Fine particle composite oxide yellow pigment and its manufacturing method

A two-step precipitation and controlled firing process produces a fine particle composite oxide yellow pigment with Fe, Al, and Ti, addressing the limitations of existing pigments by achieving excellent heat resistance, transparency, and durability for diverse applications.

JP7587076B1Active Publication Date: 2024-11-19DAINICHISEIKA COLOR & CHEMICALS MFG CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024053254
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-03-28
Publication Date
2024-11-19
Estimated Expiration
2044-03-28

AI Technical Summary

Technical Problem

Existing yellow pigments face challenges in achieving fine particle size, excellent heat resistance, transparency, and durability while avoiding harmful metals, limiting their application in inkjet inks, metallic and clear paints, and transparent coatings.

Method used

A method to produce a pseudobrookite-type fine particle composite oxide yellow pigment composed of Fe, Al, and Ti, involving a two-step precipitation process followed by firing at controlled temperatures to achieve an average primary particle diameter of 80 nm or less, with specific metal oxide proportions.

Benefits of technology

The method results in a yellow pigment with excellent heat resistance, transparency, and durability, suitable for applications requiring fine particle size and transparency, such as engineering plastics and ceramic coloring, while avoiding harmful metals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587076000003
    Figure 0007587076000003
  • Figure 0007587076000001
    Figure 0007587076000001
  • Figure 0007587076000002
    Figure 0007587076000002
Patent Text Reader

Abstract

The present invention provides a method for producing a fine particle composite oxide yellow pigment having excellent heat resistance, transparency, and durability. [Solution] A method for producing a pseudobrookite-type fine particle composite oxide yellow pigment composed of Fe, Al, and Ti, comprising the steps of: generating an Al precipitate in water using a metal salt of Al and an alkali to obtain a first reaction liquid; generating a pigment precursor in water using the first reaction liquid, metal salts of Fe and Ti, and an alkali to obtain a second reaction liquid; and filtering, washing with water, and drying the pigment precursor, and then calcining it at a temperature of 600°C or higher and 900°C or lower to obtain the fine particle composite oxide yellow pigment, wherein the fine particle composite oxide yellow pigment has an average primary particle diameter of 80 nm or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a fine particle composite oxide yellow pigment having excellent transparency, heat resistance and durability, and a method for producing the same. [Background technology]

[0002] Pigments are used in a wide range of situations as colorants for paints, inks, building materials, etc. Therefore, depending on the situation, not only color but also heat resistance, weather resistance, chemical resistance, etc. may be required. Inorganic yellow pigments generally have excellent heat resistance and weather resistance, but in recent years, there has been a strong movement to avoid pigments containing Cd, Cr, or Pb due to environmental concerns, and their use is being restricted. In the past, there were yellow pigments such as cadmium yellow and yellow lead, but they are now rarely used. Titanium yellow is a composite oxide type, but it contains metals such as Cr, Sb, or Ni, and pigments that do not contain these metals are required. On the other hand, organic yellow pigments exhibit vivid hues, but many of them have low heat resistance and poor weather resistance, and their use is limited depending on the application. In addition, goethite (α-FeOOH) is a yellow pigment that does not contain harmful metals and is in use, but this pigment has low heat resistance, and when it exceeds 200°C, it becomes hematite (α-Fe2O3) through dehydration and changes color to brown. For this reason, it may not be usable depending on the application. This pigment is also available in fine particle form, but since it has the same chemical structure, it also has low heat resistance. In this situation, Fe2TiO5 (pseudobrookite) pigments have been proposed as heat-resistant pigments that do not contain harmful metals. However, even the finest of these pigments are submicron in size, and no nano-sized pigments with excellent transparency have been found.

