Curable composition for forming hard coat layer containing specific urethane (meth)acrylate

A curable composition using urethane (meth)acrylate and perfluoropolyether with active energy ray polymerizable groups forms a hard coat layer with high scratch resistance, stretchability, and antistatic properties, addressing the limitations of existing hard coat layers for flexible displays.

JP7587201B2Active Publication Date: 2024-11-20NISSAN CHEM CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020154006
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-14
Publication Date
2024-11-20
Estimated Expiration
2040-09-14

AI Technical Summary

Technical Problem

Existing hard coat layers for flexible displays lack both high scratch resistance and stretchability, and often do not provide antistatic properties, making them unsuitable for protecting bendable displays from scratches and static electricity.

Method used

A curable composition comprising urethane (meth)acrylate with specific partial structures, perfluoropolyether with active energy ray polymerizable groups, a polymerization initiator, and optionally an antistatic agent, which forms a hard coat layer with excellent scratch resistance, stretchability, and antistatic properties when cured.

Benefits of technology

The composition achieves a hard coat layer with both high scratch resistance and stretchability, and can impart antistatic properties, suitable for flexible displays, providing protection against scratches and static electricity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587201000001
    Figure 0007587201000001
  • Figure 0007587201000002
    Figure 0007587201000002
  • Figure 0007587201000003
    Figure 0007587201000003
Patent Text Reader

Abstract

To provide a curable composition capable of forming a hard coat layer which achieves both high scratch resistance and stretchability and can be imparted with antistatic properties.SOLUTION: The curable composition contains: (a) 100 pts.mass of at least one urethane (meth)acrylate having any one of a partial structure of an allophanate-modified product of a diisocyanate, a partial structure of a biuret-modified product of the diisocyanate, and a partial structure of an isocyanurate-modified product of the diisocyanate; (b) 0.05 to 10 pts.mass of a perfluoropolyether having an active energy ray-polymerizable group at a terminal of a molecular chain containing a poly(oxyperfluoroalkylene) group; and (c) 1 to 20 pts.mass of a polymerization initiator which generates radicals by means of active energy rays.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a curable composition useful as a material for forming a hard coat layer applied to the surface of various display elements such as flexible displays, and relates to a curable composition capable of forming a hard coat layer that is excellent in abrasion resistance and stretchability and can also be imparted with antistatic properties. [Background technology]

[0002] Smartphones have become the most common form of mobile phone and are indispensable in our daily lives. A cover glass is used on the surface of a smartphone to prevent the display from being scratched. In recent years, bendable displays, so-called flexible displays, have been developed as the above-mentioned displays. Flexible displays are expected to have a wide range of applications as displays that can be bent and rolled up. However, glass is generally hard and difficult to bend back, so it cannot be applied to flexible displays. Therefore, instead of glass, attempts have been made to apply a plastic film with a hard coat layer that has scratch resistance to prevent scratches to the surface of a flexible display. When a flexible display with a plastic film with a hard coat layer applied to its surface is curved with the display side facing outward (i.e., with the hard coat layer facing outward), a stress in the tensile direction is generated in the hard coat layer on the outermost surface, so the hard coat layer is required to have a certain degree of extensibility.

[0003] In addition, a method for imparting scratch resistance to a hard coat layer generally involves, for example, forming a high-density crosslinked structure, i.e., forming a crosslinked structure with low molecular mobility to increase surface hardness and provide resistance to external forces. Currently, the most commonly used material for forming these hard coat layers is a multifunctional acrylate-based material that undergoes three-dimensional crosslinking by radicals. However, due to its high crosslinking density, multifunctional acrylate-based materials usually have poor stretchability. Thus, there is a trade-off between the stretchability and scratch resistance of the hard coat layer, and the challenge is to achieve both properties at the same time.

[0004] As one of the methods for improving scratch resistance, a method of adding a silicone or fluorine-based surface modifier to the curable composition forming the hard coat layer to impart slipperiness to the cured film surface has been known. It has also been reported that a certain level of scratch resistance can be achieved by using an aliphatic urethane (meth)acrylate having an alicyclic skeleton and a photopolymerizable unsaturated group in combination with a fluorine-containing compound having a photopolymerizable unsaturated group (Patent Document 1).

[0005] On the other hand, when a hard coat film is used as a front protective material for a display, it is sometimes required to have antistatic properties in order to prevent adhesion of dust and other particles due to static electricity generated during lamination and to prevent malfunction of the display. 10 It is desirable for the resistance to be on the order of Ω / □. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2016-125049 A Summary of the Invention [Problem to be solved by the invention]

[0007] The hard coat layer described in Patent Document 1 has a certain level of scratch resistance, but the level is not satisfactory. The present invention aims to provide a curable composition capable of forming a hard coat layer that has both high scratch resistance and stretchability and can further impart antistatic properties. [Means for solving the problem]

[0008] A first aspect of the present invention is a curable composition comprising: (a) 100 parts by mass of at least one urethane (meth)acrylate having any one of partial structures represented by the following formulae [1] to [3]; (b) 0.05 to 10 parts by mass of a perfluoropolyether having an active energy ray-polymerizable group at an end of a molecular chain containing a poly(oxyperfluoroalkylene) group; and (c) 1 to 20 parts by mass of a polymerization initiator that generates radicals by active energy rays. [ka] (In the above formula, R 1 , R 2 and R 3 each represents a divalent hydrocarbon group having 4 to 15 carbon atoms; R 0 represents the residue of a monohydric alcohol.

[0009] The (a) urethane (meth)acrylate is, for example, a reaction product of (a1) a (meth)acrylate compound having at least one hydroxy group and (a2) at least one isocyanate compound selected from the group consisting of compounds represented by the following formulas [1'] to [3']: [ka] (In the above formula, R 0 and R 1 is defined as in the above formula [1], and R 2 is defined as in the above formula [2], and R 3 is defined as in formula [3] above.)

