Antibacterial and antiviral treatment method for metal components

A three-step roughening treatment using micro-etching agents on metal surfaces creates complex shapes, significantly enhancing antibacterial and antiviral properties, surpassing conventional blasting methods in activity values.

JP7587298B2Active Publication Date: 2024-11-20MEC CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023040658
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-03-15
Publication Date
2024-11-20
Estimated Expiration
2043-03-15

AI Technical Summary

Technical Problem

Existing methods for imparting antibacterial and antiviral properties to metal surfaces, such as the blasting process, result in insufficient activity values, particularly for stainless steel, necessitating an improvement in surface treatment techniques to enhance these properties.

Method used

A three-step roughening treatment process using micro-etching agents, including organic, inorganic, and alkaline-based agents, is applied to metal surfaces to create complex roughened shapes, enhancing antibacterial and antiviral properties.

Benefits of technology

The treatment significantly improves antibacterial and antiviral activity values, forming complex roughened surfaces that surpass the capabilities of conventional blasting methods, demonstrating remarkable efficacy against various pathogens.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587298000009
    Figure 0007587298000009
  • Figure 0007587298000010
    Figure 0007587298000010
  • Figure 0007587298000011
    Figure 0007587298000011
Patent Text Reader

Abstract

To provide an antibacterial and antiviral treatment method of a metallic component capable of imparting excellent antibacterial property and an antiviral property to metal components.SOLUTION: An antibacterial and antiviral treatment method for metal members comprises a roughening process that imparts antibacterial and antiviral properties to a surface of a metal member by contacting a microetching agent on the surface of the metal member to form a roughened shape on the surface of the metal member. The roughening process preferably has three steps: a pre-processing step, a main processing step, and a post-processing step. The microetching agent is preferably at least one microetching agent selected from the group consisting of an organic acid-based micro-etching agent, an inorganic acid-based micro-etching agent, an alkali-based micro-etching agent, and a hydrogen peroxide-based micro-etching agent. The metal member is preferably aluminum, aluminum alloy, copper or copper alloy.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an antibacterial and antiviral treatment method for a metal component. [Background technology]

[0002] In recent years, there has been a particular demand for providing antibacterial and antiviral properties to the surfaces of materials that people touch with their hands in order to prevent infection with COVID-19, the so-called novel coronavirus disease.

[0003] The following Patent Document 1 describes an anti-viral surface treatment method in which a projection process (hereinafter also referred to as a "blast process") is performed in which shot material is projected onto the surface of a component, thereby randomly forming countless minute projections and recesses having a specific projection pitch width and recess depth width, thereby imparting anti-viral properties to the surface of the component. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2022-28394 A Summary of the Invention [Problem to be solved by the invention]

[0005] One of the evaluation criteria for antiviral properties is the "antiviral activity value," and in the technology described in Patent Document 1, the comparative object (stainless steel plate material) does not exhibit antiviral properties, but when subjected to the antiviral surface treatment method, the antiviral activity value is 0.4 to 0.7 after 24 hours at 25° C. However, as a result of studies by the present inventors, it was found that the antibacterial and antiviral properties obtained by the technology described in Patent Document 1 are insufficient and further improvements in antibacterial and antiviral properties are necessary, since the blast treatment involves a projection treatment in which shot material is projected onto the surface of the component, and therefore only a convex shape can be imparted toward the back surface of the component.

[0006] In view of the above, an object of the present invention is to provide an antibacterial and antiviral treatment method for a metal component that can impart excellent antibacterial and antiviral properties to the metal component. [Means for solving the problem]

[0007] The above problems can be solved by the following configuration: The present invention relates to an antibacterial and antiviral treatment method for a metal member (1), comprising a roughening treatment step of imparting antibacterial and antiviral properties to the surface of the metal member by contacting the surface of the metal member with a microetching agent to form a roughened shape on the surface of the metal member.

[0008] In the above-mentioned antibacterial and antiviral treatment method for metal members (1), an antibacterial and antiviral treatment method for metal members (2) is preferred, in which the roughening treatment process has three steps: a pretreatment step, a main treatment step, and a post-treatment step.

