Ceramic particles, ceramic particle aggregate, and method for producing ceramic particles
Ceramic particles with single crystal structure and nitrogen-filled closed pores address the challenges of mechanical strength and thermal stability in conventional porous bodies, enabling stable performance under high temperatures.
Patent Information
- Application Number
- JP2020114248
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-01
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-07-01
AI Technical Summary
Conventional porous ceramic bodies with open pores face challenges in uniform electrode application and mechanical strength, especially when exposed to high-temperature environments, leading to structural changes and reduced mechanical stability.
Ceramic particles with a single crystal structure containing closed pores within them, formed by heat-treating metal oxide particles in an atmosphere containing ammonia and oxygen, which results in nitrogen-filled closed pores, enhancing mechanical strength and thermal stability.
The ceramic particles exhibit high mechanical strength, excellent thermal stability, and reduced weight, making them suitable for applications requiring stable structures even in high-temperature environments.
Smart Images

Figure 0007586420000002 
Figure 0007586420000003 
Figure 0007586420000004
Abstract
Description
[Technical field]
[0001] The present invention relates to ceramic particles, a ceramic particle aggregate, and a method for producing ceramic particles. [Background technology]
[0002] Ceramics have a wide range of applications, including electrical components, daily necessities, and catalysts. To realize and improve the functionality of ceramics in these applications, it is very important to control their microstructure. One example of the microstructure of ceramics is a porous body.
[0003] Conventionally known ceramic porous bodies are divided into type 1, in which pores are formed on the surface of a substrate, and type 2, in which pores are formed as voids within aggregates by aggregating fine particles. FIG. 1, which is a schematic diagram of type 1, is an example. FIG. 1 is obtained by subjecting a bulk body containing two or more phases with different chemical properties to etching to dissolve a specific phase or subjecting it to electrochemical corrosion. Alternatively, it is obtained by a method of forming holes at predetermined positions by applying a resist to a single-phase bulk body and then etching it. For example, Non-Patent Document 1 discloses a technology for forming a porous structure in a substrate by an electrochemical method.
[0004] Another form of type 1 is shown in Fig. 2, which is a schematic diagram. The form in Fig. 2 is a structure obtained by growing needle-like crystals or the like on the surface of a substrate. For example, Fig. 3(a) of Patent Document 1 discloses a structure in which needle-like crystals of zinc oxide are precipitated and grown on a substrate. This type of structure has only open pores. This type of structure is suitable for applications requiring a high surface area, such as catalysts and adsorbents.
[0005] FIG. 3 is a schematic diagram showing the form of Type 2. As shown in FIG. 3, Type 2 has a porous structure as an aggregate of particles. This porous structure can be obtained without densification by sintering at a relatively low temperature where material transport in a solid is suppressed by adding a sintering aid or the like. For example, Patent Document 2 discloses a technique for forming a ceramic porous body. In Patent Document 2, a porous body is formed by mixing a resin and an oxide powder, forming the mixture, and then firing the mixture to burn off the resin. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2012-144384 A [Patent Document 2] JP 2006-342054 A [Non-patent literature]
[0007] [Non-Patent Document 1] Hiroyo Segawa, Shoji Kure, Satoru Inoue, Control and Functionalization of Nanostructures by Anodic Oxidation. MATERIALS INTEGRATION, 25
[10] (2012)32-37 Summary of the Invention [Problem to be solved by the invention]
[0008] The main use and purpose of porous bodies is to reduce the weight of components. One example of reducing the weight of components is the weight of electronic ceramics, which are components used in electronic components. On the other hand, electrodes need to be connected to electronic ceramics. However, the porous bodies of the above-mentioned type 1 or type 2 have open pores and therefore do not have a flat surface, making it difficult to attach electrodes uniformly to the surface of the electronic ceramics. In other words, the porous bodies of the above-mentioned type 1 or type 2 are not suitable for electronic components such as elements that require electrodes to be connected.
[0009] In addition, the aforementioned porous body of type 2, particularly the particle aggregate, is manufactured by performing firing under relatively mild conditions to suppress densification of the aggregate. As a result, the resulting aggregate has weaker grain boundary bonds and lower mechanical strength than a dense body obtained by high-temperature firing. In the aforementioned Patent Document 2, firing is also performed at a low temperature, and it is difficult to say that strong bonds are formed between alumina particles in the obtained ceramic porous body. Therefore, further consideration is required to obtain a ceramic porous body that requires a certain level of strength. Incidentally, pumice is known as a porous body. However, its material is generally weak against mechanical deformation, and the constituent particles easily come off, so it cannot be used as a ceramic porous body that requires a certain level of strength.
[0010] Furthermore, when the porous bodies of the above-mentioned types 1 and 2 are exposed to high-temperature environments, the particles tend to aggregate, i.e., densification is promoted, and the properties of the porous body tend to be lost. For this reason, the properties required are excellent thermal stability, i.e., the structure is hardly changed even in high-temperature environments.
[0011] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide ceramic particles that have high mechanical strength, excellent thermal stability, and can realize lightweight components, a ceramic particle aggregate containing the ceramic particles, and a method for manufacturing the ceramic particles. [Means for solving the problem]
[0012] According to one aspect of the present invention, there is provided ceramic particles which are formed of a metal oxide containing titanium, are single crystals, and contain closed pores within the single crystal.
[0013] According to another aspect of the present invention, there is provided a ceramic particle aggregate comprising a plurality of ceramic particles according to the present invention.
[0014] According to another aspect of the present invention, there is provided a method for producing ceramic particles or ceramic particles contained in a ceramic particle aggregate according to the present invention, comprising the steps of: The method includes a step of heat-treating ceramic raw material particles formed of a metal oxide containing titanium at 900° C. or higher in an atmosphere containing ammonia and oxygen, The method for producing ceramic particles is provided in which the amount of ammonia supplied is set to an amount that corresponds to the amount of unreacted ammonia contained in the exhaust gas after the heat treatment. Effect of the Invention
[0015] According to the present invention, it is possible to provide ceramic particles that have high mechanical strength and excellent thermal stability, and that can realize lightweight components, a ceramic particle aggregate containing the ceramic particles, and a method for producing the ceramic particles. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a schematic diagram showing the structure of Type 1, which is a conventional porous body structure. [Diagram 2] FIG. 2 is a schematic diagram showing the structure of Type 2, which is another conventional porous body structure. [Diagram 3] FIG. 3 is a schematic diagram showing another structure of Type 2, which is another conventional porous body structure. [Figure 4] FIG. 4 is a schematic diagram illustrating the structure of the ceramic particle of the present invention. [Diagram 5] FIG. 5 is a diagram showing an example of a transmission electron microscope photograph of calcium titanate particles according to one embodiment of the present invention. [Figure 6] FIG. 6 is a diagram showing an example of an optical microscope view of a fracture surface of a titanium oxide single crystal according to one embodiment of the present invention. [Figure 7A] FIG. 7A is a diagram showing analysis positions of electron energy loss spectroscopy of closed pores of a calcium titanate particle according to one embodiment of the present invention. [Figure 7B] FIG. 7B is a diagram showing the results of EELS analysis at the analysis position of FIG. 7A. [Figure 8A]FIG. 8A is a diagram showing analysis positions in electron energy loss spectroscopy of a portion other than closed pores of a calcium titanate particle according to one embodiment of the present invention. [Figure 8B] FIG. 8B is a diagram showing the results of EELS analysis at the analysis position of FIG. 8A. [Figure 9] FIG. 9 is a diagram showing the positions of EELS analysis of barium titanate particles according to one embodiment of the present invention. [Figure 10] FIG. 10 is a diagram showing the results of EELS analysis at the analysis positions in FIG. [Figure 11] FIG. 11 is a diagram showing an intensity mapping image of a Raman spectrum originating from nitrogen molecules for a titanium oxide single crystal according to one embodiment of the present invention. [Figure 12] FIG. 12 is an average particle size distribution diagram of barium titanate particles according to one embodiment of the present invention. [Figure 13] FIG. 13 is a schematic diagram illustrating the structure of a ceramic particle aggregate of the present invention. [Figure 14] FIG. 14 is a diagram showing the thermal history and the results of desorbed gas component analysis of an aggregate of barium titanate particles according to one embodiment of the present invention. [Figure 15] FIG. 15 is a diagram showing the thermal history of ceramic particles and the results of an analysis of desorbed gas components in an example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] As a result of intensive research, the inventors have found that ceramic particles formed of a metal oxide containing titanium, having a single crystal crystal structure and containing closed pores in the single crystal have high mechanical strength and excellent thermal stability, and can realize weight reduction of components. The ceramic particles, a ceramic particle aggregate containing the ceramic particles, and a method for producing the ceramic particles will be described in this order below. In the following, an embodiment of the present invention will be described in detail with reference to the drawings as appropriate. The drawings used in the following description may show characteristic parts in an enlarged manner for the sake of convenience in order to make the features of the present invention easier to understand, and the dimensional ratios of each component may differ from the actual ones. The materials, dimensions, etc. exemplified in the following description are merely examples, and the present invention is not limited to them, and can be appropriately modified and implemented within the scope of the present invention.
