine, dimethylguanidine, diphenylguanidine, trimethylguanidine, tetramethylguanidine, pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, and 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene. Examples of such biguanide include o-[4.4.0]dec-5-ene, 1-methylbiguanide, 1-ethylbiguanide, 1-n-butylbiguanide, 1-n-octadecylbiguanide, 1,1-dimethylbiguanide, 1,1-diethylbiguanide, 1-cyclohexylbiguanide, 1-allylbiguanide, 1-phenylbiguanide, and 1-(o-tolyl)biguanide. Of these, dicyandiamide and 1,5,7-triazabicyclo[4.4.0]dec-5-ene are preferred.

[0072] Examples of metal-based curing accelerators include organometallic complexes or organometallic salts of metals such as cobalt, copper, zinc, iron, nickel, manganese, and tin. Specific examples of organometallic complexes include organocobalt complexes such as cobalt(II) acetylacetonate and cobalt(III) acetylacetonate, organocopper complexes such as copper(II) acetylacetonate, organozinc complexes such as zinc(II) acetylacetonate, organoiron complexes such as iron(III) acetylacetonate, organonickel complexes such as nickel(II) acetylacetonate, and organomanganese complexes such as manganese(II) acetylacetonate. Examples of organometallic salts include zinc octylate, tin octylate, zinc naphthenate, cobalt naphthenate, tin stearate, and zinc stearate.

[0073] From the viewpoint of significantly obtaining the desired effects of the present invention, the content of the (D) component, relative to 100 mass% of the non-volatile components in the resin composition, is preferably 0.01 mass% or more, more preferably 0.02 mass% or more, even more preferably 0.03 mass% or more, and is preferably 1 mass% or less, more preferably 0.5 mass% or less, even more preferably 0.1 mass% or less.

[0074] <(E) Thermoplastic resin> The resin composition may contain (E) a thermoplastic resin as an optional component. (E) Thermoplastic resins include, for example, phenoxy resins, polyvinyl acetal resins, polyolefin resins, polyimide resins, polyamideimide resins, polyetherimide resins, polysulfone resins, polyethersulfone resins, polyetheretherketone resins, polyester resins, etc., and phenoxy resins are preferred. The thermoplastic resins may be used alone or in combination of two or more.

[0075] The polystyrene-equivalent weight average molecular weight of the (E) thermoplastic resin is preferably 38,000 or more, more preferably 40,000 or more, and even more preferably 42,000 or more. The upper limit is preferably 100,000 or less, more preferably 70,000 or less, and even more preferably 60,000 or less. The polystyrene-equivalent weight average molecular weight of the (E) thermoplastic resin is measured by gel permeation chromatography (GPC). Specifically, the polystyrene-equivalent weight average molecular weight of the (E) thermoplastic resin is measured at a column temperature of 40° C. using a measuring device LC-9A / RID-6A manufactured by Shimadzu Corporation, a column Shodex K-800P / K-804L / K-804L manufactured by Showa Denko K.K., chloroform or the like as a mobile phase, and can be calculated using a calibration curve of standard polystyrene.

[0076] Examples of the phenoxy resin include phenoxy resins having one or more skeletons selected from the group consisting of bisphenol A skeleton, bisphenol F skeleton, bisphenol S skeleton, bisphenolacetophenone skeleton, novolac skeleton, biphenyl skeleton, fluorene skeleton, dicyclopentadiene skeleton, norbornene skeleton, naphthalene skeleton, anthracene skeleton, adamantane skeleton, terpene skeleton, and trimethylcyclohexane skeleton. The terminal of the phenoxy resin may be any functional group such as a phenolic hydroxyl group or an epoxy group. The phenoxy resin may be used alone or in combination of two or more. Specific examples of phenoxy resins include "1256" and "4250" (both of which are phenoxy resins containing a bisphenol A skeleton), "YX8100" (phenoxy resin containing a bisphenol S skeleton), and "YX6954" (phenoxy resin containing a bisphenol acetophenone skeleton) manufactured by Mitsubishi Chemical Corporation. Other examples include "FX280" and "FX293" manufactured by Nippon Steel Chemical & Material Co., Ltd., and [YX7200B35], "YL7500BH30", "YX6954BH30", "YX7553", "YX7553BH30", "YL7769BH30", "YL6794", "YL7213", "YL7290", and "YL7482" manufactured by Mitsubishi Chemical Corporation.

[0077] Examples of polyvinyl acetal resin include polyvinyl formal resin and polyvinyl butyral resin, and polyvinyl butyral resin is preferred.Specific examples of polyvinyl acetal resin include "Denka Butyral 4000-2", "Denka Butyral 5000-A", "Denka Butyral 6000-C", and "Denka Butyral 6000-EP" manufactured by Denki Kagaku Kogyo Co., Ltd., and S-LEC BH series, BX series (e.g. BX-5Z), KS series (e.g. KS-1), BL series, and BM series manufactured by Sekisui Chemical Co., Ltd.

[0078] Specific examples of polyimide resins include "Rikacoat SN20" and "Rikacoat PN20" manufactured by New Japan Chemical Co., Ltd. Specific examples of polyimide resins also include modified polyimides such as linear polyimides obtained by reacting bifunctional hydroxyl-terminated polybutadiene, a diisocyanate compound, and a tetrabasic acid anhydride (polyimides described in JP-A-2006-37083), and polysiloxane skeleton-containing polyimides (polyimides described in JP-A-2002-12667 and JP-A-2000-319386, etc.).

[0079] Specific examples of polyamide-imide resins include "Viromax HR11NN" and "Viromax HR16NN" manufactured by Toyobo Co., Ltd. Specific examples of polyamide-imide resins also include modified polyamide-imides such as "KS9100" and "KS9300" (polysiloxane skeleton-containing polyamide-imide) manufactured by Hitachi Chemical Co., Ltd.

[0080] A specific example of the polyether ether ketone resin is "Sumiploy K" manufactured by Sumitomo Chemical Co., Ltd. A specific example of the polyetherimide resin is "Ultem" manufactured by GE Corporation.

[0081] Specific examples of polysulfone resins include polysulfones "P1700" and "P3500" manufactured by Solvay Advanced Polymers.

[0082] Examples of polyolefin resins include ethylene-based copolymer resins such as low-density polyethylene, very low-density polyethylene, high-density polyethylene, ethylene-vinyl acetate copolymer, ethylene-ethyl acrylate copolymer, and ethylene-methyl acrylate copolymer; and polyolefin-based elastomers such as polypropylene and ethylene-propylene block copolymer.

[0083] Examples of the polyester resin include polyethylene terephthalate resin, polyethylene naphthalate resin, polybutylene terephthalate resin, polybutylene naphthalate resin, polytrimethylene terephthalate resin, polytrimethylene naphthalate resin, and polycyclohexane dimethyl terephthalate resin.

[0084] Among these, the thermoplastic resin (E) is preferably a phenoxy resin. Therefore, the preferred thermoplastic resin is a phenoxy resin, and a phenoxy resin having a weight average molecular weight of 40,000 or more is particularly preferred.

[0085] The content of the (E) thermoplastic resin is preferably 0.1% by mass or more, more preferably 0.3% by mass or more, and even more preferably 0.5% by mass or more, based on 100% by mass of the non-volatile components in the resin composition. The upper limit is preferably 5% by mass or less, more preferably 4% by mass or less, and even more preferably 3% by mass or less.

[0086] <(F) Hardener> The resin composition may contain a curing agent (F) as an optional component. However, the component (F) does not include components that fall under the category of component (B). By including the curing agent (F) in the resin composition, it becomes possible to further suppress unevenness in the cured substrate.

[0087] Examples of the (F) curing agent include phenol-based curing agents, naphthol-based curing agents, benzoxazine-based curing agents, cyanate ester-based curing agents, carbodiimide-based curing agents, amine-based curing agents, acid anhydride-based curing agents, maleimide-based curing agents, (meth)acrylic-based curing agents, polyphenylene ether-based curing agents (styrene-based curing agents), allyl-based curing agents, active ester-based curing agents other than component (B), etc. The (F) curing agent may be used alone or in combination of two or more types.

[0088] As the phenol-based curing agent and naphthol-based curing agent, those having a novolak structure are preferred from the viewpoint of heat resistance and water resistance, and from the viewpoint of adhesion to the conductor layer, nitrogen-containing phenol-based curing agents are preferred, and triazine skeleton-containing phenol-based curing agents are more preferred.

[0089] Specific examples of phenol-based curing agents and naphthol-based curing agents include, for example, "MEH-7700", "MEH-7810", and "MEH-7851" manufactured by Meiwa Chemical Industry Co., Ltd.; "NHN", "CBN", and "GPH" manufactured by Nippon Kayaku Co., Ltd.; "SN170", "SN180", "SN190", "SN475", "SN485", "SN495", "SN-495V", and "SN375" manufactured by Nippon Steel & Sumikin Chemical Co., Ltd.; and "TD-2090", "LA-7052", "LA-7054", "LA-1356", "LA-3018-50P", and "EXB-9500" manufactured by DIC Corporation.

[0090] Specific examples of benzoxazine-based curing agents include "ODA-BOZ" manufactured by JFE Chemical Corporation, "HFB2006M" manufactured by Showa Polymer Co., Ltd., and "Pd" and "Fa" manufactured by Shikoku Chemical Industry Co., Ltd.

[0091] Examples of cyanate ester curing agents include bifunctional cyanate resins such as bisphenol A dicyanate, polyphenol cyanate, oligo(3-methylene-1,5-phenylene cyanate), 4,4'-methylenebis(2,6-dimethylphenyl cyanate), 4,4'-ethylidene diphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanate phenylmethane), bis(4-cyanate-3,5-dimethylphenyl)methane, 1,3-bis(4-cyanate phenyl-1-(methylethylidene))benzene, bis(4-cyanate phenyl)thioether, and bis(4-cyanate phenyl)ether; polyfunctional cyanate resins derived from phenol novolac and cresol novolac; and prepolymers in which these cyanate resins are partially converted to triazine. Specific examples of cyanate ester-based curing agents include "PT30" and "PT60" (phenol novolac type multifunctional cyanate ester resins), "ULL-950S" (multifunctional cyanate ester resin), "BA230", and "BA230S75" (prepolymers in which part or all of bisphenol A dicyanate has been converted to triazine to form a trimer), all of which are manufactured by Lonza Japan.

[0092] Specific examples of carbodiimide-based curing agents include "V-03" and "V-07" manufactured by Nisshinbo Chemical Inc.

[0093] The amine-based curing agent may be a curing agent having one or more amino groups in one molecule, such as aliphatic amines, polyether amines, alicyclic amines, aromatic amines, etc., and among them, aromatic amines are preferred from the viewpoint of achieving the desired effects of the present invention. The amine-based curing agent is preferably a primary amine or a secondary amine, and more preferably a primary amine. Specific examples of amine-based curing agents include 4,4'-methylenebis(2,6-dimethylaniline), diphenyldiaminosulfone, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylsulfone, 3,3'-diaminodiphenylsulfone, m-phenylenediamine, m-xylylenediamine, diethyltoluenediamine, 4,4'-diaminodiphenylether, 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dihydroxybenzidine, 2,2-bis(3-amino-4-hydroxyphenyl)propanediamine, and the like. bis(4-aminophenyl)propane, 3,3-dimethyl-5,5-diethyl-4,4-diphenylmethanediamine, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-(4-aminophenoxy)phenyl)propane, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, bis(4-(4-aminophenoxy)phenyl)sulfone, bis(4-(3-aminophenoxy)phenyl)sulfone, etc. The amine-based curing agent may be a commercially available product, for example, "KAYABOND C-200S", "KAYABOND C-100", "KAYAHARD AA", "KAYAHARD AB", "KAYAHARD AS" manufactured by Nippon Kayaku Co., Ltd., "Epicure W" manufactured by Mitsubishi Chemical Corporation, etc.

