Photosensitive resin composition set, optical waveguide and its manufacturing method, photoelectric hybrid board, sheet set, core resin composition, clad resin composition, and resin sheet

A photosensitive resin composition set with phenolic resin, photoacid generator, and crosslinking agent for core and cladding layers addresses high transmission losses in optical waveguides, enabling efficient and durable low-loss waveguides for high-speed communication.

JP7586349B2Active Publication Date: 2024-11-19AJINOMOTO CO INC
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2023576808
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-01-27
Filing Date
2023-01-17
Publication Date
2024-11-19
Estimated Expiration
2043-01-17

AI Technical Summary

Technical Problem

Conventional photosensitive resin compositions used for forming optical waveguides on opto-electrical hybrid boards result in high transmission losses, which hinder efficient high-speed communication.

Method used

A photosensitive resin composition set comprising a core resin composition with phenolic resin, photoacid generator, and crosslinking agent, combined with a cladding resin composition, is developed to achieve a numerical aperture within a specific range, reducing transmission losses in optical waveguides.

Benefits of technology

The solution enables the manufacturing of optical waveguides with low transmission loss, enhancing communication efficiency by minimizing signal attenuation and improving mechanical strength and heat resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586349000055
    Figure 0007586349000055
  • Figure 0007586349000056
    Figure 0007586349000056
  • Figure 0007586349000057
    Figure 0007586349000057
Patent Text Reader

Abstract

The present invention provides a photosensitive resin composition set which is capable of producing an optical waveguide that has a low transmission loss. The present invention provides a photosensitive resin composition set which comprises a resin composition for cores and a resin composition for claddings, wherein: the resin composition for cores contains (A) a phenolic resin, (B) a photoacid generator and (C) a crosslinking agent; the resin composition for claddings contains (a) a phenolic resin, (b) a photoacid generator and (c) a crosslinking agent; and the numerical aperture NA obtained from the refractive index of a cured product of the resin composition for cores and the refractive index of a cured product of the resin composition for claddings is within a specific range.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a photosensitive resin composition set, an optical waveguide and a method for producing the same, an optoelectronic hybrid board, a sheet set, a core resin composition, a cladding resin composition, and a resin sheet. [Background technology]

[0002] Technological advances such as 5G communications, autonomous driving, IoT, artificial intelligence, and big data have led to an increasing demand for ultra-high-speed and large-capacity communications. Semiconductor packages, which are the backbone of these communications, have traditionally supported high-speed communications by passing high-frequency currents through them. However, in recent years, issues of noise generation, communication loss, and heat generation due to high-speed communications have become evident. To solve these issues, active efforts have been made in recent years to implement optical circuits on electrical wiring boards and achieve energy savings, low latency, and high-speed communications (Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-211540 A [Patent Document 2] Patent No. 5771978 Summary of the Invention [Problem to be solved by the invention]

[0004] Especially in data centers where high-speed transmission is required, research into the introduction of silicon photonics is being actively conducted. Silicon photonics is highly compatible with conventional LSI manufacturing processes. Therefore, it is expected that the use of silicon photonics will enable the formation of nanometer-sized thin-wire waveguides at low cost based on the technology cultivated in electronic circuit integration technology.

[0005] For example, silicon photonics is expected to form an optical integrated circuit on a chip using a fine-wire waveguide. When manufacturing an optoelectronic hybrid board mounting this chip, it is required to provide an optical waveguide on the optoelectronic hybrid board in order to extract signal light from the fine-wire waveguide in the chip to the outside of the chip and connect it to wiring between chips. From the viewpoint of efficiently forming a fine optical waveguide, it is desirable to form the optical waveguide from a cured product of a photosensitive resin composition. However, optical waveguides formed using conventional photosensitive resin compositions have a large transmission loss.

[0006] The present invention has been devised in view of the above-mentioned problems, and aims to provide a photosensitive resin composition set capable of producing an optical waveguide with low transmission loss; an optical waveguide capable of reducing transmission loss and a method for producing the same; an optoelectronic hybrid board comprising the optical waveguide; and a sheet set, a core resin composition, a clad resin composition, and a resin sheet capable of forming an optical waveguide with low transmission loss. [Means for solving the problem]

[0007] The present inventors have conducted extensive research to solve the above problems, and as a result, have found that when a core resin composition containing (A) a phenolic resin, (B) a photoacid generator, and (C) a crosslinking agent is combined with a cladding resin composition containing (a) a phenolic resin, (b) a photoacid generator, and (c) a crosslinking agent to produce an optical waveguide having a numerical aperture NA in a specific range, the optical transmission loss can be suppressed, and have completed the present invention. That is, the present invention includes the following.

[0008] [1] A photosensitive resin composition set including a core resin composition and a clad resin composition; The core resin composition comprises (A) a phenolic resin, (B) a photoacid generator, and (C) a crosslinking agent; The cladding resin composition comprises (a) a phenolic resin, (b) a photoacid generator, and (c) a crosslinking agent; A photosensitive resin composition set having a numerical aperture NA represented by the following formula (1) greater than 0.05 and less than 0.4:

number

number

[10] The optical waveguide according to [8] or [9], which is a single-mode optical waveguide.

[11] An optical / electrical hybrid board comprising the optical waveguide according to any one of [8] to

[10] .

[12] A step of forming a first composition layer containing a cladding resin composition; A step of subjecting the first composition layer to an exposure treatment; curing the first composition layer; forming a second composition layer containing a core resin composition on the first composition layer; a step of subjecting the second composition layer to an exposure treatment; subjecting the second composition layer to a development treatment; curing the second composition layer; forming a third composition layer containing a cladding resin composition on the second composition layer; a step of subjecting the third composition layer to an exposure treatment; curing the third composition layer, in this order; The core resin composition comprises (A) a phenolic resin, (B) a photoacid generator, and (C) a crosslinking agent; The cladding resin composition comprises (a) a phenolic resin, (b) a photoacid generator, and (c) a crosslinking agent; A method for producing an optical waveguide, wherein a numerical aperture NA represented by the following formula (1) is greater than 0.05 and less than 0.4:

number

[13] A sheet set including a core resin sheet and a clad resin sheet; the core resin sheet includes a core resin composition layer including a core resin composition including (A) a phenolic resin, (B) a photoacid generator, and (C) a crosslinking agent; The clad resin sheet includes a clad resin composition layer including a clad resin composition including (a) a phenolic resin, (b) a photoacid generator, and (c) a crosslinking agent; A sheet set having a numerical aperture NA represented by the following formula (1) greater than 0.05 and less than 0.4.

number

[14] A core resin composition for forming a core layer in a cladding layer, comprising a cured product of a cladding resin composition comprising (a) a phenolic resin, (b) a photoacid generator, and (c) a crosslinking agent; The core resin composition comprises (A) a phenolic resin, (B) a photoacid generator, and (C) a crosslinking agent; A core resin composition having a numerical aperture NA represented by the following formula (1) greater than 0.05 and less than 0.4:

number

[15] A resin sheet comprising a resin composition layer containing the core resin composition according to

[14] .

[16] A clad resin composition for forming a clad layer covering a core layer, the clad resin composition comprising a cured product of a core resin composition comprising (A) a phenolic resin, (B) a photoacid generator, and (C) a crosslinking agent; The cladding resin composition comprises (a) a phenolic resin, (b) a photoacid generator, and (c) a crosslinking agent; A resin composition for cladding, having a numerical aperture NA represented by the following formula (1) of more than 0.05 and less than 0.4:

number

[17] A resin sheet comprising a resin composition layer containing the cladding resin composition according to

[16] . Effect of the Invention

[0009] According to the present invention, there can be provided a photosensitive resin composition set with which an optical waveguide with low transmission loss can be manufactured; an optical waveguide with low transmission loss and a manufacturing method thereof; an optoelectronic hybrid board including the optical waveguide; and a sheet set, a core resin composition, a clad resin composition, and a resin sheet with which an optical waveguide with low transmission loss can be formed. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a perspective view showing a schematic diagram of an optical waveguide according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view for illustrating step (I) of the method for producing an optical waveguide according to one embodiment of the present invention. [Diagram 3]FIG. 3 is a schematic cross-sectional view for explaining step (III) of the method for producing an optical waveguide according to one embodiment of the present invention. [Figure 4] FIG. 4 is a schematic cross-sectional view for explaining step (IV) of the method for producing an optical waveguide according to one embodiment of the present invention. [Diagram 5] FIG. 5 is a schematic cross-sectional view illustrating step (V) of the method for producing an optical waveguide according to one embodiment of the present invention. [Figure 6] FIG. 6 is a schematic cross-sectional view for illustrating step (VI) of the method for producing an optical waveguide according to one embodiment of the present invention. [Figure 7] FIG. 7 is a schematic cross-sectional view for illustrating step (VII) of the method for producing an optical waveguide according to one embodiment of the present invention. [Figure 8] FIG. 8 is a schematic cross-sectional view for explaining step (VIII) of the method for producing an optical waveguide according to one embodiment of the present invention. [Figure 9] FIG. 9 is a schematic cross-sectional view for explaining step (X) of the method for producing an optical waveguide according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will be described in detail below with reference to the following embodiments and examples. However, the present invention is not limited to the following embodiments and examples, and may be modified and practiced as desired without departing from the scope of the claims and their equivalents.

[0012] In the following description, unless otherwise specified, the term "(meth)acrylic acid" includes acrylic acid, methacrylic acid, and combinations thereof, and the term "(meth)acrylate" includes acrylate, methacrylate, and combinations thereof.

[0013] [1. Overview of photosensitive resin composition set] The photosensitive resin composition set according to one embodiment of the present invention includes a core resin composition and a clad resin composition. The core resin composition and the clad resin composition can be used for producing an optical waveguide including a core layer containing a cured product of the core resin composition and a clad layer containing a cured product of the clad resin composition.

[0014] The core resin composition contains (A) a phenolic resin, (B) a photoacid generator, and (C) a crosslinking agent. The cladding resin composition contains (a) a phenolic resin, (b) a photoacid generator, and (c) a crosslinking agent. The refractive index n of the cured product of the core resin composition is core and the refractive index n of the cured product of the cladding resin composition clad Therefore, the numerical aperture NA defined by the following formula (1) is within a specific range.

[0015]

number

[0016] According to the photosensitive resin composition set of the present embodiment, an optical waveguide with small transmission loss can be manufactured. Specifically, when a core layer is formed from a cured product of the core resin composition and a clad layer is formed from a cured product of the clad resin composition, an optical waveguide having a core layer and a clad layer can be manufactured. The optical waveguide manufactured in this manner can suppress the transmission loss of light transmitted through the optical waveguide.

[0017] Since the core resin composition and the clad resin composition are photosensitive resin compositions, it is usually possible to efficiently produce a fine optical waveguide by a method including exposure and development. Moreover, the optical waveguide usually has excellent reflow resistance.

[0018] [2. Core resin composition] The core resin composition includes (A) a phenolic resin, (B) a photoacid generator, and (C) a crosslinking agent. Since the core resin composition can be a photosensitive resin composition, a core layer having a desired pattern can be formed by a method including exposure and development. The "pattern" of the core layer refers to the shape of the core layer as viewed from the thickness direction, unless otherwise specified.

[0019] Specifically, the photoacid generator (B) can generate an acid when irradiated with light. This acid can promote the crosslinking reaction of the crosslinking agent (C). Therefore, the core resin composition can have a reduced solubility in a developer in the area irradiated with light (hereinafter sometimes referred to as the "exposed area"). Therefore, the core resin composition can form a latent image by exposure to light.

[0020] Moreover, the core resin composition can usually be removed by a developer. In particular, since the (A) phenolic resin is usually alkali-soluble, the core resin composition can be easily removed by an alkaline developer. Therefore, the core resin composition in the portion not irradiated with light (hereinafter sometimes referred to as the "non-exposed portion") can be removed by a developer to develop the latent image. "Alkali-soluble" refers to the property that the alkali-soluble component is soluble in an alkaline aqueous solution (for example, a 2.38 mass% aqueous solution of tetramethylammonium hydroxide).

[0021] Therefore, the core resin composition can form a core layer with a fine pattern by a method including exposure and development. This core layer can be combined with a clad layer formed by a cured product of the clad resin composition to produce an optical waveguide capable of transmitting light through the core layer. As described above, the optical waveguide including the combination of the core layer and the clad layer can suppress the transmission loss of light.

[0022] Furthermore, the core resin composition usually has excellent resolution, and the cured product of the core resin composition usually has excellent mechanical strength such as elongation at break, and excellent heat resistance such as reflow resistance.

[0023] [2.1.(A) Phenolic resin] The core resin composition contains a phenolic resin (A) as component (A). The phenolic resin (A) is soluble in an appropriate type of developer, and is particularly soluble in an alkaline developer. The phenolic resin (A) preferably reacts with a crosslinking agent (C) to bond, and thus can react with the crosslinking agent (C) to effectively reduce the solubility of the core composition in the developer.

[0024] The (A) phenolic resin contains a phenolic hydroxyl group in the molecule. The phenolic hydroxyl group refers to a hydroxyl group bonded to an aromatic ring such as a benzene ring or a naphthalene ring. The number of phenolic hydroxyl groups in the (A) phenolic resin may be one or two or more per molecule. In particular, from the viewpoint of promoting the crosslinking reaction by the (C) crosslinking agent and increasing the degree of crosslinking to increase the mechanical strength of the cured product, it is preferable that the (A) phenolic resin has two or more phenolic hydroxyl groups per molecule.

[0025] The (A) phenolic resin may be used alone or in combination of two or more. Preferred examples of the (A) phenolic resin include a compound having a structure represented by the following formula (A-1), a compound having a structure represented by formula (A-2), and a compound having a structure represented by formula (A-3). In the following description, the compound having a structure represented by formula (A-1), the compound having a structure represented by formula (A-2), and the compound having a structure represented by formula (A-3) may be referred to as the (A-1) component, the (A-2) component, and the (A-3) component, respectively. When these (A-1) to (A-3) components are used, the transmission loss of the optical waveguide can be effectively suppressed, and further, usually, the resolution of the core resin composition and the mechanical strength and heat resistance of the cured product of the core resin composition can be particularly improved.

[0026] [ka]

[0027] (In formula (A-1), R 1 each independently represents a divalent hydrocarbon group which may have a substituent; X 1 each independently represents an alkyl group which may have a substituent, an aryl group which may have a substituent, a halogen atom, or a monovalent heterocyclic group which may have a substituent. n1 represents an integer of 0 to 4, and m1 represents an integer of 1 to 200. * represents a bond. In formula (A-2), R 2 represents a divalent group represented by the following formula (r-1), a divalent group represented by the following formula (r-2), a divalent group represented by the following formula (r-3), or a divalent group consisting of a combination thereof; X 2 and X 3 each independently represents an alkyl group which may have a substituent, an aryl group which may have a substituent, a halogen atom, or a monovalent heterocyclic group which may have a substituent. n2 and n3 each independently represent an integer of 0 to 4. In formula (A-3), R 3 represents a divalent group represented by the following formula (r-1), a divalent group represented by the following formula (r-2), a divalent group represented by the following formula (r-3), or a divalent group consisting of a combination thereof; X 4 and X 5 each independently represents an alkyl group which may have a substituent, an aryl group which may have a substituent, a halogen atom, or a monovalent heterocyclic group which may have a substituent. n4 and n5 each independently represent an integer of 0 to 3.

[0028] [ka]

[0029] (In formula (r-1), R 11 and R 12 each independently represents a hydrogen atom, an optionally substituted alkyl group, an optionally substituted aryl group, an optionally substituted monovalent heterocyclic group, an amino group, a carbonyl group, a carboxyl group, or a group consisting of a combination thereof; R 11 and R 12may be bonded to each other to form a ring. * represents a bond. In formula (r-2), X 11 each independently represents an alkyl group which may have a substituent, p1 represents an integer of 0 to 4, and * represents a bond. In formula (r-3), X 12 and X 13 each independently represents an alkyl group which may have a substituent; p2 and p3 each independently represent an integer of 0 to 4; * represents a bond.

[0030] -Component (A-1): A compound having a structure represented by formula (A-1)- The component (A-1) represents a compound containing a structure represented by the following formula (A-1): The component (A-1) may be used alone or in combination of two or more types.

[0031] [ka]

[0032] (In formula (A-1), R 1 each independently represents a divalent hydrocarbon group which may have a substituent; X 1 each independently represents an alkyl group which may have a substituent, an aryl group which may have a substituent, a halogen atom, or a monovalent heterocyclic group which may have a substituent. n1 represents an integer of 0 to 4, and m1 represents an integer of 1 to 200. * represents a bond.

[0033] In formula (A-1), X 1 each independently represents an alkyl group which may have a substituent, an aryl group which may have a substituent, a halogen atom, or a monovalent heterocyclic group which may have a substituent. 1 As the alkyl group, an optionally substituted alkyl group, an optionally substituted aryl group, or a halogen atom is preferable, an optionally substituted alkyl group and an optionally substituted aryl group are more preferable, and an optionally substituted alkyl group is even more preferable.

[0034] The alkyl group may be a straight-chain, branched-chain, or cyclic alkyl group. The cyclic alkyl group may be either a monocyclic or polycyclic alkyl group. The alkyl group is preferably an alkyl group having 1 to 10 carbon atoms, more preferably an alkyl group having 1 to 6 carbon atoms, and even more preferably an alkyl group having 1 to 3 carbon atoms. Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, an isopropyl group, a s-butyl group, a t-butyl group, a 2-methylpropyl group, and a 3-heptyl group. Among them, a methyl group is particularly preferred.

[0035] The aryl group is preferably an aryl group having 6 to 30 carbon atoms, more preferably an aryl group having 6 to 20 carbon atoms, and even more preferably an aryl group having 6 to 10 carbon atoms. Examples of the aryl group include a phenyl group and a naphthyl group.

[0036] Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom, with a fluorine atom being preferred.

[0037] The monovalent heterocyclic group is preferably a monovalent heterocyclic group having 3 to 21 carbon atoms, more preferably a monovalent heterocyclic group having 3 to 15 carbon atoms, and even more preferably a monovalent heterocyclic group having 3 to 9 carbon atoms. The monovalent heterocyclic group also includes a monovalent aromatic heterocyclic group (heteroaryl group). Examples of the monovalent heterocyclic group include a thienyl group, a pyrrolyl group, a furanyl group, a furyl group, a pyridyl group, a pyridazinyl group, a pyrimidyl group, a pyrazinyl group, a triazinyl group, a pyrrolidyl group, a piperidyl group, a quinolyl group, and an isoquinolyl group. Among them, a pyrrolidyl group is preferable. The monovalent heterocyclic group refers to a group obtained by removing one hydrogen atom from a heterocyclic ring of a heterocyclic compound.

[0038] X 1 The alkyl group, aryl group, and monovalent heterocyclic group represented by may have a substituent. Examples of the substituent include a halogen atom such as a fluorine atom, -OH, -OC1-6 An alkyl group, -N(C 1-6 alkyl group)2, C 1-6 alkyl group, C 6-10 an aryl group, -NH2, -NH(C 1-6 alkyl group), -CN, -C(O)O-C 1-6 alkyl group, -C(O)H, -NO2, etc. may be mentioned.

[0039] In this specification, the expression "may have a substituent" means unsubstituted or having a substituent unless otherwise specified. The number of substituents may be 1 or 2 or more. In one example, the number of substituents may usually be 1 to 5 (preferably 1, 2 or 3). When having a plurality of substituents, these substituents may be the same or different from each other. Also, in this specification, the term "C p-q "(p and q are positive integers and satisfy p < q.) represents that the number of carbon atoms of the organic group described immediately after this term is p to q. For example, the expression "C 1-6 alkyl group" represents an alkyl group having 1 to 6 carbon atoms.

[0040] In formula (A-1), R 1 each independently represents a divalent hydrocarbon group which may have a substituent. Preferably, R 1 each independently represents a divalent group represented by formula (r-1).

[0041]

Chemical formula

[0042] (In formula (r-1), R 11 and R 12 each independently represent a hydrogen atom, an alkyl group which may have a substituent, an aryl group which may have a substituent, a monovalent heterocyclic group which may have a substituent, an amino group, a carbonyl group, a carboxyl group, or a group composed of a combination thereof, and R 11 and R 12 may be bonded to each other to form a ring. * represents a bond.)

[0043] In formula (r-1), R 11 and R 12 each independently represents a hydrogen atom, an optionally substituted alkyl group, an optionally substituted aryl group, an optionally substituted monovalent heterocyclic group, an amino group, a carbonyl group, a carboxyl group, or a group consisting of a combination thereof; R 11 and R 12 may be bonded to each other to form a ring. Among these, a hydrogen atom and an alkyl group are preferred.

[0044] R 11 and R 12 The optionally substituted alkyl group, the optionally substituted aryl group, and the optionally substituted monovalent heterocyclic group represented by X in formula (A-1) are 1 The optionally substituted alkyl group, the optionally substituted aryl group, and the optionally substituted monovalent heterocyclic group represented by the formula (I) may be the same as the optionally substituted alkyl group, the optionally substituted aryl group, and the optionally substituted monovalent heterocyclic group represented by the formula (I).

[0045] Examples of groups formed from these combinations include a group formed from a combination of an alkyl group and a carbonyl group, a group formed from a combination of an aryl group and a carbonyl group, a group formed from a combination of an alkyl group, an amino group and a carbonyl group, and a group formed from a combination of an aryl group, an amino group and a carbonyl group.

[0046] R 11 and R 12 may be bonded to each other to form a ring. 11 and R 12 The ring structure which may be formed by R also includes a spiro ring and a fused ring. 11 and R 12 is preferably a group forming a cyclopentane ring, a group forming a cyclohexane ring, a group forming a 2,2-dimethyl-4-methylcyclohexane ring, a group forming a fluorene ring, a group forming a pyrrolidine ring, or a group forming a γ-lactam ring.

[0047] Specific examples of the divalent group represented by formula (r-1) include the following groups: In the formula, "*" represents a bond.

[0048] [ka]

[0049] [ka]

[0050] In formula (A-1), R 1 may each independently be a divalent group represented by formula (r-4).

[0051] [ka]

[0052] (In formula (r-4), R 13 and R 14 each independently represents an alkylene group; 14 each independently represents an alkyl group which may have a substituent, p4 represents an integer of 0 to 4, and m2 represents an integer of 1 to 3. * represents a bond.

[0053] In formula (r-4), R 13 and R 14 each independently represents an alkylene group. The number of carbon atoms in the alkylene group is usually 1 or more, and preferably 18 or less, more preferably 12 or less, even more preferably 6 or less, and particularly preferably 4 or less. Examples of the alkylene group include a methylene group, an ethylene group, a propylene group, and a butylene group.

[0054] In formula (r-4), X 14 Each of X independently represents an alkyl group which may have a substituent. 14 is X in formula (A-1) 1 The alkyl group may be the same as the alkyl group which may have a substituent represented by the formula (1).

[0055] In formula (r-4), p4 represents an integer of 0 to 4, preferably an integer of 0 to 3, more preferably 0 or 1, and particularly preferably 0.

[0056] In formula (r-4), m2 represents an integer of 1 to 3, preferably an integer of 1 or 2, and particularly preferably 2.

