Impedance and phase angle difference measuring probe and method for controlling slag composition in converter using same
The probe with adjustable electrode terminals for slag composition control in steelmaking converters addresses measurement inaccuracies by separating resistance components, enabling precise slag composition control and reducing costs.
Patent Information
- Application Number
- JP2021005617
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-18
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2041-01-18
AI Technical Summary
Existing methods for estimating slag composition in steelmaking converters, such as those described in Patent Documents 1 and 2, suffer from large measurement errors and inaccuracies due to fluctuations in exhaust gas information and variations in operational conditions, making it difficult to accurately control the amount of CaO source added, which affects steelmaking costs and slag composition.
A probe with at least three electrode terminals is used to measure impedance and phase angle difference, allowing for the separation of solution resistance and charge transfer resistance by varying the distance between electrodes, enabling precise estimation of slag basicity and iron oxide content through impedance information and thermodynamic modeling.
This approach allows for accurate control of slag composition by separating solution resistance and charge transfer resistance, improving estimation accuracy and reducing steelmaking costs by optimizing CaO source addition.
Smart Images

Figure 0007587134000004 
Figure 0007587134000005 
Figure 0007587134000006
Abstract
Description
[Technical field]
[0001] The present application relates to an impedance and phase angle difference measuring probe and a method for controlling slag composition in a converter using the same. [Background technology]
[0002] In the steel refining process, it is extremely important to control the concentrations of P, S, and C in molten iron according to the required properties of the steel. In particular, P has a significant effect on the cracking sensitivity of steel, and in response to the recent increase in demand for offshore structures that require low-temperature toughness, there is a demand to stably reduce the P concentration in steel to 0.010 mass% or less.
[0003] Generally, the amount of P in steel is 0.1-0.2 mass% in the molten iron tapped from the blast furnace, and this P is removed by adding a CaO source such as quicklime at the molten iron stage, which is thermodynamically favorable for the progress of the dephosphorization reaction, to promote the slag-metal reaction shown in formula (1). Here, in formula (1), [] indicates the components in the steel, and () indicates the components in the slag. The P in the steel is also taken up in the slag as P2O5. 2[P]+3(CaO)+5(FeO)→(3CaO P2O5)+5Fe...(1)
[0004] The reaction vessels in which the reaction in formula (1) proceeds include torpedo cars, ladles, and converters, and these are selected according to the integrated production capacity of the steelmaking process. In general, converters are selected because they have a large reaction vessel volume, allow for strong stirring, and can proceed with the dephosphorization reaction more kinetically in a short period of time. In such cases, the production capacity is determined by the converter's blowing time, which is based on the premise of short-time treatment, so it is important to efficiently proceed with the refining reaction in the converter.
[0005] Here, in order to thermodynamically efficiently proceed with the dephosphorization reaction, it is possible, based on equation (1), to increase the CaO and FeO concentrations in the slag and to decrease the P2O5 concentration in the slag.
[0006] As a method for increasing the CaO concentration, for example, adding a large amount of quicklime from the converter furnace is considered, but the addition of excessive quicklime increases production costs, inhibits slag foaming at the end of the dephosphorization blowing, and leads to poor intermediate slag removal in the MURC (Multi-Refining Converter) process, which causes the rephosphorization reaction to proceed during the decarburization blowing. In addition, a large amount of steelmaking slag is generated, and the slag treatment is also costly. Alternatively, powdered quicklime with a small particle size is sprayed onto the hot point or into the steel, but the supply rate of the auxiliary material is slower than that of the lump-sum addition, so the CaO concentration in the slag cannot be sufficiently increased by short-term treatment. In addition, the production of powdered quicklime increases the steelmaking cost.
[0007] From the above, in order to accelerate the dephosphorization reaction, it is important to melt the CaO source in the slag as early as possible without excessive supply. In the actual process, the blower estimates the CaO / SiO2 (basicity) of the slag and adjusts the amount of CaO source added.
[0008] More specifically, the amount of quicklime added is adjusted based on various information so that the CaO / SiO2 (basicity) of the slag at the end of blowing is in a range where the solid phase does not crystallize excessively from the complete liquid phase composition (for example, basicity = 1.3) depending on the target P concentration of the steel. Here, the various information refers to the CaO / SiO2 (basicity) of the slag calculated from the auxiliary raw materials such as quicklime added to the converter, the amount and composition of the reactants generated by the refining reaction, the timing of the slopping phenomenon where the slag flows out of the throat, and the difference between the target P and the actual P in the previous charge (one converter blowing operation), etc.
[0009] However, this information contains a lot of subjective judgment by the blower, and when the basicity of the target and the actual result deviate, the P concentration in the steel becomes higher than the target composition, so the blower adds excess quicklime to account for this variation. In other words, the dephosphorization process is carried out at a certain level, which increases the steelmaking cost.