[0009] In the above-mentioned antibacterial and antiviral treatment method for metal members (1) or (2), the antibacterial and antiviral treatment method for metal members (3) is preferred, in which the microetching agent is at least one type of microetching agent selected from the group consisting of organic acid-based microetching agents, inorganic acid-based microetching agents, alkaline microetching agents, and hydrogen peroxide-based microetching agents.

[0010] In any of the above antibacterial and antiviral treatment methods for metal members (1) to (3), the antibacterial and antiviral treatment method for metal members (4) is preferred, in which the metal members are made of aluminum, an aluminum alloy, copper or a copper alloy. Effect of the Invention

[0011] According to the antibacterial and antiviral treatment method for a metal member of the present invention, it is possible to provide a metal member that exhibits not only antibacterial properties but also excellent antiviral properties, specifically a high antiviral activity value. Although the reason why the method can impart superior antibacterial and antiviral properties to a metal member compared to blast treatment is not clear, the following reasons can be assumed.

[0012] Since the projection process involves projecting shot material onto the surface of the member, the blast process can only form a convex shape toward the back surface of the member. On the other hand, in the antibacterial and antiviral treatment method for a metal member according to the present invention, in the roughening process step, a microetching agent is brought into contact with the surface of the metal member to roughen the surface of the metal member, thereby forming a roughened shape on the surface of the metal member. Therefore, as shown in the experimental results described below, a much more complex shape can be formed compared to the roughened surface formed by the blast process. It should be noted that the present inventors have discovered for the first time that the antiviral and antibacterial properties obtained by the complex shape (roughened shape) formed on the surface of the metal member by the roughening process step of the present invention are significantly superior to the antiviral and antibacterial properties that can be imparted to a metal surface by other treatment methods, particularly blast treatment. [Brief description of the drawings]

[0013] [Figure 1] 1 is a scanning electron microscope photograph (magnification: 1,500 times) of the surface of an (untreated) metal member of Comparative Example 1. [Diagram 2] 1 is a scanning electron microscope photograph (magnification: 5000 times) of the surface of an (untreated) metal member of Comparative Example 1. [Diagram 3] 1 is a scanning electron microscope photograph (magnification: 1,500 times) of the surface of the metal member produced in Example 1. [Figure 4] 2 is a scanning electron microscope photograph (magnification: 5000 times) of the surface of the metal member produced in Example 1. [Diagram 5] 1 is a scanning electron microscope photograph (magnification: 1,500 times) of the surface of the metal member produced in Example 2. [Figure 6] 4 is a scanning electron microscope photograph (magnification: 5000 times) of the surface of the metal member produced in Example 2. [Figure 7] 1 is a scanning electron microscope photograph (magnification: 1,500 times) of the surface of an (untreated) metal member of Comparative Example 2. [Figure 8] 1 is a scanning electron microscope photograph (magnification: 5000 times) of the surface of an (untreated) metal member of Comparative Example 2. [Figure 9] 1 is a scanning electron microscope photograph (magnification: 1,500 times) of the surface of the metal member produced in Example 3. [Figure 10] 1 is a scanning electron microscope photograph (magnification: 5000 times) of the surface of the metal member produced in Example 3. [Figure 11] 1 is a scanning electron microscope photograph (magnification: 1,500 times) of the surface of the metal member produced in Example 4. [Figure 12] 1 is a scanning electron microscope photograph (magnification: 5000 times) of the surface of the metal member produced in Example 4. [Figure 13] Scanning electron microscope photograph (magnification 1500x) of the surface of an untreated stainless steel component that has not been roughened. [Figure 14] Scanning electron microscope photograph (magnification 5000x) of the surface of an untreated stainless steel component that has not been roughened. [Figure 15] Scanning electron microscope photograph (magnification 1500x) of the surface of an untreated stainless steel component after blasting. [Figure 16] Scanning electron microscope photograph (magnification 5000x) of the surface of an untreated stainless steel component after blasting. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The antibacterial and antiviral treatment method for a metal component according to the present invention includes a roughening treatment step in which a microetching agent is brought into contact with the surface of the metal component to form a roughened shape on the surface of the metal component, thereby imparting antibacterial and antiviral properties to the surface of the metal component.

