cap

The cap design addresses the cost issue of complex layer structures by using an anodized film and acrylic-modified epoxy phenolic resin, achieving cost reduction and easy opening without compromising adhesion.

JP7585929B2Active Publication Date: 2024-11-19ALTEMIRA CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021053444
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-26
Publication Date
2024-11-19
Estimated Expiration
2041-03-26

AI Technical Summary

Technical Problem

The existing caps for beverage bottles with a complex layer structure, including a size coat layer, increase production costs due to their complexity.

Method used

A cap design that omits the size coat layer by using an anodized film with a porosity of 5% or less and a thickness of 50 nm to 300 nm, topped with a top coat layer made of acrylic-modified epoxy phenolic resin, which enhances adhesion and includes a sheet-shaped sealing material for reduced opening torque.

Benefits of technology

The solution reduces costs by eliminating the size coat layer while maintaining good adhesion and providing a smooth opening mechanism.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007585929000006
    Figure 0007585929000006
  • Figure 0007585929000007
    Figure 0007585929000007
  • Figure 0007585929000001
    Figure 0007585929000001
Patent Text Reader

Abstract

To reduce cost by omitting a size coat layer.SOLUTION: A cap comprises a cap body formed by an aluminum material or an aluminum alloy material, has a sheet-shaped seal material provided inside the cap body, and is fitted to a mouthpiece of a bottle can. A ground layer provided with an anodic oxide film is formed inside the cap body. The anodic oxide film has a porosity of 5% or lower and a thickness of 50 nm or more and 300 nm or less. A top coat layer made of an acrylic modified epoxy-acrylic resin is formed on the surface of the ground layer.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cap that is attached to a mouth portion of a bottle can that is filled with a beverage. [Background technology]

[0002] 2. Description of the Related Art Conventionally, as a cap that is attached to a mouth portion of a bottle can into which a beverage is filled, there is a cap described in Patent Document 1, for example. The cap is provided with a base layer on the inner and outer surfaces of the cap, in which an anodized coating and a silane coupling agent are formed in this order, the coating has a porosity of 5% or less and contains 200 to 50,000 ppm of silicon (Si), and the silane coupling agent is present on the surface of the coating in an amount of 0.5 to 5,000 mg / m 2 The inner surface of the base layer is coated with a size coat layer made of polyester / amino resin and a liner adhesive layer, in that order, and the outer surface of the base layer is coated with a size coat layer made of polyester / amino resin, with a coating film on the surface of this layer, and with a top coat layer covering these. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 4393809 Summary of the Invention [Problem to be solved by the invention]

[0004] Incidentally, the cap described in Patent Document 1 has a base layer having a silane coupling agent layer on an anodized film of an aluminum alloy, a liner adhesive layer on the inner surface side, and a top coat layer on the outer surface side, with a size coat layer interposed between them. In this case, the size coat layer has flexibility, so that it can suppress cracks during molding of the liner adhesive layer and top coat layer formed thereon, and can improve adhesion to the base layer. However, the presence of the size coat layer complicates the layer structure, leading to increased costs.

[0005] The present invention has been made in view of the above circumstances, and has an object to reduce costs by omitting the size coat layer. [Means for solving the problem]

[0006] The cap of the present invention has a cap body formed from an aluminum material or an aluminum alloy material and is attached to the nozzle of a bottle can, wherein a base layer with an anodized coating is formed on the inner surface of the cap body, and the anodized coating has a porosity of 5% or less and a thickness of 50 nm to 300 nm, and a topcoat layer made of an acrylic-modified epoxy phenolic resin is formed on the surface of the base layer.

[0007] Acrylic-modified epoxy phenolic resin is a compound of epoxy resin, phenolic hardener, and epoxy resin modified with acrylic, and the adhesion can be improved by partially introducing acrylic groups. By using this as a top coat, it can be formed directly on the surface of the base layer and has good adhesion. Therefore, the size coat layer required for the cap described in Patent Document 1 can be omitted.