[0003] Various attempts have been made to develop yellow pigments of composite oxides of Fe and Ti. For example, Patent Document 1 discloses a yellow pigment made of a mixture of pseudobrookite type in which Al is dissolved and rutile type titanium oxide. This pigment is obtained by adding iron salt and aluminum salt to hydrous titanium oxide, neutralizing with an alkali, and then calcining the mixture, and the particle size of this pigment is in the submicron range. Patent Document 2 discloses a pigment having a pseudobrookite structure that contains various metals other than Fe and Ti. However, the manufacturing method of this pigment involves mixing submicron raw material powders and firing them at high temperatures of 1000° C. or more, and so it is assumed that the resulting pigment is a submicron pigment, not a fine-particle pigment with excellent transparency. Patent Document 3 discloses a pigment consisting of Fe, Ti, and Al, or a pigment having other metals introduced therein. This method of producing a pigment involves mechanochemically treating raw material powder to produce a pigment with excellent color development and coloring power, but the pigment obtained here is a submicron pigment, and no pigment having fine particles smaller than submicron has been obtained. In Non-Patent Document 1, fine particles are synthesized using a gas phase method. In this case, TiCl4-FeCl3 is used, and fine powder with an average particle size of 0.03 μm to 0.1 μm is obtained in the TiO2-Fe2O3 system by a gas phase reaction at 800°C to 1250°C. However, these fine particles are composed of TiO2, Fe2TiO5, and αFe2O3, and the pigment has a strong reddish color due to the inclusion of Fe2O3, so it cannot be used as a yellow pigment. As described above, in the prior art, a fine particle yellow pigment having excellent heat resistance, transparency, and durability has not been obtained. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 8-73224 [Patent Document 2] Japanese Patent Application Publication No. 9-221323 [Patent Document 3] International Publication No. 2001 / 070632 [Non-patent literature]

[0005] [Non-Patent Document 1] Yoko Suyama, Akio Kato, Color Materials, 53, 1035-1043 (1980) Summary of the Invention [Problem to be solved by the invention]

[0006] Due to the growing concern about the environment, it is desirable to develop pigments that do not contain harmful metals, and Fe2TiO5-based pseudobrookite pigments have been proposed as inorganic yellow pigments. These pigments have excellent heat resistance and durability, and therefore have been applied to coloring paints or plastics. On the other hand, when applying them to inkjet printers in an attempt to expand the range of applications by taking advantage of the good points of not containing harmful metals, heat resistance, and durability that are not found in conventional pigments, it is difficult to stabilize the ink due to their large specific gravity or large particle size. When applying them to paints for metallic paints or clear paints, there are problems such as high hiding power and poor transparency, which makes it difficult to obtain a metallic feel. In addition, when coloring glass or films, when a transparent coloring is desired, there are problems such as high hiding power and poor transparency, even with submicron particles that are considered to have a small particle size. As a yellow pigment, FeTi pseudobrookite pigments have excellent heat resistance and durability, but when trying to expand the range of applications, problems such as those mentioned above arise. Conventional techniques have not been able to obtain fine particle pigments smaller than submicron, and even if attempts have been made, they have only resulted in a strong reddish color, so there is a strong demand for fine particle yellow pigments with good color development that solve the above problems as a yellow pigment.

[0007] An object of the present invention is to provide a fine particle composite oxide yellow pigment having excellent heat resistance, transparency and durability, and a method for producing the same. [Means for solving the problem]

[0008] According to the present invention, there are provided a fine particle composite oxide yellow pigment and a method for producing the same, which are shown below. [1] A method for producing a pseudobrookite-type yellow composite oxide pigment composed of Fe, Al, and Ti, comprising the steps of: A step of forming an aluminum precipitate in water using an aluminum metal salt and an alkali to obtain a first reaction solution; a step of producing a pigment precursor in water using the first reaction liquid, metal salts of Fe and Ti, and an alkali to obtain a second reaction liquid; and a step of filtering the pigment precursor, washing with water, drying, and then calcining the pigment precursor at a temperature of 600° C. or more and 900° C. or less to obtain a fine particle composite oxide yellow pigment. The average primary particle diameter of the fine particle composite oxide yellow pigment is 80 nm or less. A method for producing a fine-particle composite oxide yellow pigment. [2] A method for producing a fine particle composite oxide yellow pigment according to claim 1, wherein, when the fine particle composite oxide yellow pigment is produced by converting and dividing each of the constituent metals into the respective oxide constituent units, which are Fe2O3, Al2O3, and TiO2, the proportion of Fe2O3 is 30% by mass or more and 40% by mass or less, the proportion of Al2O3 is 20% by mass or more and 30% by mass or less, and the proportion of TiO2 is 35% by mass or more and 45% by mass or less. [3] A pseudobrookite-type fine composite oxide yellow pigment composed of Fe, Al, and Ti, When each constituent metal is converted into its respective oxide constituent unit, divided, and these are designated as Fe2O3, Al2O3, and TiO2, the proportion of Fe2O3 is 30% by mass or more and 40% by mass or less, the proportion of Al2O3 is 20% by mass or more and 30% by mass or less, and the proportion of TiO2 is 35% by mass or more and 45% by mass or less, The average primary particle diameter of the fine particle composite oxide yellow pigment is 80 nm or less. Fine particle composite oxide yellow pigment. Effect of the Invention