[0010] The (a2) isocyanate compound is, for example, a compound represented by the formula [1'].

[0011] The (b) perfluoropolyether has an active energy ray-polymerizable group at the end of the molecular chain containing the poly(oxyperfluoroalkylene) group, for example via a urethane bond.

[0012] The (b) perfluoropolyether has at least two active energy ray-polymerizable groups at the terminals of the molecular chain containing the poly(oxyperfluoroalkylene) group, for example via a urethane bond.

[0013] The (b) perfluoropolyether has at least two active energy ray-polymerizable groups, for example, via a urethane bond, at each of both ends of the molecular chain containing the poly(oxyperfluoroalkylene) group.

[0014] The poly(oxyperfluoroalkylene) group of the (b) perfluoropolyether has both the repeating unit -[CF2O]- and the repeating unit -[CF2CF2O]-, and is a group formed by bonding these repeating units through block bonds, random bonds, or block bonds and random bonds.

[0015] The molecular chain containing the poly(oxyperfluoroalkylene) group has, for example, a structure represented by the following formula [4]. [ka] (In the above formula [4], n is the total number of the repeating units -[CF2CF2O]- and the repeating units -[CF2O]- and represents an integer of 5 to 30, and the repeating units -[CF2CF2O]- and the repeating units -[CF2O]- are bonded to each other through block bonds, random bonds, or block bonds and random bonds.)

[0016] The curable composition of the present invention may further comprise 10 to 55 parts by mass of (d) an antistatic agent. The (d) antistatic agent may comprise, for example, metal oxide particles. The metal oxide particles may comprise, for example, an oxide of at least one element selected from the group consisting of tin, zinc, and indium. The metal oxide particles may comprise, for example, tin oxide to which a dopant may be added. The metal oxide particles may comprise, for example, at least one of phosphorus-doped tin oxide and tin oxide the surface of which is coated with antimony pentoxide.

[0017] The curable composition of the present invention may further comprise (e) a solvent.

[0018] A second aspect of the present invention is a cured film obtained from the curable composition of the present invention.

[0019] A third aspect of the present invention is a hardcoat film comprising a hardcoat layer on at least one surface of a film substrate, the hardcoat layer being made of a cured film obtained from the curable composition of the present invention.

[0020] The hard coat layer is formed, for example, by a method including a step of applying the curable composition of the present invention onto a film substrate to form a coating film, and a step of irradiating the coating film with active energy rays to cure it.

[0021] The hard coat layer is formed, for example, by a method including a step of applying the curable composition of the present invention onto a film substrate to form a coating film, a step of removing the solvent from the coating film by heating, and a step of irradiating the coating film with active energy rays to cure it.

[0022] The hard coat layer has a thickness of, for example, 1 μm to 10 μm.

[0023] A fourth aspect of the present invention is a method for producing a laminate, comprising the steps of applying the curable composition of the present invention onto a film substrate to form a coating film, and irradiating the coating film with active energy rays to cure it. Effect of the Invention

[0024] According to the present invention, it is possible to provide a curable composition useful for forming a cured film and a hard coat layer that have both excellent scratch resistance and high stretchability even in a thin film having a thickness of 1 μm to 10 μm. In addition, according to the present invention, it is possible to provide a hard coat film having a cured film obtained from the curable composition or a hard coat layer made of the cured film, and it is possible to provide a hard coat film having excellent scratch resistance and stretchability, which are in a trade-off relationship. Furthermore, according to the present invention, it is possible to provide a curable composition useful for forming a cured film and a hard coat layer that is imparted with antistatic properties in addition to the above-mentioned scratch resistance and stretchability, and a hard coat film having a hard coat layer that is excellent in these three properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] <Curable composition> Each component of the curable composition of the present invention will be described below. [(a) Urethane (meth)acrylate] In the curable composition of the present invention, the (a) urethane (meth)acrylate is a compound having any one of the partial structures represented by the formulae [1] to [3], and is, for example, a reaction product obtained by reacting the (a1) (meth)acrylate compound having at least one hydroxyl group with (a2) at least one isocyanate compound selected from the group consisting of the compounds represented by the formulae [1'] to [3'], by a known method. Among them, the (a) urethane (meth)acrylate having the partial structure represented by the formula [1] is most preferable.

[0026] Examples of the (a1) (meth)acrylate compound having at least one hydroxy group include 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, 2-hydroxypropyl methacrylate, 2-hydroxybutyl acrylate, 2-hydroxybutyl methacrylate, 4-hydroxybutyl acrylate, 4-hydroxybutyl methacrylate, 2-(2-hydroxyethoxy)ethyl acrylate, 2-(2-hydroxyethoxy)ethyl methacrylate, glycerin diacrylate, glycerin dimethacrylate, pentaerythritol triacrylate, pentaerythritol trimethacrylate, dipentaerythritol pentaacrylate, and dipentaerythritol pentamethacrylate.

[0027] In the formulas [1'] to [3'], R 1 , R 2 and R 3 is a group obtained by removing two isocyanate groups from a diisocyanate compound, and examples thereof include a tetramethylene group, a pentamethylene group, a hexamethylene group, a tolylene group, a xylylene group, a phenylene group, a naphthylene group, a dicyclohexylmethane group, a trimethylhexamethylene group, an isophorone group, and a diphenylmethane group. 0 is a group obtained by removing an OH group from a monohydric alcohol that reacts with a diisocyanate compound to form a urethane bond.

[0028] The urethane (meth)acrylate (a) in the curable composition of the present invention may be used alone or in combination of two or more.