[0015] Examples of metal members that can be used in the present invention include aluminum, aluminum alloys, copper, copper alloys, nickel, nickel alloys, stainless steel, titanium, titanium alloys, iron or iron alloys. Among these, it is preferable to use aluminum, aluminum alloys, copper or copper alloys as the metal members in the present invention. The shape and size of the metal members can be appropriately designed according to the application to be used after the antibacterial and antiviral properties are imparted. In the blasting treatment, since shot material is projected onto the surface of the member, it is preferable that the treated surface (surface) of the metal member to which antibacterial and antiviral properties are imparted is a flat surface. However, in the antibacterial and antiviral treatment method for metal members according to the present invention, since the surface of the metal member is roughened by contacting the surface of the metal member with a microetching agent, the treated surface of the metal member is not limited to a flat surface, and it is also characterized in that antibacterial and antiviral properties can be imparted to a surface of any shape.

[0016] As the microetching agent used in the roughening treatment step, for example, an organic acid microetching agent, an inorganic acid microetching agent, an alkali microetching agent, or a hydrogen peroxide microetching agent can be used.

[0017] Examples of organic acid-based microetching agents include microetching agents made of an aqueous solution containing an organic acid, a metal ion source, a halide ion source, and the like.

[0018] Examples of inorganic acid microetching agents include microetching agents made of an acidic aqueous solution containing an inorganic acid, a metal ion source, a halide ion source, and the like.

[0019] Examples of alkaline microetching agents include microetching agents made of an aqueous solution containing an alkali source, an amphoteric metal ion source, nitrate ions, a thio compound, and the like.

[0020] Examples of hydrogen peroxide-based microetchants include microetchants made of an aqueous solution containing hydrogen peroxide and sulfuric acid as main components.

[0021] In the antibacterial and antiviral treatment method for a metal member according to the present invention, the roughening treatment step may be performed in one step, but in order to further enhance the antibacterial and antiviral properties of the metal member to be manufactured, it is preferable to perform it in two steps, and it is particularly preferable to perform it in three steps, including a pretreatment step, a main treatment step, and a post-treatment step. An embodiment in which the roughening treatment step is performed in three steps will be described below.

[0022] The pretreatment step may be, for example, a step of immersing at least the surface to be treated of the metal member in an alkaline soft etching agent such as a hydrogen peroxide-based soft etching agent consisting of an aqueous solution mainly composed of dilute nitric acid, hydrogen peroxide, and sulfuric acid, or an aqueous solution containing the above-mentioned alkali source, an amphoteric metal ion source, nitrate ions, a thio compound, etc. The treatment temperature may be, for example, 15 to 40°C, and the treatment time may be, for example, about 3 seconds to 10 minutes.

[0023] In this treatment step, at least the treatment surface of the metal member is immersed in the above-mentioned organic acid microetchant, inorganic acid microetchant, alkaline microetchant, hydrogen peroxide microetchant, etc. The treatment temperature is, for example, 10 to 40°C, and the treatment time is, for example, about 5 seconds to 10 minutes.

[0024] The post-treatment step may be, for example, a step of immersing at least the treatment surface of the metal member in dilute nitric acid, etc. The treatment temperature may be, for example, 15 to 40° C., and the treatment time may be, for example, about 3 to 40 seconds.

[0025] After the roughening treatment process, a complex roughened shape is formed on the surface of the metal member. This provides the surface of the metal member with excellent antibacterial and antiviral properties. Specific examples of the complex roughened shape formed on the surface of the metal member after the roughening treatment process will be described later.

[0026] The antibacterial and antiviral treatment method for metal components according to the present invention makes it possible to manufacture metal components with excellent antibacterial and antiviral properties. The antiviral activity value, which indicates the level of antiviral properties, can be calculated from the following formula with reference to JIS R1756:2020 (visible light responsive photocatalyst, antiviral, film adhesion method). V D =Log(B D )-Log(C D ) (1) In the above formula (1), V D indicates antiviral activity value, D indicates dark place, B indicates infectivity value of unprocessed product, and C indicates infectivity value of processed product.

[0027] As described above, the antibacterial and antiviral treatment method for a metal member according to the present invention can produce a metal member having excellent antibacterial and antiviral properties. Therefore, the antibacterial and antiviral treatment method for a metal member according to the present invention is particularly useful as a treatment method for imparting antibacterial and antiviral properties to metal members used in home appliances, housing building materials / equipment, toilet-related facilities / supplies, kitchen-related facilities / supplies, bathroom-related facilities / supplies, office equipment / office supplies, printing (printed matter, laminated products and paper), transportation equipment, industrial equipment / industrial supplies (films, packaging materials / films for food, etc., packaging materials, etc.), medical / nursing / health, communication-related / accessories, pet supplies, daily necessities (shoes, cleaning supplies, cosmetics, etc.), etc. EXAMPLES

[0028] An example of an embodiment of the present invention will be described below, but the present invention is not limited to this description in any way.

