Method for manufacturing optical film, optical film, optical member, image display device, method for manufacturing optical member, and method for manufacturing image display device

By using a mask material with specific thickness ratios and a controlled manufacturing process, the method prevents the anti-glare layer from impairing the transparency of the transparent layer in optical films, ensuring clear and distortion-free images.

JP7587404B2Active Publication Date: 2024-11-20NITTO DENKO CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020199185
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-30
Publication Date
2024-11-20
Estimated Expiration
2040-11-30

AI Technical Summary

Technical Problem

The manufacturing process of optical films with perforated anti-glare layers and transparent clear hard coat layers can result in the anti-glare layer forming liquid remaining in recesses of the clear hard coat layer, impairing its transparency.

Method used

A method involving a mask material with specific thickness ratios and a manufacturing process that includes laminating a non-transparent layer on a base material, forming a transparent layer in through holes, and then removing the mask material, ensuring the thickness ratio of the transparent layer's thinnest part to the mask material's minimum thickness at the outer periphery satisfies T2/T1 ≤ 3, thereby preventing the anti-glare layer from remaining in recesses.

Benefits of technology

This method ensures the transparency of the transparent layer is maintained by preventing the anti-glare layer from forming non-transparent parts, enhancing the optical film's clarity and reducing distortions during image viewing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587404000004
    Figure 0007587404000004
  • Figure 0007587404000005
    Figure 0007587404000005
  • Figure 0007587404000006
    Figure 0007587404000006
Patent Text Reader

Abstract

To provide an optical film manufacturing method that does not damage the transparency of a transparent layer.SOLUTION: A manufacturing method of an optical film 10 having a transparent layer 13 formed in a through-hole of a non-transparent layer 12 includes: a mask material coating step of coating one surface of a substrate 11 with a mask material 21 in which a through-hole 21h for transparent layer formation is formed; a transparent layer formation step of applying a transparent layer forming liquid to the inside of the through-hole 21h for transparent layer formation so as to form the transparent layer 13; a mask material removal step of removing the mask material 21 from the substrate 11; and a non-transparent layer formation step of applying a non-transparent layer forming liquid to a transparent layer 13 forming surface of the substrate 11 so as to form the non-transparent layer 12. The optical film 10 is characterized in that T2 / T1 is equal to or smaller than 3, in which T2 (μm) is the minimum thickness of the mask material 21 on the outer periphery of the through-hole 21h for transparent layer formation, and T1 (μm) is the thickness of the thinnest part of the transparent layer 13.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an optical film, an optical film, an optical member, an image display device, a method for producing an optical member, and a method for producing an image display device. [Background technology]

[0002] 2. Description of the Related Art In optical films used in image display devices and the like, non-transparent layers such as antiglare layers are sometimes formed by coating with a liquid (Patent Document 1, etc.). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2009-109683 A Summary of the Invention [Problem to be solved by the invention]

[0004] On the other hand, in such optical films, there are cases where a part of the antiglare layer is perforated and a transparent clear hard coat layer is formed in the perforated area, but in this case, the following problems may occur in the manufacturing process of the optical film.

[0005] An example of the manufacturing process of the optical film as described above is shown in the process cross-sectional views of Figures 4(a) and (b). First, as shown in Figure 4(a), one surface of the substrate 11 is covered with a mask material 21. A through hole 21h is formed in the mask material 21. Next, a clear hard coat layer forming liquid is applied (coated) from above the mask material 21. As the clear hard coat layer forming liquid solidifies, a clear hard coat layer (transparent layer) 13 is formed in the through hole 21h of the mask material 21 as shown in Figure 4(a). As the clear hard coat layer forming liquid solidifies, an unnecessary layer 13b is formed on the mask material 21.

[0006] Next, as shown in FIG. 4(b), the mask material 21 is peeled off and removed from the substrate 11 together with the unnecessary layer 13b. Furthermore, the antiglare layer forming liquid is applied to the surface of the substrate 11 on which the clear hard coat layer 13 is formed, and solidified to form the antiglare layer (non-transparent layer) 12 as shown in the figure. However, at this time, if the recesses on the surface of the clear hard coat layer 13 are deep, there is a risk that the antiglare layer forming liquid will remain in the recesses on the surface of the clear hard coat layer 13. If the remaining antiglare layer forming liquid solidifies, a non-transparent portion 12d will be formed on the surface of the clear hard coat layer 13 as shown in FIG. 4(b), and the transparency of the clear hard coat layer 13 may be impaired.

[0007] Therefore, an object of the present invention is to provide a method for producing an optical film that does not impair the transparency of a transparent layer, an optical film, an optical member, an image display device, a method for producing an optical member, and a method for producing an image display device. [Means for solving the problem]

[0008] In order to achieve the above object, the method for producing an optical film of the present invention comprises the steps of: A method for producing an optical film having a non-transparent layer laminated on a substrate, comprising the steps of: the non-transparent layer has a through hole, and a transparent layer is formed in the through hole; The manufacturing method includes a mask material coating step, a transparent layer forming step, a mask material removing step, and a non-transparent layer forming step, In the mask material coating step, one surface of the base material is coated with a mask material having the transparent layer formation through hole formed therein; After the mask material coating step, in the transparent layer forming step, a transparent layer forming liquid is applied into the transparent layer forming through hole to form the transparent layer; After the transparent layer forming step, in the mask material removing step, the mask material is removed from the base material; After the mask material removing step, in the non-transparent layer forming step, a non-transparent layer forming liquid is applied onto the transparent layer forming surface of the base material to form the non-transparent layer; The transparent layer is characterized in that the thickness of the thinnest portion and the minimum thickness of the mask material on the outer periphery of the transparent layer-forming through hole satisfy the relationship of the following mathematical formula (1). T2 / T1≦3 (1) In the formula (1), T1 is the thickness (μm) of the thinnest part of the transparent layer, and T2 is the minimum thickness (μm) of the mask material on the outer periphery of the transparent layer-forming through hole.

[0009] The optical film of the present invention is an optical film produced by the above-mentioned method for producing an optical film of the present invention.