[0018] [Ceramic particles (primary particles)] (Crystal structure of ceramic particles) The ceramic particles of the present invention are single crystals and contain closed pores within the single crystal. In the ceramic particles of the present invention, the inner surfaces of the closed pores preferably have a plane orientation. In general, when a particle having a cavity is exposed to high temperatures, it acts in a direction to reduce the energy of the inner surface of the cavity, for example, reconstruction of the inner surface may occur. However, if the surface energy of the inner surface is small and the shape is stable, large-scale reconstruction of the inner surface can be suppressed when loaded at high temperatures. In the present invention, it is considered that the inner surface of the closed pore has a plane orientation reflecting the crystal habit as a preferred embodiment, so that the inner surface of the closed pore is more thermally stable. In contrast, in the above-mentioned type 2, closed pores may be formed by being surrounded by multiple crystal particles, but there may be places where the crystal particles are not bonded to each other. Therefore, it is considered that the closed pores formed in type 2 are unstable and have low mechanical strength and thermal stability.
[0019] FIG. 4 is a schematic diagram illustrating the structure of the ceramic particle of the present invention. The ceramic particle of the present invention, unlike the above-mentioned Type 1 and Type 2, contains closed pores inside the single crystal particle. In this specification, "closed pores" refer to cavities that exist inside the ceramic particle and do not communicate with the ceramic particle surface. In contrast, cavities that communicate with the ceramic particle surface, such as those of Type 1, are called "open pores."
[0020] In this specification, the term "single crystal" refers to (i) a single crystal in which the periodic arrangement of atoms in a particle is determined only by three crystallographic unit translation vectors, or (ii) a single crystal containing a ferroelastic domain structure, a ferroelectric domain structure, or a twin structure bonded with a crystallographic mirror image relationship. The above (ii) is a crystal in which each twin domain is recognized as a single crystal in an electron beam diffraction analysis performed under the conditions of selected area diffraction using a general transmission electron microscope. In addition, the term "grain boundary" in this specification does not include ferroelectric or ferroelastic domain walls or twin planes where single crystals having a mirror image relationship are joined, but refers to a small-angle grain boundary formed by sintering or a grain boundary accompanied by a disordered grain orientation where a mirror image relationship does not exist at the interface.
[0021] The ceramic particles according to the present invention are single crystals. This distinguishes them from polycrystalline bodies having closed pores obtained by bonding multiple particles as shown in FIG. 3 and inferior mechanical strength. The closed pores of the polycrystalline body shown in FIG. 3 are accompanied by grain boundaries. Therefore, the presence of closed pores as shown in FIG. 3 leads to a situation in which the mechanical strength is reduced, and the gas in the closed pores escapes to the outside by diffusion through multiple grain boundaries with disordered atomic arrangement. On the other hand, the closed pores shown in FIG. 4 do not include the multiple grain boundaries and have a structure that is completely blocked from the outside. Therefore, the mechanical strength is excellent. In addition, since the particles shown in FIG. 4 are single crystal particles, the inner surfaces of the closed pores are formed by stable crystal habit planes. In other words, since the inner surfaces of the closed pores are chemically stable surfaces, they have the advantage of being less likely to break even when heated.
[0022] The shape of the closed pores is not particularly limited. The closed pores may be in the form of a sphere, an elliptical sphere, a polyhedron, a pyramid, a cube, a rectangular parallelepiped, or the like, a cylinder, a cone, a pyramid, a sphere, a hemisphere, an ellipsoid, or a semi-ellipsoid. The shape may be selected from the group consisting of irregularly shaped contours and any combination thereof. The inner surface forming the closed pores may have irregularities.
[0023] As described above, it is preferable that the closed pores have a plane orientation on a part of their inner surface. Examples of the shape of the closed pores having such a plane orientation include hexahedrons including rectangular parallelepipeds and cubes.
[0024] Fig. 5 is a diagram showing an example of a transmission electron microscope photograph of calcium titanate particles according to one embodiment of the present invention. Electron beam diffraction measurement and high-resolution electron microscope observation have confirmed that calcium titanate particles 7 are single crystals. In Fig. 5, multiple nearly rectangular contrasts are observed. These nearly rectangular contrasts are closed pores 8 formed in calcium titanate particles 7. The presence of these closed pores 8 can reduce the weight of components and improve optical properties.
[0025] In Fig. 5, 9 indicates the crystal axis of a single crystal calcium titanate particle. In Fig. 5, for example, each closed pore 8 has a rectangular shape formed by the axial direction 9 and another axial direction perpendicular to it. It can be seen that the plane orientation of the inner surface of the closed pore is (001) or (010). In other words, Fig. 5 shows that the inner surfaces of the closed pores present in the ceramic particles have a plane orientation.
[0026] The plane orientation may be a plane in which any one or two of h, k, and l in (hkl) are zero, a (111) plane, or a (112) plane. In FIG. 5, the arrow 9 is the a-axis, the axis perpendicular to the arrow 9 is the b-axis, and the axis perpendicular to the a-axis, b-axis, and the paper surface is the c-axis. The a-axis, b-axis, and c-axis can be determined by electron beam diffraction. In FIG. 5, most of the closed pores observed have various ratios of the lengths of the a-axis and b-axis, but the inner surfaces of all of them are in the a-axis and b-axis directions. Alternatively, in the ceramic particles shown in FIG. 11 described later, the x-axis is the a-axis 17, the z-axis is the b-axis 18, and the y-axis is the c-axis 19. In the present invention, "having a plane orientation" also includes a range inclined up to ±30° with respect to each plane.
[0027] (Ceramic particle size) The size of the ceramic particles (primary particles) is not particularly limited. One embodiment of the ceramic particles includes fine particles having an average particle diameter of, for example, 1 μm or less, and even 500 nanometers or less. Another embodiment of the ceramic particles includes coarse particles having an average particle diameter of, for example, millimeter order or centimeter order.
[0028] The size of the ceramic particles can be measured, for example, by a method of determining the average particle size of ceramic particles (primary particles) contained in powder or aggregates from an image of a scanning electron microscope, or by a powder evaluation device such as laser scattering. FIG. 12 is a diagram illustrating the measurement results of the particle size of ceramic particles (primary particles) constituting a powder-like ceramic particle aggregate. In detail, FIG. 12 shows that a straight line is drawn on an image observed by SEM, the points where the line intersects with the particle surface are picked out, and the average value between the points is calculated to determine the average particle size. From FIG. 12, the particle size of all randomly extracted particles is 500 nanometers or less, the peak indicating the average particle size is about 200 to 300 nanometers, and the average particle size is 294 nanometers. Even if the ceramic particles are not spherical or polygonal, but have a dendrite or snowflake-like shape, the average particle size can be measured by the above method. The same results can be obtained even when the measurement is performed using an apparatus that measures particle size distribution using a laser scattering method.
[0029] As an embodiment of the ceramic particles, there may be mentioned ceramic particles having an average particle size of 1 μm or less, or even an average particle size of 500 nanometers or less, and having closed pores with an average dimension of 100 nanometers or less on the longest side. Alternatively, when the ceramic particles are bulky coarse particles with an average particle size of the order of millimeters or centimeters, there may be ceramic particles having closed pores with a maximum dimension of 100 micrometers or more on the longest side. Alternatively, there may be cases where the coarse particles have only fine closed pores with an average dimension of 100 nanometers or less on the longest side, or where both the coarse closed pores and the fine closed pores are present.
[0030] Also, in Figure 5, the largest closed pore 8 has a longest side of 100 nanometers or less. That is, Figure 5 shows one embodiment of a ceramic particle of the present invention in which the average dimension of the closed pores is a longest side of 100 nanometers or less.
[0031] Fig. 6 is a diagram showing an example of an optical microscope photograph of a fracture surface of a titanium oxide single crystal according to one embodiment of the present invention. Unlike Fig. 5, Fig. 6 shows relatively coarse closed pores. Fig. 6 is an optical microscope photograph of a fracture surface of a rutile-type titanium oxide single crystal plate having a thickness of 500 micrometers and a (010) surface. This single crystal plate has closed pores, and here <010> Axis and <001> The optical microscope photograph shows the fracture surface of a specimen broken by the axis. <001> the axis, and the left-right direction is the thickness direction of the single crystal plate; <100> At a depth of about 50 to 100 micrometers from the (010) surface of the single crystal, <001> There are closed pores 15 with a length in the direction of about 300 micrometers. That is, Figure 6 shows an embodiment of a ceramic particle of the present invention in which the average dimension of the closed pores is 100 micrometers or more on the longest side.
[0032] Comparing Figures 5 and 6, it can be seen that as the size of the closed pores increases, the directionality of the inner surfaces of the closed pores decreases. However, Figure 6 shows a tendency for the closed pores to have inner surfaces that are parallel to the ceramic particle surfaces.
[0033] In addition, there is a difference in the shape of the closed pores between Figures 5 and 6. Figure 5 shows the presence of closed pores that are close to squares, while Figure 6 shows rectangular closed pores with a large axial ratio. This corresponds to the difference in the crystal structure between the two. The calcium titanate in Figure 5 has a perovskite crystal structure, while the titanium oxide in Figure 6 has a rutile structure. The perovskite structure is a crystal structure close to a cube with no singular axis, while the rutile structure is a crystal structure with the c-axis as the singular axis. The symmetry of the crystal is reflected in the shape of the pores, so in Figure 6, the closed pores are long in the direction of the c-axis, which is the singular axis. In particular, when the main cause of the formation of closed pores is the manifestation of the diffusion of elements in a solid, the shape of the closed pores is likely to be influenced by the anisotropy of the diffusion coefficient in the crystal.