[0029] Ref.(-) (glass plate) was prepared as an "unprocessed product". Next, an unused aluminum alloy plate (A-6063-t5) (40 mm x 40 mm x t2 mm) was prepared as an untreated aluminum alloy member that had not been subjected to roughening treatment. A scanning electron microscope photograph (magnification 1500 times) of the surface of this (untreated) aluminum alloy member is shown in FIG. 1, and a scanning electron microscope photograph (magnification 5000 times) is shown in FIG. 2. Even with reference to FIGS. 1 and 2, and especially the photograph in FIG. 2, it can be seen that the surface of the (untreated) aluminum alloy member has no irregularities and is close to a mirror surface. The (untreated) aluminum alloy member is designated as Comparative Example 1.

[0030] Example 1 An unused aluminum alloy plate (A-6063-t5) (40 mm × 40 mm × t2 mm) was subjected to a roughening treatment process (three steps: pre-treatment step, main treatment step, and post-treatment step) under the following conditions (hereinafter, the roughening treatment process in Example 1 is referred to as "roughening treatment 1"). The conditions for each step are shown below. (Pre-processing step) The surface of the aluminum alloy plate to be treated is immersed in dilute nitric acid (left stationary). Treatment temperature: 35°C. Treatment time: 5 to 10 minutes. (Main processing step) Following the pretreatment, the surface of the aluminum alloy plate to be treated is immersed (left stationary) in an alkaline microetching agent (aqueous solution containing an alkali source, an amphoteric metal ion source, nitrate ions, a thio compound, etc.). Treatment temperature: 35°C. Treatment time: 4 minutes. (Post-processing step) Following this treatment, the surface of the aluminum alloy plate to be treated is immersed in dilute nitric acid (left stationary). Treatment temperature: room temperature. Treatment time: 30 seconds. Following the post-treatment, ultrasonic cleaning was performed in pure water for 1 minute.

[0031] A scanning electron microscope photograph (magnification 1500x) of the surface of the aluminum alloy member (referred to as "(roughening treatment 1) aluminum alloy member") obtained after the roughening treatment step (roughening treatment 1) of Example 1 is shown in FIG. 3, and a scanning electron microscope photograph (magnification 5000x) is shown in FIG. 4. It can be seen from the photograph in FIG. 3 that a complex roughened shape is formed over the entire surface of the aluminum alloy member by the roughening treatment step 1. With particular reference to the photograph in FIG. 4, it can be seen that convex shapes are formed in arbitrary directions on the surface of the aluminum alloy member.

[0032] For reference, a scanning electron microscope photograph (magnification 1500 times) of the surface of an untreated stainless steel member that has not been roughened is shown in FIG. 13, a scanning electron microscope photograph (magnification 5000 times) is shown in FIG. 14, a scanning electron microscope photograph (magnification 1500 times) of the surface of the untreated stainless steel member after blasting is shown in FIG. 15, and a scanning electron microscope photograph (magnification 5000 times) is shown in FIG. 16. As is clear from a comparison of FIG. 13 with FIG. 15 and FIG. 14 with FIG. 16, it can be seen that the blasting treatment can only form a convex shape toward the back surface of the member, and therefore a complex roughened shape cannot be formed on the stainless steel surface. On the other hand, referring to FIG. 3 and FIG. 4, and especially the photograph of FIG. 4, it can be seen that a much more complex roughened shape is formed on the surface of the aluminum alloy member (roughening treatment 1) compared to the stainless steel surface that has been blasted.

