Manufacturing method for joint structure of concrete pipe

The joint structure for concrete pipes uses fiber sheets with controlled adhesive application to enhance flexibility and prevent separation, addressing movement and water leakage issues, ensuring a durable and reliable connection.

JP7587366B2Active Publication Date: 2024-11-20NIPPON HUME CORP +1
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
JP2020128972
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-07-30
Publication Date
2024-11-20
Estimated Expiration
2040-07-30

AI Technical Summary

Technical Problem

Conventional waterproof flexible joints for concrete pipes are prone to movement during earthquakes, leading to pipe collision and damage, and require periodic checks due to loose expansion bands that can cause water leakage.

Method used

A joint structure for concrete pipes using fiber sheets with controlled adhesive application to ensure flexibility and range of motion, minimizing inner bulges and separation, combined with a sealing material to prevent water ingress.

Benefits of technology

The joint structure provides enhanced flexibility and resistance to separation, reducing the risk of pipe collision and water leakage, while eliminating the need for periodic checks on loose connections.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587366000001
    Figure 0007587366000001
  • Figure 0007587366000002
    Figure 0007587366000002
Patent Text Reader

Abstract

To provide a joint structure of a concrete pipe which is hardly released while having proper flexibility and a movable area and which is small in a bulge to an inner face, and its manufacturing method.SOLUTION: A joint structure of a concrete pipe comprises a fiber sheet 20 which is pasted to internal peripheral faces of both concrete pipes 10 so as to straddle a connection part 11 of the adjacent concrete pipes 10, and the fiber sheet 20 adheres to the internal peripheral faces of both the concrete pipes 10 with an additive 30 with an interval while sandwiching the connection part 11. Also, an interval of adhesion regions 31 in each of which the fiber sheet 20 adheres to the internal peripheral faces of both the concrete pipes 10 with the additive 30 is set to 50 to 500 mm with the connection part 11 sandwiched therebetween. Furthermore, the fiber sheet 20 adheres to the internal peripheral faces of both the concrete pipes 10 with the additive 30 in a prescribed region with the connection part 11 sandwiched therebetween.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a joint structure for concrete pipes that covers the inner surface of a joint portion of a concrete pipe to stop water from entering through the joint structure, and a manufacturing method thereof. [Background technology]

[0002] As a joint structure for concrete pipes, a watertight flexible joint has been proposed that has a cylindrical flexible joint body and an expansion band for pressing the flexible joint body against the pipe wall (see, for example, Patent Document 1). The outer peripheral surface of the flexible joint body is provided with a plurality of annular watertight protrusions, which press against the inner peripheral surface of the concrete pipe to maintain a watertight state. As a result, even if displacement occurs in the joint due to an earthquake or ground subsidence, the watertight flexible joint follows and deforms, while the watertight protrusions maintain the watertight state. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2008-51207 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, while the conventional technology is highly flexible, it has the problem that in the event of an earthquake or other event, the joints can easily move, causing concrete pipes to collide with each other at the joints and become damaged again. In addition, the expansion band has a split structure for carrying it into the pipeline, and the joints protrude into the inner surface of the concrete pipe, causing a problem of increased pressure loss. Furthermore, because the expansion band is designed to stop water from entering the pipe, water leaks will occur if the expansion force loosens. Therefore, there is also the problem that the expansion band must be regularly checked for loosening due to weak operation.

