Cutting Tools

WC-based cemented carbide tools with optimized binder phase distribution and Σ2-compatible grain boundaries address the issue of plastic deformation resistance, resulting in extended tool life during high-load cutting operations.

JP7587205B2Active Publication Date: 2024-11-20MITSUBISHI MATERIALS CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2021003953
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-14
Publication Date
2024-11-20
Estimated Expiration
2041-01-14

AI Technical Summary

Technical Problem

Conventional WC-based cemented carbide tools exhibit insufficient plastic deformation resistance during continuous cutting of materials like steel and stainless steel, particularly under high loads, leading to premature tool failure.

Method used

The WC-based cemented carbide tools are designed with specific binder phase particle size distribution and increased Σ2-compatible grain boundaries, along with controlled compositions of Co, Cr, and optional additives like TaC, NbC, TiC, and ZrC, to enhance plastic deformation resistance and tool life.

Benefits of technology

The tools demonstrate improved plastic deformation resistance and extended tool life during continuous cutting of stainless steel and similar materials, reducing chipping and deformation, thereby enhancing durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587205000001
    Figure 0007587205000001
  • Figure 0007587205000002
    Figure 0007587205000002
  • Figure 0007587205000003
    Figure 0007587205000003
Patent Text Reader

Abstract

To provide a WC-based carbide tool and a surface-coated WC-based carbide tool, which demonstrate excellent plastic deformation resistance in continuous cutting alloy steel or the like.SOLUTION: Provided is a WC-based cemented carbide cutting tool, having Co:6.0-14.0 mass%, Cr3C2:0.1-1.4 mass%, and the balance WC with inevitable impurities, or further, containing 4.0 mass% or less in total of one or more of TaC, NbC, TiC and ZrC. In the WC-based cemented carbide alloy cutting tool, in a grain size distribution of a binder phase on the cemented carbide alloy cross section, a cumulative 10% grain area A10 is 0.15 μm2 to 0.30 μm2, and a cumulative 90% grain area A90 / A10 is 15.0 to 50.0, and further, in the WC-based cemented carbide alloy cutting tool, the average grain size of the WC is 0.2 μm to 4.0 μm, an existence ratio (a ratio of Σ2 corresponding grain boundaries) of Σ2 corresponding grain boundaries of WC in all WC / WC grain boundaries is 15% or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cutting tool made of a WC-based cemented carbide (also referred to as a "WC-based cemented carbide tool") and a surface-coated WC-based cemented carbide cutting tool (also referred to as a "surface-coated WC-based cemented carbide tool") that exhibits excellent resistance to plastic deformation in continuous cutting (e.g., continuous turning) of alloy steel and the like (steel, stainless steel, Ni-based alloy, etc.). [Background technology]

[0002] WC-based cemented carbide has high hardness and toughness, and therefore WC-based cemented carbide tools and surface-coated WC-based cemented carbide tools using this alloy as a base exhibit excellent wear resistance and are known as cutting tools having a long life over long periods of use. However, in recent years, various proposals have been made to further improve the cutting performance and tool life of WC-based cemented carbide tools depending on the type of work material, cutting conditions, etc.

[0003] For example, Patent Document 1 proposes that in a cemented carbide alloy having a hard phase mainly composed of tungsten carbide and a binder phase mainly composed of an iron group element (including cobalt, the cobalt content of which is preferably 8 mass % or more in the cemented carbide alloy), when the number of tungsten carbide particles is A and the number of tungsten carbide particles having one or less contact points with other tungsten carbide particles is B, by satisfying B / A≦0.05, the plastic deformation resistance of the cemented carbide alloy is improved, and as a result, the life of a WC-based cemented carbide tool is extended in wet continuous cutting of carbon steel and stainless steel.

[0004] In Patent Document 2, in a WC-based cemented carbide tool containing 10 to 13 mass% Co, a ratio of 2 to 8% Cr to Co, at least one of TaC and NbC in a range such that the total amount of TaC and NbC is 0.2 to 0.5 mass%, with the remainder being WC, and having a hardness of 88.6 HRA to 89.5 HRA, it is proposed that the ratio D80 / D20 of the WC cumulative grain size 80% diameter D80 to the cumulative grain size 20% diameter D20 in the area ratio on the polished surface is set to a range of 2.0≦D80 / D20≦4.0, D80 is set to a range of 4.0 to 7.0 μm, and the WC adhesion degree c is set to 0.36≦c≦0.43, thereby preventing adhesion of the workpiece and improving chipping resistance in cutting difficult-to-cut materials such as stainless steel.