[0034] The reasons why closed pores of a particular shape are formed are thought to be as follows. For example, it is thought that the inner surface of the closed pore becomes a stable surface, and as a result, the closed pores may have the above-mentioned hexahedral shape. Alternatively, as mentioned above, it is thought that the closed pores tend to be elongated in the direction parallel to the axis along which the diffusion of elements in the solid, for example, the diffusion of oxygen, is fast. As mentioned above, in the case of rutile-type titania, long flat pores are formed in the c-axis direction due to the anisotropy of the diffusion rate of oxygen diffusion.
[0035] As described above, the ceramic particles of the present invention contain closed pores within the single crystal, and the main component of the gas in the closed pores is nitrogen gas.
[0036] In general, when closed pores filled with reactive gas are exposed to high temperatures or long-term light irradiation, a chemical reaction occurs between the crystals constituting the inner surface of the closed pores and the reactive gas, which may impair the stability of the closed pores and cause the closed pores to disappear. In contrast, in the ceramic particles of the present invention, the main component of the gas in the closed pores is nitrogen gas. Nitrogen gas is a molecule formed by triple bonds of nitrogen atoms, and is a stable gas that requires a very large amount of heat to dissociate. Therefore, by filling the closed pores with nitrogen gas, a chemical reaction between the inner surface of the closed pores and the gas in the closed pores is unlikely to occur, and the closed pores can be stably maintained. As a result, it is possible to achieve and maintain weight reduction, high thermal stability, and high mechanical strength.
[0037] The presence of nitrogen gas in the closed pores can be confirmed by observing energy loss due to nitrogen molecules in electron energy-loss spectroscopy (EELS).
[0038] FIG. 7 shows an example of the results of electron energy loss spectroscopy analysis of calcium titanate particles according to one embodiment of the present invention. FIG. 7A shows an analysis position in a calcium titanate particle, and FIG. 7B shows the results of EELS analysis of the analysis position. In FIG. 7B, in addition to the signals of titanium, oxygen, and calcium, which are the original constituent elements of calcium titanate particles, a high nitrogen signal (spectrum) was confirmed. The observed nitrogen spectrum had a spectral shape specific to nitrogen molecules, different from that of nitrogen ions contained in nitrides and oxynitrides. This spectrum is the electron energy loss spectroscopy spectrum of the electron beam that penetrated the closed pores. In the present invention, as described later, the peak with the highest peak is called the "main component" except for the peak derived from the metal oxide containing titanium in the solid part of the ceramic particle. From FIG. 7, it can be seen that the main component of the closed pores is nitrogen gas, since the peak of the nitrogen molecule is the highest. According to EELS, it is possible to determine whether nitrogen is in an atomic state or a molecular state from the energy position, and it was possible to confirm from FIG. 7 that nitrogen is in a stable nitrogen molecular state.
[0039] Figure 8 shows an example of the EELS analysis results of a portion that is not a closed pore, i.e., a calcium titanate portion, measured for comparison with Figure 7 above. Figure 8A shows the analysis position in a calcium titanate particle, and Figure 8B shows the EELS analysis results. In Figure 8B, signals for titanium, oxygen, and calcium, which are the original constituent elements of calcium titanate particles, were confirmed, and the nitrogen signal was much smaller than that in Figure 7 above.
[0040] FIG. 9 shows the analysis positions in barium titanate particles produced under the same conditions as the calcium titanate particles. In FIG. 9, reference numeral 1 indicates the inside of closed pores, and reference numeral 2 indicates the non-closed pores, i.e., the barium titanate portion. FIG. 10 shows the results of EELS analysis of these analysis positions. FIG. 10A shows the measurement result of reference numeral 1, and it can be seen that the nitrogen signal due to the nitrogen gas in the closed pores is high. In contrast, FIG. 10B shows the EELS analysis result of reference numeral 2, which is not a closed pore, and it was confirmed that a high nitrogen signal like that in FIG. 10A was not observed. In addition, since the analysis position in this EELS analysis is small, as shown in FIG. 7, FIG. 8, and FIG. 10, the analysis result of the closed pores also contains some signals due to the calcium titanate or barium titanate portions around the closed pores, while the analysis result of the calcium titanate or barium titanate portions also contains some nitrogen signals in the numerous closed pores.
[0041] The EELS analysis can be measured using the following equipment. That is, a system was used that was equipped with a JEM-ARM200G type transmission electron microscope (200 kV, spherical aberration correction mechanism, annular STEM detector, cold cathode field emission electron source, etc.) manufactured by JEOL, a JED-2300 type EDX detector (SDD) manufactured by the same company, and a high-definition TV camera (One View) and an EELS detector (ENFINIUM) manufactured by Gatan Corporation of the United States. Gatan's software "Digital Micrograph" was used to acquire and analyze the TEM / STEM images and EELS data. Alternatively, a similar analysis was possible using a system equipped with a JEOL JEM-2100F transmission electron microscope (200 kV, annular STEM detector, Schottky field emission electron source, etc. as standard equipment) and the same company's JED-2300 EDX detector (SDD), a Gatan Corporation (USA) TV camera (ORIUS), and an EELS detector (ENFINA1000), and using Gatan Corporation's software for acquiring and analyzing TEM / STEM images and EELS data.
[0042] The observation of the spectrum of nitrogen molecules in FIG. 7B means that the position of the contrast (rectangular black portion) shown in FIG. 5 is a closed pore. If the contrast is an open pore, nitrogen gas cannot be sealed in. From this, it was confirmed that the closed pore 8 in FIG. 5 is filled with nitrogen gas.
[0043] Nitrogen gas in the closed pores can also be confirmed by observing the vibration spectrum of nitrogen molecules using Raman spectroscopy. In other words, by obtaining nitrogen gas signals using Raman spectroscopy, it is possible to evaluate the state and characteristics of materials. Raman scattering spectroscopy can perform three-dimensional mapping measurements, and it is also possible to capture the spatial distribution of closed pores.
[0044] FIG. 11 is a diagram showing an intensity mapping image of the Raman spectrum originating from nitrogen molecules of a titanium oxide single crystal according to one embodiment of the present invention, and shows the results of analyzing nitrogen gas in the closed pores in the titanium oxide single crystal used in the observation of FIG. 6. In FIG. 11, the black portion indicated by 15 indicates a portion where the intensity of the Raman spectrum originating from nitrogen gas is high. In other words, FIG. 11 shows that nitrogen gas is filled in the closed pores contained in the titanium oxide single crystal. Furthermore, the scale axis of FIG. 11 shows that the closed pores 15 are pores whose longest side is 100 micrometers or more. In other words, FIG. 11 shows one embodiment of the ceramic particles of the present invention in which the average dimension of the closed pores is 100 micrometers or more on the longest side.
[0045] The detailed conditions for the Raman analysis are as follows: A Renishaw inVia Raman spectrometer equipped with a three-dimensional mapping function of a pseudo-confocal optical system (spatial resolution of 1 μm or less) was used, the excitation light source was a 532 nm DPSS laser, and the optical system had a wavenumber resolution of 0.3 cm -1 Using the automatic mapping stage built into the instrument, the Raman shift corresponding to nitrogen molecules was measured at 2330 cm -1 The scattering peak intensities of the samples were three-dimensionally mapped.
[0046] As shown above, the presence of nitrogen molecules in the closed pores in the ceramic particles of the present invention can be confirmed by at least one of EELS and Raman spectroscopy. The above analysis method can be selected according to the size of the closed pores. In the present invention, in the gas analysis in the closed pores, the peak with the highest peak in the EELS or Raman measurement result, excluding the peak derived from the titanium-containing metal oxide in the solid part of the ceramic particles, is called the "main component". The gas in the closed pores may contain gas other than the main component nitrogen gas. Inevitably, it may contain plastic components (hydrocarbon-based) and components of the filter material that constitutes the reactor.
[0047] As described above, by evaluating the gas composition inside ceramic particles, it is possible to quantitatively describe the material properties. In addition, by obtaining the material property values, it is possible to estimate the properties of devices, etc., that use the material, and to more accurately design the devices, etc.
[0048] In addition to the above-mentioned method of measuring the size of closed pores by observation with a transmission electron microscope, it is also possible to embed the particles in a resin, polish them to expose their cross sections, and then observe the cross sections with a scanning electron microscope.
[0049] In one embodiment of the ceramic particles of the present invention, the average dimension of the closed pores is 100 nanometers or less on the longest side. Porous bodies generally have the property of scattering light. In particular, the presence of pores smaller than the wavelength of light such as visible light makes it possible to control the light scattering characteristics. In addition, by arranging fine closed pores, it is expected that the function of suppressing crack growth at the time of fracture will be achieved while maintaining the same porosity. The ceramic particles of the present invention can exert these functions, for example, when the average dimension of the closed pores is 100 nanometers or less on the longest side.
[0050] Alternatively, in another embodiment of the ceramic particles of the present invention, the average dimension of the closed pores is 100 micrometers or more on the longest side. For example, when trying to reduce the weight of an element, it may be effective to use a single crystal with larger cavities. When fine closed pores are arranged, the number of inner surfaces separating the closed pores inevitably increases, resulting in a limit to weight reduction. Therefore, from the viewpoint of weight reduction, the ceramic particles of the present invention may have large closed pores with an average dimension of 100 micrometers or more on the longest side.
[0051] (Ceramic particle material (composition)) The ceramic particles of the present invention are formed of a titanium-containing metal oxide. This titanium-containing metal oxide essentially contains titanium and oxygen. The titanium-containing metal oxide may further contain one or more elements selected from the group consisting of barium, calcium, strontium, magnesium, and lanthanide elements as metal elements other than titanium. For example, (Ba 1-x Sr x ) TiO3, etc. may also be used.