[0010] As a method for preventing such excessive addition of quicklime, estimating the component concentrations of slag has been considered. For example, Patent Document 1 discloses a technique for estimating the component concentrations in slag from the flow rate of exhaust gas discharged from a refining facility and the measurement results of the component concentrations in the exhaust gas. Patent Document 2 discloses a technique for estimating the component concentrations in slag using the discharge start angle of the primary blowing slag from a converter and other explanatory variables. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] Patent No. 6579136 [Patent Document 2] International Publication No. 2019 / 117200 [Non-patent literature]
[0012] [Non-Patent Document 1] Y.Harada et.al., “Structural Evaluation of Molten Aluminosilicate by Combining Impedance Measurements and Cell Model Calculations”, ISIJ International, Vol.60(2020),No.1,pp.42-50 Summary of the Invention [Problem to be solved by the invention]
[0013] Thus, Patent Document 1 discloses a method for indirectly estimating the component concentration in slag from the component concentration in exhaust gas. However, generally, the information measured on exhaust gas has a large error. For example, the flow rate of exhaust gas is often estimated from the exhaust gas pressure difference in flow passages with different cross-sectional areas based on the Venturi effect, but the pressure, temperature, and flow rate of this exhaust gas repeatedly fluctuate greatly during operation, which tends to increase the measurement error. Therefore, the component concentration in slag estimated from exhaust gas information with a large measurement error also has a problem of a large estimation error. Patent Document 2 is a method for determining the amount of CaO source added by prediction using a model with a small statistical variance between prediction and actual results. However, such a statistical distribution may cause variance between the predicted value and the actual value. In addition, when an operation that is not included in the data on which the prediction model is based, such as abnormal blowing, is performed, there is a risk that the statistical model cannot predict it. In that case, the amount of CaO source added is determined based on the sensory information of the blower. These have a certain variance, and it is difficult to add the appropriate amount of CaO source with high accuracy.
[0014] Therefore, in the methods described in Patent Documents 1 and 2, it is difficult to accurately estimate the composition of the slag, and it is also difficult to accurately adjust the amount of CaO source added to the slag in the converter. Therefore, it is also difficult to accurately control the composition of the slag in the converter.
[0015] In view of the above-mentioned circumstances, an object of the present application is to provide an impedance and phase angle difference measuring probe used to accurately control the composition of slag, and a slag composition control method using said probe. [Means for solving the problem]
[0016] As described above, the amount of CaO source added during blowing in a converter depends on the sensory information of the blower, and the addition of an excessive amount of CaO source increases the steelmaking cost and also increases the cost of treating the steelmaking slag generated during the treatment. In response to this problem, the inventors have conceived that the amount of CaO source added can be accurately adjusted by estimating the basicity of the slag during blowing, which is particularly important in determining the amount of CaO source added.
[0017] Here, the present inventors have focused on a method reported in Non-Patent Document 1 for estimating the NBO / T of SiO2-Al2O3-MO (M: Ca or Mg) molten slag by impedance information of the molten slag. In this method, a platinum electrode is immersed in slag molten in a platinum crucible, and an AC voltage is applied to the molten slag. The method is a method for predicting NBO / T by combining the values of multiple impedance components obtained by equivalent circuit analysis of impedance information (Nyquist plot) obtained by applying an AC voltage to the molten slag and a known thermodynamic model. Here, NBO / T is an index indicating the proportion of non-bridging oxygen at that temperature. Since non-bridging oxygen can bond with Ca ions, this result is considered to indicate the possibility of predicting the basicity of slag by impedance information.
[0018] Therefore, the inventors have considered using this impedance measurement technology to measure the slag basicity that changes during blowing. Specifically, a Nyquist plot is created from impedance information of multiple slags having different basicities, and the resistance of the slag (combined resistance described below) is obtained from the Nyquist plot and a specified formula. Next, a calibration curve is created based on the relationship between the basicity and resistance of the slag. Then, the impedance of the slag to be measured is separately measured, the resistance is obtained from the Nyquist plot and a specified formula, and the basicity of the slag to be measured is estimated by applying the resistance value to the calibration curve.
[0019] As a result, it was found that, when the slag basicity was estimated by this method, a certain degree of accuracy could be maintained, but there was still room for improvement. This is because the slag resistance obtained by this method was the combined resistance of the solution resistance and the charge transfer resistance, and both the solution resistance and the charge transfer resistance were related to the slag basicity (CaO / SiO2) and the iron oxide (FeO) content, so it was difficult to separate and estimate only the slag basicity from the combined resistance.