[0057] In formula (A-1), R 1 may each independently be a divalent group represented by formula (r-5).

[0058] [ka]

[0059] (In formula (r-5), X 15 each independently represents an alkyl group which may have a substituent, and p5 represents an integer of 0 to 12. * represents a bond.

[0060] In formula (r-5), X 15 Each of X independently represents an alkyl group which may have a substituent. 15 is X in formula (A-1) 1 The alkyl group may be the same as the alkyl group which may have a substituent represented by the formula (1).

[0061] In formula (r-5), p5 represents an integer of 0 to 12, preferably an integer of 0 to 2, more preferably 0 or 1, and particularly preferably 0.

[0062] R 1 is preferably bonded to any one of the ortho, meta, and para positions relative to the OH group of the phenol moiety in formula (A-1), more preferably bonded to any one of the meta and para positions, and even more preferably bonded to a mixture of the meta and para positions. 1 and R is attached to the para position of the OH group of the phenol moiety in formula (A-1).1 When the (A-1) component contains a structure in which R is bonded to the meta position, 1 The mass of the bonded structure is m, and R is 1 The mass of the structure in which R is bonded is represented by p. In this case, the mixture ratio (m:p) is preferably 1:0.1 to 1:10, more preferably 1:0.1 to 1:5, further preferably 1:0.1 to 1:2, and particularly preferably 1:0.5 to 1:1. 1 When is a divalent group represented by formula (r-1), it is particularly preferable that the mixing ratio (m:p) is within the above range.

[0063] In formula (A-1), n1 represents an integer of 0 to 4, preferably an integer of 0 to 3, and more preferably 0 or 1. 1 When R is a divalent group represented by formula (r-1), n1 is particularly preferably 1. 1 When is a divalent group represented by formula (r-4) or a divalent group represented by formula (r-5), n1 is particularly preferably 0.

[0064] In formula (A-1), m1 represents an integer of 1 to 200. In detail, m1 is usually 1 or more, and may be 2 or more. Moreover, m1 is usually 200 or less, preferably 150 or less, more preferably 100 or less, and particularly preferably 50 or less.

[0065] Specific examples of the component (A-1) include resins represented by the following formulas (A-1-1) to (A-1-3). In the specific example represented by formula (A-1-1), it is preferable that 60% of the methylene groups are bonded to the meta positions and 40% are bonded to the para positions relative to the OH groups of the phenol moieties. In the following formulas (A-1-1) to (A-1-3), n6, n7, and n8 represent integers from 1 to 200.

[0066] [ka]

[0067] The (A-1) component may be a commercially available product. Specific examples of commercially available (A-1) components include "TR4020G" (resin represented by formula (A-1-1)) manufactured by Asahi Yukizai Co., Ltd.; AV Light series such as "TR4050G", "TR4080G", "TR5020G", "TR5050G", "TR6020G", "TR6050G", and "TR6080G" manufactured by Asahi Yukizai Co., Ltd.; photoresist resin series manufactured by Sumitomo Bakelite Co., Ltd.; Resitop series manufactured by Gun-ei Chemical Industry Co., Ltd.; "PR-30-40P", "PR-100L", and "PR-100L" manufactured by DIC Corporation. 00H", "PR-50", "PR-55", "PR-56-1", "PR-56-2", "WR-101", "WR-102", "WR-103", "WR-104" and other Phenolite series; Lignite Corporation's "LF-100", "LF-110", "LF-120", "LF-200", "LF-400", and "LF-500"; Meiwa Chemical Co., Ltd.'s photoresist base resin series, MEH-7851 series; and JFE Chemical Corporation's J-DPP series.

[0068] The amount of the (A-1) component is preferably 10% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, even more preferably 50% by mass or more, and is preferably 95% by mass or less, more preferably 90% by mass or less, even more preferably 85% by mass or less, based on 100% by mass of the total (A) phenolic resin. When the amount of the (A-1) component is within the above range, the transmission loss of the optical waveguide can be effectively suppressed, and furthermore, the resolution of the core resin composition and the mechanical strength and heat resistance of the cured product of the core resin composition can be particularly improved.

[0069] The amount of component (A-1) is preferably 10% by mass or more, more preferably 20% by mass or more, even more preferably 30% by mass or more, even more preferably 40% by mass or more, and is preferably 80% by mass or less, more preferably 70% by mass or less, even more preferably 60% by mass or less, based on 100% by mass of the non-volatile components of the core resin composition. When the amount of component (A-1) is within the above range, the transmission loss of the optical waveguide can be effectively suppressed, and furthermore, the resolution of the core resin composition and the mechanical strength and heat resistance of the cured product of the core resin composition can be particularly improved.

[0070] -Component (A-2): Compound having a structure represented by formula (A-2)- The component (A-2) is a compound having a structure represented by the following formula (A-2): The component (A-2) may be used alone or in combination of two or more types.

[0071] [ka]

[0072] (In formula (A-2), R 2 represents a divalent group represented by the following formula (r-1), a divalent group represented by the following formula (r-2), a divalent group represented by the following formula (r-3), or a divalent group consisting of a combination thereof; X 2 and X 3 each independently represents an alkyl group which may have a substituent, an aryl group which may have a substituent, a halogen atom, or a monovalent heterocyclic group which may have a substituent. n2 and n3 each independently represent an integer of 0 to 4.

[0073] [ka]

[0074] (In formula (r-1), R 11 and R 12each independently represents a hydrogen atom, an optionally substituted alkyl group, an optionally substituted aryl group, an optionally substituted monovalent heterocyclic group, an amino group, a carbonyl group, a carboxyl group, or a group consisting of a combination thereof; R 11 and R 12 may be bonded to each other to form a ring. * represents a bond. In formula (r-2), X 11 each independently represents an alkyl group which may have a substituent, p1 represents an integer of 0 to 4, and * represents a bond. In formula (r-3), X 12 and X 13 each independently represents an alkyl group which may have a substituent; p2 and p3 each independently represent an integer of 0 to 4; * represents a bond.

[0075] In formula (A-2), R 2 represents a divalent group represented by formula (r-1), a divalent group represented by formula (r-2), a divalent group represented by formula (r-3), or a divalent group consisting of a combination thereof. The divalent group represented by formula (r-1) is as described above.

[0076] X in formulas (r-2) to (r-3) 11 , X 12 , and X 13 Each of X independently represents an alkyl group which may have a substituent. 11 ~X 13 is X in formula (A-1) 1 The alkyl group may be the same as the alkyl group which may have a substituent represented by the formula (1).

[0077] In the formulae (r-2) to (r-3), p1, p2, and p3 each independently represent an integer of 0 to 4, preferably an integer of 0 to 3, and more preferably 0 or 1.

[0078] Specific examples of the divalent group represented by formula (r-2) include the following groups: In the formula, "*" represents a bond.

[0079] [ka]

[0080] Specific examples of the divalent group represented by formula (r-3) include the following groups: In the formula, "*" represents a bond.

[0081] [ka]

[0082] Specific examples of the divalent group formed by combining a divalent group represented by formula (r-2) with a divalent group represented by formula (r-3), the divalent group formed by combining a divalent group represented by formula (r-1) with a divalent group represented by formula (r-2), and the divalent group formed by combining a divalent group represented by formula (r-1) with a divalent group represented by formula (r-3) include the following groups, in which "*" represents a bond.

[0083] [ka]

[0084] In formula (A-2), the OH group of the phenol moiety is R 2 With respect to the above, it is preferably bonded to any one of the ortho-, meta-, and para-positions, more preferably bonded to any one of the meta- and para-positions, and particularly preferably bonded to the para-position.

[0085] In formula (A-2), X 2 and X 3 each independently represents an alkyl group which may have a substituent, an aryl group which may have a substituent, a halogen atom, or a monovalent heterocyclic group which may have a substituent. 2 and X 3 Each independently represents X in formula (A-1). 1 It can be similar to:

[0086] In formula (A-2), n2 and n3 each independently represent an integer of 0 to 4 and can be the same as n1 in formula (A-1).

[0087] Specific examples of the component (A-2) include the following groups.

[0088] [ka]

[0089] [ka]

[0090] [ka]

[0091] [ka]

[0092] [ka]

[0093] [ka]

[0094] [ka]

[0095] [ka]

[0096] [ka]

[0097] [ka]

[0098] The component (A-2) may be a commercially available product. Specific examples of commercially available components (A-2) include: “BisP-E”, “Bis-AF” manufactured by Asahi Yokuzai; “BisE”, “BisP-TMC” manufactured by Honshu Kagaku; “BisA”, “BisF”, “BisP-M” manufactured by Mitsui Chemicals Fine; “BisP-AP”, “Bis” manufactured by Honshu Chemical P-MIBK", "BisP-B", "Bis-Z", "BisP-CP", "o,o'-BPF", "BisP-IOTD", "BisP-IBTD", "BisP-DED", "BisP-BA"; "BisP-BA" manufactured by Honshu Kagaku Co., Ltd. -C", "Bis26X-A", "BisOPP-A", "BisOTBP-A", "BisOCHP-A", "BisOFP-A", "BisOC-Z", "BisOC-FL", "BisOC-CP", "BisOCHP -Z", "methylenebisP-CR", "TM-BPF", "BisOC-F", "Bis3M6B-IBTD", "BisOC-IST", "BisP-IST", "BisP-PRM", "BisP-LV", etc.

[0099] The amount of the (A-2) component is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, relative to 100% by mass of the total (A) phenolic resin, and is preferably 60% by mass or less, more preferably 50% by mass or less, and even more preferably 40% by mass or less. When the amount of the (A-2) component is within the above range, the transmission loss of the optical waveguide can be effectively suppressed, and furthermore, the resolution of the core resin composition and the mechanical strength and heat resistance of the cured product of the core resin composition can be particularly improved.

[0100] The amount of component (A-2) is preferably 1% by mass or more, more preferably 3% by mass or more, and even more preferably 5% by mass or more, and is preferably 40% by mass or less, more preferably 30% by mass or less, and even more preferably 25% by mass or less, based on 100% by mass of the non-volatile components of the core resin composition. When the amount of component (A-2) is within the above range, the transmission loss of the optical waveguide can be effectively suppressed, and furthermore, the resolution of the core resin composition and the mechanical strength and heat resistance of the cured product of the core resin composition can be particularly improved.

[0101] When the mass of the (A-1) component relative to 100% by mass of the (A) phenolic resin is Wa1, and the mass of the (A-2) component relative to 100% by mass of the (A) phenolic resin is Wa2, the mass ratio Wa2 / Wa1 is preferably in a specific range. Specifically, the mass ratio Wa2 / Wa1 is preferably 0.01 or more, more preferably 0.05 or more, more preferably 0.1 or more, and preferably 4 or less, more preferably 2 or less, and even more preferably 1 or less. When the mass ratio Wa2 / Wa1 is in the above range, the transmission loss of the optical waveguide can be effectively suppressed, and furthermore, the resolution of the core resin composition, and the mechanical strength and heat resistance of the cured product of the core resin composition can be particularly improved.

[0102] -Component (A-3): Compound having a structure represented by formula (A-3)- The component (A-3) is a compound having a structure represented by the following formula (A-3): The component (A-3) may be used alone or in combination of two or more types.

[0103] [ka]

[0104] (In formula (A-3), R 3 represents a divalent group represented by the formula (r-1), a divalent group represented by the formula (r-2), a divalent group represented by the formula (r-3), or a divalent group consisting of a combination thereof; X 4 and X 5each independently represents an alkyl group which may have a substituent, an aryl group which may have a substituent, a halogen atom, or a monovalent heterocyclic group which may have a substituent. n4 and n5 each independently represent an integer of 0 to 3.

[0105] In formula (A-3), R 3 represents a divalent group represented by formula (r-1), a divalent group represented by formula (r-2), a divalent group represented by formula (r-3), or a divalent group consisting of a combination thereof. The divalent group represented by formula (r-1), the divalent group represented by formula (r-2), the divalent group represented by formula (r-3), and the divalent group consisting of a combination thereof are as described above.

[0106] In formula (A-3), the OH group of the phenol moiety is R 3 Preferably, the bond is at any one of the ortho, meta, and para positions relative to the above, more preferably at any one of the meta and para positions, and particularly preferably at the para position.

[0107] In formula (A-3), X 4 and X 5 each independently represents an alkyl group which may have a substituent, an aryl group which may have a substituent, a halogen atom, or a monovalent heterocyclic group which may have a substituent. 4 and X 5 Each independently represents X in formula (A-1). 1 It can be similar to:

[0108] In formula (A-3), n4 and n5 each independently represent an integer of 0 to 3. It is more preferable that n4 and n5 each independently represent 0 or 1, and 0 is particularly preferable.

[0109] Specific examples of the component (A-3) include the following groups.

[0110] [ka]

[0111] The component (A-3) may be a commercially available product. A specific example of a commercially available component (A-3) is "TBIS-RX" manufactured by Taoka Chemical Co., Ltd.

[0112] The amount of the (A-3) component is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, relative to 100% by mass of the total (A) phenolic resin, and is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less. When the amount of the (A-3) component is within the above range, the transmission loss of the optical waveguide can be effectively suppressed, and furthermore, the resolution of the core resin composition and the mechanical strength and heat resistance of the cured product of the core resin composition can be particularly improved.

[0113] The amount of component (A-3) is preferably 1% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more, and is preferably 40% by mass or less, more preferably 30% by mass or less, and even more preferably 20% by mass or less, based on 100% by mass of the non-volatile components of the core resin composition. When the amount of component (A-3) is within the above range, the transmission loss of the optical waveguide can be effectively suppressed, and furthermore, the resolution of the core resin composition and the mechanical strength and heat resistance of the cured product of the core resin composition can be particularly improved.

[0114] -Component (A-4): Compound other than components (A-1) to (A-3)- As the (A) phenolic resin, a compound other than the components (A-1) to (A-3) may be used. As the (A) phenolic resin (hereinafter sometimes referred to as "component (A-4)") other than the components (A-1) to (A-3), for example, "Marukalinker M" (polyparahydroxystyrene) manufactured by Maruzen Chemical Co., Ltd., "SPDI" manufactured by JFE Chemical Corporation, and the like can be mentioned.

[0115] The weight average molecular weight of the (A) phenolic resin is not particularly limited. In terms of a preferred range, the weight average molecular weight of the (A) phenolic resin is preferably 150 or more, more preferably 160 or more, particularly preferably 170 or more, and is preferably less than 15,000, more preferably 14,000 or less, particularly preferably 13,000 or less, and may be less than 2,500. The weight average molecular weight can be measured as a polystyrene-equivalent value by gel permeation chromatography (GPC).

[0116] The phenolic hydroxyl group equivalent of the (A) phenolic resin is preferably 50 g / eq or more, more preferably 100 g / eq or more, and is preferably less than 3000 g / eq, more preferably 1000 g / eq or less, even more preferably 500 g / eq or less, and particularly preferably 300 g / eq or less. The phenolic hydroxyl group equivalent of the (A) phenolic resin refers to the mass of the (A) phenolic resin per equivalent of a phenolic hydroxyl group.

[0117] Refractive index n of the cured product of the core resin composition core can be adjusted, for example, by the composition of the (A) phenolic resin. Usually, when a large amount of the (A) phenolic resin having a low refractive index is used, the refractive index n core When a large amount of the phenolic resin (A) having a high refractive index is used, the refractive index n core can be increased. The specific refractive index of the (A) phenolic resin can be calculated by the Lorentz-Lorenz equation. Therefore, the type and amount of the (A) phenolic resin may be selected based on the refractive index of the (A) phenolic resin derived based on the Lorentz-Lorenz equation. For the Lorentz-Lorenz equation, for example, "Refractive index control of optical polymers: Theoretical prediction and molecular design method" (Ando Shinji, "Optics" Vol. 44, No. 8, 2015, pp. 298-303) and "Optical properties and high performance of transparent polymers" (Tanio Yoshihisa, "Industrial Materials" March 2021 issue, pp. 16-18) may be referred to. For example, according to a phenolic resin containing fluorine atoms, the refractive index n of the cured product is coreIn the following description, a phenolic resin containing fluorine atoms may be referred to as a "fluorine-based phenolic resin."

[0118] The (A) phenolic resin of the core resin composition preferably contains one or more phenolic resins that are the same as those contained in the clad resin composition. That is, it is preferable that one or more phenolic resins are contained in both the core resin composition and the clad resin composition. When the core resin composition and the clad resin composition contain a common phenolic resin in this way, the affinity between the core layer and the clad layer can be increased. Therefore, the smoothness of the interface between the core layer and the clad layer can be improved, so that attenuation of light due to scattering at the interface can be effectively suppressed, and therefore, transmission loss can be effectively suppressed. In addition, the adhesion of the interface between the core layer and the clad layer can be increased, so that the mechanical strength and heat resistance of the optical waveguide can be improved. Furthermore, usually, the thermal expansion coefficient of the core layer and the thermal expansion coefficient of the clad layer can be made close to each other, so that deformation of the optical waveguide due to thermal changes can be suppressed.

[0119] The phenolic resin commonly contained in both the core resin composition and the cladding resin composition is sometimes referred to as a "common phenolic resin". The range of the amount of the common phenolic resin contained in the (A) phenolic resin relative to 100% by mass of the total (A) phenolic resin of the core resin composition is preferably 40% by mass or more, more preferably 50% by mass or more, particularly preferably 60% by mass or more, and usually 100% by mass or less, preferably 99% by mass or less, more preferably 97% by mass or less, particularly preferably 95% by mass or less. When the amount of the common phenolic resin is within the above range, the transmission loss of the optical waveguide can be effectively suppressed, and furthermore, usually, the mechanical strength and heat resistance of the cured product of the core resin composition can be particularly improved.

[0120] The amount of the (A) phenolic resin is preferably 40% by mass or more, more preferably 50% by mass or more, and even more preferably 60% by mass or more, and is preferably 90% by mass or less, more preferably 80% by mass or less, and may be 70% by mass or less, based on 100% by mass of the non-volatile components of the core resin composition. When the amount of the (A) phenolic resin is within the above range, the transmission loss of the optical waveguide can be effectively suppressed, and furthermore, the resolution of the core resin composition and the mechanical strength and heat resistance of the cured product of the core resin composition can be particularly improved.

[0121] [2.2.(B) Photoacid generator] The core resin composition contains a photoacid generator (B) as component (B). The photoacid generator (B) generates an acid when irradiated with active light such as ultraviolet light, and the generated acid can promote the crosslinking reaction of the crosslinking agent (C). Therefore, the solubility of the core resin composition in a developer can be effectively reduced by exposure to light, so that the formation of a negative pattern by exposure can be effectively promoted. The photoacid generator (B) may be used alone or in combination of two or more kinds.

[0122] As the photoacid generator, a compound that generates an acid by irradiation with active light can be used. Examples of the photoacid generator include a halogen-containing compound, an onium salt compound, a diazoketone compound, a sulfone compound, a sulfonic acid compound, a sulfonimide compound, a diazomethane compound, and an oxime ester compound. Among them, an oxime ester compound is preferable.

[0123] Examples of halogen-containing compounds that can be suitably used as photoacid generators include haloalkyl group-containing hydrocarbon compounds, haloalkyl group-containing heterocyclic compounds, etc. Specific examples of suitable halogen-containing compounds include 2-[2-(furan-2-yl)ethenyl]-4,6-bis(trichloromethyl)-s-triazine, 2-[2-(5-methylfuran-2-yl)ethenyl]-4,6-bis(trichloromethyl)-s-triazine, 2-(methoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine, 2-[2-(4-methoxyphenyl)ethenyl]-4,6-bis(trichloromethyl)-s-triazine, 2-[2-(3,4-dimethoxyphenyl)ethenyl]-4,6-bis(trichloromethyl)-s-triazine, Examples of the s-triazine derivatives include phenyl-bis(trichloromethyl)-s-triazine, 1,10-dibromo-n-decane, 1,1-bis(4-chlorophenyl)-2,2,2-trichloroethane, phenyl-bis(trichloromethyl)-s-triazine, 4-methoxyphenyl-bis(trichloromethyl)-s-triazine, styryl-bis(trichloromethyl)-s-triazine, and naphthyl-bis(trichloromethyl)-s-triazine. The halogen-containing compound may be a commercially available product, and examples of the commercially available product include "TFE-triazine", "TME-triazine", "MP-triazine", "MOP-triazine", and "dimethoxytriazine" (a halogen-containing compound-based photoacid generator having a triazine skeleton) manufactured by Sanwa Chemical Co., Ltd.

[0124] Examples of onium salt compounds that can be suitably used as photoacid generators include iodonium salts, sulfonium salts, phosphonium salts, diazonium salts, and pyridinium salts. Specific preferred examples of the onium salt compound include tris(4-methylphenyl)sulfonium trifluoromethanesulfonate, tris(4-methylphenyl)sulfonium hexafluorophosphonate, diphenyliodonium trifluoromethanesulfonate, diphenyliodonium p-toluenesulfonate, diphenyliodonium hexafluoroantimonate, diphenyliodonium hexafluorophosphate, diphenyliodonium tetrafluoroborate, triphenylsulfonium trifluoromethanesulfonate, triphenylsulfonium p-toluenesulfonate, triphenylsulfonium hexafluoroantimonate, 4-tert-butylphenyl diphenylsulfonium trifluoromethanesulfonate, 4-tert-butylphenyl diphenylsulfonium p-toluenesulfonate, 4,7-di-n-butoxynaphthyl tetrahydrothiophenium trifluoromethanesulfonate, and the like. Commercially available onium salt compounds can be used, and examples of commercially available products include "TS-01" and "TS-91" manufactured by Sanwa Chemical Co., Ltd.; "CPI-110A", "CPI-210S", "HS-1", "LW-S1", "IK-1", and "CPI-310B" manufactured by San-Apro Co., Ltd.; and "SI-110L", "SI-180L", and "SI-100L" manufactured by Sanshin Chemical Industry Co., Ltd.

[0125] Examples of diazoketone compounds that can be suitably used as a photoacid generator include 1,3-diketo-2-diazo compounds, diazobenzoquinone compounds, diazonaphthoquinone compounds, etc. Specific examples of suitable diazoketone compounds include 1,2-naphthoquinonediazide-4-sulfonic acid ester compounds of phenols, etc.

[0126] Examples of sulfone compounds that can be suitably used as photoacid generators include β-ketosulfone compounds, β-sulfonylsulfone compounds, and α-diazo compounds of these compounds, etc. Specific examples of suitable sulfone compounds include 4-trisphenacylsulfone, mesitylphenacylsulfone, bis(phenacylsulfonyl)methane, etc.

[0127] Examples of sulfonic acid compounds that can be suitably used as photoacid generators include alkylsulfonates, haloalkylsulfonates, arylsulfonates, iminosulfonates, etc. Specific examples of suitable sulfonic acid compounds include benzoin tosylate, pyrogallol tristrifluoromethanesulfonate, o-nitrobenzyl trifluoromethanesulfonate, o-nitrobenzyl p-toluenesulfonate, etc.

[0128] Specific examples of sulfonimide compounds that can be suitably used as a photoacid generator include N-(trifluoromethylsulfonyloxy)succinimide, N-(trifluoromethylsulfonyloxy)phthalimide, N-(trifluoromethylsulfonyloxy)diphenylmaleimide, N-(trifluoromethylsulfonyloxy)bicyclo[2.2.1]hept-5-ene-2,3-dicarboximide, and N-(trifluoromethylsulfonyloxy)naphthylimide.

