How Graphene is Made

A method for producing graphene with large area and good crystallinity using a crystallized Ni layer on a sapphire substrate addresses electron mobility issues, enabling high-quality graphene production for integrated circuits.

JP7586485B2Active Publication Date: 2024-11-19MEIJO UNIVERSITY

Patent Information

Application Number
JP2021042623
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-16
Publication Date
2024-11-19
Estimated Expiration
2041-03-16

AI Technical Summary

Technical Problem

Existing methods for producing graphene result in decreased electron mobility at boundaries and require graphene with large area and good crystallinity for use in transistors and integrated circuits, necessitating a metal catalyst layer with larger crystal grains and a method for easy production.

Method used

A method involving a first lamination step of crystallized Ni on a sapphire substrate, followed by an amorphous Ni layer, heat treatment, and application of nanodiamonds to produce high-quality graphene with large area and good crystallinity, using a metal catalyst layer with a face-centered cubic structure aligned with the substrate's corundum structure.

Benefits of technology

The method produces high-quality graphene with no wrinkles over a large area, suitable for integrated circuits, by ensuring single-crystalline metal catalyst layers and controlled graphene layer formation without defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586485000001
    Figure 0007586485000001
  • Figure 0007586485000002
    Figure 0007586485000002
  • Figure 0007586485000003
    Figure 0007586485000003
Patent Text Reader

Abstract

To provide a metal catalyst layer capable of generating good quality graphene; and to provide a production method of the metal catalyst layer, a production method of graphene, and good quality graphene.SOLUTION: A metal catalyst layer 20 laminated and crystallized on c surface of a sapphire substrate 10 having a corundum structure, has a face-centered cubic structure, and [111] direction is c surface axial direction of the sapphire substrate 10, and [01-1] direction agrees with [11-20] direction of the sapphire substrate 10.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention Hagu How to make laphene By law This is related to. [Background technology]

[0002] In Patent Document 1, a film pattern of a catalytic metal is formed on an insulating substrate by vapor deposition, graphene is grown on the film pattern, and then a drain electrode and a source electrode are formed on both sides of the graphene, and a gate electrode is formed on the graphene via a gate insulating film. Patent Document 1 describes that the catalytic metal film patterns are separated by an insulating film, but since the graphene extends laterally at the ends of the film pattern, a structure is obtained in which the graphene extends from the film patterns on both sides of the insulating separation film and is connected on the insulating separation film. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2009-164432 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, when graphene is produced by the method described in Patent Document 1, there are cases where the mobility of electrons is reduced at the boundary where the graphene extending from the film patterns on both sides is connected. In order to improve this point and produce a transistor with better characteristics, a technology that can produce graphene with a large area and graphene with good crystallinity without connecting graphene in the middle has been desired. If graphene with a large area can be obtained, it will be possible to use graphene not only in transistors but also in larger integrated circuits and the like. However, in order to produce graphene with good crystallinity over a large area, it is necessary to increase the crystal grains of the metal catalyst layer for growing graphene. Therefore, in order to produce graphene with good crystallinity over a large area, a metal catalyst layer with larger crystal grains and a method for easily producing such a metal catalyst layer have been desired.

[0005] The present invention has been made in consideration of the above-mentioned conventional circumstances, and has an object to be achieved by providing a metal catalyst layer capable of producing good-quality graphene, a method for producing a metal catalyst layer, a method for producing graphene, and good-quality graphene. [Means for solving the problem]

[0006] The metal catalyst layer of the first invention is A metal catalyst layer laminated and crystallized on a c-plane of a substrate having a corundum structure, It has a face-centered cubic structure,

[0111] The direction is the c-plane axial direction of the substrate, The [01-1] direction is the [11-20] direction of the substrate.

[0007] The method for producing a metal catalyst layer according to the second aspect of the present invention comprises the steps of: a first deposition step of forming a first layer of crystallized catalytic metal on the surface of the substrate; a second lamination step of forming a second layer of the catalytic metal in an amorphous state on a surface of the first layer; a first heat treatment step of performing a heat treatment to crystallize the second layer after the first lamination step and the second lamination step are performed; Equipped with.

[0008] The method for producing graphene according to the third aspect of the present invention comprises the steps of: a carbon raw material laminating step of laminating a carbon raw material on a surface of the metal catalyst layer after carrying out the first heat treatment step in the method for producing a metal catalyst layer of the second invention; a second heat treatment step of carrying out a heat treatment after carrying out the carbon raw material lamination step to precipitate graphene between the substrate and the metal catalyst layer; Equipped with.

[0009] The graphene of the fourth invention is 0.01 cm 2 From 180cm 2 The area is free of wrinkles.

[0010] Use of the metal catalyst layer of the first aspect of the invention makes it possible to produce graphene of good quality.

[0011] The method for producing a metal catalyst layer according to the second aspect of the present invention can produce a metal catalyst layer having good crystal quality.

[0012] The graphene production method of the third invention makes it easy to produce large-area graphene with good crystallinity that has no wrinkles at the interface between the substrate and the metal catalyst layer.