[0033] Example 2 An unused aluminum alloy plate (A-6063-t5) (40 mm × 40 mm × t2 mm) was subjected to a roughening treatment process (three steps: pre-treatment step, main treatment step, and post-treatment step) under the following conditions (hereinafter, the roughening treatment process in Example 2 is referred to as "roughening treatment 2"). The conditions for each step are shown below. (Pre-processing step) The surface of the aluminum alloy plate to be treated is immersed in an alkaline soft etching agent (left stationary). Treatment temperature: 35°C. Treatment time: 1 minute. (Main processing step) Following the pretreatment, the surface of the aluminum alloy plate to be treated is immersed (left stationary) in an inorganic acid microetching agent (aqueous solution containing inorganic acid, amphoteric metal ion source, halide ion source, etc.). Treatment temperature: 30°C. Treatment time: 10 minutes. (Post-processing step) Following this treatment, the surface of the aluminum alloy plate to be treated is immersed in dilute nitric acid (left stationary). Treatment temperature: room temperature. Treatment time: 30 seconds. Following the post-treatment, ultrasonic cleaning was performed in pure water for 1 minute.

[0034] FIG. 5 shows a scanning electron microscope photograph (magnification 1500 times) of the surface of the aluminum alloy member (referred to as "(roughening treatment 2) aluminum alloy member") obtained after the roughening treatment step (roughening treatment 2) of Example 2, and FIG. 6 shows a scanning electron microscope photograph (magnification 5000 times). From the photograph in FIG. 5, it can be seen that a complex roughened shape is formed on the entire surface of the aluminum alloy member by the roughening treatment step 2. With particular reference to the photograph in FIG. 6, it can be seen that a convex shape is formed in any direction on the surface of the aluminum alloy member. In other words, it can be seen that a much more complex roughened shape is formed on the surface of the aluminum alloy member compared to blast treatment, which can only form a convex shape toward the back surface of the member.

[0035] [Antiviral evaluation] Using Ref.(-) (glass plate) as an unprocessed product, the antiviral properties of the (untreated) aluminum alloy member of Comparative Example 1 and the aluminum alloy members which had been subjected to the antiviral treatment methods for metal members of Examples 1 and 2 (the (roughening treatment 1) aluminum alloy member and the (roughening treatment 2) aluminum alloy member) were evaluated under the following conditions. [Test Standards] Refer to JIS R1756:2020 (visible light responsive photocatalyst, anti-virus, film adhesion method) [Unprocessed product name] Ref.(-)(Glass plate) [Test item name] (Untreated) Aluminum alloy member (Comparative Example 1), (Roughening treatment 1) Aluminum alloy member (Example 1), (Roughening treatment 2) Aluminum alloy member (Example 2) [Size of test piece (aluminum alloy component)] 40mm×40mm×t2mm [n number] n=1 [Test phage] bacteriophage Qβ (NBRC 20012) [host E. coli (NBRC 106373)]; the results are shown in Table 1. Bacteriophage φ6 (NBRC 105899, not JIS standard) [host Pseudomonas syringae (NBRC 14084)]; the results are shown in Table 2. [Dilution of test phage] 1 / 500NB [Sterilization of test samples] Sterilization with UV254nm (15 minutes on each side) [Conditions for operation] Temperature 25℃, dark place, action time 0 hours, 4 hours [Adhesive film] Polypropylene film (VF-10, KOKUYO), 30mm x 30mm

[0036] [Table 1]

[0037] As shown in Table 1, the aluminum alloy members (roughening treatment 1) and (roughening treatment 2) obtained in Examples 1 and 2 showed a significant decrease in infectivity titer after 4 hours in a dark place at 25°C. Similarly, the antiviral activity value increased to 5 after 4 hours in a dark place at 25°C. From these results, it can be seen that the metal members produced by the antiviral treatment methods for metal members in Examples 1 and 2 have a remarkable effect on antiviral properties due to the formation of an extremely complex roughened shape on the surface of the metal member.

[0038] [Table 2]

[0039] As shown in Table 2, the infectivity titer of the aluminum alloy member (roughening treatment 1) and the aluminum alloy member (roughening treatment 2) obtained in Example 1 and Example 2 significantly decreased after 4 hours in a dark place at 25°C. Similarly, the antiviral activity value increased to 5.3 after 4 hours in a dark place at 25°C. From these results, it can be understood that the metal members manufactured by the antiviral treatment methods for metal members in Examples 1 and 2 have a remarkable effect on antiviral properties regardless of the test phage, that is, regardless of norovirus, influenza virus, or even coronavirus, due to the formation of a very complex roughened shape on the surface of the metal member.