[0129] Specific examples of diazomethane compounds that can be suitably used as a photoacid generator include bis(trifluoromethylsulfonyl)diazomethane, bis(cyclohexylsulfonyl)diazomethane, bis(phenylsulfonyl)diazomethane, etc. Commercially available diazomethane compounds can be used.

[0130] Specific examples of oxime ester compounds that can be suitably used as photoacid generators include benzeneacetonitrile, 2-methyl-α-[2-[[(propylsulfonyl)oxy]imino]-3(2H)-thienylidene], benzeneacetonitrile, 2-methyl-α-[2-[[[(4-methylphenyl)sulfonyl]oxy]imino]-3(2H)-thienylidene], etc. Commercially available products include, for example, "PAG103", "PAG121", "PAG169", "PAG203", etc. manufactured by BASF.

[0131] From the viewpoint of increasing the affinity between the core layer and the clad layer, it is preferable that the (B) photoacid generator of the core resin composition contains one or more photoacid generators that are the same as those contained in the clad resin composition. That is, it is preferable that one or more photoacid generators are contained in both the core resin composition and the clad resin composition. A photoacid generator that is commonly contained in both the core resin composition and the clad resin composition is sometimes called a "common photoacid generator". The range of the amount of the common photoacid generator contained in the (B) photoacid generator relative to 100% by mass of the total (B) photoacid generator of the core resin composition is preferably 80% by mass or more, more preferably 90% by mass or more, and particularly preferably 100% by mass.

[0132] The amount of (B) photoacid generator is preferably in the range of 0.01 mass% or more, more preferably 0.05 mass% or more, and even more preferably 0.1 mass% or more, relative to 100 mass% of nonvolatile components in the core resin composition as the photosensitive resin composition, and is preferably 3 mass% or less, more preferably 2 mass% or less, and particularly preferably 1.5 mass% or less.

[0133] [2.3.(C) Crosslinking Agent] The core resin composition contains a (C) crosslinking agent as component (C). The (C) crosslinking agent is capable of generating a crosslinking reaction. The crosslinking reaction of the (C) crosslinking agent makes the core resin composition insoluble in a developer, or hardens the composition to form a core layer. However, the (C) crosslinking agent does not include those that fall under the category of (A) phenolic resin.

[0134] As the (C) crosslinking agent, an amino resin is preferred. When the amino resin is combined with the (A) phenolic resin, a photosensitive resin composition having excellent photosensitivity can be obtained. Therefore, it is possible to improve the photosensitivity of the core resin composition.

[0135] In addition, the (C) crosslinking agent is preferably one capable of crosslinking with the (A) phenolic resin. Examples of the (C) crosslinking agent capable of crosslinking with the (A) phenolic resin include compounds containing an alkoxymethyl group in the molecule. The alkoxymethyl group is a group represented by the following formula (C-1). In formula (C-1), "*" represents a bond.

[0136] [ka]

[0137] In formula (C-1), R 21 represents an alkyl group which may have a substituent. The alkyl group may be a straight-chain, branched-chain, or cyclic alkyl group. The cyclic alkyl group may be either a monocyclic or polycyclic alkyl group. The alkyl group is preferably an alkyl group having 1 to 10 carbon atoms, more preferably an alkyl group having 1 to 6 carbon atoms, and even more preferably an alkyl group having 1 to 4 carbon atoms. Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, an isopropyl group, a s-butyl group, and a t-butyl group. Among them, a methyl group and a butyl group are preferable, and a methyl group is more preferable. R 21 The alkyl group represented by may have a substituent.

[0138] The alkoxymethyl group is preferably contained in an alkoxymethylamino group represented by the following formula (C-1'). Therefore, the (C) crosslinking agent preferably contains an alkoxymethylamino group represented by formula (C-1'), and more preferably contains two or more alkoxymethylamino groups represented by formula (C-1') in the molecule. In the formula, "*" represents a bond.

[0139] [ka]

[0140] In formula (C-1'), R 22 is R in formula (C-1). 21 R represents a hydrogen atom or an alkoxymethyl group.

[0141] As the (C) crosslinking agent, an amino resin containing two or more alkoxymethyl groups in the molecule is particularly preferred. Examples of the amino resin containing two or more alkoxymethyl groups in the molecule include melamine resin and urea resin, and melamine resin is preferred.

[0142] As the melamine resin, for example, a melamine resin having a structure represented by the following formula (C-2) is preferable.

[0143] [ka]

[0144] In formula (C-2), X 21 , X 22 , X 23 and X 24 R each independently represents a hydrogen atom or an alkoxymethyl group. 50 represents a hydrogen atom, an amino group, an alkyl group which may have a substituent, an aryl group which may have a substituent, or an alkoxymethylamino group represented by formula (C-1'). 50 When represents a hydrogen atom, an optionally substituted alkyl group, or an optionally substituted aryl group, X21 , X 22 , X 23 , and X 24 At least two of the groups are alkoxymethyl groups.

[0145] X 21 ~X 24 The alkoxymethyl group represented by R may be the same as the group represented by formula (C-1). 50 When represents a hydrogen atom, an optionally substituted alkyl group, or an optionally substituted aryl group, X 21 ~X 24 At least two of R are alkoxymethyl groups. 50 represents a hydrogen atom, an amino group, an optionally substituted alkyl group, or an optionally substituted aryl group, X 21 ~X 24 At least two of X are alkoxymethyl groups. 21 ~X 24 At least three of X are preferably alkoxymethyl groups. 21 ~X 24 It is more preferable that at least four of these groups are alkoxymethyl groups.

[0146] R 50 R represents a hydrogen atom, an amino group, an alkyl group which may have a substituent, an aryl group which may have a substituent, or an alkoxymethylamino group represented by the formula (C-1'). 50 R is preferably an aryl group which may have a substituent, or an alkoxymethylamino group represented by formula (C-1'), and more preferably an alkoxymethylamino group represented by formula (C-1'). 50 The alkyl group which may have a substituent represented by X in formula (A-1) is 1 The alkyl group may be the same as the alkyl group which may have a substituent represented by R 50 The optionally substituted aryl group represented by X in formula (A-1) is 1 The aryl group may be the same as the optionally substituted aryl group represented by the formula (1).

[0147] The melamine resin having the structure represented by formula (C-2) is preferably a melamine resin having a structure represented by formula (C-2').

[0148] [ka]

[0149] In formula (C-2'), X 25 , X 26 , X 27 , X 28 , X 29 and X 30 each independently represents a hydrogen atom or an alkoxymethyl group. 25 , X 26 , X 27 , X 28 , X 29 and X 30 At least two of the groups are alkoxymethyl groups.

[0150] X 25 ~X 30 The alkoxymethyl group represented by formula (C-1) may be the same as the group represented by formula (C-2). 25 ~X 30 At least two of X are alkoxymethyl groups; 25 ~X 30 At least three of X are preferably alkoxymethyl groups. 25 ~X 30 More preferably, at least four of X are alkoxymethyl groups. 25 ~X 30 It is more preferable that all of the groups are alkoxymethyl groups.

[0151] Specific examples of the melamine resin include the following melamine resins.

[0152] [ka]

[0153] The melamine resin may be a commercially available product, such as "MW-390", "MW-100LM", or "MX-750LM" manufactured by Sanwa Chemical Co., Ltd.; or the Cymel series manufactured by Allnex Japan Co., Ltd.

[0154] The urea resin is preferably, for example, a urea resin having either a structure represented by the following formula (C-3) or a structure represented by the following formula (C-4).

[0155] [ka]

[0156] In formula (C-3), X 31 , X 32 , X 33 and X 34 each independently represents a hydrogen atom or an alkoxymethyl group. 31 , X 32 , X 33 and X 34 At least two of X are alkoxymethyl groups. 31 ~X 34 At least three of X are preferably alkoxymethyl groups. 31 ~X 34 It is more preferable that at least four of these groups are alkoxymethyl groups. In formula (C-4), X 35 , and X 36 represents an alkoxymethyl group. X 31 ~X 36 The alkoxymethyl group represented by formula (C-1) can be the same as the group represented by formula (C-1).

[0157] The urea resin may be a commercially available product, such as "MX-270", "MX-279", and "MX-280" manufactured by Sanwa Chemical Co., Ltd., or the Cymel series manufactured by Allnex Japan Co., Ltd.

[0158] The crosslinking agent (C) may be used alone or in combination of two or more kinds.

[0159] The weight average molecular weight of the (C) crosslinking agent is not particularly limited. In terms of a preferred range, the weight average molecular weight of the (C) crosslinking agent is preferably 150 or more, more preferably 160 or more, particularly preferably 170 or more, and is preferably less than 15,000, more preferably 14,000 or less, particularly preferably 13,000 or less, and may be less than 2,500.

[0160] The (C) crosslinking agent may contain a crosslinkable group such as an alkoxymethyl group as a group capable of causing a crosslinking reaction. The crosslinkable group equivalent of the (C) crosslinking agent is preferably 50 g / eq. or more, more preferably 100 g / eq. or more, and is preferably less than 3000 g / eq., more preferably 1000 g / eq. or less, even more preferably 500 g / eq. or less, and particularly preferably 300 g / eq. or less. The crosslinkable group equivalent of the (C) crosslinking agent refers to the mass of the (C) crosslinking agent per equivalent of the crosslinkable group.

[0161] From the viewpoint of increasing the affinity between the core layer and the clad layer, it is preferable that the (C) crosslinking agent of the core resin composition contains one or more crosslinking agents that are the same as those contained in the clad resin composition. That is, it is preferable that one or more crosslinking agents are contained in both the core resin composition and the clad resin composition. A crosslinking agent that is commonly contained in both the core resin composition and the clad resin composition is sometimes called a "common crosslinking agent". The range of the amount of the common crosslinking agent contained in the (C) crosslinking agent relative to 100% by mass of the total (C) crosslinking agent of the core resin composition is preferably 80% by mass or more, more preferably 90% by mass or more, and particularly preferably 100% by mass.

[0162] The amount of (C) crosslinking agent is preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 20% by mass or more, and is preferably 40% by mass or less, more preferably 35% by mass or less, and particularly preferably 30% by mass or less, based on 100% by mass of the non-volatile components of the core resin composition. When the amount of (C) crosslinking agent is within the above range, the transmission loss of the optical waveguide can be effectively suppressed, and furthermore, the resolution of the core resin composition and the mechanical strength and heat resistance of the cured product of the core resin composition can be particularly improved.

[0163] [2.4.(D) Polymers] The core resin composition may further contain a (D) polymer as an optional component in combination with the above-mentioned (A) to (C) components. The (D) polymer as the (D) component usually has a weight average molecular weight of 2,500 or more. In detail, the range of the weight average molecular weight of the (D) polymer is usually 2,500 or more, more preferably 5,000 or more, particularly preferably 10,000 or more, and preferably 100,000 or less, more preferably 80,000 or less, and even more preferably 60,000 or less. When the core resin composition contains the (D) polymer, the smoothness of the surface of the core layer can be improved, and the smoothness of the interface between the core layer and the clad layer can be improved, so that the transmission loss of the optical waveguide can be effectively reduced. Furthermore, the core resin composition can usually be easily coated and the toughness of the core layer can be increased. Furthermore, the (D) polymer usually effectively increases the heat resistance and flexibility of the core layer, and effectively suppresses the transmission loss by increasing the transparency of the core layer. However, the (D) polymer does not include those that fall under the above-mentioned (A) to (C) components.

[0164] The (D) polymer may be a homopolymer or a copolymer. Examples of the (D) polymer include acrylic resins, phenoxy resins, polyvinyl acetal resins, polyolefin resins, polybutadiene resins, polyimide resins, polyamideimide resins, polyetherimide resins, polysulfone resins, polyethersulfone resins, polyphenylene ether resins, polycarbonate resins, polyetheretherketone resins, and polyester resins. Among these, acrylic resins are preferred.

[0165] The acrylic resin may be a polymer containing a repeating unit having a structure formed by polymerizing an acrylic monomer such as acrylic acid, acrylate, methacrylic acid, or methacrylate, and may be produced, for example, by polymerizing an acrylic monomer. The acrylic resin may be a homopolymer of an acrylic monomer, a copolymer of two or more kinds of acrylic monomers, or a copolymer of an acrylic monomer and any monomer other than an acrylic monomer. When an acrylic resin is used as the (D) polymer, the heat resistance and flexibility of the core layer can be effectively increased, and the transparency of the core layer can be increased to effectively suppress the transmission loss of the optical waveguide. Specific examples of the acrylic resin include "Alphon" (registered trademark) manufactured by Toa Gosei Co., Ltd., "ART CURE" manufactured by Negami Chemical Industries, Ltd., and "Actflow" manufactured by Soken Chemical Industries, Ltd.

[0166] Examples of the phenoxy resin include phenoxy resins having one or more skeletons selected from the group consisting of bisphenol A skeleton, bisphenol F skeleton, bisphenol S skeleton, bisphenolacetophenone skeleton, novolac skeleton, biphenyl skeleton, fluorene skeleton, dicyclopentadiene skeleton, norbornene skeleton, naphthalene skeleton, anthracene skeleton, adamantane skeleton, terpene skeleton, and trimethylcyclohexane skeleton. The terminal of the phenoxy resin may be any functional group such as a phenolic hydroxyl group or an epoxy group. Specific examples of phenoxy resins include "1256" and "4250" (both of which are phenoxy resins containing a bisphenol A skeleton), "YX8100" (phenoxy resin containing a bisphenol S skeleton), "YX6954" (phenoxy resin containing a bisphenol acetophenone skeleton), "YX7553", "YL6794", "YL7213", "YL7290", and "YL7482" manufactured by Mitsubishi Chemical Corporation; and "FX280" and "FX293" manufactured by Nippon Steel Chemical & Material Co., Ltd.

[0167] Examples of polyvinyl acetal resin include polyvinyl formal resin and polyvinyl butyral resin, and polyvinyl butyral resin is preferred.Specific examples of polyvinyl acetal resin include "Denka Butyral 4000-2", "Denka Butyral 5000-A", "Denka Butyral 6000-C", and "Denka Butyral 6000-EP" manufactured by Denka Co., Ltd.; and S-LEC BH series, BX series, KS series, BL series, and BM series manufactured by Sekisui Chemical Co., Ltd.

[0168] Specific examples of polyimide resins include "Rikacoat SN20" and "Rikacoat PN20" manufactured by New Japan Chemical Co., Ltd. Specific examples of polyimide resins also include modified polyimides such as linear polyimides obtained by reacting bifunctional hydroxyl-terminated polybutadiene, a diisocyanate compound, and a tetrabasic acid anhydride (disclosed in JP-A-2006-37083), and polysiloxane skeleton-containing polyimides (disclosed in JP-A-2002-12667 and JP-A-2000-319386, etc.).

[0169] Specific examples of polyamide-imide resins include "Viromax HR11NN" and "Viromax HR16NN" manufactured by Toyobo Co., Ltd. Specific examples of polyamide-imide resins also include modified polyamide-imides such as polysiloxane skeleton-containing polyamide-imides "KS9100" and "KS9300" manufactured by Hitachi Chemical Co., Ltd.

[0170] A specific example of the polyethersulfone resin is "PES5003P" manufactured by Sumitomo Chemical Co., Ltd.

[0171] Specific examples of polysulfone resins include polysulfones "P1700" and "P3500" manufactured by Solvay Advanced Polymers.

[0172] The (D) polymer may be used alone or in combination of two or more kinds.

[0173] It is preferable that the (D) polymer does not contain a functional group capable of reacting with a phenolic hydroxyl group or a crosslinkable group to form a bond. Even if the (D) polymer contains a functional group, it is preferable that the functional group is few. Therefore, it is preferable that the functional group equivalent of the (D) polymer is large. The functional group equivalent of the (D) polymer indicates the mass of the (D) polymer per equivalent of the functional group. Specifically, the functional group equivalent of the (D) polymer is preferably 3000 g / eq. or more, more preferably 4000 g / eq. or more, and particularly preferably 5000 g / eq. or more. In addition, the range of the phenolic hydroxyl group equivalent of the (D) polymer may be the same as the range of the functional group equivalent of the (D) polymer. The phenolic hydroxyl group equivalent of the (D) polymer indicates the mass of the (D) polymer per equivalent of the phenolic hydroxyl group. Furthermore, the range of the crosslinkable group equivalent of the (D) polymer may be the same as the range of the functional group equivalent of the (D) polymer. The crosslinkable group equivalent of the (D) polymer refers to the mass of the (D) polymer per equivalent of the crosslinkable group. In particular, the (D) polymer preferably does not have a functional group, and therefore preferably does not have a phenolic hydroxyl group and preferably does not have a crosslinkable group.

[0174] From the viewpoint of increasing the affinity between the core layer and the clad layer, the (D) polymer of the core resin composition preferably contains one or more polymers that are the same as those contained in the clad resin composition. That is, it is preferable that one or more polymers are contained in both the core resin composition and the clad resin composition. A polymer that is commonly contained in both the core resin composition and the clad resin composition may be called a "common polymer". The amount of the common polymer contained in the (D) polymer is preferably 80% by mass or more, more preferably 90% by mass or more, and particularly preferably 100% by mass, based on 100% by mass of the total (D) polymer of the core resin composition.

[0175] The amount of the (D) polymer may be in the range of 0% by mass or more than 0% by mass, and is preferably 1% by mass or more, more preferably 2% by mass or more, and particularly preferably 5% by mass or more, and is preferably 30% by mass or less, more preferably 20% by mass or less, and particularly preferably 10% by mass or less, relative to 100% by mass of the non-volatile components of the core resin composition.

[0176] [2.5.(E) Amine compounds] The core resin composition may further contain (E) a compound represented by the following formula (E-1) as an optional component in combination with the above-mentioned (A) to (D) components. The compound represented by (E) formula (E-1) as the (E) component may be hereinafter referred to as "(E) amine-based compound". The (E) amine-based compound functions as a quencher in the core resin composition and can suppress the diffusion speed of the acid generated by the (B) photoacid generator in the resin composition. Thus, the (E) amine-based compound can improve the resolution of the core resin composition. However, the (E) amine-based compound does not include those corresponding to the above-mentioned (A) to (D) components.

[0177] [ka]

[0178] In formula (E-1), R e1 , R e2 and R e3 are each independently a hydrogen atom or a hydrocarbon group. The hydrocarbon group may be an aliphatic hydrocarbon group or an aromatic hydrocarbon group. The aliphatic hydrocarbon group may be a saturated aliphatic hydrocarbon group or an unsaturated aliphatic hydrocarbon group. The hydrocarbon group may contain a ring. Thus, the aliphatic hydrocarbon group may be an alicyclic hydrocarbon group. The number of carbon atoms in the hydrocarbon group is usually 1 or more, preferably 2 or more, particularly preferably 5 or more, and preferably 20 or less, more preferably 18 or less, particularly preferably 12 or less. Examples of the hydrocarbon group include alkyl groups such as methyl, ethyl, hexyl, octyl, and decyl groups; cycloalkyl groups such as cyclopentyl and cyclohexyl groups; aryl groups such as phenyl and naphthyl groups; and groups formed by combining these groups. In addition, R e1 and R e2 may be bonded to form a ring.

[0179] Examples of the (E) amine compound include ammonia, primary aliphatic amine compounds, secondary aliphatic amine compounds, tertiary aliphatic amine compounds, aromatic amine compounds, and the like.

[0180] Examples of primary aliphatic amine compounds include methylamine, ethylamine, n-propylamine, isopropylamine, n-butylamine, isobutylamine, sec-butylamine, tert-butylamine, pentylamine, tert-pentylamine, cyclopentylamine, hexylamine, cyclohexylamine, heptylamine, octylamine, nonylamine, decylamine, dodecylamine, and cetylamine.

[0181] Examples of secondary aliphatic amine compounds include dimethylamine, diethylamine, di-n-propylamine, diisopropylamine, di-n-butylamine, diisobutylamine, di-sec-butylamine, dipentylamine, dicyclopentylamine, dihexylamine, dicyclohexylamine, diheptylamine, dioctylamine, dinonylamine, didecylamine, didodecylamine, dicetylamine, and pyrrolidine.

[0182] Examples of tertiary aliphatic amine compounds include trimethylamine, triethylamine, tri-n-propylamine, triisopropylamine, tri-n-butylamine, triisobutylamine, tri-sec-butylamine, tripentylamine, tricyclopentylamine, trihexylamine, tricyclohexylamine, triheptylamine, trioctylamine, trinonylamine, tridecylamine, tridodecylamine, tricetylamine, dimethylethylamine, and methylethylpropylamine.

[0183] Examples of the aromatic amine compound include benzylamine, phenethylamine, benzyldimethylamine, diphenyl(p-tolyl)amine, methyldiphenylamine, triphenylamine, and naphthylamine; aniline; aniline derivatives such as N-methylaniline, N-ethylaniline, N-propylaniline, N,N-dimethylaniline, 2-methylaniline, 3-methylaniline, 4-methylaniline, ethylaniline, propylaniline, trimethylaniline, and N,N-dimethyltoluidine; pyrrole; and pyrrole derivatives such as 2H-pyrrole, 1-methylpyrrole, 2,4-dimethylpyrrole, 2,5-dimethylpyrrole, and N-methylpyrrole.

[0184] From the viewpoint of increasing the affinity between the core layer and the clad layer, it is preferable that the (E) amine-based compound of the core resin composition contains one or more amine-based compounds that are the same as those contained in the clad resin composition. That is, it is preferable that one or more amine-based compounds are contained in both the core resin composition and the clad resin composition. An amine-based compound that is commonly contained in both the core resin composition and the clad resin composition is sometimes called a "common amine-based compound". The amount of the common amine-based compound contained in the (E) amine-based compound is preferably 80% by mass or more, more preferably 90% by mass or more, and particularly preferably 100% by mass, based on 100% by mass of the total (E) amine-based compounds of the core resin composition.

[0185] The amount of the (E) amine compound may be in the range of 0 mass% or more than 0 mass%, and is preferably 0.01 mass% or more, more preferably 0.05 mass% or more, and particularly preferably 0.1 mass% or more, and is preferably 5 mass% or less, more preferably 2 mass% or less, and particularly preferably 1 mass% or less, relative to 100 mass% of the non-volatile components of the core resin composition.

[0186] 2.6.(F) Optional Additives The core resin composition may further contain an optional additive (F) in combination with the above-mentioned components (A) to (E) as long as the effects of the present invention are not significantly impaired. The optional additive (F) does not include those corresponding to the above-mentioned components (A) to (E). The optional additive (F) may be used alone or in combination of two or more kinds.

[0187] Examples of the optional (F) additives include ultraviolet absorbers, silane coupling agents, plasticizers, flame retardants, antistatic agents, antioxidants, antibacterial agents, defoamers, leveling agents, thickeners, adhesion imparting agents, thixotropy imparting agents, release agents, surface treatment agents, dispersants, surface modifiers, and stabilizers.