[0005] The present invention has been made in consideration of the above-mentioned problems, and aims to solve the problems and provide a joint structure for concrete pipes that has appropriate flexibility and range of motion, is not easily separated, and has small bulges on the inner surface, and a manufacturing method thereof. [Means for solving the problem]

[0006] Books The method for manufacturing a joint structure of a concrete pipe of the present invention is to apply a primer having a viscosity of 1000 at 20°C when mixed with a base agent and a hardener to a predetermined area on the inner circumferential surface of both of the concrete pipes that sandwich the joint portion of the adjacent concrete pipes. m The method is characterized in that a low-viscosity epoxy resin of less than Pa·s is applied, and an epoxy resin having a viscosity of 1000 to 50000 mPa·s at 20°C when mixed with the base agent and hardener is applied as an adhesive to the inner surfaces of both of the concrete pipes to which the primer has been applied, with a gap between them and sandwiching the connection part, and a fiber sheet is attached so as to come into contact with the adhesive applied to the inner surfaces of both of the concrete pipes. Effect of the Invention

[0007] According to the present invention, a fiber sheet is attached to the inner surfaces of both concrete pipes with an adhesive, with a gap between them on either side of the connection portion, so that the fiber sheet has a moderate flexibility and range of motion while being difficult to come off.In addition, because the fiber sheet is attached to the inner surfaces of the concrete pipes, a concrete pipe joint structure can be realized that has small bulges on the inner surface. [Brief description of the drawings]

[0008] [Figure 1] 1 is a cross-sectional perspective view showing a configuration of an embodiment of a joint structure for concrete pipes according to the present invention; [Diagram 2] FIG. 2 is an enlarged view of a region X shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. In the following embodiments, components having similar functions are denoted by the same reference numerals and descriptions thereof will be omitted as appropriate.

[0010] Referring to Figures 1 and 2, the joint structure of this embodiment is a tubular body 1 formed by connecting a plurality of concrete pipes 10, in which the connection portions 11 on the inner surfaces of adjacent concrete pipes 10 are covered from the inside with a fiber sheet 20 to reinforce and waterproof the joint structure.

[0011] The fiber sheets 20 are attached to the inner circumferential surfaces of both concrete pipes 10 so as to straddle the connection portion 11. Referring to Fig. 2, the fiber sheets 20 are attached to the entire circumference of both sides of the connection portion 11 at locations spaced a predetermined distance from the connection portion 11 in the longitudinal direction of the concrete pipe 10 (hereinafter simply referred to as the longitudinal direction) with an adhesive 30. In other words, at least a portion of the fiber sheet 20 is bonded to the inner circumferential surfaces of both concrete pipes 10 with the adhesive 30. Hereinafter, the regions where the fiber sheet 20 is attached to the inner circumferential surface of the concrete pipe 10 with the adhesive 30 will be referred to as bonded regions 31.

[0012] In the region between the two adhesive regions, i.e., in regions at a predetermined distance on both sides in the longitudinal direction from the connection portion 11, the fiber sheet 20 is attached over the entire circumference to the inner surface of the concrete pipe 10 by the adhesive 40. Hereinafter, the region where the fiber sheet 20 is attached to the inner surface of the concrete pipe 10 by the adhesive 40 will be referred to as the adhesive region 41.

[0013] In the adhesive region 31, the adhesive 30 hardens and the fiber sheet 20 is firmly attached to the inner surface of the concrete pipe 10, whereas in the cohesive region 41, the adhesive 40 itself has extensibility and the reaction has already been completed, allowing peeling and re-adhesion, so the fiber sheet 20 can expand and contract. Therefore, when stress acts on the joint, the fiber sheet 20 can expand and contract in the cohesive region 41, allowing the joint to move as much as necessary. In addition, because the fiber sheet 20 is firmly attached to the inner surface of the concrete pipe 10 in the cohesive regions 31 arranged on both sides of the cohesive region 41, it is possible to control the joint not to come off until the fiber sheet 20 peels off or breaks.

[0014] The interval between the adhesive regions 31, i.e., the longitudinal length of the region (adhesive region 41) that is not firmly bonded with the adhesive 30, is set to about 50 to 500 mm across the joint 11. This makes it possible to prevent the fiber sheet 20 from peeling off due to expansion and contraction in the adhesive region 41, even if the concrete pipe 10 is bent at the joint once or more. If the fiber sheet 20 is firmly attached across the joint 11 with the adhesive 30, the adjacent concrete pipe 10 becomes too difficult to move, and even slight bending cannot be tolerated at the joint of the concrete pipe 10, narrowing the range of application.