[0040] [Antibacterial evaluation] Using Ref.(-) (glass plate) as an untreated product, the antibacterial properties of the (untreated) aluminum alloy member of Comparative Example 1 and the aluminum alloy members which had been subjected to the antibacterial treatment methods for metal members of Examples 1 and 2 (the (roughening treatment 1) aluminum alloy member and the (roughening treatment 2) aluminum alloy member) were evaluated under the following conditions. [Test Standards] Refer to JIS Z2801:2012 [Unprocessed product name] Ref.(-)(Glass plate) [Test item name] (Untreated) Aluminum alloy member (Comparative Example 1), (Roughening treatment 1) Aluminum alloy member (Example 1), (Roughening treatment 2) Aluminum alloy member (Example 2) [Size of test piece (aluminum alloy component)] 40mm×40mm×t2mm [n number] n=1 [Test bacteria] Staphylococcus aureus (NBRC12732); the results are shown in Table 3. - Escherichia coli (NBRC3972); the results are shown in Table 4. [Dilution of test phage] 1 / 500NB [Sterilization of test samples] Sterilization with UV254nm (15 minutes on each side) [Conditions for operation] Temperature 25℃, dark place, action time 0 hours, 8 hours [Adhesive film] Polypropylene film (VF-10, KOKUYO), 30mm x 30mm

[0041] [Table 3]

[0042] As shown in Table 3, the aluminum alloy members (roughening treatment 1) and (roughening treatment 2) obtained in Examples 1 and 2 showed a significant decrease in the viable bacterial count after 8 hours in a dark place at 25°C. Similarly, the antibacterial activity value increased to 3.8 to 4.2 after 8 hours in a dark place at 25°C. From these results, it can be seen that the metal members produced by the antibacterial treatment methods for metal members in Examples 1 and 2 have a remarkable effect in terms of antibacterial properties due to the formation of a very complex roughened shape on the surface of the metal member.

[0043] [Table 4]

[0044] As shown in Table 4, the aluminum alloy members (roughening treatment 1) and (roughening treatment 2) obtained in Examples 1 and 2 showed a significant decrease in the number of live bacteria after 8 hours in a dark place at 25°C. Similarly, the antibacterial activity value increased to 4.5 after 8 hours in a dark place at 25°C. From these results, it can be understood that the metal members produced by the antibacterial treatment methods for metal members in Examples 1 and 2 have a significant effect on antibacterial properties regardless of the test phage, that is, regardless of Staphylococcus aureus or Escherichia coli, due to the formation of a very complex roughened shape on the surface of the metal member.

[0045] Ref.(-) (glass plate) was prepared as an "unprocessed product". Next, an unused copper member (50 mm x 50 mm x t1.3 mm) was prepared as an untreated copper member that had not been subjected to a roughening treatment. A scanning electron microscope photograph (magnification 1500 times) of the surface of this (untreated) copper member is shown in FIG. 7, and a scanning electron microscope photograph (magnification 5000 times) is shown in FIG. 8. Referring to FIGS. 7 and 8, and especially the photograph in FIG. 8, it can be seen that the surface of the (untreated) copper member is completely free of irregularities and is close to a mirror surface. The (untreated) copper member is designated as Comparative Example 2.

[0046] Example 3 An unused copper plate (50 mm × 50 mm × t1.3 mm) was subjected to a roughening treatment process (three steps: pretreatment step, main treatment step, and post-treatment step) under the following conditions (hereinafter, the roughening treatment process in Example 3 is referred to as "roughening treatment 3"). The conditions for each step are shown below. (Pre-processing step) The surface of the copper plate to be treated is sprayed with dilute hydrochloric acid. Treatment temperature: room temperature. Treatment time: 10 seconds. (Main processing step) Following the pretreatment, the surface of the copper plate to be treated is sprayed with an organic acid microetchant (aqueous solution containing organic acid, metal ion source, halide ion source, etc.). Treatment temperature: 30°C. Treatment time: 60 seconds. (Post-processing step) Following this treatment, the surface of the copper plate to be treated is sprayed with dilute hydrochloric acid. Treatment temperature: room temperature. Treatment time: 15 seconds.