[0008] In this cap, a sheet-like sealing material is provided on the inside of the cap body. In this cap, a sealing material is disposed on the top coat layer, so that when the cap is rotated to open the container while sealing the mouth of the container, the sealing material slides between the top coat layer of the cap body and the cap, reducing the torque required to open the container. Effect of the Invention

[0009] According to the present invention, by forming a top coat layer made of an acrylic modified epoxy phenolic resin on the surface of the base layer, good adhesion is obtained and the size coat layer can be omitted, thereby reducing costs. [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is a front view of a half cross-section of a part of a cap and a bottle-shaped can according to one embodiment of the present invention. [Diagram 2] FIG. 2 is an enlarged cross-sectional view showing a schematic coating structure of the cap body. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. As shown in FIG. 1, the cap 10 is made of a cap body 20 formed in a cup shape from an aluminum material or an aluminum alloy material, and a seal material 40 provided on the inner surface of the cap body 20 . The cap body 20 has a top surface portion 21 and a cylindrical portion 22 that is approximately hanging down from the periphery of the top surface portion 21. The cylindrical portion 22 is provided with a plurality of knurls 23 and vent holes 24 formed in a concave-convex shape around the entire circumference of the upper end, a groove 25 formed with a small diameter and continuing to the lower end of the knurls 23 and the vent hole 24, a screw portion formation portion 26 formed with a larger diameter than the groove 25 and continuing to the lower end of the groove 25, a bead 27 formed with a larger diameter than the screw portion formation portion 26 and continuing to the lower end of the screw portion formation portion 26, a plurality of slits 28 formed at approximately the center of the bead 27 with a predetermined gap in the circumferential direction and penetrating the wall of the cylindrical portion 22, and a belt-shaped pilfer-proof portion 29 formed with the lower end of the bead 27. A seal material 40 is provided on the inner surface of the top surface portion 21.

[0012] The sealing material 40 has a two-layer structure consisting of a sliding layer 41 that slides against the inner surface of the top surface 21 of the cap body 20, and a sealing layer 42 laminated on the sliding layer 41. The sliding layer 41 has a higher hardness than the sealing layer 42, and is formed in a disk shape of approximately uniform thickness from polypropylene resin or the like. The sealing layer 42 is formed from a flexible elastomer resin or the like, and has a sealing function of abutting against a curled portion 52 (described below) when attached to the mouth portion 51 of the bottle-can 50 to seal the inside of the bottle-can 50. The cap 10 of this embodiment is a pill-proof cap that is attached to the mouth portion 51 of an aluminum or aluminum alloy (metal) bottle can 50 having a mouth diameter of, for example, 38 mm (the outer diameter of the threaded portion 53 of the bottle 50 is 36 mm to 38 mm) to provide a tight seal.

[0013] As shown in Fig. 2, the inner surface 20a and the outer surface 20b of the cap body 20 are provided with a base layer 34 formed by applying a silane coupling agent 33 to an anodized film 32 on the surface of an aluminum base material 31. The anodized film 32 has a porosity of 5% or less, a thickness of 50 nm to 300 nm, and contains silicon Si in an amount of 200 ppm to 50,000 ppm. The silane coupling agent 33 is applied in an amount of 0.5 mg / m 2 More than 5000mg / m 2 The following is applied to the surface of the anodized coating 32.

[0014] The porosity of the anodized film 32 is set to 5% or less because, although the higher the porosity, the better the adhesion of coatings such as paints and printing inks, the easier it becomes for corrosive substances to reach the aluminum base material, reducing the corrosion resistance of the material, and the electrolyte components and adsorbed moisture remaining in the pores are released after the coating is dried or baked, reducing the adhesion of the silane coupling agent 33 formed on the surface of the film 32. Therefore, the porosity of the anodized film 32 is set to 5% or less, and preferably 0 (zero)%. The porosity of the anodic oxide film 32 can be calculated by dividing the total area of ​​micropores within a given field of view in electron microscope observation by the area of ​​the film 32.