[0029] [(b) Perfluoropolyether] The (b) perfluoropolyether preferred in the curable composition of the present invention has an active energy ray polymerizable group at the end of the molecular chain containing a poly(oxyperfluoroalkylene) group via a urethane bond. The end of the molecular chain of the perfluoropolyether may be all ends or some ends of the molecular chain. When the molecular chain of the perfluoropolyether is linear, all ends and some ends of the molecular chain are both ends and one end of the linear molecular chain, respectively. Examples of the linking group between the poly(oxyperfluoroalkylene) group and the urethane bond include a hydrocarbon group having an ether bond, and at least one of the hydrogen atoms of the hydrocarbon group may be substituted with a fluorine atom. In the curable composition of the present invention, the (b) perfluoropolyether plays a role as a surface modifier in the hard coat layer formed from the curable composition of the present invention. In addition, the (b) perfluoropolyether has excellent compatibility with the (a) urethane (meth)acrylate, so that it is possible to form a hard coat layer that is suppressed from becoming cloudy and has a transparent appearance.

[0030] As the poly(oxyperfluoroalkylene) group, from the viewpoint of obtaining a cured film with good scratch resistance, a group having both -[CF2O]-(oxyperfluoromethylene group) and -[CF2CF2O]-(oxyperfluoroethylene group) as repeating units is preferred. In this case, the bond of these oxyperfluoroalkylene groups may be either block bond or random bond. The number of repeating units of the oxyperfluoroalkylene group is preferably in the range of 5 to 30, more preferably in the range of 7 to 21, as the total number of repeating units.

[0031] The molecular chain containing the poly(oxyperfluoroalkylene) group preferably has a structure represented by the following formula [4]. [ka] In formula [4], n represents the total number of the repeating units -[CF2CF2O]- and the repeating units -[CF2O]-, and is preferably an integer in the range of 5 to 30, and more preferably an integer in the range of 7 to 21. The ratio of the number of the repeating units -[CF2CF2O]- to the number of the repeating units -[CF2O]- is preferably in the range of 2:1 to 1:2, and more preferably in the range of about 1:1. The bonds of these repeating units may be either block bonds or random bonds.

[0032] Examples of the active energy ray polymerizable group include (meth)acryloyl group and vinyl group. (b) Perfluoropolyether is not limited to those having one active energy ray polymerizable group at the end of the molecular chain containing poly(oxyperfluoroalkylene) group, but may have two or more active energy ray polymerizable groups. Examples of the end structure containing active energy ray polymerizable group include the structures of formulas [A1] to [A5] shown below, and structures in which the acryloyl group in these structures is replaced with a methacryloyl group. Among these structures, the structures of formulas [A3], [A4] and [A5] having two or more active energy ray polymerizable groups, and structures in which the acryloyl group in these structures is replaced with a methacryloyl group are preferred. [ka]

[0033] In the curable composition of the present invention, the content of (b) perfluoropolyether is 0.05 to 10 parts by mass, preferably 0.05 to 5 parts by mass, based on 100 parts by mass of (a) urethane (meth)acrylate. When the content of (b) perfluoropolyether is 0.05 parts by mass or more, sufficient scratch resistance can be imparted to the hard coat layer, and when the content of (c) perfluoropolyether is 10 parts by mass or less, it is sufficiently compatible with (a) urethane (meth)acrylate, and a hard coat layer with less cloudiness can be obtained.

[0034] In addition, (b) perfluoropolyether can be used alone or in combination of two or more. When combining two or more, perfluoropolyether may be included that has an active energy ray polymerizable group via urethane bond at one end (one end) of molecular chain containing poly(oxyperfluoroalkylene) group, and has a hydroxyl group at the other end (other end) of the molecular chain. In addition, (b) perfluoropolyether can be added with the condition that it does not have a poly(oxyalkylene) group between the poly(oxyperfluoroalkylene) group and the urethane bond, and between the poly(oxyperfluoroalkylene) group and the hydroxyl group.

[0035] [(c) Polymerization initiator] The (c) polymerization initiator preferred in the curable composition of the present invention is, for example, a polymerization initiator that generates radicals when exposed to active energy rays such as electron beams, ultraviolet rays, and X-rays, particularly when exposed to ultraviolet rays.

[0036] Examples of the (c) polymerization initiator include benzoins, alkylphenones, thioxanthones, azos, azides, diazos, o-quinone diazides, acylphosphine oxides, oxime esters, organic peroxides, benzophenones, biscoumarins, bisimidazoles, titanocenes, thiols, halogenated hydrocarbons, trichloromethyltriazines, and onium salts such as iodonium salts and sulfonium salts. These polymerization initiators may be used alone or in combination of two or more. In the present invention, from the viewpoints of transparency, surface curability, and thin film curability, it is preferable to use alkylphenones as the (c) polymerization initiator. By using alkylphenones, a cured film with improved scratch resistance can be obtained.

[0037] Examples of the alkylphenones include α-hydroxyalkylphenones such as 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 2-hydroxy-1-(4-(2-hydroxyethoxy)phenyl)-2-methylpropan-1-one, and 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)-2-methylpropan-1-one; α-aminoalkylphenones such as 2-methyl-1-(4-(methylthio)phenyl)-2-morpholinopropan-1-one and 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butan-1-one; 2,2-dimethoxy-1,2-diphenylethan-1-one; and methyl phenylglyoxylate.

[0038] In the curable composition of the present invention, the content of the polymerization initiator (c) is 1 to 20 parts by mass, preferably 2 to 10 parts by mass, based on 100 parts by mass of the urethane (meth)acrylate (a).

[0039] [(d) Antistatic agent] The curable composition of the present invention may contain an optional component (d) an antistatic agent. An example of the antistatic agent (d) is an antistatic agent containing metal oxide particles. As the metal oxide particles, fine particles having a primary particle diameter of 4 nm to 100 nm can be used. By setting the primary particle diameter of the metal oxide particles within the above numerical range, antistatic properties can be imparted without affecting scratch resistance and extensibility, and a cured film that leads to realization of transparency can be obtained. In the present invention, the primary particle diameter of the metal oxide particles refers to the particle diameter of each particle observed using a transmission electron microscope.

