Resin composition, laminate with resin composition layer, laminate, and electromagnetic wave shielding film
A resin composition for flexible printed wiring boards, combining polyester polyurethane, epoxy, and polyolefin resins, addresses conductivity and adhesion issues in high-humidity conditions, ensuring long-term stability and heat resistance.
Patent Information
- Application Number
- JP2021526998
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-06-28
- Filing Date
- 2020-06-23
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2040-06-23
AI Technical Summary
Conventional resin compositions for flexible printed wiring boards do not maintain sufficient electrical conductivity after long-term storage in high-temperature, high-humidity environments, and they lack adequate adhesive strength and heat resistance.
A resin composition comprising polyester polyurethane resin, epoxy resin, and polyolefin resin, with specific molecular weight ranges and ratios, along with optional organic and metal fillers, to enhance conductivity, adhesion, and heat resistance.
The composition maintains excellent conductivity and adhesive strength even after 1,000 hours in a high-temperature, high-humidity environment, with improved soldering heat resistance and stability.
Smart Images

Figure 0007587208000001 
Figure 0007587208000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyester polyurethane resin composition which has high adhesive strength to polyimide films and metals, and when cured has heat resistance and moist heat resistance, and is excellent in liquid stability and processability, and is an effective member for producing a printed wiring board, in particular a flexible printed wiring board or a multilayer printed wiring board by a build-up method.The present invention further relates to a bonding film in which the resin composition is applied to a release film, a laminate with a resin composition layer in which the resin composition is applied to a base film, a laminate having a layer formed by curing the resin composition, and an electromagnetic wave shielding film which is applied to a flexible printed wiring board or the like and is suitably used for shielding electromagnetic noise generated from an electric circuit. [Background technology]
[0002] Flexible printed wiring boards are capable of three-dimensional and high-density mounting even in a limited space, and therefore their applications are expanding. In recent years, with the miniaturization and weight reduction of electronic devices, products related to flexible printed wiring boards have become more diverse and the demand for them has increased. Such related products include flexible copper-clad laminates in which copper foil is bonded to a polyimide film, flexible printed wiring boards in which an electronic circuit is formed on a flexible copper-clad laminate, flexible printed wiring boards with reinforcement plates in which a flexible printed wiring board and a reinforcement plate are bonded together, flexible copper-clad laminates or multilayer boards in which flexible printed wiring boards are stacked and bonded, and the like. For example, when manufacturing a flexible copper-clad laminate, an adhesive is usually used to bond the polyimide film and the copper foil.
[0003] As a conventional adhesive composition or a conventional laminate, the methods described in Patent Documents 1 to 3 are known. Patent Document 1 describes a halogen-free flame-retardant adhesive composition comprising (A) a solvent-soluble polyamide resin that is solid at 25°C, (B) a phenoxy resin, (C) an epoxy resin that does not contain halogen atoms, and (D) a phosphorus-based flame retardant having a structure represented by the following general formula (1), wherein the epoxy resin (C) is an epoxy resin having three or more epoxy groups in one molecule, the content of the phenoxy resin (B) is 100 to 450 parts by mass per 100 parts by mass of the polyamide resin (A), the content of the epoxy resin (C) is 1 to 60 parts by mass per 100 parts by mass of the total of the polyamide resin (A) and the phenoxy resin (B), and the content of the phosphorus-based flame retardant (D) is 5 to 100 parts by mass per 100 parts by mass of the polyamide resin (A) and the phenoxy resin (B).
[0004] Patent Document 2 describes a laminate comprising a polyester polymer (a) containing two or more carboxyl groups in the molecule, a number average molecular weight of 5,000 to 100,000, and a molecular weight per carboxyl group of 1,500 to 10,000, an epoxy resin (b) containing two or more epoxy groups in the molecule, and an epoxy resin curing accelerator (c), the curable resin composition being capable of retaining thermoplasticity for five months or more at 5°C, laminated on at least one surface of a polyimide film, a polyester film, or a metal foil, and a laminate in which the curable resin composition of the laminate is cured and laminated on a metal foil (including a metal circuit).
[0005] In addition, Patent Document 3 describes a method for producing a carboxyl group-containing polymer having an acid value (unit: equivalent / 10 6 g) is 100 or more and 1000 or less, and the number average molecular weight is 5.0 × 10 3 Above 1.0×10 5The document describes a resin composition for adhesives, which comprises a polyurethane resin (a) having a glass transition temperature of -10°C or more and 70°C or less, an epoxy resin (b) containing nitrogen atoms, and an epoxy resin (c) having a dicyclopentadiene skeleton, wherein the blending ratio of the resin (b) is 0.1 mass % or more and 20 mass % or less of the total epoxy resins contained in the resin composition.
[0006] Patent Document 1: Patent No. 5846290 Patent Document 2: JP 2005-125724 A Patent Document 3: JP 2010-84005 A Summary of the Invention [Problem to be solved by the invention]
[0007] The problem to be solved by the present invention is to provide a resin composition that has excellent electrical conductivity even after long-term (1,000 hours) storage in a high-temperature, high-humidity environment (85° C., 85% RH). Another object of the present invention is to provide a laminate having a resin composition layer, a laminate or an electromagnetic wave shielding film using the resin composition. [Means for solving the problem]
[0008] Means for solving the above problems include the following aspects. <1> A resin composition comprising a polyester polyurethane resin (A), an epoxy resin (B), and a polyolefin resin (C). <2> The content of the polyester polyurethane resin (A) is 10% by mass to 70% by mass, and the content of the polyolefin resin (C) is 10% by mass to 70% by mass, based on the total amount of resin solids excluding the filler component. <1> The resin composition according to claim 1. <3> Further containing an organic filler (D) <1> or <2> The resin composition according to claim 1. <4> The organic filler (D) is contained in an amount of 5 to 40 parts by mass per 100 parts by mass of the total amount of resin solids excluding the filler component. <3> The resin composition according to claim 1. <5> The epoxy resin (B) contains a bisphenol type epoxy resin and / or a bisphenol novolac type epoxy resin. <1> ~ <4> 10. The resin composition according to claim 9 . <6> The number average molecular weight of the polyester polyurethane resin (A) is 10,000 to 80,000, and the molecular weight per urethane bond in the polyester polyurethane resin (A) is 200 to 8,000. <1> ~ <5> 10. The resin composition according to claim 9 . <7> The polyester polyurethane resin (A) contains a polyester polyurethane resin having a polyester structure and a number average molecular weight of 8,000 to 30,000. <1> ~ <6> 10. The resin composition according to claim 9 . <8> The acid value of the polyester polyurethane resin (A) is 0.1 mgKOH / g to 20 mgKOH / g. <1> ~ <7> 10. The resin composition according to claim 9 . <9> The diol component constituting the polyester polyurethane resin (A) contains a diol having a side chain. <1> ~ <8> 10. The resin composition according to claim 9 . <10> The polyolefin resin (C) is a polypropylene resin graft-modified with a modifier containing an α,β-unsaturated carboxylic acid or a derivative thereof, and the content of the grafted portion is 0.1% by mass to 20% by mass based on the total mass of the polyolefin resin (C). <1> ~ <9> 10. The resin composition according to claim 9 . <11> Further containing a metal filler (E) <1> ~ <10> 10. The resin composition according to claim 9 . <12> Contains 10 to 350 parts by mass of metal filler (E) per 100 parts by mass of the total amount of resin solids excluding filler components <11> The resin composition according to claim 1. <13> The metal filler (E) is a conductive filler. <11> or <12> The resin composition according to claim 1. <14> <1> ~ <13> 1. A laminate with a resin composition layer, comprising a resin composition layer made of the resin composition according to any one of the above items 1 to 5, and a base film in contact with at least one side of the resin composition layer, wherein the resin composition layer is in a B-stage state. <15> <1> ~ <13> 13. A laminate comprising a cured layer obtained by curing the resin composition according to any one of the above items. <16> <1> ~ <13> 1. An electromagnetic wave shielding film having a resin composition layer made of the resin composition according to any one of claims 1 to 9. Effect of the Invention
[0009] According to the present invention, it is possible to provide a resin composition that has excellent electrical conductivity even after long-term (1,000 hours) storage in a high-temperature, high-humidity environment (85° C., 85% RH). Furthermore, according to the present invention, it is possible to provide a laminate having a resin composition layer, a laminate or an electromagnetic wave shielding film using the resin composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The following description of the constituent elements may be based on a representative embodiment of the present invention, but the present invention is not limited to such an embodiment. In this specification, the word "to" is used to mean that the numerical values before and after it are included as the lower limit and upper limit. In the present specification, the upper or lower limit of one numerical range may be replaced with the upper or lower limit of another numerical range. In addition, in the present specification, the upper or lower limit of the numerical range may be replaced with a value shown in the examples. In the present invention, when a plurality of substances corresponding to each component are present in the composition, the amount of each component in the composition means the total amount of the plurality of substances present in the composition, unless otherwise specified. In the present invention, the term "step" includes not only an independent step, but also a step that cannot be clearly distinguished from other steps, as long as the intended purpose of the step is achieved. In the present invention, "mass %" and "weight %" are synonymous, and "parts by mass" and "parts by weight" are synonymous. Also, in the present invention, a combination of two or more preferred embodiments is a more preferred embodiment. In addition, in this specification, "(meth)acrylic" refers to both or either of acrylic and methacrylic. In the present disclosure, the term "main chain" refers to the relatively longest bond chain in the molecule of the polymer compound that constitutes the resin, and the term "side chain" refers to a carbon chain branching off from the main chain. Furthermore, in some of the compounds in this specification, the hydrocarbon chain may be represented by a simplified structural formula in which the symbols for carbon (C) and hydrogen (H) are omitted. The present invention will be described in detail below.
[0011] (Resin composition) The resin composition of the present invention contains a polyester polyurethane resin (A), an epoxy resin (B), and a polyolefin resin (C). The resin composition of the present invention can be suitably used as an adhesive composition, more suitably used as an adhesive composition for bonding polyimide or metal, and particularly suitably used as an adhesive composition for bonding polyimide and metal.