[0013] The graphene of the fourth invention can be used in devices requiring a large area, such as integrated circuits. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a schematic diagram showing a method for producing a metal catalyst layer and a method for producing graphene in Example 1. [Diagram 2] 13 shows images obtained by observing, using an SEM, the surfaces of samples in which the temperature for depositing Ni was changed to five different values ​​in the first lamination step in the graphene production method of Example 1. [Diagram 3]13 shows the results of measuring samples obtained by changing the temperature at which Ni is evaporated in five different steps in the first lamination step in the graphene production method of Example 1, using an In-plane X-ray diffraction measurement method. [Figure 4] FIG. 2 is a schematic diagram showing the crystal structure of the surface of a sapphire substrate when viewed from the front. [Diagram 5] 1 is a schematic diagram showing a crystal structure of a surface of a sapphire substrate after a first lamination step, as viewed from the front. FIG. [Figure 6] 1 shows images of the surfaces of samples of Example 2, Comparative Example 1, and Comparative Example 2 observed using a differential interference contrast microscope. [Figure 7] The results are obtained by measuring the samples of Example 2, Comparative Example 1, and Comparative Example 2 by an out-plane X-ray diffraction measurement method. [Figure 8] The results are obtained by measuring the samples of Example 2, Comparative Example 1, and Comparative Example 2 by an In-plane X-ray diffraction measurement method. [Figure 9] 1 shows an image of the graphene surface of the sample of Example 2 observed using a differential interference contrast microscope, and a result of evaluating the graphene surface of the sample of Example 2 by Raman scattering spectroscopy. [Figure 10] FIG. 10 is an image of the graphene surface of the sample of Example 2 observed with an optical microscope at a position different from that in FIG. 9, and shows the magnitude of the D / G value within a rectangular frame shown in the image by using light and dark. [Figure 11] This shows the results of measuring the sample of Example 2 using an In-plane X-ray diffraction measurement method after the second heat treatment process was performed. [Figure 12] FIG. 11 is a schematic diagram showing the orientation relationship of the sample of Example 3. [Figure 13] 13 is an image of the graphene surface of the sample of Example 3 observed using a microscope. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] A preferred embodiment of the present invention will now be described.

[0016] The carbon raw material in the graphene production method of the third invention may be nanodiamond. In this case, graphene can be continuously grown during heat treatment at a growth rate determined by the heat treatment temperature, and the number of graphene layers produced at the interface between the substrate and the metal can be easily controlled.

[0017] Next, first to third embodiments of the present invention will be described with reference to the drawings.

[0018] <Example 1> First, a method for producing a metal catalyst layer using a catalytic metal having good crystal quality over the entire surface of a desired substrate, and a method for producing graphene that produces graphene that does not have wrinkles at the interface between the produced metal catalyst layer and the substrate will be described.

[0019] First, as shown in FIG. 1(A), a sapphire substrate 10 is prepared as a substrate. The outer shape of the sapphire substrate 10 is a square of approximately 10 mm×10 mm. Then, the sapphire substrate 10 is set in a chamber of a molecular beam epitaxy apparatus (not shown). The molecular beam epitaxy apparatus can perform a molecular beam epitaxy method (MBE) (hereinafter, simply referred to as an MBE method). The c-plane ((0001) plane) of the sapphire substrate 10 is the surface (the front is the upper side in FIG. 1; the same applies below). The crystal structure of sapphire is a corundum structure. That is, the sapphire substrate 10 has a corundum structure.

[0020] [Method of generating metal catalyst layer] Next, as shown in FIG. 1(B), a first lamination step is performed to form a first layer 11 of a crystallized catalytic metal on the surface of the sapphire substrate 10. Specifically, the first layer 11 is laminated by crystal growth of Ni, which is a catalytic metal, on the surface of the sapphire substrate 10 using the MBE method. The thickness of the first layer 11 is about 100 nm. The thickness of the first layer 11 may be in the range of 20 nm to 300 nm as long as the aggregation of Ni does not progress significantly. Note that if the thickness of the first layer 11 is less than 20 nm, the Ni layer remains in an island shape, making it difficult to use. At this time, the temperature of the sapphire substrate 10 is 600° C. to 700° C. The crystal structure of Ni is a face-centered cubic structure. That is, Ni has a face-centered cubic structure. By performing the first lamination step, the crystallized first layer 11 can be laminated on the surface of the sapphire substrate 10.

[0021] Next, as shown in FIG. 1(C), a second lamination step is performed to form a second layer 12 of a catalytic metal in an amorphous state on the surface of the first layer 11. Specifically, Ni is evaporated on the surface of the first layer 11 by electron beam evaporation to laminate the second layer 12. The thickness of the second layer 12 is about 300 nm. Here, the thickness of the second layer 12 may be in the range of 200 nm to 700 nm, as long as it is a thickness that allows crystallization in the next first heat treatment step. If the thickness is thicker than this, crystallization may start from the surface of the second layer 12 when the first heat treatment step is performed, and crystallization using the crystal information of the first layer 11 cannot be performed on the surface side of the second layer 12, resulting in polycrystals. By performing the second lamination step, the second layer 12 of Ni in an amorphous state can be laminated on the surface of the first layer 11.