[0005] In Patent Document 3, when the composition of the WC-based cemented carbide is expressed as WC-x mass %, Co-y mass %, Cr3C2-z mass %, VC, in a WC-based cemented carbide tool, the following conditions are satisfied: 6≦x≦14, 0.4≦y≦0.8, 0≦z≦0.6, (y+z)≦0.1x. In addition, the WC adhesion degree C of the WC-based cemented carbide is expressed as C=1-V b α When expressed as ·exp(0.391·L), the value of the binder phase volume fraction of the WC-based cemented carbide in this formula, V b is 0.11≦V b In addition, the value L of (standard deviation of WC particle size distribution) / (average WC particle size) is within the range of 0.3≦L≦0.7, and the coefficient α satisfies the value of 0.3≦α≦0.55. In this way, a WC-based cemented carbide tool has been proposed that has improved toughness and enhanced chipping resistance without reducing hardness and rigidity in cutting Al alloys, carbon steel, etc.

[0006] In Patent Document 4, when the length of the WC-WC adhesive interface in a WC-based cemented carbide tool is L1 and the length of the WC-Co adhesive interface is L2, R>(0.82-0.086×D)×(10 / V) It has been proposed that the thermal plastic deformation resistance and toughness of WC-based cemented carbide tools can be improved in cutting Ni-based heat-resistant alloys by satisfying the following equation. In addition, R = (L1) / ((L1)+(L2)) D: WC area average particle size (μm), which is in the range of 0.6≦D≦1.7. Here, the above D refers to the particle size of WC when the area ratio of WC is 50%. V: binder phase volume (vol%), which is in the range of 9≦V≦14.

[0007] Patent Document 5 proposes a WC-Co based cemented carbide part for cutting tools, which has a composition by weight consisting of Cr or / and Cr compounds: 0-4% (in terms of Cr), V or / and V compounds: 0-4% (in terms of V), TaC: 0-2%, TiC: 0-2%, N or / and N compounds: 0-1% (in terms of N), Co: 0.1-10%, WC and inevitable impurities: the remainder, and has a Co average thickness (CFP) of 0.06-30 nanometers, and is densified by applying a pressure of 3 atm to 200 atm using gas as a pressure medium in a part or the whole range of the temperature range of 900°C to 1600°C during heating during sintering. It is said that the toughness of this WC-Co based cemented carbide part, preferably an ultrafine grain low Co cemented carbide part having an average WC grain size of 1 μm or less and a CFP in the range of 0.06-30 nm, can be improved. Here, CFP is the average Co thickness (nm), CFP=0.58*A / (100-A)*R where A is Co (wt %) and 2R is the average WC particle size (nm). [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2016-20541 A [Patent Document 2] JP 2017-88999 A [Patent Document 3] JP 2017-148895 A [Patent Document 4] JP 2017-179433 A [Patent Document 5] Japanese Patent Application Publication No. 7-305136 Summary of the Invention [Problem to be solved by the invention]

[0009] According to the conventional WC-based cemented carbide tools proposed in the above Patent Documents 1 to 5, the cutting performance and tool characteristics of the WC-based cemented carbide tools are improved by controlling the number of contact points between WC-WC particles, the particle size of the WC, the degree of WC adhesion, or manufacturing conditions, etc. However, when the conventional tools are used in continuous cutting of steel, alloy steel, stainless steel, and the like, particularly in continuous cutting under high load such as continuous turning, the plastic deformation resistance of the base body is insufficient, and the occurrence of tool deformation and the like cannot be sufficiently suppressed, resulting in a problem that the tool reaches the end of its life. [Means for solving the problem]

[0010] Therefore, the present inventors have focused on the morphology of the binder phase of WC-based cemented carbide alloys and conducted extensive research to develop a WC-based cemented carbide tool that exhibits excellent resistance to plastic deformation in continuous cutting processes under high loads, such as continuous turning processes of steel, alloy steel, stainless steel, and the like, and have obtained the following findings.