[0040] The metal oxide particles may contain at least one oxide of an element selected from the group consisting of tin, zinc, and indium.Specific examples include tin oxide (SnO2), tin-doped indium oxide (ITO), fluorine-doped tin oxide (FTO), antimony-doped tin oxide (ATO), phosphorus-doped tin oxide (PTO), gallium-doped zinc oxide (GZO), aluminum-doped zinc oxide (AlZO), antimony-doped zinc oxide (AZO), indium-doped zinc oxide or zinc oxide-doped indium oxide (IZO), and indium gallium zinc oxide (IGZO).Among these, the oxide of the above element to which a dopant is added is preferred as an antistatic agent, and phosphorus-doped tin oxide (PTO) is particularly preferred.

[0041] The above-mentioned metal oxide particles can also include surface-coated metal oxide particles having a metal oxide core and the surface of which is coated with an acidic or basic oxide. Examples of the core can include the above-mentioned metal oxide particles such as tin oxide, as well as titanium oxide, titanium oxide-tin oxide complex, zirconium oxide-tin oxide complex, tungsten oxide-tin oxide complex, and titanium oxide-zirconium oxide-tin oxide complex. Examples of the acidic or basic oxide can include antimony pentoxide, silicon oxide-antimony pentoxide complex, and silicon oxide-tin oxide complex.

[0042] In the present invention, when the (d) antistatic agent is contained, the content thereof is 10 to 55 parts by mass relative to 100 parts by mass of the (a) urethane (meth)acrylate. The (d) antistatic agent may be used alone or in combination of two or more kinds.

[0043] [(e) Solvent] The curable composition of the present invention may contain a solvent (e) as an optional component, i.e., may be in the form of a varnish. The solvent (e) may be appropriately selected in consideration of the solubility and dispersibility of the components (a) to (c) and the optional component (d), as well as the workability during application of the curable composition for forming a cured film (hard coat layer) described below, drying properties before and after curing, etc.

[0044] Examples of the solvent (e) include aromatic hydrocarbons such as benzene, toluene, xylene, ethylbenzene, and tetralin; aliphatic or alicyclic hydrocarbons such as n-hexane, n-heptane, mineral spirits, and cyclohexane; halides such as methyl chloride, methyl bromide, methyl iodide, dichloromethane, chloroform, carbon tetrachloride, trichloroethylene, perchloroethylene, and o-dichlorobenzene; esters or ester ethers such as ethyl acetate, propyl acetate, butyl acetate, methoxybutyl acetate, methyl cellosolve acetate, ethyl cellosolve acetate, and propylene glycol monomethyl ether acetate (PGMEA); diethyl ether, tetrahydrofuran (THF), 1,4-dioxane, methyl cellosolve, ethyl cellosolve, butyl cellosolve, propylene glycol monomethyl ether, propylene glycol monoethyl ether, and the like. Examples of the solvent include ethers such as polypropylene glycol ether (PGME), propylene glycol mono-n-propyl ether, propylene glycol monoisopropyl ether, and propylene glycol mono-n-butyl ether; ketones such as acetone, methyl ethyl ketone (MEK), methyl isobutyl ketone (MIBK), di-n-butyl ketone, and cyclohexanone; alcohols such as methanol, ethanol, n-propanol, isopropyl alcohol, n-butanol, isobutyl alcohol, tert-butyl alcohol, 2-ethylhexyl alcohol, benzyl alcohol, and ethylene glycol; amides such as N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), and N-methyl-2-pyrrolidone (NMP); and sulfoxides such as dimethyl sulfoxide (DMSO), as well as mixtures of two or more of these solvents.

[0045] In the curable composition of the present invention, the content of the (e) solvent is not particularly limited, but is, for example, a concentration such that the solid content concentration of the curable composition of the present invention is 1% by mass to 70% by mass, preferably 5% by mass to 50% by mass. Here, the solid content concentration (also referred to as non-volatile content concentration) represents the content of solids (all components excluding the solvent component) relative to the total mass (total mass) of the (a) to (c) components of the curable composition of the present invention, the (d) component which is an optional component, and other additives.

[0046] <Cured film> The curable composition of the present invention can be applied (coated) on a substrate to form a coating film, and the coating film can be polymerized (cured) by irradiating the coating film with active energy rays to form a cured film, which is also the subject of the present invention. In addition, the above-mentioned cured film can be used as a hard coat layer in a hard coat film described later.

[0047] Examples of the substrate include various resins (polycarbonate, polymethacrylate, polystyrene, polyesters such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), polyurethane, thermoplastic polyurethane (TPU), polyolefin, polyamide, polyimide, epoxy resin, melamine resin, triacetyl cellulose (TAC), acrylonitrile-butadiene-styrene copolymer (ABS), acrylonitrile-styrene copolymer (AS), norbornene resin), metal, wood, paper, glass, and slate. The shape of these substrates may be a plate, a film, or a three-dimensional molded product.

[0048] The coating method on the substrate may be appropriately selected from cast coating, spin coating, blade coating, dip coating, roll coating, spray coating, bar coating, die coating, inkjet printing, printing (letterpress printing, intaglio printing, lithographic printing, screen printing, etc.), among which the roll-to-roll method can be used. From the viewpoint of thin film coating, it is preferable to use letterpress printing, particularly gravure coating. It is preferable to filter the curable composition of the present invention using a filter having a pore size of about 0.2 μm before coating. When coating, a solvent may be further added to the curable composition as necessary. Examples of the solvent in this case include the various solvents listed in [(e) Solvent] above.