[0022] Next, after the first lamination step and the second lamination step are performed, a first heat treatment step is performed to crystallize the second layer 12 by heat treatment. In detail, the sapphire substrate 10 on which the first layer 11 and the second layer 12 are laminated is taken out from the chamber of the vacuum deposition device and set in a heat treatment device (not shown). The sapphire substrate 10 on which the first layer 11 and the second layer 12 are laminated is heated to 1000°C in a hydrogen atmosphere and maintained in this state for 30 minutes. Thereafter, the temperature of the sapphire substrate 10 is lowered to 650°C at a rate of 3°C / min, and then the temperature is returned to room temperature (for example, about 23°C). In this way, the second layer 12 is crystallized. In this way, as shown in FIG. 1(D), a metal catalyst layer 20 having the first layer 11 and the second layer 12 is generated. Here, the temperature lowering rate is not limited to 3°C / min, and may be 10°C / min.

[0023] [How to produce graphene] Next, as shown in FIG. 1(E), after the first heat treatment step, a carbon raw material lamination step is performed in which nanodiamond 13, which is a carbon raw material, is applied and laminated on the surface of the metal catalyst layer 20. Nanodiamond is a type of artificial diamond, and has a particle shape with a particle size of several nm. Nanodiamond is a metastable sp 3 It has a bond structure and is stable sp 2 Graphene can be produced at a lower temperature than when other carbon raw materials having a bond structure are used. Nanodiamond 13 is dispersed in an aqueous solution and applied to the surface of the metal catalyst layer 20 using a spin coater. The rotation speed and rotation time of the spin coater when applying nanodiamond 13 to the surface of the metal catalyst layer 20 are, for example, 6000 rpm and 30 seconds.

[0024] Next, as shown in FIG. 1(F), after the carbon raw material lamination step, a second heat treatment step is performed in which heat treatment is performed to precipitate graphene 14 between the sapphire substrate 10 and the metal catalyst layer 20. Specifically, the sapphire substrate 10 with the nanodiamond 13 applied to the surface of the metal catalyst layer 20 is set in a heat treatment device (not shown). Then, with the sapphire substrate 10 set, the heat treatment device is heated for approximately 10 minutes. -4The pressure is set to 10 Pa. Then, the temperature of the sapphire substrate 10 is set to about 900°C. Then, the sapphire substrate 10 is subjected to a heat treatment for about 30 minutes. As a result, C (carbon) of the nanodiamond 13 is dissolved in the metal catalyst layer 20, and the dissolved C precipitates as graphene 14 at the interface between the sapphire substrate 10 and the metal catalyst layer 20. Then, the temperature of the sapphire substrate 10 is lowered to 300°C at a rate of 3°C / min, and then the temperature is lowered to room temperature (for example, about 23°C). At this time, C (carbon) of the nanodiamond 13 dissolved in the metal catalyst layer 20 precipitates as graphene 14, 24 at the interface between the sapphire substrate 10 and the metal catalyst layer 20 and at the interface between the nanodiamond 13 and the metal catalyst layer 20.

[0025] Next, as shown in FIG. 1(G), an etching process is performed to remove the metal catalyst layer 20 from the sapphire substrate 10. More specifically, the sapphire substrate 10 is taken out of the heat treatment device and immersed in a solution of ferric chloride and pure water in a ratio of 1:3 for 72 hours. This removes the metal catalyst layer 20, the graphene 24 formed on the surface of the metal catalyst layer 20, and the nanodiamonds 13 from the sapphire substrate 10. In this way, the surface of the graphene 14 formed over the entire surface of the sapphire substrate 10 is exposed.

[0026] [Verification of the effect of temperature in the first lamination process] Five types of samples were prepared by carrying out the first lamination step by changing the temperature at which Ni crystals were grown in five different temperatures in the first lamination step in the method for producing a metal catalyst layer in Example 1. The samples were produced by setting the temperatures at which Ni crystals were grown by molecular beam epitaxy (MBE) in the first lamination step to 350°C, 450°C, 550°C, 600°C, and 700°C. Hereinafter, the samples are simply referred to as the 350°C sample, the 450°C sample, the 550°C sample, the 600°C sample, and the 700°C sample.

[0027] The results of observing these five types of samples with a SEM (scanning electron microscope) are shown in Fig. 2(A) to Fig. 2(E). In the 350°C sample, Ni is laminated on the surface of the sapphire substrate 10 with a slightly rough surface. In the 450°C sample, Ni is laminated almost uniformly and flatly on the surface of the sapphire substrate 10. In the 550°C sample, Ni is laminated almost uniformly and flatly on the surface of the sapphire substrate 10, but there are some unevennesses in the thickness of the Ni. In the 600°C sample, Ni is laminated almost uniformly and flatly on the surface of the sapphire substrate 10, but the unevenness of the Ni thickness is more noticeable than in Example 4. In the 700°C sample, the unevenness of the Ni thickness is more noticeable than in Examples 4 and 5, and the Ni surface grows slightly granular.