[0012] The present inventors have found that conventional resin compositions do not have sufficient electrical conductivity after long-term storage in a high-temperature and high-humidity environment. As a result of intensive research, the present inventors have found that by containing three types of resins, namely, a polyester polyurethane resin (A), an epoxy resin (B), and a polyolefin resin (C), these three types of resins act in a synergistic manner and complement each other, and thus it is possible to provide a resin composition that has excellent electrical conductivity even after long-term storage under a high-temperature and high-humidity environment, although the detailed mechanism is unknown.
[0013] Furthermore, the resin composition of the present invention contains three types of resins, namely, the polyester polyurethane resin (A), the epoxy resin (B), and the polyolefin resin (C), and therefore has excellent adhesion and solder heat resistance. In particular, the resin composition of the present invention contains three types of resin, namely, a polyester polyurethane resin (A), an epoxy resin (B), and a polyolefin resin (C), and therefore has high adhesion to polyimides and metals, excellent electrical conductivity both initially and after soldering, and excellent heat resistance.
[0014] The present invention will be described in detail below. In this specification, "polyester polyurethane resin (A)" and the like are also referred to as "component (A)" and the like.
[0015] <Polyester polyurethane resin (A)> The resin composition of the present invention contains a polyester polyurethane resin (A). The polyester polyurethane resin (A) may be any resin having two or more ester bonds and two or more urethane bonds, but is preferably a resin having a polyester chain and two or more urethane bonds. In addition, the polyester polyurethane resin (A) is preferably a resin obtained by reacting at least a polyester polyol, a polyisocyanate, and a chain extender as raw materials, and more preferably a resin obtained by reacting at least a polyester polyol, a polyisocyanate, and a diol compound.
[0016] The polyester portion in the polyester polyurethane resin (A) is preferably formed from an acid component and an alcohol component. The acid component is preferably a polycarboxylic acid compound, more preferably a dicarboxylic acid compound. In addition, a sulfocarboxylic acid compound or the like can also be used as the acid component. Furthermore, an aromatic acid is preferably used as the acid component. As the alcohol component, a polyhydric alcohol compound is preferable, and a diol compound is more preferable. The polyester portion may be formed from a hydroxycarboxylic acid compound. When the total amount of all acid components constituting the polyester portion of the polyester polyurethane resin (A) is taken as 100 mol %, from the viewpoints of adhesion, heat resistance, and moist heat resistance, aromatic acids preferably account for 30 mol % or more of the total acid components, more preferably 45 mol % or more, and particularly preferably 60 mol % or more.
[0017] Examples of aromatic acids include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, orthophthalic acid, naphthalenedicarboxylic acid, biphenyldicarboxylic acid, and 5-hydroxyisophthalic acid. In addition, aromatic dicarboxylic acids having a sulfonic acid group or a sulfonic acid group such as sulfoterephthalic acid, 5-sulfoisophthalic acid, 4-sulfophthalic acid, 4-sulfonaphthalene-2,7-dicarboxylic acid, 5-(4-sulfophenoxy)isophthalic acid, sulfoterephthalic acid, and / or their metal salts and ammonium salts, and aromatic oxycarboxylic acids such as p-hydroxybenzoic acid, p-hydroxyphenylpropionic acid, p-hydroxyphenylacetic acid, 6-hydroxy-2-naphthoic acid, and 4,4-bis(p-hydroxyphenyl)valeric acid can be mentioned. Among these, from the viewpoint of adhesiveness, it is preferable that the acid component contains terephthalic acid and / or isophthalic acid, and terephthalic acid and / or isophthalic acid are particularly preferable. Furthermore, the acid component may be a derivative of an acid compound such as an ester during resin synthesis.
[0018] Examples of other acid components include alicyclic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, and 1,2-cyclohexanedicarboxylic acid and their acid anhydrides, and aliphatic dicarboxylic acids such as succinic acid, adipic acid, azelaic acid, sebacic acid, dodecanedioic acid, and dimer acid.
[0019] On the other hand, preferred examples of the polyhydric alcohol component include an aliphatic diol compound, an alicyclic diol compound, an aromatic diol compound, and an ether bond-containing diol compound. Examples of the aliphatic diol compound include ethylene glycol, 1,2-propylene diol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, neopentyl glycol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, 1,9-nonanediol, 2-butyl-2-ethyl-1,3-propanediol, hydroxypivalic acid neopentyl glycol ester, dimethylol heptane, and 2,2,4-trimethyl-1,3-pentanediol. Examples of the alicyclic diol compound include 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, tricyclodecanediol, tricyclodecanedimethylol, spiroglycol, hydrogenated bisphenol A, and ethylene oxide and propylene oxide adducts of hydrogenated bisphenol A. Examples of aromatic diol compounds include glycols obtained by adding 1 to several moles of ethylene oxide or propylene oxide to two phenolic hydroxyl groups of bisphenols, such as paraxylene glycol, metaxylene glycol, ortho-xylene glycol, 1,4-phenylene glycol, an ethylene oxide adduct of 1,4-phenylene glycol, bisphenol A, an ethylene oxide adduct of bisphenol A, and a propylene oxide adduct of bisphenol A. Examples of the ether bond-containing diol compound include diethylene glycol, triethylene glycol, dipropylene glycol, polyethylene glycol, polypropylene glycol, polytetramethylene glycol, neopentyl glycol ethylene oxide adduct, and neopentyl glycol propylene oxide adduct. Among these diols, diols having a side chain such as neopentyl glycol and 2-butyl-2-ethyl-1,3-propanediol are preferred for reasons of compatibility with epoxy resins, polyolefin resins, etc. and solution stability. That is, the diol component constituting the polyester polyurethane resin (A) preferably contains a diol having a side chain from the viewpoints of compatibility with epoxy resins, polyolefin resins, etc. and solution stability. Among them, from the viewpoints of compatibility with epoxy resins, polyolefin resins, etc., solution stability, and electrical conductivity, it is more preferable that the chain extender constituting the polyester polyurethane resin (A) contains a diol having a side chain. That is, from the viewpoints of compatibility with epoxy resins, polyolefin resins, etc., solution stability, and electrical conductivity, it is more preferable that the polyester polyurethane resin (A) is a resin obtained by reacting at least a polyester polyol, a polyisocyanate, and a diol having a side chain as raw materials.
[0020] In addition, hydroxycarboxylic acid compounds having a hydroxy group and a carboxy group in their molecular structure can also be used as polyester raw materials, and examples of such compounds include 5-hydroxyisophthalic acid, p-hydroxybenzoic acid, p-hydroxyphenethyl alcohol, p-hydroxyphenylpropionic acid, p-hydroxyphenylacetic acid, 6-hydroxy-2-naphthoic acid, and 4,4-bis(p-hydroxyphenyl)valeric acid.
[0021] As a component constituting the polyester portion of the polyester polyurethane resin (A), about 0.1 mol % to 5 mol % of trifunctional or higher polycarboxylic acids and / or polyols may be copolymerized with respect to the total acid components or total polyhydric alcohol components constituting the polyester portion, if necessary, for the purpose of introducing a branched skeleton. In particular, when a cured layer is obtained by reacting with a curing agent, the introduction of a branched skeleton increases the terminal group concentration (reaction points) of the resin, and a cured layer with high crosslink density can be obtained. In this case, examples of polycarboxylic acids having three or more functional groups include trimellitic acid, trimesic acid, ethylene glycol bis(anhydrotrimellitate), glycerol tris(anhydrotrimellitate), trimellitic anhydride, pyromellitic anhydride (PMDA), oxydiphthalic dianhydride (ODPA), 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), 3,3',4,4'-diphenyltetracarboxylic dianhydride (BPDA), 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride (DSDA), 4,4'-(hexafluoroisopropylidene)diphthalic dianhydride (6FDA), 2,2'-bis[(dicarboxyphenoxy)phenyl]propane dianhydride (BSAA), and the like. On the other hand, examples of polyols having three or more functional groups include glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, and the like. When a trifunctional or higher functional polycarboxylic acid and / or polyol is used, it is preferable to copolymerize it in an amount of preferably 0.1 mol % to 5 mol %, more preferably 0.1 mol % to 3 mol %, based on the total acid components or total polyhydric alcohol components.
[0022] The polyester portion of the polyester polyurethane resin (A) may be subjected to acid addition in an amount of about 0.1 mol % to 10 mol % based on the total acid components or polyhydric alcohol components constituting the polyester portion for the purpose of introducing a carboxy group as necessary. When a monocarboxylic acid, dicarboxylic acid, or polyfunctional carboxylic acid compound is used for acid addition, a decrease in molecular weight occurs due to ester exchange, so it is preferable to use an acid anhydride. Examples of acid anhydrides that can be used include succinic anhydride, maleic anhydride, orthophthalic acid, 2,5-norbornene dicarboxylic anhydride, tetrahydrophthalic anhydride, trimellitic anhydride, pyromellitic anhydride (PMDA), oxydiphthalic dianhydride (ODPA), 3,3',4,4'-benzophenone tetracarboxylic dianhydride (BTDA), 3,3',4,4'-diphenyl tetracarboxylic dianhydride (BPDA), 3,3',4,4'-diphenyl sulfone tetracarboxylic dianhydride (DSDA), 4,4'-(hexafluoroisopropylidene) diphthalic dianhydride (6FDA), and 2,2'-bis[(dicarboxyphenoxy)phenyl]propane dianhydride (BSAA). Acid addition can be carried out directly in bulk after polyester polycondensation, or by dissolving the polyester and then adding the acid. The reaction in bulk is fast, but adding a large amount of acid can cause gelation, and the reaction is carried out at high temperatures, so care must be taken to prevent oxidation by blocking oxygen gas. On the other hand, acid addition in solution is slow, but allows for the stable introduction of a large number of carboxyl groups.