[0094] Examples of the acid anhydride curing agent include a curing agent having one or more acid anhydride groups in one molecule. Specific examples of the acid anhydride curing agent include phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride, hydrogenated methylnadic anhydride, trialkyltetrahydrophthalic anhydride, dodecenyl succinic anhydride, 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, trimellitic anhydride, pyromellitic anhydride, and benzophenonetetracarboxylic dianhydride. Examples of acid anhydrides include anhydrides, biphenyltetracarboxylic dianhydride, naphthalenetetracarboxylic dianhydride, oxydiphthalic dianhydride, 3,3'-4,4'-diphenylsulfonetetracarboxylic dianhydride, 1,3,3a,4,5,9b-hexahydro-5-(tetrahydro-2,5-dioxo-3-furanyl)-naphtho[1,2-C]furan-1,3-dione, ethylene glycol bis(anhydrotrimellitate), and polymeric acid anhydrides such as styrene-maleic acid resin, which is a copolymer of styrene and maleic acid.

[0095] The maleimide curing agent is a compound containing a maleimide group represented by the following formula (F-1) in the molecule. The maleimide curing agent includes a solid maleimide curing agent and a liquid or semi-solid maleimide curing agent. [ka]

[0096] Here, the determination of liquid, semi-solid, and solid state is made in accordance with the "Method of Confirming Liquid State" in Appendix 2 of the Ministerial Ordinance on the Testing and Properties of Hazardous Materials (Ministry of Home Affairs Ordinance No. 1 of 1989). The specific determination method is as follows.

[0097] (1) Equipment Thermostatic water bath: Use a container equipped with an agitator, heater, thermometer, and automatic temperature controller (capable of controlling temperature to within ±0.1°C) and with a depth of 150 mm or more. In determining whether a substance is liquid, semi-solid, or solid, a combination of a low-temperature constant temperature water bath (model BU300) and an input type constant temperature device Thermomate (model BF500) manufactured by Yamato Scientific Co., Ltd. is used. Approximately 22 liters of tap water is placed into the low-temperature constant temperature water bath (model BU300), the Thermomate (model BF500) attached to it is turned on and set to the set temperature (20°C or 60°C), and the water temperature can be fine-tuned using the Thermomate (model BF500) to within ±0.1°C of the set temperature; however, any device capable of similar adjustments can be used.

[0098] Test tube: The test tubes used are cylindrical, flat-bottomed transparent glass tubes with an inner diameter of 30 mm and a height of 120 mm, as shown in Fig. 1, with marked lines 11A and 12B at heights of 55 mm and 85 mm from the bottom of the tube, respectively, and a test tube 10a for liquid determination, with the mouth of the test tube sealed with a rubber stopper 13a, and a test tube 10b for temperature measurement, with the mouth of the test tube sealed with a rubber stopper 13b of the same size and marked lines with a hole in the center for inserting and supporting a thermometer, and a thermometer 14 inserted into the rubber stopper 13b. Hereinafter, the marked line at a height of 55 mm from the bottom of the tube will be referred to as "line A", and the marked line at a height of 85 mm from the bottom of the tube will be referred to as "line B". As the thermometer 14, a thermometer for measuring the freezing point (SOP-58 scale range 0 to 100°C) as specified in JIS B7410 (1982) "Glass thermometer for testing petroleum products" is used, but any thermometer that can measure temperatures in the range of 0 to 100°C will do.

[0099] (2) Test procedure The sample that has been left for 24 hours or more under atmospheric pressure at a temperature of 60±5°C is poured into the liquid determination test tube 10a shown in Figure 1(a) and the temperature measurement test tube 10b shown in Figure 1(b) up to the 11A line. The two test tubes 10a and 10b are placed upright in a low-temperature constant temperature water bath so that the 12B line is below the water surface. The thermometer is placed so that its bottom end is 30 mm below the 11A line. After the sample temperature reaches the set temperature ±0.1° C., maintain the state for 10 minutes. After 10 minutes, remove the liquid state determination test tube 10a from the low-temperature constant temperature water bath and immediately lay it horizontally on a horizontal test table. Use a stopwatch to measure and record the time it takes for the tip of the liquid level in the test tube to move from line 11A to line 12B.

[0100] Similarly, for samples that have been left for 24 hours or more under atmospheric pressure at a temperature of 20±5°C, the test is carried out in the same manner as for samples that have been left for 24 hours or more under atmospheric pressure at a temperature of 60±5°C, and the time it takes for the tip of the liquid level in the test tube to move from line 11A to line 12B is measured and recorded with a stopwatch.

[0101] At 20°C, a liquid is determined to be in a state where the measurement time is within 90 seconds. A sample that has a measured time of more than 90 seconds at 20°C and 90 seconds or less at 60°C is judged to be semi-solid. At 60°C, a specimen that lasts for more than 90 seconds is considered to be solid.

[0102] The number of maleimide groups per molecule of the solid maleimide-based curing agent is, from the viewpoint of significantly obtaining the desired effects of the present invention, preferably 1 or more, more preferably 2 or more, even more preferably 3 or more, and is preferably 10 or less, more preferably 6 or less, and particularly preferably 3 or less.

[0103] From the viewpoint of significantly obtaining the desired effects of the present invention, the solid maleimide-based curing agent preferably has either an aliphatic hydrocarbon group or an aromatic hydrocarbon group, and more preferably has an aliphatic hydrocarbon group and an aromatic hydrocarbon group.

[0104] The aliphatic hydrocarbon group is preferably a divalent aliphatic hydrocarbon group, more preferably a divalent saturated aliphatic hydrocarbon group, and further preferably an alkylene group. The alkylene group is preferably an alkylene group having 1 to 10 carbon atoms, more preferably an alkylene group having 1 to 6 carbon atoms, further preferably an alkylene group having 1 to 3 carbon atoms, and particularly preferably a methylene group.

[0105] As the aromatic hydrocarbon group, monovalent and divalent aromatic hydrocarbon groups are preferred, and aryl and arylene groups are more preferred. As the arylene group, an arylene group having 6 to 30 carbon atoms is preferred, an arylene group having 6 to 20 carbon atoms is more preferred, and an arylene group having 6 to 10 carbon atoms is even more preferred. Examples of such an arylene group include a phenylene group, a naphthylene group, an anthracenylene group, an aralkyl group, a biphenylene group, and a biphenylaralkyl group, and among these, a phenylene group, an aralkyl group, a biphenylene group, and a biphenylaralkyl group are preferred, and a phenylene group, an aralkyl group, and a biphenylene group are even more preferred. As the aryl group, an aryl group having 6 to 30 carbon atoms is preferred, an aryl group having 6 to 20 carbon atoms is more preferred, an aryl group having 6 to 10 carbon atoms is even more preferred, and a phenyl group is particularly preferred.

[0106] In the solid maleimide-based curing agent, from the viewpoint of significantly obtaining the desired effects of the present invention, it is preferable that the nitrogen atom of the maleimide group is directly bonded to a monovalent or divalent aromatic hydrocarbon group, where "directly" means that there is no other group between the nitrogen atom of the maleimide group and the aromatic hydrocarbon group.

[0107] The solid maleimide-based curing agent preferably has a structure represented by the following formula (F-2), for example. [ka] In formula (F-2), R 31 and R 36 represents a maleimide group, and R 32 , R 33 , R 34 and R 35 each independently represents a hydrogen atom, an alkyl group, or an aryl group, and each D independently represents a divalent aromatic group. m1 and m2 each independently represent an integer of 1 to 10, and a represents an integer of 1 to 100.

[0108] R in formula (F-2) 32 , R 33 , R34 and R 35 each independently represents a hydrogen atom, an alkyl group, or an aryl group, and is preferably a hydrogen atom.

[0109] The alkyl group is preferably an alkyl group having 1 to 10 carbon atoms, more preferably an alkyl group having 1 to 6 carbon atoms, and even more preferably an alkyl group having 1 to 3 carbon atoms. The alkyl group may be linear, branched, or cyclic. Examples of such alkyl groups include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, and an isopropyl group.

[0110] The aryl group is preferably an aryl group having 6 to 20 carbon atoms, more preferably an aryl group having 6 to 15 carbon atoms, and even more preferably an aryl group having 6 to 10 carbon atoms. The aryl group may be a single ring or a condensed ring. Examples of such aryl groups include a phenyl group, a naphthyl group, and an anthracenyl group.

[0111] The alkyl group and the aryl group may have a substituent. The substituent is, for example, R 11 The substituents are the same as those that the aliphatic hydrocarbon group represented by the formula (I) may have.

[0112] D in formula (F-2) represents a divalent aromatic group. Examples of the divalent aromatic group include a phenylene group, a naphthylene group, an anthracenylene group, an aralkyl group, a biphenylene group, and a biphenylaralkyl group. Among them, a biphenylene group and a biphenylaralkyl group are preferable, and a biphenylene group is more preferable. The divalent aromatic group may have a substituent. Examples of the substituent include R in general formula (1). 11 The substituents are the same as those that the aliphatic hydrocarbon group represented by the formula (I) may have.

[0113] m1 and m2 each independently represent an integer of 1 to 10, preferably 1 to 6, more preferably 1 to 3, even more preferably 1 or 2, and still more preferably 1.

[0114] "a" represents an integer of 1 to 100, preferably 1 to 50, more preferably 1 to 20, and further preferably 1 to 5.

[0115] As the solid maleimide-based curing agent, a resin represented by formula (F-3) is preferable. [ka] In formula (F-3), R 37 and R 38 represents a maleimide group. a1 represents an integer of 1 to 100.

[0116] a1 is the same as a in formula (F-2), and the preferred range is also the same.

[0117] As the solid maleimide-based curing agent, a commercially available product can be used, for example, "MIR-3000-70MT" manufactured by Nippon Kayaku Co., Ltd.

[0118] The liquid or semi-solid maleimide-based curing agent is a compound having at least one maleimide group in the molecule.

[0119] In the maleimide-based curing agent, the alkyl group having 5 or more carbon atoms and the alkylene group having 5 or more carbon atoms are preferably directly bonded to the nitrogen atom of the maleimide group.

[0120] The number of maleimide groups per molecule of the maleimide curing agent may be 1, but is preferably 2 or more, and is preferably 10 or less, more preferably 6 or less, and particularly preferably 3 or less. By using a maleimide curing agent having 2 or more maleimide groups per molecule, the effects of the present invention can be significantly obtained.

[0121] The maleimide-based curing agent is preferably represented by the following general formula (F-4). [ka] In formula (F-4), M represents an alkylene group having 5 or more carbon atoms which may have a substituent, and L represents a single bond or a divalent linking group.

[0122] M represents an alkylene group having 5 or more carbon atoms which may have a substituent. The alkylene group of M is the same as the alkylene group having 5 or more carbon atoms described above. The substituent of M is R 11 The substituent is the same as the substituent that the aliphatic hydrocarbon group represented by the formula (I) may have, and the substituent is preferably an alkyl group having 5 or more carbon atoms.

[0123] L represents a single bond or a divalent linking group. Examples of the divalent linking group include an alkylene group, an alkenylene group, an alkynylene group, an arylene group, -C(=O)-, -C(=O)-O-, -NR 0 -(R 0 is a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, an oxygen atom, a sulfur atom, or C(=O)NR 0 -, a divalent group derived from phthalimide, a divalent group derived from pyromellitic diimide, and a group consisting of a combination of two or more of these divalent groups. The alkylene group, alkenylene group, alkynylene group, arylene group, divalent group derived from phthalimide, divalent group derived from pyromellitic diimide, and a group consisting of a combination of two or more of these divalent groups may have an alkyl group having 5 or more carbon atoms as a substituent. The divalent group derived from phthalimide represents a divalent group derived from phthalimide, specifically a group represented by general formula (F-5). The divalent group derived from pyromellitic diimide represents a divalent group derived from pyromellitic diimide, specifically a group represented by general formula (F-6). In the formula, "*" represents a bond. [ka]

[0124] The alkylene group as the divalent linking group in L is preferably an alkylene group having 1 to 50 carbon atoms, more preferably an alkylene group having 1 to 45 carbon atoms, and particularly preferably an alkylene group having 1 to 40 carbon atoms. This alkylene group may be linear, branched, or cyclic. Examples of such alkylene groups include a methylethylene group, a cyclohexylene group, a pentylene group, a hexylene group, a heptylene group, an octylene group, a nonylene group, a decylene group, an undecylene group, a dodecylene group, a tridecylene group, a heptadecylene group, a hexatriacontylene group, a group having an octylene-cyclohexylene structure, a group having an octylene-cyclohexylene-octylene structure, and a group having a propylene-cyclohexylene-octylene structure.