[0188] (F) The optional additive may contain inorganic particles. For example, when metal oxide nanoparticles are contained, the refractive index of the cured product of the core resin composition can be increased. However, from the viewpoint of effectively suppressing the transmission loss of the optical waveguide, it is preferable that the amount of inorganic particles contained in the core resin composition is small. Specifically, the range of the amount of inorganic particles is preferably 10% by mass or less, more preferably 5% by mass or less, even more preferably 1% by mass or less, and ideally 0% by mass, relative to 100% by mass of the non-volatile components of the core resin composition. Therefore, it is preferable that the core resin composition does not contain inorganic particles.

[0189] 2.7.(G) Solvents The core resin composition may contain a (G) solvent as a volatile component in combination with the above-mentioned (A) to (F) components. The (G) solvent as the (G) component can adjust the viscosity of the core resin composition. Examples of the (G) solvent include organic solvents.

[0190] Examples of the (G) solvent include ketone solvents such as ethyl methyl ketone and cyclohexanone; aromatic hydrocarbon solvents such as toluene, xylene, and tetramethylbenzene; glycol ether solvents such as methyl cellosolve, butyl cellosolve, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; ester solvents such as ethyl acetate, butyl acetate, butyl cellosolve acetate, carbitol acetate, and ethyl diglycol acetate; ether ester solvents such as propylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, ethyl diglycol acetate, γ-butyrolactone, and methyl methoxypropionate; aliphatic hydrocarbon solvents such as octane and decane; and petroleum-based solvents such as petroleum ether, petroleum naphtha, hydrogenated petroleum naphtha, and solvent naphtha. The (G) solvent may be used alone or in combination of two or more.

[0191] The amount of the solvent is preferably adjusted appropriately from the viewpoint of the coatability of the core resin composition.

[0192] [2.8. Method for producing core resin composition] The core resin composition can be produced by mixing each component to be contained in the core resin composition. Thus, the core resin composition can be produced by mixing the components (A) to (C) and, if necessary, the components (D) to (G). When mixing, if necessary, kneading may be performed using a kneading device such as a triple roll, a ball mill, a bead mill, or a sand mill, or stirring may be performed using a stirring device such as a super mixer or a planetary mixer. There is no restriction on the order in which the components are mixed. In addition, cooling or heating may be performed during the process of mixing the components.

[0193] [2.9. Characteristics of Core Resin Composition] The core resin composition preferably has excellent resolution. For example, a line layer having an L / S (line / space) of 10 μm / 10 μm, 5 μm / 50 μm, and 3 μm / 3 μm is formed using the core resin composition by the method described in [Evaluation of Resolution of Resin Composition] in the Examples described later. In this case, the aspect ratio of the line layer in each line layer can be preferably 0.6 or more, more preferably 1 or more. Here, in L / S, L (line) represents the width of the line layer, and S (space) represents the interval between the line layers. The aspect ratio of the line layer represents the ratio represented by the "layer thickness / line width" of the line layer. According to the core resin composition having such excellent resolution, a core layer having a small width and interval can be formed, and the miniaturization of the optical waveguide can be achieved.

[0194] The above-mentioned core resin composition can be cured by exposure to light and, if necessary, heating. Thus, a cured product can be obtained from the core resin composition. Generally, among the components contained in the core resin composition, volatile components such as (G) solvent can be volatilized by heat during drying or curing, but non-volatile components such as components (A) to (F) do not volatilize. Thus, the cured product of the core resin composition can contain the non-volatile components of the core resin composition or their reaction products.

[0195] The core resin composition can provide a cured product having a refractive index suitable for forming an optical waveguide. core is not limited as long as an optical waveguide having a desired aperture NA can be obtained. For example, the refractive index n core is preferably 1.4500 or more, more preferably 1.5000 or more, particularly preferably 1.6000 or more, and is preferably 1.7000 or less, more preferably 1.6500 or less, particularly preferably 1.6150 or less. The refractive index of the core resin composition can be measured by the method described in [Measurement of refractive index of cured product of resin composition] in the Examples below.

[0196] The core resin composition can provide a cured product with excellent mechanical strength. For example, when the elongation at break of the cured product is measured by the method described in the below-mentioned Examples [Measurement of elongation at break of cured product of resin composition], the cured product preferably has an elongation at break of 1% or more.

[0197] The core resin composition can provide a cured product with excellent heat resistance. For example, when the cured product obtained under the conditions described in the examples below is subjected to a heat treatment under the conditions described in "(Observation of Appearance after Reflow)", the generation of voids can be suppressed.

[0198] According to the cured product of the core resin composition, the surface of the cured product can be made highly smooth. Therefore, according to the core resin composition, a core layer with a smooth surface can be formed, and transmission loss can be effectively suppressed. For example, when a core layer is formed by the cured product of the core resin composition under the conditions described in the examples described later, the arithmetic mean roughness of the core layer can be reduced. Specifically, the arithmetic surface roughness of the core layer is preferably 200 nm or less, more preferably 180 nm or less, and particularly preferably 150 nm or less. There is no particular restriction on the lower limit, and it can be, for example, 10 nm or more. The surface roughness of the core layer can be measured by the method described in [Measurement of surface roughness of core layer] in the examples described later.

[0199] The core resin composition can be used as a photosensitive resin composition for forming a core layer of an optical waveguide. For example, the core resin composition can be used for forming an optical waveguide capable of transmitting light having a wavelength of 1300 nm to 1320 nm. In particular, the core resin composition is preferably used for forming a single-mode optical waveguide, for example, for forming a single-mode optical waveguide for light having a wavelength of 1310 nm.

[0200] From the viewpoint of use for forming an optical waveguide of light having a wavelength of 1300 nm to 1320 nm, it is preferable that the solution of the core resin composition has a small absorbance at a wavelength of 1310 nm. Usually, when the absorbance of the resin composition solution is small, the absorbance of the cured product of the resin composition is small, so it is preferable that the absorbance of the resin composition solution at a wavelength of 1310 nm is small. For example, it is preferable that the absorbance of a 20 mass% solution of the core resin composition obtained under the conditions described in the examples described later is small. To give a specific example, the absorbance of the solution of the core resin composition at an optical path length of 1 cm measured by the method described in [Measurement of absorbance of the solution of the resin composition] in the examples is preferably 0.020 or less, more preferably 0.018 or less, and particularly preferably 0.015 or less.

[0201] [3. Cladding resin composition] The cladding resin composition includes (a) a phenolic resin, (b) a photoacid generator, and (c) a crosslinking agent. The cladding resin composition may be a photosensitive resin composition, and therefore a cladding layer can be formed by a method including exposure to light. Similarly to the core resin composition, the cladding resin composition may form a cladding layer having a desired pattern by a method including exposure to light and development. Unless otherwise specified, the "pattern" of the cladding layer refers to the shape of the cladding layer as viewed from the thickness direction.

[0202] The clad layer can be combined with a core layer formed from a cured product of the core resin composition to produce an optical waveguide capable of transmitting light through the core layer. As described above, the optical waveguide including the core layer and the clad layer in combination can suppress the transmission loss of light.

[0203] Furthermore, the cladding resin composition usually has excellent resolution, and the cured product of the cladding resin composition usually has excellent mechanical strength such as elongation at break, and excellent heat resistance such as reflow resistance.

[0204] [3.1.(a) Phenolic resins] The clad resin composition includes a phenolic resin (a) as the component (a). The phenolic resin (a) of the clad resin composition may be in the same range as the phenolic resin (A) of the core resin composition. The amount of the phenolic resin (a) contained in the clad resin composition may be in the same range as the amount of the phenolic resin (A) contained in the core resin composition. Thus, the amount of the phenolic resin (a) relative to 100% by mass of the non-volatile components of the clad resin composition may be in the same range as the amount of the phenolic resin (A) relative to 100% by mass of the non-volatile components of the core resin composition. The amount of the components (A-1), (A-2), and (A-3) relative to 100% by mass of the non-volatile components of the clad resin composition may be in the same range as the amount of the components (A-1), (A-2), and (A-3) relative to 100% by mass of the non-volatile components of the core resin composition. The ranges of the amounts of the (A-1), (A-2) and (A-3) components relative to 100% by mass of the (a) phenolic resin may be the same as the ranges of the amounts of the (A-1), (A-2) and (A-3) components relative to 100% by mass of the (A) phenolic resin. Furthermore, the range of the mass ratio Wa2 / Wa1 of the (A-1) component to the (A-2) component in the (a) phenolic resin may be the same as the range of the mass ratio Wa2 / Wa1 in the (A) phenolic resin. The (a) phenolic resin can provide the cladding resin composition with the same advantages as those provided by the (A) phenolic resin in the core resin composition.

[0205] The (a) phenolic resin contained in the cladding resin composition and the (A) phenolic resin contained in the core resin composition may be the same or different.

[0206] The refractive index n of the cured product of the cladding resin composition is the same as that of the cured product of the core resin composition. clad can be adjusted by the composition of the (a) phenolic resin. Therefore, the specific type and amount of the (a) phenolic resin are determined based on the refractive index n clad Therefore, from the viewpoint of obtaining an optical waveguide having a desired numerical aperture NA by adjusting the composition of the (a) phenolic resin, it is preferable that at least a part of the (a) phenolic resin in the cladding resin composition is different from the (A) phenolic resin in the core resin composition.

[0207] On the other hand, from the viewpoint of effectively improving the transmission loss, mechanical strength and heat resistance of the optical waveguide by increasing the affinity between the core layer and the clad layer, it is preferable that at least a part of the (a) phenolic resin in the clad resin composition is the same as the (A) phenolic resin in the core resin composition, i.e., it is preferable that one or more common phenolic resins are contained in both the core resin composition and the clad resin composition.

[0208] Therefore, the amount of the common phenolic resin contained in the (a) phenolic resin (i.e., the phenolic resin contained in both the core resin composition and the clad resin composition) relative to the total 100 mass% of the (a) phenolic resin in the clad resin composition may be 100 mass% or less, but is preferably in a specific range less than 100 mass%. Specifically, the amount of the common phenolic resin contained in the (a) phenolic resin is preferably 40 mass% or more, more preferably 50 mass% or more, particularly preferably 60 mass% or more, and is preferably 99.0 mass% or less, more preferably 98.5 mass% or less, particularly preferably 98.0 mass% or less.

[0209] A preferred combination of the (A) phenolic resin of the core resin composition and the (a) phenolic resin of the cladding resin composition is, for example, a combination of the (A) phenolic resin containing a phenolic resin having a structure having an effect of increasing the refractive index, and the (a) phenolic resin not containing the phenolic resin having a structure having an effect of increasing the refractive index. Another example is a combination of the (a) phenolic resin containing a phenolic resin (e.g., a fluorine-based phenolic resin) having a structure having an effect of decreasing the refractive index, and the (A) phenolic resin not containing a phenolic resin having a structure having an effect of decreasing the refractive index. In any combination, it is preferable that the (A) phenolic resin and the (a) phenolic resin contain one or more common phenolic resins.

[0210] When the (a) phenolic resin of the clad resin composition contains a fluorine-based phenolic resin, the amount of the fluorine-based phenolic resin relative to 100 mass% of the total (a) phenolic resin is preferably 0.1 mass% or more, more preferably 0.2 mass% or more, and particularly preferably 0.5 mass% or more, and is preferably 40 mass% or less, more preferably 30 mass% or less, and particularly preferably 20 mass% or less.

[0211] Furthermore, the range of the mass of fluorine atoms contained in the clad resin composition relative to 100 mass% of the non-volatile components of the clad resin composition is preferably 0.01 mass% or more, more preferably 0.02 mass% or more, and particularly preferably 0.03 mass% or more, and is preferably 10 mass% or less, more preferably 7 mass% or less, even more preferably 5 mass% or less, and may be 1.0 mass% or less, 0.9 mass% or less, 0.8 mass% or less, etc.

[0212] [3.2.(b) Photoacid generator] The cladding resin composition includes a photoacid generator (b) as the component (b). The photoacid generator (b) of the cladding resin composition may be in the same range as the photoacid generator (B) of the core resin composition. The amount of the photoacid generator (b) contained in the cladding resin composition may be in the same range as the amount of the photoacid generator (B) contained in the core resin composition. Therefore, the amount of the photoacid generator (b) relative to 100% by mass of the nonvolatile components of the cladding resin composition may be in the same range as the amount of the photoacid generator (B) relative to 100% by mass of the nonvolatile components of the core resin composition. The photoacid generator (b) can provide the cladding resin composition with the same advantages as those provided by the photoacid generator (B) of the core resin composition.

[0213] The (b) photoacid generator contained in the cladding resin composition and the (B) photoacid generator contained in the core resin composition may be the same or different. From the viewpoint of increasing the affinity between the core layer and the cladding layer, the (b) photoacid generator in the cladding resin composition preferably contains one or more common photoacid generators that are the same as those contained in the core resin composition. The amount of the common photoacid generator contained in the (b) photoacid generator relative to 100% by mass of the total (b) photoacid generator in the cladding resin composition is preferably 80% by mass or more, more preferably 90% by mass or more, and particularly preferably 100% by mass.

[0214] 3.3.(c) Crosslinking Agents The clad resin composition includes a (c) crosslinking agent as the (c) component. The (c) crosslinking agent of the clad resin composition may be in the same range as the (C) crosslinking agent of the core resin composition. The amount of the (c) crosslinking agent contained in the clad resin composition may be in the same range as the amount of the (C) crosslinking agent contained in the core resin composition. Therefore, the amount of the (c) crosslinking agent relative to 100% by mass of the non-volatile components of the clad resin composition may be in the same range as the amount of the (C) crosslinking agent relative to 100% by mass of the non-volatile components of the core resin composition. The (c) crosslinking agent can provide the clad resin composition with the same advantages as those provided by the (C) crosslinking agent in the core resin composition.

[0215] The (c) crosslinking agent contained in the clad resin composition and the (C) crosslinking agent contained in the core resin composition may be the same or different. From the viewpoint of increasing the affinity between the core layer and the clad layer, the (c) crosslinking agent of the clad resin composition preferably contains one or more common crosslinking agents that are the same as those contained in the core resin composition. The amount of the common crosslinking agent contained in the (c) crosslinking agent relative to 100% by mass of the total (c) crosslinking agent of the clad resin composition is preferably 80% by mass or more, more preferably 90% by mass or more, and particularly preferably 100% by mass.

[0216] 3.4.(d) Polymers The clad resin composition may further contain a (d) polymer as an optional component in combination with the above-mentioned (a) to (c) components. The (d) polymer as the (d) component of the clad resin composition may be in the same range as the (D) polymer of the core resin composition. The amount of the (d) polymer contained in the clad resin composition may be in the same range as the amount of the (D) polymer contained in the core resin composition. Therefore, the amount of the (d) polymer relative to 100% by mass of the non-volatile components of the clad resin composition may be in the same range as the amount of the (D) polymer relative to 100% by mass of the non-volatile components of the core resin composition. The (d) polymer can provide the clad resin composition with the same advantages as those provided by the (D) polymer in the core resin composition.

[0217] The (d) polymer contained in the clad resin composition and the (D) polymer contained in the core resin composition may be the same or different. From the viewpoint of increasing the affinity between the core layer and the clad layer, it is preferable that the (d) polymer of the clad resin composition contains one or more common polymers that are the same as those contained in the core resin composition. The amount of the common polymer contained in the (d) polymer is preferably 80% by mass or more, more preferably 90% by mass or more, and particularly preferably 100% by mass, based on 100% by mass of the total (d) polymer of the clad resin composition.

[0218] [3.5.(e) Amine compounds] The clad resin composition may further contain an amine compound (e) (i.e., a compound represented by formula (E-1)) as an optional component in combination with the above-mentioned components (a) to (d). The amine compound (e) as the component (e) of the clad resin composition may be in the same range as the amine compound (E) of the core resin composition. The amount of the amine compound (e) contained in the clad resin composition may be in the same range as the amount of the amine compound (E) contained in the core resin composition. Thus, the amount of the amine compound (e) relative to 100% by mass of the non-volatile components of the clad resin composition may be in the same range as the amount of the amine compound (E) relative to 100% by mass of the non-volatile components of the core resin composition. The amine compound (e) can provide the clad resin composition with the same advantages as those provided by the amine compound (E) in the core resin composition.

[0219] The amine compound (e) contained in the clad resin composition and the amine compound (E) contained in the core resin composition may be the same or different. From the viewpoint of increasing the affinity between the core layer and the clad layer, the amine compound (e) of the clad resin composition preferably contains one or more common amine compounds contained in the core resin composition. The amount of the common amine compound contained in the amine compound (e) relative to 100% by mass of the total amine compounds (e) of the clad resin composition is preferably 80% by mass or more, more preferably 90% by mass or more, and particularly preferably 100% by mass.

[0220] 3.6.(f) Optional Additives The cladding resin composition may further contain an optional additive (f) as an optional component in combination with the above-mentioned components (a) to (e). The optional additive (f) as the component (f) of the cladding resin composition may be in the same range as the optional additive (F) of the core resin composition. The amount of the optional additive (f) contained in the cladding resin composition may be in the same range as the amount of the optional additive (F) contained in the core resin composition.

[0221] 3.7.(g) Solvents The clad resin composition may contain a (g) solvent as a volatile component in combination with the non-volatile components such as the above-mentioned (a) to (f) components. The (g) solvent as the (g) component of the clad resin composition may be in the same range as the (G) solvent of the core resin composition. The amount of the (g) solvent contained in the clad resin composition may be in the same range as the amount of the (G) solvent contained in the core resin composition. The (g) solvent can provide the clad resin composition with the same advantages as those provided by the (G) solvent in the core resin composition.

[0222] [3.8. Method for producing cladding resin composition] The clad resin composition can be produced by mixing the components to be contained in the clad resin composition. Thus, the clad resin composition can be produced by mixing components (a) to (c) and, if necessary, components (d) to (g). The mixing method may be the same as that for producing the core resin composition.

[0223] [3.9. Characteristics of Cladding Resin Composition] The cladding resin composition preferably has excellent resolution. For example, line layers with L / S (line / space) of 10 μm / 10 μm, 5 μm / 50 μm, and 3 μm / 3 μm are formed using the cladding resin composition by the method described in the "Evaluation of Resolution of Resin Composition" section of the Examples below. In this case, the aspect ratio of the line layer can be preferably 0.6 or more, more preferably 1 or more, in each line layer.

[0224] The above-mentioned cladding resin composition can be cured by exposure to light and, if necessary, heating. Thus, a cured product can be obtained from the cladding resin composition. Among the components contained in the cladding resin composition, volatile components such as (g) solvent can be volatilized by heat during drying or curing, but non-volatile components such as components (a) to (f) do not volatilize. Thus, the cured product of the cladding resin composition can contain the non-volatile components of the cladding resin composition or their reaction products.

[0225] The cladding resin composition can provide a cured product having a refractive index suitable for forming an optical waveguide. clad is not limited as long as an optical waveguide having a desired aperture NA can be obtained. For example, the refractive index n clad is preferably 1.4000 or more, more preferably 1.5000 or more, particularly preferably 1.5900 or more, and is preferably 1.6500 or less, more preferably 1.61000 or less, particularly preferably 1.6006 or less. The refractive index of the cladding resin composition can be measured by the method described in [Measurement of refractive index of cured product of resin composition] in the Examples below.

[0226] The cladding resin composition can provide a cured product with excellent mechanical strength. For example, when the elongation at break of the cured product is measured by the method described in the "Measurement of elongation at break of cured product of resin composition" in the examples below, the cured product preferably has an elongation at break of 1% or more.

[0227] The cladding resin composition can provide a cured product with excellent heat resistance. For example, when the cured product obtained under the conditions described in the Examples below is subjected to a heat treatment under the conditions described in "(Observation of Appearance after Reflow)", the generation of voids can be suppressed. In addition, the composition can preferably suppress peeling of the cured product from a substrate such as a silicon wafer.

[0228] The cladding resin composition can be used as a photosensitive resin composition for forming a cladding layer of an optical waveguide. For example, the cladding resin composition can be used to form an optical waveguide capable of transmitting light having a wavelength of 1300 nm to 1320 nm. In particular, the cladding resin composition is preferably used to form a single-mode optical waveguide, for example, a single-mode optical waveguide for light having a wavelength of 1310 nm.

[0229] [4. Relationship between the cured product of the core resin composition and the cured product of the cladding resin composition] The cured product of the core resin composition and the cured product of the cladding resin composition described above have a refractive index n core and the refractive index n clad has.

[0230]

number

[0231] In formula (1), n core represents the refractive index of the cured product of the core resin composition, and n clad represents the refractive index of the cured product of the cladding resin composition. Refractive index n core and the refractive index n clad The measurement wavelength is the wavelength of light transmitted through the optical waveguide, for example, 1310 nm. The numerical aperture NA is, specifically, usually larger than 0.05, preferably larger than 0.06, particularly preferably larger than 0.065, and usually smaller than 0.4, preferably 0.35 or less, further preferably 0.3 or less, particularly preferably 0.2 or less.

[0232] The refractive index of the cured product of the photosensitive resin composition such as the core resin composition and the cladding resin composition can be measured by the following method. The photosensitive resin composition is exposed to light at an optimal exposure dose of 3000 mJ, and then heated at 90°C for 3 minutes. Furthermore, a 2.38 mass% aqueous solution of tetramethylammonium hydroxide at 23°C is sprayed as a developer at a spray pressure of 0.1 MPa for 30 seconds to perform development. After this development, the refractive index of the cured product of the photosensitive resin composition is measured by the following method. The ... 2 The cured product is then subjected to UV irradiation for 100 s, followed by heat treatment at 190°C for 90 minutes in a nitrogen atmosphere to obtain a cured product. The refractive index of the cured product is measured at room temperature and normal pressure (23°C and 1 atm). The specific measurement method may be the method described in the "Measurement of the refractive index of the cured product of the resin composition" section of the Examples.

[0233] When the numerical aperture NA falls within the above range, an optical waveguide having a core layer containing a cured product of the core resin composition and a clad layer containing a cured product of the clad resin composition can suppress the transmission loss of light. For example, when the refractive index n core and n clad The transmission loss of the light having the measurement wavelength can be preferably 2.0 dB / cm or less, more preferably 1.8 dB / cm or less, and particularly preferably 1.6 dB / cm or less. The lower limit of the transmission loss is ideally 0.0 dB / cm, but is usually 0.1 dB / cm or more. The transmission loss of the optical waveguide can be measured by the method described in [Evaluation of Optical Waveguide] in the Examples below.

[0234] Moreover, the optical waveguide generally has excellent heat resistance and therefore excellent reflow resistance. Specifically, when the optical waveguide is subjected to a heat treatment using a reflow device, the optical waveguide generally can suppress the formation of voids. Furthermore, when the optical waveguide is subjected to the heat treatment, the optical waveguide generally can suppress the peeling off from the substrate (e.g., silicon wafer) on which the optical waveguide is provided. The heat treatment using a reflow device can be carried out, for example, by the method described in [Evaluation of optical waveguide] in the examples described later.

[0235] The present inventors speculate that the mechanism by which the above-mentioned effects are obtained is as follows, although the technical scope of the present invention is not limited to the mechanism below.

[0236] In general, factors that cause transmission loss in an optical waveguide include attenuation due to light absorption by the material contained in the core layer, and attenuation of light when reflected at the interface between the core layer and the clad layer. In contrast, a cured product of the core resin composition containing a combination of components (A) to (C) can suppress light absorption.

