Solid-liquid separation method, nickel oxide ore hydrometallurgy method
By adjusting the flocculant amount based on filtration time, the method optimizes clarity and reduces usage, addressing inefficiencies in nickel oxide ore processing.
Patent Information
- Application Number
- JP2021007855
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-21
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-01-21
AI Technical Summary
Existing solid-liquid separation methods in hydrometallurgical smelting of nickel oxide ores require significant amounts of organic flocculant, leading to inefficiencies and increased costs.
Adjust the amount of organic flocculant added based on the filtration time of the supernatant liquid sampled from the first-stage thickener, using a membrane filter with a pore size of 0.45 μm, to optimize clarity and reduce flocculant usage.
Reduces the amount of organic flocculant used while improving the clarity of the supernatant liquid, preventing filter clogging and nickel loss, and enhancing the overall efficiency of the hydrometallurgical process.
Smart Images

Figure 0007585804000003 
Figure 0007585804000004 
Figure 0007585804000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a solid-liquid separation method, and more particularly to a solid-liquid separation method in which a slurry is washed in multiple stages while an organic flocculant is added to separate solids in the slurry to obtain a highly clear solution, and a hydrometallurgical method for nickel oxide ore to which the method is applied. [Background technology]
[0002] In recent years, a hydrometallurgical method known as the HPAL method, in which acid leaching is performed under high temperature and pressure using an autoclave, has been used to recover nickel from low-grade nickel oxide ores.
[0003] Specifically, the hydrometallurgical refining method using the HPAL method includes a leaching step of performing acid leaching using an autoclave, a solid-liquid separation step of separating a leachate containing nickel and cobalt (hereinafter also referred to as "nickel pregnant solution") and a leach residue from the leach slurry, a neutralization step of neutralizing and removing impurities such as iron contained in the leachate, a dezincification step of separating zinc from the final neutralization solution, and a sulfurization step of obtaining a mixed sulfide of nickel and cobalt from the solution after the zinc has been removed.
[0004] In the hydrometallurgical method, the leaching slurry obtained through the leaching process in the leaching step contains undissolved leaching residue and excess free acid that was not involved in the reaction. Therefore, after a preliminary neutralization process for neutralizing and removing the free acid, the slurry is sent to a solid-liquid separation process using multiple countercurrent multi-stage washing to separate the nickel pregnant liquor and the leaching residue using multiple solid-liquid separation thickeners.
[0005] In the solid-liquid separation process using countercurrent multi-stage washing, it is required that the nickel pregnant liquor obtained as the supernatant has a high clarity and that the leaching residue obtained as the precipitate has a high solids concentration. To achieve both of these, an organic flocculant is added.
[0006] Here, Patent Document 1 discloses a solid-liquid separation method in which the solid content is separated and removed while washing the slurry in multiple stages, and proposes a method for effectively washing the slurry to improve the clarity of the supernatant liquid. Specifically, the method is characterized in that a flocculant is added to the feed well of the first-stage thickener, and part of the flocculant is added to the overflow of the second-stage thickener.
[0007] According to the method disclosed in Patent Document 1, a highly clear supernatant liquid (nickel pregnant liquor) can be obtained, and it is also possible to treat the mixture using a fewer number of thickener stages, thereby reducing the installation space required for a solid-liquid separator, and therefore the method can be considered an effective technique.
[0008] However, further improvements are required in order to further reduce the amount of flocculant used in the solid-liquid separation treatment and perform the treatment more efficiently. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] International Publication No. 2014 / 112248 Summary of the Invention [Problem to be solved by the invention]
[0010] The present invention has been proposed in view of the above-mentioned circumstances, and aims to provide a technology that enables efficient processing by reducing the amount of flocculant added in a process in which a slurry is subjected to solid-liquid separation while undergoing multi-stage washing using a multi-stage thickener. [Means for solving the problem]
[0011] The present inventors have conducted extensive research to solve the above-mentioned problems. As a result, they have found that when adding an organic flocculant to a slurry to be treated, the amount of the organic flocculant to be added can be effectively reduced by sampling the liquid in the first-stage thickener and adjusting the amount of the organic flocculant to be added based on the measured value of the filtration time of the sampled liquid, and have completed the present invention.
[0012] (1) The first invention of the present invention is a solid-liquid separation treatment method in which a slurry is washed in multiple stages using thickeners, while an organic coagulant is added to separate the solids in the slurry, and a solution from which the solids have been removed is obtained. When adding the organic coagulant to the slurry, the liquid in the first-stage thickener is sampled, the filtration time of the sampled liquid is measured, and the amount of the organic coagulant added is adjusted based on the measured filtration time.