[0010] The optical member of the present invention is an optical member that includes the optical film of the present invention.

[0011] The image display device of the present invention is an image display device that includes the optical film of the present invention or the optical member of the present invention.

[0012] The method for producing an optical member of the present invention includes a step of producing the optical film of the present invention by the method for producing an optical film of the present invention.

[0013] The method for producing an image display device of the present invention includes a step of producing the optical film of the present invention by the method for producing an optical film of the present invention. Effect of the Invention

[0014] According to the present invention, it is possible to provide a method for producing an optical film that does not impair the transparency of a transparent layer, an optical film, an optical member, an image display device, a method for producing an optical member, and a method for producing an image display device. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1 is a cross-sectional view showing an example of the optical film of the present invention and a process for producing the same. [Diagram 2]FIG. 2 is a plan view of the optical film of the present invention produced by the production method of FIG. [Diagram 3] FIG. 3 is a cross-sectional view showing another process of an example of the method for producing the optical film of the present invention. [Figure 4] FIG. 4 is a cross-sectional view showing steps of an example of a method for producing an optical film related to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Next, the present invention will be described in more detail with reference to examples, but the present invention is not limited to the following description in any way.

[0017] In the method for producing an optical film of the present invention, for example, the major axis R1 of the transparent layer may be 2.5 mm or more.

[0018] In the method for producing an optical film of the present invention, for example, the water contact angle of the surface of the transparent layer may be 85° or more.

[0019] In the method for producing an optical film of the present invention, for example, in the transparent layer, the thickness of the thinnest part and the thickness of the thickest part may satisfy the relationship of the following mathematical formula (2). H1 / T1≦3.5 (2) In the formula (2), T1 is the thickness (μm) of the thinnest part of the transparent layer, and H1 is the thickness (μm) of the thickest part of the transparent layer.

[0020] In the method for producing an optical film of the present invention, for example, the transparent layer may have a light transmittance at a wavelength of 550 nm of 80% or more, or 81% or more.

[0021] In the method for producing an optical film of the present invention, for example, the transparent layer may be a clear hard coat layer.

[0022] In the method for producing an optical film of the present invention, for example, the non-transparent layer may have a light transmittance at a wavelength of 550 nm of less than 80% or 79% or less.

[0023] In the method for producing an optical film of the present invention, for example, the non-transparent layer may be an antiglare layer.

[0024] The method for producing the optical film of the present invention includes, for example, The substrate and the mask material are long-sized, The mask material coating step, the transparent layer forming step, the mask material removing step, and the non-transparent layer forming step may be performed successively while the base material is being transported.

[0025] The optical member of the present invention may be, for example, a polarizing plate.

[0026] In the present invention, unless otherwise specified, "weight" and "mass" may be read interchangeably. For example, "parts by mass" may be read as "parts by weight", "parts by weight" may be read as "parts by mass", "% by mass" may be read as "% by weight", and "% by weight" may be read as "% by mass".

[0027] [1. Manufacturing method of optical film] The method for producing an optical film of the present invention will be described in more detail below with reference to examples.

[0028] [1-1. Overview of manufacturing methods for optical films] The process cross-sectional views of FIGS. 1(a) to (d) show one example of the method for producing the optical film of the present invention.

[0029] First, as shown in FIG. 1(a), a substrate 11 is prepared. The substrate 11 may be, for example, a resin film. Next, as shown in the figure, one surface of the substrate 11 is covered with a mask material 21 in which a transparent layer-forming through hole 21h is formed (mask material covering step). Then, a transparent layer-forming liquid is applied (coated) on the mask material 21. As a result, the transparent layer-forming liquid is applied in the transparent layer-forming through hole 21h, and is solidified to form a transparent layer 13 as shown in FIG. 1(b) (transparent layer forming step). At this time, an unnecessary layer 13b is formed on the mask material 21 by solidification of the transparent layer-forming liquid. Then, the mask material 21 is peeled off from the substrate 11 together with the unnecessary layer 13b and removed (mask material removing step). Then, an antiglare layer-forming liquid is applied to the surface of the substrate 11 on which the transparent layer 13 is formed, and is solidified to form a non-transparent layer 12 as shown in FIG. 1(d) (non-transparent layer forming step). In this manner, the optical film 10 of the present invention shown in Fig. 1(d) can be manufactured. In Fig. 1(d), the non-transparent layer 12 is an anti-glare layer, and the non-transparent layer (anti-glare layer) 12 is formed by containing particles 12b in a resin layer 12a, and unevenness is formed on the surface of the resin layer 12a. However, this is merely an example, and the non-transparent layer in the present invention is not limited to this.

[0030] In the present invention, the "non-transparent layer" refers to a layer having a light transmittance of less than 80% at a wavelength of 550 nm. The non-transparent layer may have a light transmittance of, for example, 79% or less, 78% or less, 77% or less, 76% or less, or 75% or less at a wavelength of 550 nm, or may have a light transmittance of, for example, 1% or more, 2% or more, 3% or more, 4% or more, or 5% or more.

[0031] In the present invention, the non-transparent layer is not particularly limited, and may be, for example, an antiglare layer as described above, or may be a protective layer, a light diffusing layer, a surface coating layer, a hard coat layer, etc. The antiglare layer may be, for example, an antiglare hard coat layer.

[0032] In the present invention, the "transparent layer" refers to a layer having a light transmittance of 80% or more at a wavelength of 550 nm. In the present invention, the transparent layer may have a light transmittance of 81% or more, 82% or more, 83% or more, 84% or more, or 85% or more at a wavelength of 550 nm, and the upper limit is not particularly limited, but may be, for example, 100% or less, and may be, for example, 99% or less, 98% or less, 97% or less, 96% or less, or 95% or less.

[0033] In the present invention, the transparent layer is not particularly limited, and may be, for example, a clear hard coat layer as described above, or a protective layer, a surface coating layer, a hard coat layer, etc. The transparent layer may be, for example, a transparent layer for a camera hole of an image display device, or a transparent layer for a lens, etc.