[0052] From the viewpoint of easily forming the above structure, the titanium-containing metal oxide is preferably one or more selected from the group consisting of barium titanate, calcium titanate, strontium titanate, lanthanum titanate, and titanium oxide, or one further containing a doping element such as manganese that substitutes for titanium. The above-mentioned lanthanum titanate is not a compound in which titanium is trivalent such as LaTiO3, but a compound in which titanium is tetravalent such as La2Ti2O7. More preferably, it is one or more of barium titanate, calcium titanate, and titanium oxide, further preferably barium titanate and calcium titanate, and most preferably barium titanate.
[0053] In addition to the above main components, if necessary to control the material properties, a doping element such as manganese that substitutes for titanium may be included. The "doping element" here refers to an element that substitutes for an element that constitutes the ceramic particles, such as titanium, and has a different atomic valence from the element that constitutes the ceramic particles. Examples of doping elements include trivalent manganese that substitutes for tetravalent titanium, and trivalent lanthanum that substitutes for divalent calcium.
[0054] The titanium-containing metal oxide can exhibit many functions such as paint, content, catalyst, dielectric, thermoelectric material, electrode agent, and optical function. Examples of titanium-containing metal oxides having the above functions include titanium oxides having photocatalytic properties and titanium-containing oxides such as barium titanate having ferroelectricity. By forming the ceramic particle structure of the present invention, in addition to the above properties, it is possible to further reduce the weight and control the thermal properties, and as a result, it is possible to further expand the applications and performance.
[0055] When the ceramic particles of the present invention are heated to 1000°C, the percentage of broken closed pores among all closed pores may be 10% or less. For example, if the wall of the hole is thin, there may be a certain probability that the wall will crack and open pores will be formed in the particle. For example, a hole with a broken wall may have a shape like the hole in the upper left corner of Figure 6.
[0056] [Ceramic particle aggregates] One embodiment of the present invention is a ceramic particle aggregate containing a plurality of the above-mentioned ceramic particles.
[0057] Since the above ceramic particles have closed pores, by bonding multiple ceramic particles together to form a ceramic particle aggregate, it is possible to realize components, materials, and elements that are both strong and lightweight, unlike the above-mentioned type 2.
[0058] As one embodiment of the ceramic particle aggregate, a schematic diagram of the structure of a ceramic particle aggregate of the present invention is shown in Fig. 13. Fig. 13 shows a ceramic particle aggregate (secondary particle) formed by agglomeration of a crystal matrix 6 and a plurality of ceramic particles having closed pores 5 therein, but the embodiment of the present invention is not limited to a ceramic particle aggregate formed only from the ceramic particles in this manner.
[0059] As another embodiment of the ceramic particle aggregate, the ceramic particle aggregate may contain the ceramic particles and ceramic particles other than those specified in the present invention. For example, the aggregate may contain ceramic particles having the same composition as the ceramic particles of the present invention or a different composition, but having a different crystal structure from that of the present invention (i.e., not a single crystal and / or not having closed pores). As a composition different from the ceramic particles of the present invention, for example, a ceramic composite of strontium titanate and bismuth oxide is considered.
[0060] As another embodiment of the ceramic particle aggregate, it may be a composite material of the ceramic particles and an optional component, such as a resin, whose material is different from the ceramic.
[0061] The optional components may further include, for example, resins such as epoxy resins, phenolic resins, amino resins, diallyl phthalate resins, thermosetting urethane resins, and thermosetting acrylic resins; sintering aids such as yttrium oxide, magnesium oxide, aluminum oxide, cerium oxide, magnesium carbonate, calcium carbonate, and silicic acid; conductive or insulating materials such as various metals and oxides; optical adjusters; antistatic agents; colorants (organic or inorganic pigments, dyes, and the like); etc. The resins can also be used as organic binders.
[0062] For example, a resin can be used as the organic binder to strengthen the bond between particles, or the conductive material can be contained to control the electrical conductivity, dielectric constant, etc. of the ceramic particle aggregate. Alternatively, for example, a glass material can be added and then heated at a relatively low temperature to achieve densification. Alternatively, an optical adjuster such as light scattering particles can be added to control the refractive index. Since high refractive index materials generally contain heavy elements, when it is necessary to reduce the weight of the material, the high refractive index material can be combined with the ceramic particles of the present invention to reduce the weight while maintaining the light scattering ability.
[0063] (Proportion of ceramic particles defined in the present invention contained in the ceramic particle aggregate) The ratio of the ceramic particles in the ceramic particle aggregate is not limited. For example, in one embodiment, the volume fraction of the ceramic particles in the ceramic particle aggregate is 80% or more. In other words, additives such as the sintering aids are allowed in the ceramic particle aggregate, for example, within a range of 20% or less in volume fraction. The volume fraction of the ceramic particles may be 85% or more, further 90% or more, further 95% or more, or may be 100%, that is, the ceramic particle aggregate may be formed only of ceramic particles.
[0064] Examples of members formed from ceramic particle aggregates include laminates and composites that form multilayer ceramic capacitors, in which the volume fraction of ceramic particles may be less than 50%.
[0065] The volume fraction of any component other than the ceramic particles contained in the ceramic particle aggregate can be, for example, 20% or less, further 15% or less, further 10% or less, further 5% or less, or even 0%.
[0066] [Characteristics] (mechanical strength) The ceramic particles of the present invention have high mechanical strength. In the case of the porous body shown in Fig. 3, when an external load is applied, the grain boundaries break and collapse. In contrast, the porous body of this embodiment shown in Fig. 4 can ensure strength without grain boundary cracking.
[0067] (thermal stability) Furthermore, the ceramic particles have excellent thermal stability. The above-mentioned type 2 structure, i.e., a structure such as sintered ceramics composed of a large number of particles, generally has polycrystalline pores surrounded by a plurality of aggregated crystal particles. In that case, the pores are in contact with the grain boundaries. In general, grain boundaries having a disordered structure tend to play a role as a material transport path in ceramics. Therefore, it is expected that the grain boundary structure will change and material exchange will occur between the gas stored in the closed pores and the outside air as the temperature increases. In addition, when heat is applied to a structure having closed pores, surface reconstruction will occur to reduce surface energy, or the closed pores will not be able to maintain their shape due to chemical reactions between the inner surfaces of the closed pores and the gas, and the pores may disappear due to structural changes, or part of the crystals may be destroyed and converted into open pores.
[0068] Generally, ceramic members are synthesized at high temperatures of about 1000°C. Therefore, it is required that closed pores are maintained even after exposure to high temperatures of about 1000°C, i.e., that the thermal stability is excellent. When heated to 1000°C, the ceramic particles of the present invention suppress the number of broken closed pores to 10% or less of all closed pores.
[0069] Fig. 14 shows the thermal history of an aggregate of barium titanate particles according to one embodiment of the present invention and the results of a component analysis of desorbed gas when a ceramic particle aggregate containing 80 volume % or more of barium titanate ceramic particles obtained by the method described in Example 1 below was heated in a vacuum to 1200°C. The aggregate may also contain substances other than those specified in the present invention, such as ceramic particles that do not have closed pores and sintering aids.
[0070] In Figure 14, the signal with mass number 14 and the signal with mass number 28 move in parallel, which indicates that they correspond to nitrogen atoms and nitrogen molecules, respectively, and that the signal with mass number 28 is not carbon monoxide (CO) which has the same mass number as nitrogen, and the signal with mass number 14 is not CH2, a fragment of decomposed hydrocarbons, and it was confirmed that these signals show the desorption of nitrogen gas. Furthermore, since desorption is prominent at 1000°C or higher, it was confirmed that nitrogen desorption occurs at 1000°C or higher.
[0071] As shown in Fig. 14, a small amount of nitrogen gas component was observed to be desorbed near 1000°C. When the ceramic particles that had been heated to 1200°C were observed under an electron microscope, it was found that the nitrogen gas desorbed was due to the destruction of some of the closed pores in the ceramic particles, and most of the closed pores remained intact.
[0072] In other words, the ceramic particles of the present invention have closed pores that have high thermal stability, and the ceramic particles exhibiting such high thermal stability, as well as ceramic particle aggregates containing the ceramic particles, can fully exert the effects of the closed pores, such as weight reduction and light scattering, even after the synthesis of the above-mentioned ceramic component.
[0073] (Lightweight) Furthermore, a ceramic particle aggregate containing the ceramic particles of the present invention can be made lightweight. One embodiment of the ceramic particle aggregate of the present invention has a relative density of 95% or less of the true density when the ceramic particles contained in the ceramic particle aggregate do not contain closed pores.
[0074] The functions of ceramics are generally determined by their chemical composition and crystal structure. For example, (Ba 1-x Sr xIn the case of ceramics represented by the formula BaTiO3 (0≦x≦1), by increasing the Sr content x, it is possible to reduce the weight of the ceramics due to the difference in mass number. However, if the Sr content x is greater than 0.3, the characteristics of the ferroelectric at room temperature are lost. In other words, while the chemical formula weight of BaTiO3 is 233.2, when 30% of barium is replaced with strontium (Ba 0.7 Sr 0.3 The chemical formula weight of TiO3 is 218.3, and a weight reduction of about 6.5 percent in comparison with the chemical formula weight impairs the ferroelectric properties at room temperature. In such a case, by using ceramic particles with closed pores as in the present invention, it is possible to reduce the weight without lowering the Curie temperature as a ferroelectric.
[0075] The relative density is more preferably 93% or less, even more preferably 90% or less, and even more preferably 85% or less.
