Method for manufacturing epitaxial silicon wafer
The method addresses autodoping in epitaxial silicon wafers by using dry and wet etching techniques to maintain a thick backside oxide film, stabilizing resistivity and ensuring high-quality impurity diffusion layers.
Patent Information
- Application Number
- JP2021140104
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-08-30
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-08-30
AI Technical Summary
During the manufacturing of epitaxial silicon wafers using low resistivity silicon substrates, autodoping occurs due to dopant diffusion from the substrate into the epitaxial layer, and the removal of surface oxide films for patterning also thins or removes the protective backside oxide film, leading to instability in resistivity.
A method involving dry etching of surface oxide films while attracting the silicon substrate's backside to an electrostatic chuck, followed by wet etching to ensure the backside oxide film remains thick, preventing autodoping and maintaining stable resistivity.
The method effectively prevents autodoping by maintaining a sufficient thickness of the backside oxide film, ensuring stable resistivity and high-quality embedded impurity diffusion layers in epitaxial silicon wafers.
Smart Images

Figure 0007586031000001 
Figure 0007586031000002 
Figure 0007586031000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an epitaxial silicon wafer and a method for manufacturing the same, and more particularly to a method for manufacturing an epitaxial silicon wafer having a buried diffusion layer into which impurities are ion-implanted. [Background technology]
[0002] There is known a technique for forming an impurity diffusion layer on a silicon wafer obtained from a silicon single crystal ingot produced by the Czochralski method (CZ method) or the floating zone melting method (FZ method), and then vapor-growing an epitaxial layer thereon to obtain an epitaxial silicon wafer for devices such as bipolar devices, BiCMOS devices, power ICs, etc. For example, Patent Document 1 discloses an example of a method for forming a buried diffusion layer. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2007-150001 A Summary of the Invention [Problem to be solved by the invention]
[0004] When epitaxial silicon wafers are manufactured using silicon substrates with low resistivity (0.02 Ωcm or less) that contain a large amount of dopant, the dopants in the silicon substrate diffuse outward during vapor phase growth of the epitaxial layer and are incorporated into the epitaxial layer, which is known as autodoping. Autodoping is also a problem not only during epitaxial layer formation, but also in the device manufacturing process. To prevent autodoping, it is necessary to form an oxide film with a thickness of about 200 to 800 nm on the back surface of the silicon substrate.
[0005] However, when an oxide film is formed on the surface of the epitaxial layer, if an attempt is made to remove this oxide film by wet etching, the oxide film for preventing autodoping formed on the back surface of the silicon substrate is also removed together, resulting in a problem that a back surface oxide film of sufficient thickness cannot be left on the back surface of the silicon substrate.
[0006] The oxide film formed on the surface of the epitaxial layer is used, for example, as an oxide film mask for forming a recess (step pattern) on the surface of the epitaxial layer. The recess can be formed by patterning the epitaxial layer using the oxide film mask, and functions as an alignment mark for identifying the position for forming the buried diffusion layer. In addition, a sacrificial oxide film may be formed on the surface of the epitaxial layer when forming an impurity diffusion layer. When an attempt is made to remove such an oxide film formed on the surface of the epitaxial layer by wet etching, the oxide film on the back side of the silicon substrate is also removed together with the oxide film mask. In particular, when a thick oxide film is formed on the surface of the epitaxial layer and the difference in thickness with the back side oxide film is small, the problem of autodoping due to disappearance or thinning of the back side oxide film is prominent.
[0007] Therefore, an object of the present invention is to provide a method for manufacturing an epitaxial silicon wafer having a buried diffusion layer, which is capable of removing a surface oxide film while leaving a back surface oxide film of an appropriate thickness on the back surface side of the silicon substrate. Another object of the present invention is to provide an epitaxial silicon wafer having a buried diffusion layer, which is formed using a silicon substrate with low resistivity and in which the resistivity of the epitaxial layer is stable. [Means for solving the problem]
[0008] In order to solve the above-mentioned problems, a method for producing an epitaxial silicon wafer according to the present invention includes the steps of: forming a back surface oxide film on a back surface of a silicon substrate containing a dopant and having a resistivity of 0.02 Ωcm or less; forming a first epitaxial layer on a front surface of the silicon substrate; forming a first surface oxide film on a front surface of the first epitaxial layer; dry etching the first surface oxide film; forming an impurity diffusion layer in a predetermined region on a front surface of the first epitaxial layer before or after dry etching the first surface oxide film; and forming a second epitaxial layer on the front surface of the first epitaxial layer to embed the impurity diffusion layer.