[0015] The reason why the thickness of the anodized coating 32 is set to 50 nm or more and 300 nm or less is that a thickness less than 50 nm does not provide the necessary corrosion resistance and reduces adhesion due to corrosion, and a thickness exceeding 300 nm makes the anodized coating 32 susceptible to cracks during thread forming and other processes, reducing corrosion resistance. Therefore, the thickness of the anodized coating 32 is preferably 50 nm or more and 300 nm or less, more preferably 70 nm or more and 200 nm or less.

[0016] The reason why the anodized coating 32 contains silicon Si in an amount of 200 ppm or more and 50,000 ppm or less is that when silicon Si is incorporated into the anodized coating 21, it can improve the corrosion resistance of the coating 32. If the silicon Si concentration is less than 200 ppm, the effect of improving corrosion resistance is small, and if it exceeds 50,000 ppm, the corrosion resistance does not improve and instead the anodized coating 32 becomes brittle.

[0017] Silane coupling agent 33 applied at a dose of 0.5 mg / m 2 More than 5000mg / m 2 The reason for applying the coating below is to achieve good adhesion between the layer (size coat layer 36 or top coat layer 35 described below) formed thereon and the undercoat layer 34. The coating amount was 0.5 mg / m 2 If the concentration is less than 5000 mg / m, good adhesion cannot be achieved. 2 If the temperature exceeds this range, the adhesion between the silane coupling agent 33 and the anodized film 32 may decrease.

[0018] As described above, among the undercoat layers 34 formed on both sides of the aluminum base material 31, a topcoat layer 35 made of an acrylic-modified epoxy phenolic resin is formed on the inner surface 20a side of the cap body 20. The acrylic-modified epoxy phenolic resin is a compound of an epoxy resin, a phenolic hardener, and an epoxy resin modified with acrylic, and the adhesion can be improved by partially introducing an acrylic group. In this embodiment, a solid polyethylene resin and a liquid ester oil are mixed into the acrylic-modified epoxy phenolic resin as a lubricant so that the sliding layer 41 can slide more easily between the cap body 20 and the cap 10 when the cap 10 is opened after being attached to the mouth part 51 of the bottle can 50. The film thickness is 30 mg / dm 2 More than 60mg / dm 2 Less than 30 mg / dm 2 If it is less than 60 mg / dm 2 If the thickness of the top coat layer 35 exceeds 35 mg / dm2, the plug opening property is hindered and the cost is increased. 2More than 45mg / dm 2 It is preferable that:

[0019] A size coat layer 36 made of polyester / amino resin is formed on the outer surface 20b side of the cap body 20, a coating film 37 of paint or printing ink is formed on the surface of this size coat layer 36, and an overcoat layer 38 made of polyester / amino resin is formed to cover the size coat layer 36 and the coating film 37. The size coat layer 36 has a thickness of, for example, 10 mg / dm 2 More than 20mg / dm 2 The overcoat layer 38 is 45 mg / dm 2 More than 55mg / dm 2 It is formed as follows:

[0020] The cap body 20 having such a coating structure is formed by electrolysis in an electrolyte solution using an aluminum base material 31 made of aluminum or an aluminum alloy as an anode, forming an anodized coating 32 on the surface, and then applying a silane coupling agent 33 to the surface of the anodized coating 32 to form a base layer 34. To make the anodized coating 32 contain silicon Si, a silicate solution is used as the electrolyte solution. Alternatively, after the anodized coating 32 is formed, an aqueous solution containing silicate may be applied and dried. Then, on one side of the undercoat layer 34, a size coat layer 36, a coating film 37, and an overcoat layer 38 are formed in that order, and on the other side, a top coat layer 35 is formed. In this case, the topcoat layer 35 is baked by maintaining it at a temperature of 170° C. to 190° C. for 6 minutes to 15 minutes, or on average, at 180° C. for 10 minutes.