[0023] The polyisocyanate used in the production of the polyester polyurethane resin (A) may be one of diisocyanates, their dimers (uretdione), their trimers (isocyanurates, triol adducts, biuret), etc., or a mixture of two or more of them. For example, examples of the diisocyanate component include 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, p-phenylene diisocyanate, diphenylmethane diisocyanate, m-phenylene diisocyanate, hexamethylene diisocyanate, tetramethylene diisocyanate, 3,3'-dimethoxy-4,4'-biphenylene diisocyanate, 1,5-naphthalene diisocyanate, 2,6-naphthalene diisocyanate, 4,4'-diisocyanate diphenyl ether, m-xylylene diisocyanate, 1,3-diisocyanate methylcyclohexane, 1,4-diisocyanate methylcyclohexane, 4,4'-diisocyanate cyclohexane, 4,4'-diisocyanate cyclohexylmethane, isophorone diisocyanate, dimer acid diisocyanate, and norbornene diisocyanate. Among these, from the viewpoint of transparency, aliphatic or alicyclic diisocyanates are preferred, and from the viewpoint of availability and economical reasons, hexamethylene diisocyanate and isophorone diisocyanate are particularly preferred.
[0024] In producing the polyester polyurethane resin (A), a chain extender may be used, if necessary. Examples of the chain extender include the diol compounds already described as components of the polyester portion, and compounds having one carboxy group and two hydroxy groups, such as dimethylolpropionic acid and dimethylolbutanoic acid. Among these, as the chain extender, from the viewpoint of electrical conductivity, a diol compound is preferable, a diol compound having a side chain is more preferable, and a diol compound having a branched chain is particularly preferable. From the viewpoint of electrical conductivity, the diol compound having a side chain preferably contains at least one compound selected from the group consisting of neopentyl glycol, 2-butyl-2-ethyl-1,3-propanediol, and 2,2-dimethylolpropionic acid, and particularly preferably contains at least one compound selected from the group consisting of neopentyl glycol and 2-butyl-2-ethyl-1,3-propanediol and 2,2-dimethylolpropionic acid.
[0025] The method for producing the polyester polyurethane resin (A) is not particularly limited, and a known method can be used. For example, the polyester polyol and the polyisocyanate, and if necessary, the chain extender, may be charged in a reaction vessel all at once, or may be charged in portions. In any case, the ratio of the functional group of the isocyanate group / hydroxy group is preferably 0.9 or more and 1.1 or less, more preferably 0.98 or more and 1.02 or less, and particularly preferably 1, with respect to the total hydroxyl value of the polyester polyol and the chain extender in the system and the total isocyanate group of the polyisocyanate. This reaction can be produced by reacting in the presence or absence of a solvent inert to the isocyanate group. Examples of the solvent include ester solvents (ethyl acetate, butyl acetate, ethyl butyrate, etc.), ether solvents (dioxane, tetrahydrofuran, diethyl ether, etc.), ketone solvents (cyclohexanone, methyl ethyl ketone, methyl isobutyl ketone, etc.), aromatic hydrocarbon solvents (benzene, toluene, xylene, etc.), and mixed solvents thereof, with ethyl acetate and methyl ethyl ketone being preferred from the viewpoint of reducing the environmental load. The reaction apparatus is not limited to a reaction vessel equipped with a stirrer, and a mixing and kneading apparatus such as a kneader or a twin-screw extruder can also be used.
[0026] In order to promote the urethane reaction, catalysts used in ordinary urethane reactions can be used, such as tin-based catalysts (trimethyltin laurate, dimethyltin dilaurate, trimethyltin hydroxide, dimethyltin dihydroxide, stannous octoate, etc.), lead-based catalysts (red oleate, red-2-ethylhexoate, etc.), and amine-based catalysts (triethylamine, tributylamine, morpholine, diazabicyclooctane, diazabicycloundecene, etc.).
[0027] From the viewpoints of adhesion, electrical conductivity, and heat resistance, the glass transition temperature (Tg) of the polyester portion in the polyester polyurethane resin (A) is preferably 40°C to 150°C, more preferably 45°C to 120°C, even more preferably 50°C to 90°C, and particularly preferably 60°C to 70°C. From the viewpoints of adhesion, conductivity, and heat resistance, the glass transition temperature (Tg) of the polyester polyurethane resin (A) is preferably 30°C to 150°C, more preferably 40°C to 140°C, and particularly preferably 50°C to 120°C.
[0028] From the viewpoints of electrical conductivity and heat resistance, the number average molecular weight (Mn) of the polyester polyurethane resin (A) is preferably from 5,000 to 100,000, more preferably from 10,000 to 80,000, further preferably from 20,000 to 60,000, and particularly preferably from 25,000 to 50,000. In the present invention, the number average molecular weight (Mn) and weight average molecular weight (Mw) of the resin can be obtained by gel permeation chromatography (GPC).
[0029] The molecular weight per urethane bond in the polyester polyurethane resin (A) is preferably from 100 to 15,000, more preferably from 200 to 8,000, and particularly preferably from 300 to 2,000, from the viewpoints of electrical conductivity and heat resistance.
[0030] From the viewpoints of adhesion and conductivity, the acid value of the polyester polyurethane resin (A) is preferably 0 mgKOH / g to 50 mgKOH / g, more preferably 0.1 mgKOH / g to 20 mgKOH / g, further preferably 0.1 mgKOH / g to 5 mgKOH / g, and particularly preferably 1.0 mgKOH / g to 5.0 mgKOH / g. From the viewpoint of heat resistance, the acid value of the polyester polyurethane resin (A) is preferably 20 mgKOH / g or less, and particularly preferably 5 mgKOH / g or less. In the present invention, the acid value of a resin is measured by neutralizing a sample with a potassium hydroxide benzyl alcohol solution using a phenolphthalein solution as an indicator to determine the acid value.
[0031] Among these, from the viewpoints of adhesion, conductivity, and heat resistance, the number average molecular weight of the polyester structure of the polyester polyurethane resin (A) is preferably 1,000 to 50,000, more preferably 2,000 to 40,000, even more preferably 3,000 to 30,000, and particularly preferably 8,000 to 30,000.
[0032] The resin composition of the present invention may contain one type of polyester polyurethane resin (A) alone, or may contain two or more types. From the viewpoints of adhesion, conductivity, and heat resistance, the content of the polyester polyurethane resin (A) is preferably 5% by mass to 90% by mass, more preferably 10% by mass to 70% by mass, and particularly preferably 30% by mass to 70% by mass, based on the total amount of resin solids excluding the filler component in the resin composition. The resin solids excluding the filler components refer to the resin components (such as the polyester polyurethane resin (A), the epoxy resin (B), and the polyolefin resin (C)) which are non-volatile components excluding the organic filler (D), the metal filler (E), and the inorganic fillers other than the metal filler (E) described below, and the curing accelerator described below. The resin components and the curing accelerator may be solid or liquid at room temperature (25°C). Furthermore, from the viewpoints of adhesion, electrical conductivity, and heat resistance, it is preferable that in the resin composition of the present invention, the content of the polyester polyurethane resin (A) is 10% by mass to 70% by mass, and the content of the polyolefin resin (C) is 10% by mass to 70% by mass, based on the total amount of resin solids excluding the filler component.
[0033] <Epoxy resin (B)> The resin composition of the present invention contains an epoxy resin (B). The epoxy resin (B) is a component that imparts adhesiveness and heat resistance to the cured portion after adhesion. The epoxy resin (B) in the present invention includes not only high molecular weight compounds having an epoxy group, but also low molecular weight compounds having an epoxy group. The number of epoxy groups in the epoxy resin (B) is preferably 2 or more. Examples of the epoxy resin (B) include glycidyl esters such as orthophthalic acid diglycidyl ester, isophthalic acid diglycidyl ester, terephthalic acid diglycidyl ester, p-hydroxybenzoic acid diglycidyl ester, tetrahydrophthalic acid diglycidyl ester, succinic acid diglycidyl ester, adipic acid diglycidyl ester, sebacic acid diglycidyl ester, and trimellitic acid triglycidyl ester; diglycidyl ether of bisphenol A and its oligomers, ethylene glycol diglycidyl ether, and propylene glycol diglycidyl ether. glycidyl ethers such as 1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane triglycidyl ether, pentaerythritol tetraglycidyl ether, tetraphenylglycidyl ether ethane, triphenylglycidyl ether ethane, polyglycidyl ether of sorbitol, and polyglycerol polyglycidyl ether; and novolac epoxy resins such as phenol novolac epoxy resin, o-cresol novolac epoxy resin, and bisphenol A novolac epoxy resin. In addition, brominated bisphenol A type epoxy resins, phosphorus-containing epoxy resins, dicyclopentadiene skeleton-containing epoxy resins, naphthalene skeleton-containing epoxy resins, anthracene type epoxy resins, tertiary butyl catechol type epoxy resins, biphenyl type epoxy resins, and bisphenol S type epoxy resins that have been imparted with flame retardancy can also be used. Among these, from the viewpoints of adhesion and heat resistance, the epoxy resin (B) preferably contains a bisphenol type epoxy resin and / or a novolac type epoxy resin, and more preferably contains a bisphenol type epoxy resin and a phenol novolac type epoxy resin.
[0034] In the present invention, in order to achieve high heat resistance after curing, it is preferable that the epoxy resin (B) contains a compound having three or more epoxy groups in one molecule. When such a compound is used, the crosslinking reactivity with the polyester polyurethane resin (A) and the polyolefin resin (C) becomes higher than when an epoxy resin having two epoxy groups is used, and sufficient heat resistance is obtained. From the viewpoint of heat resistance, the content of the compound having three or more epoxy groups in one molecule in the epoxy resin (B) is preferably 15 mass % or more, more preferably 20 mass % or more, and particularly preferably 25 mass % or more, based on the total mass of the epoxy resin (B).
[0035] The resin composition of the present invention may contain one type of epoxy resin (B) alone, or may contain two or more types of epoxy resin (B). From the viewpoints of adhesion, electrical conductivity, and heat resistance, the content of the epoxy resin (B) is preferably 1 mass % to 60 mass %, more preferably 2 mass % to 50 mass %, even more preferably 3 mass % to 35 mass %, and particularly preferably 3 mass % to 20 mass %, relative to the total amount of resin solids excluding the filler component in the resin composition.