[0009] According to the present invention, it is possible to prevent the back surface oxide film from disappearing or becoming thin due to the back surface oxide film being removed together with the first front surface oxide film, and therefore it is possible to solve the problem of autodoping, in which the resistivity of the second epitaxial layer fluctuates due to outward diffusion of dopants in the silicon substrate during epitaxial growth.
[0010] The method for producing an epitaxial silicon wafer according to the present invention preferably further comprises the steps of: after forming the first surface oxide film and before forming the impurity diffusion layer, patterning the first surface oxide film to expose a predetermined region on the surface of the first epitaxial layer; forming a second surface oxide film on the exposed surface of the first epitaxial layer; removing the second surface oxide film together with the first surface oxide film by dry etching to form an alignment mark consisting of a recess on the surface of the first epitaxial layer; and removing the first surface oxide film remaining on the surface of the first epitaxial layer by wet etching. According to the present invention, when removing the first surface oxide film used as an oxide film mask for forming the alignment mark, disappearance or thinning of the back surface oxide film can be prevented, thereby maintaining the autodoping prevention function of the back surface oxide film.
[0011] The method for producing an epitaxial silicon wafer according to the present invention further comprises the step of forming an alignment mark consisting of a recess on the surface of the first epitaxial layer by patterning using a resist mask after forming the first epitaxial layer and before forming the first surface oxide film, and it is preferable that the first surface oxide film is formed on the surface of the first epitaxial layer on which the alignment mark is formed, and the formation of the impurity diffusion layer is performed before dry etching the first surface oxide film. According to the present invention, it is possible to prevent the disappearance or thinning of the back surface oxide film when removing the first surface oxide film used as a sacrificial oxide film for forming the impurity diffusion layer, thereby maintaining the autodome prevention function of the back surface oxide film.
[0012] In the method for producing an epitaxial silicon wafer according to the present invention, it is preferable to perform the dry etching in a state where the back surface side of the silicon substrate on which the back surface oxide film is formed is attracted to an electrostatic chuck. By performing the dry etching in a state where the back surface side of the silicon substrate is attracted to an electrostatic chuck in this manner, it is possible to remove the front surface oxide film while preventing the back surface oxide film from disappearing or becoming thinner.
[0013] The method for producing an epitaxial silicon wafer according to the present invention preferably further comprises a step of performing wet etching after the dry etching to further remove the first surface oxide film remaining on the surface of the first epitaxial layer, and the step of forming the second epitaxial layer is preferably performed after the wet etching. In this manner, by performing wet etching after dry etching, the first surface oxide film can be completely removed. Also, by reducing the amount of the back surface oxide film etched by the wet etching, a back surface oxide film of sufficient thickness can be left on the back surface of the silicon substrate.
[0014] In the present invention, the difference in thickness between the back surface oxide film and the first surface oxide film immediately before the dry etching is preferably 200 nm or less. In this way, even if the difference in thickness between the back surface oxide film and the first surface oxide film is small, the surface oxide film can be removed while ensuring a sufficient thickness of the back surface oxide film.
[0015] The thickness of the back surface oxide film immediately before the formation of the first epitaxial layer is preferably 400 nm or more, which makes it possible to prevent autodoping during vapor phase growth of the first epitaxial layer.
[0016] The thickness of the back surface oxide film immediately before the formation of the second epitaxial layer is preferably 400 nm or more, which makes it possible to prevent autodoping during vapor phase growth of the second epitaxial layer.
[0017] Moreover, an epitaxial silicon wafer according to the present invention is characterized in comprising: a silicon substrate containing a dopant and having a resistivity of 0.02 Ωcm or less; an epitaxial layer formed on a surface of the silicon substrate; an impurity diffusion layer embedded inside the epitaxial layer; an alignment mark consisting of a recess formed on the surface of the epitaxial layer; and a back surface oxide film having a thickness of 400 nm or more formed on a back surface of the silicon substrate.