[0034] In the present invention, the method for measuring the light transmittance is not particularly limited, but it can be measured, for example, by the measurement method described in the Examples below.

[0035] Furthermore, as described above, the method for manufacturing an optical film of the present invention is characterized in that the thickness of the thinnest part of the transparent layer and the minimum thickness of the mask material on the outer periphery of the through hole for forming the transparent layer satisfy the relationship of the following mathematical formula (1). T2 / T1≦3 (1) In the formula (1), T1 is the thickness (μm) of the thinnest part of the transparent layer, and T2 is the minimum thickness (μm) of the mask material on the periphery of the through hole for forming a transparent layer. Note that the "minimum thickness" of the mask material on the periphery of the through hole for forming a transparent layer refers to the thickness of the thinnest part of the mask material on the periphery of the through hole for forming a transparent layer.

[0036] In the present invention, the "thinnest part" refers to the part having the smallest thickness, and the "thickest part" refers to the part having the largest thickness. In the present invention, the method for measuring the thickness is not particularly limited, but can be, for example, measured by the measurement method described in the examples below.

[0037] An example of the method for producing an optical film of the present invention is shown in the process cross-sectional views of Figures 3(a) and (b). Figure 3(a) shows the state after the mask material coating process and the transparent layer forming process, and shows the same state as Figure 1(b). As shown in the figure, in this production method, the thickness T1 (μm) of the thinnest part of the transparent layer 13 and the minimum thickness T2 (μm) of the mask material 21 on the periphery of the transparent layer forming through hole 21h satisfy the relationship T2 / T1≦3 (the above formula (1)).

[0038] FIG. 4(a) above shows an example where T2 / T1 exceeds 3. When T2 / T1 exceeds 3, as described above, the recesses on the surface of the transparent layer 13 become deep, and non-transparent parts 12d are formed in the recesses, which may impair the transparency of the transparent layer 13. On the other hand, according to the present invention, such a problem is solved by making T2 / T1 3 or less, and an optical film in which the transparency of the transparent layer is not impaired can be provided. In the present invention, the method for measuring the transparency of the transparent layer is not particularly limited, and can be measured, for example, by the measurement method described in the examples below.

[0039] In the method for producing an optical film of the present invention, the thickness of the mask material is not particularly limited, and may be, for example, 50 μm or less, 47 μm or less, 44 μm or less, 41 μm or less, or 38 μm or less, and may be, for example, 2 μm or more, 5 μm or more, 8 μm or more, 11 μm or more, or 14 μm or more. For example, from the viewpoints of the following [1] to [5], it is preferable to use a mask material that is as thin as possible. [1] The use of a thin mask material makes it easier to improve the processing accuracy of drilling holes (forming through holes) in the mask material, which in turn makes it easier to improve the accuracy (uniformity) of the dimensions and shape of the edges of the transparent layer. [2] By using a thin masking material, it becomes easier to drill holes of various shapes. [3] A thin mask material is less likely to produce burrs when drilling holes and is less likely to trap air bubbles when attached to the base material. [4] By using a thin masking material, the depth of the recesses in the transparent layer can be reduced, thereby reducing distortion when viewing an image through the transparent layer. [5] Using a thin masking material can prevent the transparent layer from becoming thicker than expected.

[0040] In the method for producing an optical film of the present invention, T2 / T1 is not particularly limited except that the relationship of the above-mentioned mathematical formula (1) is satisfied. The lower limit of T2 / T1 is not particularly limited, but is a value exceeding 0, and may be, for example, 0.7 or more, 0.8 or more, 0.9 or more, 1.0 or more, 1.1 or more, 1.2 or more, 1.3 or more, 1.4 or more, or 1.5 or more. The upper limit of T2 / T1 is 3 or less as described above, and may be, for example, 2.9 or less, 2.8 or less, 2.7 or less, 2.6 or less, or 2.5 or less.

[0041] As described above, in the method for producing an optical film of the present invention, the transparent layer may have a thickness T1 (μm) of the thinnest part and a thickness H1 (μm) of the thickest part satisfying the relationship H1 / T1≦3.5 (the above formula (2)). FIG. 3(b) shows such an example. For the sake of simplicity, FIG. 3(b) shows the non-transparent layer 12 as having a flat surface and not including particles or the like.

[0042] By making H1 / T1 3.5 or less, the depth of the recesses of the transparent layer is suppressed, so that the phenomenon that the non-transparent layer forming liquid remains in the recesses of the transparent layer and the non-transparent portion is formed can be further suppressed. In addition, by suppressing the depth of the recesses of the transparent layer, distortion when an image is viewed through the transparent layer can be suppressed. Furthermore, by suppressing the depth of the recesses of the transparent layer, for example, the scratch resistance of the transparent layer is improved. The lower limit of H1 / T1 is not particularly limited, but is 1 or more, and may be, for example, 1.2 or more, 1.4 or more, 1.6 or more, 1.8 or more, or 2.0 or more. The upper limit of H1 / T1 is 3.5 or less as described above, and may be, for example, 3.4 or less, 3.3 or less, 3.2 or less, 3.1 or less, or 3.0 or less.

[0043] The thickness of the thinnest part of the transparent layer is not particularly limited, but may be, for example, 1.0 μm or more, 1.2 μm or more, 1.4 μm or more, 1.6 μm or more, or 1.8 μm or more, and may be, for example, 30 μm or less, 28 μm or less, 26 μm or less, 24 μm or less, or 22 μm or less. The thickness of the thickest part of the transparent layer is not particularly limited, but may be, for example, 1.0 μm or more, 1.2 μm or more, 1.4 μm or more, 1.6 μm or more, or 1.8 μm or more, and may be, for example, 50 μm or less, 48 ​​μm or less, 46 μm or less, 44 μm or less, or 42 μm or less.