[0009] According to one aspect of the present invention, it is possible to provide a fine particle composite oxide yellow pigment having excellent heat resistance, transparency, and durability, and a method for producing the same. [Brief description of the drawings]

[0010] [Figure 1] Photographs showing TEM images of the yellow pigments of Example 2 and Comparative Example 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] <Method of manufacturing fine particle composite oxide yellow pigment> Hereinafter, an embodiment of the present invention will be described, but the present invention is not limited to the following embodiment. The method for producing a fine particle yellow composite oxide pigment according to this embodiment (hereinafter, also referred to as the production method according to this embodiment) is a method for producing a fine particle yellow composite oxide pigment of pseudobrookite type composed of Fe, Al, and Ti. The manufacturing method according to this embodiment includes a step of forming an Al precipitate in water using an Al metal salt and an alkali to obtain a first reaction liquid (hereinafter also referred to as the first step), a step of forming a pigment precursor in water using the first reaction liquid, Fe and Ti metal salts and an alkali to obtain a second reaction liquid (hereinafter also referred to as the second step), and a step of filtering, washing with water, drying and then calcining the pigment precursor at a temperature of 600° C. to 900° C. to obtain a fine particle composite oxide yellow pigment (hereinafter also referred to as the third step). The average primary particle diameter of the obtained fine particle composite oxide yellow pigment is required to be 80 nm or less.

[0012] The reason why the production method according to the present embodiment can provide a fine particle composite oxide yellow pigment having excellent heat resistance, transparency, and durability is not entirely clear, but the present inventors speculate as follows. That is, since the pseudobrookite of Fe2TiO5 is a little reddish, in this embodiment, it is presumed that the solid solution of Al in this will have a yellowish hue and be a good yellow pigment. In addition, in this embodiment, since the solid solution of Al does not cause any problems in physical properties such as heat resistance, a fine particle pigment is produced with a three-component system of Fe, Al, and Ti. In the synthesis of pigments, there is a method in which raw material powders are mixed and fired to produce a pigment, which is generally called a dry method, but even if fine particle materials are used as raw materials, grain growth occurs during firing, making it unsuitable for producing fine particles with excellent transparency. For this reason, in this embodiment, the pigment is produced by a method called a wet method in which an alkali is applied to a metal salt in water to produce a precipitate, which is then filtered, washed with water, dried, and then fired.

[0013] In this embodiment, the synthesis method is a wet method in which an alkali is applied to a metal salt to form a precipitate, and the pigment is synthesized. However, it has been found that if an alkali is applied to a mixed solution of three metal salt components to form a precipitate, only a reddish pigment is obtained under these conditions, and the desired yellow fine particle pigment with good color development cannot be obtained. Furthermore, the same tendency was observed when an Fe precipitate was prepared after an Al and Ti precipitate was prepared, and the same tendency was observed when a Ti precipitate was prepared after an Al and Fe precipitate was prepared. As a result of intensive research by the present inventors, it was found that it is necessary to prepare a precipitate in which Fe and Ti are in a highly reactive state and mixed in the nano region, and that the state in which Al is dissolved in Fe and Ti as they crystallize is the condition for a pigment with good yellow color development despite being fine particles, and therefore it is necessary to prepare the Al precipitate and the Fe and Ti precipitates separately. In addition, with this type of pigment, there is a tendency for pigments with a strong reddish hue to be obtained, but fine particle pigments with good yellow color development can only be obtained under specific synthesis conditions, and the inventors speculate that this may be the reason why fine particle yellow pigments have not been proposed until now. From the above, the present inventors presume that the fine particle composite oxide yellow pigment obtained by the production method according to this embodiment has excellent heat resistance, transparency, and durability.