[0021] The cap material 30 thus obtained is press-molded to form the cap body 20, and then the seal material 40 is attached to the inside thereof. The sealing material 40 is attached to the cap body 20 by forming the sealing material 40 into a sheet and pushing it into the open end of the cap body 20 to place it on the inner surface of the top surface 21, or by dropping molten synthetic resin balls into the cap body 20 with the open end of the cap body 20 facing upward, and molding the sealing material 40 within the cap body 20. When molding the sealing material 40 within the cap body 20, a method can be used in which the sliding layer 41 is formed separately from a sheet and inserted into the cap body 20, and the sealing layer 42 is molded on the sliding layer 41, or the sliding layer 41 is also molded within the cap body 20, and the sealing layer 42 is molded on top of the sliding layer 41.

[0022] The cap 10 thus manufactured is fitted onto the mouthpiece 51 of a bottle can 50 filled with a beverage or the like. Then, depending on the type of the filled beverage, the bottle is subjected to retort sterilization, hot water sterilization, warm water sterilization, or the like. In the bottle-can 50 with the cap 10 fastened, the inner surface 20a of the cap body 20 contacts the mouthpiece 51 of the bottle-can 50 or the sliding layer 41 of the sealing material 40. The surface on the inner surface 20a side is formed by the topcoat layer 35, and a good opening torque is maintained even after the above-mentioned sterilization steps. EXAMPLES

[0023] A JIS 5151 aluminum alloy plate with a thickness of 0.230 mm was anodized to form an anodized coating with a thickness of about 100 nm and a porosity of 5% or less, and then a silane coupling agent was applied to the anodized coating to form a base layer. A size coat layer, a print layer, and an overcoat layer were formed in this order on the surface that would become the outer surface of the cap. In addition, a top coat layer made of an acrylic modified epoxy phenolic resin was formed on the base layer on the surface that would become the inner surface of the cap to a thickness shown in the table. The baking temperature of this top coat layer was as shown in the table. As a conventional example, a cap was also produced in which a size coat layer was formed on the surface that would become the inner surface of the cap and then a top coat layer was formed. The thickness and baking temperature of the topcoat layer on the inner surface of these cap materials are shown in Table 1.

[0024] [Table 1]

[0025] The cap material thus produced was press molded to form a cap body with a nominal outer diameter of 38 mm. A two-layered sheet consisting of a sliding layer made of polypropylene resin and a sealing layer made of styrene-based elastomer resin was used as the sealing material and placed inside the cap body. On the other hand, the following various contents were filled into bottle cans to prepare samples. (1) A bottle can was filled with hot water at 75°C and the headspace was replaced with nitrogen. The cap was then attached to the nozzle and tightened, after which it was retorted at 123°C for 23 minutes. (2) The bottles were filled with 85°C hot water and replaced with nitrogen, then the caps were tightened and the cans were pasteurized (hot water sterilized) at 70°C for 10 minutes. (3) A bottle was filled with 5°C carbonated water, the cap was then tightened, and the bottle was then treated with 40°C hot water.

[0026] The cap opening torque of these filled containers was measured. The opening torque was measured for 10 cans at each temperature in the table, including the torque when the cap starts to turn during opening (referred to as 1st torque) and the torque when the bridge subsequently breaks (referred to as 2nd torque), and the average was calculated.

[0027] In addition, to evaluate the physical properties of the coating, commonly performed pencil hardness tests in accordance with JIS K 5600, hot water scratch tests, MEK rubbing tests, DuPont impact tape peel tests in accordance with JIS K 5600, cross-cut peel tests, and dynamic friction coefficient measurements were conducted.

[0028] For the hot water scratch test, a flat painted test piece and a convex surface of a painted test piece with a radius of 1 / 4 inch were dipped back and forth in hot water at 85°C with a load of 200g applied. The number of reciprocations when the paint peeled off was recorded.

[0029] The MEK rubbing test involved fixing 16 layers of No. 1 gauze to the round convex surface of a 2-pound hammer, thoroughly wetting the gauze with methyl ethyl ketone before placing it on the painted surface, and then moving it back and forth over the painted test piece at a speed of 2 seconds per stroke while keeping the hammer so that only the weight of the hammer was applied to the painted surface. The number of strokes at which the paint peeled off was recorded.