[0013] (2) The second invention of the present invention is a solid-liquid separation treatment method, in which the amount of the organic coagulant added is adjusted so that the filtration time of the liquid, when measured using a membrane filter having a pore size of 0.45 μm, is 10 seconds or more and 15 seconds or less, in the first invention.
[0014] (3) A third invention of the present invention is a solid-liquid separation treatment method according to the first or second invention, wherein the thickener is provided with a settling tank having an overflow section disposed on the periphery thereof for discharging supernatant liquid, and a cylindrical feedwell disposed vertically in the center thereof, and the supernatant liquid flowing through the overflow section is sampled, and the filtration time of the supernatant liquid is measured.
[0015] (4) A fourth aspect of the present invention is the solid-liquid separation method according to any one of the first to third aspects, wherein the slurry is a slurry obtained by subjecting nickel oxide ore to an acid leaching treatment in a hydrometallurgical method for nickel oxide ore.
[0016] (5) A fifth invention of the present invention is a hydrometallurgical method for nickel oxide ore, which comprises the steps of: adding an acid to nickel oxide ore to perform a leaching treatment; separating a leach slurry obtained by solid-liquid separation; and recovering nickel and cobalt from the separated leachate; the hydrometallurgical method includes a step of performing a solid-liquid separation treatment of adding an organic coagulant to separate a leach residue, which is a solid content in the leach slurry, while washing the leach slurry in multiple stages using thickeners provided in multiple stages; and obtaining a leachate from which the leach residue has been removed; and in the solid-liquid separation treatment, when adding the organic coagulant to the leach slurry, the liquid in a first-stage thickener is sampled, the filtration time of the sampled liquid is measured, and the amount of the organic coagulant added is adjusted based on the measured filtration time. Effect of the Invention
[0017] According to the present invention, in a process in which a slurry is subjected to solid-liquid separation while being washed in multiple stages using a multiple-stage thickener, the amount of flocculant added can be reduced, and the process can be performed efficiently. [Brief description of the drawings]
[0018] [Figure 1] FIG. 1 is a graph showing the results of an investigation into the relationship between the filtration time of the supernatant sampled from inside the first-stage thickener and the turbidity index. [Diagram 2] This is a diagram showing the configuration of a processing device that performs the CCD method by connecting thickeners in multiple stages. [Diagram 3] FIG. 3 is a configuration diagram of a thickener constituting each stage of the processing apparatus shown in FIG. 2. [Figure 4] FIG. 1 is a process diagram showing the flow of a hydrometallurgical method for producing nickel oxide ore. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] A specific embodiment of the present invention (hereinafter, also referred to as "the present embodiment") will be described in detail below. Note that the present invention is not limited to the following embodiment, and can be implemented with appropriate modifications within the scope of the present invention.
[0020] ≪1. Solid-liquid separation treatment method≫ <1-1. Overview> The solid-liquid separation method according to the present embodiment is a method for adding an organic flocculant to separate the solids contained in a slurry and obtaining a solution from which the solids have been removed. The solid-liquid separation process is carried out using an apparatus equipped with multiple thickener stages, and the solids in the slurry are separated while the slurry is washed in multiple stages.
[0021] Specifically, the solid-liquid separation processing method according to this embodiment is characterized in that, when adding an organic coagulant to the slurry to be processed, the liquid in the first stage thickener is sampled, the filtration time of the sampled liquid is measured, and the amount of organic coagulant to be added is adjusted based on the measured filtration time.
[0022] The slurry to be subjected to the solid-liquid separation treatment is not particularly limited, but may be, for example, a slurry (leach slurry) obtained by subjecting nickel oxide ore to an acid leaching treatment in a hydrometallurgical process for nickel oxide ore. When the leach slurry is subjected to the solid-liquid separation treatment, the treatment can separate the leach residue, which is a solid content containing impurity metals such as iron, and recover a leachate containing nickel and cobalt (hereinafter also referred to as "nickel pregnant solution").
[0023] The present inventors conducted a study on the relationship between the turbidity of the supernatant liquid obtained from the first-stage thickener and the filtration time of the supernatant liquid in the solid-liquid separation treatment performed while performing multi-stage washing on the above-mentioned leaching slurry, and obtained the results shown in Figure 1. The filtration time was measured using a membrane filter with a pore size of 0.45 μm.
[0024] That is, as shown in Figure 1, the shorter the filtration time of the supernatant, the higher its turbidity index tends to be, and no significant drop in turbidity is observed after the filtration time exceeds 15 seconds. From this, it was found that the "filtration time" of the supernatant obtained from the first thickener can be used as an indicator for managing the turbidity of the supernatant. It was also found that by using the filtration time of the supernatant as an indicator and adjusting the amount of organic flocculant added based on the measurement results of the filtration time, it is possible to suppress the increase in turbidity and improve clarity while adding an appropriate amount of organic flocculant. The turbidity index is the value obtained by dividing the actually measured turbidity (unit: NTU) by a predetermined turbidity (unit: NTU).