[0028] The results of measuring these five types of samples by the in-plane X-ray diffraction measurement method are shown in Figure 3. In the in-plane method performed here, X-rays were incident almost parallel to the surface (c-plane) of the sapphire substrate 10 that had been subjected to the first lamination process, a light receiving unit that receives the diffracted X-rays was fixed, and the sapphire substrate 10 was rotated around the c-axis to measure the intensity of the diffracted X-rays.

[0029] As shown in Fig. 3, the sapphire substrate 10 in each sample has steep peaks at every 60°, i.e., 0°, 60°, 120°, and 180°. When the surface of the sapphire substrate 10 is viewed from the front, O (oxygen) and Al (aluminum) are arranged as shown in the schematic diagram of Fig. 4. The position of the peak of the sapphire substrate 10 in Fig. 3 corresponds to the diffracted X-rays from the a-plane (11-20) of the crystal of the sapphire substrate 10. The a-plane (11-20) is a plane perpendicular to the a-axis [11-20] shown in Fig. 4 of the crystal of the sapphire substrate 10.

[0030] In contrast, the samples at 350°C, 450°C, and 550°C have peaks at 30°, 90°, and 150° originating from the (01-1) plane of the first layer 11. In other words, it is found that the [01-1] direction of the first layer 11 in the samples at 350°C, 450°C, and 550°C is shifted by 30° with respect to the a-axis [11-20] of the sapphire substrate 10, as shown in Fig. 5(A), and is parallel to the m-axis [1-100] of the sapphire substrate 10.

[0031] In the 600°C and 700°C samples, similar to the sapphire substrate 10, steep peaks appear at every 60°, i.e., 0°, 60°, 120°, and 180°, originating from the (01-1) plane of the first layer 11. In other words, it is found that the [01-1] direction of the first layer 11 in the 600°C and 700°C samples is parallel to the a-axis [11-20] in the crystal of the sapphire substrate 10, as shown in FIG.

[0032] These results show that when the temperature for depositing Ni in the first lamination process is increased from 350°C to 550°C, the [01-1] direction of the first layer 11 becomes parallel to the m-axis [1-100] of the sapphire substrate 10, and when the temperature for depositing Ni in the first lamination process is increased from 600°C to 700°C, the [01-1] direction of the first layer 11 becomes parallel to the a-axis [11-20] direction of the sapphire substrate 10 crystal.

[0033] <Example 2, Comparative Example 1, Comparative Example 2> Next, samples of Example 2 and Comparative Example 1 were prepared by carrying out up to the first heat treatment step in the method for producing a metal catalyst layer of Example 1 on the 550°C sample and the 600°C sample. The sample of Example 2 was obtained by carrying out the second lamination step on the 600°C sample. The sample of Comparative Example 1 was obtained by carrying out the second lamination step on the 550°C sample. The sample of Comparative Example 2 was obtained by carrying out the second lamination step and the first heat treatment step without carrying out the first lamination step.

[0034] The surfaces of the second layer 12 (i.e., the surfaces of the metal catalyst layer 20) of the samples of Example 2, Comparative Example 1, and Comparative Example 2 were observed using a differential interference microscope after the first heat treatment step, and the results are shown in Figures 6(A) to (C). The dotted lines in the figures indicate the boundaries of crystal grains. As shown in Figure 6(A), it was found that the metal catalyst layer 20 of the sample of Comparative Example 1 was divided into multiple crystal grains.

[0035] In contrast, as shown in FIG. 6(B), the sample of Example 2 was found to be composed of a single crystal having the same size as the surface of the sapphire substrate 10, without forming boundaries between crystal grains in the metal catalyst layer 20. That is, the metal catalyst layer 20 of Example 2 was monocrystallized as a single crystal over the entire surface of the sapphire substrate 10, and was laminated on the c-plane of the sapphire substrate 10. Therefore, it was found that when the temperature for depositing Ni in the first lamination step was set to 600° C., the metal catalyst layer 20 was formed as a single crystal having a size roughly similar to that of the surface of the sapphire substrate 10. Although not shown, the same results were obtained when the sample in which the temperature for depositing Ni in the first lamination step was 700° C. was subjected to the first heat treatment step. Therefore, it was found that the temperature for depositing Ni in the first lamination step is preferably 600° C. to 700° C.

[0036] 6(C), it was found that the second layer 12 of the sample of Comparative Example 2 was divided into a plurality of crystal grains, similar to the sample of Comparative Example 1. It was found that the size of the crystal grains of the second layer 12 of the sample of Comparative Example 2 was rather larger than the crystal grains of the metal catalyst layer 20 of the sample of Comparative Example 1.