[0015] The fibers constituting the fiber sheet 20 are not particularly limited, but aramid fibers, which are excellent in strength, elongation, adhesiveness, etc., are particularly preferred. In addition, fiber sheets 20 made of glass fibers, aromatic polyamide fibers (aramid fibers), carbon fibers, polyparaphenylene benzoxal fibers, aromatic polyester fibers, ultra-high molecular weight polyethylene fibers, polyamide fibers (nylon fibers), polyester fibers, polyvinyl alcohol fibers (vinylon fibers), polyethylene fibers, polypropylene fibers, basalt fibers, etc. can be used.

[0016] The basis weight (weight) of the fiber sheet 20 is not particularly limited, but is preferably 100 g / m from the viewpoint of strength and rigidity. 2 It is preferable that the thickness is 1000 g / m or more, and from the viewpoint of workability, it is preferable that the thickness is 1000 g / m or more. 2It is preferable that the thickness is less than 100 g / m 2 In the case of a basis weight below 1000 g / m, the durability, strength and rigidity of the fiber sheet 20 are insufficient, and the concrete pipes 10 may not be able to sufficiently suppress movement between each other. 2 In the above cases, the fiber sheet 20 is thick and bulges toward the inner surface of the concrete pipe 10, so that it is easily peeled off due to water flow inside the pipe, and durability is reduced. 2 In the above cases, the fiber sheet 20 itself becomes heavy, and workability decreases.

[0017] It is preferable to use one or two of the above-mentioned sheets as the fiber sheet 20, with the overlapping portion limited to the overlapping portion of two sheets. If three or more fiber sheets are stacked, peeling between the fiber sheets is likely to occur, which is not preferable.

[0018] The fiber sheet 20 is a woven or knitted fabric having a strength in the weft direction of 500 to 50,000 N / cm and a breaking elongation in the range of 1 to 20%, and is attached so that the weft is oriented in the longitudinal direction of the concrete pipe 20.

[0019] The adhesive 30 for bonding the fiber sheet 20 to the inner surface of the concrete pipe 10 is not particularly limited, but epoxy resin is preferable from the viewpoints of adhesion and ease of handling at the site. Other examples of the adhesive 30 that can be used include vinyl ester resin, phenol resin, acrylic resin, polyurea resin, isocyanate resin, and the like.

[0020] Furthermore, if the fiber sheet 20 is adhered to the inner surface of the concrete pipe 10 with the adhesive 30 after the primer 50 has been applied to the inner surface of the concrete pipe 10, the adhesive 30 can be made to adhere more firmly to the inner surface of the concrete pipe 10. It is preferable that the inner surface of the concrete pipe 10 is polished and dust removed before the primer 50 is applied.

[0021] It is preferable to use a primer 50 having a viscosity of less than 1000 mPa·s (for example, a two-liquid type epoxy resin having a viscosity of less than 1000 mPa·s at 20°C when the base agent and hardener are mixed) and an adhesive 30 having a viscosity of 1000 to 50000 mPa·s (for example, a two-liquid type epoxy resin having a viscosity of 1000 to 50000 mPa·s at 20°C when the base agent and hardener are mixed). By using a primer 50 having a viscosity of less than 1000 mPa·s, the primer 50 penetrates into the inner surface of the concrete pipe 10, forming an epoxy resin layer on the inner surface of the concrete pipe 10, and facilitating adhesion to the fiber sheet 20. In addition, by using an adhesive 30 having a viscosity of 1000 mPa·s or more, it is possible to prevent the adhesive from dripping during application and to apply the adhesive 30 uniformly. Furthermore, by using an adhesive 30 with a viscosity of less than 50,000 mPa·s, the adhesive 30 can sufficiently penetrate between the individual fibers constituting the fiber sheet 20, improving the adhesiveness.