[0011] That is, in the WC-based cemented carbide tools shown in the above Patent Documents 1 to 4, improvements were made mainly focusing on WC particles, and in the WC-based cemented carbide tool shown in the above Patent Document 5, improvements were made mainly focusing on CFP. However, the present inventors have changed their viewpoint from the conventional techniques and conducted repeated research focusing on the morphology of the binder phase. As a result, by adjusting the sintering conditions for the binder phase particles (mainly Co particles) of a WC-based cemented carbide, it has been found that when a predetermined number of binder phase particles of an appropriate size are present, that is, in a WC-based cemented carbide, a scanning electron microscope (SEM) observation is performed at a magnification of 500 times, and the area occupied by one binder phase particle at a cumulative 10% particle area of ​​the binder phase calculated by image analysis of the obtained scanning electron microscope (SEM) image is defined as A10 (μm 2 ), and the area occupied by one binder phase particle at 90% cumulative particle area is A90 (μm2 ) when A10 is 0.15μm 2 or more, 0.30μm 2 or less and A90 / A10 satisfies 15.0 or more and 50.0 or less, the plastic deformation resistance is improved, and therefore, when a WC-based cemented carbide tool using such a WC-based cemented carbide substrate is used for continuous cutting of steel, alloy steel, stainless steel, etc., in particular, continuous turning of stainless steel, etc., the tool life can be extended.

[0012] Furthermore, the present inventors have conducted extensive research into maintaining and improving the excellent plastic deformation resistance of WC-based cemented carbide tools using the above-mentioned WC-based cemented carbide substrate, and have found that by increasing the ratio of the Σ2 coincidence grain boundary, which has the least crystal arrangement disorder and the strongest atomic bonds compared to general grain boundaries (random grain boundaries), to the total WC / WC grain boundary length (hereinafter also referred to as the "Σ2 coincidence grain boundary ratio"), it is possible to exhibit better plastic deformation resistance even in continuous cutting processes under high loads, such as continuous turning of the above-mentioned steel, alloy steel, stainless steel, etc., and to achieve a further increase in the tool life.

[0013] The present invention has been made based on the above findings, "(1) In a cutting tool made of WC-based cemented carbide having a WC-based cemented carbide as a substrate, The composition of the WC-based cemented carbide is as follows: Co is 6.0 to 14.0 mass % and Cr3C2 is 0.1 to 1.4 mass % as binder phase forming components, and the remainder is WC and inevitable impurities; WC-based cemented carbide of The particle size distribution of the binder phase in the cross section of the substrate is analyzed, and the area occupied by one binder phase particle at 10% cumulative particle area is defined as A10 (μm 2 ), and the area occupied by one binder phase particle at 90% cumulative particle area is A90 (μm 2 ), A10 is 0.15μm 2 or more, 0.30μm 2and A90 / A10 is 15.0 or more and 50.0 or less. (2) The WC-based cemented carbide cutting tool according to (1), further comprising at least one selected from the group consisting of TaC, NbC, TiC and ZrC in a total amount of 4.0 mass% or less. (3) A cutting tool made of a WC-based cemented carbide according to (1) or (2), characterized in that the average grain size of WC in the WC-based cemented carbide is 0.2 μm or more and 4.0 μm or less, and the presence ratio of Σ2 corresponding grain boundaries of WC to all WC / WC grain boundaries (Σ2 corresponding grain boundary ratio) is 15% or more. (4) A surface-coated WC-based cemented carbide cutting tool, characterized in that a hard coating layer is formed on at least the cutting edge of the WC-based cemented carbide cutting tool according to any one of (1) to (3). The present invention is characterized by the following: The contents of Cr3C2, TaC, NbC, TiC, and ZrC in the above (1) to (4) are the Cr, Ta, Nb, Ti, and Zr amounts measured on a cross section of the WC-based cemented carbide, all of which are calculated as carbide equivalents. In addition, in this specification, when a numerical range is indicated using the symbol "to", it means that the numerical range includes the lower limit and the upper limit. Effect of the Invention

[0014] The WC-based cemented carbide tool and the surface-coated WC-based cemented carbide cutting tool according to the present invention have a specific composition range for the components Co, Cr3C2, and / or TaC, NbC, TiC, and ZrC of the WC-based cemented carbide constituting the substrate, and the particle size distribution of the binder phase is analyzed to define the area occupied by one binder phase particle at 10% cumulative particle area as A10 (μm 2 ), and the area occupied by one binder phase particle at 90% cumulative particle area is A90 (μm 2 ), A10 is 0.15μm 2 or more, 0.30μm 2By satisfying the A90 / A10 ratio of 15.0 or more and 50.0 or less, the plastic deformation resistance is improved and a significant effect of providing a long cutting life is achieved. Furthermore, by setting the average grain size of WC in the WC-based cemented carbide to 0.2 μm or more and 4.0 μm or less, and increasing the ratio of WC Σ2 corresponding grain boundaries to all WC / WC grain boundaries (Σ2 corresponding grain boundary ratio) to 15% or more, or even 25% or more, the plastic deformation resistance is further improved. Therefore, the WC-based cemented carbide tool and surface-coated WC-based cemented carbide tool of the present invention have excellent resistance to plastic deformation in continuous cutting, particularly continuous turning, of steel, alloy steel, stainless steel, and the like. In addition, when the Σ2 corresponding grain boundary ratio is increased, they also have the effect of suppressing chipping, thereby extending the tool life. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The present invention will be described in detail below.