[0037] The results of measuring the samples of Example 2, Comparative Example 1, and Comparative Example 2 by the out-plane method of X-ray diffraction measurement are shown in Fig. 7. In the out-plane method performed here, X-rays were incident on the surfaces of the samples of Example 2, Comparative Example 1, and Comparative Example 2 at a predetermined angle, and a light receiving unit that receives the diffracted X-rays was oriented in a direction that intersects with the surface of the sample to measure the diffracted X-rays.

[0038] As shown in FIG. 7, each sample has a steep peak at approximately 45°. This is a peak derived from the (111) plane of the metal catalyst layer 20. In addition, peaks derived from the (200) and (220) planes of the metal catalyst layer 20 were not observed. Therefore, it was found that the

[0111] direction of the metal catalyst layer 20 is oriented in the c-plane axial direction of the sapphire substrate 10 in the samples of Example 2, Comparative Example 1, and Comparative Example 2. In addition, the graph shown at the bottom in FIG. 7 is for the sample of Example 2 before the second lamination step and the first heat treatment step, and even at this stage, a slight peak derived from the (111) plane appears. It can be seen that when the first heat treatment step is performed, a steep Ni(111) peak appears as in the spectrum of Example 2.

[0039] The results of measuring the samples of Example 2, Comparative Example 1, and Comparative Example 2 by the in-plane X-ray diffraction measurement method are shown in Fig. 8. As shown in Fig. 8(A) to (C), in the sapphire substrate 10 of each sample of Example 2, Comparative Example 1, and Comparative Example 2, steep peaks derived from the a-plane appear approximately every 60° at 30°, 90°, and 150° in the measurement profile of the sapphire substrate 10 on the lower side of the figure.

[0040] In contrast, as shown in FIG. 8(A), the sample of Comparative Example 1 has peaks at 60°, 120°, and 180° originating from the (01-1) plane of the metal catalyst layer 20, which are oriented 30° out of alignment with the peak of the sapphire substrate 10. As shown in FIG. 8(C), the sample of Comparative Example 2 has peaks at 0°, 60°, 120°, and 180° originating from the (01-1) plane of the second layer 12, which are oriented 30° out of alignment with the peak of the sapphire substrate 10. The average FWHM (full width at half maximum) of the peaks at 0°, 60°, 120°, and 180° of the sample of Comparative Example 2 was 3.7°. In contrast, the average FWHM of the peaks at 60°, 120°, and 180° of the sample of Comparative Example 1 was 8.3°. Therefore, it was found that the sample of Comparative Example 1 has a less favorable in-plane orientation of the crystal than the sample of Comparative Example 2.

[0041] On the other hand, as shown in FIG. 8(B), the sample of Example 2 has steep peaks derived from the (01-1) plane of the metal catalyst layer 20 at approximately every 60° of 30°, 90°, and 150°, similar to the sapphire substrate 10. This peak appears at the same position as the peak of the sapphire substrate 10, and it is found that the orientation is parallel to the a-axis [11-20] direction of the peak of the sapphire substrate 10. The average value of the FWHM of the peak derived from the (01-1) plane of the metal catalyst layer 20 at 30°, 90°, and 150° of the sample of Example 2 was 0.23°. From this, it was found that the crystal orientation of the sample of Example 2 is extremely good. In addition, the maximum value of the FWHM of the peak derived from the (01-1) plane of the metal catalyst layer 20 at 30°, 90°, and 150° of the sample of Example 2 was 0.25, and the minimum value was 0.18.

[0042] [Evaluation of graphene produced using a sample in which the Ni deposition temperature in the first lamination process was set to 650°C] Next, the carbon raw material lamination step and the second heat treatment step of the graphene production method of Example 1 were performed on the sample of Example 2, and the metal catalyst layer 20 was removed. The results of evaluation by Raman scattering spectroscopy are shown in Figures 9(A) and (B). Raman scattering spectroscopy is commonly used in the evaluation of graphene. Graphene can be evaluated based on three types of Raman peaks, the D peak, the G peak, and the G' peak. The D peak is a peak derived from structural defects in graphene and the edges of graphene. The G peak is a peak derived from the vibration of stretching within the plane of graphene, and the sp 2 The G' peak is a peak related to multi-step transitions including band-to-band transitions in graphene. When the G and G' peaks appear in the results of graphene evaluation using Raman scattering spectroscopy, it indicates that graphene has been produced. In addition, by comparing the magnitudes of the G and G' peaks, it is possible to obtain information regarding the number of stacked layers of the produced graphene.

[0043] The results of evaluation by Raman scattering spectroscopy shown in FIG. 9(B) are obtained at points A and B in an image of the surface of the graphene 14 of the sample of Example 2 shown in FIG. 9(A) observed using a differential interference microscope. The graphene 14 at point A is multi-layered. The graphene 14 at point B is also multi-layered, but the number of layers is smaller than that at point A. The results of evaluation by Raman scattering spectroscopy at point A were D / G of 0.01 and G' / G of 0.33. The results of evaluation by Raman scattering spectroscopy at point B were D / G of 0.08 and G' / G of 0.29. From these results, it was found that the graphene 14 generated on the surface of the sapphire substrate 10 had good crystallinity and was high-quality multi-layered graphene 14.