[0049] After the curable composition of the present invention is applied onto a substrate to form a coating film, the coating film is pre-dried with a heating means such as a hot plate or oven as necessary to remove the solvent (solvent removal step). The conditions for the heat drying at this time are preferably, for example, 40°C to 120°C and about 30 seconds to 10 minutes. After drying, the coating film is cured by irradiating it with active energy rays such as ultraviolet rays. Examples of active energy rays include ultraviolet rays, electron beams, and X-rays, and ultraviolet rays are particularly preferred. Examples of light sources used for ultraviolet irradiation include sunlight, chemical lamps, low-pressure mercury lamps, high-pressure mercury lamps, metal halide lamps, xenon lamps, and UV-LEDs. Furthermore, the polymerization may be completed by performing post-baking, specifically by heating using a heating means such as a hot plate or oven.

[0050] The thickness of the cured film formed after drying and curing is usually 0.1 to 50 μm, preferably 0.5 to 20 μm.

[0051] <Hard coat film> The curable composition of the present invention can be used to produce a hard coat film having a hard coat layer on at least one side (surface) of a film substrate. The hard coat film is also an object of the present invention, and the hard coat film is suitably used to protect the surfaces of various display elements such as touch panels and liquid crystal displays.

[0052] The hard coat layer in the hard coat film of the present invention can be formed by a method including a step of applying the curable composition of the present invention onto a film substrate to form a coating film, a step of removing the solvent by heating as necessary, and a step of irradiating the coating film with active energy rays such as ultraviolet rays to cure the coating film. A method for producing a hard coat film having a hard coat layer on at least one side of a film substrate, including these steps, is also within the scope of the present invention.

[0053] The film substrate may be any of the transparent resin films usable for optical applications among the substrates listed in the above-mentioned <Cured film>. Preferred resin films include, for example, films of polyesters such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), and polyethylene naphthalate (PEN), polyurethane, thermoplastic polyurethane (TPU), polycarbonate, polymethacrylate, polystyrene, polyolefin, polyamide, polyimide, and triacetyl cellulose (TAC).

[0054] The method for applying the curable composition of the present invention onto the film substrate (coating film forming step) and the method for irradiating the coating film with active energy rays (curing step) can be the methods listed in the above-mentioned <cured film>. When the curable composition of the present invention contains a solvent (in the form of a varnish), the coating film may be dried to remove the solvent after the coating film forming step, if necessary. In this case, the method for drying the coating film (solvent removal step) listed in the above-mentioned <cured film> can be used.

[0055] The hard coat layer thus obtained has a thickness (film thickness) of, for example, 1 μm to 20 μm, and preferably 1 μm to 10 μm. EXAMPLES

[0056] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples. In the examples, the apparatus and conditions used for preparing samples and analyzing physical properties are as follows.

[0057] (1) Coating with a bar coater Equipment: PM-9050MC manufactured by SMT Co., Ltd. Bar: OSG System Products Co., Ltd. A-Bar OSP-22, maximum wet film thickness 22μm (equivalent to wire bar #9) Coating speed: 4m / min (2) Oven Equipment: Sanki Instruments Co., Ltd. 2-layer clean oven (upper and lower type) PO-250-45-D (3)UV curing Equipment: Heraeus CV-110QC-G Lamp: Heraeus H-bulb electrodeless lamp (4) Gel Permeation Chromatography (GPC) Equipment: Tosoh Corporation HLC-8220GPC Column: Shodex (registered trademark) GPC K-804L, GPC K-805L manufactured by Showa Denko K.K. Column temperature: 40℃ Eluent: Tetrahydrofuran Detector: RI (5) Scratch test Equipment: Reciprocating wear tester TRIBOGEAR TYPE:30S manufactured by Shinto Scientific Co., Ltd. Scanning speed: 5,000 mm / min Scanning distance: 50mm (6) Tensile test Equipment: Shimadzu Corporation, tabletop precision universal testing machine Autograph AGS-10kNX Grip: 1kN manual screw type flat grip Grip teeth: High-strength rubber-coated grip teeth Pulling speed: 10mm / min Measurement temperature: 23℃ (7) Surface resistance measurement Equipment: Mitsubishi Chemical Corporation high resistivity meter Hiresta UP MCP-HT450 Probe: URS probe Cashier table: UFL Applied voltage: 10V

[0058] The abbreviations have the following meanings: Polyfunctional acrylate having one hydroxy group (a1-1): Dipentaerythritol pentaacrylate / hexaacrylate mixture [Aronix (registered trademark) M-403 manufactured by Toagosei Co., Ltd., pentaacrylate ratio 50% to 60% (catalog value), estimated hydroxyl value = 63.3 mg KOH / g (calculated assuming pentaacrylate 55% and hexaacrylate 45%)] Allophanate polyisocyanates (a2-1): Allophanate modified hexamethylene diisocyanate [Duranate (registered trademark) A201H, Asahi Kasei Chemicals Corporation, isocyanate group content = 17.2 mass%, bifunctional] Biuret polyisocyanate (a2-2): Biuret modified hexamethylene diisocyanate [Duranate (registered trademark) 24A-100, Asahi Kasei Chemicals Corporation, isocyanate group content = 23.5 mass%, trifunctional] Isocyanurate polyisocyanates (a2-3): Isocyanurate modified hexamethylene diisocyanate [Duranate (registered trademark) TLA-100, Asahi Kasei Chemicals Corporation, isocyanate group content = 23.3 mass%, trifunctional] Adduct polyisocyanate (a2-4): Adduct modified product of hexamethylene diisocyanate [Duranate (registered trademark) P301-75E, manufactured by Asahi Kasei Chemicals Corporation, isocyanate group content = 12.5 mass%, bifunctional] PFPE: Perfluoropolyether having two hydroxyl groups at each end without a poly(oxyalkylene) group [Fomblin (registered trademark) T4, manufactured by Solvay Specialty Polymers] BEI: 1,1-bis(acryloyloxymethyl)ethyl isocyanate [Karenz (registered trademark) BEI, manufactured by Showa Denko K.K.] DOTDD: Dioctyltin dineodecanoate [Neostan (registered trademark) U-830, manufactured by Nitto Kasei Co., Ltd.] SM2: Perfluoropolyether urethane acrylate having a total of four acryloyl groups at both ends [FLUOROLINK (registered trademark) AD-1700, manufactured by Solvay Specialty Polymers, 70% by weight non-volatile solution] SM3: Polydimethylsiloxane having a methacryloyl group at one end [Silaplane (registered trademark) FM-0721, manufactured by JNC Corporation] O2959: 2-hydroxy-1-(4-(2-hydroxyethoxy)phenyl)-2-methylpropan-1-one [OMNIRAD (registered trademark) 2959, manufactured by IGM Resins] MEK: Methyl ethyl ketone MeOH: Methanol Antistatic agent d-1: Phosphorus-doped tin oxide 20% by mass dispersion sol in isopropyl alcohol [Nissan Chemical Co., Ltd., Celnax (registered trademark) CX-S204IP, primary particle diameter: 5 nm to 20 nm, secondary particle diameter: 10 nm to 20 nm] *The primary particle size and secondary particle size here refer to the average particle size measured by observation with a transmission electron microscope. The particle size was measured by dropping the sol onto a copper mesh, drying it, and observing it with a transmission electron microscope (JEM-1020, manufactured by JEOL Ltd.) at an accelerating voltage of 100 kV, and averaging the measurements of 100 particles to obtain the average primary particle size. Antistatic agent D-2: A 30% by mass methanol dispersion sol of core-shell particles with a primary particle diameter of 30 to 40 nm, in which the core is made of tin oxide and the surface is coated with antimony pentoxide [Nissan Chemical Co., Ltd., Celnax (registered trademark) HX-307M1]