[0125] The alkenylene group as the divalent linking group in L is preferably an alkenylene group having 2 to 20 carbon atoms, more preferably an alkenylene group having 2 to 15 carbon atoms, and particularly preferably an alkenylene group having 2 to 10 carbon atoms. This alkenylene group may be linear, branched, or cyclic. Examples of such alkenylene groups include a methylethylenylene group, a cyclohexenylene group, a pentenylene group, a hexenylene group, a heptenylene group, and an octenylene group.

[0126] The alkynylene group as the divalent linking group in L is preferably an alkynylene group having 2 to 20 carbon atoms, more preferably an alkynylene group having 2 to 15 carbon atoms, and particularly preferably an alkynylene group having 2 to 10 carbon atoms. This alkynylene group may be linear, branched, or cyclic. Examples of such alkynylene groups include a methylethynylene group, a cyclohexynylene group, a pentynylene group, a hexynylene group, a heptynylene group, and an octynylene group.

[0127] The arylene group as the divalent linking group in L is preferably an arylene group having 6 to 24 carbon atoms, more preferably an arylene group having 6 to 18 carbon atoms, still more preferably an arylene group having 6 to 14 carbon atoms, and even more preferably an arylene group having 6 to 10 carbon atoms. Examples of the arylene group include a phenylene group, a naphthylene group, and an anthracenylene group.

[0128] The alkylene group, alkenylene group, alkynylene group, and arylene group, which are the divalent linking groups in L, may have a substituent. Examples of the substituent include R 11 The substituent is the same as the substituent that the aliphatic hydrocarbon group represented by the formula (I) may have, and is preferably an alkyl group having 5 or more carbon atoms.

[0129] Examples of the group consisting of a combination of two or more divalent groups in L include a divalent group consisting of a combination of an alkylene group, a divalent group derived from phthalimide, and an oxygen atom; a divalent group consisting of a combination of a divalent group derived from phthalimide, an oxygen atom, an arylene group, and an alkylene group; a divalent group consisting of a combination of an alkylene group and a divalent group derived from pyromellitic diimide; and the like. The group consisting of a combination of two or more divalent groups may form a ring such as a condensed ring by the combination of the respective groups. In addition, the group consisting of a combination of two or more divalent groups may be a repeating unit having a repeating unit number of 1 to 10.

[0130] Among them, L in the general formula (F-4) is preferably an oxygen atom, an arylene group having 6 to 24 carbon atoms which may have a substituent, an alkylene group having 1 to 50 carbon atoms which may have a substituent, an alkyl group having 5 or more carbon atoms, a divalent group derived from phthalimide, a divalent group derived from pyromellitic diimide, or a divalent group consisting of a combination of two or more of these groups. Among them, L is more preferably an alkylene group; a divalent group having a structure of an alkylene group-a divalent group derived from phthalimide-oxygen atom-a divalent group derived from phthalimide; a divalent group having a structure of an alkylene group-a divalent group derived from phthalimide-oxygen atom-arylene group-alkylene group-arylene group-oxygen atom-a divalent group derived from phthalimide; or a divalent group having a structure of an alkylene-a divalent group derived from pyromellitic diimide.

[0131] The maleimide-based curing agent represented by general formula (F-4) is preferably represented by general formula (F-7). [ka] In general formula (F-7), M 1 each independently represents an alkylene group having 5 or more carbon atoms which may have a substituent, each Z independently represents an alkylene group having 5 or more carbon atoms which may have a substituent or a divalent group having an aromatic ring which may have a substituent, and t represents an integer of 1 to 10.

[0132] M 1 Each of M independently represents an alkylene group having 5 or more carbon atoms which may have a substituent. 1 is the same as M in general formula (F-4).

[0133] Each Z independently represents an alkylene group having 5 or more carbon atoms which may have a substituent, or a divalent group having an aromatic ring which may have a substituent. The alkylene group in Z may be any of linear, branched, and cyclic, and among them, a cyclic alkylene group having 5 or more carbon atoms which may have a substituent is preferred. The number of carbon atoms of the alkylene group is preferably 6 or more, more preferably 8 or more, preferably 50 or less, more preferably 45 or less, and even more preferably 40 or less. Examples of such alkylene groups include a group having an octylene-cyclohexylene structure, a group having an octylene-cyclohexylene-octylene structure, and a group having a propylene-cyclohexylene-octylene structure.

[0134] Examples of the aromatic ring in the divalent group having an aromatic ring represented by Z include a benzene ring, a naphthalene ring, an anthracene ring, a phthalimide ring, a pyromellitic diimide ring, and an aromatic heterocycle, and the like are mentioned, with a benzene ring, a phthalimide ring, and a pyromellitic diimide ring being preferred. That is, the divalent group having an aromatic ring is preferably a divalent group having a benzene ring which may have a substituent, a divalent group having a phthalimide ring which may have a substituent, or a divalent group having a pyromellitic diimide ring which may have a substituent. Examples of the divalent group having an aromatic ring include a group consisting of a combination of a divalent group derived from phthalimide and an oxygen atom; a group consisting of a combination of a divalent group derived from phthalimide, an oxygen atom, an arylene group, and an alkylene group; a group consisting of a combination of an alkylene group and a divalent group derived from pyromellitic diimide; a divalent group derived from pyromellitic diimide; a group consisting of a combination of a divalent group derived from phthalimide and an alkylene group; and the like. The arylene group and alkylene group are the same as the arylene group and alkylene group in the divalent linking group represented by L in general formula (F-4).

[0135] The alkylene group and the divalent group having an aromatic ring represented by Z may have a substituent. Examples of the substituent include R 11 The substituents are the same as those that the aliphatic hydrocarbon group represented by the formula (I) may have.

[0136] Specific examples of the group represented by Z include the following groups: In the formula, "*" represents a bond. [ka] [ka]

[0137] The maleimide curing agent represented by general formula (F-4) is preferably any one of a maleimide curing agent represented by general formula (F-8) and a maleimide curing agent represented by general formula (F-9). [ka] In general formula (F-8), M 2 and M 3 each independently represents an alkylene group having 5 or more carbon atoms which may have a substituent; R 40 each independently represents an oxygen atom, an arylene group, an alkylene group, or a divalent group consisting of a combination of two or more of these groups. t1 represents an integer of 1 to 10. In general formula (F-9), M 4 , M 6 and M 7 each independently represents an alkylene group having 5 or more carbon atoms which may have a substituent; M 5 each independently represents a divalent group having an aromatic ring which may have a substituent; R 41 and R 42 each independently represents an alkyl group having 5 or more carbon atoms. t2 represents an integer of 0 to 10, and u1 and u2 each independently represent an integer of 0 to 4.

[0138] M 2 and M 3 Each of M independently represents an alkylene group having 5 or more carbon atoms which may have a substituent. 2 and M 3 is the same as the alkylene group having 5 or more carbon atoms represented by M in general formula (F-4), and a hexatriacontylene group is preferred.

[0139] R 40 R each independently represents an oxygen atom, an arylene group, an alkylene group, or a group consisting of a combination of two or more of these divalent groups. The arylene group and the alkylene group are the same as the arylene group and the alkylene group in the divalent linking group represented by L in the general formula (F-4). 40 is preferably an oxygen atom or a group formed from a combination of two or more divalent groups.

[0140] R 40 In the formula, examples of the group consisting of a combination of two or more divalent groups include a combination of an oxygen atom, an arylene group, and an alkylene group. Specific examples of the group consisting of a combination of two or more divalent groups include the following groups. In the formula, "*" represents a bond. [ka]

[0141] M 4 , M 6 and M 7 Each of M independently represents an alkylene group having 5 or more carbon atoms which may have a substituent. 4 , M 6 and M 7 is the same as the alkylene group having 5 or more carbon atoms which may have a substituent represented by M in general formula (F-4), and is preferably a hexylene group, a heptylene group, an octylene group, a nonylene group, or a decylene group, and more preferably an octylene group.

[0142] M 5 Each of M independently represents a divalent group having an aromatic ring which may have a substituent. 5is the same as the divalent group having an aromatic ring which may have a substituent represented by Z in general formula (F-7), and is preferably a group consisting of a combination of an alkylene group and a divalent group derived from pyromellitic diimide; a group consisting of a combination of a divalent group derived from phthalimide and an alkylene group, and more preferably a group consisting of a combination of an alkylene group and a divalent group derived from pyromellitic diimide. The arylene group and alkylene group are the same as the arylene group and alkylene group in the divalent linking group represented by L in general formula (F-4).

[0143] M 5 Specific examples of the group represented by the formula include the following groups: In the formula, "*" represents a bond. [ka]

[0144] R 41 and R 42 R each independently represents an alkyl group having 5 or more carbon atoms. 41 and R 42 is the same as the above-mentioned alkyl group having 5 or more carbon atoms, and is preferably a hexyl group, a heptyl group, an octyl group, a nonyl group, or a decyl group, and more preferably a hexyl group or an octyl group.

[0145] Each of u1 and u2 independently represents an integer of 1 to 15, and an integer of 1 to 10 is preferable.

[0146] Specific examples of the maleimide-based curing agent include the following compounds (F1) to (F3). However, the maleimide-based curing agent is not limited to these specific examples. In the formula, v represents an integer of 1 to 10. [ka] [ka]

[0147] Specific examples of maleimide-based curing agents include "BMI1500" (compound of formula (F1)), "BMI1700" (compound of formula (F2)), and "BMI689" (compound of formula (F3)), all of which are manufactured by Designer Molecules.

[0148] From the viewpoint of significantly obtaining the desired effects of the present invention, the maleimide group equivalent of the maleimide curing agent is preferably 50 g / eq. to 2000 g / eq., more preferably 100 g / eq. to 1000 g / eq., and further preferably 150 g / eq. to 500 g / eq. The maleimide group equivalent is the mass of the maleimide curing agent containing one equivalent of maleimide group.

[0149] The polyphenylene ether-based curing agent is a curing agent having a vinylphenyl group, which is a group having the structure shown below. [ka] (* represents a bond.)

[0150] The polyphenylene ether curing agent preferably has two or more vinylphenyl groups per molecule, from the viewpoint of obtaining a cured product with a low dielectric tangent.

[0151] The polyphenylene ether curing agent preferably has a cyclic structure from the viewpoint of obtaining a cured product with a low dielectric tangent. The cyclic structure is preferably a divalent cyclic group. The divalent cyclic group may be either a cyclic group containing an alicyclic structure or a cyclic group containing an aromatic ring structure. In addition, the polyphenylene ether curing agent may have a plurality of divalent cyclic groups.

[0152] From the viewpoint of significantly obtaining the desired effects of the present invention, the divalent cyclic group is preferably a 3-membered or larger ring, more preferably a 4-membered or larger ring, and even more preferably a 5-membered or larger ring, and is preferably a 20-membered or smaller ring, more preferably a 15-membered or smaller ring, and even more preferably a 10-membered or smaller ring. In addition, the divalent cyclic group may be a monocyclic structure or a polycyclic structure.

[0153] The ring in the divalent cyclic group may have a ring skeleton constituted by a heteroatom other than carbon atoms. Examples of the heteroatom include an oxygen atom, a sulfur atom, and a nitrogen atom, and an oxygen atom is preferred. The ring may have one or more heteroatoms.

[0154] Specific examples of the divalent cyclic group include the following divalent groups (xii) and (xiii). [ka] (In the divalent groups (xii) and (xiii), R 51 , R 52 , R 55 , R 56 , R 57 , R 61 , and R 62 each independently represents a halogen atom, an alkyl group having 6 or less carbon atoms, or a phenyl group; R 53 , R 54 , R 58 , R 59 , and R 60 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 6 or less carbon atoms, or a phenyl group.

[0155] Examples of halogen atoms include fluorine, chlorine, bromine, and iodine atoms. Examples of alkyl groups having 6 or less carbon atoms include methyl, ethyl, propyl, butyl, pentyl, and hexyl groups, with methyl being preferred. 51 , R 52 , R 55 , R 56 , R 57 , R 61 , and R 62 R preferably represents a methyl group. 53 , R 54 , R 58 , R 59 , and R 60 is preferably a hydrogen atom or a methyl group.