[0030] The DuPont impact test was performed using a 300g weight with a tip radius of R 1 / 2 inch, with a drop height of 400mm. The coated test piece was machined to a convex surface, and adhesive tape (Nichiban Cellotape (registered trademark)) was applied to the machined surface, which was then quickly peeled off and the peeling state of the coating was visually observed.

[0031] The dynamic friction coefficient was measured using a measuring device TR-2 manufactured by Toyo Seiki Seisakusho Co., Ltd., with three steel balls as the contact points. Specifically, a sled was prepared with SUS304 steel balls with a diameter of 15.8 mm (R 5 / 8 inch) fixed in an equilateral triangle (distance between contact points: 30 mm), the three steel balls were brought into contact with the coating surface, a string was attached to the sled and connected to a load cell, and the sled was moved along the coating surface under the following conditions, causing the sled to slide on the coating surface, and the tensile load was measured with the load cell. Thread weight: 1000g Pulling speed: 1200mm / min Load cell capacity: 5N The coefficient of dynamic friction μD is The coefficient of kinetic friction μD is calculated by the formula: kinetic friction force (load cell measurement value) Fd / contact force (sled weight x gravitational constant g) Fp. In addition to the measurements at room temperature, measurements were also taken on samples that had been subjected to a sterilization process. The test conditions for the pencil hardness test and the DuPont impact tape peel test are shown in Table 2.

[0032] The results of the coating film performance evaluation are shown in Table 2. The opening torque after various sterilization treatments are also shown in Tables 3 to 5. Table 3 shows the results of retort sterilization (above (1)), Table 4 shows the results of pasteurization (above (2)), and Table 5 shows the results of hot water sterilization (above (3)).

[0033] [Table 2]

[0034] [Table 3]

[0035] [Table 4]

[0036] [Table 5]

[0037] As can be seen from these tables, the caps of the examples are comparable to the conventional examples in terms of the coating film properties shown in Table 2. As for the opening torque, as shown in Tables 3 to 5, the first torque was higher in some cases than in the conventional examples, but generally was not much different from the conventional examples. The second torque was roughly the same as or slightly smaller than the conventional examples. From these results, it can be seen that the cap of the embodiment has almost the same performance as the conventional example, even though the size coat layer on the inner surface is omitted. [Explanation of symbols]

[0038] 10 Cap 20 Cap body 20a Inside 20b External surface 21 Top section 22 Cylindrical part 23 Nar 24 Vent Hole 25 Groove 26 Thread formation area 27 Bead 28 Slit 29 Pilfer Proof Section 30 Cap material 31 Aluminum substrate 32 Anodic oxide film 33 Silane coupling agents 34 Base layer 35 Topcoat layer 36 Size Coat Layer 37 Paint Film 38 Overcoat layer 40 Sealing material 41 Sliding layer 42 Sealing layer 50 Bottle Can 51 Cap part 52 Curl section

Claims

1. A cap having a cap body made of an aluminum material or an aluminum alloy material, a sheet-like sealing material that slides against the inner surface of the cap body is provided on the inside of the cap body, and the cap is attached to the nozzle part of a bottle can, wherein a base layer with an anodized film is formed on the inner surface of the cap body, the anodized film has a porosity of 5% or less and a thickness of 50 nm to 300 nm, and a top coat layer made of an acrylic-modified epoxy phenolic resin is formed directly on the surface of the base layer with a film thickness of 30 mg / dm2 to 60 mg / dm2.

2. A cap as described in claim 1, characterized in that a lubricant is mixed into the acrylic modified epoxy phenolic resin.

Citation Information

Patent Citations

  • Thin-walled drawn can

    JP1993139436A

  • Surface treated aluminum can end material having excellent resin adhesion property and method for manufacturing the same

    JP2002266099A

  • Coated metal sheet and metal package using the same

    JP2002355924A

  • Sheet material for surface-treated aluminum can

    JP2003147550A

  • cap

    JP2005067618A