[0020] Therefore, the inventors have further studied and have come up with the idea of obtaining the combined resistance of the slag by separating the solution resistance and the charge transfer resistance. Specifically, since the solution resistance of the slag depends on the distance between the electrode terminals of the probe, while the charge transfer resistance does not depend on the distance between the electrode terminals, the inventors have come up with the idea that the solution resistance and the charge transfer resistance can be obtained separately by changing the distance between the electrode terminals to obtain the combined resistance of the slag.
[0021] Furthermore, the present inventors have developed a probe that is more suitable for the above method, which has at least three electrode terminals and is arranged so that the distance between the electrode terminals is different. This makes it possible to measure impedance, etc., by changing the combination of two electrode terminals used for measurement, changing the distance between the electrode terminals, and obtain the combined resistance of the slag, so that the solution resistance and charge transfer resistance of the slag can be obtained separately. Then, by using the solution resistance and charge transfer resistance of the slag, it becomes possible to separate and measure only the basicity of the slag with greater accuracy, and the slag composition can be controlled with greater accuracy. The present invention has been completed based on the above findings. Each aspect of the present invention will be described below.
[0022] The first aspect is a probe for measuring the impedance and phase angle difference of a high-temperature molten material, which has at least three electrode terminals formed of a metal or a conductive refractory material, and is arranged so that the distances between the electrode terminals are different.
[0023] In the above probe, the distance between the electrode terminals may be 2 mm to 100 mm, and the length of the electrode terminals may be 1 mm to 100 mm. The probe may also have a temperature measuring sensor. Furthermore, the probe may be attachable to a converter sublance or a sampling device.
[0024] A second aspect is a method for controlling the composition of slag in a converter using the probe of the first aspect, comprising a first step of preparing a plurality of test slags of the same type as the slag to be measured and each having a different basicity; a second step of selecting one of the test slags, immersing the probe in the test slag, selecting two electrode terminals of the probe to apply a voltage, and passing a current while changing the frequency to measure impedance, creating a Nyquist plot for each test slag based on the impedance, and obtaining a combined resistance of the test slag from the Nyquist plot and the following formula (1); a third step of repeating the process of changing the combination of the two electrode terminals to apply a voltage in the second step and obtaining a combined resistance of the test slag; and a third step of calculating a solution resistance and a charge transfer resistance of the test slag from the relationship between the combined resistance of the test slag obtained by the second and third steps and the distance between the electrode terminals used for the measurement. a fourth step of calculating the solution resistance and charge transfer resistance of the test slag by changing the type of test slag and repeating the calculation of the solution resistance and charge transfer resistance of the test slag by the same method as the second step to the fourth step; a sixth step of obtaining a basicity calibration curve based on the basicity of the test slag and the solution resistance and charge transfer resistance obtained by the fourth step and the fifth step; a seventh step of obtaining a combined resistance of the slag for the slag to be measured by the same method as the second and third steps; an eighth step of calculating the solution resistance and charge transfer resistance of the slag from the relationship between the combined resistance of the slag obtained in the seventh step and the distance between the electrode terminals used in the measurement; a ninth step of estimating the basicity of the slag based on the solution resistance and charge transfer resistance obtained in the eighth step based on the basicity calibration curve; and a tenth step of adjusting the amount of CaO source to be added to the slag based on operation information of the converter including the basicity of the slag estimated in the ninth step.
[0025]
number
[0026] In the above slag composition control method, in the sixth step, a calibration curve of the iron oxide content is obtained based on the iron oxide content of the test slag and the solution resistance and charge transfer resistance obtained in the fourth and fifth steps, in the ninth step, the iron oxide content of the slag is estimated based on the iron oxide content calibration curve from the solution resistance and charge transfer resistance obtained in the eighth step, and in the tenth step, the iron oxide content of the slag estimated in the ninth step may be included in the operation information of the converter to adjust the amount of CaO source added to the slag. In addition, in at least one of the second step, the third step, the fifth step, and the seventh step, the impedance measured when the frequency of the current flowing through the electrode terminal is 10 kHz may be 10 mΩ to 100 kΩ. Furthermore, in the tenth step, the temperature of the slag may be included in the operation information of the converter to adjust the amount of CaO source added to the slag. Effect of the Invention
[0027] According to the first aspect of the probe, the impedance can be measured in one step by changing the combination of two electrode terminals used for the measurement and changing the distance between the electrode terminals. In other words, the impedance can be measured by changing the distance between the electrode terminals while suppressing the influence of the change in the composition of the high-temperature molten material over time.