[0059] [Production Example 1] Production of surface modifier SM1 In a screw tube, 1.19g (0.5mmol) of PFPE, 0.52g (2.0mmol) of BEI, 0.017g of DOTDD (0.01 times the total mass of PFPE and BEI), and 1.67g of MEK were charged. This mixture was stirred for 72 hours at room temperature (approximately 23°C) using a stirrer tip to obtain a 50% by mass MEK solution of the target compound, the surface modifier. The weight average molecular weight: Mw of the obtained SM1 measured in terms of polystyrene by GPC was 3,000, and the dispersity: Mw (weight average molecular weight) / Mn (number average molecular weight) was 1.2.

[0060] [How to determine the amount of isocyanate to be used when manufacturing urethane acrylate] When a polyfunctional acrylate (a1-1) having one hydroxy group is reacted with various polyisocyanates (a2-1) to (a2-4) to produce a urethane acrylate, the amount of the polyisocyanate to be charged was calculated using [hydroxyl value of (a1-1) / 561) × (42 × 100 / isocyanate group content) × [amount of (a1-1) / 100] × (number of NCO groups / number of OH groups).

[0061] [Production Example 2] Production of urethane acrylate UA1 In a screw tube, 10 g of (a1-1) and 2.76 g of allophanate polyisocyanate (a2-1) were charged so that the number of OH groups / the number of NCO groups = 1, and 0.13 g of DOTDD [0.01 times the total mass of (a1-1) and (a2-1)] and 3.22 g of MEK were further charged. The resulting mixture was stirred at room temperature (approximately 23°C) using a stirrer tip until it reached the 2260 cm3 value indicating the isocyanate group. -1 After stirring until the infrared absorption spectrum of disappeared, an 80 mass % MEK solution of the target compound, urethane acrylate UA1, was obtained.

[0062] [Production Example 3] Production of urethane acrylate UA2 In a screw tube, 10 g of (a1-1) and 3.02 g of biuret polyisocyanate (a2-2) were charged so that the number of OH groups / the number of NCO groups was 2 / 3, and 0.13 g of DOTDD [0.01 times the total mass of (a1-1) and (a2-2)] and 2.96 g of MEK were further charged. The resulting mixture was stirred using a stirrer tip at room temperature (approximately 23°C) for about 3 hours, after which 0.33 g of MeOH was charged to eliminate the remaining isocyanate groups, and the 2260 cm3 indicating the isocyanate groups was measured at room temperature (approximately 23°C). -1 After stirring until the infrared absorption spectrum of disappeared, an 80 mass % MEK / MeOH solution of the target compound, urethane acrylate UA2, was obtained.

[0063] [Production Example 4] Production of urethane acrylate UA3 In a screw tube, 10 g of (a1-1) and 3.05 g of isocyanurate polyisocyanate (a2-3) were charged so that the number of OH groups / the number of NCO groups was 2 / 3, and 0.13 g of DOTDD [0.01 times the total mass of (a1-1) and (a2-3)] and 2.97 g of MEK were further charged. The resulting mixture was stirred using a stirrer tip at room temperature (approximately 23°C) for about 3 hours, after which 0.33 g of MeOH was charged to eliminate the remaining isocyanate groups, and the 2260 cm3 indicating the isocyanate groups was measured at room temperature (approximately 23°C). -1 After stirring until the infrared absorption spectrum of disappeared, an 80 mass % MEK / MeOH solution of the target compound, urethane acrylate UA3, was obtained.

[0064] [Production Example 5] Production of urethane acrylate UA4 In a screw tube, 10 g of (a1-1) and 3.73 g of adduct polyisocyanate (a2-4) were charged so that the number of OH groups / the number of NCO groups = 1, and 0.14 g of DOTDD [0.01 times the total mass of (a1-1) and (a2-4)] and 3.47 g of MEK were further charged. The resulting mixture was stirred at room temperature (approximately 23°C) using a stirrer tip until it reached the 2260 cm3 value indicating the isocyanate group. -1After stirring until the infrared absorption spectrum of disappeared, an 80 mass % MEK solution of the target compound, urethane acrylate UA4, was obtained.