[0025] In particular, it has been found that it is more preferable to adjust the amount of the organic flocculant added based on the filtration time being in the range of 10 seconds or more and 15 seconds or less as a standard.
[0026] Therefore, in the solid-liquid separation method according to the present embodiment, when an organic coagulant is added to the slurry to be treated, the liquid in the first-stage thickener is sampled, the filtration time of the sampled liquid is measured, and the amount of organic coagulant added is adjusted based on the measured filtration time. According to this method, the clarity of the solution obtained by the solid-liquid separation treatment, i.e., the solution obtained by separating and removing the solids, can be improved and stabilized, and the amount of organic coagulant used in the treatment can be reduced, thereby realizing efficient treatment.
[0027] Here, the nickel pregnant liquor is required to have high clarity. In the wet smelting process of nickel oxide ore, the nickel pregnant liquor obtained by solid-liquid separation (treatment in the solid-liquid separation step) is sent to the neutralization step and the dezincification step in sequence. If the nickel pregnant liquor, which is the supernatant liquid obtained by the solid-liquid separation step, has a large amount of SS (Suspended Substances) and has a low clarity, it may cause filter clogging during filtration and other operations in the neutralization step and the dezincification step, significantly impairing the workability. In addition, the leaching residue obtained as a precipitate through the solid-liquid separation treatment of the leaching slurry is required to have a high solid concentration in order to prevent the loss of nickel contained in the nickel pregnant liquor that accompanies the leaching residue.
[0028] In this regard, by applying the solid-liquid separation method according to the present embodiment, the clarity of the resulting nickel pregnant liquor can be effectively improved, and the occurrence of problems such as filter clogging in the subsequent process can be effectively suppressed, and nickel loss can be prevented. In addition, the amount of organic coagulant used can be effectively reduced, so that the efficiency of the entire hydrometallurgical process can be improved.
[0029] <1-2. Operation of solid-liquid separation treatment by countercurrent multi-stage washing> Before describing the solid-liquid separation process in more detail, an operation of performing the solid-liquid separation process while washing in multiple stages using multiple thickeners will be described. Note that the treatment object will be described by taking as an example a leaching slurry obtained through a leaching step in a hydrometallurgical process for nickel oxide ore.
[0030] In the solid-liquid separation process, thickeners, which are solid-liquid separation treatment devices, are connected in multiple stages, and multi-stage washing is performed using a countercurrent multi-stage washing method (CCD method) in which the leaching slurry is contacted with a nickel-free washing solution in a countercurrent manner, while separating the solids contained in the leaching slurry (leaching residue), and obtaining nickel pregnant liquor (leachate), which is a solution from which the solids have been removed.
[0031] [Thickener configuration and multi-stage cleaning] Fig. 2 is a block diagram showing an example of a solid-liquid separation treatment device (hereinafter, also simply referred to as a "treatment device") in which thickeners are connected in multiple stages to perform the CCD method. Note that, although the treatment device 1 shown in Fig. 2 shows an example in which thickeners are connected in five stages, the number of stages is not limited to this.
[0032] In the CCD method, a treatment device is used in which a thickener consisting of a settling tank where solid-liquid separation is performed and a stirring tank is connected in series in multiple stages, for example, 5 to 8 stages. In the treatment device 1, the leaching slurry to be treated is charged into the first stage thickener at one end (side A in Fig. 2), and a cleaning liquid such as industrial water is charged into the final stage (fifth stage) thickener at the other end (side B in Fig. 2). The leaching slurry and the cleaning liquid come into contact with each other in a countercurrent flow in the treatment device 1, and at the same time, an organic flocculant is added to the leaching slurry charged from the A end to flocculate the solids in the slurry and promote solid-liquid separation.
[0033] [About each stage of thickener and mixing tank] Fig. 3 is a configuration diagram of a thickener (only one stage) constituting each stage of the treatment device 1 shown in Fig. 2. As described above, the treatment device 1 is configured by connecting a plurality of thickeners in multiple stages, and the thickener 10 is configured to include an agitation tank 11 and a sedimentation tank 12.
[0034] The stirring tank 11 is a tank equipped with stirring members such as a stirring shaft and stirring blades inside. In the stirring tank 11, the leaching slurry and the overflow liquid sent from the thickener in the subsequent stage are respectively charged and stirred and mixed. Note that the stirring tank 11 of the thickener in the final stage (the fifth stage in the example of Figure 2) is charged with fresh wash water, not the overflow liquid. In the stirring tank 11, the leaching slurry and the overflow liquid are stirred and mixed, so that the leaching slurry is washed and the adhering water adhering to the solid content is washed away.