[0028] In addition, according to the second aspect of the slag composition control method, by using the probe of the first aspect, the solution resistance and charge transfer resistance of the slag can be obtained separately, so that the basicity of the slag can be estimated separately from the iron oxide content, and at the same time, the estimation accuracy can be improved, and the slag composition can be controlled more accurately than before. [Brief description of the drawings]
[0029] [Figure 1] FIG. 1 is a schematic diagram of a probe 10. [Diagram 2] FIG. 2 is a schematic diagram of the measurement surface side of the probe 10. [Diagram 3] FIG. 2 is a schematic diagram of a side view of the probe 10. [Figure 4] FIG. 13 is a diagram showing an example of the relationship between the combined resistance of a test slug and the inter-electrode distance in an embodiment. [Diagram 5] In the examples, multiple regression analysis was performed based on the solution resistance and charge transfer resistance of the test slag. (a) is the result of multiple regression analysis of slag basicity based on the solution resistance and charge transfer resistance. (b) is the result of multiple regression analysis of iron oxide content based on the solution resistance and charge transfer resistance. [Figure 6] 1 is an example of the relationship between slag basicity (CaO+FeO) / SiO2 and composite resistivity obtained using a conventional probe. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0030] [Impedance and phase angle measurement probe] A probe for measuring impedance and phase angle difference of a high-temperature molten material according to a first aspect will be described with reference to Fig. 1. Fig. 1 is a schematic diagram of a probe 10 for measuring impedance and phase angle difference according to one embodiment.
[0031] A probe 10 for measuring the impedance and phase angle difference of a high-temperature molten material (hereinafter sometimes referred to as "probe 10") includes a substrate 1 and three electrode terminals 2. However, in the probe of the first embodiment, the number of electrode terminals 2 needs to be at least three, and may be four or more. Preferably, it is five or more. The greater the number of electrode terminals 2, the more impedances of the high-temperature molten material that can be measured in one step by changing the distance between the electrode terminals.
[0032] Here, the "high-temperature melt" refers to a melt composed of high-temperature oxides, and mainly means slag. In this specification, "slag" can be read as "high-temperature melt." In addition, since the phase angle difference is measured in impedance measurement, in this specification, impedance and phase angle difference are sometimes simply referred to as "impedance."
[0033] The substrate 1 has a cylindrical shape, the outside is formed of a metal, and the inside is filled with a refractory. Examples of the metal constituting the outside include iron and molybdenum. Examples of the refractory filled inside include refractories such as Al2O3 and MgO. It is preferable that the surface of the measurement side of the base 1 except for the electrode terminals 2 is coated with a heat-resistant insulating material (e.g., oxides such as spinel) by thermal spraying or the like to ensure insulation. This allows current to flow only between the electrode terminals 2, and the variation in the measured impedance value can be suppressed. This also makes it possible to create a stable Nyquist plot with small variation, enabling precise measurement. The shape of the substrate 1 of the probe of the first embodiment is not particularly limited, and does not have to be cylindrical. The dimensions of the substrate 1 can be set appropriately according to the purpose.
[0034] The electrode terminal 2 is a member for applying a voltage to measure the impedance of the slag between the electrode terminals 2, and one end is provided so as to protrude from the substrate 1, and the other end is connected to a device for measuring impedance, etc. The electrode terminal 2 is made of a metal or a conductive refractory. An example of the metal forming the electrode terminal 2 is tungsten. An example of the conductive refractory is a zirconia-based refractory or a magnesia carbon-based refractory.
[0035] Next, a description will be given of the positional relationship of the electrode terminals 2. Fig. 2 is a schematic diagram of the measurement surface side of the probe 10, and Fig. 3 is a schematic diagram of the side surface of the probe 10.
[0036] As shown in FIG. 2, the probe 10 is arranged so that the distances (d1, d2, d3) between the electrode terminals 2 are different. This is to obtain the impedance of the slug measured in one process by changing the distance between the electrode terminals 2. Here, the distance between the electrode terminals 2 is the distance between the centers of the electrode terminals. In addition, it is preferable that the distance between the electrode terminals 2 is a distance obtained by selecting the electrode terminals 2 that form the sides of a polygon formed by the electrode terminals 2. For example, as shown in FIG. 2, when the polygon formed by the electrode terminals 2 is a triangle, it is preferable to use pairs of electrode terminals 2 corresponding to each side of the triangle for measurement.
[0037] The distance (d1, d2, d3) between the electrode terminals 2 is preferably 2 mm to 100 mm. If the distance between the electrode terminals 2 is less than 2 mm, for example, bubbles may be generated in the slag, and if the bubbles are present between the electrode terminals 2, the measurement accuracy may decrease. If the distance between the electrode terminals 2 exceeds 100 mm, in addition to discharging to the paired electrode terminal 2, discharging to the crucible, furnace wall, lance, etc., may decrease the measurement accuracy. If the measurement accuracy decreases, it may become difficult to create a Nyquist plot. According to what the present inventors have confirmed, from the viewpoint of further improving the measurement accuracy, the distance between the electrode terminals 2 is more preferably 10 mm to 30 mm.