[0047] FIG. 9 shows a scanning electron microscope photograph (magnification 1500 times) of the surface of the copper member (referred to as "(roughening treatment 3) copper member") obtained after the roughening treatment step (roughening treatment 3) of Example 3, and FIG. 10 shows a scanning electron microscope photograph (magnification 5000 times). From the photograph in FIG. 9, it can be seen that a complex roughened shape is formed on the entire surface of the copper member by the roughening treatment step 3. With particular reference to the photograph in FIG. 10, it can be seen that a convex shape is formed in any direction on the surface of the copper member. In other words, it can be seen that a much more complex roughened shape is formed on the surface of the copper member compared to blast treatment, which can only form a convex shape toward the back surface of the member.

[0048] Example 4 An unused copper plate (50 mm × 50 mm × t1.3 mm) was subjected to a roughening treatment process (three steps: pretreatment step, main treatment step, and post-treatment step) under the following conditions (hereinafter, the roughening treatment process in Example 4 is referred to as "roughening treatment 4"). The conditions for each step are shown below. (Pre-processing step) The surface of the copper plate to be treated is sprayed with dilute hydrochloric acid. Treatment temperature: room temperature. Treatment time: 10 seconds. (Main processing step) Following the pretreatment, the surface of the copper plate to be treated is sprayed with an organic acid microetchant (aqueous solution containing organic acid, metal ion source, halide ion source, etc.). Treatment temperature: 30°C. Treatment time: 150 seconds. (Post-processing step) Following this treatment, the surface of the copper plate to be treated is sprayed with dilute hydrochloric acid. Treatment temperature: room temperature. Treatment time: 15 seconds.

[0049] FIG. 11 shows a scanning electron microscope photograph (magnification 1500 times) of the surface of the copper member (referred to as "(roughening treatment 4) copper member") obtained after the roughening treatment step (roughening treatment 4) of Example 4, and FIG. 12 shows a scanning electron microscope photograph (magnification 5000 times). From the photograph in FIG. 11, it can be seen that a complex roughened shape is formed on the entire surface of the copper member by the roughening treatment step 4. With particular reference to the photograph in FIG. 12, it can be seen that a convex shape is formed in any direction on the surface of the copper member. In other words, it can be seen that a much more complex roughened shape is formed on the surface of the copper member compared to blast treatment, which can only form a convex shape toward the back surface of the member.

[0050] [Antiviral evaluation] Using Ref.(-) (glass plate) as an unprocessed product, the antiviral properties of the (untreated) copper member of Comparative Example 2 and the copper members subjected to the antiviral treatment methods for metal members of Examples 3 and 4 (the (roughening treatment 3) copper member and the (roughening treatment 4) copper member) were evaluated under the following conditions. [Test Standards] Refer to JIS R1756:2020 (visible light responsive photocatalyst, anti-virus, film adhesion method) [Unprocessed product name] Ref.(-)(Glass plate) [Test item name] (Untreated) copper member (Comparative Example 2), (Roughening treatment 3) copper member (Example 3), (Roughening treatment 4) copper member (Example 4) [Size of test sample (copper material)] 50mm×50mm×t1.3mm [n number] n=1 [Test phage] bacteriophage Qβ (NBRC 20012) [host E. coli (NBRC 106373)]; the results are shown in Table 5. Bacteriophage φ6 (NBRC 105899, non-JIS standard) [host Pseudomonas syringae (NBRC 14084)]; the results are shown in Table 6. [Dilution of test phage] 1 / 20NB [Sterilization of test samples] Sterilization with UV254nm (15 minutes on each side) [Conditions for operation] Temperature 25℃, dark place, action time 0 minutes, 30 minutes [Adhesive film] Polypropylene film (VF-10, KOKUYO), 40mm x 40mm

[0051] [Table 5]

[0052] As shown in Table 5, the copper members (roughening treatment 3) and (roughening treatment 4) obtained in Examples 3 and 4 showed a significant decrease in infectivity titer after 30 minutes in a dark place at 25° C. Similarly, the antiviral activity value increased to 5.3 after 30 minutes in a dark place at 25° C. From these results, it can be seen that the metal members produced by the antiviral treatment methods for metal members in Examples 3 and 4 have a remarkable effect on antiviral properties due to the formation of an extremely complex roughened shape on the surface of the metal member.