[0036] <Polyolefin resin (C)> The resin composition of the present invention contains a polyolefin resin (C). The polyolefin resin (C) is preferably a solid at 25°C. The polyolefin resin (C) is not particularly limited, but is preferably a modified polyolefin resin, more preferably a modified polyolefin resin having an acid group, and particularly preferably a modified polyolefin resin having a carboxy group.
[0037] The polyolefin resin (C) is not particularly limited as long as it has a structural unit derived from an olefin, but homopolymers or copolymers having 2 to 20 carbon atoms, such as ethylene, propylene, butene, pentene, hexene, heptene, octene, and 4-methyl-1-pentene, are preferably used. In the present invention, a homopolymer or copolymer of an olefin having 2 to 6 carbon atoms is particularly preferred. The content ratio of the structural units in the polyolefin resin can be selected arbitrarily, but when adhesion to a poorly adhesive adherend is performed, the modified polyolefin resin is preferably an ethylene-propylene copolymer, a propylene-butene copolymer, or a modified resin of an ethylene-propylene-butene copolymer. From the viewpoint of adhesiveness, it is preferable to use a polyolefin resin having a propylene unit content ratio of 50 mol % to 98 mol %. When the propylene unit content ratio is within the above range, flexibility can be imparted to the bonded part after bonding two members. The weight average molecular weight (Mw) of the polyolefin resin (C) is preferably 30,000 to 250,000, and more preferably 50,000 to 200,000. When the weight average molecular weight (Mw) of the polyolefin resin (C) is within the above range, a resin composition having excellent solubility in a solvent and adhesiveness to an adherend can be obtained. Furthermore, these can also be suitably used as unmodified polyolefin resins which are raw materials for modified polyolefin resins.
[0038] The modified polyolefin resin is preferably a resin having a portion derived from an unmodified polyolefin resin and a graft portion derived from a modifying agent, and is more preferably one obtained by graft polymerization of a modifying agent containing an α,β-unsaturated carboxylic acid or a derivative thereof in the presence of an unmodified polyolefin resin. The modified polyolefin resin can be produced by graft polymerization using a known method, and a radical initiator may be used during the production. Examples of methods for producing modified polyolefin resins include a solution method in which an unmodified polyolefin resin is heated and dissolved in a solvent such as toluene, and the modifier and radical initiator are added, and a melt method in which an unmodified polyolefin resin, a modifier, and a radical initiator are melt-kneaded using a Banbury mixer, a kneader, an extruder, etc. The method for using the unmodified polyolefin resin, the modifier, and the radical initiator is not particularly limited, and they may be added to the reaction system all at once or successively.
[0039] When producing a modified polyolefin resin, a modifying assistant for improving the grafting efficiency of the α,β-unsaturated carboxylic acid, a stabilizer for adjusting the resin stability, etc. can be further used.
[0040] The modifier includes α,β-unsaturated carboxylic acids and their derivatives. Examples of α,β-unsaturated carboxylic acids include maleic acid, fumaric acid, tetrahydrophthalic acid, itaconic acid, citraconic acid, crotonic acid, aconitic acid, and norbornene dicarboxylic acid. Examples of derivatives of unsaturated polycarboxylic acids include acid anhydrides, acid halides, amides, imides, and esters. The modifying agent is preferably itaconic anhydride, maleic anhydride, aconitic anhydride, or citraconic anhydride, and itaconic anhydride or maleic anhydride is particularly preferred in terms of adhesiveness. When a modifying agent is used, it may be one or more selected from α,β-unsaturated carboxylic acids and their derivatives, and may be a combination of one or more α,β-unsaturated carboxylic acids and one or more derivatives thereof, a combination of two or more α,β-unsaturated carboxylic acids, or a combination of two or more derivatives of α,β-unsaturated carboxylic acids.
[0041] The modifying agent used in the present invention may contain other compounds (other modifying agents) in addition to the α,β-unsaturated carboxylic acid, etc., depending on the purpose. Examples of the other compounds (other modifiers) include (meth)acrylic acid esters represented by the following formula (1), (meth)acrylic acid, other (meth)acrylic acid derivatives, aromatic vinyl compounds, cyclohexyl vinyl ether, etc. These other compounds may be used alone or in combination of two or more. CH2=CR A1 COOR A2 (1) (In the formula, R A1 is a hydrogen atom or a methyl group, R A2 is a hydrocarbon group.)
[0042] In the formula (1), R A1 is preferably a methyl group. A2 is preferably an alkyl group having 8 to 18 carbon atoms. Examples of the compound represented by the formula (1) include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, and benzyl (meth)acrylate. These compounds may be used alone or in combination of two or more. In the present invention, since the heat-resistant adhesiveness is improved, it is preferable to use a modifier further containing a (meth)acrylic acid ester having an alkyl group having 8 to 18 carbon atoms, and it is particularly preferable to contain octyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, or stearyl (meth)acrylate.
[0043] Examples of (meth)acrylic acid derivatives other than (meth)acrylic acid esters include hydroxyethyl (meth)acrylate, glycidyl (meth)acrylate, and isocyanate-containing (meth)acrylic acid. Examples of the aromatic vinyl compound include styrene, o-methylstyrene, p-methylstyrene, and α-methylstyrene. By using an α,β-unsaturated carboxylic acid or its derivative in combination with another modifier as the modifier, it is possible to improve the graft ratio by the modifier, improve the solubility in a solvent, and further improve the adhesiveness. When using another modifier other than the (meth)acrylic acid ester represented by the formula (1), it is preferable that the amount used does not exceed the total amount used of the α,β-unsaturated carboxylic acid and its derivative and the (meth)acrylic acid ester.
[0044] As described above, the modified polyolefin resin preferably has at least a graft portion derived from a modifier. Hereinafter, the content ratio of the graft portion contained in the modified polyolefin resin (hereinafter, also referred to as "graft mass") will be described.
[0045] The modified polyolefin resin preferably has a graft portion derived from an α,β-unsaturated carboxylic acid or a derivative thereof. In the modified polyolefin resin, the graft mass of the graft portion derived from an α,β-unsaturated carboxylic acid or a derivative thereof is preferably 0.1% by mass to 20% by mass, more preferably 0.2% by mass to 18% by mass, based on 100% by mass of the modified polyolefin resin, from the viewpoint of adhesiveness. When the graft mass is 0.1% by mass or more, the solubility in a solvent is excellent, and the adhesiveness to an adherend made of metal or the like is particularly excellent. When the graft mass is 20% by mass or less, sufficient adhesiveness to an adherend made of resin or the like can be obtained.
[0046] The graft mass derived from an α,β-unsaturated carboxylic acid or a derivative thereof in a modified polyolefin resin can be determined by an alkali titration method. However, when the derivative of the α,β-unsaturated carboxylic acid is an imide or the like that does not have an acid group, the graft mass can be determined by Fourier transform infrared spectroscopy.
[0047] When the modified polyolefin resin contains a graft portion derived from a (meth)acrylic acid ester represented by the formula (1), the graft mass is preferably 0.1% by mass to 30% by mass, and more preferably 0.3% by mass to 25% by mass, relative to 100% by mass of the modified polyolefin resin. When the graft mass is 0.1% by mass to 30% by mass, the resin has excellent solubility in solvents and excellent compatibility with other resins or elastomers, which will be described later, when such resins or elastomers are contained, and the adhesiveness to the adherend can be further improved.
[0048] When the modifying agent contains a (meth)acrylic acid ester represented by the above formula (1), the graft mass in the obtained modified polyolefin resin can be determined by Fourier transform infrared spectroscopy.
[0049] The radical initiator used in the production of the modified polyolefin resin can be appropriately selected from known ones. For example, it is preferable to use an organic peroxide such as benzoyl peroxide, dicumyl peroxide, lauroyl peroxide, di-t-butyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, or cumene hydroperoxide.
[0050] Examples of the modifying auxiliary that can be used in the production of the modified polyolefin resin include divinylbenzene, hexadiene, dicyclopentadiene, etc. Examples of the stabilizer that can be used include hydroquinone, benzoquinone, nitrosophenyl hydroxy compounds, etc.
[0051] The weight average molecular weight (Mw) of the polyolefin resin (C) is preferably from 10,000 to 300,000, more preferably from 30,000 to 250,000, and particularly preferably from 50,000 to 200,000, from the viewpoints of solubility, adhesiveness, and solvent resistance after curing.
[0052] The acid value of the modified polyolefin resin is preferably 0.1 mgKOH / g to 50 mgKOH / g, more preferably 0.5 mgKOH / g to 40 mgKOH / g, and even more preferably 1.0 mgKOH / g to 30 mgKOH / g, from the viewpoints of the stability over time, adhesion, and solder reflow properties of the resin composition.
[0053] The resin composition of the present invention may contain one type of polyolefin resin (C) alone, or may contain two or more types. From the viewpoints of adhesion, electrical conductivity, and heat resistance, the content of the polyolefin resin (C) is preferably 5% by mass to 90% by mass, more preferably 10% by mass to 70% by mass, and particularly preferably 30% by mass to 70% by mass, based on the total amount of resin solids excluding the filler component in the resin composition. Furthermore, from the viewpoints of adhesion, conductivity, and heat resistance, the content of the polyester polyurethane resin (A) and the polyolefin resin (C) in the resin composition is preferably 50% by mass to 98% by mass, more preferably 70% by mass to 97% by mass, and particularly preferably 75% by mass to 95% by mass, based on the total amount of resin solids excluding the filler component.