[0237] Furthermore, when the numerical aperture NA is within the above-mentioned specific range, attenuation during reflection at the interface between the core layer and the cladding layer can be suppressed. For example, in general, when forming an optical waveguide, heat is applied to the core resin composition and the clad resin composition. Thus, the core layer and the clad layer are given a thermal history, but this thermal history may be locally non-uniform in a part of the optical waveguide. In this case, the refractive index difference between the core layer and the clad layer in the part may become too small, and the reflection at the interface of that part may be insufficient. However, when the numerical aperture NA is within the above-mentioned specific range, even if a part with a non-uniform thermal history occurs, the refractive index difference between the core layer and the clad layer can be stably increased, so that attenuation during reflection at the interface can be suppressed.

[0238] Furthermore, for example, generally, when the core layer and the clad layer are formed of a cured product of a resin composition, the refractive index of part or all of the cured product may vary due to stress applied during handling. If the refractive index varies and a portion is generated in which the refractive index difference between the core layer and the clad layer is too small, reflection at the interface may be insufficient in that portion. However, when the numerical aperture NA is equal to or greater than the lower limit of the above range, the refractive index difference between the core layer and the clad layer can be stably increased even if stress is applied during handling. Therefore, attenuation during reflection at the interface can be suppressed.

[0239] In addition, when the numerical aperture NA is equal to or less than the upper limit of the above range, the cured product of the core resin composition and the cured product of the clad resin composition have similar refractive indices, and therefore have similar compositions. Therefore, even if there is a change in refractive index due to the influence of heat, moisture, etc. applied during production and use, the change can occur to the same extent in the core layer and the clad layer. Therefore, the change in the refractive index difference between the core layer and the clad layer can be suppressed, and the refractive index difference can be stably increased, so that attenuation during reflection at the interface can be suppressed. In addition, when the cured product of the core resin composition and the cured product of the clad resin composition have similar compositions, the affinity between the core layer and the clad layer can be increased, so that the smoothness of the interface can be highly improved. Therefore, it is possible to suppress the occurrence of a portion where the angle of incidence of light to the interface is small when viewed microscopically, so that it is possible to suppress the light in the core layer from leaking into the clad layer, and it is possible to suppress attenuation during reflection at the interface.

[0240] Furthermore, the numerical aperture of a commonly used light-collecting module is relatively small. In contrast, an optical waveguide having the numerical aperture NA described above can suppress light leakage when transmitting light to a light-collecting module having a small numerical aperture as described above. Therefore, it is possible to suppress the connection loss at the output side of the optical waveguide, which also suppresses the transmission loss. Therefore, the transmission loss can be suppressed.

[0241] In addition, the cured product of the core resin composition and the cured product of the clad resin composition can usually have high heat resistance. Furthermore, since the cured product of the core resin composition and the cured product of the clad resin composition can have high affinity, the adhesion between the core layer and the clad layer can be smoothly achieved, and therefore, the air remaining at the interface between the core layer and the clad layer can be suppressed. Furthermore, since the adhesion between the core layer and the clad layer can be increased, peeling at the interface between the core layer and the clad layer can be suppressed. Therefore, the formation of voids during heat treatment can be suppressed. Furthermore, since the cured product of the core resin composition and the cured product of the clad resin composition can have high mechanical strength, the occurrence of peeling (delamination) accompanied by resin destruction can be suppressed, and therefore, peeling from the substrate can be suppressed. Therefore, usually, high heat resistance can be obtained.

[0242] Furthermore, when the cured product of the core resin composition and the cured product of the clad resin composition have similar compositions, the core layer and the clad layer can have similar properties such as the coefficient of linear thermal expansion (CTE) and elasticity. Therefore, the core layer and the clad layer can show similar refractive index fluctuation behavior in durability tests such as long-term heat resistance tests and moist heat tests. Therefore, the heat resistance and moist heat resistance of the optical waveguide can be improved, and the numerical aperture NA can be prevented from unintentionally deviating from the design range due to the durability test, thereby suppressing the transmission loss.

[0243] From the viewpoint of improving the heat resistance and moist heat resistance of the optical waveguide, it is preferable that the difference ΔCTE between the linear thermal expansion coefficient of the cured product of the core resin composition and the linear thermal expansion coefficient of the cured product of the clad resin composition is small. The specific range of the difference ΔCTE in the linear thermal expansion coefficient is preferably 20 ppm / °C or less, more preferably 18 ppm / °C or less, and particularly preferably 15 ppm / °C or less. The linear thermal expansion coefficient of the cured product of the core resin composition may be larger than the linear thermal expansion coefficient of the cured product of the clad resin composition, but it is preferable that the linear thermal expansion coefficient of the cured product of the clad resin composition is larger than the linear thermal expansion coefficient of the cured product of the core resin composition. The linear thermal expansion coefficient of the cured product of the core resin composition and the linear thermal expansion coefficient of the cured product of the clad resin composition can be measured by the method described in [Measurement of the linear thermal expansion coefficient of the cured product of the resin composition] in the examples.

[0244] The wavelength of light transmitted by the optical waveguide produced using the above-mentioned core resin composition and clad resin composition can be selected from various wavelengths. For example, the preferred wavelength range of the transmitted light can be 840 nm to 860 nm (e.g., 850 nm), 1300 nm to 1320 nm (e.g., 1310 nm), 1540 nm to 1560 nm (e.g., 1550 nm), etc. Among them, the above-mentioned core resin composition and clad resin composition are preferably used for producing an optical waveguide capable of transmitting light with a wavelength of 1300 nm to 1320 nm.

[0245] Optical waveguides include single-mode optical waveguides and multi-mode optical waveguides. The above-mentioned core resin composition and clad resin composition may be used for producing a single-mode optical waveguide, or may be used for producing a multi-mode optical waveguide. Among them, the above-mentioned core resin composition and clad resin composition are preferably used for producing a single-mode optical waveguide. Therefore, for example, it is preferable to use them for producing a single-mode optical waveguide for light in the above-mentioned preferred wavelength range.

[0246] [5. Sheet set] The photosensitive resin compositions such as the core resin composition and the clad resin composition described above may be used as a resin sheet. The resin sheet is a sheet having a resin composition layer containing the photosensitive resin composition. Thus, from the core resin composition, a resin sheet having a resin composition layer containing the core resin composition (hereinafter, sometimes referred to as a "core resin sheet") is obtained. Also, from the clad resin composition, a resin sheet having a resin composition layer containing the clad resin composition (hereinafter, sometimes referred to as a "clad resin sheet") is obtained. Then, a sheet set including the core resin sheet and the clad resin sheet can be obtained as a sheet set for manufacturing an optical waveguide. According to these sheet sets, the core resin sheet, and the clad resin sheet, the same advantages as those of the photosensitive resin composition set, the core resin composition, and the clad resin composition described above can be obtained, and further, since it is possible to manufacture an optical waveguide by a lamination method, it is possible to easily manufacture an optical waveguide.

[0247] [5.1. Core resin sheet] The resin composition layer of the core resin sheet usually contains the core resin composition, and preferably contains only the core resin composition. The thickness of the resin composition layer of the core resin sheet can be set according to the thickness of the core layer. In terms of specific ranges, the thickness of the resin composition layer of the core resin sheet is preferably 0.5 μm or more, more preferably 1 μm or more, even more preferably 3 μm or more, and is preferably 100 μm or less, more preferably 50 μm or less, and particularly preferably 20 μm or less.

[0248] The core resin sheet may include a support. For example, the core resin sheet may include a support and a resin composition layer formed on the support. Examples of the support include polyethylene terephthalate film, polyethylene naphthalate film, polypropylene film, polyethylene film, polyvinyl alcohol film, triacetyl acetate film, and the like, and polyethylene terephthalate film is particularly preferred. Examples of commercially available supports include polyethylene terephthalate films such as those manufactured by Oji Paper Co., Ltd. under the product names "Alphan MA-410" and "E-200C", polypropylene films manufactured by Shin-Etsu Film Co., Ltd., and those manufactured by Teijin Ltd. under the product name "PS-25" and the like in the PS series. In order to facilitate the peeling of the support after lamination, a release agent such as an alkyd-based release agent or a silicone coating agent may be applied to the surface of the support. The thickness of the support is preferably in the range of 5 μm to 100 μm, and more preferably in the range of 10 μm to 50 μm.

[0249] The core resin sheet may have a protective film for protecting the resin composition layer. Usually, the protective film is provided on the opposite side of the resin composition layer from the support. For example, a film made of the same material as the support can be used as the protective film. The adhesive strength between the protective film and the resin composition layer is preferably smaller than the adhesive strength between the support and the resin composition layer. Usually, the core resin sheet is used after peeling off the protective film.

[0250] The core resin sheet can be produced, for example, by applying the core resin composition onto a support. From the viewpoint of smooth application, a varnish-like core resin composition containing a solvent may be prepared, and the varnish-like core resin composition may be applied. When the core resin composition containing a solvent is applied, drying may be performed after application, if necessary.

[0251] The resin composition layer of the core resin sheet may contain a solvent, but the amount of the solvent is preferably small. In one example, the amount of the solvent contained in the resin composition layer is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 2% by mass or less, based on 100% by mass of the total amount of the resin composition layer.

[0252] [5.2. Cladding resin sheets] The resin composition layer of the clad resin sheet usually contains the clad resin composition, and preferably contains only the clad resin composition. The thickness of the resin composition layer of the clad resin sheet can be set according to the thickness of the clad layer. In terms of specific ranges, the thickness of the resin composition layer of the clad resin sheet is preferably 5 μm or more, more preferably 7 μm or more, even more preferably 10 μm or more, and is preferably 40 μm or less, more preferably 30 μm or less, and particularly preferably 20 μm or less.

[0253] The clad resin sheet may be the same as the core resin sheet, except that it has the above-mentioned resin composition layer containing the clad resin composition instead of the resin composition layer containing the core resin composition. Therefore, the clad resin sheet may have a support. The support of the clad resin sheet may be the same as the support of the core resin sheet. In addition, the clad resin sheet may have a protective film. The protective film of the clad resin sheet may be the same as the protective film of the core resin sheet. Usually, the clad resin sheet is used after peeling off the protective film.

[0254] The clad resin sheet can be produced in the same manner as the core resin sheet, except that the clad resin composition is used instead of the core resin composition.

[0255] The resin composition layer of the clad resin sheet may contain a solvent, but the amount of the solvent is preferably small. In one example, the amount of the solvent contained in the resin composition layer of the clad resin sheet may be in the same range as the amount of the solvent contained in the resin composition layer of the core resin sheet.

[0256] [6. Optical waveguide] The above-mentioned core resin composition, core resin sheet, clad resin composition, clad resin sheet, photosensitive resin composition set, and sheet set can be used for producing an optical waveguide. Hereinafter, an embodiment of the optical waveguide will be described with reference to the drawings.

[0257] Fig. 1 is a perspective view showing a schematic diagram of an optical waveguide 10 according to one embodiment of the present invention. As shown in Fig. 1, the optical waveguide 10 includes a core layer 100 and a clad layer 200. The core layer 100 includes a cured product of a core resin composition, and preferably includes only a cured product of the core resin composition. The clad layer 200 includes a cured product of a clad resin composition, and preferably includes only a cured product of the clad resin composition.

[0258] The core layer 100 is provided in the clad layer 200. Thus, the core layer 100 is covered by the clad layer 200. Usually, the entire peripheral surface of the core layer 100 is covered by the clad layer 200. The core layer 100 and the clad layer 200 are in direct contact with each other without any other layer therebetween, and therefore, an interface 100I can be formed between the core layer 100 and the clad layer 200. Usually, light (not shown) can be transmitted through the core layer 100 from one end (the end on the incident side) 100A of the core layer 100 to the other end (the end on the exit side) 100B while repeatedly being reflected at the interface 100I.

[0259] The wavelength of light that can be transmitted by the optical waveguide 10 can be selected from various wavelengths. For example, the preferred wavelength range of the transmitted light can be 840 nm to 860 nm (e.g., 850 nm), 1300 nm to 1320 nm (e.g., 1310 nm), 1540 nm to 1560 nm (e.g., 1550 nm), etc. Among them, the preferred wavelength range of the light transmitted through the optical transmission line 10 is 1300 nm to 1320 nm.

[0260] The optical waveguide 10 may be a single-mode optical waveguide or a multimode optical waveguide, but is preferably a single-mode optical waveguide. In particular, the optical waveguide 10 is preferably a single-mode optical waveguide for light in the above-mentioned preferred wavelength range. For example, the optical waveguide 10 is preferably a single-mode optical waveguide for light of 1310 nm.

[0261] It is desirable to set the width L of the core layer 100 appropriately within a range in which light transmission is possible. A specific range of the line width L of the core layer 100 is preferably 0.5 μm or more, more preferably 1 μm or more, particularly preferably 2 μm or more, and is preferably 50 μm or less, more preferably 30 μm or less, particularly preferably 20 μm or less, and may be 10 μm or less or 5 μm or less. The width L of the core layer 100 corresponds to the line width (line) of the core layer 100 when viewed in the thickness direction.

[0262] It is desirable to set the interval S of the core layers 100 appropriately within a range in which light transmission is possible. A specific range of the interval S of the core layers 100 is preferably 50 μm or more, more preferably 70 μm or more, particularly preferably 100 μm or more, and preferably 1000 μm or less, more preferably 500 μm or less, particularly preferably 300 μm or less. The interval S of the core layers 100 corresponds to the interval (space) of the core layers as viewed in the thickness direction.

[0263] It is desirable to appropriately set the thickness T of the core layer 100 within a range in which light transmission is possible. A specific range of the thickness T of the core layer 100 is preferably 0.5 μm or more, more preferably 1 μm or more, particularly preferably 2 μm or more, and is preferably 50 μm or less, more preferably 30 μm or less, particularly preferably 20 μm or less, and may be 10 μm or less.

[0264] The thickness of the cladding layer 200 is usually greater than the thickness of the core layer 100. The specific thickness of the cladding layer 200 is preferably 5 μm or more, more preferably 7 μm or more, particularly preferably 10 μm or more, and is preferably 100 μm or less, more preferably 60 μm or less, even more preferably 40 μm or less, even more preferably 30 μm or less, and particularly preferably 20 μm or less.

[0265] The optical waveguide 10 may include any element other than the core layer 100 and the clad layer 200, as necessary. For example, the optical waveguide 10 may include a substrate 300. In the optical waveguide 10 including the substrate 300, the clad layer 200 is usually provided on the substrate 300, and the core layer 100 is provided in the clad layer 200.

[0266] The substrate 300 may be a hard substrate such as a glass substrate, a metal substrate, a ceramic substrate, a wafer, or a circuit substrate. The wafer may be a semiconductor wafer such as a silicon wafer, a gallium arsenide (GaAs) wafer, an indium phosphide (InP) wafer, a gallium phosphide (GaP) wafer, a gallium nitride (GaN) wafer, a gallium telluride (GaTe) wafer, a zinc selenium (ZnSe) wafer, or a silicon carbide (SiC) wafer, or a pseudo wafer. The pseudo wafer may be a plate-shaped member having a mold resin and electronic components embedded in the mold resin. The circuit substrate may be a glass epoxy substrate, a metal substrate, a polyester substrate, a polyimide substrate, a BT resin substrate, or a thermosetting polyphenylene ether substrate. The circuit substrate may be a substrate having a patterned conductor layer (circuit) formed on one or both sides of the substrate. The substrate 300 may be a film formed of a plastic material such as polyethylene terephthalate, polyimide, or polyester. Furthermore, a flexible circuit board may be employed as the substrate 300 .

[0267] Furthermore, the optical waveguide 10 may include, as an optional element, a protective layer (not shown) for protecting the core layer 100 and the cladding layer 200. The protective layer may be provided, for example, so as to cover the surface of the cladding layer 200 opposite to the substrate 300.

[0268] As described above, the optical waveguide 10 can have a small transmission loss. Moreover, the optical waveguide 10 usually has excellent heat resistance, for example, excellent reflow resistance. Furthermore, since the optical waveguide 10 can be formed using a core resin composition and a clad resin composition having excellent resolution, the core layer can be finely wired, and it can be formed with a small line width L as described above.

[0269] The optical waveguide 10 can be produced by using a combination of the above-mentioned core resin composition and clad resin composition. For example, the optical waveguide 10 can be produced by A step (I) of forming a first composition layer containing a cladding resin composition; A step (II) of subjecting the first composition layer to an exposure treatment; A step (III) of curing the first composition layer; A step (IV) of forming a second composition layer containing a core resin composition on the first composition layer; A step (V) of subjecting the second composition layer to an exposure treatment; A step (VI) of subjecting the second composition layer to a development treatment; (VII) curing the second composition layer; (VIII) forming a third composition layer containing a cladding resin composition on the second composition layer; A step (IX) of exposing the third composition layer to light; A step (X) of curing the third composition layer; It can be produced by a process comprising the steps of:

[0270] Fig. 2 is a schematic cross-sectional view for explaining step (I) of the method for producing an optical waveguide according to one embodiment of the present invention. As shown in Fig. 2, the method for producing an optical waveguide according to one embodiment of the present invention includes step (I) of forming a first composition layer 210 containing a cladding resin composition. In this embodiment, an example of forming the first composition layer 210 on a substrate 300 will be shown and explained.

[0271] There is no particular limitation on the method for forming the first composition layer 210. For example, the first composition layer 210 may be formed by applying a clad resin composition onto the substrate 300. From the viewpoint of smooth application, a varnish-like clad resin composition containing a solvent may be prepared, and the varnish-like clad resin composition may be applied.

[0272] Examples of coating methods include gravure coating, microgravure coating, reverse coating, kiss reverse coating, die coating, slot die, lip coating, comma coating, blade coating, roll coating, knife coating, curtain coating, chamber gravure coating, slot orifice, spin coating, slit coating, spray coating, dip coating, hot melt coating, bar coating, applicator, air knife coating, curtain flow coating, offset printing, brush coating, and screen printing.

[0273] The cladding resin composition may be applied in one application or in multiple applications. Also, different application methods may be combined. In order to avoid contamination by foreign matter, it is preferable to apply the composition in an environment where foreign matter is unlikely to be generated, such as a clean room.

[0274] After application of the cladding resin composition, the first composition layer 210 may be dried as necessary. Drying can be performed using a drying device such as a hot air oven or a far infrared oven. It is preferable to set the drying conditions appropriately according to the composition of the cladding resin composition. To give a specific example, the drying temperature is preferably 50° C. or higher, more preferably 70° C. or higher, particularly preferably 80° C. or higher, and preferably 150° C. or lower, more preferably 130° C. or lower, particularly preferably 120° C. or lower. The drying time is preferably 30 seconds or higher, more preferably 60 seconds or higher, particularly preferably 120 seconds or higher, and preferably 60 minutes or less, more preferably 20 minutes or less, particularly preferably 5 minutes or less.

[0275] The first composition layer 210 may be formed, for example, by using a resin sheet for cladding. As a specific example, the resin composition layer of the resin sheet for cladding is laminated onto the substrate 300, thereby forming the first composition layer 210 on the substrate 300. The lamination is usually performed by pressing the resin composition layer of the resin sheet onto the substrate 300 while heating it. This lamination is preferably performed under reduced pressure by a vacuum lamination method. Furthermore, prior to the lamination, a preheat treatment may be performed to heat the resin sheet and the substrate, if necessary.

[0276] The lamination conditions are, for example, a pressure bonding temperature (lamination temperature) of 70°C to 140°C and a pressure bonding pressure of 1kgf / cm. 2 ~11kgf / cm 2 (9.8×10 4 N / m 2 ~107.9×10 4 N / m 2 ) and a pressure bonding time of 5 to 300 seconds. The lamination is preferably carried out under reduced pressure with an air pressure of 20 mmHg (26.7 hPa) or less. The lamination may be carried out in a batch manner or continuously using a roll.

[0277] The vacuum lamination method can be performed using a commercially available vacuum laminator, such as a vacuum applicator manufactured by Nikko Materials Co., Ltd., a vacuum pressure laminator manufactured by Meiki Seisakusho Co., Ltd., a roll-type dry coater manufactured by Hitachi Industries Co., Ltd., and a vacuum laminator manufactured by Hitachi AIC Co., Ltd.

[0278] When the first composition layer 210 is formed using a clad resin sheet having a support, the support is usually peeled off at an appropriate time before the step (IV).

[0279] The first composition layer 210 formed on the substrate 300 in step (I) usually contains a cladding resin composition, and preferably contains only a cladding resin composition.

[0280] The method for producing an optical waveguide according to one embodiment of the present invention includes a step (II) of performing an exposure treatment on the first composition layer 210 after the step (I). In this exposure treatment, the first composition layer 210 is irradiated with light. When irradiated with light, the photoacid generator (b) in the first composition layer 210 generates an acid. As the light used in the exposure treatment, it is preferable to use an appropriate actinic ray according to the composition of the cladding resin composition. The wavelength of the actinic ray is usually 190 nm to 1000 nm, preferably 240 nm to 550 nm, but light rays of other wavelengths may also be used. Specific examples of the actinic light source include ultraviolet light, visible light, electron beams, X-rays, etc., and ultraviolet light is particularly preferable.

[0281] The amount of light exposure is desirably set so that the curing of the first composition layer 210 in step (III) can proceed. In one example, the specific range of the amount of light exposure is preferably 10 mJ / cm 2 More preferably, 50 mJ / cm 2 More than 200 mJ / cm 2 or more, preferably 10,000 mJ / cm 2 Less than or equal to 8,000 mJ / cm 2 Less than 4,000 mJ / cm, more preferably 4,000 mJ / cm 2Below 1,000 mJ / cm, particularly preferably 2 The following is the result.

[0282] When the first composition layer 210 is formed using a clad resin sheet having a support, in step (II), a support (not shown) may be present on the first composition layer 210. When a support is present on the first composition layer 210, exposure may be performed through the support, or exposure may be performed after peeling off the support.

[0283] The method for producing an optical waveguide according to one embodiment of the present invention includes a step (III) of curing the first composition layer 210 after the step (II). This step (III) usually includes a heat treatment of the first composition layer 210. The heat treatment can proceed with a crosslinking reaction of the crosslinking agent (c) using the acid generated in the step (II) as a catalyst, thereby curing the first composition layer 210. The conditions for the heat treatment may be selected according to the type and amount of the resin component in the cladding resin composition, and may be preferably in the range of 150°C to 250°C for 20 minutes to 180 minutes, more preferably in the range of 160°C to 230°C for 30 minutes to 120 minutes. The heat treatment is preferably performed in an inert atmosphere such as a nitrogen atmosphere.

[0284] Fig. 3 is a schematic cross-sectional view for explaining step (III) of the method for producing an optical waveguide according to one embodiment of the present invention. By curing the first composition layer 210 in step (III), a cured first composition layer 220 is obtained on the substrate 300, as shown in Fig. 3. This cured first composition layer 220 forms a part of the cladding layer 200, and may be referred to as the "lower cladding layer" 220 hereinafter.