[0038] In addition, when the distance values between the electrode terminals 2 are arranged in order, the difference in the distance values between adjacent electrode terminals 2 is preferably 1 to 10 mm. This is to improve the calculation accuracy of the solution resistance and the charge transfer resistance in the slag composition control method described later.
[0039] The length l' of the electrode terminal 2 in the direction protruding from the substrate 1 is preferably 1 mm to 100 mm. If the length l' is less than 1 mm, the effect of current concentration on the end of the electrode terminal 2 may increase, resulting in a risk of reduced measurement accuracy. If the length l' exceeds 500 mm, the effect of external electromagnetic noise on the electrode terminal 2 may increase, resulting in a risk of reduced measurement accuracy. According to the findings of the present inventors, from the viewpoint of further improving measurement accuracy, the length l is more preferably 10 mm to 50 mm.
[0040] The dimensions and arrangement of the other electrode terminals 2 are not particularly limited and can be set appropriately depending on the purpose.
[0041] In addition to these terminals, the probe 10 may be equipped with a temperature sensor. This allows the slag temperature to be measured simultaneously in addition to the impedance measurement. The slag temperature is an important index for determining the amount of CaO source to be added when controlling the basicity of the slag.
[0042] The probe 10 is configured to be attachable to a converter sublance or sampling device, as the probe 10 is used to measure slag impedance and phase angle difference, among other things, in a converter.
[0043] The probe for measuring the impedance and phase angle difference of a high-temperature molten material according to the first aspect has been described above using one embodiment of the probe 10. The probe according to the first aspect has at least three electrode terminals, and the distance between the electrodes is different, so that the impedance of the high-temperature molten material can be measured in one step by changing the combination of two electrode terminals used for measurement and changing the distance between the electrode terminals.
[0044] Since the composition of the slag in the converter changes over time, by obtaining the impedance measured by changing the distance between the electrode terminals in one process, it is less susceptible to the effects of changes in the slag composition over time. Since the conventional probe has two electrode terminals, in order to obtain the impedance measured by changing the distance between the electrode terminals, it is necessary to prepare multiple probes with different distances between the electrode terminals and immerse each probe in the slag to measure the impedance, which requires a certain amount of time and there is a risk that the composition of the slag will change during that time.
[0045] Therefore, by using the probe of the first aspect, the influence of the change in the slag composition due to the time change can be suppressed, and the impedance of the slag measured by changing the distance between the electrode terminals can be obtained. This makes it possible to accurately estimate the slag basicity, etc., in the slag composition control method described later.
[0046] [Slag composition control method] Next, a method for controlling the composition of slag in a converter according to a second embodiment will be described. The method for controlling the composition of slag in a converter according to the second embodiment is characterized in that the basicity of the slag is estimated from the impedance of the slag measured using the probe according to the first embodiment, and the amount of CaO source added is adjusted based on converter operation information including information on the estimated basicity of the slag, thereby controlling the slag composition.
[0047] Hereinafter, the slag composition control method of the second aspect will be described using one embodiment, although the slag composition control method of the second aspect is not limited thereto.
[0048] The slag composition control method of one embodiment includes steps 1 to 10. Each step will be described below.
[0049] <1st process> The first step is to prepare a number of test slags which are the same type as the slag to be measured but have different basicities.
[0050] The "slag to be measured" refers to slag in a converter, the composition of which is to be controlled. The components of the slag to be measured preferably contain CaO. This is because a CaO source is used as an additive to adjust the basicity of the slag. For example, CaO-SiO2-FeO slag can be mentioned. For "slag basicity," various indicators can be used depending on the constituents of the slag. When the slag composition is CaO-SiO2-FeO, for example, (CaO+FeO) / SiO2 (weight ratio) and CaO / SiO2 (weight ratio) can be used as indicators of slag basicity. Among these, the most important indicator in an actual converter is CaO / SiO2 (weight ratio), which can be estimated with high accuracy. A "test slag" is a slag of the same type as the slag to be measured and of known composition.
[0051] <Second process> The second step is a step of selecting one of the above test slags, immersing the probe of the first embodiment in the test slag, selecting two of the electrode terminals of the probe to which a voltage is applied, passing a current through the terminals while changing the frequency to measure the impedance, creating a Nyquist plot of each test slag based on the impedance, and obtaining the combined resistance of the test slag from the Nyquist plot and the following equation (2).