[0044] In addition, in the method for producing an optical film of the present invention, as described above, the major axis R1 of the transparent layer may be 2.5 mm or more. In the present invention, the "major axis" refers to the diameter of the part with the longest diameter. For example, in the case of a circle, the diameter is the major axis, in the case of an ellipse, the length of the major axis is the major axis, and in the case of a rectangle, the length of the diagonal is the major axis. The larger the diameter of the transparent layer, the less likely the non-transparent layer forming liquid will remain in the recess of the transparent layer, and the transparency of the transparent layer tends to be less likely to be impaired (easier to be partially cleared). By not impairing the transparency of the transparent layer, blurring when an image is viewed through the transparent layer can be suppressed. The major axis R1 of the transparent layer may be, for example, 2.6 mm or more, 2.7 mm or more, 2.8 mm or more, 2.9 mm or more, or 3.0 mm or more, and may be, for example, 100 mm or less, 90 mm or less, 80 mm or less, 70 mm or less, or 60 mm or less.

[0045] In addition, in the method for producing an optical film of the present invention, as described above, the water contact angle of the transparent layer surface may be 85° or more. A large water contact angle means high hydrophobicity. When the transparent layer surface is highly hydrophobic, the non-transparent layer forming liquid is easily repelled, so that the non-transparent layer forming liquid is less likely to adhere to the transparent layer surface. Since the non-transparent layer forming liquid is less likely to adhere, the formation of a non-transparent part on the transparent layer surface can be suppressed. Therefore, blurring when an image is viewed through the transparent layer can be suppressed. Furthermore, since the transparent layer is easily repelled (the non-transparent layer forming liquid is less likely to adhere), the types of non-transparent layer forming liquid that can be used are increased, and the properties of the non-transparent layer can be changed arbitrarily. The water contact angle of the transparent layer surface may be, for example, 85° or more, 86° or more, 87° or more, 88° or more, or 89° or more, and may be, for example, 115° or less, 114° or less, 113° or less, 112° or less, or 110° or less. In the present invention, the method for measuring the water contact angle is not particularly limited, but it can be measured, for example, by the measurement method described in the Examples below.

[0046] Hereinafter, each step of the method for producing the optical film of the present invention will be described in more detail with reference to examples. In the following, an example will be mainly described in which the non-transparent layer is an anti-glare layer, and the optical film of the present invention produced is an anti-glare film. However, as described above, the present invention is not limited thereto. In the following, the optical film of the present invention that is an anti-glare film may be referred to as the "anti-glare film of the present invention".

[0047] [1-2. Masking material coating process] First, one surface of the base material is covered with a mask material in which the through holes for forming the transparent layer are formed (mask material covering step).

[0048] The substrate is not particularly limited, but may be, for example, a light-transmitting substrate, and specifically, for example, a transparent plastic film substrate. The transparent plastic film substrate is not particularly limited, but is preferably one having excellent visible light transmittance (preferably a light transmittance of 90% or more) and excellent transparency (preferably a haze value of 1% or less), and for example, the transparent plastic film substrate described in JP-A-2008-90263 is exemplified. As the transparent plastic film substrate, one having optically low birefringence is suitably used. The optical film of the present invention can be used, for example, as a protective film for a polarizing plate, and in this case, the transparent plastic film substrate is preferably a film formed from triacetyl cellulose (TAC), polycarbonate, an acrylic polymer, a polyolefin having a cyclic or norbornene structure, or the like. In addition, in the present invention, the transparent plastic film substrate may be a polarizer itself. With such a configuration, a protective layer made of TAC or the like is not required, and the structure of the polarizing plate can be simplified, so that the number of manufacturing steps for the polarizing plate or the image display device can be reduced, and production efficiency can be improved. In addition, such a configuration allows the polarizing plate to be made thinner. When the transparent plastic film substrate is a polarizer, for example, the non-transparent layer serves as a protective layer. In addition, such a configuration allows the optical film of the present invention to also function as a cover plate when attached to the surface of a liquid crystal cell, for example.

[0049] In the present invention, the thickness of the substrate is not particularly limited, but considering strength, workability such as handleability, thin layer property, etc., it is, for example, in the range of 10 to 500 μm, 20 to 300 μm, or 30 to 200 μm. The refractive index of the substrate is not particularly limited. The refractive index is, for example, in the range of 1.30 to 1.80 or 1.40 to 1.70.

[0050] In the present invention, the term "refractive index" refers to the refractive index at a wavelength of 550 nm unless otherwise specified. In the present invention, the method of measuring the refractive index is not particularly limited, but the refractive index of fine substances such as particles can be measured using, for example, the Becke method. The Becke method is a measurement method in which a measurement sample is dispersed in a standard refractive index liquid on a slide glass, and the refractive index of the standard refractive index liquid when the outline of the sample disappears or becomes blurred when observed under a microscope is taken as the refractive index of the sample. In addition, the method of measuring the refractive index of a measurement object (e.g., an anti-glare film, an anti-glare layer, or a resin constituting an anti-glare layer) whose refractive index cannot be measured by the Becke method is not particularly limited, but can be measured using, for example, a general refractometer (instrument for measuring refractive index). The refractometer is also not particularly limited, but examples thereof include an Abbe refractometer. Examples of the Abbe refractometer include a multi-wavelength Abbe refractometer DR-M2 / 1550 (product name) manufactured by Atago Co., Ltd.

[0051] In the optical film manufacturing method of the present invention and the optical film of the present invention, for example, the resin contained in the substrate may include an acrylic resin. Also, for example, the substrate may be an acrylic film.

[0052] The mask material is not particularly limited, and may be, for example, a PET (polyethylene terephthalate) film, a PE (polyethylene) film, a TAC (triacetyl cellulose) film, a COP (cycloolefin) film, etc. The thickness of the mask material is, for example, as described above.

[0053] When covering one side of the substrate with the mask material, the mask material and one side of the substrate may be bonded together with an adhesive or the like. The adhesive is not particularly limited, but examples thereof include acrylic adhesives, polyethylene adhesives, polypropylene adhesives, polyolefin adhesives, and the like. In the subsequent mask removal step, the mask material needs to be removed from the substrate, so the adhesive needs to be one that can be peeled off from the substrate again. The thickness of the adhesive applied is not particularly limited, but may be, for example, 1 μm or more, 2 μm or more, 3 μm or more, 4 μm or more, or 5 μm or more, and may be, for example, 10 μm or less, 9 μm or less, 8 μm or less, 7 μm or less, or 6 μm or less. In addition, for example, the mask material may simply be superimposed on one side of the substrate without using an adhesive.