[0044] FIG. 10(A) is an image obtained by observing the surface of the graphene 14 of the sample of Example 2 at a position different from that of FIG. 9 using a microscope. FIG. 10(A) shows that the graphene near the top layer of the multi-layer graphene 14 is generated in an island shape at adjacent positions, and these island-like graphene 14 are bonded at the position of the dotted line. FIG. 10(B) is a diagram showing the magnitude of the value of D / G in each part within the rectangular frame in FIG. 10(A) by light and dark. In FIG. 10(B), a lighter color tone indicates a larger value of D / G, and a darker color tone indicates a smaller value of D / G. As shown in FIG. 10(B), the position of the dotted line in FIG. 10(A) corresponds to the position where adjacent island-like graphene are bonded, but the brightness is generally uniform even in this part. Therefore, it was found that the sample of Example 2 was bonded with good crystal quality in the region where the multiple island-shaped graphenes 14 formed at adjacent positions were bonded without generating a defective region indicated by a large D / G ratio. This can be explained by the fact that the graphene layer shown below exhibits high orientation with well-aligned crystal directions. In other words, when island-shaped graphenes 14 with aligned crystal directions are bonded, the bonds are smoothly connected and no defects are generated.

[0045] FIG. 11 shows the results of measuring the sample of Example 2 by the In-plane X-ray diffraction measurement method after the second heat treatment process is performed. The results in FIG. 11 are obtained by measuring the diffraction angles of the sapphire substrate 10, the metal catalyst layer 20, and the graphene 14 at 37.8°, 76.5°, and 65.8°. As shown in FIG. 11, the peaks derived from the a-plane of the sapphire substrate 10 appear steeply at 60° angles of 0°, 60°, and 120°. The peaks derived from the (01-1) plane of the metal catalyst layer 20 appear steeply at 60° angles of 0°, 60°, and 120°, similar to the sapphire substrate 10, and appear at the same positions as the peaks of the sapphire substrate 10.

[0046] In contrast, the (10) diffraction of graphene 14 in the sample of Example 2 appears steeply at every 60° of 30°, 90°, and 150°. The average value of the FWHM of the peaks of graphene 14 in the sample of Example 2 at 30°, 90°, and 150° was 0.18°. This indicates that the crystal orientation of graphene 14 produced in the sample of Example 2 is extremely good. In addition, the maximum value of the FWHM of the peaks of graphene 14 in the sample of Example 2 at 30°, 90°, and 150° was 0.22, and the minimum value was 0.14.

[0047] In order to explain the above orientation relationship, a schematic diagram showing the relationship of the atomic arrangement of each layer (sapphire substrate 10, metal catalyst layer 20, graphene 14) is shown in FIG. 12. It can be seen that the sharp direction of the six-membered ring of graphene 14 is the same as the [11-20] axial direction of the sapphire substrate 10 and the [01-1] direction of the metal catalyst layer 20. It can also be seen that the

[10] direction of graphene 14 is shifted by 30° from the a-axis direction of the sapphire substrate 10 and faces the m-axis [1-100] direction. Unlike the case of this embodiment, graphene formed on a Ni catalyst using a conventional method does not show such excellent orientation that a half-width is shown. In view of the above, it is considered that the excellent orientation of this embodiment is due to the fact that graphene 14 is precipitated and grown at the interface between the crystallized metal catalyst layer 20 and the sapphire substrate 10. That is, in an interface where the orientation (molecular arrangement) of the top and bottom (between the metal catalyst layer 20 and the sapphire substrate 10) is perfectly aligned, carbon atoms are forced to precipitate only at certain interface atomic positions, and the orientation relationship of the six-membered rings is also uniquely defined when the respective carbon atoms form the six-membered rings of graphene 14. As a result, it is considered that the orientation relationship of graphene 14 has a fixed relationship with the sapphire substrate 10 and the metal catalyst layer 20 as described above.

[0048] <Example 3> FIG. 13 shows the result of observing the surface of a sample obtained by carrying out the method for producing a metal catalyst layer and the method for producing graphene in Example 1 with an optical microscope. The outer shape of the sapphire substrate 10 used in the sample in Example 3 is a square shape of 10 mm×15 mm. As shown in FIG. 13, it was found that the sample in Example 3 has high-quality graphene 14 with few defects produced over the entire surface of the sapphire substrate 10 in the image. The graphene 14 is present over the entire surface in FIG. 13. The white island-like regions in contrast correspond to multi-layer graphene 14 with a large number of layers.

[0049] For example, in the sample of Comparative Example 1, the metal catalyst layer 20 is divided into a plurality of crystal grains. Therefore, when graphene 14 is produced on the surface of the sapphire substrate 10 using the sample of Comparative Example 1, carbon atoms diffuse at low temperatures in the areas where the boundaries of the crystal grains are located, and poor-quality graphene with many defects is formed during the temperature rise process. In addition, the orientation of the metal catalyst layer 20 in the sample of Comparative Example 1 is different for each grain. Therefore, the orientation of the island-like graphene 14 grown in each grain is not aligned, and defects occur in the island-like graphene 14 at the bonding portions.