[0054] <Organic filler (D)> The resin composition of the present invention preferably contains an organic filler (D) from the viewpoints of the extensibility, electrical conductivity, and moist heat resistance of the resulting cured product. Examples of the organic filler (D) include (meth)acrylic resin particles, polybutadiene particles, nylon particles, polyolefin particles, polyester particles, polycarbonate particles, polyvinyl alcohol particles, polyvinyl ether particles, polyvinyl butyral particles, silicone rubber particles, polyurethane particles, phenolic resin particles, and polytetrafluoroethylene particles. The present inventors have found that when an organic filler is mixed with a polyester polyurethane resin (A), an epoxy resin (B) and a polyolefin resin (C), the compatibility of these resins is further improved. Furthermore, from the viewpoint of further improving the compatibility and liquid stability of these resins, silicone particles, polybutadiene particles, (meth)acrylic resin particles, or polyurethane particles are particularly preferred as the organic filler (D). From the viewpoint of electrical conductivity, (meth)acrylic resin particles or polyurethane particles are preferred.
[0055] The average particle size of the organic filler (D) is not particularly limited, but from the viewpoints of coatability and coat thickness control, it is preferably 0.5 μm to 50 μm, and more preferably 1 μm to 30 μm.
[0056] The resin composition of the present invention may contain one type of organic filler (D) alone, or may contain two or more types. From the viewpoints of adhesion, conductivity, and curability, the content of the organic filler (D) in the resin composition is preferably 1 to 50 parts by mass, more preferably 5 to 40 parts by mass, and particularly preferably 10 to 20 parts by mass, per 100 parts by mass of the total amount of resin solids excluding the filler component.
[0057] <Metal filler (E)> From the viewpoints of electrical conductivity and heat resistance, the resin composition of the present invention preferably contains a metal filler (E). From the viewpoints of electrical conductivity and heat resistance, the metal filler (E) is preferably an electrically conductive filler, and more preferably a metal particle made of an electrically conductive metal such as gold, platinum, silver, copper, or nickel, or an alloy thereof. Also, from the viewpoint of cost reduction, particles having a core of metal or resin, and a coating layer formed of a material with high electrical conductivity, rather than particles of a single composition, are also preferable. The core is preferably made of at least one material selected from the group consisting of nickel, silica, copper, and resin, and more preferably made of an electrically conductive metal or an alloy thereof. The coating layer is preferably a layer made of a material with excellent electrical conductivity, and is preferably a layer made of an electrically conductive metal or an electrically conductive polymer. Examples of conductive metals include gold, platinum, silver, tin, manganese, and indium, as well as alloys thereof. Examples of conductive polymers include polyaniline and polyacetylene. Among these, silver is preferred in terms of electrical conductivity.
[0058] From the viewpoints of cost and electrical conductivity, the particles consisting of the core and the coating layer preferably have the coating layer in a ratio of 1 part by mass to 40 parts by mass, and more preferably 5 parts by mass to 30 parts by mass, per 100 parts by mass of the core.
[0059] The particles consisting of the core and the coating layer are preferably particles in which the coating layer completely covers the core. However, in reality, there are cases where a part of the core is exposed. Even in such cases, if 70% or more of the core surface area is covered with a conductive material, the conductivity is easily maintained.
[0060] The shape of the metal filler (E) is not limited as long as the desired electrical conductivity is obtained. Specifically, for example, a spherical, flake, leaf, dendritic, plate, needle, rod, or grape shape is preferable.
[0061] From the viewpoints of electrical conductivity and storage stability, the average particle size of the metal filler (E) is preferably from 1 μm to 100 μm, more preferably from 3 μm to 50 μm, and particularly preferably from 4 μm to 15 μm. The average particle size of the particles in this disclosure is the D50 average particle size obtained by measuring each conductive fine particle powder with a tornado dry powder sample module using a laser diffraction / scattering particle size distribution analyzer LS 13320 (manufactured by Beckman Coulter, Inc.), and the average particle size of the particle diameter at which the cumulative value of the particles is 50% is used. The refractive index was set to 1.6. The average particle size of the metal filler (E) can also be determined by averaging about 20 randomly selected particles in an electron microscope magnified image (approximately 1,000 to 10,000 times). In this case, the average particle size is also preferably 1 μm to 100 μm, more preferably 3 μm to 50 μm. When the metal filler (E) has a long axis direction and a short axis direction (e.g., rod-shaped particles), the average particle size is calculated based on the length in the long axis direction.
[0062] The resin composition of the present invention may contain one type of metal filler (E) alone, or may contain two or more types. From the viewpoints of electrical conductivity, heat resistance, and storage stability, the content of the metal filler (E) in the resin composition is preferably 1 part by mass to 500 parts by mass, more preferably 10 parts by mass to 350 parts by mass, and particularly preferably 10 parts by mass to 50 parts by mass, per 100 parts by mass of the total amount of resin solids excluding the filler component.
[0063] The resin composition of the present invention may contain additives other than the above-mentioned components. Other additives may include thermoplastic resins other than those mentioned above, tackifiers, flame retardants, curing agents, curing accelerators, coupling agents, heat aging inhibitors, leveling agents, defoamers, inorganic fillers, solvents, and the like, to the extent that they do not affect the functions of the resin composition.
[0064] Examples of the other thermoplastic resins include phenoxy resins, polyester resins, polycarbonate resins, polyphenylene oxide resins, polyurethane resins, polyacetal resins, polyethylene-based resins, polypropylene-based resins, polyvinyl-based resins, etc. These thermoplastic resins may be used alone or in combination of two or more.
[0065] Examples of the tackifier include coumarone-indene resin, terpene resin, terpene-phenol resin, rosin resin, pt-butylphenol-acetylene resin, phenol-formaldehyde resin, xylene-formaldehyde resin, petroleum-based hydrocarbon resin, hydrogenated hydrocarbon resin, turpentine-based resin, etc. These tackifiers may be used alone or in combination of two or more.
[0066] The flame retardant may be either an organic flame retardant or an inorganic flame retardant. Examples of organic flame retardants include phosphorus-based flame retardants such as melamine phosphate, melamine polyphosphate, guanidine phosphate, guanidine polyphosphate, ammonium phosphate, ammonium polyphosphate, ammonium amido phosphate, ammonium amido polyphosphate, carbamate phosphate, carbamate polyphosphate, aluminum trisdiethylphosphinate, aluminum trismethylethylphosphinate, aluminum trisdiphenylphosphinate, zinc bisdiethylphosphinate, zinc bismethylethylphosphinate, zinc bisdiphenylphosphinate, titanyl bisdiethylphosphinate, titanium tetrakisdiethylphosphinate, titanyl bismethylethylphosphinate, titanium tetrakismethylethylphosphinate, titanyl bisdiphenylphosphinate, and titanium tetrakisdiphenylphosphinate; nitrogen-based flame retardants such as triazine-based compounds such as melamine, melam, and melamine cyanurate, cyanuric acid compounds, isocyanuric acid compounds, triazole-based compounds, tetrazole compounds, diazo compounds, and urea; and silicon-based flame retardants such as silicone compounds and silane compounds. Examples of inorganic flame retardants include metal hydroxides such as aluminum hydroxide, magnesium hydroxide, zirconium hydroxide, barium hydroxide, and calcium hydroxide; metal oxides such as tin oxide, aluminum oxide, magnesium oxide, zirconium oxide, zinc oxide, molybdenum oxide, and nickel oxide; zinc carbonate, magnesium carbonate, calcium carbonate, barium carbonate, zinc borate, and hydrated glass. These flame retardants may be used alone or in combination of two or more.
[0067] The curing agent is a component for forming a crosslinked structure by reaction with the epoxy resin (B), and examples thereof include amine-based curing agents such as aliphatic diamines, aliphatic polyamines, cyclic aliphatic diamines, and aromatic diamines, polyamidoamine-based curing agents, acid-based curing agents such as aliphatic polycarboxylic acids, alicyclic polycarboxylic acids, aromatic polycarboxylic acids, and acid anhydrides thereof, basic active hydrogen-based curing agents such as dicyandiamide and organic acid dihydrazides, polymercaptan-based curing agents, novolac resin-based curing agents, urea resin-based curing agents, and melamine resin-based curing agents. These curing agents may be used alone or in combination of two or more.
[0068] Examples of the aliphatic diamine curing agent include ethylenediamine, 1,3-diaminopropane, 1,4-diaminobutane, hexamethylenediamine, polymethylenediamine, polyetherdiamine, 2,5-dimethylhexamethylenediamine, and trimethylhexamethylenediamine.
[0069] Examples of the aliphatic polyamine curing agent include diethylenetriamine, iminobis(hexamethylene)triamine, trihexatetramine, tetraethylenepentamine, aminoethylethanolamine, tri(methylamino)hexane, dimethylaminopropylamine, diethylaminopropylamine, and methyliminobispropylamine.
[0070] Examples of cyclic aliphatic diamine curing agents include benzenediamine, isophoronediamine, bis(4-amino-3-methyldicyclohexyl)methane, diaminodicyclohexylmethane, bis(aminomethyl)cyclohexane, N-ethylaminopiperazine, 3,9-bis(3-aminopropyl)2,4,8,10-tetraoxaspiro[5.5]undecane, and hydrogenated metaxylylenediamine.
[0071] Examples of the aromatic diamine curing agent include metaphenylenediamine, diaminodiphenylmethane, diaminodiphenylsulfone, diaminodiethyldiphenylmethane, and metaxylylenediamine.
[0072] Examples of the aliphatic polyvalent carboxylic acid-based hardener and the acid anhydride-based hardener include succinic acid, adipic acid, dodecenyl succinic anhydride, polyadipic anhydride, polyazelaic anhydride, and polysebacic anhydride.
[0073] Examples of alicyclic polyvalent carboxylic acid curing agents and acid anhydride curing agents include methyltetrahydrophthalic acid, methylhexahydrophthalic acid, methylhimic acid, hexahydrophthalic acid, tetrahydrophthalic acid, trialkyltetrahydrophthalic acid, methylcyclodicarboxylic acid, and acid anhydrides thereof.
[0074] Examples of aromatic polyvalent carboxylic acid-based curing agents and acid anhydride-based curing agents include phthalic acid, trimellitic acid, pyromellitic acid, benzophenone tetracarboxylic acid, ethylene glycol glycol bistrimellitic acid, glycerol tristrimellitic acid, and acid anhydrides thereof.