[0054] [1-3. Transparent layer formation process] After the mask material coating step, a transparent layer forming liquid is applied into the transparent layer forming through hole to form the transparent layer (transparent layer forming step).

[0055] The transparent layer forming liquid is not particularly limited, but may be the same as a general clear hard coat layer forming liquid, for example. The transparent layer forming liquid may be, for example, a monomer that can be polymerized (cured) by heating or light irradiation, dissolved in a solvent. The monomer is not particularly limited, but examples include polyfunctional acrylates and monofunctional acrylates, and one type may be used alone or two or more types may be used in combination. The content of the monomer is not particularly limited, but may be, for example, 1 mass% or more, 2 mass% or more, 3 mass% or more, 4 mass% or more, or 5 mass% or more of the total solid content (components other than the solvent) in the transparent layer forming solution, and may be, for example, 60 mass% or less, 59 mass% or less, 58 mass% or less, 57 mass% or less, or 56 mass% or less. In addition to or in place of the monomer, any substance that can be polymerized (cured) by heating or light irradiation may be used. The substance that can be polymerized (cured) by heating or light irradiation may be, for example, a prepolymer such as urethane acrylate.

[0056] The transparent layer forming liquid may also contain, for example, an antifouling agent. When the transparent layer forming liquid contains an antifouling agent, the non-transparent layer forming liquid is less likely to adhere to the transparent layer surface, and the transparency of the transparent layer can be prevented from being impaired. The antifouling agent is not particularly limited, but examples thereof include fluorine-based antifouling agents and silicone-based antifouling agents, and specific examples thereof include "KY-1203" (trade name) manufactured by Shin-Etsu Chemical Co., Ltd., "LE-303" (trade name) manufactured by Kyoeisha Chemical Co., Ltd., and "PC4100" (trade name) manufactured by DIC Corporation. The content of the antifouling agent is not particularly limited, but may be, for example, 0.1% by mass or more, 0.2% by mass or more, 0.3% by mass or more, 0.4% by mass or more, or 0.5% by mass or more of the total solid content (components other than the solvent) in the transparent layer forming solution, and may be, for example, 20% by mass or less, 18% by mass or less, 16% by mass or less, 14% by mass or less, or 12% by mass or less.

[0057] The solvent is not particularly limited, and various solvents can be used, and one type may be used alone, or two or more types may be used in combination. Specific examples of the solvent include alcohols such as methanol, ethanol, isopropyl alcohol (IPA), butanol, t-butyl alcohol (TBA), and 2-methoxyethanol; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclopentanone; esters such as methyl acetate, ethyl acetate, and butyl acetate; ethers such as diisopropyl ether and propylene glycol monomethyl ether; glycols such as ethylene glycol and propylene glycol; cellosolves such as ethyl cellosolve and butyl cellosolve; aliphatic hydrocarbons such as hexane, heptane, and octane; and aromatic hydrocarbons such as benzene, toluene, and xylene. In addition, for example, the solvent may include a hydrocarbon solvent and a ketone solvent. The hydrocarbon solvent may be, for example, an aromatic hydrocarbon. The aromatic hydrocarbon may be, for example, at least one selected from the group consisting of toluene, o-xylene, m-xylene, p-xylene, ethylbenzene, and benzene. The ketone solvent may be, for example, cyclopentanone, and at least one selected from the group consisting of acetone, methyl ethyl ketone, methyl isobutyl ketone, diethyl ketone, cyclohexanone, isophorone, and acetophenone.

[0058] The coating thickness of the transparent layer forming liquid is not particularly limited, and may be appropriately set so that the thickness of the transparent layer falls within the above range, for example.

[0059] Furthermore, the transparent layer forming liquid (unnecessary layer 13b in Figs. 1 and 3) that has been applied and solidified on the mask material becomes unnecessary and will be removed later together with the mask material. Therefore, when applying the transparent layer forming liquid, it is preferable to adjust the ejection position of the transparent layer forming liquid so that the transparent layer forming liquid is not applied to any area other than the transparent layer forming through hole. This makes it possible to suppress waste of the transparent layer forming liquid and reduce the amount of the transparent layer forming liquid used.

[0060] After the application of the transparent layer forming liquid, the transparent layer may be formed, for example, by drying and curing the transparent layer forming liquid. The drying may be, for example, natural drying, air drying by blowing air, heat drying, or a combination of these methods.

[0061] The drying temperature of the transparent layer forming liquid may be, for example, in the range of 30 to 200° C. The drying temperature may be, for example, 40° C. or more, 50° C. or more, 60° C. or more, 70° C. or more, 80° C. or more, 90° C. or more, or 100° C. or more, and may be 190° C. or less, 180° C. or less, 170° C. or less, 160° C. or less, 150° C. or less, 140° C. or less, 135° C. or less, 130° C. or less, 120° C. or less, or 110° C. or less. The drying time is not particularly limited, and may be, for example, 30 seconds or more, 40 seconds or more, 50 seconds or more, or 60 seconds or more, and may be 150 seconds or less, 130 seconds or less, 110 seconds or less, or 90 seconds or less.

[0062] The method for curing the coating film formed by drying the transparent layer-forming liquid is not particularly limited, but ultraviolet curing is preferred. The irradiation dose of the energy ray source is 50 to 500 mJ / cm2 as the cumulative exposure dose at an ultraviolet wavelength of 365 nm. 2 The irradiation dose is preferably 50 mJ / cm. 2 If the curing rate is 500 mJ / cm or more, the curing process will proceed sufficiently and the hardness of the transparent layer formed will tend to be high. 2 If the content is equal to or less than this, coloring of the transparent layer to be formed can be prevented.