[0016] 1.WC-based cemented carbide Co: Co is contained as a main component for forming the binder phase of the WC-based cemented carbide. If the Co content is less than 6.0 mass%, sufficient toughness cannot be maintained in high-efficiency machining of steel, alloy steel, stainless steel, etc., while if the Co content exceeds 14.0 mass%, the material will soften rapidly, the desired hardness required for a cutting tool will not be obtained, and deformation and wear will progress significantly. Therefore, the Co content in the WC-based cemented carbide is set to 6.0 to 14.0 mass%. The binder phase may contain W and C, which are components of the hard phase, and other unavoidable impurities. The binder phase may contain at least one of Cr, Ta, Nb, Ti and Zr, and when these elements are present in the binder phase, they are presumed to be in a state of solid solution in the binder phase. The mass % of Co can be determined by mirror-finishing any surface or cross section of the cemented carbide and subjecting the machined surface to fluorescent X-ray diffraction measurement.

[0017] Cr3C2: Cr3C2 dissolves as Cr in Co, which forms the main binder phase, and inhibits the growth of the WC phase, which forms the hard phase, refining the grain size of the WC phase, making the WC-based cemented carbide a fine-grained, uniform-grained structure, and improving toughness. However, this effect is insufficient when the Cr3C2 content is less than 0.1 mass%, while when the Cr3C2 content exceeds 10% relative to the Co content, a composite carbide of Cr and W precipitates, reducing toughness and becoming the starting point for chipping. In the present invention, the upper limit of the Co content is 14.0 mass%, so the upper limit of Cr3C2 is The upper limit of the Co content was set at 1.4 mass%, which is 10%. Therefore, the Cr3C2 content in the WC-based cemented carbide is set to 0.1 to 1.4 mass%.

[0018] TaC, NbC, TiC, ZrC: The WC-based cemented carbide of the present invention may further contain, as its components, at least one selected from the group consisting of TaC, NbC, TiC and ZrC in a total amount of 4.0 mass % or less. Ta, Nb, Ti, and Zr all have the effect of increasing hardness by dissolving in Co, which forms the main binder phase. However, if the total content of these elements calculated as carbides exceeds 4.0 mass%, carbides will precipitate, reducing toughness and becoming the starting point for chipping. Therefore, when at least one selected from TaC, NbC, TiC and ZrC is contained as a component in the WC-based cemented carbide, the total content is desirably 4.0 mass % or less. The contents of Cr3C2, TaC, NbC, TiC and ZrC mentioned above are values ​​calculated by converting the amounts of Cr, Ta, Nb, Ti and Zr in the WC-based cemented carbide alloy measured by EPMA into carbide amounts.

[0019] WC: WC is contained as a main component for forming the hard phase of the WC-based cemented carbide. The hard phase may contain unavoidable impurities that are inevitably mixed in during the manufacturing process.

[0020] (1) Average particle size: If the average grain size of WC is less than 0.2 μm, slippage between hard phases during cutting is likely to occur, resulting in insufficient resistance to plastic deformation and chipping. On the other hand, if the average grain size exceeds 4.0 μm, sufficient wear resistance cannot be obtained. Therefore, it is preferable to select the grain size from the range of 0.2 μm or more and 4.0 μm or less. The average grain size of WC is determined by mirror-finishing any surface or cross section of the cemented carbide, observing the machined surface by electron backscatter diffraction (EBSD), determining the area of ​​at least 300 hard phases by image analysis, and calculating the diameter of the circle equal to the area, and averaging the results. For the mirror finishing, for example, a focused ion beam device (FIB device), a cross-section polisher device (CP device), or the like is used.