[0285] 4 is a schematic cross-sectional view for explaining step (IV) of the method for producing an optical waveguide according to one embodiment of the present invention. The method for producing an optical waveguide according to one embodiment of the present invention includes, after step (III), step (IV) of forming a second composition layer 110 containing a core resin composition on a lower clad layer 220 as a cured first composition layer, as shown in FIG.

[0286] There is no particular limitation on the method for forming the second composition layer 110. For example, the second composition layer 110 may be formed by applying a core resin composition onto the lower clad layer 220. From the viewpoint of smooth application, a varnish-like core resin composition containing a solvent may be prepared, and the varnish-like core resin composition may be applied. The application of the core resin composition may be performed in the same manner as the application of the clad resin composition. After application of the core resin composition, the second composition layer 110 may be dried as necessary. The drying of the second composition layer 110 may be performed using the same method and conditions as those for drying the first composition layer 210.

[0287] The second composition layer 110 may be formed, for example, by using a core resin sheet. As a specific example, the resin composition layer of the core resin sheet is laminated on the lower clad layer 220, thereby forming the second composition layer 110 on the lower clad layer 220. The lamination of the core resin sheet can be performed in the same manner as the lamination of the clad resin sheet. Furthermore, when the second composition layer 110 is formed using a core resin sheet having a support, the support is usually peeled off at an appropriate time before the step (VI).

[0288] The second composition layer 110 formed on the lower clad layer 220 in step (IV) usually contains a core resin composition, and preferably contains only a core resin composition.

[0289] 5 is a schematic cross-sectional view for explaining step (V) of the method for producing an optical waveguide according to one embodiment of the present invention. As shown in FIG. 5, the method for producing an optical waveguide according to one embodiment of the present invention includes, after step (IV), step (V) of subjecting the second composition layer 110 to an exposure treatment.

[0290] In step (V), a latent image is formed in the second composition layer 110 by exposure treatment. Specifically, in the exposure treatment, light P is selectively irradiated to a specific portion of the second composition layer 110. Thus, when the exposure treatment is performed, the second composition layer 110 is provided with an exposed portion 111 that is irradiated with light and a non-exposed portion 112 that is not irradiated with light. Usually, the core resin composition functions as a negative photosensitive resin composition, so that the exposed portion 111 forms a latent image corresponding to the core layer.

[0291] From the viewpoint of performing selective exposure, the exposure treatment in the step (V) is usually performed using a mask 400. Specifically, in this exposure treatment, the second composition layer 110 is irradiated with light P through the mask 400 having a light-transmitting portion 410 and a light-shielding portion 420. The light P passes through the light-transmitting portion 410 and enters the exposed portion 111, but cannot pass through the light-shielding portion 420 and therefore cannot enter the non-exposed portion 112. Therefore, the exposed portion 111 and the non-exposed portion 112 corresponding to the light-transmitting portion 410 and the light-shielding portion 420 can be provided in the second composition layer 110. The mask 400 may be brought into close contact with the second composition layer 110 as shown in FIG. 5 (contact exposure method), or exposure may be performed using parallel light without being in close contact (non-contact exposure method).

[0292] In general, the light-transmitting portion 410 of the mask 400 is formed to have a planar shape corresponding to the core layer of the optical waveguide. Therefore, the light-shielding portion 420 of the mask 400 is formed to have a planar shape corresponding to the portion of the optical waveguide where the core layer is not present. Unless otherwise specified, the "planar shape" refers to the shape seen from the thickness direction. The light-transmitting portion 410 formed in the planar shape corresponding to the core layer may be referred to as a "mask pattern" hereinafter.

[0293] The light P used in the exposure treatment in step (V) may be active light in the same range as that used in the exposure treatment of the first composition layer 210 in step (II). The exposure dose of the light P is preferably set so that a desired core layer can be formed after curing in step (VII). In one example, the specific range of the exposure dose in step (V) may be the same as that of the first composition layer 210 in step (II).

[0294] When the second composition layer 110 is formed using a core resin sheet having a support, in step (V), a support (not shown) may be present on the second composition layer 110. When a support is present on the second composition layer 110, exposure may be performed through the support, or exposure may be performed after peeling off the support.

[0295] Since the core resin composition functions as a negative photosensitive resin composition, in the exposed area 111, the photoacid generator (B) generates an acid. Then, since the acid acts as a catalyst, the crosslinking reaction of the crosslinking agent (C) proceeds, and the solubility in the developer decreases. On the other hand, in the non-exposed area 112, the photoacid generator (B) does not generate an acid, so the crosslinking reaction of the crosslinking agent (C) does not proceed or proceeds only slightly, and therefore the solubility in the developer is high. Utilizing the difference in solubility between the exposed area 111 and the non-exposed area 112, the development process in the subsequent step (VI) is performed.

[0296] The method for producing an optical waveguide according to one embodiment of the present invention may include a step (XI) of heating the second composition layer 110 after the step (V) and before the step (VI). The heating in the step (XI) can promote the crosslinking reaction of the (C) crosslinking agent. Therefore, the solubility of the exposed portion 111 in the developer can be quickly reduced. The heating in the step (XI) may be performed using a hot plate or an oven. The heating temperature may be, for example, 40° C. or more and 110° C. or less. The heating time may be, for example, 30 seconds or more and 60 minutes or less.

[0297] FIG. 6 is a schematic cross-sectional view for explaining step (VI) of the method for producing an optical waveguide according to one embodiment of the present invention. The method for producing an optical waveguide according to one embodiment of the present invention includes step (VI) of subjecting the second composition layer 110 to a development treatment after step (V). The development treatment allows the latent image formed in step (V) to be developed. Since the core resin composition functions as a negative photosensitive resin composition, as shown in FIG. 6, the exposed portion 111 is not removed by the development treatment, while the non-exposed portion 112 (see FIG. 5) is removed. The exposed portion 111 of the second composition layer 110 remaining after development may have the same planar shape as the mask pattern of the light-transmitting portion 410 (see FIG. 5) of the mask 400 used in step (V).

[0298] The developing method is usually a wet developing method in which the second composition layer 110 is brought into contact with a developer. Examples of the developer include an alkaline aqueous solution, a water-based developer, and an organic solvent.

[0299] Examples of the alkaline aqueous solution as a developer include an aqueous solution of an alkali metal compound. Examples of the alkaline metal compound include an alkali metal hydroxide such as lithium hydroxide, sodium hydroxide, or potassium hydroxide; an alkali metal carbonate or bicarbonate such as sodium carbonate or sodium bicarbonate; an alkali metal phosphate such as sodium phosphate or potassium phosphate; and an alkali metal pyrophosphate such as sodium pyrophosphate or potassium pyrophosphate. Examples of the alkaline aqueous solution include an aqueous solution of an organic base that does not contain metal ions, such as tetraalkylammonium hydroxide. The alkaline aqueous solution may be used alone or in combination of two or more. Among them, an aqueous solution of tetramethylammonium hydroxide (TMAH) is preferred because it does not contain metal ions. In one example, the pH range of the alkaline aqueous solution is preferably 8 or more, more preferably 9 or more, and preferably 14 or less, more preferably 12 or less, and particularly preferably 11 or less. The base concentration of the alkaline aqueous solution is preferably 0.1% by mass to 10% by mass.

[0300] Examples of organic solvents used as the developer include acetone, ethyl acetate, alkoxyethanol having an alkoxy group having 1 to 4 carbon atoms, ethyl alcohol, isopropyl alcohol, butyl alcohol, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, and diethylene glycol monobutyl ether. One type of organic solvent may be used alone, or two or more types may be used in combination. The concentration of the organic solvent is usually 2% by mass or more, preferably 50% by mass or more, more preferably 70% by mass or more, and particularly preferably 90% by mass or more, based on the total amount of the developer. The developer may be 100% by mass of organic solvent. Examples of organic solvent-based developers used alone include 1,1,1-trichloroethane, N-methylpyrrolidone, N,N-dimethylformamide, cyclohexanone, methyl isobutyl ketone, and γ-butyrolactone.

[0301] The developer may contain additives such as a surfactant and an antifoaming agent, if necessary, to improve the developing action.

[0302] The development time is preferably 10 seconds to 5 minutes. The temperature of the developer during development is not particularly limited, but is preferably 20° C. or higher and preferably 50° C. or lower, more preferably 40° C. or lower.

[0303] Examples of the developing method include a paddle method, a spray method, an immersion method, a brushing method, a slapping method, and an ultrasonic method. Among them, the spray method is suitable for improving the resolution. When the spray method is adopted, the spray pressure is preferably 0.05 MPa to 0.3 MPa.

[0304] After development using the developer, the second composition layer 110 may be further rinsed. Rinsing is preferably performed with a solvent different from the developer. For example, rinsing may be performed with the same type of solvent contained in the core resin composition or water. The rinsing time is preferably 5 seconds to 1 minute.

[0305] The method for producing an optical waveguide according to one embodiment of the present invention includes, after step (VI), step (VII) of curing the second composition layer 110. This step (VII) usually includes heat treating the second composition layer 110. The heat treatment can promote the crosslinking reaction of the (C) crosslinking agent to cure the second composition layer 110. The heat treatment conditions may be selected depending on the type and amount of the resin component in the core resin composition. For example, the heat treatment conditions in step (VII) may be the same as the heat treatment conditions for the first composition layer 210 in step (III).

[0306] 7 is a schematic cross-sectional view for explaining step (VII) of the method for producing an optical waveguide according to one embodiment of the present invention. By curing the second composition layer 110 in step (VII), a core layer 100 is obtained as a cured second composition layer on the lower clad layer 220, as shown in FIG.

[0307] 8 is a schematic cross-sectional view for explaining step (VIII) of the method for producing an optical waveguide according to one embodiment of the present invention. As shown in FIG. 8, the method for producing an optical waveguide according to one embodiment of the present invention includes, after step (VII), step (VIII) of forming a third composition layer 230 containing a cladding resin composition on the core layer 100. The third composition layer 230 is usually formed so as to cover the entire surface of the core layer 100 that is not in contact with the lower cladding layer 220. Thus, the third composition layer 230 is formed so as to cover the core layer 100 and is also formed on the lower cladding layer 220.

[0308] There is no particular limitation on the method of forming the third composition layer 230. For example, the third composition layer 230 may be formed by applying a clad resin composition onto the core layer 100. When applying the clad resin composition onto the core layer 100, the clad resin composition may be applied to the lower clad layer 220 as necessary. The application of the clad resin composition for forming the third composition layer 230 may be performed in the same manner as the application of the clad resin composition for forming the first composition layer 210. After the application of the clad resin composition, the third composition layer 230 may be dried as necessary. The third composition layer 230 may be dried by the same method and conditions as those for drying the first composition layer 210.

[0309] The third composition layer 230 may be formed, for example, using a clad resin sheet. As a specific example, the resin composition layer of the clad resin sheet is laminated on the core layer 100 to form the third composition layer 230 on the core layer 100. When the resin composition layer of the clad resin sheet is laminated on the core layer 100, the resin composition layer of the clad resin sheet may be laminated on the lower clad layer 220 as necessary. The lamination of the clad resin sheet for forming the third composition layer 230 may be performed in the same manner as the lamination of the clad resin sheet for forming the first composition layer 210. When the third composition layer 230 is formed using a clad resin sheet provided with a support, the support may be peeled off in any step.

[0310] The third composition layer 230 formed on the core layer 100 in step (VIII) usually contains a cladding resin composition, and preferably contains only a cladding resin composition.

[0311] The method for producing an optical waveguide according to one embodiment of the present invention includes, after step (VIII), step (IX) of subjecting the third composition layer 230 to an exposure treatment. In this exposure treatment, the third composition layer 230 is irradiated with light. When irradiated with light, the (b) photoacid generator in the third composition layer 230 generates acid. The exposure treatment of the third composition layer 230 can be carried out in the same manner as the exposure treatment of the first composition layer 210.

[0312] The method for producing an optical waveguide according to one embodiment of the present invention includes, after step (IX), step (X) of curing the third composition layer 230. This step (X) usually includes heat treating the third composition layer 230. The heat treatment can cause the crosslinking reaction of the crosslinking agent (c) to proceed using the acid generated in step (IX) as a catalyst, thereby curing the third composition layer 230. The heat treatment of the third composition layer 230 can be carried out in the same manner as the heat treatment of the first composition layer 210.

[0313] 9 is a schematic cross-sectional view for explaining step (X) of the method for producing an optical waveguide according to one embodiment of the present invention. By curing the third composition layer 230 in step (X), a cured third composition layer 240 is obtained on the core layer 100 as shown in FIG. This cured third composition layer 240 forms a part of the cladding layer 200, and may be referred to as the "upper cladding layer" 240 hereinafter. The upper cladding layer 240 and the lower cladding layer 220 form the cladding layer 200. Thus, an optical waveguide 10 including the cladding layer 200 including the lower cladding layer 220 and the upper cladding layer 240, and the core layer 100 provided in the cladding layer 200 can be obtained.

[0314] The method for producing the optical waveguide 10 may further include any optional steps in combination with the steps described above. The method for manufacturing the optical waveguide 10 may include, for example, a step of forming a protective layer (not shown). The method for manufacturing the optical waveguide 10 may also include, for example, a step of dicing the manufactured optical waveguide 10.

[0315] The above-mentioned steps may be repeated in the method for producing the optical waveguide 10. For example, steps (I) to (XI) may be repeated to produce an optical waveguide having a multilayer structure in which core layers and clad layers are alternately provided on the substrate 300 in the thickness direction.

[0316] [7. Optical / electrical hybrid board] An optical / electrical hybrid board according to an embodiment of the present invention includes the optical waveguide described above. Typically, the optical / electrical hybrid board includes an optical waveguide and an electric circuit board. The electric circuit board may include electronic components and wiring connected to the electronic components. Examples of the electronic components include passive components such as capacitors, inductors, and resistors; active components such as semiconductor chips; and the like. The optical waveguide and the wiring of the electric circuit board may be connected via a photoelectric conversion element. The photoelectric conversion element may include a combination of a light-emitting element (e.g., a surface-emitting light-emitting diode) capable of converting electricity into light, and a light-receiving element (e.g., a photodiode) capable of converting light into electricity. Furthermore, the optical / electrical hybrid board may include an optical element such as a mirror for adjusting the optical path.

[0317] A preferred example of an opto-electrical hybrid board is one that includes a chip in which an optical integrated circuit is formed on a silicon wafer. This chip is expected to be put to practical use in the near future using silicon photonics, and is expected to be mounted, for example, in a semiconductor package. An opto-electrical hybrid board that includes this chip includes, for example, an electric circuit board, a chip mounted on the electric circuit board, and an optical waveguide. The optical waveguide can be used to connect the wiring of the electric circuit board to the chip, or to connect multiple chips together.

[0318] In chips manufactured by silicon photonics, generally, light with wavelengths of 1310 nm and 1550 nm is often used, with 1310 nm being the most common (Sho Yoshida, Daisuke Suganuma, Takaaki Ishigure, "Fabrication of Single-Mode Polymer Waveguides and Low Loss Using the Mosquito Method," 28th Spring Lecture Meeting of the Japan Institute of Electronics Packaging, 2014). Therefore, it is preferable that the optical waveguide is capable of transmitting light with wavelengths of 1310 nm and 1550 nm or close thereto, and for example, it is preferable that the optical waveguide is capable of transmitting light with wavelengths of 1300 nm to 1320 nm. The optical waveguide according to the above-mentioned embodiment is capable of transmitting light with these wavelengths.

[0319] Generally, the single mode can achieve faster transmission than the multimode. Therefore, from the viewpoint of high-speed transmission, the single mode optical waveguide is preferable as an optical waveguide applied to an optical-electrical hybrid circuit. In the single mode optical waveguide, the width of the core layer is preferably small. For example, it is preferable to form a core layer having a width of 10 μm or less, or 5 μm or less. In addition, an optical waveguide having such a small core layer is preferable from the viewpoint of increasing the degree of freedom in package design when the optical waveguide is applied to a semiconductor package. According to the optical waveguide according to the above-mentioned embodiment, it is possible to reduce the width of the core layer as described above.

[0320] In addition, it is generally desirable for a single-mode optical waveguide to have a small numerical aperture NA. The optical waveguide according to the above-described embodiment can have a small numerical aperture NA, and therefore can be applied to a single mode in terms of the numerical aperture NA as well.

[0321] On the other hand, when connecting multiple opto-electric hybrid boards, the boards may be connected via optical fibers. For example, multiple opto-electric hybrid boards may be installed in a rack, and the opto-electric hybrid boards may be connected to each other via optical fibers. Multimode optical fibers are the mainstream for connecting boards in this way. Therefore, from the viewpoint of enabling connection with the optical fibers, a multimode optical waveguide may be adopted as the optical waveguide provided in the opto-electric hybrid board.

[0322] From the viewpoint of increasing versatility, it is desirable that the optical waveguide is applicable to both single mode and multimode. Furthermore, it is desirable to reduce the minimum width of the core layer of the optical waveguide to increase the degree of freedom of the line width of the core layer. According to the optical waveguide according to the above-mentioned embodiment, a high fine wiring formation ability can be achieved by using a core resin composition and a clad resin composition as a photosensitive resin composition having excellent resolution, so that the minimum width of the core layer can be reduced. Furthermore, according to the optical waveguide according to the above-mentioned embodiment, both single mode and multimode optical waveguides can be obtained. Therefore, the optical waveguide according to the above-mentioned embodiment can be applied in a wide range. And, since it is applicable in such a wide range and can suppress the transmission loss of light, the optical waveguide according to the above-mentioned embodiment is suitable for application to an optical-electrical hybrid board.

[0323] When connecting optical waveguides, it is preferable that the modes of the optical waveguides to be connected are the same, and it is preferable that the numerical apertures NA are close to each other. For example, when sending light from a first optical waveguide having a numerical aperture NA1 to a second optical waveguide having a numerical aperture NA2, it is preferable that NA1≧Na2 in terms of suppressing light leakage at the connection part. Therefore, when connecting multiple optical waveguides provided on one opto-electrical hybrid board, it is preferable to appropriately set the numerical apertures NA of those optical waveguides as described above.

[0324] In addition, when connecting an optical waveguide to an optical fiber, it is desirable that the optical waveguide has a numerical aperture NA in an appropriate range according to the numerical aperture of the optical fiber. For example, as a single-mode optical fiber with a large numerical aperture, one with a numerical aperture of 0.35 has been put to practical use. Therefore, from the viewpoint of enabling connection to a single-mode optical fiber, it is desirable that the single-mode optical waveguide has a numerical aperture NA that is equal to or less than the numerical aperture of the optical fiber. According to the optical waveguide of the above-mentioned embodiment, the transmission loss can be suppressed at a numerical aperture NA of 0.35 or less, and therefore it is preferably applicable to an optical waveguide to be connected to a single-mode optical fiber. EXAMPLES

[0325] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples. In the following description, "parts" and "%" representing amounts mean "parts by mass" and "% by mass", respectively, unless otherwise specified. Furthermore, the operations described below were carried out in the atmosphere at room temperature and normal pressure (23°C and 1 atm), unless otherwise specified.

[0326] (Synthesis Example 1) A reaction solution was obtained by mixing 100 g of 4-hydroxyphenyl methacrylate (Seiko Chemical Co., Ltd.), 300 g of N,N-dimethylacetamide, and 4.0 g of azobisisobutyronitrile (Tokyo Chemical Industry Co., Ltd.) in a flask. The reaction solution was heated to 80°C under a nitrogen atmosphere and subjected to a polymerization reaction for 8 hours. Then, 200 g of methanol was added to the reaction solution and dropped into a large amount of stirred ion-exchanged water. The precipitated polymer was filtered and dried to obtain a polymer. The weight average molecular weight of the polymer was measured by GPC and found to be 20,000 in terms of polystyrene.

[0327] [Manufacturing Examples 1-13] The materials shown in Tables 1 and 2 were blended in the amounts shown and mixed using a high-speed rotating mixer to obtain a resin varnish as a resin composition. In Tables 1 and 2, the numerical values ​​of each component represent parts by mass. In addition, the meanings of the abbreviations in Tables 1 and 2 are as follows.

[0328] <(A) Phenolic resin> "TR4020G": Manufactured by Asahi Yokuzai Co., Ltd., weight average molecular weight: 13000. "BisP-E": 1,1-bis(4-hydroxyphenyl)propane, manufactured by Asahi Organic Chemicals. "Bis-AF": 2,2-bis(4-hydroxyphenyl)hexafluoropropane, manufactured by Asahi Organic Chemicals Co., Ltd. "Marukalinker M": Polyparahydroxystyrene manufactured by Maruzen Petrochemical Co., Ltd. "Synthesis Example 1": the polymer synthesized in Synthesis Example 1. "J-DPP-85": Dicyclopentadiene skeleton phenol manufactured by JFE Chemical Corporation. "SPDI": Spirobiindanphenol manufactured by JFE Chemical Corporation. "TBIS-RX": spiro[fluorene-9,9'-xanthene]-3',6'-diol, manufactured by Taoka Chemical Industry Co., Ltd.

[0329] <(B) Photoacid generator> "PAG-103": a compound manufactured by BASF and having the following structural formula.

[0330] [ka]

[0331] <(C) Crosslinking agent> "MW-390" Hexamethoxymethylmelamine, manufactured by Sanwa Chemical Co., Ltd.

[0332] <(D) Polymer> "CB-3098": Manufactured by Soken Chemical Industries, an acrylic resin that does not contain phenolic hydroxyl groups or methoxymethyl groups. Weight average molecular weight: 3000.

[0333] <(E) Amine Compound> "Trioctylamine": Tri-n-octylamine manufactured by TCI.

[0334] <(F) Optional Component> "ZCR-1797H": acid-modified epoxy acrylate having a biphenyl skeleton, manufactured by Nippon Kayaku Co., Ltd. (70% solution). "FA-324A": Ethylene oxide modified bisphenol A diacrylate, manufactured by Showa Denko. "NC-3000H": Biphenyl-based epoxy resin, manufactured by Nippon Kayaku Co., Ltd. "Omnirad819": phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, manufactured by IGM.

[0335] <(G) Solvent> "MEK": Methyl ethyl ketone, manufactured by Junsei Chemical Co., Ltd. "Cyclohexanone": dipentaerythritol hexaacrylate, manufactured by Nippon Kayaku Co., Ltd. "PGMEAc": propylene glycol monomethyl ether acetate, manufactured by Kanto Chemical Co., Ltd.

[0336] [Manufacturing of resin sheets] Using the resin varnish produced in the above-mentioned Production Example, a plurality of resin sheets having resin composition layers with different thicknesses were produced by the following method.

[0337] A polyethylene terephthalate film (Toray Industries, Inc., "Lumirror T6AM", thickness 38 μm, softening point 130 ° C.) was prepared as a support. The resin varnish was uniformly applied to the support with a die coater so that the thickness of the resin composition layer after drying was 5 μm, 6.5 μm, 8 μm, 10 μm, 15 μm or 20 μm, and dried at 80 ° C. to 110 ° C. (maximum temperature 110 ° C.) for 7 minutes to form a resin composition layer. Next, a cover film (biaxially oriented polypropylene film, Oji F-Tex Co., Ltd., "MA-411") was placed on the surface of the resin composition layer and laminated at 80 ° C. to produce a resin sheet having a three-layer structure of support / resin composition layer / cover film.