[0156] In addition, the divalent cyclic group may be a combination of a plurality of divalent cyclic groups. Specific examples of the combination of divalent cyclic groups include the divalent cyclic group represented by the following formula (F4) (divalent group (a)). [ka] (In formula (F4), R 71 , R 72 , R 75 , R 76 , R 77 , R 81 , R 82 , R 85 and R 86 each independently represents a halogen atom, an alkyl group having 6 or less carbon atoms, or a phenyl group; R 73 , R 74 , R 78 , R 79 , R 80 , R 83 and R 84 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 6 or less carbon atoms, or a phenyl group. d1 and d2 each represent an integer of 0 to 300, except for the case where one of d1 and d2 is 0.

[0157] R 71 , R 72 , R 85 and R 86 R in formula (xii) 51 is the same as R 73 , R 74 , R 83 and R 84 R in formula (xii) 53 is the same as R 75 , R 76 , R 77 , R 81 , and R 82 R in formula (xiii) 55 is the same as R 78 , R 79 , and R 80 R in formula (xiii) 58 is the same as:

[0158] d1 and d2 represent an integer of 0 to 300, except when one of d1 and d2 is 0. d1 and d2 preferably represent an integer of 1 to 100, more preferably an integer of 1 to 50, and even more preferably an integer of 1 to 10. d1 and d2 may be the same or different.

[0159] The divalent cyclic group may have a substituent, such as a halogen atom, an alkyl group, an alkoxy group, an aryl group, an arylalkyl group, a silyl group, an acyl group, an acyloxy group, a carboxy group, a sulfo group, a cyano group, a nitro group, a hydroxy group, a mercapto group, or an oxo group, and an alkyl group is preferred.

[0160] The vinylphenyl group may be directly bonded to the divalent cyclic group, or may be bonded via a divalent linking group. Examples of the divalent linking group include an alkylene group, an alkenylene group, an arylene group, a heteroarylene group, -C(=O)O-, -O-, -NHC(=O)-, -NC(=O)N-, -NHC(=O)O-, -C(=O)-, -S-, -SO-, -NH-, and the like, and may be a group in which a plurality of these are combined. The alkylene group is preferably an alkylene group having 1 to 10 carbon atoms, more preferably an alkylene group having 1 to 6 carbon atoms, and even more preferably an alkylene group having 1 to 5 carbon atoms or an alkylene group having 1 to 4 carbon atoms. The alkylene group may be linear, branched, or cyclic. Examples of such alkylene groups include methylene, ethylene, propylene, butylene, pentylene, hexylene, and 1,1-dimethylethylene groups, and are preferably methylene, ethylene, or 1,1-dimethylethylene. As the alkenylene group, an alkenylene group having 2 to 10 carbon atoms is preferred, an alkenylene group having 2 to 6 carbon atoms is more preferred, and an alkenylene group having 2 to 5 carbon atoms is even more preferred. As the arylene group or heteroarylene group, an arylene group or heteroarylene group having 6 to 20 carbon atoms is preferred, and an arylene group or heteroarylene group having 6 to 10 carbon atoms is more preferred. As the divalent linking group, an alkylene group is preferred, and among them, a methylene group is preferred.

[0161] The polyphenylene ether curing agent is preferably represented by the following formula (F-10). [ka] (In formula (F-10), R 91 and R 92 each independently represents a divalent linking group. Ring B1 represents a divalent cyclic group.

[0162] R 91 and R 92 each independently represents a divalent linking group. The divalent linking group is the same as the divalent linking group described above.

[0163] Ring B1 represents a divalent cyclic group. Ring B1 is the same as the above divalent cyclic group.

[0164] Ring B1 may have a substituent. The substituent is the same as the substituent that the above divalent cyclic group may have.

[0165] Specific examples of polyphenylene ether-based curing agents are shown below, but the present invention is not limited thereto. [ka] (q1 is the same as d1 in formula (F4), and q1 is the same as d2 in formula (F4).)

[0166] The polyphenylene ether-based curing agent may be a commercially available product, such as "OPE-2St" manufactured by Mitsubishi Gas Chemical Co., Inc. The polyphenylene ether-based curing agent may be used alone or in combination of two or more kinds.

[0167] From the viewpoint of significantly obtaining the desired effects of the present invention, the number average molecular weight of the polyphenylene ether-based curing agent is preferably 3000 or less, more preferably 2500 or less, even more preferably 2000 or less, or 1500 or less. The lower limit is preferably 100 or more, more preferably 300 or more, even more preferably 500 or more, or 1000 or more. The number average molecular weight is a polystyrene-equivalent number average molecular weight measured using gel permeation chromatography (GPC).

[0168] The (meth)acrylic curing agent is a compound containing an acryloyl group, a methacryloyl group, and a combination thereof. In order to significantly obtain the desired effects of the present invention, the (meth)acrylic curing agent preferably has two or more (meth)acryloyl groups per molecule. The term "(meth)acryloyl group" includes an acryloyl group, a methacryloyl group, and a combination thereof.

[0169] The (meth)acrylic curing agent preferably has a cyclic structure from the viewpoint of significantly obtaining the desired effects of the present invention. The cyclic structure is preferably a divalent cyclic group. The divalent cyclic group may be either a cyclic group containing an alicyclic structure or a cyclic group containing an aromatic ring structure. Among them, from the viewpoint of significantly obtaining the desired effects of the present invention, a cyclic group containing an alicyclic structure is preferable.

[0170] From the viewpoint of significantly obtaining the desired effects of the present invention, the divalent cyclic group is preferably a 3-membered or larger ring, more preferably a 4-membered or larger ring, and even more preferably a 5-membered or larger ring, and is preferably a 20-membered or smaller ring, more preferably a 15-membered or smaller ring, and even more preferably a 10-membered or smaller ring. In addition, the divalent cyclic group may be a monocyclic structure or a polycyclic structure.

[0171] The ring in the divalent cyclic group may have a ring skeleton constituted by a heteroatom other than carbon atoms. Examples of the heteroatom include an oxygen atom, a sulfur atom, and a nitrogen atom, and an oxygen atom is preferred. The ring may have one or more heteroatoms.

[0172] Specific examples of the divalent cyclic group include the following divalent groups (i) to (xi). Among them, the divalent cyclic group is preferably (x) or (xi). [ka]

[0173] The divalent cyclic group may have a substituent, such as a halogen atom, an alkyl group, an alkoxy group, an aryl group, an arylalkyl group, a silyl group, an acyl group, an acyloxy group, a carboxy group, a sulfo group, a cyano group, a nitro group, a hydroxy group, a mercapto group, or an oxo group, and an alkyl group is preferred.

[0174] The (meth)acryloyl group may be directly bonded to the divalent cyclic group, or may be bonded via a divalent linking group. Examples of the divalent linking group include an alkylene group, an alkenylene group, an arylene group, a heteroarylene group, -C(=O)O-, -O-, -NHC(=O)-, -NC(=O)N-, -NHC(=O)O-, -C(=O)-, -S-, -SO-, -NH-, and the like, and may be a group in which a plurality of these are combined. The alkylene group is preferably an alkylene group having 1 to 10 carbon atoms, more preferably an alkylene group having 1 to 6 carbon atoms, and even more preferably an alkylene group having 1 to 5 carbon atoms or an alkylene group having 1 to 4 carbon atoms. The alkylene group may be linear, branched, or cyclic. Examples of such alkylene groups include methylene, ethylene, propylene, butylene, pentylene, hexylene, and 1,1-dimethylethylene groups, and are preferably methylene, ethylene, or 1,1-dimethylethylene. As the alkenylene group, an alkenylene group having 2 to 10 carbon atoms is preferred, an alkenylene group having 2 to 6 carbon atoms is more preferred, and an alkenylene group having 2 to 5 carbon atoms is even more preferred. As the arylene group or heteroarylene group, an arylene group or heteroarylene group having 6 to 20 carbon atoms is preferred, and an arylene group or heteroarylene group having 6 to 10 carbon atoms is more preferred. As the divalent linking group, an alkylene group is preferred, and among them, a methylene group or a 1,1-dimethylethylene group is preferred.

[0175] The (meth)acrylic curing agent is preferably represented by the following formula (F-11). [ka] (In formula (F-11), R 101 and R 104 each independently represents an acryloyl group or a methacryloyl group, R 102 and R 103 each independently represents a divalent linking group. Ring B2 represents a divalent cyclic group.

[0176] R 101 and R 104each independently represents an acryloyl group or a methacryloyl group, and an acryloyl group is preferred.

[0177] R 102 and R 103 each independently represents a divalent linking group. The divalent linking group is the same as the divalent linking group which may have a (meth)acryloyl group bonded thereto.

[0178] Ring B2 represents a divalent cyclic group. Ring B2 is the same as the divalent cyclic group. Ring B2 may have a substituent. The substituent is the same as the substituent that the divalent cyclic group may have.

[0179] Specific examples of the (meth)acrylic curing agent include the following, but the present invention is not limited thereto. [ka]

[0180] As the (meth)acrylic curing agent, commercially available products may be used, and examples thereof include "A-DOG" manufactured by Shin-Nakamura Chemical Co., Ltd., "DCP-A" manufactured by Kyoeisha Chemical Co., Ltd., "NPDGA", "FM-400", "R-687", "THE-330", "PET-30", and "DPHA" manufactured by Nippon Kayaku Co., Ltd., and "NK Ester DCP" manufactured by Shin-Nakamura Chemical Co., Ltd.

[0181] From the viewpoint of significantly obtaining the desired effects of the present invention, the (meth)acryloyl group equivalent of the (meth)acrylic curing agent is preferably 30 g / eq. to 400 g / eq., more preferably 50 g / eq. to 300 g / eq., and further preferably 75 g / eq. to 200 g / eq. The (meth)acryloyl group equivalent is the mass of the (meth)acrylic curing agent containing one equivalent of a (meth)acryloyl group.

[0182] An allyl-based curing agent is a compound having at least one allyl group in the molecule. Here, among phenol-based curing agents, naphthol-based curing agents, benzoxazine-based curing agents, cyanate ester-based curing agents, carbodiimide-based curing agents, amine-based curing agents, acid anhydride-based curing agents, maleimide-based curing agents, (meth)acrylic-based curing agents, polyphenylene ether-based curing agents, and styrene-based curing agents, those having an allyl group are allyl-based curing agents. The allyl-based curing agent is preferably liquid or semi-solid. The determination of liquid, semi-solid, and solid is as described above.

[0183] The allyl curing agent preferably has one or more allyl groups per molecule, and more preferably has two or more allyl groups. There is no particular lower limit, but it is preferably 10 or less, more preferably 5 or less.

[0184] In addition, from the viewpoint of obtaining the desired effects of the present invention more significantly, the allyl-based curing agent preferably has, in addition to the allyl group, any one of a benzoxazine ring, a phenol ring, an epoxy group, and a carboxylic acid derivative having a cyclic structure, and from the viewpoint of obtaining the desired effects of the present invention more significantly, it is more preferable that the allyl-based curing agent has a benzoxazine ring.

[0185] In the allyl curing agent having a benzoxazine ring, from the viewpoint of significantly obtaining the desired effects of the present invention, the allyl group is preferably bonded to either a nitrogen atom constituting the benzoxazine ring or a carbon atom constituting the benzoxazine ring, and more preferably bonded to a carbon atom.

[0186] The allyl-based curing agent having a benzoxazine ring is preferably, for example, an allyl-based curing agent having a benzoxazine ring represented by the following formula (F-12). [ka] In formula (F-12), R 20 , and R 21 represents an allyl group, and R 22represents a y-valent group, where y is an integer of 1 to 4, x1 is an integer of 0 to 4, and x2 is an integer of 0 to 2.

[0187] R in formula (F-12) 22 The y-valent group represented by R is preferably an allyl group, a y-valent aromatic hydrocarbon group, a y-valent aliphatic hydrocarbon group, an oxygen atom, or a y-valent group consisting of a combination thereof. 22 When R has an allyl group, the allyl group may be a substituent of either a y-valent aromatic hydrocarbon group or a y-valent aliphatic hydrocarbon group. For example, when y is 2, R 22 is preferably an arylene group, an alkylene group, an oxygen atom, or a group consisting of a combination of two or more of these divalent groups, more preferably an arylene group or a group consisting of a combination of two or more of these divalent groups, and even more preferably a group consisting of a combination of two or more of these divalent groups.