[0076] The above relative density is easily achieved when the ceramic particles are made of one or more materials selected from the group consisting of barium titanate, calcium titanate, lanthanum titanate, and titanium oxide, and is therefore preferable.
[0077] As an embodiment of the present invention, the results of measuring the relative density of a ceramic particle aggregate are shown in Table 1. Table 1 shows the results of measuring the relative density of a ceramic particle aggregate containing 80 volume % or more of barium titanate ceramic particles obtained by the method described in Example 1 below. The above measurement was performed twice, and a density of 5.5 grams per cubic centimeter was obtained in both cases. This density is about 92% of the theoretical density of barium titanate, which is 6.02. From Measurement 2 in Table 1, the volume of the ceramic particle aggregate occupied by the barium titanate ceramic particles is about 0.452 cubic centimeters. From this, 0.041 cubic centimeters of the total volume of the ceramic particle aggregate are closed pores, that is, 10.2 volume % of the total volume are closed pores.
[0078] [Table 1]
[0079] In addition, when the size of the ceramic particles (primary particles) is large, for example, on the order of millimeters or centimeters, closed pores may not be formed near the center of the particle, but may be formed only in the region close to the surface. In such a case, the relative density shows a value almost close to the true density when the ceramic particles contained in the ceramic particle aggregate do not contain closed pores. On the other hand, if the primary particle diameter is 1 μm or less, further, for example, 500 nanometers or less, it is possible to form closed pores up to the center of the particle, making it easy to achieve the above relative density.
[0080] [Method of manufacturing ceramic particles] A method for producing the ceramic particles or the ceramic particles contained in the ceramic particle aggregate includes a step of heat-treating ceramic raw material particles formed of a metal oxide containing titanium in an atmosphere containing ammonia and oxygen at 900°C or higher, and the amount of ammonia supplied is set to the amount of unreacted ammonia contained in the exhaust gas after the heat treatment.
[0081] To form closed pores within ceramic particles, rather than forming closed pores by agglomerating multiple particles as in Type 2, it is necessary to precipitate gas within the ceramic (solid) that constitutes the particles. The method of the present invention is an effective means for achieving this.
[0082] In the present invention, ammonia is used as the reactive gas. An atmosphere containing ammonia at a high temperature of 900°C or higher is an environment in which the effective chemical potential of nitrogen is increased. It is believed that by exposing ceramic raw material particles to an atmosphere containing ammonia at a high temperature of 900°C or higher, the ammonia reacts with the ceramic (solid) particle surface and dissociates ammonia molecules. As a result, the resulting nitrogen ions diffuse into the ceramic (solid), reassemble in the ceramic (solid), and re-precipitate as high-concentration nitrogen gas, that is, precipitate as stable gas phase molecules that are difficult to dissociate, forming closed pores filled with nitrogen gas.
[0083] Incidentally, even if heating is performed in nitrogen gas instead of the reactive gas ammonia, the above reaction mechanism does not occur. In addition, when only oxygen gas is used as the reactive gas, oxygen gas dissociates relatively easily, and may become oxygen ions and be taken into the solid, forming closed pores. However, since the oxygen gas that formed the closed pores is likely to react with the ceramic (solid), it is thought to diffuse inside the ceramic (solid), and as a result, it is dissipated from the outermost surface, and the closed pores are closed. In general, when the cavity is in a vacuum, the cavity tends to disappear when heated, according to the thermodynamic phenomenon that the system is energetically stabilized by reducing the surface area, but according to the method of the present invention, the cavity is filled with the stable nitrogen gas, and therefore it is thought that the cavity does not disappear.
[0084] In the present invention, the reaction is carried out in an atmosphere containing oxygen together with ammonia. For example, nitridation is easily promoted when calcium oxide is heated in ammonia, as calcium nitride is formed when calcium oxide is heated in ammonia. However, by using an atmosphere containing a mixed gas of ammonia and oxygen, it is possible to suppress the nitridation of ceramic (solid) particles while promoting the transport of nitrogen into the ceramic (solid) interior, and to reprecipitate nitrogen as nitrogen gas within the crystal particles, thereby forming closed pores filled with nitrogen gas. Nitrogen molecules are representative of molecules that are difficult to dissociate, and once they are taken into closed pores, they dissociate to become nitrogen ions, which do not diffuse through the solid and are not released to the outside.
[0085] The coexistence of the oxygen can fully exert the effect of suppressing nitridation. When the oxygen is supplied as a gas, for example, the oxygen is supplied at a volume fraction of 0.5% or more relative to the ammonia supplied. On the other hand, from the viewpoint of suppressing spontaneous combustion of ammonia, the volume fraction of oxygen is set to 10% or less relative to the ammonia supplied. However, oxygen is not limited to being supplied as a gas. For example, when a zirconia reaction tube is used as the reaction tube, ammonia may be introduced as a gas, and oxygen may be supplied from the outside air via the zirconia forming the reaction tube.
[0086] On the other hand, to realize the above reaction mechanism, it is necessary to diffuse a sufficient amount of nitrogen ions into the solid. When the nitrogen ion concentration in the solid is low, the probability of the nitrogen ions associating in the solid becomes extremely low, and as a result, closed pores filled with nitrogen gas are unlikely to form, and isolated nitrogen ions are merely contained as impurities.
[0087] In particular, nitrogen ions (N 3- ) is dissolved into another N with a certain probability while diffusing in the solid. 3- When they approach, two N 3- They can combine with each other to become N2 molecules. To form closed pores, the precipitation of these N2 molecules must be activated, i.e., N 3- We need to increase the probability that they will approach each other. This probability is N 3- The reaction is correlated with the concentration of N and the environment in the ceramic (solid), i.e., the Fermi level, and the defects and impurities present in the surroundings. 3- Incorporating N into a solid 3- It is essential to carry out heat treatment in an environment where the molecules can associate with each other to form N2 molecules.
[0088] The amount of ammonia to be supplied must be determined taking into consideration the spontaneous decomposition of ammonia due to heat in the reactor. When ammonia spontaneously decomposes due to heat to form nitrogen molecules and hydrogen molecules, its activity as a reactive gas is impaired. Therefore, taking into consideration the thermal decomposition of ammonia, it is necessary to supply a large amount of ammonia to the reactor, which exceeds the reaction rate at which ammonia is thermally decomposed in the reactor, that is, to the extent that unreacted ammonia remains even after the ammonia is consumed. The exhaust gas must contain ammonia that has not reacted in the thermal treatment, that is, ammonia that is not decomposed or absorbed in the thermal treatment and is discharged.
[0089] The amount of ammonia supplied is preferably adjusted so that the ammonia content in the exhaust gas is 5% or more. The ammonia content in the exhaust gas is more preferably 10% or more. On the other hand, the ammonia content in the exhaust gas is preferably 90% or less. The ammonia content in the exhaust gas is more preferably 5 to 40%, and further preferably 10 to 30%.
[0090] As a specific embodiment of the above-mentioned ammonia supply, it is preferable to continue to flow a certain amount of ammonia into the reactor. More specifically, in the process in which two reactions, spontaneous decomposition and incorporation into crystal particles for the formation of closed pores, proceed simultaneously, it is necessary to continue to flow a large amount of ammonia into the reactor so that unreacted ammonia remains even after ammonia is consumed. That is, in the present invention, in order to always flow fresh ammonia and to make the exhaust gas generated by the reaction in the heat treatment contain ammonia that was not decomposed or absorbed in the heat treatment, it is necessary to analyze the composition of the reacted exhaust gas discharged from the reactor, confirm the amount of unreacted ammonia in the exhaust gas, and introduce a sufficient amount of ammonia into the reactor so that unreacted ammonia can be detected in the exhaust gas.
[0091] As described above, in order to form closed pores, nitrogen ions must associate with each other in the ceramic (solid) to form nitrogen molecules. For example, if the diffusion rate of nitrogen ions is high, even if nitrogen ions are introduced into ceramic particles, they will diffuse toward the inside of the ceramic particles and penetrate the ceramic particles, making it difficult for the nitrogen ion concentration in the crystal to increase. In other words, the probability of nitrogen ions associating with each other decreases, making it difficult for nitrogen molecules to form. On the other hand, if the diffusion rate of nitrogen ions is slow, the next nitrogen will enter from the surface faster than the nitrogen ions introduced to the surface diffuse into the inside, making it easy for nitrogen molecules to precipitate on the surface of the particles, making it difficult for closed pores to form inside the ceramic particles. Therefore, in order to form closed pores, it is necessary to design the manufacturing process taking into account the diffusion coefficient (material transport property), the equilibrium solid solubility limit of nitrogen ions, and other solid physical properties and particle size of the ceramic particles used as raw materials, as well as the flow rate of the supplied ammonia gas and the reaction temperature.
[0092] The ceramic raw material particles do not have to be single crystals, and may be, for example, a sintered body or a powder.
[0093] By controlling the crystal orientation of the ceramic raw material particles in which closed pores are to be formed, the plane orientation of the closed pores can also be controlled. For example, in the photograph of FIG. 6 of the ceramic particles made of titanium oxide produced in Example 5 described later, flat closed pores nearly parallel to the surface of the ceramic raw material particles are formed. This is because titanium oxide, which is a tetragonal crystal, is used as the ceramic raw material particles, and it is believed that the flat closed pores nearly parallel to the surface of the ceramic raw material particles are formed due to the tendency of diffusion derived from the crystal orientation in which the gas diffusion coefficient is large in the c-axis direction in these ceramic raw material particles. That is, since diffusion is slow in the left-right direction of the paper in FIG. 6 and diffusion is fast in the up-down direction of the paper corresponding to the c-axis direction, the introduced nitrogen ions remain near the surface, and nitrogen actively diffuses in the in-plane direction parallel to the surface, so that vacancies parallel to the surface are formed as closed pores.