[0052]
number
[0053] where Z is impedance, V is voltage between electrode terminals, I is current between electrode terminals, and R sol :Solution resistance, R ct : charge transfer resistance, C: double layer capacitance, ω: angular frequency, j: imaginary unit. sol , R ct and C are the impedance components obtained by equivalent circuit analysis.
[0054] The "frequency" of the current passed through the probe during impedance measurement is not particularly limited and can be set appropriately so that a Nyquist plot can be created. For example, the frequency is set to 50 Hz to 100 kHz, and the current is passed while changing the frequency. A "Nyquist plot" is an impedance spectrum plotted on a complex plane, and is generally plotted as a semicircle around a solid line. The point of intersection of the Nyquist plot with the horizontal axis that is farthest from the origin corresponds to the composite resistance of the slug. Therefore, by creating a Nyquist plot and applying the impedance value at the point of intersection of the plot with the horizontal axis that is farthest from the origin to the above formula (2), the composite resistance of the slug can be calculated. "Total resistance" refers to the combined resistance of solution resistance and electrolytic transfer resistance. Solution resistance is the liquid resistance of the slag between the electrodes and depends on the distance between the electrodes. Charge transfer resistance is the transfer resistance of the charge (electrons) that moves with the electrode reaction and does not depend on the distance between the electrodes.
[0055] <3rd process> The third step is a step of repeating the second step by changing the combination of the two electrode terminals to which the voltage is applied to obtain the combined resistance of the test slug. By the second and third steps, it is possible to obtain the impedance (combined resistance) measured for one test slug by changing the distance between the electrode terminals.
[0056] Here, the number of repetitions can be appropriately set according to the number of combinations of electrode terminals and the purpose. In addition, the second and third steps can be regarded as one step because the measurements are performed on the same test slug.
[0057] <4th process> This is a step of calculating the solution resistance and charge transfer resistance of the test slag from the relationship between the combined resistance of the test slag obtained in the second and third steps and the distance between the electrode terminals used in the measurement. This makes it possible to obtain the solution resistance and charge transfer resistance of the test slag used in the second and third steps. In this way, in the second aspect, by using the probe of the first aspect, the combined resistance of the slag can be separated into the solution resistance and the charge transfer resistance and calculated.
[0058] The specific method for calculating the combined resistance of the slag by separating it into the solution resistance and the charge transfer resistance is as follows. The combined resistance of the slag is plotted on the vertical axis and the distance between the electrode terminals on the horizontal axis, and the results are plotted and an approximation line is applied. The solution resistance can be obtained from the slope of the resulting straight line, and the charge transfer resistance can be obtained from the intercept value of the vertical axis. In this way, the solution resistance and the charge transfer resistance can be obtained by using the relationship between the combined resistance of the slag (vertical axis) and the distance between the electrodes (horizontal axis). Note that, strictly speaking, the intercept value of the vertical axis is the sum of the charge transfer resistance and the contact resistance, etc., but in this specification, these are collectively referred to as the charge transfer resistance.
[0059] <5th process> The fifth step is a step of repeatedly calculating the solution resistance and charge transfer resistance of the test slag by changing the type of test slag used in the second to fourth steps in the same manner as in the second to fourth steps. This allows the solution resistance and charge transfer resistance of each test slag used in the measurement to be calculated. The number of repetitions can be appropriately set depending on the number of types of test slags and the purpose.
[0060] <6th process> The sixth step is to obtain a basicity calibration curve based on the basicity of the test slag used in the measurement and the solution resistance and charge transfer resistance obtained in the fourth and fifth steps. The basicity calibration curve can be obtained by multiple regression analysis. Specifically, the basicity calibration curve can be created from a regression equation obtained by multiple regression with the slag basicity CaO / SiO2 (weight ratio) as the response variable and the solution resistance and charge transfer resistance as explanatory variables.
[0061] When using a conventional probe, the composite resistivity obtained from the measurement of the test slag includes the effects of the iron oxide content as well as the basicity, so that it is not possible to separate the iron oxide content from the basicity index, and (CaO+FeO) / SiO2 (weight ratio) is used as the index.
[0062] On the other hand, when the probe of the first embodiment is used, the solution resistance and the charge transfer resistance can be separated from the combined resistance of the slag and can be estimated from the two resistances, so that CaO / SiO2, which is more important and accurate in an actual converter, can be used as an indicator of the slag basicity, and therefore a more accurate basicity calibration curve can be obtained.
[0063] Here, in the sixth step, an iron oxide content calibration curve may be obtained based on the iron oxide content (wt%) of the test slag and the solution resistance and charge transfer resistance of the test slag obtained in the fourth and fifth steps. The iron oxide content calibration curve can be obtained by multiple regression analysis, similar to the method for obtaining the basicity calibration curve. Specifically, the iron oxide content calibration curve can be created from a regression equation obtained by multiple regression in which the iron oxide content (wt%) of the test slag is the response variable and the solution resistance and charge transfer resistance are explanatory variables.