[0065] [Examples 1 to 4, Comparative Examples 1 to 3] The components shown in Table 1 were mixed to prepare a curable composition having a solid content concentration shown in Table 1. The solid content here refers to components other than the solvent. In addition, in Table 1, [parts] refers to [parts by mass]. In addition, the urethane acrylate and the surface modifier in Table 1 each represent a solid content.

[0066] [Table 1]

[0067] These curable compositions were applied to an A4 size double-sided easy-adhesion treated PET film [Lumirror (registered trademark) U403, manufactured by Toray Industries, Inc., thickness 100 μm] using a bar coater to obtain a coating film. This coating film was dried in an oven at 80° C. for 3 minutes to remove the solvent. The obtained film was exposed to light at a dose of 300 mJ / cm under a nitrogen atmosphere. 2 A hard coat film having a hard coat layer (cured film) was produced by exposing the film to UV light.

[0068] The homogeneity of each curable composition, and the scratch resistance and stretchability of the obtained hard coat film were evaluated. The evaluation procedures are shown below. The results are also shown in Table 2. [Composition homogeneity] The appearance of the curable composition was visually inspected 2 hours after preparation and evaluated according to the following criteria. A: Clear solution (no floating matter or sediment) C: Both floating matter and sediment are present [Scratch resistance] The surface of the hard coat layer of the obtained hard coat film was rubbed 10 times with steel wool [BONSTAR (registered trademark) #0000 (ultrafine)] attached to a reciprocating abrasion tester, with a stroke of 60 mm, and the load shown in Table 2. Thereafter, the degree of damage in the area excluding the range of 5 mm on both ends of the stroke of 60 mm was visually confirmed and evaluated according to the following criteria A, B, and C. Note that, when assuming actual use as a hard coat layer, at least B is required, and A is preferable. A: No scratches (0 scratches) B: Scratches (1 to 4 scratches less than 5 mm long) C: Scratches (5 or more scratches less than 5 mm long, or 1 or more scratches 5 mm long or longer) [Stretchability] The obtained hard-coated film was cut into a rectangle of 60 mm in length and 10 mm in width to prepare a test piece. The test piece was attached to the grip of a universal testing machine so that 20 mm was gripped from each end in the longitudinal direction, and a tensile test was performed at 1% intervals so that the stretch ratio (= (increase in the distance between the grippers) ÷ (distance between the grippers) × 100) was 4%, 5%, and 6%. The hard-coated film after the tensile test was visually observed to confirm the maximum stretch ratio at which no cracks occurred in the hard-coated layer of the test piece. The stretch ratio of Comparative Example 1 was set to 100, and the stretchability was calculated based on this.

[0069] [Table 2]

[0070] As shown in Table 1, the curable compositions of Examples 1 to 4 contain urethane acrylate UA1, UA2, or UA3 obtained by using the compound represented by the formula [1'], the compound represented by the formula [2'], or the compound represented by the formula [3'] as an isocyanate compound, and perfluoropolyether SM1 or SM2 having acryloyl groups at both ends of the molecular chain via urethane bonds as a surface modifier. On the other hand, the curable composition of Comparative Example 1 contains urethane acrylate UA4 obtained by using an adduct polyisocyanate that is a compound not represented by the formulas [1'] to [3'] as an isocyanate compound, and SM1 as a surface modifier. And as shown in Table 2, the hard coat film having a hard coat layer obtained from the curable composition of Examples 1 to 4 exhibited better scratch resistance and showed equal or greater stretchability than the hard coat film having a hard coat layer obtained from the curable composition of Comparative Example 1.

[0071] The adduct structure skeleton of the adduct polyisocyanate, which is a compound not represented by the formula [1'] to formula [3'], is easily deformed by external forces because the ether moiety in the urethane bond has a high degree of rotational freedom, and therefore the molecular chain of the urethane acrylate UA4 is easily broken and is considered to have poor scratch resistance. On the other hand, the structure skeleton of the isocyanate compound represented by the formula [1'] to formula [3'] has a urea bond that does not have an ether moiety, so it is difficult to deform by external forces, and the urethane acrylates UA1 to UA3 are considered to have excellent scratch resistance. Among them, the hard coat film having a hard coat layer obtained from the curable composition of Example 1 and Example 4 containing the urethane acrylate UA1 obtained by using the compound represented by the formula [1'] as the isocyanate compound was shown to have the best stretchability while maintaining excellent scratch resistance. The structure of the isocyanate compound represented by the formula [1'] has both a urethane bond and a urea bond. In addition, R 0It is presumed that the monohydric alcohol residue represented by the formula has a high degree of rotational freedom and can mitigate the applied external force as thermal energy. Therefore, it is considered that urethane acrylate UA1 has the best stretchability while maintaining excellent scratch resistance.

[0072] On the other hand, the curable composition of Comparative Example 2 contains urethane acrylate UA1 and polydimethylsiloxane SM3 having a methacryloyl group at one end as a surface modifier, but the compatibility of the surface modifier SM3 is poor, and a good composition could not be obtained. Furthermore, the hard coat film having a hard coat layer obtained from the curable composition of Comparative Example 3 not containing a surface modifier was shown to have inferior scratch resistance compared to the hard coat films having hard coat layers obtained from the curable compositions of Examples 1 to 4.

[0073] [Examples 5 and 6] The components shown in Table 3 were mixed to prepare a curable composition having a solid content concentration shown in Table 3. The solid content here refers to components other than the solvent and the dispersion medium. In Table 3, [parts] refers to [parts by mass] and [%] refers to [% by mass]. In Table 3, the urethane acrylate, surface modifier, and antistatic agent each refer to a solid content.

[0074] [Table 3]

[0075] These curable compositions were applied to an A4 size double-sided easy-adhesion treated PET film [Lumirror (registered trademark) U403, manufactured by Toray Industries, Inc., thickness 100 μm] using a bar coater to obtain a coating film. This coating film was dried in an oven at 60° C. for 3 minutes to remove the solvent. The obtained film was exposed to light at a dose of 300 mJ / cm under a nitrogen atmosphere. 2 By exposing the film to UV light, a hard coat film having a hard coat layer (cured film) with a layer thickness (film thickness) of approximately 4 μm was produced.