[0053] [Table 6]

[0054] As shown in Table 6, the infectivity titer of the (roughening treatment 3) copper member and the (roughening treatment 4) copper member obtained in Example 3 and Example 4 significantly decreased after 30 minutes in the dark at 25°C. Similarly, the antiviral activity value increased to 5.6 after 30 minutes in the dark at 25°C. From these results, it can be understood that the metal members manufactured by the antiviral treatment methods for metal members in Examples 3 and 4 have a remarkable antiviral effect regardless of the test phage, that is, regardless of the norovirus, influenza virus, or even coronavirus, due to the formation of an extremely complex roughened shape on the surface of the metal member.

[0055] [Antibacterial evaluation] Using Ref.(-) (glass plate) as an untreated product, the antibacterial properties of the (untreated) copper member of Comparative Example 2 and the copper members subjected to the antibacterial treatment methods for metal members of Examples 3 to 4 ((Roughening Treatment 3) copper member and (Roughening Treatment 4) copper member) were evaluated under the following conditions. [Test Standards] Refer to JIS Z2801:2012 [Unprocessed product name] Ref.(-)(Glass plate) [Test item name] (Untreated) copper member (Comparative Example 2), (Roughening treatment 3) copper member (Example 3), (Roughening treatment 4) copper member (Example 4) [Size of test sample (copper material)] 50mm×50mm×t1.3mm [n number] n=1 [Test bacteria] Staphylococcus aureus (NBRC12732); the results are shown in Table 7. - Escherichia coli (NBRC3972); the results are shown in Table 8. [Dilution of test phage] 1 / 20NB (Staphylococcus aureus), 1 / 500NB (Escherichia coli) [Sterilization of test samples] Sterilization with UV254nm (15 minutes on each side) [Conditions for operation] Temperature 25℃, dark place, action time 0 minutes, 15 minutes [Adhesive film] Polypropylene film (VF-10, KOKUYO), 40mm x 40mm

[0056] [Table 7]

[0057] As shown in Table 7, the copper members (roughening treatment 3) and (roughening treatment 4) obtained in Examples 3 and 4 showed a significant decrease in the viable bacterial count after 15 minutes at 25°C in the dark. Similarly, the antibacterial activity value increased to 3.5 to 3.7 after 15 minutes at 25°C in the dark. From these results, it can be seen that the metal members produced by the antibacterial treatment methods for metal members in Examples 3 and 4 have a remarkable effect in terms of antibacterial properties due to the formation of a very complex roughened shape on the surface of the metal member.

[0058] [Table 8]

[0059] As shown in Table 8, the copper members (roughening treatment 3) and (roughening treatment 4) obtained in Examples 3 and 4 showed a significant decrease in the viable bacterial count after 15 minutes at 25°C in the dark. Similarly, the antibacterial activity value increased to 3.9 after 15 minutes at 25°C in the dark. From these results, it can be seen that the metal members produced by the antibacterial treatment methods for metal members in Examples 3 and 4 have a significant effect on antibacterial properties regardless of the type of test bacteria, that is, regardless of Staphylococcus aureus or Escherichia coli, due to the formation of an extremely complex roughened shape on the surface of the metal member.

Claims

[Claim 1] A roughening treatment step is provided in which a microetching agent is brought into contact with a copper surface to form a roughened shape on the copper surface, thereby imparting antibacterial and antiviral properties to the copper surface; The method for antibacterial and antiviral treatment of copper, characterized in that the roughening treatment process comprises three steps: a pretreatment step of immersing at least the copper treatment surface in a hydrogen peroxide-based soft etching agent or dilute hydrochloric acid; a main treatment step of contacting the copper treatment surface with an organic acid-based micro-etching agent containing an organic acid, a metal ion source, and a halide ion source; and a posttreatment step of immersing at least the copper treatment surface in dilute nitric acid or dilute hydrochloric acid.

Citation Information

Patent Citations

  • Antivirus surface treatment method of member and antivirus member

    JP2022028394A

  • JPP6695558B

  • Nanostructured Surfaces

    US20130199539A1

  • Heat exchanger including fins with surface having bactericidal activity, metallic member with surface having bactericidal activity, method for inhibiting mold growth and sterilization method both using surface of fins of heat exchanger or surface of metallic member, and electrical water boiler, beverage supplier, and lunch box lid all including metallic member

    WO2016021367A1

  • Formation of monolithic nanostructures on prosthetic devices

    WO2021239877A1