[0050] In contrast, in the sample of Example 3, by carrying out the method for producing a metal catalyst layer of Example 1, the metal catalyst layer 20 is single-crystallized over the entire surface of the sapphire substrate 10, there are no grain boundaries, carbon does not diffuse into grain boundaries at low temperatures, and high-quality graphene grows. Therefore, the graphene 14 in the sample of Example 3 was produced without defects over the entire surface of the sapphire substrate 10. In addition, since the metal catalyst layer 20 is single-crystallized without grains, the orientation direction of the island-like graphene is uniform, and even when the island-like graphene are bonded to each other, no defects are generated at the bonded portions of adjacent graphene.

[0051] In addition to the above-mentioned high quality, when the metal catalyst layer 20 single-crystallized by the method of the present invention is used, wrinkles do not occur in the graphene produced when, for example, after the second heat treatment step for precipitation growth, the graphene is cooled at a temperature drop rate slower than about 30° C. / min. During cooling, the sapphire substrate 10, the metal catalyst layer 20, and the graphene 14 each shrink differently and non-uniformly due to differences in their respective thermal expansion coefficients. For this reason, in the conventional method, stress is applied to the graphene 14, causing wrinkles in the graphene 14.

[0052] However, in the sample of Example 3, graphene 14 is generated between the sapphire substrate 10 and the metal catalyst layer 20, and the graphene 14 does not have a bond to the sapphire substrate 10 and the metal catalyst layer 20, so that the upper and lower sapphire substrates 10 and the metal catalyst layer 20 can slide easily against each other. This makes it possible to match the different thermal contraction relationships, and with the slow cooling rate (about 30° C. / min) as described above, sufficient sliding occurs between the sapphire substrate 10 and the metal catalyst layer 20 over the entire substrate surface, completely relaxing the stress, and a state in which the graphene 14 does not wrinkle can be obtained.

[0053] At this time, the graphene 14 is generated between the sapphire substrate 10 and the metal catalyst layer 20, and the structure in which the graphene 14 is sandwiched between the sapphire substrate 10 and the metal catalyst layer 20 from above and below in a flat gap (i.e., a sandwich structure) is also effective in preventing wrinkles from being formed. In the conventional method in which the metal catalyst layer 20 has many grains, a larger gap is generated between the metal catalyst layer 20 and the sapphire substrate 10 at the grain boundary than the surrounding area. In addition, the metal catalyst layer may be displaced at the grain boundary, making the graphene 14 more likely to deform at this portion, and wrinkles may be formed in the graphene 14. Therefore, in this embodiment, the metal catalyst layer 20 is single crystallized and does not have grains, which is also considered to be one of the reasons why wrinkles do not occur. This wrinkle-free state of the graphene 14 is maintained even after the metal catalyst layer 20 is removed by etching, and wrinkle-free graphene 14 can be obtained over the entire surface of the sapphire substrate 10.

[0054] The diameter of a c-plane sapphire substrate that is currently available is approximately 6 inches. Therefore, according to the method for producing a metal catalyst layer of the present invention, it is possible to produce a metal catalyst layer 20 of one crystal having roughly the same size as the surface of a c-plane sapphire substrate having a diameter of approximately 6 inches. Therefore, when the method for producing a metal catalyst layer of the present invention and the method for producing graphene of the present invention are carried out using a c-plane sapphire substrate having a diameter of 6 inches, the surface area of ​​the metal catalyst layer 20 is approximately 180 cm. 2As described above, according to the present invention, it is possible to produce graphene 14 having no wrinkles with an area of ​​at least 0.01 cm, which was difficult to achieve with the conventional method, as shown in FIG. 2 In other words, the graphene 14 of the present invention can be produced without wrinkles over an area of ​​0.01 cm 2 From 180cm 2 In other words, the area is wrinkle-free.

[0055] Next, the effects of the above embodiment will be described.

[0056] The metal catalyst layer 20 of the present invention is formed by stacking and crystallizing on the c-plane of a sapphire substrate 10 having a corundum structure. The metal catalyst layer 20 has a face-centered cubic structure. The

[0111] direction of the metal catalyst layer 20 is the c-plane axial direction of the sapphire substrate 10. The [01-1] direction of the metal catalyst layer 20 is the [11-20] direction of the sapphire substrate 10. By using this metal catalyst layer 20, graphene 14 with good quality can be produced.

[0057] The method for producing a metal catalyst layer of the present invention includes a first lamination step of forming a first layer 11 of crystallized Ni on the surface of a sapphire substrate 10, a second lamination step of forming a second layer 12 of amorphous Ni on the surface of the first layer 11, and a first heat treatment step of performing a heat treatment to crystallize the second layer 12 after performing the first lamination step and the second lamination step. With this configuration, a metal catalyst layer 20 with good crystal quality can be produced.