[0021] (2) Σ2 corresponding grain boundary ratio: The inventors have conducted extensive research to impart excellent plastic deformation resistance to cemented carbide, and have discovered that by increasing the ratio of the Σ2 coincidence grain boundary length, which has the least crystal arrangement disorder and the strongest atomic bonds compared to general grain boundaries (random grain boundaries), to the total WC / WC grain boundary length, i.e., the Σ2 coincidence grain boundary ratio, it is possible to obtain excellent wear resistance and plastic deformation resistance depending on the application. If the Σ2 corresponding grain boundary ratio is less than 15%, the ratio of WC / WC grain boundaries with high grain boundary strength becomes insufficient and fracture resistance is not satisfied, so it is specified to be 15% or more.More preferably, it is 25% or more. The Σ2 coincidence grain boundary ratio can be measured, for example, by using the SEM-EBSD method. That is, in an SEM, multiple fields of view are observed with a pixel size of 0.1 μm × 0.1 μm in a field of view of 24 μm × 72 μm, and the number of WC is 1000 or more, and the grain boundary analyzed by EBSD in which the (0001) planes of adjacent WC have an orientation relationship rotated 90° around the axis of the

[0001] direction or the [1-210] direction is defined as the Σ2 coincidence grain boundary, and the ratio of the Σ2 coincidence grain boundary length to the total WC / WC grain boundary length is calculated. However, according to Brandon's condition, the Σ2 corresponding grain boundary is defined as one that includes an angle range of within 10.6° in both directions from the above-mentioned 90° orientation relationship. Therefore, we defined a Σ2 corresponding grain boundary as one in which the (0001) planes of adjacent WC have an orientation relationship of 79.4° or more and 100.6° or less with respect to the axis of the

[0001] direction or the [1-210] direction.

[0022] Inevitable impurities: As described above, the hard phase and binder phase may contain impurities that are inevitably mixed in during the manufacturing process, and the amount of such impurities is preferably 0.3 mass % or less based on the total mass of the cemented carbide.

[0023] Binder phase particle size distribution: In the present invention, in the WC-based cemented carbide, the binder phase particles are distributed in a coarse and fine mixed grain form, so that the degree of WC / WC adhesion is greatly increased in the regions other than the coarse binder phase, thereby obtaining a structure with excellent resistance to plastic deformation. Specifically, the particle size distribution of the binder phase in a WC-based cemented carbide was analyzed, and the area occupied by one binder phase particle at 10% of the cumulative particle area was defined as A10, and the area occupied by one binder phase particle at 90% of the cumulative particle area was defined as A90. When A10 was 0.15 μm 2 or more, 0.30μm 2 By satisfying the above condition and the A90 / A10 ratio being 15.0 or more and 50.0 or less, the WC skeleton structure is firmly constructed, and the effect of improving the resistance to plastic deformation is obtained. In contrast, A10 is 0.15 μm 2 If A10 is less than 0.30μm, a large amount of fine binder phase is present and a shortage of coarse binder phase occurs, resulting in insufficient plastic deformation resistance. 2 If the temperature exceeds this range, the WC aggregate structure is insufficient, and the plastic deformation resistance deteriorates. Furthermore, when A90 / A10 is less than 15.0, there are not enough coarse Co particles, the particle size distribution of the binder phase is narrow, and a homogeneous structure is formed, improving the resistance to chipping. However, the WC skeleton structure is disrupted, making it difficult to exhibit sufficient resistance to plastic deformation. On the other hand, when A90 / A10 exceeds 50.0, cavities are easily formed, deteriorating the resistance to plastic deformation. The binder phase can be extracted from the SEM image using, for example, image analysis software ImageJ. The areas of the extracted binder phase particles are accumulated starting from the smallest particle, and the area occupied by one binder phase particle at 10% of the cumulative particle area is determined as A10, and the area occupied by one binder phase particle at 90% of the cumulative particle area is determined as A90. In the present invention, each binder phase region divided by WC in a cross-sectional image of a WC-based cemented carbide is referred to as a binder phase particle.

[0024] 2.Cutting tools The WC-based cemented carbide tool and the surface-coated WC-based cemented carbide tool according to the present invention can be produced, for example, by the following steps. First, raw material powders consisting of coarse-grained WC powder, fine-grained WC powder, coarse-grained Co powder, fine-grained Co powder, and Cr3C2 powder having a predetermined average particle size, and further containing one or more types of powder selected from TaC powder, NbC powder, TiC powder, and ZrC powder as required, are blended and mixed to obtain a composition defined in the cemented carbide of the present invention, to prepare a mixed powder. In particular, the WC powder is subjected to press molding, heat treatment, and crushing processes multiple times before being mixed with other raw material powders, thereby increasing the Σ2 corresponding grain boundary ratio in the WC powder, which can then be mixed with other raw material powders, resulting in a cutting tool with excellent resistance to plastic deformation. The pretreated WC powder can be mixed with other raw material powders using media-less mixing, such as an ultrasonic homogenizer or a cyclone mixer, which allows the powders to be blended and mixed without applying a large crushing force, thereby preventing the disappearance of the Σ2 grain boundaries of WC formed during carbonization and pretreatment. Next, the mixed powder is molded to produce a powder compact. In the sintering process of the powder compact, as solid phase sintering progresses, it becomes difficult for Σ2 grain boundaries to be formed during the subsequent liquid phase sintering. Therefore, in the temperature range in which solid phase sintering progresses (1000°C to 1350°C), the heating rate is increased to 40°C / min or more to suppress solid phase sintering, and the main sintering is performed at 1350°C to 1450°C in a vacuum atmosphere for 10 to 80 minutes. This prevents the Σ2 grain boundaries formed in the fine-grained WC from being burned away due to dissolution and reprecipitation, and makes it possible to obtain a WC sintered body in which the Σ2 grain boundary ratio is maintained at 15% or more, or even 25% or more.