[0094] In order to form closed pores having a shape in a desired direction, it is preferable to take into consideration the diffusion coefficient of nitrogen and to use, as ceramic raw material particles, crystals cut to have the desired direction.
[0095] In order to obtain the desired ceramic particles, the method may include a step of subjecting the ceramic raw material particles used in the production of the ceramic particles to a treatment.
[0096] The reaction between ceramic raw material particles and ammonia begins with the adsorption of reactive gases onto the ceramic particle surfaces and the dissociation of ammonia. If the surfaces of the ceramic raw material particles are highly active against surface adsorption and molecular dissociation, the introduction of nitrogen ions as described above is promoted, and closed pores can be formed. In other words, the surface reactivity of the ceramic raw material particles is important. However, if the ceramic raw material particles are, for example, idiomorphic particles formed with highly stable crystal faces, the diffusion of nitrogen ions due to the decomposition of ammonia is hindered, and as a result, ceramic particles with closed pores may not be formed.
[0097] In such a case, a preliminary treatment (pretreatment) can be carried out, for example, by mechanically crushing the stable ceramic raw material particles to expose active surfaces.
[0098] In addition, to generate an interaction with visible light, a particle size of about the wavelength, i.e., about 500 nm, is desirable. On the other hand, when the ceramic raw material particles are fine, they may be synthesized by precipitation from a solution and contain moisture. Therefore, when the particle size of the raw material particles is around 100 nm or less than 100 nm, it is preferable to perform another pretreatment, such as heating in an oxygen-containing atmosphere, for example, heat treatment in air at 1000°C for about 4 hours, in order to dehydrate the ceramic raw material particles, modify the surface, and increase the size.
[0099] The method for producing ceramic particles may also include a step of heating in an oxygen-containing atmosphere after the heat treatment in the ammonia-containing atmosphere. For example, when used in optical applications in visible light, the substrate may be required to exhibit transparency. To form closed pores, treatment under conditions that cause oxygen vacancies may be required. Depending on the oxide constituting the ceramic raw material particles, when treated in a high-concentration ammonia atmosphere, the transparency may be impaired and colored due to the formation of oxygen vacancies. However, since the closed pores formed are thermally stable, as described above, a step of heating in an oxygen-containing atmosphere after the formation of the closed pores can be provided to eliminate the oxygen vacancies. For example, heating at a relatively high oxygen partial pressure, such as heat treatment in air, for example at 600°C for 1 hour, that is, by performing a treatment to eliminate oxygen vacancies, the blackness can be removed to realize transparency or whiteness, and the optical properties can be adjusted.
[0100] (Method for producing ceramic particle aggregate) When forming an aggregate using only the ceramic particles obtained by the above method, for example, a method for producing the aggregate may include forming the ceramic particles into an aggregate shape and then sintering the formed aggregate at a relatively low temperature so as not to crush the closed pores, for example, at about 800°C, to obtain a ceramic particle aggregate.
[0101] In the case of obtaining an aggregate containing the ceramic particles and a resin as the ceramic particle aggregate, in which the resin is used as an organic binder, the ceramic particles and the organic binder can be kneaded (a solvent may be added during kneading as necessary), molded, and solidified by exposure to light or by leaving the mixture. EXAMPLES
[0102] The present invention will be described in more detail below with reference to examples. The present invention is not limited to the following examples, and can be practiced with appropriate modifications within the scope of the above and below-mentioned aims, and all such modifications are included in the technical scope of the present invention. EXAMPLES
[0103] Barium titanate raw material powder, which is composed of particles with an irregular shape and an average particle diameter of 2 microns, was heat-treated in a reaction tube heated to 1000°C while circulating a gas containing air and ammonia. In detail, the reaction tube was made of refractory material and had an inner diameter of 50 mm. The gas discharged from the reaction tube was analyzed by a general gas chromatograph. In detail, the heat treatment was performed for 60 hours with the temperature of the reaction tube reaching 1000°C, the air volume being 0.02 liters, and the ammonia gas flow rate being increased to 0.5 liters per minute, to obtain a powder as a reaction product.
[0104] The exhaust gas from the heat treatment device (reaction tube) contained nitrogen gas and hydrogen gas produced by decomposition of ammonia, unreacted ammonia, and water vapor produced by the reaction of the oxygen in the mixed air with the hydrogen gas. The components of the exhaust gas were analyzed by a gas chromatograph, and it was confirmed that the exhaust gas contained 23% nitrogen, 23% ammonia, 0.2% oxygen, and 0.8% water vapor in volume fractions. In other words, in Example 1, a gas having a composition such that unreacted ammonia was contained in the exhaust gas as described above was circulated and reacted.
[0105] The powder, which is the reaction product, was subjected to density measurement and X-ray diffraction measurement.
[0106] (Measurement of density) Density measurements were carried out using helium gas as a medium. The density was measured at room temperature using an Accupyc dry densitometer manufactured by Shimadzu Corporation. The volume of the powder, including the closed pores, was precisely measured using helium gas, and if the mass of the powder is already known, the density of the powder can be obtained by dividing the mass of the powder by the volume mentioned above. On the other hand, X-ray diffraction matches the reported literature value for BaTiO3, so the theoretical density calculated from the lattice constant and chemical composition can be obtained. The ratio of closed pores can be calculated by comparing the theoretical density with the density measured using a densitometer. The results are shown in Table 1. A powder was obtained whose density was reduced by 10% compared to the density before the treatment.
[0107] (X-ray diffraction measurement) X-ray diffraction measurements were performed at room temperature using a Rigaku Smart Lab type powder X-ray diffractometer. Measurements were performed using the θ-2θ method with Cu-Kα radiation as the radiation source. Note that the measurement method is not limited to this, and other companies' devices may be used without any problem, and the radiation source may be a different source. X-ray diffraction measurements were performed, and the observed diffraction pattern was the same as that of pure barium titanate before processing.
[0108] The results of the density measurement and X-ray diffraction measurement confirmed the following. That is, since no phase change was observed from the results of the X-ray diffraction measurement, the observed density change was due to the formation of closed pores in the crystal particles constituting the barium titanate powder. That is, in this Example 1, by subjecting the barium titanate raw material powder as the ceramic raw material particles to a heat treatment in an atmosphere containing ammonia and oxygen, a lightweight barium titanate powder with a density reduced by about 8% was obtained without causing phase separation.
[0109] (Observation by transmission electron microscope) The closed pores were observed using a transmission electron microscope. In detail, the reactant powder was ground in an agate mortar, and then the structure was observed using a transmission electron microscope. As a result, the image of the single crystal particle showed multiple square contrasts of about several tens of nanometers, and the contrast was characterized by the (001) plane.
[0110] Moreover, the observation by the transmission electron microscope gave the same results as those shown in Figs. 5 and 7, and it was confirmed that the obtained ceramic particles were single crystals.
[0111] (Observation of closed pores by electron energy loss spectroscopy) The contrasting rectangular area was irradiated with an electron beam and electron energy loss spectroscopy was performed, revealing that the spectrum corresponded to the electron energy loss of nitrogen molecules.
[0112] The above-mentioned transmission electron microscope observation and electron energy loss spectroscopy measurements revealed that the crystal particles had closed pores with the (001) plane as the inner surface corresponding to the crystal habit, and that the closed pores were filled with nitrogen gas. In other words, the obtained lightweight barium titanate powder had an extremely low probability of its particles being destroyed and its closed pores being converted into open pores even when crushed in a mortar, and was a lightweight barium titanate that had closed pores but exhibited high mechanical strength.
[0113] (Evaluation by high temperature heating) The reaction powder was heated to 1200°C in a vacuum, and the desorbed gases during heating were analyzed. As a result, the thermal desorption spectrum shown in FIG. 15 was obtained. FIG. 15 also shows the heat treatment pattern. From FIG. 15, a slight amount of nitrogen gas was observed when the sample temperature reached 1000°C. On the other hand, the powder in which a slight amount of nitrogen gas was observed to be desorbed by heating up to 1200°C was observed under an electron microscope, but no trace of gas desorption due to the destruction of closed pores was found. In addition, the powders after heating up to 1200°C other than the powder in which the nitrogen gas desorption was observed were also observed under an electron microscope, but no change in particle shape due to the rupture of closed pores or disappearance of closed pores was observed.
[0114] From the results of the thermal desorption spectrum and the electron microscope observation, in this example, closed pores containing nitrogen gas and covered with habit planes were formed, and thus a lightweight barium titanate was obtained in which the closed pores were not destroyed when heated up to 1000° C. It is considered that in the powder in which a small amount of nitrogen gas was observed to be desorbed, a very small number of closed pores with thin and fragile walls ruptured when the sample temperature reached 1000° C. in a vacuum, releasing the nitrogen gas inside the closed pores, resulting in the detection of nitrogen gas. EXAMPLES
[0115] The barium titanate powder was heat-treated in the same manner as in Example 1, except that the reaction time was 40 hours, to obtain a powder as a reaction product.
[0116] X-ray diffraction measurement of the obtained powder revealed no signs of phase decomposition, and the powder had the same crystal phase as barium titanate before the treatment.