[0188] R in formula (F-12) 22 The arylene group in is preferably an arylene group having 6 to 20 carbon atoms, more preferably an arylene group having 6 to 15 carbon atoms, and further preferably an arylene group having 6 to 12 carbon atoms. Specific examples of the arylene group include a phenylene group, a naphthylene group, an anthracenylene group, and a biphenylene group, and the phenylene group is preferred.

[0189] R in formula (F-12) 22 The alkylene group in is preferably an alkylene group having 1 to 10 carbon atoms, more preferably an alkylene group having 1 to 6 carbon atoms, and further preferably an alkylene group having 1 to 3 carbon atoms. Specific examples of the alkylene group include a methylene group, an ethylene group, and a propylene group, and a methylene group is preferred.

[0190] R in formula (F-12) 22Examples of the group consisting of a combination of two or more types of divalent groups in the above formula include a group in which one or more arylene groups are bonded to one or more oxygen atoms; a group in which one or more arylene groups are bonded to one or more alkylene groups, such as a group having an arylene-alkylene-arylene structure; a group in which one or more alkylene groups are bonded to one or more oxygen atoms; a group in which one or more arylene groups, one or more alkylene groups, and one or more oxygen atoms are bonded to one or more oxygen atoms; and the like. Of these, a group in which one or more arylene groups are bonded to one or more oxygen atoms and a group in which one or more arylene groups are bonded to one or more alkylene groups are preferred.

[0191] In formula (F-12), y represents an integer of 1 to 4, preferably an integer of 1 to 3, and more preferably 1 or 2.

[0192] In formula (F-12), x1 represents an integer of 0 to 4, preferably an integer of 0 to 2, more preferably 0 or 1, and still more preferably 1. In formula (F-12), x2 represents an integer of 0 to 2, preferably 0 or 1, and is preferably 0.

[0193] Examples of the allyl-based curing agent having a phenol ring include a cresol resin containing an allyl group, a novolac-type phenol resin containing an allyl group, a cresol novolac resin containing an allyl group, etc. Among them, the allyl-based curing agent having a phenol ring is preferably an allyl-based curing agent having a phenol ring represented by the following formula (F-13). [ka] In formula (F-13), R 23 , R 24 , and R 25 each independently represents an allyl group, each s1 independently represents an integer of 0 to 4, each s2 independently represents an integer of 0 to 3, and r independently represents an integer of 0 to 3.

[0194] R in formula (F-13) 23 ~R 25each independently represents an allyl group. In formula (B-2), the number of allyl groups is preferably 1 or more, more preferably 2 or more, and even more preferably 3 or more, and is preferably 25 or less, more preferably 10 or less, and even more preferably 5 or less.

[0195] In formula (F-13), s1 each independently represents an integer of 0 to 4, preferably an integer of 1 to 3, and more preferably an integer of 1 to 2.

[0196] In formula (F-13), s2 each independently represents an integer of 0 to 3, preferably an integer of 1 to 3, and more preferably an integer of 1 to 2.

[0197] In formula (F-13), r represents an integer of 0 to 3, preferably an integer of 0 to 2, and more preferably an integer of 1 to 2.

[0198] The allyl curing agent having an epoxy group preferably contains two or more epoxy groups in one molecule. The allyl curing agent having an epoxy group preferably has an aromatic structure, and when two or more allyl curing agents having an epoxy group are used, it is more preferable that at least one of them has an aromatic structure. The aromatic structure is a chemical structure generally defined as aromatic, and also includes polycyclic aromatics and aromatic heterocycles. The allyl curing agent having an epoxy group preferably has a bisphenol structure, and examples of the bisphenol structure include bisphenol A type, bisphenol F type, bisphenol AF type, etc., and among them, bisphenol A type is preferable from the viewpoint of obtaining the effect of the present invention remarkably.

[0199] As the allyl-based curing agent having a carboxylic acid derivative having a cyclic structure, an allyl carboxylate having a cyclic structure is preferred. The cyclic structure may be either a cyclic group containing an alicyclic structure or a cyclic group containing an aromatic ring structure. In addition, the cyclic group may have a ring skeleton constituted by heteroatoms other than carbon atoms. Examples of heteroatoms include oxygen atoms, sulfur atoms, and nitrogen atoms, and nitrogen atoms are preferred. The ring may have one heteroatom or two or more heteroatoms. The carboxylic acid derivative having a cyclic structure has improved compatibility and dispersibility with resin varnish due to the network structure of the cyclic structure, which results in improved lamination properties and makes it possible to obtain a cured product with excellent adhesion.

[0200] Examples of carboxylic acids having a cyclic structure include isocyanuric acid, diphenic acid, phthalic acid, cyclohexanedicarboxylic acid, etc. Examples of allyl-based curing agents having a carboxylic acid derivative having a cyclic structure include allyl isocyanurate, diallyl isocyanurate, triallyl isocyanurate, diallyl diphenate, allyl diphenate, ortho-diallyl phthalate, methadiallyl phthalate, para-diallyl phthalate, allyl cyclohexanedicarboxylate, diallyl cyclohexanedicarboxylate, etc.

[0201] The allyl-based curing agent may be a commercially available product. Examples of commercially available products include "MEH-8000H" and "MEH-8005" (allyl-based curing agent having a phenol ring) manufactured by Meiwa Kasei Co., Ltd.; "RE-810NM" (allyl-based curing agent having an epoxy group) manufactured by Nippon Kayaku Co., Ltd.; "ALP-d" (allyl-based curing agent having a benzoxazine ring) manufactured by Shikoku Kasei Kogyo Co., Ltd.; "L-DAIC" (allyl-based curing agent having an isocyanuric ring) manufactured by Shikoku Kasei Kogyo Co., Ltd.; "TAIC" (allyl-based curing agent having an isocyanuric ring (triallyl isocyanurate) manufactured by Nippon Kasei Co., Ltd.; "MDAC" (allyl-based curing agent having a cyclohexanedicarboxylic acid derivative) manufactured by Osaka Soda Co., Ltd.; "DAD" (diallyl diphenate) manufactured by Nisshoku Techno Fine Chemical Co., Ltd.; and "Daiso DAP Monomer" (ortho-diallyl phthalate) manufactured by Osaka Soda Co., Ltd.

[0202] From the viewpoint of significantly obtaining the desired effects of the present invention, the allyl group equivalent of the allyl curing agent is preferably 20 g / eq. to 1000 g / eq., more preferably 50 g / eq. to 500 g / eq., and further preferably 100 g / eq. to 300 g / eq. The allyl group equivalent is the mass of the allyl curing agent containing one equivalent of an allyl group.

[0203] As the active ester curing agent other than the component (B) (hereinafter, sometimes simply referred to as "active ester curing agent"), a compound having one or more active ester groups in one molecule can be used. Among them, as the active ester curing agent, a compound having two or more highly reactive ester groups in one molecule, such as phenol esters, thiophenol esters, N-hydroxyamine esters, and esters of heterocyclic hydroxy compounds, is preferred. The active ester curing agent is preferably one obtained by a condensation reaction between a carboxylic acid compound and / or a thiocarboxylic acid compound and a hydroxy compound and / or a thiol compound. In particular, from the viewpoint of improving heat resistance, an active ester curing agent obtained from a carboxylic acid compound and a hydroxy compound is preferred, and an active ester curing agent obtained from a carboxylic acid compound and a phenol compound and / or a naphthol compound is more preferred.

[0204] Examples of the carboxylic acid compound include benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, and pyromellitic acid.

[0205] Examples of phenol compounds or naphthol compounds include hydroquinone, resorcin, bisphenol A, bisphenol F, bisphenol S, phenolphthaline, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucin, benzenetriol, dicyclopentadiene-type diphenol compounds, phenol novolac, etc. Here, the term "dicyclopentadiene-type diphenol compounds" refers to diphenol compounds obtained by condensing one molecule of dicyclopentadiene with two molecules of phenol.

[0206] Preferred specific examples of the active ester curing agent include an active ester curing agent containing a dicyclopentadiene-type diphenol structure, an active ester curing agent containing a naphthalene structure, an active ester curing agent containing an acetylated product of phenol novolac, and an active ester curing agent containing a benzoylated product of phenol novolac. Among them, an active ester curing agent containing a naphthalene structure and an active ester curing agent containing a dicyclopentadiene-type diphenol structure are more preferred. The "dicyclopentadiene-type diphenol structure" refers to a divalent structural unit consisting of phenylene-dicyclopentylene-phenylene.

[0207] Commercially available active ester curing agents include "EXB9451", "EXB9460", "EXB9460S", "HPC8000-65T", "HPC8000H-65TM", and "EXB8000L-65TM" (manufactured by DIC Corporation) as active ester curing agents containing a dicyclopentadiene-type diphenol structure; "EXB-8100L-65T", "EXB-8150L-65T", "EXB8150-65T", and "EXB9416-70BK" (manufactured by DIC Corporation) as active ester curing agents containing a naphthalene structure; and "acetone" of phenol novolac. Examples of such curing agents include "DC808" (manufactured by Mitsubishi Chemical Corporation) as an active ester-based curing agent containing an acetylated product; "YLH1026" (manufactured by Mitsubishi Chemical Corporation) as an active ester-based curing agent containing a benzoylated product of phenol novolac; "DC808" (manufactured by Mitsubishi Chemical Corporation) as an active ester-based curing agent which is an acetylated product of phenol novolac; and "YLH1026" (manufactured by Mitsubishi Chemical Corporation), "YLH1030" (manufactured by Mitsubishi Chemical Corporation), and "YLH1048" (manufactured by Mitsubishi Chemical Corporation) as active ester-based curing agents which are benzoylated products of phenol novolac.

[0208] The ratio of the amount of the (A) component to the (F) component is the ratio of [total number of epoxy groups in the (A) component]:[total number of reactive groups in the (F) component], and is preferably in the range of 1:0.01 to 1:10, more preferably 1:0.03 to 1:5, and even more preferably 1:0.05 to 1:1. Here, the "number of epoxy groups in the (A) component" refers to the total value obtained by dividing the mass of the non-volatile component of the (A) component present in the resin composition by the epoxy equivalent. In addition, the "number of active groups in the (F) component" refers to the total value obtained by dividing the mass of the non-volatile component of the (F) component present in the resin composition by the active group equivalent. By setting the ratio of the amount of the (A) component to the (F) component within this range, the occurrence of unevenness in the cured substrate can be further suppressed.

[0209] From the viewpoint of significantly obtaining the desired effects of the present invention, the content of the (F) component is preferably 0.1 mass% or more, more preferably 0.3 mass% or more, and even more preferably 0.5 mass% or more, relative to 100 mass% of the non-volatile components in the resin composition, and is preferably 20 mass% or less, more preferably 15 mass% or less, and even more preferably 10 mass% or less.

[0210] <(G) Other Additives> The resin composition may further contain other additives as optional components in addition to the above-mentioned components. Examples of such additives include resin additives such as thickeners, defoamers, leveling agents, and adhesion promoters. These additives may be used alone or in combination of two or more. The content of each additive can be appropriately set by a person skilled in the art.

[0211] The method for preparing the resin composition of the present invention is not particularly limited, and examples thereof include a method in which the blending components are mixed and dispersed using a rotary mixer or the like, with the addition of a solvent or the like as necessary.

[0212] <Physical properties and applications of resin compositions> The resin composition contains the (A) component, a predetermined amount of the (B) component, and a predetermined amount of the (C) component. This makes it possible to suppress unevenness on the cured substrate and obtain a cured product with excellent dielectric properties. Usually, when the content of (C) is increased, unevenness on the cured substrate tends to occur easily. However, by incorporating a predetermined amount of the (B) component in combination, it becomes possible to suppress the occurrence of unevenness on the cured substrate even if the content of the (C) component is high. Furthermore, in addition to the dielectric properties, it is usually possible to obtain a cured product with excellent peel strength.