[0025] The WC-based cemented carbide tool and the surface-coated WC-based cemented carbide tool of the present invention will be specifically described with reference to examples. EXAMPLES

[0026] <WC-based carbide tool of the present invention> (a) Raw material powder First, as powders for sintering, coarse-grained WC powder with an average particle size (d50) of 10.0 to 15.0 μm on a volume basis, fine-grained WC powder with an average particle size (d50) of 0.5 to 1.0 μm, coarse-grained Co powder with an average particle size (d50) of 3.0 to 4.0 μm, fine-grained Co powder with an average particle size (d50) of 0.5 to 1.5 μm, Cr3C2 powder with an average particle size (d50) of 1.0 to 3.0 μm, and, as necessary, TaC powder, NbC powder, TiC powder, and ZrC powder, each with an average particle size (d50) of 1.0 to 3.0 μm, were prepared (see Table 2). In particular, for the coarse-grained WC powder and fine-grained WC powder used to manufacture the tool base of the present invention, WC raw material powder types A to D in Table 1 were used, and as a preparatory step before mixing with other carbide powders, the coarse-grained WC powder and the fine-grained WC powder were each subjected to press molding-heat treatment-crushing treatment multiple times in the following procedure to obtain coarse-grained WC raw material powder and fine-grained WC powder with excellent crystallinity and an increased Σ2 corresponding grain boundary ratio, and these were combined and used as the raw material. 1) The raw material WC powder is press-molded into spheres having a particle size of 1 mm to 3 mm, and heat-treated at 1300° C. to 1400° C. in an argon atmosphere of 10 Pa to 100 Pa for 30 minutes to 90 minutes. 2) The powder obtained by the heat treatment is subjected to a crushing treatment in a mortar for 3 minutes or more and 10 minutes or less. 3) By repeating steps 1) and 2) at least two times and at most ten times, WC powder with an increased Σ2 corresponding grain boundary ratio was obtained. That is, first, in step 1), the coarse-grained WC particles and the fine-grained WC particles, which were previously separate, are pressed into contact with each other and then heat-treated to bond the coarse-grained WC particles and the fine-grained WC particles together, forming corresponding grain boundaries and random grain boundaries at their interfaces. Next, in step 2), random grain boundaries with low grain boundary strength and grain boundaries with high Σ values ​​are preferentially destroyed by a crushing process, leaving Σ2 corresponding grain boundaries with high grain boundary strength. Then, in step 3), steps 1) and 2) are repeated multiple times to produce coarse-grained WC powder and fine-grained WC powder with a high ratio of Σ2 corresponding grain boundaries.

[0027] (b) Mixing process (media-less mixing process) Next, in (a), coarse-grained WC powder having an average grain size (d50) of 10.0 to 15.0 μm and fine-grained WC powder having an average grain size (d50) of 0.5 to 1.0 μm, which have an increased Σ2 corresponding grain boundary ratio, are mixed with previously prepared coarse-grained Co powder having an average grain size (d50) of 3.0 to 4.0 μm, fine-grained Co powder having an average grain size (d50) of 0.5 to 1.5 μm, and Cr3C2 powder having an average grain size (d50) of 1.0 to 3.0 μm to obtain a predetermined blend composition, or, if necessary, Furthermore, TaC powder, NbC powder, TiC powder, and ZrC powder, each with an average particle size (d50) in the range of 1.0 to 3.0 μm, were mixed to a specified composition to prepare sintering powder, and in particular, to prevent the Σ2 corresponding grain boundary formed by pretreatment of the WC powder from being destroyed, the mixture was wet mixed for 8 hours at a rotation speed of 50 rpm using a media-less attritor mixer, dried, and then pressed at a pressure of 100 MPa to produce a green compact (see Table 2).