[0076] The obtained hard coat film was evaluated for the above-mentioned [scratch resistance] and [stretchability], as well as for the surface resistance. The procedure for evaluating the surface resistance is shown below. The results are shown in Table 4. [Surface resistance] The hard coat film was placed on the register table of a high resistivity meter with the hard coat layer surface facing up, and the probe was pressed against the hard coat film (hard coat layer). The value after 10 seconds was measured three times, and the average value was taken as the surface resistance value [Ω / □].

[0077] [Table 4]

[0078] As shown in Tables 3 and 4, the hard coat films having a hard coat layer obtained from the curable compositions of Examples 5 and 6 using antistatic agents d-1 and d-2 exhibited excellent scratch resistance and stretchability, as well as antistatic properties.

Claims

1. (a) 100 parts by mass of at least one urethane (meth)acrylate having a partial structure represented by the following formula [1]: (b) 0.05 to 10 parts by mass of a perfluoropolyether having an active energy ray-polymerizable group at the end of a molecular chain containing a poly(oxyperfluoroalkylene) group, and (c) 1 to 20 parts by mass of a polymerization initiator that generates radicals when exposed to active energy rays A curable composition comprising: A curable composition in which the (a) urethane (meth)acrylate is a reaction product of (a1) a (meth)acrylate compound having at least one hydroxy group and (a2) at least one isocyanate compound represented by the following formula [1'] (however, this does not include a curable composition containing a polymerizable unsaturated group-containing monomer having no hydroxyl group and having a solubility parameter of 9 to 13 (cal / cm 3 ) 1 / 2 , a molecular weight of 350 or less, and a viscosity at 25° C. of 30 mPa·s or less). 【Chemistry 1】 (In the above formula, R1 represents a divalent hydrocarbon group having 4 to 15 carbon atoms, R 0 represents a residue of a monohydric alcohol. 【Chemistry 2】 (In the above formula, R 0 and R 1 are defined as in formula [1] above.)

2. The curable composition according to claim 1 , wherein the perfluoropolyether (b) has an active energy ray-polymerizable group via a urethane bond at an end of a molecular chain containing the poly(oxyperfluoroalkylene) group.

3. The curable composition according to claim 1 or 2, wherein the (b) perfluoropolyether has at least two active energy ray-polymerizable groups via urethane bonds at an end of a molecular chain containing the poly(oxyperfluoroalkylene) group.

4. The curable composition according to any one of claims 1 to 3, wherein the (b) perfluoropolyether has at least two active energy ray-polymerizable groups via urethane bonds at each of both ends of a molecular chain containing the poly(oxyperfluoroalkylene) group.

5. The poly(oxyperfluoroalkylene) group of the perfluoropolyether (b) is a repeating unit -[CF 2 O]- and repeating unit -[CF 2 CF 2 The curable composition according to any one of claims 1 to 4, wherein the repeating units are bonded together by block bonds, random bonds, or both block bonds and random bonds.

6. The curable composition according to claim 5 , wherein the molecular chain containing the poly(oxyperfluoroalkylene) group has a structure represented by the following formula [4]: 【Chemistry 3】 (In the above formula [4], n represents the repeating unit -[CF 2 CF 2 O]- and the number of repeating units -[CF 2 The total number of the repeating units -[CF 2 CF 2 O]- and the repeating unit -[CF 2 O]- is bonded by block bonds, random bonds, or block bonds and random bonds.

7. The curable composition according to claim 1 , further comprising: (d) 10 to 55 parts by weight of an antistatic agent.

8. The curable composition of claim 7 , wherein the (d) antistatic agent comprises metal oxide particles.

9. 9. The curable composition of claim 8, wherein the metal oxide particles comprise an oxide of at least one element selected from the group consisting of tin, zinc, and indium.

10. 10. The curable composition of claim 9, wherein the metal oxide particles comprise optionally doped tin oxide.

11. The curable composition according to claim 8 , wherein the metal oxide particles include at least one of phosphorus-doped tin oxide and tin oxide having a surface coated with antimony pentoxide.

12. The curable composition according to claim 1 , further comprising: (e) a solvent.

13. A cured film obtained from the curable composition according to any one of claims 1 to 12.

14. A hard coat film comprising a hard coat layer on at least one surface of a film substrate, the hard coat layer comprising the cured film according to claim 13.

15. 13. A hard coat film comprising a hard coat layer on at least one surface of a film substrate, the hard coat layer being formed by a method including the steps of: applying the curable composition according to claim 1 onto a film substrate to form a coating film; and irradiating the coating film with active energy rays to cure the coating film.

16. 13. A hard coat film comprising a hard coat layer on at least one surface of a film substrate, the hard coat layer being formed by a method including the steps of: applying the curable composition according to claim 12 onto a film substrate to form a coating film; removing the solvent from the coating film by heating; and irradiating the coating film with active energy rays to cure the coating film.

17. 17. The hard coat film according to claim 14, wherein the hard coat layer has a thickness of 1 μm to 10 μm.

18. A method for producing a laminate, comprising: applying the curable composition according to claim 1 onto a film substrate to form a coating film; and irradiating the coating film with active energy rays to cure the coating film.

Citation Information

Patent Citations

  • Composition for hard coat and molded product in which hard coat layer is formed

    JP2011190343A

  • Curable resin composition

    JP2012241060A

  • Photocurable resin composition and optical film using the same

    JP2016074884A

  • Photocurable resin composition, cured coating film formed from the composition and substrate with coating film, and method for producing cured coating film and substrate with coating film

    JP2016125049A

  • Curable composition for flexible coating

    WO2020008937A1