[0018] According to the present invention, since the back surface oxide film effectively functions as a protective film for preventing autodoping of the epitaxial layer during the manufacturing process of the epitaxial silicon wafer, it is possible to provide an epitaxial silicon wafer having a high-quality embedded impurity diffusion layer with stable resistivity of the epitaxial layer. Also, the epitaxial silicon wafer has a back surface oxide film of a sufficient thickness for preventing autodoping in the device manufacturing process. Effect of the Invention
[0019] According to the present invention, it is possible to provide a method for producing an epitaxial silicon wafer having a buried diffusion layer, which can reliably remove a surface oxide film while leaving a back surface oxide film of a desired thickness on the back surface side of a silicon substrate. Another object of the present invention is to provide an epitaxial silicon wafer having a buried diffusion layer, which is formed using a silicon substrate having a low resistivity and has a stable resistivity of an epitaxial layer. [Brief description of the drawings]
[0020] [Figure 1] FIG. 1 is a schematic cross-sectional view showing a structure of an epitaxial silicon wafer according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a process diagram for roughly explaining the method for manufacturing an epitaxial silicon wafer according to the embodiment of the present invention. [Diagram 3] FIG. 3 is a bar graph showing the change in thickness of the front surface oxide film and the back surface oxide film after each manufacturing process of an epitaxial silicon wafer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings.
[0022] FIG. 1 is a schematic cross-sectional view showing a structure of an epitaxial silicon wafer according to an embodiment of the present invention.
[0023] As shown in FIG. 1 , an epitaxial silicon wafer 10 according to the present embodiment is an epitaxial wafer having a buried diffusion layer, and includes a silicon substrate 11, an epitaxial layer 12 formed on a front surface 11a of the silicon substrate 11, an impurity diffusion layer 13 buried in the epitaxial layer 12, an alignment mark 14 formed on the front surface of the epitaxial layer 12, and a back surface oxide film 15 formed on a back surface 11b of the silicon substrate 11.
[0024] The silicon substrate 11 is a single crystal silicon wafer containing a p-type or n-type dopant and having a resistivity of 0.02 Ωcm or less. The dopant may be a p-type dopant such as boron (B) or gallium (Ga), or an n-type dopant such as phosphorus (P), antimony (Sb), or arsenic (As). Furthermore, the silicon substrate 11 may contain multiple types of dopants having the same or opposite conductivity types, and may contain impurities other than dopants such as nitrogen and carbon. Such a silicon substrate with low resistivity is suitable as a substrate material for bipolar devices, BiCMOS devices, power ICs, and the like.
[0025] The epitaxial layer 12 is a single crystal silicon thin film grown by vapor phase growth on the surface 11a of the silicon substrate 11. The thickness of the epitaxial layer 12 is preferably 1 to 50 μm. The epitaxial layer 12 may have a multi-layer structure in which a plurality of epitaxial layers with different characteristics are stacked. The epitaxial layer 12 contains a p-type dopant (boron) or an n-type dopant (phosphorus, arsenic, antimony), and preferably has a resistivity of 0.1 to 100 Ωcm. Usually, the resistivity of the epitaxial layer 12 is set higher than that of the silicon substrate 11.
[0026] The impurity diffusion layer 13 is a layer in which an n-type or p-type impurity (dopant) is diffused in the epitaxial layer 12. The impurity diffusion layer 13 is selectively formed in a predetermined region on the silicon substrate 11. The thickness (depth) of the impurity diffusion layer 13 is not particularly limited, but is preferably 0.1 to 10 nm.
[0027] The alignment mark 14 is provided to indicate a reference position for the formation position of the impurity diffusion layer 13 embedded in the epitaxial layer 12. The alignment mark 14 is made of a recess (step pattern) formed on the surface of the epitaxial layer 12, and has, for example, a cross shape in a plan view. The planar shape of the alignment mark 14 is not particularly limited, and may be any shape as long as it is easily recognizable by image processing.
[0028] The back surface oxide film 15 is a protective film for preventing autodoping, and covers the entire back surface 11b of the silicon substrate 11. When the back surface 11b of the silicon substrate 11 is exposed, dopants in the silicon substrate 11 volatilize from the back surface 11b side during vapor phase growth of the epitaxial layer 12 and move around to the front surface 11a side, and are taken into the epitaxial layer 12, causing a change (decrease) in the resistivity of the epitaxial layer 12. However, when the back surface oxide film 15 is formed on the back surface of the silicon substrate 11, the change in the resistivity of the epitaxial layer 12 can be prevented.