[0075] Examples of the polymercaptan-based curing agent include mercapto-modified epoxy resins and mercaptopropionic acid esters.
[0076] Examples of the novolac-based hardener include a phenol novolac-based hardener and a cresol novolac-based hardener.
[0077] When the resin composition of the present invention contains the curing agent, the content of the curing agent is set so that the functional group equivalent thereof is preferably in the range of 0.2 to 2.5 molar equivalents, more preferably in the range of 0.4 to 2.0 molar equivalents, relative to 1 molar equivalent of the epoxy group of the epoxy resin (B), from the viewpoints of adhesiveness and heat resistance.
[0078] The curing accelerator is a component used for the purpose of accelerating the reaction of the epoxy resin (B), and examples of the curing accelerator that can be used include tertiary amine curing accelerators, tertiary amine salt curing accelerators, and imidazole curing accelerators. These curing accelerators may be used alone or in combination of two or more.
[0079] Examples of the tertiary amine curing accelerator include benzyldimethylamine, 2-(dimethylaminomethyl)phenol, 2,4,6-tris(dimethylaminomethyl)phenol, tetramethylguanidine, triethanolamine, N,N'-dimethylpiperazine, triethylenediamine, and 1,8-diazabicyclo[5.4.0]undecene.
[0080] Examples of the tertiary amine salt curing accelerator include the formate, octylate, p-toluenesulfonate, o-phthalate, phenol salt, and phenol novolac resin salt of 1,8-diazabicyclo[5.4.0]undecene; and the formate, octylate, p-toluenesulfonate, o-phthalate, phenol salt, and phenol novolac resin salt of 1,5-diazabicyclo[4.3.0]nonene.
[0081] Imidazole-based curing accelerators include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-methyl-4-ethylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'- undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, and the like.
[0082] When the resin composition of the present invention contains a curing accelerator, the content of the curing accelerator is preferably 1 to 10 parts by mass, and more preferably 2 to 5 parts by mass, per 100 parts by mass of the epoxy resin (B) from the viewpoints of adhesion and heat resistance.
[0083] Examples of the coupling agent include silane-based coupling agents such as vinyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-acryloxypropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-ureidopropyltriethoxysilane, 3-mercaptopropylmethyldimethoxysilane, bis(triethoxysilylpropyl)tetrasulfide, 3-isocyanatepropyltriethoxysilane, and imidazolesilane; titanate-based coupling agents; aluminate-based coupling agents; and zirconium-based coupling agents. These may be used alone or in combination of two or more.
[0084] Examples of the heat aging inhibitor include phenol-based antioxidants such as 2,6-di-tert-butyl-4-methylphenol, n-octadecyl-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate, and tetrakis[methylene-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]methane; sulfur-based antioxidants such as dilauryl-3,3'-thiodipropionate and dimyristyl-3,3'-dithiopropionate; and phosphorus-based antioxidants such as trisnonylphenyl phosphite and tris(2,4-di-tert-butylphenyl)phosphite. These may be used alone or in combination of two or more.
[0085] Examples of the inorganic filler include powders made of calcium carbonate, titanium oxide, aluminum oxide, zinc oxide, carbon black, talc, silica, etc. These may be used alone or in combination of two or more.
[0086] The resin composition of the present invention can be prepared by mixing the polyester polyurethane resin (A), the epoxy resin (B), and the polyolefin resin (C), and, if necessary, other components. Since the resin composition of the present invention is preferably used in the state of a solution or dispersion, it preferably contains a solvent. Examples of the solvent include alcohols such as methanol, ethanol, isopropyl alcohol, n-propyl alcohol, isobutyl alcohol, n-butyl alcohol, benzyl alcohol, ethylene glycol monomethyl ether, propylene glycol monomethyl ether, diethylene glycol monomethyl ether, and diacetone alcohol; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, methyl amyl ketone, cyclohexanone, and isophorone; aromatic hydrocarbons such as toluene, xylene, ethylbenzene, and mesitylene; esters such as methyl acetate, ethyl acetate, ethylene glycol monomethyl ether acetate, and 3-methoxybutyl acetate; and aliphatic hydrocarbons such as hexane, heptane, cyclohexane, and methylcyclohexane. These solvents may be used alone or in combination of two or more. When the resin composition of the present invention is a solution or dispersion containing a solvent, coating on an adherend and formation of a resin composition layer can be smoothly performed, and a resin composition layer of a desired thickness can be easily obtained.
[0087] When the resin composition of the present invention contains a solvent, from the viewpoint of workability including film-forming property, the solvent is used so that the solid content concentration is preferably in the range of 3 mass % to 80 mass %, more preferably 10 mass % to 50 mass %.
[0088] Suitable adherends for the resin composition of the present invention are objects made of polymeric materials such as polyimide resins, polyether ether ketone resins, polyphenylene sulfide resins, aramid resins, and liquid crystal polymers; and metal materials such as copper, aluminum, and stainless steel. The shape of the adherend is not particularly limited. Two members made of the same material or different materials as the adherend can be bonded together with the resin composition of the present invention to produce an integrated composite. In addition, products having a resin composition layer with adhesive properties, such as the following coverlay films and bonding sheets, can be produced.
[0089] (Laminate with Resin Composition Layer, and Laminate) The laminate with a resin composition layer of the present invention is a laminate having a resin composition layer made of the resin composition of the present invention, and is provided with a resin composition layer made of the resin composition of the present invention and a base film in contact with at least one side of the resin composition layer, and it is preferable that the resin composition layer is in a B-stage state. In the present invention, the resin composition layer being in the B stage refers to a semi-cured state in which a part of the resin composition layer has begun to cure, and the curing of the resin composition layer can be further promoted by heating or the like. When a resin composition containing a solvent is used, the resin composition layer made of the resin composition of the present invention is preferably a layer made of the resin composition of the present invention from which at least a part of the solvent has been removed. The laminate of the present invention is a laminate having a cured layer formed by curing a resin composition comprising the resin composition of the present invention, and preferably includes a cured layer formed by curing the resin composition of the present invention and a base film in contact with at least one surface of the cured layer.
[0090] The laminate with a resin composition layer of the present invention and the laminate of the present invention preferably have a substrate, and more preferably have a layer made of the resin composition of the present invention on the substrate. The substrate is not particularly limited, and any known substrate can be used. The substrate is preferably a film-like substrate (substrate film). The substrate film is preferably a resin film, more preferably a polyimide film or an aramid film, and particularly preferably a polyimide film. The polyimide film or aramid film is not particularly limited as long as it has electrical insulation properties, and may be a film made of only a polyimide resin or an aramid resin, or a film containing the resin and an additive, and the side on which the resin composition layer is formed may be subjected to a surface treatment. The thickness of the substrate is not particularly limited, but is preferably 3 μm to 125 μm. The thickness of the resin composition layer is preferably from 5 μm to 50 μm, and more preferably from 10 μm to 40 μm.
[0091] As a method for producing a laminate with a resin composition layer of the present invention, for example, the resin composition of the present invention containing a solvent is applied to the surface of a base film such as a polyimide film to form a resin composition layer, and then at least a portion of the solvent is removed from the resin composition layer to produce a laminate having a B-stage resin composition layer. The drying temperature when removing the solvent is preferably from 40°C to 250°C, and more preferably from 70°C to 170°C. The drying is carried out by passing the laminate coated with the resin composition through a furnace in which hot air drying, far infrared heating, high frequency induction heating, or the like is performed. The laminate with a resin composition layer of the present invention may further have a release film on the surface of the resin composition layer for storage or the like, if necessary. The release film may be a known film such as a polyethylene terephthalate film, a polyethylene film, a polypropylene film, silicone release treated paper, a polyolefin resin coated paper, a polymethylpentene (TPX) film, or a fluorine-based resin film.
[0092] The thickness of the B-stage resin composition layer is preferably 5 μm to 100 μm, more preferably 5 μm to 70 μm, further preferably 5 μm to 50 μm, and particularly preferably 10 μm to 40 μm. The thickness of the base film and the resin composition layer is selected depending on the application, but the base film tends to be thinner in order to improve electrical properties. The preferred thickness of the base film is the same as the preferred thickness of the base material described above. In the laminate with a resin composition layer of the present invention, the ratio (A / B) of the thickness (A) of the resin composition layer to the thickness (B) of the base film is preferably 1 or more and 10 or less, and more preferably 1 or more and 5 or less. Furthermore, it is preferable that the thickness of the resin composition layer is thicker than the thickness of the base film.
[0093] As a method for producing the laminate of the present invention, for example, the resin composition of the present invention containing a solvent is applied to the surface of a substrate film, and then dried in the same manner as in the case of the laminate with a resin composition layer of the present invention, and then the surface of the formed resin composition layer is brought into surface contact with an adherend, and lamination, for example, thermal lamination is performed at 80° C. to 150° C. Next, this laminate (substrate film / resin composition layer / adherend) is heated and pressed, and further the resin composition layer is cured by after-curing to form a cured layer. The conditions for the thermocompression bonding are not particularly limited as long as the bonding is possible, but are preferably 150°C to 200°C, 1 MPa to 3 MPa pressure, and 1 minute to 60 minutes. The conditions for the aftercure are not particularly limited, but are preferably 100°C to 200°C, 30 minutes to 4 hours. The thickness of the cured layer is preferably from 5 μm to 100 μm, more preferably from 5 μm to 70 μm, further preferably from 5 μm to 50 μm, and particularly preferably from 10 μm to 40 μm. The adherend is not particularly limited, and examples thereof include those mentioned above. Among them, metal adherends are preferred, copper foil or plated copper foil is more preferred, and gold-plated copper foil is particularly preferred. The shape and size of the adherend are not particularly limited, and any known shape and size can be used.