[0063] [1-4. Masking material removal process] After the transparent layer forming step, the mask material is removed from the base material (mask material removing step). The method for removing the mask material is not particularly limited, but for example, the mask material may be removed from the base material by peeling it off from the base material.

[0064] [1-5. Non-transparent layer formation process] After the mask material removing step, a non-transparent layer forming liquid is applied onto the transparent layer forming surface of the substrate to form the non-transparent layer (non-transparent layer forming step). In the following, the case where the non-transparent layer is an anti-glare layer will be mainly described, but as described above, in the present invention, the non-transparent layer is not limited to only an anti-glare layer and is optional.

[0065] The non-transparent layer forming step may include, for example, a coating step of coating a non-transparent layer forming liquid (coating liquid) on the transparent layer forming surface of the substrate, and a coating film forming step of drying the applied coating liquid to form a coating film. The non-transparent layer forming step may further include, for example, a curing step of curing the coating film. The curing can be performed, for example, after the drying, but is not limited thereto. The curing can be performed, for example, by heating, light irradiation, etc. The light is not particularly limited, but may be, for example, ultraviolet light, etc. The light source for the light irradiation is also not particularly limited, but may be, for example, a high-pressure mercury lamp, etc.

[0066] The non-transparent layer forming liquid may contain, for example, a non-transparent layer forming resin and a solvent. The non-transparent layer forming liquid may be, for example, a non-transparent layer forming liquid containing the non-transparent layer forming resin, a filler, a thixotropy imparting agent, and the solvent.

[0067] The resin for forming the non-transparent layer (hereinafter, sometimes simply referred to as "resin") is not particularly limited, and for example, only one type of resin may be used, or two or more types of resins may be used in combination. The resin may include, for example, an acrylate resin (also called an acrylic resin), or may include, for example, a urethane acrylate resin. The resin may be, for example, a copolymer of a curable urethane acrylate resin and a multifunctional acrylate.

[0068] The resin is not limited to the acrylate resin, and examples thereof include thermosetting resins and ionizing radiation curable resins that are cured by ultraviolet light or light. As the resin, commercially available thermosetting resins and ultraviolet curable resins can also be used.

[0069] As the thermosetting resin or ultraviolet curing resin, for example, a curing compound having at least one of an acrylate group and a methacrylate group that is cured by heat, light (ultraviolet light, etc.), electron beam, etc. can be used, and examples thereof include oligomers or prepolymers of acrylates and methacrylates of polyfunctional compounds such as silicone resins, polyester resins, polyether resins, epoxy resins, urethane resins, alkyd resins, spiroacetal resins, polybutadiene resins, polythiolpolyene resins, polyhydric alcohols, etc. These may be used alone or in combination of two or more types.

[0070] As the resin, for example, a reactive diluent having at least one of an acrylate group and a methacrylate group can be used. The reactive diluent can be, for example, a reactive diluent described in JP-A-2008-88309, and includes, for example, a monofunctional acrylate, a monofunctional methacrylate, a polyfunctional acrylate, and a polyfunctional methacrylate. As the reactive diluent, a trifunctional or higher acrylate and a trifunctional or higher methacrylate are preferable. This is because the hardness of the non-transparent layer can be excellent. As the reactive diluent, for example, butanediol glycerin ether diacrylate, an acrylate of isocyanuric acid, a methacrylate of isocyanuric acid, and the like can be mentioned. These may be used alone or in combination of two or more kinds.

[0071] The refractive index of the resin is not particularly limited, and may be, for example, 1.48 or more, 1.49 or more, 1.50 or more, or 1.51 or more, and may be, for example, 1.60 or less, 1.59 or less, 1.58 or less, or 1.57 or less.

[0072] The filler may be, for example, inorganic particles or organic particles, and one type may be used alone or two or more types may be used in combination. Examples of the inorganic particles include particles formed of silica gel, silicone, titanium oxide, aluminum oxide, zinc oxide, calcium carbonate particles, etc. Examples of the organic particles include particles formed of resin, and examples of the resin include Pst (polystyrene), PMMA (polymethylmethacrylate), copolymers of Pst (polystyrene) and PMMA (polymethylmethacrylate), silicone resin, polycarbonate resin, melamine resin powder, polyolefin resin, polyester resin, polyamide resin, polyimide resin, polyethylene fluoride resin, etc. The particle size, refractive index, etc. of the particles are not particularly limited, and may be the same as or similar to those of a general antiglare layer.

[0073] In addition, the non-transparent layer forming liquid may or may not contain a thixotropy-imparting agent, but it is preferable to contain a thixotropy-imparting agent because it is more likely to exhibit thixotropy. In addition, by containing the thixotropy-imparting agent in the non-transparent layer forming liquid, an effect of preventing the sedimentation of the particles (thixotropic effect) can be obtained. Furthermore, the surface shape of the anti-glare layer (non-transparent layer) can be freely controlled over a wider range by the shear aggregation of the thixotropy-imparting agent itself.