[0035] The settling tank 12 is, for example, a cylindrical treatment tank, into which the leaching slurry is charged and the solids in the leaching slurry are allowed to settle and be separated.
[0036] The settling tank 12 is equipped with a cylindrical feedwell 13 disposed vertically therein. For example, when the settling tank 12 is cylindrical, the feedwell 13 is disposed approximately concentrically with the settling tank 12. The feedwell 13 serves as a passage for sending the leaching slurry supplied from the stirring tank 11 into the settling tank 12.
[0037] The settling tank 12 is provided with an overflow section 14 at the periphery of the upper part of the tank for overflowing (OF) the supernatant liquid obtained by settling and separating the solids in the leaching slurry. The overflow section 14 is shaped like a gutter, for example, and is connected to a flow path for sending the overflow liquid from the thickener in the downstream to the stirring tank 11. In the settling tank 12, the overflowed solution (hereinafter also referred to as "overflow liquid") is sent to the upstream stirring tank 11 as described above, while the slurry including the remaining solids is taken out from the bottom of the settling tank 12 and pumped by a pump 15 to the downstream stirring tank 11.
[0038] [Basic flow of multi-stage cleaning] Next, we will explain the basic flow of solid-liquid separation while washing the leaching slurry in multiple stages using a treatment device 1 (Figure 2) in which thickeners consisting of stirring tanks 11 and settling tanks 12 are connected in multiple stages. The arrows in Figure 2 indicate the flow of the leaching slurry and the overflow liquid.
[0039] First, in the first-stage thickener, the leaching slurry and overflow liquid from the settling tank 12 of the subsequent second-stage thickener are charged into the stirring tank 11, and they are stirred and mixed. In the stirring tank 11, water adhering to the solids in the leaching slurry is washed away by the overflow liquid, and then the leaching slurry is charged from the stirring tank 11 into the settling tank 12 via the feedwell 13.
[0040] At this time, in the first-stage thickener, an organic flocculant for flocculating the solids in the slurry is added together with the leaching slurry via a feedwell. The leaching slurry and the organic flocculant are mixed in the settling tank 12, and the solids in the slurry are flocculated and precipitated to be separated. The slurry containing the separated solids is extracted from the bottom of the settling tank 12 and transferred via a pump 15 to the stirring tank 11 of the second-stage thickener in the subsequent stage. Meanwhile, the supernatant liquid overflowing from the settling tank 12 via the overflow section 14 is supplied to the next process (neutralization process) in the hydrometallurgical method.
[0041] Next, in the second-stage thickener, the solids extracted from the lower part of the settling tank 12 of the first-stage thickener in the previous stage are charged into the stirring tank 11, and the overflow liquid from the settling tank 12 of the third-stage thickener in the next stage is charged, and the moisture adhering to the solids is washed away by the overflow liquid. Then, the slurry obtained by washing in the stirring tank 11 is charged into the settling tank 12 through the feed well 13, and the solids in the slurry are separated by coagulation and precipitation. The slurry containing the separated solids is discharged from the lower part of the settling tank 12 and transferred to the stirring tank 11 of the third-stage thickener in the next stage via the pump 15. On the other hand, the overflow liquid from the settling tank 12 via the overflow part 14 is charged into the stirring tank 11 via piping or the like connected to the stirring tank 11 of the first-stage thickener in the previous stage.
[0042] Thereafter, in the third and fourth thickeners, the slurry containing solids is washed in multiple stages by coming into countercurrent contact with the overflow liquid in a similar manner.
[0043] In the fifth thickener, which is the final stage, the solids extracted from the lower part of the settling tank 12 of the fourth thickener in the previous stage are charged into the stirring tank 11, and new washing water (for example, a process liquid with a low nickel concentration in a hydrometallurgical process) is charged, and the moisture adhering to the solids is washed away by the washing water. The slurry obtained by washing in the stirring tank 11 is charged into the settling tank 12 through the feed well 13, and the solids in the slurry are separated by coagulation and precipitation. The slurry containing the separated solids is extracted from the lower part of the settling tank 12 by the pump 15, and is treated as a leaching residue (CCD residue). On the other hand, the overflow liquid from the settling tank 12 via the overflow part 14 is charged into the stirring tank 11 through piping or the like connected to the stirring tank 11 of the fourth thickener in the previous stage.
[0044] By subjecting the leaching slurry to solid-liquid separation while washing in multiple stages in this way, new wash water only needs to be charged to the thickener in the final stage, and new wash water is not required for the thickeners in the remaining stages, which makes it possible to significantly save on wash water.