[0058] The graphene production method of the present invention includes a carbon raw material lamination step of laminating nanodiamonds 13 on the surface of the metal catalyst layer 20 after performing the first heat treatment step in the above-mentioned metal catalyst layer production method, and a second heat treatment step of carrying out a heat treatment after performing the carbon raw material lamination step to precipitate graphene 14 between the sapphire substrate 10 and the metal catalyst layer 20. This configuration makes it easy to produce large-area graphene 14 with good crystallinity and no wrinkles at the interface between the sapphire substrate 10 and the metal catalyst layer 20.

[0059] The graphene 14 of the present invention is 0.01 cm 2 From 180cm 2 This structure is suitable for use in devices requiring a large area, such as integrated circuits.

[0060] The carbon raw material in the graphene production method of the present invention is nanodiamond 13. According to this configuration, graphene 14 can be continuously grown during heat treatment at a growth rate determined by the heat treatment temperature, and the number of layers of graphene 14 produced at the interface between the sapphire substrate 10 and the metal catalyst layer 20 can be easily controlled.

[0061] The present invention is not limited to the first and second embodiments described above with reference to the drawings, and the following embodiments are also included within the technical scope of the present invention. (1) In the first embodiment, etching is performed using a solution of ferric chloride and pure water. However, the present invention is not limited to this, and etching may be performed using nitric acid, sulfuric acid, hydrochloric acid, hydrogen peroxide, or a mixture of these acids. (2) In the first embodiment, a sapphire substrate having a c-plane ((0001) plane) as its surface is used, but the present invention is not limited to this, and gallium oxide or the like may also be used. (3) In the first embodiment, Ni is used for the first and second layers, but this is not limiting, and other metals including transition metals such as Cu, Co, Fe, Mn, W, Re, Os, Ir, Pt, Au, etc. may be used. Of course, alloys such as AuNi and NiCu may also be used. (4) In Example 1, nanodiamond is used as the carbon raw material, but this is not limiting, and other carbon raw materials such as amorphous carbon may also be used. (5) In the first embodiment, the MBE method is used, but other methods capable of forming a first layer of crystallized catalytic metal may be used. For example, a metal catalyst layer may be formed by a vapor phase growth method. In the first embodiment, the electron beam deposition method is used, but other methods capable of forming a second layer of amorphous catalytic metal on the surface of the first layer, such as a deposition method using resistance heating or a lamination method using plating, may be used. (6) In the first embodiment, the thickness of the first layer is 100 nm, but the thickness is not limited to this and may be 20 nm to 300 nm. (7) In the first embodiment, the thickness of the second layer is 300 nm, but the thickness is not limited to this and may be 200 nm to 700 nm. (8) As long as it does not exceed the scope of the invention, the two-dimensional material to be precipitated is not limited to graphene, and may be MoS2, MoTe2, WS, Mo 1-x W x It may be other two-dimensional materials such as S2, FeTiS2, TaSe2, BN, WTe2, etc. Of course, it may be a multilayer structure in which these two-dimensional materials are layered. [Explanation of symbols]

[0062] 10...Sapphire substrate (substrate) 11…1st layer 12…Second layer 13...Nano diamond (carbon material) 14. Graphene 20…Metal catalyst layer

Claims

1. a first lamination step for forming a first layer of a crystallized catalytic metal on a c-plane of a substrate having a corundum structure; a second lamination step of forming a second layer of the catalytic metal of the same type as the first layer in an amorphous state on a surface of the first layer; a first heat treatment step of performing a heat treatment to crystallize the second layer after the first lamination step and the second lamination step to generate a metal catalyst layer having the first layer and the second layer; Equipped with The metal catalyst layer has a face-centered cubic structure, the [111] direction of the metal catalyst layer is the c-plane axial direction of the substrate, The method for producing graphene, wherein the [01-1] direction of the metal catalyst layer is the [11-20] direction of the substrate.

2. After carrying out the first heat treatment step, a carbon raw material lamination step of laminating a carbon raw material on a surface of the metal catalyst layer; a second heat treatment step of carrying out a heat treatment after carrying out the carbon raw material lamination step to precipitate graphene between the substrate and the metal catalyst layer; 2. The method of producing graphene according to claim 1 , comprising:

3. A method for producing graphene as described in claim 2, wherein the carbon raw material is nanodiamond.

4. The method of claim 1, which produces wrinkle-free graphene in an area of ​​0.01 cm 2 to 180 cm 2 .

Citation Information

Patent Citations

  • Production of silver cobalt superlattice film

    JP1992000382A

  • Method of manufacturing semiconductor apparatus, semiconductor apparatus, and wiring structure

    JP2009164432A

  • Transfer film and method of producing the same, and method of producing transparent conductive laminate

    JP2015072767A

  • Method for manufacturing graphene substrate, and graphene substrate

    WO2012086387A1

  • Method for producing graphene, and graphene

    WO2013038623A1

Cited By

  • Production method of graphene

    JP2024011551A