[0094] One embodiment of the laminate of the present invention is a flexible copper-clad laminate. That is, the flexible copper-clad laminate of the present invention has a cured layer formed by curing a resin composition comprising the resin composition of the present invention, and preferably comprises a polyimide film or aramid film, a cured layer formed by curing the resin composition of the present invention, and a copper foil laminated therewith. In the flexible copper-clad laminate of the present invention, the cured layer and the copper foil may be formed on both sides of a polyimide film or an aramid film. Since the resin composition of the present invention has excellent adhesion to an article containing copper, the flexible copper-clad laminate of the present invention has excellent stability as an integrated product.
[0095] The configuration of the polyimide film or aramid film is the same as that of the polyimide film or aramid film in the coverlay film of the present invention described above. The thickness of the hardened layer is preferably from 5 μm to 50 μm, and more preferably from 10 μm to 40 μm. The copper foil is not particularly limited, and electrolytic copper foil, rolled copper foil, etc. can be used. Additionally, the copper foil may be plated with known metals or alloys such as gold or silver.
[0096] Examples of the laminate with a resin composition layer of the present invention include a bonding film, an electromagnetic wave shielding film, a coverlay film, and the like, which will be described later.
[0097] -Bonding film- The bonding film of the present invention has a resin composition layer made of the resin composition of the present invention, and is provided with a resin composition layer made of the resin composition of the present invention and a release film in contact with at least one side of the resin composition layer, and it is preferable that the resin composition layer is in a B-stage state. The bonding film of the present invention is also one embodiment of the laminate with a resin composition layer of the present invention described below. The bonding film of the present invention may have an embodiment in which a resin composition layer is provided between two release films. As the release film, known films as described above are used. The release film preferably has a thickness of 20 μm to 100 μm. The thickness of the resin composition layer is preferably from 5 μm to 100 μm, and more preferably from 10 μm to 60 μm.
[0098] A preferred method for producing the bonding sheet of the present invention is, for example, to coat the surface of a release film with the resin composition of the present invention containing a solvent, and then drying in the same manner as in the case of the laminate with a resin composition layer of the present invention described above.
[0099] -Electromagnetic wave shielding film- The electromagnetic wave shielding film of the present invention has a resin composition layer made of the resin composition of the present invention, and may also have a base film or a release film in contact with at least one surface of the resin composition layer. The electromagnetic wave shielding film of the present invention preferably has the resin composition layer and a protective layer. The protective layer is not particularly limited as long as it is a layer made of an insulating resin composition, and any known layer can be used. The protective layer may also use the resin component used in the resin composition of the present invention. Furthermore, the protective layer may be formed of two or more layers having different compositions and hardness. Furthermore, the protective layer may contain, as necessary, a curing accelerator, a tackifier, an antioxidant, a pigment, a dye, a plasticizer, an ultraviolet absorber, an antifoaming agent, a leveling agent, a filler, a flame retardant, a viscosity adjuster, an antiblocking agent, and the like.
[0100] The thickness of the resin composition layer in the electromagnetic wave shielding film of the present invention is not particularly limited, but from the viewpoints of electrical conductivity and connectivity with a ground circuit, it is preferably 3 μm to 30 μm.
[0101] Next, a specific embodiment of the method for producing the electromagnetic wave shielding film of the present invention will be described. For example, a method can be mentioned in which a resin composition for a protective layer is coated and dried on one side of a peelable film to form a protective layer, and then the resin composition of the present invention is coated and dried on the protective layer to form a resin composition layer. By the production method as exemplified above, it is possible to obtain an electromagnetic wave shielding film having a laminated structure of resin composition layer / protective layer / peelable film.
[0102] The resin composition layer and the protective layer can be provided by a conventionally known coating method, such as a gravure coating method, a kiss coating method, a die coating method, a lip coating method, a comma coating method, a blade coating method, a roll coating method, a knife coating method, a spray coating method, a bar coating method, a spin coating method, or a dip coating method.
[0103] The electromagnetic wave shielding film of the present invention can be adhered to a printed wiring board by, for example, heat pressing. The resin composition layer is softened by heating and flows into the ground part provided on the printed wiring board by applying pressure. This electrically connects the ground circuit and the conductive adhesive, thereby enhancing the shielding effect. EXAMPLES
[0104] The present invention will be specifically described below based on examples. Note that the present invention is not limited to these examples. In the following, "parts" and "%" mean "parts by mass" and "% by mass", respectively, unless otherwise specified.
[0105] 1.Raw materials 1-1.Polyester The polyesters used in the production of the polyester polyurethane resins were either commercially available or synthetic products.
[0106] <Commercially available products> The commercially available product used was ARONMELT PES-360HVXM30 manufactured by Toagosei Co., Ltd. ARONMELT PES-360HVXM30 had a number average molecular weight of 20,000.
[0107] <Synthesis of polyester (PES-1)> A flask equipped with a stirrer, a nitrogen inlet tube, a distillation tube, and a thermometer was charged with 201 parts by mass of dimethyl terephthalate, 86 parts by mass of ethylene glycol, 140 parts by mass of neopentyl glycol, 0.9 parts by mass of trimethylolpropane, and 0.22 parts by mass of zinc acetate as a catalyst. The temperature was raised while introducing nitrogen, and methanol was distilled at 150°C to 180°C. After that, 183 parts by mass of isophthalic acid, 0.6 parts by mass of trimethylolpropane, and 0.12 parts by mass of antimony trioxide were added, and water was distilled at 180°C to 210°C. The pressure was gradually reduced, and the reaction was continued for 6 hours at 230°C under a reduced pressure of 200 Pa. The obtained polyester resin had a number average molecular weight of 7,000. 180 parts by mass of the synthesized polyester resin was taken, and 378 parts by mass of toluene and 42 parts by mass of methyl isobutyl ketone were added to obtain a polyester solution (PES-1).
[0108] 1-2. Polyester polyurethane resin The polyester polyurethane resins a1 to a7 obtained by the following method were used.
[0109] (1) Polyester polyurethane resin A1 In a flask equipped with a stirrer, a reflux dehydration device, and a distillation tube, 600 parts by mass of PES-360HVXM30, 100 parts by mass of toluene, and 20 parts by mass of neopentyl glycol were charged. After raising the temperature to 120°C to distill off 100 parts by mass of a solvent containing water, the temperature was lowered to 105°C, and 0.4 parts by mass of 2,2-bis(hydroxymethyl)propionic acid was charged and dissolved. Then, 34 parts by mass of hexamethylene diisocyanate was added, and 30 minutes later, 0.2 parts by mass of dimethyltin dilaurate was added. After continuing the reaction for 6 hours, a solution of polyester polyurethane resin a1 was obtained in which the solid content concentration was adjusted to 30% by dilution with toluene / 2-propanol. The number average molecular weight of polyester polyurethane resin a1 was 36,000, and the acid value was 2 mgKOH / g.
[0110] (2) Synthesis of polyester polyurethane resins A2 to A7 The synthesis was carried out in the same manner as in the synthesis of polyester polyurethane resin a1, except that the polyester, diol, and diisocyanate shown in Table 1 were changed to the parts by mass shown in the table.
[0111] [Table 1]
[0112] The units of the numerical values in the column for each component in Table 1 are parts by mass.
[0113] 1-3.Epoxy resin (B) The following commercially available products were used: (1) Epoxy resin B1 Bisphenol A novolac epoxy resin "EPICLON N-865" (product name) manufactured by DIC Corporation (2) Epoxy resin B2 Mitsubishi Chemical Corporation's bisphenol A epoxy resin "jER 1055" (product name)
[0114] 1-4.Polyolefin resin (C) (1) Polyolefin resin c1 100 parts by mass of a propylene-butene random copolymer consisting of 80% by mass of propylene units and 20% by mass of butene units produced using a metallocene catalyst as a polymerization catalyst, 1 part by mass of maleic anhydride, 0.3 parts by mass of lauryl methacrylate, and 0.4 parts by mass of di-t-butyl peroxide were kneaded and reacted using a twin-screw extruder with the maximum temperature of the cylinder set to 170°C. Thereafter, degassing was performed under reduced pressure in the extruder to remove the remaining unreacted material, producing polyolefin resin c1. The polyolefin resin c1 had a weight average molecular weight of 80,000 and an acid value of 10 mgKOH / g. The content of the grafted portion in the polyolefin resin c1 was 1.5% by mass. (2) Olefin resin c2 Using a metallocene catalyst as a polymerization catalyst, 80% by mass of propylene units and 20% by mass of butene units were reacted to obtain polyolefin resin c2. The polyolefin resin c2 had a weight average molecular weight of 100,000.
[0115] 1-5. Organic filler (D) (1) Filler d1 Negami Chemical Industries Co., Ltd.'s urethane beads "TK-800T" (product name, average particle size 8μm) (2) Filler d2 Acrylic beads “J-4P” manufactured by Negami Kogyo Co., Ltd. (trade name, average particle size 2.2 μm)
[0116] 1-6. Metal filler (E) Copper powder "FCC-115A" manufactured by Fukuda Metal Foil & Powder Co., Ltd. (product name, particle size distribution: particles of 45 μm or less exceed 90% by mass, particles of 45 μm to 63 μm are less than 10% by mass, and particles of 63 μm to 75 μm are less than 3% by mass).
[0117] 1-7.Flame retardants Clariant aluminum dimethylphosphinate "Exolit OP935" (product name)
[0118] 1-8.Curing accelerator Imidazole-based curing accelerator "Curesol C11-Z" (product name) manufactured by Shikoku Chemical Industry Co., Ltd.
[0119] 1-9.Solvent A mixed solvent of toluene, methyl isobutyl ketone, 2-propanol, and methylcyclohexane (mass ratio = 100:20:20:20)
[0120] (Examples 1 to 19 and Comparative Examples 1 to 3) The above raw materials were added to a flask equipped with a stirrer in the ratio shown in Table 2, and stirred for 6 hours at 60°C to dissolve component (A), component (B), component (C), and the curing accelerator in the solvent, and disperse component (D), carbon black, and the flame retardant, thereby producing a liquid adhesive composition. Then, using all of these liquid adhesive compositions, coverlay films, bonding sheets, and adhesion test pieces A and B were produced, and the following evaluations (i) to (vi) were performed.