[0213] The resin composition exhibits the characteristic of being able to suppress unevenness occurring on the cured substrate. Specifically, a resin composition layer of a resin sheet is laminated on a glass cloth-based epoxy resin double-sided copper-clad laminate having a copper foil thickness of 18 μm, and then heat-cured at 130° C. for 30 minutes and then at 170° C. for 30 minutes to form an insulating layer. The insulating layer in the portion where the resin sheet is laminated is visually observed, and the surface uniformity of the surface opposite to the glass cloth-based epoxy resin double-sided copper-clad laminate is observed. At this time, the portion inside the portion 1 cm from the outer periphery of the portion where the resin sheet is laminated is usually a uniform surface. Preferably, the entire surface of the insulating layer opposite to the laminate is a uniform surface. Details of the evaluation of unevenness of the cured substrate can be measured according to the method described in the examples described below.

[0214] The cured product obtained by thermally curing the resin composition at 200°C for 90 minutes exhibits the characteristic of a low dielectric constant. Thus, the cured product provides an insulating layer with a low dielectric constant. The dielectric constant is preferably 4 or less, more preferably 3.5 or less, and even more preferably 3 or less. The lower limit of the dielectric constant may be 0.001 or more. The dielectric constant can be measured according to the method described in the examples below.

[0215] The cured product obtained by thermally curing the resin composition at 200°C for 90 minutes exhibits the characteristic of a low dielectric loss tangent. Thus, the cured product provides an insulating layer with a low dielectric loss tangent. The dielectric loss tangent is preferably 0.01 or less, more preferably 0.008 or less, and even more preferably 0.005 or less. The lower limit of the dielectric loss tangent may be 0.0001 or more. The dielectric loss tangent can be measured according to the method described in the examples below.

[0216] A cured product obtained by thermally curing a resin composition at 130°C for 30 minutes and then at 170°C for 30 minutes usually exhibits the property of excellent peel strength between the resin composition and a conductor layer (plated conductor layer) formed by plating. Thus, the cured product provides an insulating layer with excellent peel strength between the resin composition and the plated conductor layer. The peel strength is preferably 0.3 kgf / cm or more, more preferably 0.35 kgf / cm or more, and even more preferably 0.4 kgf / cm or more. The upper limit of the peel strength may be 10 kgf / cm or less. The peel strength of the plated conductor layer can be measured according to the method described in the examples below.

[0217] The resin composition of the present invention can suppress unevenness occurring on the cured substrate, and can provide an insulating layer having excellent dielectric properties and peel strength. Therefore, the resin composition of the present invention can be suitably used as a resin composition for insulating purposes. Specifically, it can be suitably used as a resin composition for forming an insulating layer (resin composition for forming an insulating layer) for forming a conductor layer (including a rewiring layer) formed on the insulating layer.

[0218] Furthermore, in the multilayer printed wiring board described below, the resin composition can be suitably used as a resin composition for forming an insulating layer of a multilayer printed wiring board (resin composition for forming an insulating layer of a multilayer printed wiring board) and a resin composition for forming an interlayer insulating layer of a printed wiring board (resin composition for forming an interlayer insulating layer of a printed wiring board).

[0219] In addition, for example, when a semiconductor chip package is manufactured through the following steps (1) to (6), the resin composition of the present invention can be suitably used as a resin composition for a rewiring formation layer (resin composition for forming a rewiring formation layer) as an insulating layer for forming a rewiring layer, and as a resin composition for sealing a semiconductor chip (resin composition for sealing a semiconductor chip). When a semiconductor chip package is manufactured, a rewiring layer may be further formed on the sealing layer. (1) A step of laminating a temporary fixing film onto a substrate; (2) a step of temporarily fixing a semiconductor chip on a temporary fixing film; (3) forming an encapsulation layer on the semiconductor chip; (4) peeling the substrate and the temporary fixing film from the semiconductor chip; (5) forming a rewiring formation layer as an insulating layer on the surface of the semiconductor chip from which the base material and the temporary fixing film have been peeled off; and (6) A process of forming a rewiring layer as a conductor layer on the rewiring formation layer.

[0220] [Resin sheet] The resin sheet of the present invention includes a support and a resin composition layer formed from the resin composition of the present invention provided on the support.

[0221] The thickness of the resin composition layer is preferably 50 μm or less, more preferably 40 μm or less, and even more preferably 30 μm or less, from the viewpoint of making the printed wiring board thinner and being able to provide a cured product with excellent insulation even if the cured product of the resin composition is a thin film. The lower limit of the thickness of the resin composition layer is not particularly limited, but can usually be 5 μm or more.

[0222] Examples of the support include films made of plastic materials, metal foils, and release papers, with films made of plastic materials and metal foils being preferred.

[0223] When a film made of a plastic material is used as the support, examples of the plastic material include polyesters such as polyethylene terephthalate (hereinafter sometimes abbreviated as "PET") and polyethylene naphthalate (hereinafter sometimes abbreviated as "PEN"), polycarbonate (hereinafter sometimes abbreviated as "PC"), acrylics such as polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), polyether sulfide (PES), polyether ketone, polyimide, etc. Among these, polyethylene terephthalate and polyethylene naphthalate are preferred, and inexpensive polyethylene terephthalate is particularly preferred.

[0224] When a metal foil is used as the support, examples of the metal foil include copper foil, aluminum foil, etc., and copper foil is preferred. As the copper foil, a foil made of a single metal, copper, or an alloy of copper and another metal (e.g., tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.) may be used.

[0225] The surface of the support to be bonded to the resin composition layer may be subjected to a matte treatment, a corona treatment, or an antistatic treatment.

[0226] In addition, as the support, a support with a release layer having a release layer on the surface to be bonded to the resin composition layer may be used. The release agent used in the release layer of the support with a release layer may be, for example, one or more release agents selected from the group consisting of alkyd resins, polyolefin resins, urethane resins, and silicone resins. The support with a release layer may be a commercially available product, for example, "SK-1", "AL-5", and "AL-7" manufactured by Lintec Corporation, "Lumirror T60" manufactured by Toray Industries, Inc., "Purex" manufactured by Teijin Limited, and "Unipeel" manufactured by Unitika Limited, which are PET films having a release layer mainly composed of an alkyd resin-based release agent.

[0227] The thickness of the support is not particularly limited, but is preferably in the range of 5 μm to 75 μm, and more preferably in the range of 10 μm to 60 μm. When a support with a release layer is used, it is preferable that the total thickness of the support with a release layer is in the above range.

[0228] In one embodiment, the resin sheet may further include other layers as necessary. Examples of such other layers include a protective film equivalent to the support provided on the surface of the resin composition layer that is not bonded to the support (i.e., the surface opposite to the support). The thickness of the protective film is not particularly limited, but is, for example, 1 μm to 40 μm. By laminating the protective film, adhesion of dirt and the like to the surface of the resin composition layer and scratches can be suppressed.

[0229] The resin sheet can be produced, for example, by preparing a resin varnish by dissolving a resin composition in an organic solvent, applying this resin varnish onto a support using a die coater or the like, and then drying the same to form a resin composition layer.

[0230] Examples of organic solvents include ketones such as acetone, methyl ethyl ketone (MEK), and cyclohexanone; acetates such as ethyl acetate, butyl acetate, cellosolve acetate, propylene glycol monomethyl ether acetate, and carbitol acetate; carbitols such as cellosolve and butyl carbitol; aromatic hydrocarbons such as toluene and xylene; and amide solvents such as dimethylformamide, dimethylacetamide (DMAc), and N-methylpyrrolidone. The organic solvents may be used alone or in combination of two or more.

[0231] Drying may be performed by a known method such as heating or hot air blowing. Drying conditions are not particularly limited, but drying is performed so that the content of organic solvent in the resin composition layer becomes 10 mass % or less, preferably 5 mass % or less. Although it varies depending on the boiling point of the organic solvent in the resin varnish, for example, when a resin varnish containing 30 mass % to 60 mass % of organic solvent is used, the resin composition layer can be formed by drying at 50°C to 150°C for 3 minutes to 10 minutes.

[0232] The resin sheet can be stored in a rolled state. When the resin sheet has a protective film, it can be used by peeling off the protective film.

[0233] [Printed wiring board] The printed wiring board of the present invention includes an insulating layer formed from a cured product of the resin composition of the present invention.

[0234] The printed wiring board can be produced, for example, by using the above-mentioned resin sheet by a method including the following steps (I) and (II). (I) A step of laminating a resin sheet on an inner layer substrate so that a resin composition layer of the resin sheet is bonded to the inner layer substrate. (II) A step of thermally curing the resin composition layer to form an insulating layer

[0235] The "inner layer substrate" used in step (I) is a member that becomes the substrate of a printed wiring board, and examples thereof include a glass epoxy substrate, a metal substrate, a polyester substrate, a polyimide substrate, a BT resin substrate, and a thermosetting polyphenylene ether substrate. The substrate may have a conductor layer on one or both sides, and the conductor layer may be patterned. An inner layer substrate having a conductor layer (circuit) formed on one or both sides of the substrate may be called an "inner layer circuit substrate". In addition, an intermediate product on which an insulating layer and / or a conductor layer is to be further formed during the manufacture of a printed wiring board is also included in the "inner layer substrate" of the present invention. When the printed wiring board is a circuit board with built-in components, an inner layer substrate with built-in components may be used.

[0236] The lamination of the inner layer substrate and the resin sheet can be carried out, for example, by thermocompression bonding the resin sheet to the inner layer substrate from the support side. Examples of the member for thermocompression bonding the resin sheet to the inner layer substrate (hereinafter also referred to as the "thermocompression bonding member") include a heated metal plate (such as a SUS plate) or a metal roll (SUS roll). It is preferable to press the thermocompression member not directly onto the resin sheet, but via an elastic material such as heat-resistant rubber so that the resin sheet can sufficiently follow the surface irregularities of the inner layer substrate.

[0237] The lamination of the inner layer substrate and the resin sheet may be performed by a vacuum lamination method. In the vacuum lamination method, the thermocompression temperature is preferably in the range of 60°C to 160°C, more preferably in the range of 80°C to 140°C, the thermocompression pressure is preferably in the range of 0.098MPa to 1.77MPa, more preferably in the range of 0.29MPa to 1.47MPa, and the thermocompression time is preferably in the range of 20 seconds to 400 seconds, more preferably in the range of 30 seconds to 300 seconds. The lamination is preferably performed under reduced pressure conditions of 26.7hPa or less.

[0238] The lamination can be performed by a commercially available vacuum laminator, such as a vacuum pressure laminator manufactured by Meiki Seisakusho Co., Ltd., a vacuum applicator manufactured by Nikko Materials Co., Ltd., or a batch type vacuum pressure laminator.

[0239] After lamination, the laminated resin sheet may be smoothed under normal pressure (atmospheric pressure), for example, by pressing a thermocompression member from the support side. The pressing conditions for the smoothing treatment may be the same as the thermocompression conditions for the lamination. The smoothing treatment may be performed using a commercially available laminator. The lamination and smoothing treatment may be performed consecutively using the commercially available vacuum laminator.

[0240] The support may be removed between step (I) and step (II) or after step (II).

[0241] In step (II), the resin composition layer is thermally cured to form an insulating layer. The conditions for thermally curing the resin composition layer are not particularly limited, and conditions that are usually employed when forming an insulating layer for a printed wiring board may be used.

[0242] For example, the thermal curing conditions for the resin composition layer vary depending on the type of resin composition, etc., but the curing temperature is preferably 120° C. to 240° C., more preferably 150° C. to 220° C., and even more preferably 170° C. to 210° C. The curing time is preferably 5 minutes to 120 minutes, more preferably 10 minutes to 100 minutes, and even more preferably 15 minutes to 100 minutes.

[0243] Before the resin composition layer is thermally cured, the resin composition layer may be preheated at a temperature lower than the curing temperature. For example, prior to thermally curing the resin composition layer, the resin composition layer may be preheated at a temperature of 50° C. or more and less than 120° C. (preferably 60° C. or more and 115° C. or less, more preferably 70° C. or more and 110° C. or less) for 5 minutes or more (preferably 5 minutes to 150 minutes, more preferably 15 minutes to 120 minutes, and even more preferably 15 minutes to 100 minutes).