[0074] The solvent is not particularly limited, and various solvents can be used, and one type may be used alone, or two or more types may be used in combination. In order to obtain the anti-glare film of the present invention, the optimal solvent type and solvent ratio may be appropriately selected according to the composition of the resin, the type and content of the particles and the thixotropy-imparting agent, etc. The solvent is not particularly limited, and examples thereof include alcohols such as methanol, ethanol, isopropyl alcohol (IPA), butanol, t-butyl alcohol (TBA), and 2-methoxyethanol; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclopentanone; esters such as methyl acetate, ethyl acetate, and butyl acetate; ethers such as diisopropyl ether and propylene glycol monomethyl ether; glycols such as ethylene glycol and propylene glycol; cellosolves such as ethyl cellosolve and butyl cellosolve; aliphatic hydrocarbons such as hexane, heptane, and octane; and aromatic hydrocarbons such as benzene, toluene, and xylene. In addition, for example, the solvent may include a hydrocarbon solvent and a ketone solvent. The hydrocarbon solvent may be, for example, an aromatic hydrocarbon. The aromatic hydrocarbon may be, for example, at least one selected from the group consisting of toluene, o-xylene, m-xylene, p-xylene, ethylbenzene, and benzene. The ketone solvent may be, for example, at least one selected from the group consisting of cyclopentanone, acetone, methyl ethyl ketone, methyl isobutyl ketone, diethyl ketone, cyclohexanone, isophorone, and acetophenone. The solvent preferably contains the hydrocarbon solvent (for example, toluene) in order to dissolve a thixotropy-imparting agent (for example, a thickener). The solvent may be, for example, a solvent in which the hydrocarbon solvent and the ketone solvent are mixed in a mass ratio of 90:10 to 10:90. The mass ratio of the hydrocarbon solvent and the ketone solvent may be, for example, 80:20 to 20:80, 70:30 to 30:70, or 40:60 to 60:40, etc. In this case, for example, the hydrocarbon solvent may be toluene and the ketone solvent may be methyl ethyl ketone.The solvent may include, for example, toluene and may further include at least one selected from the group consisting of ethyl acetate, butyl acetate, IPA, methyl isobutyl ketone, methyl ethyl ketone, methanol, ethanol, and TBA.

[0075] When an acrylic film is used as the substrate, for example, a good solvent for the acrylic film (acrylic resin) can be suitably used. The solvent may be, for example, a solvent containing a hydrocarbon solvent and a ketone solvent. The hydrocarbon solvent may be, for example, an aromatic hydrocarbon. The aromatic hydrocarbon may be, for example, at least one selected from the group consisting of toluene, o-xylene, m-xylene, p-xylene, ethylbenzene, and benzene. The ketone solvent may be, for example, at least one selected from the group consisting of cyclopentanone, acetone, methyl ethyl ketone, methyl isobutyl ketone, diethyl ketone, cyclohexanone, isophorone, and acetophenone. The solvent may be, for example, a solvent obtained by mixing the hydrocarbon solvent and the ketone solvent in a mass ratio of 90:10 to 10:90. The mass ratio of the hydrocarbon solvent and the ketone solvent may be, for example, 80:20 to 20:80, 70:30 to 30:70, or 40:60 to 60:40, etc. In this case, for example, the hydrocarbon solvent may be toluene and the ketone solvent may be methyl ethyl ketone.

[0076] When triacetyl cellulose (TAC) is used as the base material, a good solvent for TAC can be suitably used, such as ethyl acetate, methyl ethyl ketone, or cyclopentanone.

[0077] In addition, by appropriately selecting the solvent, when containing a thixotropy-imparting agent, the thixotropy of the antiglare layer forming material (non-transparent layer forming liquid) can be well expressed.For example, when using organic clay, toluene and xylene can be preferably used alone or in combination; for example, when using oxidized polyolefin, methyl ethyl ketone, ethyl acetate, propylene glycol monomethyl ester can be preferably used alone or in combination; for example, when using modified urea, butyl acetate and methyl isobutyl ketone can be preferably used alone or in combination.

[0078] Various leveling agents can be added to the non-transparent layer forming liquid. As the leveling agent, for example, a fluorine-based or silicone-based leveling agent can be used for the purpose of preventing coating unevenness (uniformity of the coating surface). In the present invention, a leveling agent can be appropriately selected depending on the case where antifouling is required on the surface of the non-transparent layer (for example, an anti-glare layer), or the case where an anti-reflection layer (low refractive index layer) or a layer containing an interlayer filler is formed on the non-transparent layer as described below. In the present invention, for example, the non-transparent layer forming liquid can be made to exhibit thixotropy by including the thixotropy-imparting agent, so that coating unevenness is unlikely to occur. In this case, for example, it has an advantage that the selection of the leveling agent can be expanded.

[0079] The amount of the leveling agent added is, for example, 5 parts by weight or less, and preferably in the range of 0.01 to 5 parts by weight, relative to 100 parts by weight of the resin.

[0080] The non-transparent layer forming liquid may contain, as necessary, pigments, fillers, dispersants, plasticizers, ultraviolet absorbers, surfactants, antifouling agents, antioxidants, etc., within the scope of not impairing the performance. These additives may be used alone or in combination of two or more.

[0081] In the non-transparent layer forming liquid, for example, a conventionally known photopolymerization initiator such as that described in JP-A-2008-88309 can be used.

[0082] Examples of a method for applying the non-transparent layer forming liquid onto the substrate to form a coating film include coating methods such as fountain coating, die coating, spin coating, spray coating, gravure coating, roll coating, and bar coating.

[0083] Next, as described above, the coating film is dried and cured to form a non-transparent layer (e.g., an antiglare layer). The drying may be, for example, natural drying, air drying by blowing air, heat drying, or a combination of these methods.

[0084] The drying temperature of the non-transparent layer forming liquid may be, for example, in the range of 30 to 200° C. The drying temperature may be, for example, 40° C. or more, 50° C. or more, 60° C. or more, 70° C. or more, 80° C. or more, 90° C. or more, or 100° C. or more, and may be 190° C. or less, 180° C. or less, 170° C. or less, 160° C. or less, 150° C. or less, 140° C. or less, 135° C. or less, 130° C. or less, 120° C. or less, or 110° C. or less. The drying time is not particularly limited, and may be, for example, 30 seconds or more, 40 seconds or more, 50 seconds or more, or 60 seconds or more, and may be 150 seconds or less, 130 seconds or less, 110 seconds or less, or 90 seconds or less.

[0085] The method for curing the coating film is not particularly limited, but ultraviolet curing is preferred. The radiation dose of the energy ray source is 50 to 500 mJ / cm2 as the cumulative exposure dose at an ultraviolet wavelength of 365 nm. 2 The irradiation dose is preferably 50 mJ / cm. 2 If the curing rate is 500 mJ / cm or more, the curing process is likely to proceed sufficiently, and the hardness of the non-transparent layer formed is likely to be high. 2 If the content is equal to or less than this, coloring of the non-transparent layer to be formed can be prevented.