[0117] (Transmission electron microscope observation) A sample was taken from near the surface of the powder that had been exposed to the gas flow during heat treatment, and its structure was observed using a transmission electron microscope. The results showed that it was a single crystal particle containing a phase crystal with the (111) plane as the twin boundary, with the longest side being approximately 200 nanometers. The image of this single crystal particle showed a similar appearance to that shown in Figure 5, that is, multiple square contrasts of about several tens of nanometers in size, and this contrast was characterized by the (001) plane.
[0118] (Electron energy loss spectroscopy) The rectangular contrast area was irradiated with an electron beam and electron energy loss spectroscopy was performed. The resulting spectrum was similar to that shown in Figure 7, with a barium peak instead of a calcium peak and including a peak corresponding to the electron beam loss of nitrogen molecules.
[0119] From the above-mentioned transmission electron microscope observation and the above-mentioned electron energy loss spectroscopy measurement, it was found that the crystal particles had closed pores with the (001) plane corresponding to the crystal habit as the inner surface, and the closed pores were filled with nitrogen gas. That is, in this example, barium titanate particles were obtained that were lightweight due to the formation of closed pores covered with the crystal habit plane and containing gas mainly composed of nitrogen gas. EXAMPLES
[0120] A heat treatment was carried out in the same manner as in Example 2, except that calcium titanate powder was used as the raw material, to obtain a powder as a reaction product.
[0121] X-ray diffraction measurement of the obtained powder revealed no signs of phase decomposition, and the powder had the same crystal phase as calcium titanate before the treatment.
[0122] As in Example 2, a sample for observation was taken from the surface of the powder exposed to the gas flow during heat treatment, and its structure was observed using a transmission electron microscope. The results showed that the particle was a single crystal with the longest side of about 200 nanometers. The image of this single crystal particle showed multiple rectangular contrasts similar to those shown in Figure 5, and the contrast was characterized by the (001) plane.
[0123] Moreover, electron energy loss spectroscopy was performed by irradiating the rectangular contrast portion with an electron beam in the same manner as in Example 2. As a result, a spectrum including a peak corresponding to the electron beam loss of nitrogen molecules was obtained.
[0124] From the above-mentioned transmission electron microscope observation and the above-mentioned electron energy loss spectroscopy measurement, it was found that the crystal particles have closed pores with the (001) plane corresponding to the crystal habit as the inner surface, and the closed pores are filled with nitrogen gas. That is, in this example, calcium titanate particles were obtained that were lightweight due to the formation of closed pores covered with the crystal habit plane and containing gas mainly composed of nitrogen gas. EXAMPLES
[0125] A heat treatment was carried out in the same manner as in Example 2, except that strontium titanate powder was used as the raw material, to obtain a powder as a reaction product.
[0126] X-ray diffraction measurement of the obtained powder revealed no signs of phase decomposition, and the powder had the same crystal phase as strontium titanate before the treatment.
[0127] As in Example 2, a sample for observation was taken from the surface of the powder exposed to the gas flow during heat treatment, and its structure was observed using a transmission electron microscope. The results showed that the particle was a single crystal with the longest side of about 200 nanometers. The image of this single crystal particle showed a contrast of multiple squares of about several tens of nanometers, similar to the aspect shown in Figure 5, and the contrast was characterized by the (001) plane.
[0128] Moreover, electron energy loss spectroscopy was performed by irradiating the rectangular contrast portion with an electron beam in the same manner as in Example 2. As a result, a spectrum including a peak corresponding to the electron beam loss of nitrogen molecules was obtained.
[0129] From the above-mentioned transmission electron microscope observation and the above-mentioned electron energy loss spectroscopy measurement, it was found that the crystal particles have closed pores with the (001) plane corresponding to the crystal habit as the inner surface, and the closed pores are filled with nitrogen gas. That is, in this example, strontium titanate particles were obtained that were lightweight due to the formation of closed pores covered with the crystal habit plane and containing gas mainly composed of nitrogen gas. EXAMPLES
[0130] A single crystal made of titanium oxide, 10 mm in length and width and approximately 0.5 mm in thickness, was heat-treated at 1,000°C for 40 hours in an ammonia-containing atmosphere controlled at a flow rate of 100 cubic centimeters of ammonia and 20 cubic centimeters of air per minute to obtain a single crystal after the reaction.
[0131] (Optical microscope observation) The obtained single crystal was broken, and its internal structure was observed using an optical microscope. As a result, as shown in Figure 6, at a depth of about 50 to 100 micrometers from the (010) surface of the single crystal, <001> Closed pores 15 with a length in the axial direction of about 300 micrometers were observed.
[0132] (Mapping observation by Raman scattering) The obtained single crystal was subjected to mapping by Raman scattering, and the results shown in Figure 11 were obtained. In Figure 11, a Raman scattering signal corresponding to the molecular vibration of nitrogen molecules was observed from inside the closed pores. Note that nitrogen gas in the atmosphere was not observed using this measurement method.
[0133] The optical microscope observation and the Raman scattering mapping measurements show that the pores formed in the crystal were closed pores, and that the insides of these closed pores were filled with nitrogen gas. In other words, in this example, a lightweight titanium oxide single crystal was obtained that had large closed pores exceeding 100 micrometers. EXAMPLES
[0134] Titanium oxide powder (same size as in Example 5) was heat-treated at 1000°C for 40 hours in an atmosphere controlled with ammonia at a flow rate of 500 cubic centimeters per minute and air at a flow rate of 10 cubic centimeters per minute to synthesize powder. After that, heat treatment was further performed in air at 600°C for 1 hour to eliminate oxygen deficiency and obtain a powder with no black color. In other words, after the formation of closed pores, a step of heating in an oxygen-containing atmosphere was further added to adjust the optical properties.
[0135] X-ray diffraction measurement of the obtained powder revealed no signs of phase decomposition, and the powder had the same crystalline phase as the titanium oxide before treatment.
[0136] The powder thus obtained was subjected to Raman scattering spectroscopy analysis, and a signal characteristic of nitrogen molecules was observed. From the above-mentioned Raman scattering mapping measurement, it was confirmed that titanium oxide powder having closed pores containing nitrogen molecules, that is, lightweight titanium oxide powder, was obtained in Example 6. EXAMPLES
[0137] Barium titanate powder containing nitrogen gas in its closed pores, obtained under the same conditions as in Example 1, was kneaded with epoxy resin at a volume ratio of 10%, and the mixture was thoroughly degassed and solidified to obtain an aggregate of barium titanate.
[0138] When this aggregate was polished and the polished surface was observed under an electron microscope, it was confirmed that the structure was formed by barium titanate having closed pores bound and aggregated by epoxy resin. In this example, by adding epoxy resin, a ceramic particle aggregate having a high refractive index and reduced weight was obtained. EXAMPLES
[0139] In Example 8, a commercially available reagent was used as the raw strontium titanate particles, and it was confirmed by electron microscope observation that this commercial reagent was a powder consisting of cubic particles with a relatively developed (001) face and a side length of about 100±50 nanometers. The particle size and particle shape suggested that the reagent may have been synthesized by precipitation from a solution. Therefore, it was considered necessary to perform heat treatment and dehydration by burning, and the raw strontium titanate particles were subjected to heat treatment (pretreatment) in the air at 1000°C for about 4 hours, and then heat treatment was performed under the same conditions as in Example 4 to synthesize a powder.
[0140] X-ray diffraction measurement of the obtained powder showed that no phase decomposition was observed in either the heat treatment in air at 1000°C for about 4 hours or the heat treatment under the same conditions as in Example 4, and the powder had the same crystal phase as strontium titanate before the treatment. A low-density polycrystalline aggregate as shown in Figure 3 was obtained by the heat treatment in air at 1000°C (pretreatment), but subsequent heat treatment under the same conditions as in Example 4 yielded a powder made of single crystals having closed pores similar to that in Example 4. Comparative Example 1
[0141] Barium titanate raw material particles were heat-treated for 40 hours at 1000°C in an atmosphere where only pure ammonia gas was flowing at 200 cubic centimeters per minute. As a result, the powder was transformed into a mixture of Ba2TiO4 and TiN, and no light-weight barium titanate was obtained. The obtained powder was black in color due to TiN. Comparative Example 2
[0142] Barium titanate raw material particles were heat treated at 1000°C in air for 40 hours to obtain ceramic particles as a reaction product.
[0143] X-ray diffraction measurement of the obtained ceramic particles showed no signs of phase decomposition, and the crystal phase was the same as that of barium titanate before treatment. In addition, when the structure was observed using a transmission electron microscope, it was confirmed that the ceramic particles had aggregated due to the heat treatment, and that the aggregation had caused the formation of pores surrounded by multiple ceramic particles. However, in Comparative Example 2, no closed pores were observed. Comparative Example 3
[0144] The powder was synthesized by heat treating strontium titanate raw material particles at 1000°C in pure hydrogen gas for 20 hours.