[0045] <1-3. Detailed operations of solid-liquid separation treatment> As described above, in the solid-liquid separation processing method according to the present embodiment, in a process using countercurrent multistage washing with a processing facility consisting of multiple thickener stages, when an organic coagulant is added to the slurry to be processed, the liquid (e.g., the supernatant liquid) in the first-stage thickener is sampled, the filtration time of the sampled liquid is measured, and the amount of organic coagulant added is adjusted based on the measured filtration time.
[0046] The liquid is preferably sampled from an overflow section provided in the thickener. Specifically, as shown in Fig. 3, the thickener 10 is equipped with a settling tank 12 having an overflow section 14 disposed on the periphery thereof for discharging the supernatant liquid, and a cylindrical feed well 13 disposed vertically in the center thereof, and it is preferable to sample the supernatant liquid flowing through the overflow section 14 and measure the filtration time of the supernatant liquid.
[0047] The filtration time of the sampled liquid can be measured by measuring the time required to filter a certain amount of liquid, for example, about 100cc to 250cc, using a suction filter equipped with filter paper of a specified mesh size. For example, a membrane filter with a pore size of 0.45 μm can be used as the filter paper. Suction by the suction filter can be performed using, for example, a vacuum pump.
[0048] Such measurements of the filtration time are carried out periodically at regular intervals, and the amount of organic flocculant added is adjusted based on the measurement results. As shown in Figure 1, in the relationship between the filtration time of the supernatant and its turbidity, the shorter the filtration time, the higher the turbidity tends to be, and once a certain filtration time is exceeded, no significant reduction in turbidity is observed. Therefore, by sampling the supernatant from the overflow of the thickener 10, measuring the filtration time of the supernatant, and adjusting the amount of organic flocculant added based on the measured filtration time, it becomes possible to appropriately reduce turbidity by adding an appropriate amount of organic flocculant.
[0049] For example, as shown in Figure 1, when the filtration time of the supernatant is measured using a membrane filter with a pore size of 0.45 μm, if the filtration time is less than 10 seconds, the turbidity is considered to be high, and feedback is provided to increase the amount of organic coagulant added. On the other hand, if the filtration time exceeds 15 seconds, the possibility of further reduction in turbidity is considered to be low, and feedback is provided to decrease the amount of organic coagulant added.
[0050] In this way, by adjusting the amount of organic flocculant added based on the measured value of the filtration time of the sampled supernatant, the turbidity can be effectively reduced by adding the necessary amount of organic flocculant, i.e., the amount of organic flocculant used can be effectively reduced.
[0051] In particular, it is preferable to adjust the amount of organic flocculant added so that the filtration time of the supernatant liquid is 10 seconds or more and 15 seconds or less when measured using a membrane filter with a pore size of 0.45 μm. By adjusting the amount of organic flocculant added based on such a filtration time range, it is possible to increase the clarity of the supernatant liquid and stabilize the clarity, and also to more effectively reduce the amount of organic flocculant used.
[0052] If the filtration time is less than 10 seconds, the amount of flocculant added is small because the solids in the slurry do not form flocs, but some of the solids do not settle as flocs and remain in the supernatant liquid, which may increase the turbidity. If the filtration time exceeds 15 seconds, the turbidity decreases but not any further, while if the filtration time exceeds this, the effectiveness of the flocculant decreases and the amount of flocculant added may need to be increased. In this case, the viscosity may increase due to an excess of flocculant, which may increase the filtration time.
[0053] In addition, since the supernatant liquid is sampled in the first thickener and the filtration time of the supernatant liquid is measured, the amount of organic flocculant added can be adjusted quickly based on the filtration time, and a decrease in productivity due to a delay in response can be prevented. For example, if the liquid is sampled not in the thickener but in a device installed outside the facility equipped with the thickener, it is not possible to immediately respond to variations in the reactivity of the organic flocculant, making it difficult to perform appropriate turbidity adjustment. This leads to a decrease in productivity. In the solid-liquid separation treatment method according to the present embodiment, the supernatant liquid is sampled in the first thickener, so that the amount of organic flocculant added can be adjusted quickly based on the measured value of the filtration time, preventing a decrease in productivity and more effectively reducing the amount of organic flocculant used.
[0054] The type of organic flocculant is not particularly limited, but for example, a polymer flocculant can be preferably used.