[0064] <7th process> The seventh step is a step of obtaining a combined resistance of the slag to be measured by a method similar to the second and third steps.
[0065] <8th process> The eighth step is a step of calculating the solution resistance and the charge transfer resistance of the slag to be measured from the relationship between the combined resistance of the slag to be measured obtained in the seventh step and the distance between the electrode terminals used in the measurement. The specific method is the same as that in the fourth step.
[0066] <9th process> The ninth step is a step of estimating the basicity of the slag to be measured based on the solution resistance and charge transfer resistance of the slag to be measured obtained in the eighth step, based on the basicity calibration curve obtained in the sixth step.
[0067] Here, in the 9th step, the iron oxide content of the slag to be measured may be estimated from the charge transfer resistance of the slag to be measured obtained in the 8th step based on the iron oxide content calibration curve obtained in the 6th step.
[0068] <10th process> The tenth step is a step of adjusting the amount of CaO source added to the slag in the converter based on the operation information of the converter including the basicity of the slag estimated in the ninth step. This allows the slag composition to be controlled with high precision. The CaO source can be, for example, quicklime.
[0069] The basicity of the slag is an important index for adjusting the amount of CaO source added, but ultimately, it is judged taking into consideration other converter information as well. Converter operation information includes the flame and slag foaming height from the throat, in addition to the slag basicity. If the iron oxide content is estimated (step 9) and the slag temperature is measured, the converter operation information may include this information to adjust the amount of CaO source added to the slag. This further improves the accuracy of controlling the slag composition.
[0070] An example of a situation in which the amount of CaO source added is adjusted based on converter operation information is when the slag basicity is lower than expected, making it difficult for the dephosphorization reaction to proceed (above formula (1)), and therefore additional CaO source is added.
[0071] The slag composition control method of the second aspect has been described above using the slag composition control method 100, which is one embodiment of the method. According to the slag composition control method of the second aspect, the probe of the first aspect is used, and the solution resistance and the charge transfer resistance can be calculated separately from the combined resistance of the slag. This makes it possible to estimate the basicity of the slag separately from the iron oxide content, and improves the estimation accuracy. Therefore, the composition of the slag can be controlled more accurately than before.
[0072] <Additional information> Here, the slag composition control method of the second embodiment will be supplemented. That is, in at least one of the second, third, fifth, and seventh steps of the slag composition control method of the second embodiment, when the frequency of the current passing through the electrode terminal of the probe is 10 kHz, the measured impedance is preferably 10 mΩ to 100 kΩ. This allows the impedance of the slag to be stably measured. If the impedance is less than 10 mΩ at a frequency of 10 kHz, the impedance is small, so the voltage that can be applied is small, and as a result, the measured current value becomes minute, and the measurement accuracy deteriorates. If the impedance exceeds 100 kΩ, the impedance is large, so the applied voltage needs to be increased in order to obtain a sufficient measured current value, which causes a problem that the electrode itself reacts and melts. More preferably, the impedance is 100 mΩ to 10 kΩ at a frequency of 10 kHz. EXAMPLES
[0073] Following the slag control method described above, slag basicity and iron oxide content were estimated. Impedance measurements were performed on test slags under the following conditions:
[0074] A number of CaO-SiO2-FeO slags were used as test slags. The composition of the slags used was that CaO / SiO2 was in the range of 0.6 to 1.2, and the FeO content was 35% or 40%. The probe used had five electrode terminals, with the distance between each electrode terminal being 15 mm, 17.5 mm, 20 mm, 22.5 mm, and 25 mm, and the length of the electrode terminals being 20 mm. The frequency of the current passing through the electrode terminals was changed in the range of 4 Hz to 1 MHz.
[0075] From the obtained results, the solution resistance and charge transfer resistance of each test slag were calculated. As an example, the relationship between the obtained combined resistance and the distance between the electrodes for a test slag with a CaO / SiO2 ratio of 0.6 and an FeO content of 40% is shown in Figure 4. As shown in Figure 4, the slope of the obtained approximation line is the solution resistance, and the intercept of the vertical axis is the electrolytic transfer resistance.
[0076] The solution resistance and charge transfer resistance of the test slags were obtained in this manner, and the estimation accuracy of the slag basicity (CaO / SiO2:C / S) and iron oxide content (FeO (%)) was examined by multiple regression analysis. The results are shown in Figure 5. (a) shows the result of multiple regression analysis of the slag basicity based on the solution resistance, and the regression coefficient R 2 (b) shows the result of multiple regression analysis of the iron oxide content based on the charge transfer resistance, with the regression coefficient R 2 From these results, it was confirmed that the estimation accuracy of the slag basicity and iron oxide content was very high.