[0014] (First step) In the first step, a metal salt of Al and an alkali are used to form an Al precipitate in water to obtain a first reaction solution. As the metal salt of Al used in this embodiment, sulfate, chloride, and nitrate can be used. Among these, at least one of chloride and sulfate is preferable from the viewpoint of availability. The alkali used in this embodiment may be caustic soda or soda ash. Among these, soda ash is preferred from the viewpoint of dispersibility.

[0015] As an example of the first step, a solution of aluminum chloride and a solution of soda ash are added to water while adjusting the pH to 4, forming a precipitate of Al to obtain a first reaction liquid. The temperature at this time is preferably 25°C or higher and 50°C or lower, and more preferably 35°C or higher and 45°C or lower.

[0016] (Second process) In the second step, a pigment precursor is produced in water using the first reaction liquid obtained in the first step, metal salts of Fe and Ti, and an alkali to obtain a second reaction liquid. The Fe and Ti metal salts used in this embodiment are the same as the Al metal salt described above. The alkali used in this embodiment is also the same as the alkali described above.

[0017] As an example of the second step, first, while adding an alkali to the first reaction liquid obtained in the first step, the temperature is increased and the pH is adjusted. The temperature at this time is preferably 45° C. to 75° C., and more preferably 55° C. to 65° C. In addition, the pH after adjustment is preferably 5 to 7, and more preferably 5.5 to 6.5. Next, a solution of titanium tetrachloride and iron sulfate and a solution of soda ash are added to this reaction liquid while maintaining the pH at 6, forming a precipitate of Fe and Ti and producing a pigment precursor, thereby obtaining a second reaction liquid.

[0018] One of the features of the present invention is that the precipitation is performed in two stages, the first and second steps described above. Even if the precipitation is performed in two stages, if a titanium solution is added to an aluminum solution to form a mixed solution, and after the first stage of precipitation, an iron precipitate is formed in the second stage, the pigment will have a reddish hue, and a fine particle pigment with good yellow coloring will not be obtained. However, if the reaction is caused by proceeding with the firing, such as by increasing the firing temperature, the hue will become yellow, but the particle size will become large. When producing a pigment of a submicron size or larger, it is possible to produce the pigment without the two-stage precipitation, but it is difficult to produce a pigment with a transparent feel. Patent Document 1 also describes a method of producing a pigment by precipitation of some components with an alkali and firing the precipitate, but this is a method of producing a pigment by precipitation of other components using a hydrolyzed product of Ti, and the hydrolyzed product of Ti has a certain size. Therefore, even if the pigment is fired and a good coloring is obtained, the particles will be submicron particles at best. In order to obtain fine particles and a pigment with good yellow color development, it is not sufficient to simply utilize a precipitation reaction, and this is also the significance of the present invention.

[0019] (Third step) In the third step, the pigment precursor obtained in the second step is filtered, washed with water, dried, and then calcined at a temperature of 600° C. to 900° C. to obtain a fine particle composite oxide yellow pigment. The firing may be performed in air, which is an oxidizing atmosphere, and no special atmospheric adjustment is required. The firing temperature may be any temperature at which pseudobrookite crystals can be obtained, and in this embodiment, the firing temperature is 600° C. or higher and 900° C. or lower. In this embodiment, since the mixed state of each metal component is uniform in the nano region, pseudobrookite type crystals are obtained at a firing temperature lower than 800°C to 1200°C, which is the temperature usually applied to submicron. In this embodiment, from the viewpoint of hue, transparency, etc., the firing temperature is preferably 700°C or higher and 850°C or lower. This firing temperature is 100°C or higher lower than the firing temperature of conventional pigments of this type, which also suggests that the uniformity of each metal in the precipitate is high.