[0244] In manufacturing a printed wiring board, the steps of (III) drilling holes in the insulating layer, (IV) roughening the insulating layer, and (V) forming a conductor layer may be further carried out. These steps (III) to (V) may be carried out according to various methods known to those skilled in the art for use in manufacturing printed wiring boards. When the support is removed after step (II), the support may be removed between step (II) and step (III), between step (III) and step (IV), or between step (IV) and step (V). In addition, the formation of the insulating layer and the conductor layer in steps (II) to (V) may be repeated to form a multilayer wiring board, as necessary.

[0245] Step (III) is a step of drilling holes in the insulating layer, which allows holes such as via holes and through holes to be formed in the insulating layer. Step (III) may be performed using, for example, a drill, a laser, plasma, etc., depending on the composition of the resin composition used to form the insulating layer. The dimensions and shape of the holes may be appropriately determined depending on the design of the printed wiring board.

[0246] Step (IV) is a step of roughening the insulating layer. Usually, in this step (IV), smears are also removed. The procedure and conditions of the roughening treatment are not particularly limited, and known procedures and conditions that are usually used when forming an insulating layer of a printed wiring board can be adopted. For example, the insulating layer can be roughened by performing a swelling treatment with a swelling liquid, a roughening treatment with an oxidizing agent, and a neutralization treatment with a neutralizing liquid in this order. The swelling liquid used for the roughening treatment is not particularly limited, but includes an alkaline solution, a surfactant solution, and the like, and is preferably an alkaline solution, and as the alkaline solution, a sodium hydroxide solution and a potassium hydroxide solution are more preferable. Examples of commercially available swelling liquids include "Swelling Dip Securigans P", "Swelling Dip Securigans SBU", and "Swelling Dip Securigant P" manufactured by Atotech Japan. The swelling treatment using a swelling liquid is not particularly limited, but can be performed, for example, by immersing the insulating layer in a swelling liquid at 30°C to 90°C for 1 to 20 minutes. From the viewpoint of suppressing the swelling of the resin of the insulating layer to an appropriate level, it is preferable to immerse the insulating layer in a swelling liquid at 40°C to 80°C for 5 to 15 minutes. The oxidizing agent used in the roughening treatment is not particularly limited, but examples thereof include an alkaline permanganate solution in which potassium permanganate or sodium permanganate is dissolved in an aqueous solution of sodium hydroxide. The roughening treatment using an oxidizing agent such as an alkaline permanganate solution is preferably performed by immersing the insulating layer in an oxidizing agent solution heated to 60°C to 100°C for 10 to 30 minutes. In addition, the concentration of permanganate in the alkaline permanganate solution is preferably 5% by mass to 10% by mass. Examples of commercially available oxidizing agents include alkaline permanganate solutions such as "Concentrate Compact CP" and "Dosing Solution Securiganth P" manufactured by Atotech Japan. The neutralizing solution used in the roughening treatment is preferably an acidic aqueous solution, and a commercially available product is, for example, "Reduction Solution Securiganth P" manufactured by Atotech Japan. Treatment with a neutralizing solution can be performed by immersing the surface that has been roughened with an oxidizing agent in the neutralizing solution at 30°C to 80°C for 1 to 30 minutes.From the viewpoint of workability etc., a method in which the object that has been subjected to roughening treatment with an oxidizing agent is immersed in a neutralizing solution at 40° C. to 70° C. for 5 minutes to 20 minutes is preferred.

[0247] In one embodiment, the arithmetic mean roughness (Ra) of the insulating layer surface after the roughening treatment is preferably 300 nm or less, more preferably 250 nm or less, and even more preferably 200 nm or less. There is no particular limit to the lower limit, but it is preferably 30 nm or more, more preferably 40 nm or more, and even more preferably 50 nm or more. The arithmetic mean roughness (Ra) of the insulating layer surface can be measured using a non-contact surface roughness meter.

[0248] Step (V) is a step of forming a conductor layer, and the conductor layer is formed on the insulating layer. The conductor material used for the conductor layer is not particularly limited. In a preferred embodiment, the conductor layer contains one or more metals selected from the group consisting of gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin and indium. The conductor layer may be a single metal layer or an alloy layer, and examples of the alloy layer include layers formed from alloys of two or more metals selected from the above group (e.g., nickel-chromium alloy, copper-nickel alloy and copper-titanium alloy). Among these, from the viewpoints of versatility in forming the conductor layer, cost, ease of patterning, and the like, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper, or an alloy layer of a nickel-chromium alloy, a copper-nickel alloy, or a copper-titanium alloy is preferred, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper, or an alloy layer of a nickel-chromium alloy is more preferred, and a single metal layer of copper is even more preferred.

[0249] The conductor layer may be a single-layer structure or a multi-layer structure in which two or more single metal layers or alloy layers made of different kinds of metals or alloys are laminated. When the conductor layer has a multi-layer structure, the layer in contact with the insulating layer is preferably a single metal layer of chromium, zinc or titanium, or an alloy layer of a nickel-chromium alloy.

[0250] The thickness of the conductor layer depends on the desired design of the printed wiring board, but is generally 3 μm to 35 μm, and preferably 5 μm to 30 μm.

[0251] In one embodiment, the conductor layer may be formed by plating. For example, a conductor layer having a desired wiring pattern can be formed by plating the surface of the insulating layer by a conventionally known technique such as a semi-additive method or a full-additive method, and from the viewpoint of ease of production, it is preferable to form the conductor layer by the semi-additive method. An example of forming the conductor layer by the semi-additive method will be described below.

[0252] First, a plating seed layer is formed on the surface of an insulating layer by electroless plating. Next, a mask pattern is formed on the formed plating seed layer to expose a part of the plating seed layer corresponding to a desired wiring pattern. After a metal layer is formed on the exposed plating seed layer by electrolytic plating, the mask pattern is removed. Thereafter, unnecessary plating seed layer is removed by etching or the like to form a conductor layer having a desired wiring pattern.

[0253] [Semiconductor Devices] The semiconductor device of the present invention includes the printed wiring board of the present invention. The semiconductor device of the present invention can be manufactured by using the printed wiring board of the present invention.

[0254] Examples of the semiconductor device include various semiconductor devices used in electric appliances (for example, computers, mobile phones, digital cameras, and televisions) and vehicles (for example, motorcycles, automobiles, trains, ships, and aircraft).

[0255] The semiconductor device of the present invention can be manufactured by mounting a component (semiconductor chip) on a conductive portion of a printed wiring board. The "conductive portion" refers to a portion of a printed wiring board that transmits an electric signal, and the portion may be either on the surface or embedded. The semiconductor chip is not particularly limited as long as it is an electric circuit element made of semiconductor material.

[0256] The method of mounting a semiconductor chip when manufacturing a semiconductor device is not particularly limited as long as the semiconductor chip functions effectively, but specific examples include a wire bonding mounting method, a flip chip mounting method, a bumpless buildup layer (BBUL) mounting method, an anisotropic conductive film (ACF) mounting method, a non-conductive film (NCF) mounting method, etc. Here, the "bumpless buildup layer (BBUL) mounting method" refers to "a mounting method in which a semiconductor chip is directly embedded in a recess in a printed wiring board and the semiconductor chip is connected to the wiring on the printed wiring board." EXAMPLES

[0257] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples. In the following description, unless otherwise specified, "parts" and "%" mean "parts by mass" and "% by mass", respectively. It should be noted that Examples 1 and 3 to 9 are reference examples.

[0258] [Example 1. Preparation of resin composition 1] 10 parts of bixylenol type epoxy resin ("YX4000H" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent of about 185 g / eq.) and 20 parts of fluorine-containing epoxy resin ("YX7760" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent of about 236 g / eq.) were dissolved in 20 parts of toluene and 20 parts of MEK while stirring. The resulting solution was cooled to room temperature, and then 50 parts of an active ester type curing agent represented by general formula (B) ("EXB8500-65T" manufactured by DIC Corporation, active group equivalent of 223 g / eq., toluene solution with solid content of 65% by mass), 4 parts of a triazine skeleton-containing phenol type curing agent ("LA-3018-50P" manufactured by DIC Corporation, hydroxyl group equivalent of about 151 g / eq., 2-methoxypropanol solution with solid content of 50%), 10 parts of a phenoxy resin ("YX7760" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent of about 236 g / eq.) and 20 parts of toluene were dissolved in 20 parts of MEK while stirring. The resulting solution was cooled to room temperature, and then 50 parts of an active ester type curing agent represented by general formula (B) ("EXB8500-65T" manufactured by DIC Corporation, active group equivalent of 223 g / eq., toluene solution with solid content of 65% by mass), 10 parts of a phenoxy resin ("LA-3018-50P" manufactured by DIC Corporation, hydroxyl group equivalent of about 151 g / eq., 2-methoxypropanol solution with solid content of 50%) were dissolved in 20 parts of toluene and 20 parts of MEK. 10 parts of "YX7200B35", MEK solution with 35% solids by mass), 1 part of curing accelerator (MEK solution with 10% solids by mass of 4-dimethylaminopyridine (DMAP)), and 160 parts of inorganic filler (spherical silica (Admatechs' SO-C2, average particle size 0.5 μm) surface-treated with an amine-based silane coupling agent (Shin-Etsu Chemical's KBM573)) were mixed and uniformly dispersed in a high-speed rotating mixer to obtain resin composition 1.

[0259] [Example 2. Preparation of resin composition 2] In Example 1, the amount of the active ester-based curing agent represented by the general formula (B) (DIC Corporation's "EXB8500-65T", active group equivalent 223 g / eq., toluene solution with a solid content of 65% by mass) was changed from 50 parts to 100 parts, and 4 parts of the triazine skeleton-containing phenol-based curing agent (DIC Corporation's "LA-3018-50P", hydroxyl group equivalent approximately 151 g / eq., 2-methoxypropanol solution with a solid content of 50%) was changed to 8 parts of the carbodiimide-based resin (Nisshinbo Chemical Corporation's "V-03", active group equivalent approximately 216, toluene solution with a solid content of 50% by mass). Resin composition 2 was obtained in the same manner as in Example 1 except for the above items.

[0260] [Example 3. Preparation of resin composition 3] In Example 1, 1) The amount of inorganic filler (spherical silica (Admatechs' "SO-C2", average particle size 0.5 μm) surface-treated with an amine-based silane coupling agent (Shin-Etsu Chemical's "KBM573")) was changed from 160 parts to 120 parts. 2) The amount of phenoxy resin (Mitsubishi Chemical Corporation's "YX7200B35", MEK solution with a solid content of 35% by mass) was changed from 10 parts to 4 parts. 3) 4 parts of a triazine skeleton-containing phenolic hardener (DIC Corporation's "LA-3018-50P", hydroxyl equivalent of approximately 151 g / eq., 2-methoxypropanol solution with 50% solids) was replaced with 20 parts of an oligophenylene ether-styrene resin (Mitsubishi Gas Chemical Company's "OPE-2St 1200", toluene solution with 65% solids). Resin composition 3 was obtained in the same manner as in Example 1 except for the above.

[0261] [Example 4. Preparation of resin composition 4] In Example 1, the amount of phenoxy resin (Mitsubishi Chemical Corporation's "YX7200B35", MEK solution with 35% solids) was changed from 10 parts to 4 parts, and 4 parts of triazine skeleton-containing phenolic curing agent (DIC Corporation's "LA-3018-50P", hydroxyl equivalent of about 151 g / eq., 2-methoxypropanol solution with 50% solids) were changed to 4 parts of liquid bismaleimide (Designer Molecules' "BMI689", maleimide equivalent of 345 g / eq.). Resin composition 4 was obtained in the same manner as in Example 1 except for the above.

[0262] [Example 5. Preparation of resin composition 5] In Example 1, 160 parts of an inorganic filler (spherical silica ("SO-C2" manufactured by Admatechs, average particle size 0.5 μm) surface-treated with an amine-based silane coupling agent ("KBM573" manufactured by Shin-Etsu Chemical Co., Ltd.)) was mixed with spherical silica (average particle size 0.3 μm, specific surface area 30.7 m) surface-treated with a phenylaminosilane-based coupling agent ("KBM573" manufactured by Shin-Etsu Chemical Co., Ltd.). 2 / g, and "UFP-30" manufactured by Denka Co., Ltd.) was changed to 120 parts. Resin composition 5 was obtained in the same manner as in Example 1 except for the above-mentioned points.