[0022] In addition, the two-component epoxy resin used as the primer 50 and adhesive 30 both have an adhesive strength of 1.5 N / mm according to the JSCE-E545 test method. 2 If the inner circumferential surface of the concrete pipe 10 is damaged and the surface is very uneven after the primer 50 is applied, it is also preferable to use epoxy resin putty to smooth out the unevenness.

[0023] Application of the adhesive 40 to the inner surface of the concrete pipe 10 can be performed with adhesive tape having adhesive 40 applied to both sides of a substrate, which can improve workability. The adhesive tape is not particularly limited, but the substrate can be paper, nonwoven fabric, woven fabric, knitted fabric, film, foamed polymer, or the like, and the adhesive 40 can be rubber-based, acrylic-based, silicone-based, urethane-based, or the like.

[0024] The connection portion 11 is preferably filled with a sealant 60 made of synthetic resin and / or synthetic rubber. The sealant 60 can prevent water from entering from the outside and can also prevent water from entering from the inside in the unlikely event that a part of the fiber sheet 20 is peeled off due to water pressure from the inside.

[0025] The sealant 60 is not particularly limited, but from the viewpoints of adhesion to concrete, water resistance, durability, etc., silicone-based materials (for example, Silicone Sealant, manufactured by Cemedine Co., Ltd.), acrylic urethane-based materials (for example, Bond AU Quick, manufactured by Bond Co., Ltd., modified silicone-based materials (for example, POS Seal Speed, manufactured by Cemedine Co., Ltd.), etc. are suitable. Other sealant 60 that can be used include silylated acrylate-based, polyisobutylene-based, polysulfide-based, polyurethane-based, acrylic-based, and butyl rubber-based sealants. In particular, when filling the sealant 60, it is preferable to use a primer that is compatible with the sealant 60 for adhesion to concrete.

[0026] It is also preferable to use ethylene propylene diene rubber (EPDM), silicone, chloroprene rubber (CR), foamed polypropylene, foamed polyethylene, or foamed urethane sealants in combination as a secondary sealant (back-up material) in addition to the above-mentioned sealant 60. In particular, foamed urethane sealants (e.g., Insuron, manufactured by Nippon Spring Co., Ltd.) are preferably used from the viewpoints of water-stopping properties, shape-following ability, workability, etc. EXAMPLES

[0027] Next, the present invention will be described in detail with reference to examples. The concrete pipe 10 used was a type B pipe (φ800 mm×2430 mm) according to the Japan Sewage Works Association standard (JSWAS A-1-2011) with damage to the joint.

[0028] First, the connection part 11 (joint part) of the concrete pipe 10 was cleaned and any deteriorated parts of the connection part 11 were removed, and then "Silicone Primer B manufactured by Cemedine Co., Ltd." was applied as a primer for the sealant and left to stand for 30 minutes.

[0029] Next, the connection portion 11 was filled with a sealant 60, such as "Cemedine 8060 Pro Silicone Sealant, manufactured by Cemedine Co., Ltd.", and the connection portion 11 was left to cure for about 12 hours until the surface hardened.

[0030] After the joint 11 is filled with the sealant 60, the inner surface of the concrete pipe 10 is washed with acetone, and the primer 50 is applied over the entire surface of both sides of 600 mm width (one side of 300 mm width) from the joint 11 with 0.1 kg / m of epoxy resin-based primer "Bond E810LW, viscosity 400 mPa s, manufactured by Konishi Co., Ltd." 2 After application, the mixture was left to stand for 24 hours.

[0031] Next, 12 rolls of double-sided adhesive tape (Bond TM Tape R1, manufactured by Konishi Co., Ltd.; a tape with an acrylic adhesive applied to both sides of a foamed polymer base material. 1 mm thick, 25 mm wide) were used as adhesive 40 and attached over the entire area that would become the adhesive region 41, which was 300 mm wide on both sides (150 mm wide on each side) from the center of the joint.