[0145] X-ray diffraction measurement of the obtained powder showed no signs of phase decomposition, and the crystal phase was the same as that of barium titanate before treatment. In addition, the diffusion state of hydrogen into the crystal after heat treatment was checked, but no high concentration of hydrogen was diffused, and no closed pores were formed. In other words, the decomposed components of hydrogen gas did not diffuse into the crystal and were not reprecipitated, so no closed pores were formed. Heat treatment in hydrogen promotes the generation of oxygen vacancies due to oxygen elimination rather than the penetration of hydrogen, and is not effective in the formation of open pores. Comparative Example 4
[0146] The raw strontium titanate particles used were a commercially available reagent, and were confirmed to have a cubic particle shape with a developed (001) face when observed under an electron microscope. The raw strontium titanate particles were formed into a tablet shape and fired at 900°C in ammonia-free air to obtain a sintered body. The relative density of the sintered body was approximately 90%. Furthermore, when the obtained sintered body was broken and the cross section was observed, it had a structure in which pores existed between the particles as shown in Figure 3, and no particles with a structure as shown in Figure 4 were formed. Comparative Example 5
[0147] Approximately 25 grams of titanium oxide powder was heat-treated at 1000°C for 16 hours in an ammonia-containing atmosphere controlled at a flow rate of 100 cubic centimeters of ammonia and 20 cubic centimeters of air per minute to obtain heat-treated powder. Analysis of the composition of the exhaust gas during the heat treatment revealed that the ammonia concentration in the exhaust gas was low, less than 2%.
[0148] X-ray diffraction measurements were performed on the powder obtained, and the crystal phase of the powder obtained was rutile-type titanium oxide, the same as before the heat treatment. When the powder was analyzed by Raman scattering, no Raman scattering signal corresponding to the molecular vibration of nitrogen molecules was observed. In other words, it was confirmed that a structure of closed pores containing nitrogen molecules was not formed.
[0149] In the above-mentioned Example 5, the titanium oxide single crystal was heat-treated, and its mass was about 0.2 grams. In contrast, in this comparative example, about 25 g of powder was treated. Since the powder has a large surface area and the amount of powder added was more than 100 times the amount of the single crystal, it is considered that the ammonia added was almost completely decomposed, and a sufficient amount of ammonia for the formation of closed pores was not supplied, and closed pores were not formed. Therefore, in manufacturing ceramic particles having the desired closed pores, it is necessary to analyze the exhaust gas composition and confirm that the ammonia in the exhaust gas has a sufficient concentration before manufacturing. [Industrial Applicability]
[0150] The ceramic particles and ceramic particle aggregates of the present invention are capable of forming a fine pore structure, and are therefore useful as porous materials for constituting components of materials, elements, etc., with controlled thermal conductivity properties including weight reduction and thermal insulation, and are also useful as materials for thermoelectric elements, which require a structure that reduces thermal conductivity.
[0151] Furthermore, unlike conventional porous materials, open pores can be suppressed. In other words, by reducing the surface area, a porous body can be realized that suppresses external disturbance due to surface adsorption and deterioration over time due to surface reactions. For example, the porous body can be used as an electronic ceramic that is used by connecting electrodes. Furthermore, since the closed pores have the effect of scattering light rays, it can also be used as a material for adjusting optical properties. Alternatively, by providing many fine open pores and supporting a catalyst in the open pores, a catalyst with many reactive active sites and high surface chemical activity can be provided.
[0152] When the ceramic particles of the present invention are composed of, for example, barium titanate, they are useful as PTCR (Positive Temperature Coefficient of Resistivity) ceramics that utilize the grain boundary properties of the barium titanate. Since PTCR ceramics are used as temperature sensors, it is possible to realize sensitive temperature detection by reducing the heat capacity. Therefore, by forming barium titanate ceramics that have hollow closed pores and are appropriately doped with manganese, niobium, or the like, it is possible to manufacture PTCR ceramics that are lightweight and have a small heat capacity. The disclosure of this specification may include the following aspects. <1> A ceramic particle formed of a metal oxide containing titanium, which is a single crystal and contains closed pores within the single crystal. <2> The inner surfaces of the closed pores have a plane orientation. <1> The ceramic particles according to claim 1. <3> The main component of the gas in the closed pores is nitrogen gas. <1> or <2> The ceramic particles according to claim 1. <4> The plane orientation is a plane in which any one or two of h, k, and l in (hkl) are zero, a (111) plane, or a (112) plane; <2> or <3> The ceramic particles according to claim 1. <5> The closed pores have a hexahedral shape. <2> ~ <4> 13. The ceramic particles according to any one of claims 1 to 12. <6> When heated to 1000°C, the percentage of damaged closed pores among all closed pores is 10% or less. <1> ~ <5> 13. The ceramic particles according to any one of claims 1 to 12. <7> The titanium-containing metal oxide is at least one selected from the group consisting of barium titanate, calcium titanate, strontium titanate, lanthanum titanate, and titanium oxide. <1> ~ <6> 13. The ceramic particles according to any one of claims 1 to 12. <8> The average particle size of the ceramic particles is 1 μm or less, and the average dimension of the closed pores is 100 nanometers or less on the longest side. <1> ~ <7> 13. The ceramic particles according to any one of claims 1 to 12. <9> <1> ~ <8> 2. A ceramic particle aggregate comprising a plurality of ceramic particles according to any one of claims 1 to 11. <10> The volume fraction of the ceramic particles contained in the ceramic particle aggregate is 80% or more. <9> 2. The ceramic particle aggregate according to claim 1 . <11> The relative density is 95% or less of the true density when the ceramic particles contained in the ceramic particle aggregate do not contain closed pores. <9> or <10> 2. The ceramic particle aggregate according to claim 1 . <12> Further comprising a resin, <9> ~ <11> 2. The ceramic particle aggregate according to claim 1 . <13> <1> ~ <12> A method for producing ceramic particles or ceramic particles contained in a ceramic particle aggregate according to any one of the above claims, comprising the steps of: The method includes a step of heat-treating ceramic raw material particles formed of a metal oxide containing titanium at 900° C. or higher in an atmosphere containing ammonia and oxygen, The method for producing ceramic particles, wherein the amount of ammonia supplied is set to an amount that corresponds to the amount of unreacted ammonia contained in exhaust gas after heat treatment. <14> The ammonia content in the exhaust gas is 5 to 90% by volume fraction. <13> A method for producing ceramic particles according to claim 1. <15> After the heat treatment step, a step of heating in an oxygen-containing atmosphere is included. <13> or <14> A method for producing ceramic particles according to claim 1. <16> Before the heat treatment, the ceramic raw material particles formed of the titanium-containing metal oxide are heated in an oxygen-containing atmosphere. <13> ~ <15> 13. The method for producing ceramic particles according to claim 12, [Explanation of symbols]
[0153] 1 Open pores 2 Bulk body 3 Needle material 4 Substrate material 5. Closed pores 6 Crystal substrate X single crystal 7. Calcium titanate crystal particles 8, 15 Closed pores 9. a-axis direction of crystal grains 16 Titanium oxide single crystal 17 a-axis 18 b-axis 19 c-axis
Claims
1. A ceramic particle formed of a metal oxide containing titanium, the ceramic particle being a single crystal, the single crystal containing closed pores, the main component of the gas in the closed pores being nitrogen gas.
2. The ceramic particles according to claim 1 , wherein the inner surfaces of the closed pores have a plane orientation.
3. The ceramic particles according to claim 2 , wherein the plane orientation is a plane in which any one or two of h, k, and l in (hkl) are zero, a (111) plane, or a (112) plane.
4. The ceramic particles according to any one of claims 1 to 3, wherein the closed pores have a hexahedral shape.
5. 5. The ceramic particles according to claim 1, wherein when heated to 1000° C., the number of broken closed pores accounts for 10% or less of all closed pores.
6. The ceramic particles according to any one of claims 1 to 5, wherein the metal oxide containing titanium is at least one selected from the group consisting of barium titanate, calcium titanate, strontium titanate, lanthanum titanate, and titanium oxide.
7. 7. The ceramic particles according to claim 1, wherein the average particle size of the ceramic particles is 1 μm or less, and the average dimension of the longest side of the closed pores is 100 nanometers or less.
8. A ceramic particle aggregate comprising a plurality of ceramic particles according to any one of claims 1 to 7.
9. 9. A ceramic particle aggregate according to claim 8, wherein a volume fraction of the ceramic particles contained in the ceramic particle aggregate is 80% or more.
10. 10. A ceramic particle aggregate according to claim 8, having a relative density of 95% or less of a true density when the ceramic particles contained in the ceramic particle aggregate do not contain closed pores.
11. The ceramic particle aggregate according to any one of claims 8 to 10, further comprising a resin.
12. A method for producing ceramic particles according to any one of claims 1 to 7, or ceramic particles contained in a ceramic particle aggregate according to any one of claims 8 to 11, comprising the steps of: The method includes a step of heat-treating ceramic raw material particles formed of a metal oxide containing titanium at 900° C. or higher in an atmosphere containing ammonia and oxygen, The method for producing ceramic particles, wherein the amount of ammonia supplied is set to an amount that corresponds to the amount of unreacted ammonia contained in exhaust gas after heat treatment.
13. The method for producing ceramic particles according to claim 12, wherein the ammonia content in the exhaust gas is 5 to 90% by volume.
14. The method for producing ceramic particles according to claim 12 or 13, further comprising a step of heating in an oxygen-containing atmosphere after the heat treatment step.
15. The method for producing ceramic particles according to any one of claims 12 to 14, further comprising a step of heating ceramic raw material particles formed of the titanium-containing metal oxide in an oxygen-containing atmosphere before the heat treatment.
Citation Information
Patent Citations
Hollow single crystal of inorganic oxide, crystal material containing the single crystal, and methods for producing them
JP2005314190A
Ceramic porous body
JP2006342054A
Oxide hollow particles, production method thereof and apparatus for manufacturing oxide hollow particles
JP2010120786A
Method for producing conductive zinc oxide film
JP2012144384A
Oxidized-titanium spherical particle, method for producing the same, and optoelectronic device using oxidized-titanium spherical particle
JP2013043788A