[0028] (c) Sintering process 1) Heating step; (see Table 4 "Inventive step") Next, in the temperature increase process from 1000° C. to the sintering temperature of 1350° C., which is the solid-phase sintering temperature, the temperature increase rate was increased to 40° C. / min or more to suppress solid-phase sintering. In other words, during liquid phase sintering after heating in the liquid phase temperature region, new Σ2 corresponding grain boundaries are also formed, but in the temperature region before the liquid phase appears, WC molecules bond together through solid phase diffusion and necking is formed strongly, which reduces the Σ2 corresponding grain boundaries that would normally be formed during liquid phase sintering. Therefore, the heating rate was increased in the temperature region of 1000°C to 1350°C where solid phase diffusion progresses. 2) Sintering process; (see Table 4 "Inventive process") Next, in the sintering process, the temperature was raised to 1350°C or higher, and then the sintering was carried out at 1350°C to 1450°C for 10 to 80 minutes under a vacuum of 0.1 Pa or less. This prevented the Σ2 corresponding grain boundaries formed in the coarse-grained WC and fine-grained WC from dissolving and disappearing due to reprecipitation, thereby obtaining a WC-based cemented carbide sintered body.

[0029] Next, the WC-based cemented carbide sintered body was machined and ground to have the shape of CNMG432MM, and cemented carbide substrates 1 to 10 shown in Table 5 (hereinafter referred to as inventive tool substrates 1 to 10) were produced.

[0030] ≪Comparative example WC-based carbide tool≫ For comparison, comparative cemented carbide substrates 1 to 8 (hereinafter referred to as comparative tool substrates 1 to 8) were prepared. First, as the raw material powders, in addition to the WC raw material powder types A to D in Table 1 described above, raw material powders of the WC raw material powder types E to H shown in Table 1 were used. The manufacturing process is as follows: first, coarse WC powder having an average particle size (d50) of 10.0 to 18.0 μm or fine WC powder having an average particle size (d50) of 0.5 to 1.5 μm is mixed with coarse Co powder having an average particle size (d50) of 3.0 to 4.0 μm or fine Co powder having an average particle size (d50) of 0.5 to 1.5 μm and Cr3C2 powder having an average particle size (d50) of 1.0 to 3.0 μm in the mixing ratio shown in Table 3 to obtain a predetermined mixing composition; or, if necessary, one or more of TaC powder, NbC powder, TiC powder, and ZrC powder, each having an average particle size (d50) of 1.0 to 3.0 μm, are further mixed to obtain a predetermined mixing composition to obtain a sintering powder, which is wet mixed for 8 hours at a rotation speed of 50 rpm by media-less attritor mixing, dried, and then pressed at a pressure of 100 MPa to produce a green compact. Next, a sintering process was carried out under the solid phase sintering conditions and liquid phase sintering conditions of comparative processes 1' to 8' shown in Table 4, which are different from the manufacturing conditions of the tool bases 1 to 10 of the present invention, to obtain a WC-based cemented carbide sintered body. The WC-based cemented carbide sintered body was then machined and ground to have a shape of CNMG432MM, thereby producing comparative example tool bases 1 to 8 shown in Table 6.

[0031] For the cross sections of the cemented carbide of the tool bases 1 to 10 of the present invention and the comparative tool bases 1 to 8, the content of each of the elements Cr, Ti, Ta, Nb, and Zr was measured at 10 points using an electron microanalyzer (EPMA), and the average value was taken as the content of each element. The contents of the elements Cr, Ti, Ta, Nb, and Zr were calculated by converting them into carbides. Tables 5 and 6 show the average contents of each element.

[0032] Next, the cross sections of the WC-based cemented carbide of the present invention tools 1 to 10 and the comparative example tools 1 to 8 were observed at a magnification of 200 to 500 times using a scanning electron microscope (SEM), and an SEM image was obtained with an image size of 120 × 96 mm and a pixel count of 1280 × 1024 pixels. This was then processed using the image analysis software ImageJ to measure the area of ​​each binder phase within one observation field. The areas of each binder phase particle were accumulated starting from the particle with the smallest area, and the area occupied by one binder phase particle when the accumulated area exceeded 10% of the total binder phase area was determined as A10, and the area occupied by one binder phase particle when the accumulated area exceeded 90% of the total binder phase area was determined as A90. Next, the obtained A90 is divided by A10 to obtain A90 / A10. The number of binder phases is measured by counting each individual binder phase divided by WC particles as one binder phase. In addition, in order to include a sufficient number of bonding phases in the image, observations were performed at magnifications of 200 to 500 times, and the observation magnification was selected so that the number of bonding phases measured after image processing would be in the range of 5,000 to 15,000.