[0029] The initial thickness of the back surface oxide film 15 is preferably 400 nm or more. If the initial thickness of the back surface oxide film 15 is 400 nm or less, there is a risk that the autodoping suppression effect cannot be maintained when the back surface oxide film 15 becomes thinner in the subsequent processing steps.
[0030] FIG. 2 is a process diagram for roughly explaining a method for producing the epitaxial silicon wafer 10 according to the embodiment of the present invention.
[0031] 2, in the manufacture of an epitaxial silicon wafer 10 according to this embodiment, first, a silicon substrate 11 having a resistivity of 0.02 Ωcm or less is prepared (step S1). The silicon substrate 11 can be manufactured by slicing a silicon single crystal ingot grown by, for example, the CZ method or the FZ method to a predetermined thickness, and then subjecting the sliced slice to processing steps such as grinding, polishing, etching, and cleaning. In the manufacture of a silicon single crystal ingot, crystal growth conditions are appropriately set so as to obtain the desired crystal diameter, crystal orientation, resistivity, and the like.
[0032] Next, a back surface oxide film 15 is formed on the back surface 11b of the silicon substrate 11 (step S2). The method for forming the back surface oxide film 15 is not particularly limited, but for example, the back surface oxide film 15 can be formed by forming an oxide film on the back surface 11b of the silicon substrate 11 by single-wafer atmospheric pressure CVD (Chemical Vapor Deposition), and then polishing and removing the oxide film that has spread to the front surface 11a of the silicon substrate 11. The initial thickness of the back surface oxide film 15 is preferably 400 nm or more.
[0033] Next, the first epitaxial layer 12A is formed on the front surface 11a of the silicon substrate 11 by vapor phase growth (step S3). The thickness of the first epitaxial layer 12A is preferably 0.4 to 30 μm. The specific method of forming the first epitaxial layer 12A is not particularly limited, but for example, the first epitaxial layer 12A can be formed by supplying SiHCl3 as a raw material gas together with a hydrogen carrier gas into a reaction chamber in which the silicon substrate 11 is set. During the vapor phase growth of the first epitaxial layer 12A, the silicon substrate 11 is heated to a high temperature of about 1100 to 1200° C., so that when a silicon substrate 11 with low resistivity containing a large amount of dopant is used, there is a problem of autodoping. However, since a back surface oxide film 15 having a sufficient thickness of 400 nm or more is formed on the back surface 11b of the silicon substrate 11, autodoping can be prevented.
[0034] Next, a first surface oxide film 16A is formed on the surface of the first epitaxial layer 12A (step S4). The first surface oxide film 16A can be formed by thermal oxidation. The initial thickness of the first surface oxide film 16A is preferably 200 to 1000 nm. Thereafter, the first surface oxide film 16A is patterned by photolithography and dry etching to form an oxide film mask (step S5). In this way, a partial region of the surface of the first epitaxial layer 12A is exposed.
[0035] Next, the exposed surface of the first epitaxial layer 12A is thermally oxidized to form a second surface oxide film 16B (step S6). The thickness of the second surface oxide film 16B is preferably 200 to 1000 nm. At this time, the first surface oxide film 16A also becomes thicker, but the increase is not the same as the thickness of the second surface oxide film 16B, and is less than the thickness of the second surface oxide film 16B.
[0036] Next, the second surface oxide film 16B is removed by dry etching to form the alignment mark 14 on the surface of the first epitaxial layer 12A (step S7). The planar shape of the alignment mark 14 is not particularly limited, but a cross pattern, for example, is preferable.
[0037] When the second surface oxide film 16B is removed, the first surface oxide film 16A is also removed. In this embodiment, the first surface oxide film 16A is not completely removed, but remains thinly on the surface of the first epitaxial layer 12A as shown in the figure, but it may be completely removed.
[0038] In the dry etching of the second surface oxide film 16B, the first surface oxide film 16A is dry etched in a state in which the back surface 11b side of the silicon substrate 11 is attracted to the electrostatic chuck 20, so that the back surface oxide film 15 is not etched. Therefore, the first and second surface oxide films 16A and 16B can be removed while maintaining the thickness of the back surface oxide film 15.