[0055] ≪2. Hydrometallurgy method for nickel oxide ore≫ Next, a method for hydrometallurgy of nickel oxide ore to which a solid-liquid separation method is applied will be described. The above-mentioned solid-liquid separation method can be effectively applied to the treatment in the solid-liquid separation step in the hydrometallurgy process, and can improve and stabilize the clarity of the obtained leachate, while reducing the amount of organic coagulant used, thereby enabling efficient treatment. The hydrometallurgy of nickel oxide ore is a hydrometallurgy method in which nickel and cobalt are leached and recovered from nickel oxide ore using, for example, a method of performing leaching treatment with acid under high temperature and high pressure (HPAL method).
[0056] 4 is a process diagram showing an example of the flow of a hydrometallurgical method for nickel oxide ore. The hydrometallurgical method for nickel oxide ore includes a leaching step S1 in which sulfuric acid is added to nickel oxide ore and leaching treatment is performed under high temperature and high pressure, a solid-liquid separation step S2 in which the obtained leaching slurry is washed in multiple stages while separating the residue to obtain a leachate containing nickel and cobalt, a neutralization step S3 in which the pH of the leachate is adjusted to separate a neutralized precipitate containing impurity elements to obtain a neutralization end solution containing zinc together with nickel and cobalt, a dezincification step S4 in which a sulfurizing agent is added to the neutralization end solution to separate and remove zinc in the form of zinc sulfide, and a nickel recovery step S5 in which a sulfurizing agent is added to the nickel recovery mother liquor from which zinc has been removed to generate and recover a mixed sulfide containing nickel and cobalt.
[0057] (1) Leaching process In the leaching step S1, the nickel oxide ore is subjected to a leaching treatment using, for example, a high-pressure acid leaching method. Specifically, sulfuric acid is added to an ore slurry obtained by crushing the raw material nickel oxide ore, and the ore slurry is stirred by pressurizing it under a high temperature condition of 220°C to 280°C using, for example, a high-temperature pressurized vessel (autoclave), to generate a leaching slurry consisting of a leachate and a leach residue.
[0058] Nickel oxide ores are mainly so-called laterite ores such as limonite ore and saprolite ore. The nickel content of laterite ore is usually 0.8% by mass to 2.5% by mass, and is contained as hydroxide or magnesium silicate mineral. The iron content is 10% by mass to 50% by mass, and is mainly in the form of trivalent hydroxide (goethite), but some divalent iron is contained in the magnesium silicate mineral. In addition to such laterite ores, oxide ores containing valuable metals such as nickel, cobalt, manganese, and copper, such as manganese nodules existing on the deep seabed, are also used.
[0059] During the leaching process, leaching reactions and high-temperature thermal hydrolysis reactions occur, resulting in the leaching of nickel, cobalt, etc. as sulfates and the immobilization of the leached iron sulfate as hematite. However, since the immobilization of iron ions does not proceed completely, the liquid portion of the resulting leaching slurry usually contains divalent and trivalent iron ions in addition to nickel, cobalt, etc.
[0060] The amount of sulfuric acid added in the leaching process is not particularly limited, and an excess amount is used so that the iron in the ore is leached. In the leaching step S1, it is preferable to adjust the pH of the resulting leachate to 0.1 to 1.0 from the viewpoint of filterability of the leaching residue containing hematite generated in the next solid-liquid separation step S2.
[0061] (2) Solid-liquid separation process In the solid-liquid separation step S2, a treatment facility equipped with multiple thickener stages is used to wash the leaching slurry produced in the leaching step S1 in multiple stages while adding an organic coagulant to separate the leaching residue, which is the solid content contained in the leaching slurry, and obtain a leachate containing nickel and cobalt.
[0062] In the treatment in the solid-liquid separation step S2, the leaching slurry is mixed with a washing liquid, and then a solid-liquid separation treatment is performed using a thickener provided in multiple stages as a solid-liquid separation device. Specifically, the leaching slurry is first diluted with a washing liquid, and then the leaching residue in the slurry is concentrated as a sediment in the thickener. This makes it possible to reduce the nickel content adhering to the leaching residue according to the degree of dilution. In addition, by using thickeners connected in multiple stages in this manner, it is possible to improve the recovery rate of nickel and cobalt.
[0063] The cleaning solution used in the multi-stage cleaning is not particularly limited, but any solution that does not contain nickel and does not affect the process can be used. Among them, it is preferable to use an aqueous solution with a pH of 1 to 3. If the pH of the cleaning solution is high, bulky aluminum hydroxide is generated when aluminum is contained in the leaching solution, which causes poor settling of the leaching residue in the thickener. In addition, as the cleaning solution, it is preferable to repeatedly use the barren solution with a low pH (pH of about 1 to 3) obtained in the nickel recovery process S5, which is the subsequent process.