[0033] [Table 1]

[0034] [Table 2]

[0035] [Table 3]

[0036] [Table 4]

[0037] [Table 5]

[0038] [Table 6]

[0039] The above-mentioned tools 1 to 10 of the present invention and comparative tools 1 to 8 were subjected to the following wet continuous turning test in a state in which each was screwed to the tip of a tool steel bit by a fixing jig. Work material: JIS SUS304 (HB170) round bar, Cutting speed: 120m / min, Cutting depth: 1.8mm, Feed: 0.6mm / rev, Cutting time: 5 minutes, Uses wet water-soluble cutting oil. After the wet continuous cutting test, the amount of plastic deformation of the cutting edge was measured and the wear state of the cutting edge was observed. The amount of plastic deformation of the cutting edge was measured by drawing a line segment on the ridge where the rake face intersects with the flank face of the main cutting edge of the tool at a position sufficiently distant from the cutting edge, extending the line segment toward the cutting edge, and measuring the maximum distance between the extended line segment and the ridge line of the cutting edge (perpendicular to the extended line segment). When the amount of plastic deformation of the flank face was 0.04 mm or more, the wear state was determined to be cutting edge deformation. Table 7 shows the results of this test.

[0040] [Table 7]

[0041] In addition, hard coating layers having average thicknesses shown in Table 8 were formed by PVD or CVD on the cutting edge surfaces of the tools 1 to 4 of the present invention and the comparative tools 1 to 4, to produce surface-coated WC-based cemented carbide cutting tools 1 to 4 of the present invention (hereinafter referred to as "coated tools of the present invention") and comparative surface-coated WC-based cemented carbide cutting tools 1 to 4 of the comparative examples (hereinafter referred to as "coated tools of the comparative examples"). For each of the above-mentioned coated tools, the following wet continuous cutting test was carried out to measure the amount of plastic deformation on the flank of the cutting edge and to observe the state of wear of the cutting edge. Cutting conditions: Work material: JIS SUS304 (HB170) round bar, Cutting speed: 180m / min, Cutting depth: 2.1mm, Feed: 0.5mm / rev, Cutting time: 4 minutes, Uses wet water-soluble cutting oil. Table 9 shows the results of the cutting tests.

[0042] [Table 8]

[0043] [Table 9]

[0044] The test results shown in Tables 7 and 9 show that the tools of the present invention and the coated tools of the present invention exhibit excellent resistance to plastic deformation without the occurrence of fracture, whereas the comparative tools and the comparative coated tools have a short tool life due to the occurrence of fracture or plastic deformation. [Industrial Applicability]

[0045] As described above, the tool and the coated tool of the present invention exhibit excellent effects over long periods of use in heavy-duty continuous cutting, such as continuous turning of alloy steel, stainless steel, etc., and greatly contribute to extending the tool life.

Claims

1. In a WC-based cemented carbide cutting tool having a WC-based cemented carbide substrate, The composition of the WC-based cemented carbide is as follows: Co is 6.0 to 14.0 mass % as a binder phase forming component, and Cr is 1.0 to 1.0 mass %. 3 C 2 The balance is WC and inevitable impurities, The particle size distribution of the binder phase in the cross section of the substrate of the WC-based cemented carbide was analyzed, and the area occupied by one binder phase particle at a cumulative 10% particle area was defined as A10 (μm 2 ), and the area occupied by one binder phase particle at 90% cumulative particle area is A90 (μm 2 ), A10 is 0.15 μm 2 or more, 0.30μm 2 and A90 / A10 is 15.0 or more and 50.0 or less.

2. The WC-based cemented carbide cutting tool according to claim 1, characterized in that the WC-based cemented carbide further contains at least one selected from the group consisting of TaC, NbC, TiC and ZrC in a total amount of 4.0 mass% or less.

3. 3. The WC-based cemented carbide cutting tool according to claim 1, characterized in that the average grain size of WC in the WC-based cemented carbide is 0.2 μm or more and 4.0 μm or less, and the presence ratio of Σ2 correspondence grain boundaries of WC to all WC / WC grain boundaries (Σ2 correspondence grain boundary ratio) is 15% or more.

4. 4. A surface-coated WC-based cemented carbide cutting tool according to claim 1, further comprising a hard coating layer formed on at least a cutting edge of the WC-based cemented carbide cutting tool.

Citation Information

Patent Citations

  • Coated cemented carbide for cutting tool

    JP1995252579A

  • Cemented carbide parts

    JP1995305136A

  • Cemented carbide

    JP2009035802A

  • Cermet

    JP2010222650A

  • Super hard alloy and cutting tool