[0338] [Measurement of refractive index of cured resin composition] The refractive index of the cured product of the resin composition contained in the resin varnish produced in the above-mentioned Production Example was measured by the following method using a resin sheet. The cover film was peeled off from the resin sheet having a 6.5 μm-thick resin composition layer. The resin sheet was then laminated on a silicon wafer at 80° C., and the support was peeled off to form a 6.5 μm-thick resin composition layer on the silicon wafer. Thereafter, the resin composition layer was exposed to light at an optimal exposure dose of 3000 mJ using a projection exposure device (Ushio Inc.'s "UFX-2240"). After exposure, the layer was heated at 90° C. for 3 minutes, and then a 2.38 mass % aqueous solution of tetramethylammonium hydroxide at 23° C. was sprayed onto the resin composition layer as a developer at a spray pressure of 0.1 MPa for 30 seconds to perform spray development. After spray development, the resin composition layer was exposed to light at 3 J / cm 2The sample was then subjected to UV irradiation for 100 s, followed by heat treatment at 190°C for 90 minutes in a nitrogen atmosphere to obtain a sample formed of a cured product of the resin composition. The refractive index n (1310 nm) of the obtained sample was measured at room temperature and normal pressure using a 1310 nm laser beam with a 2010M prism coupler (manufactured by Metricon).

[0339] [Evaluation of Resolution of Resin Composition] The resolution of the resin composition contained in the resin varnish produced in the above-mentioned Production Example was evaluated by the following method using a resin sheet.

[0340] A copper layer of a glass epoxy substrate (copper-clad laminate) having a copper layer of 18 μm in thickness was roughened with a surface treatment agent (CZ8100, manufactured by MEC Co., Ltd.) containing an organic acid to prepare a substrate. The cover film was peeled off from the resin sheet prepared in Production Example 1, and the resin sheet was laminated to the substrate at 100° C., and the support was peeled off to form a resin composition layer. Thereafter, the entire surface of the resin composition layer was exposed to light with an optimal exposure dose of 3000 mJ using a projection exposure device ("UFX-2240" manufactured by Ushio Inc.). After exposure, the resin composition layer was heated at 90° C. for 3 minutes, and then a 2.38% by mass aqueous solution of tetramethylammonium hydroxide at 23° C. was sprayed as a developer at a spray pressure of 0.1 MPa for 30 seconds to perform spray development. After development, the resin composition layer was exposed to light with 3 J / cm 2 The copper-clad laminate was then exposed to ultraviolet light for 100 s, and then heat-treated at 190° C. for 90 minutes in a nitrogen atmosphere to form a lower clad layer on the copper-clad laminate.

[0341] The cover film was peeled off from the resin sheet having a 10 μm thick resin composition layer produced in each of the above-mentioned production examples. The resin sheet was placed on the lower clad layer so that the resin composition layer of the resin sheet and the lower clad layer were in contact with each other, and laminated using a vacuum laminator ("VP160" manufactured by Nikko Materials Co., Ltd.) to form a resin composition layer on the lower clad layer. The lamination conditions were a vacuum drawing time of 30 seconds, a pressure bonding temperature of 100°C, a pressure bonding pressure of 0.7 MPa, and a pressure application time of 30 seconds. This resulted in a laminate having a copper-clad laminate, a lower clad layer, and a resin sheet in this order. Thereafter, the support was peeled off to expose the resin composition layer.

[0342] The resin composition layer was exposed to light at an optimal exposure dose of 200 mJ to 2000 mJ using a projection exposure apparatus (Ushio Inc.'s "UFX-2240"). The exposure was performed using a quartz glass mask having a first mask pattern for drawing straight lines with L / S (line / space) 10 μm / 10 μm, a second mask pattern for drawing straight lines with L / S (line / space) 5 μm / 50 μm, and a third mask pattern for drawing straight lines with L / S (line / space) 3 μm / 3 μm. After the exposure, the resin composition layer was heated at 90° C. for 3 minutes, and then a 2.38 mass% aqueous solution of tetramethylammonium hydroxide at 23° C. was sprayed as a developer at a spray pressure of 0.1 MPa for 30 seconds to perform spray development. After the spray development, the resin composition layer was sprayed with 3 J / cm 2 This was followed by a heat treatment at 190°C for 90 minutes in a nitrogen atmosphere to obtain a sample having a silicon wafer, a lower clad layer, and a line layer (a layer formed of a cured product of the resin composition) in that order.

[0343] The obtained sample was observed with a scanning electron microscope (SEM) (magnification 2000 times) and the minimum fine line formation width (the width of the line layer with the smallest width among the line layers that could be formed) was measured. The aspect ratio was calculated by dividing the thickness of the line layer by the minimum fine line formation width. If the aspect ratio of all line layers having a line width of 10 μm or less was 1 or more, the resolution was evaluated as "excellent." If the aspect ratio of all line layers having a line width of 10 μm or less was 0.6 or more and less than 1, the resolution was evaluated as "fair." If the aspect ratio of at least one line layer having a line width of 10 μm or less was less than 0.6, the resolution was evaluated as "poor." Here, the line width refers to the width of the line layer.

[0344] [Measurement of elongation at break of cured resin composition] The cover film was peeled off from the resin film having a 15 μm thick resin composition layer produced in the above-mentioned production example. The resin composition layer was then irradiated with 1000 mJ of ultraviolet light and heated at 190° C. for 90 minutes in a nitrogen atmosphere to thermally cure the resin composition layer. The support was then peeled off to obtain a sample film formed of a cured product of the resin composition. The obtained sample film was subjected to a tensile test using a Tensilon universal testing machine (Orientec's "RTC-1250A") in accordance with the Japanese Industrial Standards (JIS K7127) to measure the elongation at break. The greater the elongation at break, the higher the strength of the sample film, and therefore the cured product has excellent mechanical strength. "Excellent": Elongation at break is 1% or more. "Poor": Elongation at break is less than 1%.

[0345] [Measurement of absorbance of resin composition solution] A solution of the resin composition contained in the resin varnish produced in the above-mentioned Production Example was prepared, and the absorbance of the solution was measured by the following method. That is, a mixed solvent of MEK and cyclopentanone (MEK:pentanone=1:1) was mixed with the resin varnish produced in the production example to prepare a solution with a resin composition concentration of 20 mass %. This solution was placed in a 1 cm quartz cell, and the absorbance Abs at a wavelength of 1310 nm was measured using a UV-Vis-NIR spectrophotometer (V-770 manufactured by Nippon Bunko Co., Ltd.).

[0346] [Measurement of the linear thermal expansion coefficient of the cured resin composition] The linear thermal expansion coefficient of the cured product of the resin composition contained in the resin varnish produced in the above-mentioned Production Example was measured by the following method using a resin sheet. That is, the cover film was peeled off from the resin film having a resin composition layer having a thickness of 15 μm produced in the production example. Then, the resin composition layer was irradiated with 1000 mJ of ultraviolet light and heated at 190 ° C for 90 minutes in a nitrogen atmosphere to thermally cure the resin composition layer. Then, the support was peeled off to obtain a cured product for evaluation. The cured product for evaluation was cut to obtain a test piece having a width of 5 mm and a length of 15 mm. A thermomechanical analysis of the test piece was performed by a tensile load method using a thermomechanical analyzer (Rigaku Corporation, Thermo Plus, TMA8310). In the thermomechanical analysis, the test piece was mounted on the device and then measured twice in succession under the measurement conditions of a load of 1 g and a temperature rise rate of 5 ° C / min. The linear thermal expansion coefficient of the cured product was measured by calculating the average linear thermal expansion coefficient (ppm) from 25 ° C to 150 ° C in the second measurement.

[0347] [Measurement of surface roughness of cured resin composition] The surface roughness of the cured product of the resin composition contained in the resin varnish produced in the above-mentioned Production Example was measured by the following method using a resin sheet. That is, the cover film was peeled off from the resin film having a 15 μm-thick resin composition layer produced in the production example. Then, a resin sheet was placed on a 4-inch silicon wafer so that the resin composition layer and the silicon wafer were in contact with each other, and laminated using a vacuum laminator ("VP160" manufactured by Nikko Materials Co., Ltd.). The lamination conditions were a vacuum drawing time of 30 seconds, a pressure bonding temperature of 100°C, a pressure bonding pressure of 0.7 MPa, and a pressure application time of 30 seconds. Then, the support was peeled off, and exposure was performed with 3000 mJ of ultraviolet light using a projection exposure device ("UFX-2240" manufactured by Ushio Inc.). After exposure, heating was performed at 90°C for 3 minutes, and then a 2.38% by mass aqueous solution of tetramethylammonium hydroxide at 23°C was sprayed as a developer on the resin composition layer at a spray pressure of 0.1 MPa for 30 seconds to perform spray development. After the spray development, the sample was placed in a clean oven, heated from room temperature to 190° C., and after reaching 190° C., heated for 90 minutes in a nitrogen atmosphere to cure the resin composition layer. The surface condition of the cured product was evaluated with a non-contact interference microscope (manufactured by WYKO Bruker AXS), and the arithmetic mean roughness Ra was measured as the surface roughness of the cured product.

[0348] [Composition and properties of resin composition] The compositions and properties of the resin compositions produced in the above-mentioned Production Examples are shown in the following Tables 1 and 2. In the following Tables 1 and 2, the amounts of the reagents are expressed in parts by mass. In addition, in the following Tables 1 and 2, the meanings of the abbreviations are as follows. F content: The amount of fluorine atoms (% by mass) relative to 100% by mass of the non-volatile components of the resin composition. n(1310 nm): The refractive index of the cured resin composition at a measurement wavelength of 1310 nm. Abs: absorbance of the resin composition solution at a measurement wavelength of 1310 nm. CTE: Coefficient of linear thermal expansion of the cured resin composition.

[0349] [Table 1]

[0350] [Table 2]

[0351] [Example 1] (1-1. Formation of the lower cladding layer) The cover film was peeled off from the resin sheet having a 10 μm-thick resin composition layer produced in Production Example 5. The resin sheet was placed on a 4-inch silicon wafer so that the resin composition layer and the silicon wafer were in contact with each other, and laminated using a vacuum laminator ("VP160" manufactured by Nikko Materials Co., Ltd.). The lamination conditions were a vacuum drawing time of 30 seconds, a pressure bonding temperature of 100°C, a pressure bonding pressure of 0.7 MPa, and a pressure application time of 30 seconds. Thereafter, the support was peeled off to obtain an intermediate laminate I having a silicon wafer and a resin composition layer.

[0352] The resin composition layer of the intermediate laminate I was exposed to 3000 mJ of ultraviolet light using a projection exposure device (Ushio Inc.'s "UFX-2240"). After exposure, the intermediate laminate I was placed in a clean oven and heated from room temperature to 190°C. After reaching 190°C, a heat treatment was carried out for 90 minutes in a nitrogen atmosphere to harden the resin composition layer. A lower clad layer was formed by hardening the resin composition layer, and an intermediate laminate II including a silicon wafer and a lower clad layer was obtained.

[0353] (1-2. Formation of the core layer) The cover film was peeled off from the resin sheet having a 5 μm-thick resin composition layer produced in Production Example 1. A resin sheet was placed on the surface of the lower clad layer of the intermediate laminate II so that the resin composition layer and the lower clad layer were in contact with each other, and laminated using a vacuum laminator ("VP160" manufactured by Nikko Materials Co., Ltd.). The lamination conditions were a vacuum drawing time of 30 seconds, a pressure bonding temperature of 100°C, a pressure bonding pressure of 0.7 MPa, and a pressure application time of 30 seconds. Thereafter, the support was peeled off to obtain an intermediate laminate III having a silicon wafer, a lower clad layer (base clad layer), and a resin composition layer in this order.

[0354] The resin composition layer of the intermediate laminate III was exposed to ultraviolet light at an optimal exposure dose of 200 mJ to 2000 mJ using a projection exposure device (Ushio Inc.'s "UFX-2240"). The exposure was performed using a quartz glass mask having a mask pattern capable of drawing multiple straight lines with a length of 1 cm and a L / S (line / space) of 5 μm / 100 μm, a mask pattern capable of drawing multiple straight lines with a length of 2 cm and a L / S (line / space) of 5 μm / 100 μm, and a mask pattern capable of drawing multiple straight lines with a length of 3 cm and a L / S (line / space) of 5 μm / 100 μm. In the L / S of this quartz glass mask, the line corresponds to the width of the core layer, and the space corresponds to the interval between the core layers. After the exposure, the resin composition layer was heated at 90°C for 3 minutes, and then sprayed with a 2.38% by mass aqueous solution of tetramethylammonium hydroxide at 23°C as a developer at a spray pressure of 0.1 MPa for 30 seconds to perform spray development. After the spray development, the intermediate laminate III was placed in a clean oven, heated from room temperature to 190°C, and after reaching 190°C, a heat treatment was performed for 90 minutes in a nitrogen atmosphere to harden the resin composition layer. A core layer was formed by hardening the resin composition layer, and an intermediate laminate IV having a silicon wafer, a lower clad layer, and a core layer in this order was obtained.

[0355] (1-3. Formation of upper cladding layer) The cover film was peeled off from the resin sheet having a 20 μm-thick resin composition layer produced in Production Example 5. A resin sheet was placed on the core layer of the intermediate laminate IV so that the resin composition layer and the core layer were in contact with each other, and laminated using a vacuum laminator ("VP160" manufactured by Nikko Materials Co., Ltd.). The lamination conditions were a vacuum drawing time of 30 seconds, a pressure bonding temperature of 100°C, a pressure bonding pressure of 0.7 MPa, and a pressure application time of 30 seconds. Thereafter, the support was peeled off to obtain an intermediate laminate V having a silicon wafer, a lower clad layer, a core layer, and a resin composition layer in this order.

[0356] The resin composition layer of the intermediate laminate V was exposed to 3000 mJ of ultraviolet light using a projection exposure device (Ushio Inc.'s "UFX-2240"). After exposure, the intermediate laminate V was placed in a clean oven and heated from room temperature to 190°C. After reaching 190°C, a heat treatment was performed for 90 minutes in a nitrogen atmosphere to harden the resin composition layer. An upper clad layer was formed by hardening the resin composition layer, and a sample laminate having a silicon wafer, a lower clad layer, a core layer, and an upper clad layer in this order was obtained.

[0357] In this sample laminate, the combination of the lower cladding layer and the upper cladding layer constituted the cladding layer. Thus, an optical waveguide was obtained that included the cladding layer and the core layer in the cladding layer. In addition, in this sample laminate, the core layer had linear patterns of lengths of 1 cm, 2 cm, and 3 cm corresponding to the mask patterns of the quartz glass mask, and the widths (line widths) and intervals (spaces) of the core layer included in these patterns were consistent with the widths (line widths) and intervals (spaces) of the mask patterns.

[0358] [Example 2] (2-1. Formation of the lower cladding layer) An intermediate laminate II comprising a silicon wafer and a lower clad layer was produced in the same manner as in step (1-1) of Example 1, except that a resin sheet having a 10 μm-thick resin composition layer produced in Production Example 3 was used as the resin sheet for forming the lower clad layer.

[0359] (2-2. Formation of the core layer) Except for using a resin sheet having a 5 μm-thick resin composition layer produced in Production Example 8 as the resin sheet for forming the core layer, a core layer was formed on the lower clad layer of the intermediate laminate II obtained in the above-mentioned step (2-1) by the same method as step (1-2) of Example 1, to obtain an intermediate laminate IV having a silicon wafer, a lower clad layer, and a core layer in this order.

[0360] (2-3. Formation of upper cladding layer) Except for using a resin sheet having a 20 μm-thick resin composition layer produced in Production Example 3 as the resin sheet for forming the upper clad layer, an upper clad layer was formed on the core layer of the intermediate laminate IV obtained in the above step (2-2) in the same manner as in step (1-3) of Example 1, to produce a sample laminate having a silicon wafer, a lower clad layer, a core layer, and an upper clad layer in this order.

[0361] [Example 3] (3-1. Formation of the lower cladding layer) An intermediate laminate II including a silicon wafer and a lower clad layer was produced in the same manner as in step (1-1) of Example 1.

[0362] (3-2. Formation of the core layer) The resin varnish produced in Production Example 2 was applied to the surface of the lower clad layer of the intermediate laminate II obtained in the above step (3-1) using a spin coater ("MS-B100" manufactured by Mikasa Co., Ltd.), and heated and dried on a hot plate at 110°C for 3 minutes to form a resin composition layer having a thickness of 3 μm. This resulted in an intermediate laminate III having a silicon wafer, a lower clad layer (base clad layer), and a resin composition layer in this order.

[0363] The resin composition layer of the intermediate laminate III was exposed to light at an optimal exposure dose of 200 mJ to 2000 mJ using a projection exposure apparatus (Ushio Inc.'s "UFX-2240"). The exposure was performed using a quartz glass mask having a mask pattern capable of drawing multiple straight lines with a length of 1 cm and a L / S (line / space) of 3 μm / 100 μm, a mask pattern capable of drawing multiple straight lines with a length of 2 cm and a L / S (line / space) of 3 μm / 100 μm, and a mask pattern capable of drawing multiple straight lines with a length of 3 cm and a L / S (line / space) of 3 μm / 100 μm. After the exposure, the resin composition layer was heated at 90° C. for 3 minutes, and then spray-developed by spraying a 2.38% by mass aqueous solution of tetramethylammonium hydroxide at 23° C. as a developer at a spray pressure of 0.1 MPa for 30 seconds. After the spray development, the intermediate laminate III was placed in a clean oven and heated from room temperature to 190° C. After reaching 190° C., a heat treatment was carried out for 90 minutes in a nitrogen atmosphere to cure the resin composition layer. A core layer was formed by curing the resin composition layer, and an intermediate laminate IV including a silicon wafer, a lower clad layer, and a core layer in this order was obtained.

[0364] (3-3. Formation of upper cladding layer) Using the same method as in step (1-3) of Example 1, an upper clad layer was formed on the core layer of the intermediate laminate IV obtained in the above step (3-2), to obtain a sample laminate having a silicon wafer, a lower clad layer, a core layer, and an upper clad layer in this order.

[0365] [Example 4] (4-1. Formation of the lower cladding layer) An intermediate laminate II comprising a silicon wafer and a lower clad layer was produced in the same manner as in step (1-1) of Example 1, except that a resin sheet having a 10 μm-thick resin composition layer produced in Production Example 6 was used as the resin sheet for forming the lower clad layer.

[0366] (4-2. Formation of the core layer) Using the same method as in step (3-2) of Example 3, a core layer was formed on the lower clad layer of the intermediate laminate II obtained in the above-mentioned step (4-1) to obtain an intermediate laminate IV having a silicon wafer, a lower clad layer, and a core layer in this order.

[0367] (4-3. Formation of upper cladding layer) Except for using a resin sheet having a 20 μm-thick resin composition layer produced in Production Example 6 as the resin sheet for forming the upper clad layer, an upper clad layer was formed on the core layer of the intermediate laminate IV obtained in the above-mentioned step (4-2) by the same method as in step (1-3) of Example 1, to obtain a sample laminate having a silicon wafer, a lower clad layer, a core layer, and an upper clad layer in this order.

[0368] [Example 5] (5-1. Formation of the lower cladding layer) An intermediate laminate II including a silicon wafer and a lower clad layer was produced in the same manner as in step (1-1) of Example 1, except that the resin composition layer was formed using the resin varnish produced in Production Example 4 in the manner described below.

[0369] A resin composition layer was formed using the resin varnish produced in Production Example 4 by the following method: The resin varnish produced in Production Example 4 was applied onto a 4-inch silicon wafer using a spin coater ("MS-B100" manufactured by Mikasa Co., Ltd.), and dried by heating on a hot plate at 110°C for 3 minutes to form a resin composition layer having a thickness of 10 μm.

[0370] (5-2. Formation of the core layer) As the resin sheet for forming the core layer, a resin sheet having a resin composition layer with a thickness of 8 μm produced in Production Example 1 was used. In addition, the quartz glass mask was changed to a quartz glass mask having a mask pattern capable of drawing a plurality of straight lines with a length of 1 cm and a L / S (line / space) of 8 μm / 100 μm, a mask pattern capable of drawing a plurality of straight lines with a length of 2 cm and a L / S (line / space) of 8 μm / 100 μm, and a mask pattern capable of drawing a plurality of straight lines with a length of 3 cm and a L / S (line / space) of 8 μm / 100 μm. A core layer was formed on the surface of the lower clad layer of the intermediate laminate II obtained in the above step (5-1) by the same method as in step (1-2) of Example 1 except for the above matters, to obtain an intermediate laminate IV having a silicon wafer, a lower clad layer, and a core layer in this order.

[0371] (5-3. Formation of upper cladding layer) An upper clad layer was formed on the core layer of the intermediate laminate IV obtained in the above-mentioned step (5-2) by the same method as step (1-3) of Example 1, except that the resin composition layer was formed using the resin varnish produced in Production Example 4 by the following method, thereby obtaining a sample laminate having a silicon wafer, a lower clad layer, a core layer, and an upper clad layer in this order.

[0372] The resin composition layer was formed using the resin varnish produced in Production Example 4 by the following method: The resin varnish produced in Production Example 4 was applied to the surface of the core layer of the intermediate laminate IV using a spin coater ("MS-B100" manufactured by Mikasa Co., Ltd.), and dried by heating on a hot plate at 110°C for 3 minutes to form a resin composition layer having a thickness of 20 μm.

[0373] [Example 6] (6-1. Formation of the lower cladding layer) An intermediate laminate II including a silicon wafer and a lower clad layer was produced in the same manner as in step (1-1) of Example 1.

[0374] (6-2. Formation of the core layer) The thickness of the resin varnish was changed to 5 μm. The quartz glass mask was changed to a quartz glass mask having a mask pattern capable of drawing a plurality of straight lines with a length of 1 cm at L / S (line / space) 8 μm / 100 μm, a mask pattern capable of drawing a plurality of straight lines with a length of 2 cm at L / S (line / space) 8 μm / 100 μm, and a mask pattern capable of drawing a plurality of straight lines with a length of 3 cm at L / S (line / space) 8 μm / 100 μm. A core layer was formed on the surface of the lower clad layer of the intermediate laminate II obtained in the above step (6-1) by the same method as in step (3-2) of Example 3 except for the above matters, to obtain an intermediate laminate IV having a silicon wafer, a lower clad layer, and a core layer in this order.

[0375] (6-3. Formation of upper cladding layer) Using the same method as in step (1-3) of Example 1, an upper clad layer was formed on the core layer of the intermediate laminate IV obtained in the above step (6-2), to obtain a sample laminate having a silicon wafer, a lower clad layer, a core layer, and an upper clad layer in this order.

[0376] [Example 7] (7-1. Formation of the lower cladding layer) An intermediate laminate II including a silicon wafer and a lower clad layer was produced in the same manner as in step (1-1) of Example 1.