[0039] When the first surface oxide film 16A is formed thick and the difference in thickness between the back surface oxide film 15 and the first surface oxide film 16A immediately before dry etching is 200 nm or less, if an attempt is made to completely remove the first surface oxide film 16A by wet etching, it is not possible to leave a back surface oxide film 15 with a thickness of 200 nm or more. However, if dry etching is used, it is possible to leave a back surface oxide film 15 with a thickness of 200 nm or more.
[0040] Next, wet etching is performed to completely remove the first surface oxide film 16A remaining on the surface of the first epitaxial layer 12A (step S8). In the wet etching, not only the first surface oxide film 16A but also the back surface oxide film 15 is etched, but since the etching amount can be set to several hundred nm, a sufficient thickness of the back surface oxide film 15 remains on the back surface 11b of the silicon substrate 11.
[0041] Next, the impurity diffusion layer 13 is formed in a predetermined region on the surface of the first epitaxial layer 12A (step S9). The impurity diffusion layer 13 can be formed by ion-implanting a p-type or n-type impurity (dopant) into a desired region formed by photolithography, and then thermally diffusing the impurity.
[0042] Next, the second epitaxial layer 12B is further grown on the first epitaxial layer 12A (step S10). The thickness of the second epitaxial layer 12B is preferably 0.4 to 30 μm. The second epitaxial layer 12B can be formed in the same manner as the first epitaxial layer 12A. In this manner, the epitaxial layer 12 in which the impurity diffusion layer 13 is embedded is formed. The step pattern on the surface of the first epitaxial layer 12A is also inherited by the second epitaxial layer 12B, and an alignment mark 14 is formed on the surface of the second epitaxial layer 12B. In this manner, the epitaxial silicon wafer 10 according to this embodiment is completed.
[0043] During vapor phase growth of the second epitaxial layer 12B, the silicon substrate 11 is heated to a high temperature of about 1100 to 1200° C., and therefore, when using a silicon substrate 11 with low resistivity containing a large amount of dopant, there is a problem of autodoping. However, since a rear surface oxide film 15 having a sufficient thickness of 400 nm or more is formed on the rear surface 11b of the silicon substrate 11, autodoping can be prevented.
[0044] As described above, if the oxide films (first surface oxide film 16A and second surface oxide film 16B) formed on the surface of the epitaxial layer 12 are removed by wet etching, the back surface oxide film 15 is also removed, and there is a risk that the dopants in the silicon substrate 11 will diffuse outward and be incorporated into the epitaxial layer 12 in the subsequent epitaxial process. However, in this embodiment, the first surface oxide film 16A and the second surface oxide film 16B are removed by dry etching, so that the disappearance or thinning of the back surface oxide film 15 is prevented and the problem of autodoping can be solved.
[0045] Although the preferred embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and various modifications are possible without departing from the spirit of the present invention, and it goes without saying that these modifications are also included within the scope of the present invention. For example, after forming the first epitaxial layer 12A and before forming the first surface oxide film 16A, a step of forming an alignment mark 14 on the surface of the first epitaxial layer 12A may be provided, or the impurity diffusion layer 13 may be formed before dry etching the first surface oxide film 16A. EXAMPLES
[0046] 300mm diameter manufactured by CZ method <100> A silicon substrate made of a silicon wafer was prepared. This silicon substrate contained a large amount of arsenic (As), which is an n-type dopant, and had a resistivity of 0.003 Ωcm.
[0047] Next, a backside oxide film (LTO film) of approximately 400 nm was formed on the backside of the silicon substrate, and then a first epitaxial layer doped with phosphorus (P) was formed on the surface of the silicon substrate using the CVD (Chemical Vapor Deposition) method, with a resistivity of 3.0 Ωcm and a thickness of 9 μm.
[0048] Then, a first surface oxide film with a thickness of 496 nm was formed on the surface of the first epitaxial layer by thermal oxidation. This thermal oxidation also thickened the back surface oxide film, increasing its thickness from approximately 400 nm to 648 nm. This first surface oxide film was processed by photolithography and dry etching to form an opening pattern corresponding to the alignment mark.
[0049] Next, the silicon substrate was thermally oxidized to form a second surface oxide film with a thickness of about 500 nm on the exposed surface of the first epitaxial layer. This thermal oxidation also thickened the back surface oxide film and the first surface oxide film, increasing the thickness of the back surface oxide film from 648 nm to 839 nm and the thickness of the first surface oxide film from 496 nm to 721 nm, respectively.