[0020] The average primary particle diameter of the fine particle composite oxide yellow pigment obtained by the manufacturing method according to the present embodiment must be 80 nm or less, preferably 60 nm or less, and more preferably 50 nm or less. If the primary particle diameter exceeds 80 nm, satisfactory transparency cannot be obtained. There is no particular lower limit, but if it is less than 10 nm, the pigment has a high tendency to aggregate, and a large amount of dispersion energy is required when dispersing it in a resin composition or a solvent, which is not practical.

[0021] In the fine particle composite oxide yellow pigment obtained by the production method according to the present embodiment, when each constituent metal is converted and divided into the constituent units of each oxide, and these are expressed as Fe2O3, Al2O3, and TiO2, it is preferable that the proportion of Fe2O3 is 30% by mass or more and 40% by mass or less, the proportion of Al2O3 is 20% by mass or more and 30% by mass or less, and the proportion of TiO2 is 35% by mass or more and 45% by mass or less. If the proportions of Fe2O3, Al2O3, and TiO2 are each within the above ranges, a yellow color with good color development tends to be obtained.

[0022] <Fine particle composite oxide yellow pigment> The fine particle composite oxide yellow pigment according to this embodiment is a pseudobrookite-type fine particle composite oxide yellow pigment composed of Fe, Al, and Ti. When each metal component of this fine particle composite oxide yellow pigment is converted and divided into its oxide constituent units, Fe2O3, Al2O3, and TiO2, the ratio of Fe2O3 is 30% to 40% by mass, the ratio of Al2O3 is 20% to 30% by mass, and the ratio of TiO2 is 35% to 45% by mass. The average primary particle diameter of this fine particle composite oxide yellow pigment must be 80 nm or less.

[0023] The reasons why the fine particle composite oxide yellow pigment according to this embodiment is a yellow pigment with a preferable hue and has excellent heat resistance, transparency, and durability are not necessarily clear, but the present inventors speculate as follows. That is, the oxide composition in this embodiment is basically (Fe,Al)2TiO5 in which Al is dissolved in the pseudobrookite type of Fe2TiO5. If there is a lot of Fe and a little Al, the hue is reddish and the transparency is reduced. If there is little Fe and a lot of Al, the hue is yellowish and the transparency is increased, but the coloring power as the color strength is reduced. Also, a composition with a lot of titanium oxide tends to have a low transparency. In particular, when hematite (Fe2O3) is formed, the hue becomes reddish and a good yellow color cannot be obtained. In this embodiment, it has been found that when the proportions of Fe2O3, Al2O3, and TiO2 are each within the above range, the hue and transparency are excellent. The reasons for the excellent heat resistance and durability are as described above. From the above, the present inventors presume that the fine particle composite oxide yellow pigment according to this embodiment is a yellow pigment with a preferable hue, and is excellent in heat resistance, transparency, and durability.

[0024] The fine particle composite oxide yellow pigment according to this embodiment is influenced by the metal composition, but is also greatly influenced by the pigment synthesis conditions, and appropriate adjustment of the composition, synthesis conditions, and firing temperature is an important factor in obtaining the desired pigment. This type of pigment tends to produce a reddish pigment if the conditions are not met. If a wet method is used as a pigment synthesis method, a pigment with small particles can be produced. However, unless a two-stage synthesis is performed as in the manufacturing method according to the present embodiment described above, the resulting pigment will inevitably be reddish. If the firing temperature is increased in an attempt to make the pigment yellowish, the hue will be adjusted, but the pigment will be inferior in terms of transparency.

[0025] The composite oxide yellow pigment fine particle according to this embodiment is a yellow fine particle having heat resistance that allows it to be used for coloring engineering plastics (heat resistance of 300°C or higher) or ceramics. This yellow pigment also has the characteristic of being usable in applications requiring transparency, such as metallic or color clear paints, and is a durable pigment with long-term weather resistance. At present, there are almost no such yellow pigments, both organic and inorganic. Another advantage is that this yellow pigment is a pigment made of Fe, Ti, and Al, and does not contain harmful metals. EXAMPLES

[0026] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the examples and comparative examples, "parts" and "%" are by weight unless otherwise specified.