[0121] (1) Preparation of coverlay film The liquid adhesive composition was roll-coated on the surface of a 25 μm-thick polyimide film so that the thickness after drying would be 15 μm, and then dried at 120° C. for 2 minutes to obtain a coverlay film having an adhesive layer.
[0122] (2) Preparation of adhesive test piece A A gold-plated copper foil with a thickness of 35 μm was prepared. The gold-plated surface was then placed on the adhesive layer surface of the coverlay film, and lamination was performed under conditions of 150° C., 0.3 MPa, and 1 m / min. The resulting laminate (polyimide film / adhesive layer / gold-plated copper foil) was heated and pressed for 5 minutes under conditions of 150° C. and 3 MPa, and then after-cured in an oven at 160° C. for 2 hours to obtain an adhesion test piece A.
[0123] (3) Preparation of bonding sheet A release PET film having a thickness of 35 μm was prepared, and the liquid adhesive composition was roll-coated on the surface of the film so that the thickness after drying was 25 μm, and the film was dried at 140° C. for 2 minutes to obtain a bonding sheet having an adhesive layer.
[0124] (4) Preparation of adhesive test piece B A flexible printed wiring board was prepared, which had a copper circuit pattern formed on the surface of a 300 μm-thick nickel-plated SUS304 plate and a 25 μm-thick polyimide film, and a 37.5 μm-thick coverlay film with a 1 mm diameter through hole was laminated on the circuit pattern. First, the nickel-plated surface of the SUS304 plate was placed in contact with the adhesive layer surface of the bonding sheet, and lamination was performed under conditions of 150°C, 0.3 MPa, and 1 m / min to obtain a laminate (SUS plate / adhesive layer / releasable PET film). The release PET film was then peeled off, and the exposed surface of the adhesive layer was heated and pressed to a flexible printed wiring board (a wiring board in which a copper foil circuit was formed on a 25 μm thick polyimide, and a 37.5 μm thick coverlay film with a 1 mm diameter through hole was laminated on the copper foil circuit) at 150°C and 3 MPa for 5 minutes, and then after-cured in an oven at 160°C for 2 hours to produce adhesive test piece B (SUS plate / adhesive layer / flexible printed wiring board).
[0125] (i) Peel adhesion strength (initial) To evaluate the adhesiveness, the 180° peel adhesive strength (N / mm) was measured when peeling the gold-plated copper foil of each adhesive test piece A from the polyimide film at a temperature of 23°C and a tensile speed of 50 mm / min in accordance with JIS C 6481 "Test methods for copper-clad laminates for printed wiring boards." The width of the adhesive test piece during measurement was 10 mm.
[0126] (ii) Solder heat resistance (peel adhesion strength after soldering and appearance when soldered) The test was conducted in accordance with JIS C 6481 under the following conditions. The above-mentioned adhesive test piece A was floated in a solder bath at 260°C for 60 seconds with the polyimide film side facing up, and the adhesive layer was visually evaluated for the presence or absence of appearance abnormalities such as swelling and peeling. As a result, those that were not observed in appearance abnormalities such as microvoids, swelling, and peeling were marked as "A", those that were slightly observed in microvoids were marked as "B", and those that were observed in appearance abnormalities such as swelling and peeling were marked as "C". Furthermore, the test piece taken out of the above-mentioned solder bath was measured for 180° peel adhesion strength (N / cm) when peeling the polyimide film from the gold-plated copper foil at 23°C in accordance with JIS C 6481. The width of the adhesive test piece during the measurement was 10 mm, and the pulling speed was 50 mm / min.
[0127] (iii) Flame retardancy The coverlay film was heat cured at 160℃ for 2 hours and evaluated for flame retardancy in accordance with UL-94. Those that passed the test (VTM-0 class) were marked with "A", and those that failed were marked with "F".
[0128] (iv) Initial conductivity (connection resistance) The connection resistance between the SUS plate and the copper foil circuit of the flexible printed wiring board of the above adhesive test piece B (SUS plate / adhesive layer / flexible printed wiring board) was measured with a resistance meter. The connection resistance was then marked as "A" if it was less than 0.5Ω, "B" if it was 0.5Ω or more but less than 1Ω, "C" if it was 1Ω or more but less than 3Ω, and "D" if it was more than 3Ω.
[0129] (v) Conductivity (connection resistance) after soldering The above-mentioned adhesive test piece B was floated in a solder bath at 260°C for 60 seconds. After that, the connection resistance between the SUS plate of the adhesive test piece B taken out of the solder bath and the copper foil circuit of the flexible printed wiring board was measured with a resistance meter. The connection resistance values were as follows: less than 0.5Ω "A", 0.5Ω or more but less than 1Ω "B", 1Ω or more but less than 3Ω "C", and over 3Ω "D".
[0130] (vi) After long-term reliability test of electrical conductivity (connection resistance) The above-mentioned adhesive test piece B was left in a thermo-hygrostat at 85°C and 85% RH for 1000 hours. After that, the connection resistance between the SUS plate of the adhesive test piece B and the copper foil circuit of the flexible printed wiring board was measured with a resistance meter. The connection resistance was then marked as "A" if it was less than 0.5Ω, "B" if it was 0.5Ω or more but less than 1Ω, "C" if it was 1Ω or more but less than 3Ω, and "D" if it was more than 3Ω.
[0131] (vii) Storage stability of the adhesive composition The adhesive compositions of Examples 1 to 19 or Comparative Examples 1 to 3 having the compositions shown in Table 2 were each placed in a glass bottle, sealed, and stored at 5° C. for a predetermined time, and the crystallinity of the composition was observed. If gelation or liquid separation of the adhesive composition was confirmed after storage for the predetermined time, this was regarded as poor storage stability and evaluation was performed. <Evaluation criteria> A: More than a week F: Less than 1 week
[0132] [Table 2]
[0133] As is clear from the results shown in Table 2, the resin compositions of Examples 1 to 19 had excellent electrical conductivity even after long-term storage in a high-temperature, high-humidity environment, compared to the resin compositions of Comparative Examples 1 to 3. Furthermore, as is clear from the results shown in Table 2, the resin compositions of Examples 1 to 19 have excellent initial and post-solder adhesion, excellent appearance after solder formation, and excellent flame retardancy after curing.
[0134] The disclosure of Japanese Patent Application No. 2019-120891, filed on June 28, 2019, is incorporated herein by reference in its entirety. All publications, patent applications, and technical standards mentioned in this specification are herein incorporated by reference to the same extent as if each individual publication, patent application, or technical standard was specifically and individually indicated to be incorporated by reference.
Claims
1. Polyester polyurethane resin (A), Epoxy resin (B), and Contains a polyolefin resin (C), Contains an organic solvent, the polyester polyurethane resin (A) is a resin obtained by reacting at least a polyester polyol, a polyisocyanate, and a chain extender, the chain extender is a polyhydric alcohol compound, and a functional group ratio of isocyanate groups / hydroxy groups in a total of hydroxy groups of the polyester polyol and the chain extender and a total of isocyanate groups of the polyisocyanate is 0.9 or more and 1.1 or less; The polyolefin resin (C) is a resin graft-modified with a modifier containing an α,β-unsaturated carboxylic acid or a derivative thereof, Resin composition.
2. The content of the polyester polyurethane resin (A) is 10% by mass to 70% by mass, and the content of the polyolefin resin (C) is 10% by mass to 70% by mass, based on the total amount of resin solids excluding the filler component. The resin composition according to claim 1.
3. The resin composition according to claim 1 or 2, further comprising an organic filler (D).
4. The resin composition according to claim 3, comprising 5 to 40 parts by mass of an organic filler (D) per 100 parts by mass of the total amount of resin solids excluding the filler component.
5. The resin composition according to any one of claims 1 to 4, wherein the epoxy resin (B) comprises a bisphenol type epoxy resin and / or a bisphenol novolac type epoxy resin.
6. The resin composition according to any one of claims 1 to 5, wherein the number average molecular weight of the polyester polyurethane resin (A) is 10,000 to 80,000, and the molecular weight per urethane bond in the polyester polyurethane resin (A) is 200 to 8,000.
7. The resin composition according to any one of claims 1 to 6, wherein the polyester polyurethane resin (A) comprises a polyester polyurethane resin having a polyester structure and a number average molecular weight of 8,000 to 30,000.
8. The resin composition according to any one of claims 1 to 7, wherein the acid value of the polyester polyurethane resin (A) is 0.1 mg KOH / g to 20 mg KOH / g.
9. The resin composition according to any one of claims 1 to 8, wherein the diol component constituting the polyester polyurethane resin (A) includes a diol having a side chain.
10. The polyolefin resin (C) is a polypropylene-based resin, and the content of the graft portion is 0.1% by mass to 20% by mass based on the total mass of the polyolefin resin (C). The resin composition according to any one of claims 1 to 9.
11. The resin composition according to any one of claims 1 to 10, further comprising a metal filler (E).
12. The resin composition according to claim 11, comprising 10 to 350 parts by mass of a metal filler (E) per 100 parts by mass of the total amount of resin solids excluding the filler component.
13. The resin composition according to claim 11 or 12, wherein the metal filler (E) is a conductive filler.
14. A resin composition layer comprising the resin composition according to any one of claims 1 to 13; A base film in contact with at least one surface of the resin composition layer, The resin composition layer is in a B-stage state. A laminate having a resin composition layer.
15. A laminate comprising a cured layer obtained by curing the resin composition according to any one of claims 1 to 13.
16. An electromagnetic wave shielding film having a resin composition layer made of the resin composition according to any one of claims 1 to 13.
Citation Information
Patent Citations
Adhesive resin composition and laminate made by using it as adhesive layer
JP1992031483A
Adhesive, its manufacturing method and plastic film-laminated sheet iron
JP2004269679A
Aqueous resin composition containing polyurethane resin aqueous dispersion
JP2009013226A
Polyurethane polyurea resin composition, and curable electromagnetic wave-shielding adherent film using it, and manufacturing method therefor
JP2010024273A
Adhesive for flexible member, adhesive sheet and display
JP2019031603A