[0050] Next, the second surface oxide film was removed by dry etching to form an alignment mark consisting of a recess. This dry etching also reduced the thickness of the first surface oxide film from 721 nm to 118 nm, but the thickness of the back surface oxide film remained at 839 nm. The first surface oxide film was then completely removed by wet etching. At this time, the etching conditions were controlled so that the etching amount of the first surface oxide film was about 200 nm. As a result, the thickness of the back surface oxide film was reduced from 839 nm to 562 nm.
[0051] Next, an impurity diffusion layer was formed in a predetermined area on the surface of the first epitaxial layer by selective ion implantation of boron (B) using a resist mask. Next, a second epitaxial layer doped with phosphorus and having a resistivity of 3 Ωcm and a thickness of 4 μm was formed on the first epitaxial layer, and a third epitaxial layer doped with phosphorus and having a resistivity of 0.8 Ωcm and a thickness of 5 μm was further formed.
[0052] Fig. 3 is a bar graph showing the change in thickness of the front surface oxide film and the back surface oxide film after each manufacturing process of the epitaxial silicon wafer is performed, and the left graph of the pair of bar graphs in each process shows the thickness of the first front surface oxide film, and the right graph shows the thickness of the back surface oxide film. As is clear from Fig. 3, it was found that the back surface oxide film does not fall below the initial film thickness of 400 nm until the epitaxial silicon wafer is completed, and a back surface oxide film of sufficient thickness can be left. In addition, no abnormality was observed in the resistivity distribution of the epilayer on the front surface measured by a spreading resistance measuring device after the formation of the first to third epitaxial layers, and it was confirmed that autodoping did not occur. [Explanation of symbols]
[0053] 10 Epitaxial silicon wafer 11 Silicon substrate 11a Surface of silicon substrate 11b Back side of silicon substrate 12 Epitaxial layer 12A First epitaxial layer 12B Second epitaxial layer 13 Impurity diffusion layer 14 Alignment Mark 15 Backside oxide film 16A 1st surface oxide film 16B 2nd surface oxide film 17 Resist mask 20 Electrostatic Chuck
Claims
1. forming a rear surface oxide film on a rear surface of a silicon substrate containing a dopant and having a resistivity of 0.02 Ω cm or less; forming a first epitaxial layer on a surface of the silicon substrate; forming a first surface oxide film on a surface of the first epitaxial layer; patterning the first surface oxide film to partially expose a surface of the first epitaxial layer; forming a second surface oxide film on an exposed surface of the first epitaxial layer; removing the second surface oxide film together with the first surface oxide film by dry etching to form an alignment mark consisting of a recess on the surface of the first epitaxial layer; removing the first surface oxide film remaining on a surface of the first epitaxial layer by wet etching; forming an impurity diffusion layer in a predetermined region of a surface of the first epitaxial layer based on the position of the alignment mark; forming a second epitaxial layer on a surface of the first epitaxial layer and burying the impurity diffusion layer.
2. 2. The method for producing an epitaxial silicon wafer according to claim 1, wherein the dry etching is performed in a state where the back surface side of the silicon substrate on which the back surface oxide film is formed is electrostatically chucked.
3. 3. The method for producing an epitaxial silicon wafer according to claim 1, wherein a difference in thickness between the back surface oxide film and the first front surface oxide film immediately before the dry etching is performed is 200 nm or less.
4. 4. The method for producing an epitaxial silicon wafer according to claim 1, wherein the back surface oxide film has a thickness of 400 nm or more immediately before forming the first epitaxial layer.
5. 5. The method for producing an epitaxial silicon wafer according to claim 1, wherein the back surface oxide film has a thickness of 400 nm or more immediately before forming the second epitaxial layer.
Citation Information
Patent Citations
Dry etching method of semiconductor wafer and manufacture of epitaxial wafer
JP2002009051A
Embedded diffusion epitaxial wafer and its manufacturing method
JP2007150001A
Manufacturing method of embedded diffused silicon epitaxial wafer
JP2010135533A
Method for manufacturing epitaxial silicon wafer
JP2011044606A
Semiconductor device manufacturing method
JP2014041866A