[0032] Next, an epoxy resin putty "Bond E395W, manufactured by Konishi Co., Ltd." is applied at 1.5 kg / m over the entire area of ​​the adhesive tape, which is to be the adhesive area 31 and has a width of 150 mm on both sides of the adhesive tape. 2 After application, the mixture was left to stand for 24 hours.

[0033] Next, an epoxy resin adhesive 30 (Bond E2500W, manufactured by Konishi Co., Ltd., viscosity 6000 mPa·s) was applied to the top of the epoxy resin putty at 1.0 kg / m 2 It was applied.

[0034] Next, a plain weave fabric (Teijin Frontier Co., Ltd., TWF3001; warp density 18 threads / inch, weft density 17 threads / inch, warp strength 7050N / inch, weft strength 7050N / inch, basis weight 455g / mm2, thickness 0.7mm) made of para-aramid fiber (Teijin Co., Ltd., Twaron, T2200, 3220dtex2000filament) was attached as a fiber sheet 20 over the entire width of both sides (300mm width on one side) from the connection part 11 so that the center part was in contact with the adhesive 40 and both sides were in contact with the adhesive 30. At this time, two 1560mm fiber sheets were prepared for the circumference length of the concrete pipe 10 of about 2510mm, and they were attached so that the top and bottom overlapped by about 300mm.

[0035] Next, in the adhesive regions 31 each having a width of 150 mm on both sides, 0.6 kg / m 2 was applied from above the fiber sheet 20 so that the adhesive 30 penetrated into the fiber sheet 20. 2 At this time, air bubbles were removed using a defoaming roller while coating, and the coating was then left to stand for one week.

[0036] Four pairs of joint structures of the concrete pipes 10 manufactured by the above process were prepared, and a pull-out test, a bending test, an inner watertightness test, and an outer watertightness test were performed.

[0037] (Withdrawal test) Hydraulic jacks were attached at three points from the outer periphery of the concrete pipe 10 to straddle the joint portion, and the longitudinal removal force was measured. As a result, the fiber sheet 20 removed at 310 kN. When the adhesive force was calculated from the area (one side) of the adhesive region 31 where the fiber sheet 20 and concrete pipe 10 were attached with the adhesive 30, the fiber sheet 20 was attached to the concrete pipe 10 by the adhesive 30 with an adhesive force of 0.82 N / mm2. It is possible to control the removal force by controlling the area where the fiber sheet 20 is attached to the inner periphery of the concrete pipe 10 with the adhesive 30.

[0038] (Bending test) One side of the concrete pipe 10 was lifted with a hydraulic jack, and the angle at which the fiber sheet 20 peeled off was measured. As a result, peeling of the fiber sheet 20 was observed when the bending angle reached 2 degrees. It is possible to control the maximum bending angle by controlling the adhesive strength of the adhesive region 31 and the area of ​​the adhesive region 41 in the center of the fiber sheet 20 where the fiber sheet 20 is attached by the adhesive 40 so that it can easily stretch.

[0039] (Internal water pressure test) Even when an internal water pressure of 1.0 MPa was applied from the inside of the concrete pipe 10 and maintained for five minutes, no water leakage was observed from the outside.

[0040] (External water pressure test) Even when an external water pressure of 0.2 MPa was applied from the outside of the concrete pipe 10 and maintained for two minutes, no water leakage was observed from the inside.

[0041] As described above, according to this embodiment, fiber sheets 20 are provided which are attached to the inner surfaces of both of the adjacent concrete pipes 10 so as to straddle the connection portions 11 of the concrete pipes 10, and the fiber sheets 20 are spaced apart across the connection portions 11 and adhered to the inner surfaces of both of the concrete pipes 10 by adhesive 30. With this configuration, the fiber sheets 20 are attached to the inner circumferential surfaces of both concrete pipes 10 with adhesive 30, with a gap between them and the connecting portion 11, so that it has a suitable flexibility and range of motion while being difficult to come off, and since the fiber sheet 20 is attached to the inner circumferential surface of the concrete pipe 10, it is possible to realize a joint structure for the concrete pipes 10 with little bulging on the inner surface. Furthermore, since it has a suitable flexibility and range of motion and allows for slight movement, periodic checking work for loosening, etc. can be omitted, and a permanent joint structure can be realized.