[0377] (7-2. Formation of the core layer) The thickness of the resin varnish was changed to 3 μm. The quartz glass mask was changed to a quartz glass mask having a mask pattern capable of drawing a plurality of straight lines with a length of 1 cm and a L / S (line / space) of 4.5 μm / 100 μm, a mask pattern capable of drawing a plurality of straight lines with a length of 2 cm and a L / S (line / space) of 4.5 μm / 100 μm, and a mask pattern capable of drawing a plurality of straight lines with a length of 3 cm and a L / S (line / space) of 4.5 μm / 100 μm. A core layer was formed on the surface of the lower clad layer of the intermediate laminate II obtained in the above step (7-1) by the same method as in step (3-2) of Example 3 except for the above items, to obtain an intermediate laminate IV having a silicon wafer, a lower clad layer, and a core layer in this order.

[0378] (7-3. Formation of upper cladding layer) Using the same method as in step (1-3) of Example 1, an upper clad layer was formed on the core layer of the intermediate laminate IV obtained in the above step (7-2), thereby obtaining a sample laminate having a silicon wafer, a lower clad layer, a core layer, and an upper clad layer in this order.

[0379] [Example 8] (8-1. Formation of the lower cladding layer) An intermediate laminate II comprising a silicon wafer and a lower clad layer was produced in the same manner as in step (1-1) of Example 1, except that a resin sheet having a 10 μm-thick resin composition layer produced in Production Example 6 was used as the resin sheet for forming the lower clad layer.

[0380] (8-2. Formation of the core layer) The thickness of the resin varnish was changed to 3 μm. The quartz glass mask was changed to a quartz glass mask having a mask pattern capable of drawing a plurality of straight lines with a length of 1 cm and a L / S (line / space) of 4.5 μm / 100 μm, a mask pattern capable of drawing a plurality of straight lines with a length of 2 cm and a L / S (line / space) of 4.5 μm / 100 μm, and a mask pattern capable of drawing a plurality of straight lines with a length of 3 cm and a L / S (line / space) of 4.5 μm / 100 μm. A core layer was formed on the surface of the lower clad layer of the intermediate laminate II obtained in the above step (8-1) by the same method as in step (3-2) of Example 3 except for the above items, to obtain an intermediate laminate IV having a silicon wafer, a lower clad layer, and a core layer in this order.

[0381] (8-3. Formation of upper cladding layer) Except for using a resin sheet having a 20 μm-thick resin composition layer produced in Production Example 6 as the resin sheet for forming the upper clad layer, an upper clad layer was formed on the core layer of the intermediate laminate IV obtained in the above-mentioned step (8-2) by the same method as in step (1-3) of Example 1, to obtain a sample laminate having a silicon wafer, a lower clad layer, a core layer, and an upper clad layer in this order.

[0382] [Example 9] (9-1. Formation of the lower cladding layer) An intermediate laminate II including a silicon wafer and a lower clad layer was produced in the same manner as in step (1-1) of Example 1.

[0383] (9-2. Formation of the core layer) As the resin sheet for forming the core layer, a resin sheet having a resin composition layer with a thickness of 15 μm produced in Production Example 1 was used. In addition, the quartz glass mask was changed to a quartz glass mask having a mask pattern capable of drawing a plurality of straight lines with a length of 1 cm and a L / S (line / space) of 15 μm / 100 μm, a mask pattern capable of drawing a plurality of straight lines with a length of 2 cm and a L / S (line / space) of 15 μm / 100 μm, and a mask pattern capable of drawing a plurality of straight lines with a length of 3 cm and a L / S (line / space) of 15 μm / 100 μm. A core layer was formed on the surface of the lower clad layer of the intermediate laminate II obtained in the above step (9-1) by the same method as in step (1-2) of Example 1 except for the above matters, to obtain an intermediate laminate IV having a silicon wafer, a lower clad layer, and a core layer in this order.

[0384] (9-3. Formation of upper cladding layer) Using the same method as in step (1-3) of Example 1, an upper clad layer was formed on the core layer of the intermediate laminate IV obtained in the above step (9-2), thereby obtaining a sample laminate having a silicon wafer, a lower clad layer, a core layer, and an upper clad layer in this order.

[0385] [Example 10] (10-1. Formation of the lower cladding layer) An intermediate laminate II comprising a silicon wafer and a lower clad layer was produced in the same manner as in step (1-1) of Example 1, except that a resin sheet having a 10 μm-thick resin composition layer produced in Production Example 12 was used as the resin sheet for forming the lower clad layer.

[0386] (10-2. Formation of the core layer) Except for using a resin sheet having a 5 μm-thick resin composition layer produced in Production Example 10 as the resin sheet for forming the core layer, a core layer was formed on the surface of the lower clad layer of the intermediate laminate II obtained in the above-mentioned step (10-1) by the same method as step (1-2) of Example 1, to obtain an intermediate laminate IV having a silicon wafer, a lower clad layer, and a core layer in this order.

[0387] (10-3. Formation of upper cladding layer) An upper clad layer was formed on the core layer of the intermediate laminate IV obtained in the above-mentioned step (10-2) by the same method as in step (1-3) of Example 1, except that a resin sheet having a 20 μm-thick resin composition layer produced in Production Example 12 was used as the resin sheet for forming the upper clad layer, thereby obtaining a sample laminate having a silicon wafer, a lower clad layer, a core layer, and an upper clad layer in this order.

[0388] [Example 11] (11-1. Formation of the lower cladding layer) An intermediate laminate II comprising a silicon wafer and a lower clad layer was produced in the same manner as in step (1-1) of Example 1, except that a resin sheet having a 10 μm-thick resin composition layer produced in Production Example 12 was used as the resin sheet for forming the lower clad layer.

[0389] (11-2. Formation of the core layer) Except for using a resin sheet having a 5 μm-thick resin composition layer produced in Production Example 11 as the resin sheet for forming the core layer, a core layer was formed on the surface of the lower clad layer of the intermediate laminate II obtained in the above-mentioned step (11-1) by the same method as step (1-2) of Example 1, thereby obtaining an intermediate laminate IV having a silicon wafer, a lower clad layer, and a core layer in this order.

[0390] (11-3. Formation of upper cladding layer) An upper clad layer was formed on the core layer of the intermediate laminate IV obtained in the above-mentioned step (11-2) by the same method as in step (1-3) of Example 1, except that a resin sheet having a 20 μm-thick resin composition layer produced in Production Example 12 was used as the resin sheet for forming the upper clad layer, thereby obtaining a sample laminate having a silicon wafer, a lower clad layer, a core layer, and an upper clad layer in this order.

[0391] [Example 12] (12-1. Formation of the lower cladding layer) An intermediate laminate II including a silicon wafer and a lower clad layer was produced in the same manner as in step (1-1) of Example 1.

[0392] (12-2. Formation of the core layer) A polyethylene terephthalate film having a rough surface (Unitika's "PTH-25", thickness 25 μm) was prepared as a support. The resin varnish produced in Production Example 1 was uniformly applied to the rough surface of the support with a die coater so that the thickness of the resin composition layer after drying was 10 μm, and dried at 80 ° C to 110 ° C (maximum temperature 110 ° C) for 7 minutes to form a resin composition layer. Next, a cover film (biaxially oriented polypropylene film, Oji F-Tex's "MA-411") was placed on the surface of the resin composition layer and laminated at 80 ° C to produce a resin sheet having a three-layer structure of support / resin composition layer / cover film. The surface of the resin composition layer on the support side of the resin sheet produced in this way had a large roughness due to being pressed against the rough surface of the support. Therefore, the above-mentioned resin sheet may be referred to as a "roughened resin sheet" below.

[0393] The roughened resin sheet was used as the resin sheet for forming the core layer. The quartz glass mask was changed to a quartz glass mask having a mask pattern capable of drawing a plurality of straight lines with a length of 1 cm at L / S (line / space) 10 μm / 100 μm, a mask pattern capable of drawing a plurality of straight lines with a length of 2 cm at L / S (line / space) 10 μm / 100 μm, and a mask pattern capable of drawing a plurality of straight lines with a length of 3 cm at L / S (line / space) 10 μm / 100 μm. A core layer was formed on the surface of the lower clad layer of the intermediate laminate II obtained in the above-mentioned step (12-1) by the same method as in step (1-2) of Example 1 except for the above matters, to obtain an intermediate laminate IV having a silicon wafer, a lower clad layer, and a core layer in this order.

[0394] (12-3. Formation of upper cladding layer) Using the same method as in step (1-3) of Example 1, an upper clad layer was formed on the core layer of the intermediate laminate IV obtained in the above step (12-2), to obtain a sample laminate having a silicon wafer, a lower clad layer, a core layer, and an upper clad layer in this order.

[0395] [Example 13] When the resin composition layer was cured in a clean oven in each of the steps of forming the lower clad layer, forming the core layer, and forming the upper clad layer, the conditions of the heat treatment were changed as follows. That is, the temperature was raised from room temperature to 100°C, and after reaching 100°C, a heat treatment was performed for 60 minutes, and then the temperature was raised to 190°C, and after reaching 190°C, a heat treatment was performed for 90 minutes in a nitrogen atmosphere to cure the resin composition layer. The same operation as in Example 12 was performed except for the above items to obtain a sample laminate having a silicon wafer, a lower clad layer, a core layer, and an upper clad layer in this order. In this Example 13, the curing conditions of the resin composition by the heat treatment were changed, so that the shape of the rough surface of the support was more greatly reflected on the surface of the core layer. Therefore, the surface roughness of the core layer was larger than that of Example 12.

[0396] [Comparative Example 1] (C1-1. Formation of the lower cladding layer) An intermediate laminate II comprising a silicon wafer and a lower clad layer was produced in the same manner as in step (1-1) of Example 1, except that a resin sheet having a 10 μm-thick resin composition layer produced in Production Example 3 was used as the resin sheet for forming the lower clad layer.

[0397] (C1-2. Formation of the core layer) Using the same method as in step (1-2) of Example 1, a core layer was formed on the lower clad layer of the intermediate laminate II obtained in the above step (C2-1) to obtain an intermediate laminate IV having a silicon wafer, a lower clad layer, and a core layer in that order.

[0398] (C1-3. Formation of upper cladding layer) Except for using a resin sheet having a 20 μm-thick resin composition layer produced in Production Example 3 as the resin sheet for forming the upper clad layer, an upper clad layer was formed on the core layer of the intermediate laminate IV obtained in the above step (C1-2) in the same manner as in step (1-3) of Example 1, to produce a sample laminate having a silicon wafer, a lower clad layer, a core layer, and an upper clad layer in this order.

[0399] [Comparative Example 2] (C2-1. Formation of the lower cladding layer) An intermediate laminate II comprising a silicon wafer and a lower clad layer was produced in the same manner as in step (1-1) of Example 1, except that a resin sheet having a 10 μm-thick resin composition layer produced in Production Example 7 was used as the resin sheet for forming the lower clad layer.

[0400] (C2-2. Formation of the core layer) Except for using a resin sheet having a 5 μm-thick resin composition layer produced in Production Example 8 as the resin sheet for forming the core layer, a core layer was formed on the lower clad layer of the intermediate laminate II obtained in the above-mentioned step (C2-1) by the same method as in step (1-2) of Example 1, to obtain an intermediate laminate IV having a silicon wafer, a lower clad layer, and a core layer in this order.

[0401] (C2-3. Formation of upper cladding layer) Except for using a resin sheet having a 20 μm-thick resin composition layer produced in Production Example 7 as the resin sheet for forming the upper clad layer, an upper clad layer was formed on the core layer of the intermediate laminate IV obtained in the above step (C2-2) in the same manner as in step (1-3) of Example 1, to produce a sample laminate having a silicon wafer, a lower clad layer, a core layer, and an upper clad layer in this order.

[0402] [Comparative Example 3] As the resin sheet for forming the lower cladding layer, a resin sheet having a resin composition layer with a thickness of 10 μm produced in Production Example 13 was used. As the resin sheet for forming the upper cladding layer, a resin sheet having a resin composition layer with a thickness of 20 μm produced in Production Example 13 was used. Aside from the above, a sample laminate having a silicon wafer, a lower cladding layer, a core layer, and an upper cladding layer in this order was produced in the same manner as in Example 1.

[0403] [Measurement of surface roughness of core layer] In the above-mentioned examples and comparative examples, after the core layer was formed and before the upper clad layer was formed, the arithmetic mean roughness Ra was measured as the surface roughness of the core layer. The measurement was performed using a surface roughness meter (WYKO NT3300 manufactured by B-CO Instruments) in VSI mode with a 50x lens to obtain the Ra value from the numerical value obtained with a measurement range of 121 μm×92 μm. For each sample, the measurement was performed by calculating the average value of 10 randomly selected points.

[0404] [Evaluation of optical waveguides] (Measurement of optical transmission loss of a calibration optical system) The transmission loss of an optical system was measured, which was configured by removing the test substrate and the light collecting module from the optical system for measuring the transmission loss of the test substrate described later. That is, a light source (1310 nm light source, THORLABS "LPSC-1310-FC") and a light receiver (Keysight optical power meter "N7742") were connected via an optical fiber (input fiber) on a vibration isolation table covered with a blackout curtain to obtain an optical system for calibration. The light source was made to emit light, and the intensity of the light that entered the light receiver was measured by the light receiver, to measure the loss of this optical system for calibration.

[0405] (Preparation of test board) From the sample laminates produced in the examples and comparative examples, the core layer and the cladding layer surrounding it were cut out at the portion where the core layer was formed, to obtain a test substrate equipped with an optical transmission path.

[0406] (Optical transmission loss measurement) A test substrate was placed on a vibration isolation table covered with a blackout curtain. A light collecting module (numerical aperture 0.18) was connected to one end (input end) of the optical waveguide of the test substrate, and a light source (1310 nm light source, THORLABS's "LPSC-1310-FC") was connected to the light collecting module via an optical fiber (input fiber). Another light collecting module (numerical aperture 0.18) was connected to the other end (output end) of the optical waveguide of the test substrate, and a light receiver (Keysight's optical power meter "N7742") was connected to the light collecting module via an optical fiber (output fiber). Through the above operations, an optical system was obtained in which light emitted from the light source passes through the optical fiber (input fiber), the light collecting module, the optical waveguide, the light collecting module, and the optical fiber (output fiber) in this order, and then enters the light receiver. Hereinafter, this optical system may be referred to as a sample optical system. The light source was turned on and the intensity of the light that entered the receiver was measured by the receiver to measure the loss of the sample optical system. The loss of the optical waveguide included in the test substrate was determined by subtracting the loss of the calibration optical system from the loss of the sample optical system.

[0407] (Measurement of transmission loss (dB / cm) of optical waveguide) The loss of the optical waveguide was measured for each of the optical waveguides with lengths of 1 cm, 2 cm, and 3 cm. The measurement results were plotted on a coordinate system with the length of the optical waveguide on the horizontal axis and the loss of the optical waveguide on the vertical axis to obtain three coordinates representing the measurement results. An approximation line of these three points was calculated using the least squares method, and the slope of the approximation line was calculated as the loss per unit distance of the optical waveguide (transmission loss).

[0408] (Check the mode) The receiver was removed and replaced with an infrared camera (InGaAs camera with 100x objective lens). The light source was turned on and the light emitted from the end of the optical fiber (output fiber) was photographed with the infrared camera. When only one circular light edge was observed, it was determined to be single mode. When multiple edges were observed, it was determined to be multimode.

[0409] (Observation of appearance after reflow) The test board was subjected to five heat treatments using a reflow device (Antom Corporation's "HAS6116") (the reflow temperature profile was in accordance with IPC / JEDEC J-STD-020C). The test board was observed after the treatment, and if there were no voids or peeling in the board, the reflow resistance was judged to be "excellent." If there were voids or peeling in the board, the reflow resistance was judged to be "poor."

[0410] [result] The results of the above-mentioned Examples and Comparative Examples are shown in the following Tables 3 and 4. In the following Tables 3 and 4, the meanings of the abbreviations are as follows. NA: Numerical aperture of the optical waveguide ΔCTE: the difference between the linear thermal expansion coefficient of the cured product of the core resin composition and the linear thermal expansion coefficient of the cured product of the cladding resin composition. "S" in the mode column: Single mode. "M" in the mode column: Multi mode.

[0411] [Table 3]

[0412] [Table 4]

[0413] [Consider] A single mode was confirmed in Examples 1 and 3 to 7, which had a small core layer and a small numerical aperture NA. In addition to the above examples and comparative examples, an optical waveguide with a numerical aperture NA of less than 0.05 was manufactured, but the refractive index in the optical waveguide changed due to process fluctuations, and light guiding could not be confirmed.

[0414] In Comparative Examples 1 and 2 in which the numerical aperture NA was 0.4 or more, the transmission loss became significant and there was a lot of noise, making it impossible to measure the value of the transmission loss. [Explanation of symbols]

[0415] 10 Optical waveguide 100 Core Layer 110 Second composition layer 111 Exposure section 112 Non-exposed area 200 Cladding Layers 210 First composition layer 220 Cured first composition layer (lower clad layer) 230 Third composition layer 240 Cured third composition layer (upper clad layer) 300 Base material 400 Mask 410 Translucent part 420 Shading part

Claims

1. A photosensitive resin composition set including a core resin composition and a clad resin composition; the core resin composition comprises (A) a phenolic resin having two or more phenolic hydroxyl groups per molecule, (B) a photoacid generator, and (C) a crosslinking agent; The cladding resin composition comprises (a) a phenolic resin having two or more phenolic hydroxyl groups per molecule, (b) a photoacid generator, and (c) a crosslinking agent; A photosensitive resin composition set having a numerical aperture NA represented by the following formula (1) greater than 0.05 and less than 0.4: [0010] (In formula (1), n core represents the refractive index of the cured product of the core resin composition, n clad represents the refractive index of the cured product of the cladding resin composition.

2. The photosensitive resin composition set described in claim 1, wherein the (C) crosslinking agent is an amino resin.

3. The photosensitive resin composition set described in claim 1, wherein the core resin composition contains (D) a polymer having a weight average molecular weight of 2,500 or more.

4. The photosensitive resin composition set described in claim 1, wherein the core resin composition contains (E) a compound represented by the following formula (E-1): 【Chemistry 1】 (In formula (E-1), R e1 , R e2 and R e3 R each independently represents a hydrogen atom or a hydrocarbon group. e1 and R e2 may be bonded to form a ring.)

5. The photosensitive resin composition set according to claim 1, which is a photosensitive resin composition set for producing an optical waveguide.

6. The photosensitive resin composition set according to claim 1, which is a photosensitive resin composition set for producing an optical waveguide capable of transmitting light having a wavelength of 1300 nm to 1320 nm.

7. The photosensitive resin composition set according to claim 1, which is a photosensitive resin composition set for producing a single-mode optical waveguide.

8. An optical waveguide having a core layer and a cladding layer; the core layer comprises a cured product of a core resin composition comprising (A) a phenolic resin having two or more phenolic hydroxyl groups per molecule, (B) a photoacid generator, and (C) a crosslinking agent; the cladding layer comprises a cured product of a cladding resin composition comprising (a) a phenolic resin having two or more phenolic hydroxyl groups per molecule, (b) a photoacid generator, and (c) a crosslinking agent; An optical waveguide having a numerical aperture NA represented by the following formula (1) that is greater than 0.05 and less than 0.

4. [0025] (In formula (1), n core represents the refractive index of the cured product of the core resin composition, n clad represents the refractive index of the cured product of the cladding resin composition.

9. 9. The optical waveguide according to claim 8, capable of transmitting light having a wavelength of 1300 nm to 1320 nm.

10. 9. The optical waveguide of claim 8 which is a single mode optical waveguide.

11. An optical / electrical hybrid board comprising the optical waveguide according to any one of claims 8 to 10.

12. forming a first composition layer containing a cladding resin composition; a step of subjecting the first composition layer to an exposure treatment; curing the first composition layer; forming a second composition layer containing a core resin composition on the first composition layer; a step of subjecting the second composition layer to an exposure treatment; subjecting the second composition layer to a development treatment; curing the second composition layer; forming a third composition layer containing the cladding resin composition on the second composition layer; a step of subjecting the third composition layer to an exposure treatment; and curing the third composition layer in this order; the core resin composition comprises (A) a phenolic resin having two or more phenolic hydroxyl groups per molecule, (B) a photoacid generator, and (C) a crosslinking agent; The cladding resin composition comprises (a) a phenolic resin having two or more phenolic hydroxyl groups per molecule, (b) a photoacid generator, and (c) a crosslinking agent; A method for manufacturing an optical waveguide, wherein a numerical aperture NA represented by the following formula (1) is greater than 0.05 and less than 0.

4. [0030] (In formula (1), n core represents the refractive index of the cured product of the core resin composition, n clad represents the refractive index of the cured product of the cladding resin composition.

13. A sheet set including a core resin sheet and a clad resin sheet; the core resin sheet is provided with a core resin composition layer including a core resin composition including (A) a phenol resin having two or more phenolic hydroxyl groups per molecule, (B) a photoacid generator, and (C) a crosslinking agent; the cladding resin sheet is provided with a cladding resin composition layer including a cladding resin composition including (a) a phenolic resin having two or more phenolic hydroxyl groups per molecule, (b) a photoacid generator, and (c) a crosslinking agent; A sheet set having a numerical aperture NA represented by the following formula (1) greater than 0.05 and less than 0.

4. [0045] (In formula (1), n core represents the refractive index of the cured product of the core resin composition, n clad represents the refractive index of the cured product of the cladding resin composition.

14. A core resin composition for forming a core layer in a cladding layer, comprising a cured product of a cladding resin composition comprising (a) a phenolic resin having two or more phenolic hydroxyl groups per molecule, (b) a photoacid generator, and (c) a crosslinking agent; the core resin composition comprises (A) a phenolic resin having two or more phenolic hydroxyl groups per molecule, (B) a photoacid generator, and (C) a crosslinking agent; A core resin composition having a numerical aperture NA represented by the following formula (1) greater than 0.05 and less than 0.4: [0050] (In formula (1), n core represents the refractive index of the cured product of the core resin composition, n clad represents the refractive index of the cured product of the cladding resin composition.

15. A resin sheet comprising a resin composition layer containing the core resin composition according to claim 14.

16. A resin composition for cladding for forming a cladding layer covering a core layer, the cladding layer comprising a cured product of a resin composition for core comprising (A) a phenolic resin having two or more phenolic hydroxyl groups per molecule, (B) a photoacid generator, and (C) a crosslinking agent; The cladding resin composition comprises (a) a phenolic resin having two or more phenolic hydroxyl groups per molecule, (b) a photoacid generator, and (c) a crosslinking agent; A resin composition for cladding, having a numerical aperture NA represented by the following formula (1) of greater than 0.05 and less than 0.4: [006] (In formula (1), n core represents the refractive index of the cured product of the core resin composition, n clad represents the refractive index of the cured product of the cladding resin composition.

17. A resin sheet comprising a resin composition layer containing the cladding resin composition according to claim 16.

Citation Information

Patent Citations

  • Window frame and apparatus for fixing it

    JP1982071978A

  • Photosensitive resin composition for forming optical waveguide, optical waveguide, and method for forming optical waveguide pattern

    JP2007052120A

  • Photosensitive insulating resin composition, cured product thereof, and electronic component having same

    JP2008077057A

  • Negative photosensitive resin composition for silica glass optical waveguide formation

    JP2009198767A

  • Photosensitive resin composition for forming polymer optical waveguide, optical waveguide, and method for forming optical waveguide pattern