[0263] [Example 6. Preparation of resin composition 6] In Example 5, 4 parts of the triazine skeleton-containing phenol-based curing agent (DIC Corporation's "LA-3018-50P", hydroxyl equivalent of about 151 g / eq., 2-methoxypropanol solution with a solid content of 50%) was changed to 10 parts of a bifunctional acrylate ((meth)acrylic curing agent, Shin-Nakamura Chemical Co., Ltd.'s "NK Ester A-DOG", molecular weight 326). Resin composition 6 was obtained in the same manner as in Example 5 except for the above.

[0264] [Example 7. Preparation of resin composition 7] In Example 5, 4 parts of the triazine skeleton-containing phenol-based curing agent (DIC Corporation's "LA-3018-50P", hydroxyl equivalent of about 151 g / eq., 2-methoxypropanol solution with 50% solids) were changed to 2 parts of a benzoxazine-based curing agent (JFE Chemical Corporation's "ODA-BOZ"). Resin composition 7 was obtained in the same manner as in Example 5 except for the above.

[0265] [Example 8. Preparation of resin composition 8] In Example 1, 4 parts of a triazine skeleton-containing phenolic curing agent (DIC Corporation's "LA-3018-50P", hydroxyl equivalent of about 151 g / eq., 2-methoxypropanol solution with a solid content of 50%) was not used. Resin composition 8 was obtained in the same manner as in Example 1 except for the above points.

[0266] [Example 9. Preparation of resin composition 9] In Example 5, 4 parts of a triazine skeleton-containing phenolic curing agent (DIC Corporation's "LA-3018-50P", hydroxyl equivalent of about 151 g / eq., 2-methoxypropanol solution with a solid content of 50%) was not used. Resin composition 9 was obtained in the same manner as in Example 5 except for the above points.

[0267] [Comparative Example 1. Preparation of Comparative Resin Composition 1] In Example 1, 50 parts of the active ester curing agent represented by general formula (B) (DIC Corporation's "EXB-8500-65T", active group equivalent 223 g / eq., toluene solution with solid content of 65% by mass) was changed to 46.4 parts of an active ester curing agent containing a naphthalene structure (DIC Corporation's "EXB9416-70BK", active group equivalent approximately 330 g / eq., methyl isobutyl ketone solution with non-volatile content of 70% by mass). Comparative resin composition 1 was obtained in the same manner as in Example 1 except for the above.

[0268] [Comparative Example 2. Preparation of Comparative Resin Composition 2] In Example 1, the amount of the active ester curing agent represented by general formula (B) (DIC Corporation's "EXB-8500-65T", active group equivalent 223 g / eq., toluene solution with solid content of 65% by mass) was changed from 50 parts to 200 parts, and the amount of the inorganic filler (spherical silica (Admatechs Corporation's "SO-C2", average particle size 0.5 μm) surface-treated with an amine-based silane coupling agent (Shin-Etsu Chemical Co., Ltd.'s "KBM573")) was changed from 160 parts to 250 parts. Comparative resin composition 2 was obtained in the same manner as in Example 1 except for the above.

[0269] [Preparation of resin sheet] As a support, a polyethylene terephthalate film ("Lumirror R80" manufactured by Toray Industries, Inc., thickness 38 μm, softening point 130° C.) that had been subjected to a release treatment with an alkyd resin-based release agent ("AL-5" manufactured by Lintec Corporation) was prepared.

[0270] Resin compositions 1 to 9 and comparative resin compositions 1 and 2 were each uniformly applied to a support by a die coater so that the thickness of the resin composition layer after drying was 30 μm, and dried at 70° C. to 95° C. for 3 minutes to form a resin composition layer on the support. Next, a rough surface of a polypropylene film (Oji F-Tex Co., Ltd. "Alphan MA-411", thickness 15 μm) was attached as a protective film to the surface of the resin composition layer that was not bonded to the support. This resulted in a resin sheet A having a support, a resin composition layer, and a protective film in this order.

[0271] [Evaluation of unevenness on cured substrates, measurement of peel strength of plated conductor layer] (1) Preparation of inner layer board Both sides of a glass cloth-based epoxy resin double-sided copper-clad laminate (copper foil thickness 18 μm, substrate thickness 0.4 mm, Panasonic "R1515A") with an inner layer circuit formed were etched 1 μm with a microetching agent (Mec "CZ8101") to roughen the copper surface.

[0272] (2) Lamination of resin sheet The protective film was peeled off from the resin sheet A to expose the resin composition layer. Using a batch-type vacuum pressure laminator (Nikko Materials Co., Ltd., 2-stage build-up laminator "CVP700"), the resin composition layer was laminated on both sides of the inner layer substrate so that it was in contact with the inner layer substrate. The lamination was performed by reducing the pressure for 30 seconds to adjust the air pressure to 13 hPa or less, and then pressing at 120°C and a pressure of 0.74 MPa for 30 seconds. Next, a heat press was performed at 100°C and a pressure of 0.5 MPa for 60 seconds.

[0273] (3) Thermal curing of the resin composition layer Thereafter, the inner layer substrate laminated with the resin sheet was placed in an oven at 130°C and heated for 30 minutes, and then transferred to an oven at 170°C and heated for 30 minutes to thermally cure the resin composition layer and form an insulating layer. Thereafter, the support was peeled off to obtain a cured substrate A having the insulating layer, the inner layer substrate, and the insulating layer in this order.

[0274] <Evaluation of unevenness on cured substrate> For both sides of the cured substrate A, the surface uniformity of the area where the resin sheet was laminated was visually observed and evaluated as follows. ⊚: No unevenness was observed at all, and the surface was completely uniform. ◯: Unevenness was observed only in the area 1 cm from the outer periphery of the part where the resin sheet was laminated, and the area inside this had a completely uniform surface. ×: Uneven areas were observed in the area 1 cm inside from the outer periphery of the area where the resin sheet was laminated.

[0275] (4) Roughening treatment A desmear treatment was carried out as a roughening treatment on the cured substrate A. The desmear treatment was the following wet desmear treatment. (Wet desmear treatment) The cured substrate A was immersed in a swelling liquid (Atotech Japan's "Swelling Dip Securigant P", an aqueous solution of diethylene glycol monobutyl ether and sodium hydroxide) at 60°C for 5 minutes, then immersed in an oxidizing agent solution (Atotech Japan's "Concentrate Compact CP", an aqueous solution of potassium permanganate at approximately 6% and sodium hydroxide at approximately 4%) at 80°C for 15 minutes, and then immersed in a neutralizing liquid (Atotech Japan's "Reduction Solution Securigant P", an aqueous sulfuric acid solution) at 40°C for 5 minutes, and then dried at 80°C for 15 minutes.

[0276] (5) Formation of the conductor layer A conductor layer was formed on the roughened surface of the insulating layer according to the semi-additive method. That is, the substrate after the roughening treatment was immersed in an electroless plating solution containing PdCl2 at 40°C for 5 minutes, and then immersed in an electroless copper plating solution at 25°C for 20 minutes. Next, an annealing treatment was performed by heating at 150°C for 30 minutes, and then an etching resist was formed and a pattern was formed by etching. Then, copper sulfate electrolytic plating was performed to form a conductor layer with a thickness of 30 μm, and an annealing treatment was performed at 200°C for 60 minutes. The obtained substrate is called "evaluation substrate B".

[0277] <Measurement of peel strength of plated conductor layer> The peel strength of the insulating layer and the conductor layer was measured in accordance with the Japanese Industrial Standard (JIS C6481). Specifically, a cut was made in the conductor layer of evaluation board B, measuring 10 mm wide and 100 mm long, and one end of the cut was peeled off and held with a gripper. The load (kgf / cm) was measured when 35 mm was peeled off vertically at a speed of 50 mm / min at room temperature, and the peel strength was calculated. A tensile tester (TSE's "AC-50C-SL") was used for the measurement.

[0278] [Measurement of dielectric properties (dielectric constant, dielectric tangent)] The protective film was peeled off from the resin sheets prepared in the examples and comparative examples, and the resin composition layer was thermally cured by heating at 200°C for 90 minutes, and then the support was peeled off. The obtained cured product was referred to as "evaluation cured product C". The evaluation cured product C was cut into a test piece having a width of 2 mm and a length of 80 mm. The dielectric constant and dielectric loss tangent of the test piece were measured at a measurement frequency of 5.8 GHz and a measurement temperature of 23°C by a cavity resonance perturbation method using an Agilent Technologies "HP8362B". Measurements were performed on three test pieces, and the average value was calculated.

[0279] [Table 1] *In the table, "content of component (A)" indicates the content of component (A) when the nonvolatile components in the resin composition are 100% by mass, "content of component (B)" indicates the content of component (B) when the nonvolatile components in the resin composition are 100% by mass, and "content of component (C)" indicates the content of component (C) when the nonvolatile components in the resin composition are 100% by mass. C ) represents the content of the ingredient.

[0280] In Examples 1 to 9, it was confirmed that even when components (D) to (F) were not contained, the results were similar to those of the above Examples, although to a different extent.

Claims

1. (A) an epoxy resin, (B) an active ester-based curing agent having a structural unit represented by the following general formula (1) and a structural unit represented by the following general formula (2): (C) an inorganic filler, and (F) a resin composition containing a curing agent (excluding those corresponding to component (B)), The component (F) contains a carbodiimide-based curing agent, The content of the (B) component is 30% by mass or less, based on 100% by mass of the non-volatile components in the resin composition; The content of the component (C) is 60% by mass or more, based on 100% by mass of the non-volatile components in the resin composition; A resin composition, wherein the content of the (F) component is 0.1 mass% or more, relative to 100 mass% of nonvolatile components in the resin composition. [Formula 1] (In general formula (1), R 11 each independently represents an optionally substituted aliphatic hydrocarbon group, an optionally substituted aryl group, or an optionally substituted aralkyl group, Z represents an optionally substituted isophthaloyl group, or an optionally substituted naphthalenedicarbonyl group, and n1 represents an integer of 1 to 3. In general formula (2), R 12 each independently represents an aliphatic hydrocarbon group which may have a substituent, an aryl group which may have a substituent, or an aralkyl group which may have a substituent. n2 represents an integer from 1 to 3. The bond represented by * in the structural unit represented by general formula (1) is bonded to the bond represented by * in the structural unit represented by general formula (2), and the structural unit represented by general formula (1) and the structural unit represented by general formula (2) are the molecular structure of a phenol resin.

2. R in general formula (1) 11 and R in general formula (2) 12 The resin composition according to claim 1 , wherein each independently represents an aliphatic hydrocarbon group which may have a substituent.

3. The resin composition according to claim 1 or 2, wherein the aliphatic hydrocarbon group represents an alkyl group having a branched structure.

4. The resin composition according to any one of claims 1 to 3, wherein the content of the (B) component when the nonvolatile components in the resin composition are 100% by mass is b, and the content of the (C) component when the nonvolatile components in the resin composition are 100% by mass is c, and the ratio b / c is 0.01 or more and 0.5 or less.

5. The resin composition according to any one of claims 1 to 4, wherein the component (A) comprises a fluorine-containing epoxy resin.

6. The resin composition according to any one of claims 1 to 5, which is for forming an insulating layer.

7. A resin composition described in any one of claims 1 to 6, which is a resin composition for forming an insulating layer, which is used to form a conductor layer formed on an insulating layer.

8. A resin sheet comprising a support and a resin composition layer provided on the support, the resin composition layer comprising the resin composition according to any one of claims 1 to 7.

9. A printed wiring board comprising an insulating layer formed from a cured product of the resin composition according to any one of claims 1 to 7.

10. A semiconductor device comprising the printed wiring board according to claim 9.

Citation Information

Patent Citations

  • Resin composition, prepreg, metal foil-clad laminate, resin sheet, and printed wiring board

    JP2019006869A

  • Curable resin composition, dry film, cured product and electronic component

    JP2019178307A

  • Curable resin composition, dry film, cured product and electronic component

    JP2019178308A

  • Adhesive sheet with support medium

    JP2019196442A

  • Curable composition, dry film, cured product, laminate and electronic component

    JP2020147728A