[0027] As for the metal salt, the following materials were used. (iron salts) A1: Ferrous sulfate heptahydrate crystals A2: Ferric chloride hexahydrate crystals (aluminum salts) B1: Aluminum chloride hexahydrate crystals B2: Aluminum sulfate 16-hydrate crystals (Titanium salts) C1: Titanium tetrachloride aqueous solution (containing 16.2% Ti) C2: Titanyl sulfate crystal (33% TiO2 content)

[0028] <Example 1> Dissolve 94.7g of aluminum chloride in 200mL of water to prepare a metal salt aqueous solution for the first stage synthesis. Dissolve 230g of soda ash in 1000mL of water to prepare an alkaline aqueous solution. In a container separate from the aluminum chloride, dissolve 139.3g of iron sulfate and 148.0g of titanium tetrachloride solution in 400mL of water in advance. Add 1500mL of water to a beaker and heat to 40°C while stirring. Add the aluminum chloride aqueous solution and soda ash solution dropwise to form a precipitate at pH 4 (first stage synthesis). After the aluminum solution has been added dropwise, increase the temperature to 60°C. At the same time, add soda ash dropwise to raise the pH to 6. Once the temperature reaches 60°C, a pre-dissolved mixed solution of iron sulfate and titanium tetrachloride and soda ash are added dropwise, and a precipitate is formed at pH 6 (second stage synthesis). Once the metal salt solution has finished being added dropwise, the pH is raised to 6.5 and the temperature is raised to 70°C, after which the mixture is aged for one hour. After aging, the slurry is decanted to wash away the remaining salt, and then filtered and dried in a dryer. The dried pigment precursor is placed in a crucible and fired in an electric furnace at 800°C for one hour. After firing, the mixture is pulverized in a grinder to obtain a yellow pigment. <Examples 2 to 7> A yellow pigment was produced in the same manner as in Example 1, except that the types of raw materials shown in Table 1 were mixed so as to obtain the metal composition ratios shown in Table 1.

[0029] <Comparative Example 1> A yellow pigment was prepared in the same manner as in Example 2, except that a metal salt of Ti was dissolved in a metal salt of Al to perform the first synthesis step, and then Fe was precipitated in the second synthesis step. <Comparative Example 2> The first step of the synthesis was carried out by dissolving the metal salt of Fe in the metal salt of Al, and then the precipitation of Ti was carried out in the second step. 6 A yellow pigment was prepared in the same manner as above. <Comparative Example 3> The metal salts of Al, Fe, and Ti were dissolved in the same solution, and the synthesis was carried out in the first step only. 7 A yellow pigment was prepared in the same manner as above. <Comparative Example 4> A yellow pigment was produced in the same manner as in Example 2, except that the synthesized pigment precursor was calcined at 950°C. <Comparative Example 5> A commercially available pseudobrookite type yellow pigment with similar Fe, Al, and Ti metal content was used.