[0042] Furthermore, according to this embodiment, the spacing between the adhesive regions 31 in which the fiber sheet 20 is adhered to the inner surfaces of both concrete pipes 10 by the adhesive 30 is set to 50 to 500 mm across the connection portion 11. With this configuration, even if the concrete pipe 10 is bent at the joint portion once or more, the fiber sheet 20 can be prevented from peeling off due to expansion and contraction at the adhesive region 41.

[0043] Furthermore, according to this embodiment, the fiber sheet 20 is adhered to the inner circumferential surfaces of both concrete pipes 10 by the adhesive 30 in predetermined areas sandwiching the joint portion 11 . With this configuration, the fiber sheet 20 can be attached to the inner surface of the concrete pipe 10 while maintaining its elasticity.

[0044] Furthermore, according to this embodiment, the fiber sheet 20 has a basis weight of 100 to 1000 g / m 2 The woven fabric has a strength in the weft direction of 500 to 50,000 N / cm and a breaking elongation in the weft direction of 1 to 20%. The fiber sheet 20 is attached to the concrete pipe 10 so that the fibers constituting the woven fabric are oriented in the longitudinal direction of the concrete pipe 10. This configuration makes it possible to realize a joint structure for the concrete pipe 10 that has appropriate flexibility and range of motion while being difficult to come loose.

[0045] Furthermore, according to this embodiment, the connection portion 11 is filled with a sealant 60 made of synthetic resin and / or synthetic rubber. As the sealant 60, one or more of silicone-based, acrylic urethane-based, and modified silicone-based sealants are used. This configuration can prevent water from entering from the outer surface, and can also prevent water from entering from the inner surface in the unlikely event that a portion of the fiber sheet 20 is peeled off due to water pressure from the inner surface.

[0046] It is clear that the present invention is not limited to the above-described embodiments, and each embodiment can be appropriately modified within the scope of the technical concept of the present invention. Furthermore, the number, position, shape, etc. of the above-described components are not limited to the above-described embodiments, and the number, position, shape, etc. can be set to be suitable for implementing the present invention. In each drawing, the same components are given the same reference numerals. [Explanation of symbols]

[0047] 10 Concrete pipe 11 Connection 20 Fiber Sheet 30. Glue 31 Adhesion area 40 Adhesive 41 Adhesive area 50 Primer 60 Sealant

Claims

[Claim 1] A low-viscosity epoxy resin having a viscosity of less than 1000 mPa·s at 20°C when mixed with a base agent and a hardener is applied as a primer to a predetermined area on the inner surface of both of the concrete pipes that sandwich the joints of the adjacent concrete pipes; An epoxy resin having a viscosity of 1000 to 50000 mPa·s at 20°C when mixed with a base agent and a hardener is applied as an adhesive to the inner peripheral surfaces of both of the concrete pipes to which the primer has been applied, with a gap therebetween and sandwiching the connection portion; A method for manufacturing a concrete pipe joint structure, characterized in that a fiber sheet is attached so that it comes into contact with the adhesive applied to the inner surfaces of both of the concrete pipes.

Citation Information

Patent Citations

  • JP1982115477U

  • The inner surface of existing pipe joint leakage preventing structure

    JP1983104485U

  • Headrace tunnel structure and reparing method for headrace tunnel

    JP1993231095A

  • High strength rubberized fabric for flexible film-made undulating weir

    JP1998219661A

  • Pipe lining material and pipe lining method

    JP2000177010A