[0064] In this embodiment, the solid-liquid separation method described above in detail is applied to the treatment in the solid-liquid separation step S2. Specifically, when adding an organic flocculant to the leaching slurry, the supernatant in the first-stage thickener is sampled, the filtration time of the sampled supernatant is measured, and the amount of organic flocculant added is adjusted based on the measured filtration time.
[0065] The processing operation is the same as that described above, and therefore a detailed explanation will be omitted here; however, by carrying out such a solid-liquid separation processing method, it is possible to increase the clarity of the obtained leachate and stabilize that clarity, and also to reduce the amount of organic coagulant used, thereby enabling efficient processing.
[0066] (3) Neutralization process In the neutralization step S3, the pH of the leachate separated in the solid-liquid separation step S2 is adjusted, and a neutralized precipitate containing impurity elements is separated to obtain a neutralized end solution containing zinc together with nickel and cobalt.
[0067] Specifically, while suppressing oxidation of the separated leachate, a neutralizing agent such as calcium carbonate is added to the leachate so that the pH of the resulting neutralized end solution is 4 or less, preferably 3.0 to 3.5, and more preferably 3.1 to 3.2, to produce a neutralized end solution that is the source of the mother solution for nickel recovery, and a neutralized precipitate slurry containing trivalent iron as an impurity element. By neutralizing the leachate in this manner, the excess acid used in the leaching treatment by the high-pressure acid leaching method is neutralized to produce a neutralized end solution that is the source of the mother solution for nickel recovery, and impurities such as trivalent iron ions and aluminum ions remaining in the solution are removed as neutralized precipitates.
[0068] (4) Dezincification process In the dezincing step S4, a sulfurizing agent such as hydrogen sulfide gas is added to the neutralization end liquor obtained in the neutralization step S3 to perform a sulfurization treatment to generate zinc sulfide, and the zinc sulfide is separated and removed to obtain a nickel recovery mother liquor (dezincing end liquor) containing nickel and cobalt.
[0069] Specifically, for example, a neutralization end liquid containing zinc together with nickel and cobalt is charged into a pressurized vessel, and a sulfurizing agent is added to selectively sulfurize the zinc relative to the nickel and cobalt, thereby producing zinc sulfide and a mother liquor for nickel recovery.
[0070] (5) Nickel recovery process In the nickel recovery step S5, a sulfurizing agent such as hydrogen sulfide gas is blown into the mother liquor for nickel recovery obtained by separating and removing the zinc, which is an impurity element, to cause a sulfurization reaction, thereby producing a sulfide containing nickel and cobalt (nickel-cobalt mixed sulfide) and a barren liquor.
[0071] The mother liquor for nickel recovery is a sulfuric acid solution in which impurities have been reduced from the leachate of nickel oxide ore through the neutralization step S3 and the dezincification step S4, and is, for example, a solution having a pH of 3.2 to 4.0, a nickel concentration of 2 to 5 g / L, and a cobalt concentration of 0.1 to 1.0 g / L. Note that the mother liquor for nickel recovery may contain several g / L of iron, magnesium, manganese, and the like as impurities, but these impurities have low stability as sulfides relative to the nickel and cobalt to be recovered, and are not contained in the sulfides produced.
[0072] In the nickel recovery step S5, a nickel-cobalt mixed sulfide with few impurity components and a barren solution with a stabilized nickel concentration at a low level are generated and recovered. Specifically, the nickel-cobalt mixed sulfide slurry obtained by the sulfurization reaction is subjected to a sedimentation separation treatment using a sedimentation separation device such as a thickener, and the nickel-cobalt mixed sulfide as a precipitate is separated and recovered from the bottom of the thickener. Meanwhile, the aqueous solution components are allowed to overflow and recovered as a barren solution. As mentioned above, the barren solution contains impurity elements such as iron, magnesium, and manganese that are not sulfurized. EXAMPLES
[0073] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples in any way.
[0074] In the hydrometallurgical process of nickel oxide ore, the leaching slurry obtained through the leaching process was subjected to solid-liquid separation by the countercurrent multistage washing method (CCD method). Specifically, the treatment was carried out using a treatment facility with six connected thickeners under the following treatment conditions. (Processing conditions) Solids ratio of leaching slurry: 44.8% by mass Leaching slurry pH: 2.3 Flow rate of leaching slurry: 249m 3 / h Cleaning solution: Process water with low nickel concentration Flow rate of cleaning fluid: 225m 3 / h Thickener volume: 1500m 3 (Same for each stage)
[0075] In this case, in Example 1, the supernatant in the overflow trough in the first-stage thickener was sampled every two hours, and the filtration time of the sampled supernatant was measured. The filtration time was measured by taking 200 cc of the supernatant and using a membrane filter with a pore size of 0.45 μm.
[0076] Based on the measurement results of the filtration time of the supernatant, the amount of organic flocculant added was adjusted every two hours so that the filtration time was approximately 13 seconds.