[0030] The resulting pigments were evaluated in the following manner. <Average primary particle size and TEM image> Generally, a solution in which a pigment is dispersed in a solvent such as water is measured using a dynamic scattering type particle size distribution measuring device, but the pigment of the present invention is a fine particle, and it is difficult to disperse it down to primary particles. Therefore, here, we decided to calculate from a transmission electron microscope image (TEM image). In detail, the prepared pigment powder was photographed with a transmission electron microscope, and the average primary particle size was calculated from 50 randomly selected particles using image analysis software (Mac-View, manufactured by Mountec Co., Ltd.). The obtained results are shown in Table 1. TEM images of the yellow pigments of Example 2 and Comparative Example 5 are shown in FIG. <Color and transparency> The pigment for evaluation was made into paint and its hue and transparency were evaluated. Melamine alkyd baked paint was prepared, and the pigment content was 20 PHR (ratio of additives to 100 parts by mass of resin). Zirconia beads of 1 mm diameter were used as the dispersion medium, and the dispersion was performed for 2 hours with a paint shaker, and the color was spread on art paper with a black band and baked at a temperature of 120°C to prepare an evaluation sample, whose hue and transparency were visually evaluated. The evaluation was performed according to the following criteria. The obtained results are shown in Table 1. The hue appears different depending on the pigment content and film thickness. In addition, transparency is evaluated as being more transparent when the black of the base is clearly visible in the black band of the art paper and there is no whitishness, but since it is difficult to judge numerically, the judgment was made by visual inspection. (hue) ◎: Excellent yellow coloring. ◯: Yellowish, but with a slight reddish hue. △: Reddish yellow hue. ×: Completely reddish hue. (transparency) ◎: Excellent transparency. ◯: Transparency is present but slightly inferior. △: slightly less transparent. ×: Hiding properties are observed and transparency is poor. <Hue measurement> Similar evaluation samples for hue and transparency were prepared and were measured using a spectrophotometer (CM-3600A, manufactured by Konica Minolta, Inc.). The colorimetry was performed on the pigments obtained in Example 2, Comparative Example 1, Comparative Example 2, and Comparative Example 4. The results are shown in Table 2.

[0031] [Table 1]

[0032] [Table 2]

[0033] From the results shown in Table 1, it was found that the yellow pigments according to the present invention (Examples 1 to 7) had good evaluation results in terms of hue and transparency. Furthermore, from the results shown in Table 2, it was found that the yellow pigment according to the present invention (Example 2) had a low lightness L* in the black belt area and a sense of transparency, and also had a low chroma a* in the white belt area and was a yellow with a weak reddish tinge. Furthermore, the yellow pigments according to the present invention (Examples 1 to 7) are fine particle composite oxides, and therefore have excellent heat resistance and durability. From these, it was confirmed that the yellow pigments according to the present invention (Examples 1 to 7) are excellent in heat resistance, transparency, and durability.

Claims

1. A method for producing a pseudobrookite-type yellow composite oxide pigment comprising Fe, Al, and Ti, comprising the steps of: A step of forming an aluminum precipitate in water using an aluminum metal salt and an alkali to obtain a first reaction solution; a step of producing a pigment precursor in water using the first reaction liquid, metal salts of Fe and Ti, and an alkali to obtain a second reaction liquid; and a step of filtering, washing with water, drying, and then calcining the pigment precursor at a temperature of 600° C. or higher and 900° C. or lower to obtain a fine particle composite oxide yellow pigment. The fine particle composite oxide yellow pigment has an average primary particle diameter of 80 nm or less, When the fine particle composite oxide yellow pigment is prepared by converting each constituent metal into the constituent unit of each oxide, dividing them into Fe 2 O 3 , Al 2 O 3 , and TiO 2 , the proportion of Fe 2 O 3 is 30 mass% or more and 40 mass% or less, the proportion of Al 2 O 3 is 20 mass% or more and 30 mass% or less, and the proportion of TiO 2 is 35 mass% or more and 45 mass% or less. A method for producing a fine-particle composite oxide yellow pigment.

2. A pseudobrookite-type fine particle composite oxide yellow pigment composed of Fe, Al, and Ti, Each constituent metal is converted into its respective oxide unit, divided, and these are separated into Fe 2 O 3 , Al 2 O 3 , and TiO 2 When this is done, Fe 2 O 3 The proportion of Al is 30 mass% or more and 40 mass% or less, 2 O 3 The ratio of TiO is 20 mass% or more and 30 mass% or less. 2 The ratio of is 35% by mass or more and 45% by mass or less, The average primary particle diameter of the fine particle composite oxide yellow pigment is 80 nm or less. Fine particle composite oxide yellow pigment.

Citation Information

Patent Citations

  • Pigment and its production

    JP1996073224A

  • Heat resistant inorganic powdery pigment and its production

    JP1997221323A

  • Yellow coating material and yellow rubber / resin composition

    JP2001040288A

  • Scaly particle and method for producing the same

    JP2012121739A

  • Iron-titanium based composite oxide brown pigment

    JP2016121038A