[0077] Furthermore, when a conventional probe (two electrode terminals) is used, the obtained resistance is a composite resistance that includes the effects of iron oxide content as well as basicity, so it is not possible to separate the iron oxide content from the basicity indicator, and an indicator with lower accuracy than CaO / SiO2, (CaO+FeO) / SiO2 (weight ratio), is used. As an example, Figure 6 shows the relationship between (CaO+FeO) / SiO2 and composite resistance (R * ) is shown in Figure 6. [Explanation of symbols]
[0078] 1 Base material 2 electrode terminals 10 Probes
Claims
1. At least three electrode terminals made of a metal or a conductive refractory material and a temperature measuring sensor are provided, In order to obtain the impedance of the slag measured by changing the distance between the electrode terminals in a single process that is not easily affected by changes in the slag composition over time, The distance between the electrode terminals is The electrode terminals forming the sides of a polygon formed from the electrode terminals are arranged at different distances obtained by selecting the electrode terminals. Probe for impedance and phase angle difference measurements of high temperature melts.
2. A probe for measuring the impedance and phase angle difference of a high-temperature molten material as described in claim 1, wherein the number of the electrode terminals is five or more.
3. A method for controlling the composition of slag in a converter using the probe according to claim 1 or 2, comprising the steps of: a first step of preparing a plurality of test slags of the same type as the slag to be measured, each having a different basicity; a second step of selecting one of the test slugs, immersing the probe in the test slug, selecting two of the electrode terminals of the probe to which a voltage is applied, passing a current through the electrode terminals while changing the frequency to measure impedance, creating a Nyquist plot for each of the test slugs based on the impedance, and calculating a combined resistance of the test slug from the Nyquist plot and the following formula (1); a third step of repeating the second step of changing the combination of the two electrode terminals to which a voltage is applied to obtain the combined resistance of the test slug; a fourth step of calculating the solution resistance and the charge transfer resistance of the test slug from the relationship between the combined resistance of the test slug obtained by the second step and the third step and the distance between the electrode terminals used in the measurement; A fifth step of repeatedly calculating the solution resistance and the charge transfer resistance of the test slag by changing the type of the test slag and using the same method as in the second step to the fourth step; A sixth step of obtaining a basicity calibration curve based on the basicity of the test slag and the solution resistance and the charge transfer resistance obtained in the fourth step and the fifth step; A seventh step of obtaining the combined resistance of the slug to be measured by a method similar to the second and third steps; an eighth step of calculating the solution resistance and the charge transfer resistance of the slag from a relationship between the combined resistance of the slag obtained in the seventh step and a distance between the electrode terminals used in the measurement; A ninth step of estimating the basicity of the slag from the solution resistance and the charge transfer resistance obtained in the eighth step based on the basicity calibration curve; and a tenth step of adjusting an amount of CaO source to be added to the slag based on operation information of the converter including the basicity of the slag estimated in the ninth step. Methods for controlling slag composition. [0010] Here, Z is impedance, V is voltage between electrode terminals, I is current between electrode terminals, Rsol is solution resistance, Rct is charge transfer resistance, C is double layer capacitance, ω is angular frequency, and j is imaginary unit.
4. In the sixth step, an iron oxide content calibration curve is obtained based on the iron oxide content of the test slag and the solution resistance and charge transfer resistance obtained in the fourth and fifth steps; in the ninth step, the iron oxide content of the slag is estimated based on the iron oxide content calibration curve from the solution resistance and charge transfer resistance obtained in the eighth step; In the tenth step, the iron oxide content of the slag estimated in the ninth step is included in the operation information of the converter, and the amount of CaO source added to the slag is adjusted. The method for controlling slag composition according to claim 3.
5. 5. The slag composition control method according to claim 3, wherein in at least one of the second step, the third step, the fifth step, and the seventh step, when the frequency of the current passing through the electrode terminal is 10 kHz, the measured impedance is 10 mΩ to 100 kΩ.
6. The slag composition control method according to any one of claims 3 to 5, wherein in the tenth step, the operation information of the converter includes the temperature of the slag to adjust the amount of CaO source added to the slag.
Citation Information
Patent Citations
Method and apparatus for measurement of basicity of slag
JP2003207473A
Boundary position detection method, boundary position detection system and data measurement probe used in boundary position detection system
JP2012251884A
Measuring probe for measurement in molten metal or slag
JP2014092545A
Refining process state estimation device, refining process state estimation method, and molten metal manufacturing method
JP6579136B2
Slag oxygen sensor
US6340418B1