[0077] The results of such solid-liquid separation treatment are shown in the following Table 1 (average value) and Table 2 (standard deviation). Note that the flocculant addition ratio in the tables is a value calculated as the ratio of the addition flow rate of an organic flocculant at a predetermined concentration taking into consideration handleability, etc., to the flow rate of the slurry containing the leaching residue introduced into the first-stage thickener.
[0078] As shown in Table 1, in Example 1, the turbidity index for the turbidity of the nickel pregnant liquor, which is the supernatant liquid, was 238 on average, which was about 15% higher than in Comparative Example 1 described later. In addition, the standard deviation of the turbidity index was 67, which was about 30% lower than in Comparative Example 1, and clarity was stabilized. Furthermore, the amount of organic flocculant used was reduced by about 20% compared to Comparative Example 1. Here, the turbidity index refers to the value obtained by dividing the actually measured turbidity (unit: NTU) by a predetermined turbidity (unit: NTU).
[0079] [Comparative Example 1] In Comparative Example 1, similar to Example 1, the supernatant liquid in the overflow trough in the first-stage thickener was sampled every two hours, and the filtration time of the sampled supernatant liquid was measured. However, the amount of organic coagulant added was not adjusted based on the filtration time measurements, and the amount of organic coagulant added was adjusted based on the turbidity measurements so that the turbidity index would be 300 or less.
[0080] The results of such solid-liquid separation treatment are shown in Table 1 (average values) and Table 2 (standard deviation) below. As shown in Table 1, in Example 1, the turbidity index of the nickel pregnant liquor, which is the supernatant liquid, was 238 on average, which was about 15% higher than in Comparative Example 1 described below. In addition, the standard deviation of the turbidity index was 67, which was about 30% lower than in Comparative Example 1, making it possible to stabilize clarity. Furthermore, the amount of organic flocculant used was reduced by about 20% compared to Comparative Example 1.
[0081] [Table 1]
[0082] [Table 2] [Explanation of symbols]
[0083] 1. Solid-liquid separation equipment 10 Thickener 11 Mixing tank 12 Sedimentation tank 13 Feedwell 14 Overflow section
Claims
1. A solid-liquid separation method comprising the steps of: providing multiple thickeners to wash a slurry in multiple stages; adding an organic flocculant to separate solids in the slurry; and obtaining a solution from which the solids have been removed, the method comprising the steps of: When adding the organic flocculant to the slurry, The liquid in the first stage thickener was sampled, Measure the filtration time of the sampled liquid, which is the time from when the slurry is added until solid-liquid separation is completed; adjusting the amount of the organic flocculant added based on the measured filtration time; Solid-liquid separation processing method.
2. The amount of the organic flocculant added is adjusted so that the filtration time of the liquid is 10 seconds or more and 15 seconds or less when measured using a membrane filter having a pore size of 0.45 μm. The solid-liquid separation method according to claim 1.
3. The thickener includes a sedimentation tank having an overflow section disposed on the periphery thereof for discharging supernatant liquid, and a cylindrical feed well disposed vertically in the center thereof; the supernatant liquid flowing through the overflow section is sampled, and the filtration time of the supernatant liquid is measured; The solid-liquid separation method according to claim 1 or 2.
4. The slurry is a slurry obtained by subjecting nickel oxide ore to an acid leaching treatment in a hydrometallurgical method for nickel oxide ore. The solid-liquid separation method according to any one of claims 1 to 3.
5. A method for hydrometallurgy of nickel oxide ore, comprising the steps of adding an acid to nickel oxide ore to perform a leaching treatment, subjecting the resulting leached slurry to solid-liquid separation, and recovering nickel and cobalt from the separated leachate, The method includes a step of performing a solid-liquid separation process in which the leaching slurry is washed in multiple stages using thickeners provided in multiple stages, while an organic flocculant is added to separate the leaching residue, which is a solid content in the leaching slurry, to obtain a leachate from which the leaching residue has been removed, In the solid-liquid separation treatment, when the organic flocculant is added to the leaching slurry, The liquid in the first stage thickener was sampled, Measure the filtration time of the sampled liquid, which is the time from when the leaching slurry is added until solid-liquid separation is completed; adjusting the amount of the organic flocculant added based on the measured filtration time; Hydrometallurgical method.
Citation Information
Patent Citations
Water treatment method and water treatment apparatus
JP2004025109A
Flocculating, precipitating and filtering system
JP2013198865A
Solid-liquid separation method of nickel high-pressure leach residue
JP2020132982A
Solid-liquid-separation processing method, and hydrometallurgical method for nickel oxide ore
WO2014112248A1