[0086] [1-6. Continuous manufacturing, etc.] The optical film manufacturing method of the present invention can be a continuous manufacturing method. That is, as described above, the optical film manufacturing method of the present invention may be a manufacturing method in which the substrate and the mask material are long, and the mask material coating step, the transparent layer forming step, the mask material removing step, and the non-transparent layer forming step are continuously performed while transporting the substrate. More specifically, for example, the long substrate and the long mask material may each be in a roll shape, and the optical film manufacturing method of the present invention may be performed while unwinding the substrate and the mask material from the roll. Such a method may be, for example, called a roll-to-roll method.

[0087] In the masking material coating step, for example, a masking material having a plurality of holes in both the width direction and the roll flow direction may be attached to the base material roll while being unwound from a roll.

[0088] In the transparent layer forming step, the transparent layer may be formed by applying a transparent layer forming liquid into the transparent layer forming through holes of the masking material while transporting the substrate to which the masking material is attached (covered with the masking material). At this time, as described above, the transparent layer forming liquid (unnecessary layer 13b in Figs. 1 and 3) that is applied and solidified on the masking material becomes unnecessary and is later removed together with the masking material. Therefore, when applying the transparent layer forming liquid, it is preferable to adjust the position of the liquid discharge part of the transparent layer forming liquid so that the transparent layer forming liquid is not applied to any part other than the transparent layer forming through holes as much as possible. This can suppress waste of the transparent layer forming liquid and reduce the amount of the transparent layer forming liquid used.

[0089] The mask material removing step and the non-transparent layer forming step can also be performed continuously while transporting the substrate. In this way, the mask material covering step, the transparent layer forming step, the mask material removing step, and the non-transparent layer forming step are all performed continuously at once, and a long film in which the transparent layer and the non-transparent layer are formed on the substrate can be manufactured. By cutting the long film to the desired size, a plurality of the desired optical films of the present invention can be manufactured. In this way, for example, by using a roll-to-roll method in the manufacturing method of the optical film of the present invention, the optical film of the present invention can be manufactured efficiently and at low cost.

[0090] As described above, the optical film manufacturing method of the present invention can be carried out to manufacture the optical film of the present invention. However, the optical film manufacturing method of the present invention is not limited thereto. For example, the optical film manufacturing method of the present invention may or may not include steps other than the mask material coating step, the transparent layer forming step, the mask material removing step, and the non-transparent layer forming step as appropriate. For example, other layers may or may not be formed on the non-transparent layer. The other layers are not particularly limited, but may be, for example, a low refractive index layer, an anti-reflection layer, a high refractive index layer, a hard coat layer, a pressure-sensitive adhesive layer, etc. The method of forming the other layers is also not particularly limited, and may be, for example, the same as or similar to the method of forming a general low refractive index layer, an anti-reflection layer, a high refractive index layer, a hard coat layer, a pressure-sensitive adhesive layer, etc.

[0091] According to the manufacturing method of the optical film of the present invention, for example, the antiglare layer (non-transparent layer) can be formed using a coating liquid (non-transparent layer forming liquid) in the same manner as in the manufacturing method of a general antiglare film without using a non-liquid antiglare layer forming material. Therefore, for example, the same antiglare layer (non-transparent layer) as in a general antiglare film can be applied to the optical film of the present invention, and the same appearance as that of a general antiglare film can be realized. When the antiglare layer is formed using a non-liquid antiglare layer forming material, there is a risk that the blackness (black tightness) of the screen display is not fully realized and white blurring occurs. However, according to the manufacturing method of the optical film of the present invention, the antiglare layer can be used using a liquid antiglare layer forming material (non-transparent layer forming liquid), so such a problem can be solved. In addition, since the non-transparent layer forming liquid is not particularly limited in the manufacturing method of the optical film of the present invention, it is possible to deal with antiglare layers and antiglare films with any optical properties.

[0092] [2. Optical films, optical members and image display devices] The optical film of the present invention is not particularly limited, and may be, for example, an antiglare film, a protective film, a light diffusion film, a hard coat film, etc. The antiglare film may be, for example, an antiglare hard coat film.

[0093] In the optical film of the present invention, the transparent layer is not particularly limited, and may be, for example, a clear hard coat layer as described above, or a protective layer, a surface coating layer, a hard coat layer, etc. The transparent layer may be, for example, a transparent layer for a camera hole of an image display device, or a transparent layer of a lens, etc. The non-transparent layer may be, for example, an anti-glare layer as described above, or a protective layer, a light diffusion layer, a surface coating layer, a hard coat layer, etc. The anti-glare layer may be, for example, an anti-glare hard coat layer.

[0094] The optical member of the present invention is not particularly limited, but may be, for example, a polarizing plate. The polarizing plate is also not particularly limited, but may include, for example, the antiglare film of the present invention and a polarizer, and may further include other components. Each component of the polarizing plate may be bonded together, for example, with an adhesive or a pressure sensitive adhesive.

[0095] The image display device of the present invention is not particularly limited and may be any image display device, examples of which include a liquid crystal display device, an organic EL display device, an inorganic EL display device, and a plasma display device.

[0096] The configuration of the image display device of the present invention is not particularly limited, and may be the same as that of a general image display device. For example, in the case of an LCD, it can be manufactured by appropriately assembling each component such as a liquid crystal cell, optical members such as a polarizing plate, and an illumination system (backlight, etc.) as necessary, and incorporating a driving circuit.

[0097] The use of the image display device of the present invention is not particularly limited, and it can be used for any use. Examples of the use include office automation equipment such as personal computer monitors, notebook computers, tablets, smartphones, and copy machines, portable devices such as mobile phones, watches, digital cameras, personal digital assistants (PDAs), and portable game consoles, home electric appliances such as video cameras, televisions, and microwave ovens, in-vehicle equipment such as back monitors, monitors for car navigation systems, and car audio, exhibition equipment such as information monitors for commercial stores, security equipment such as surveillance monitors, nursing and medical equipment such as nursing monitors and medical monitors, smart glasses, and VR equipment. The image display device of the present invention may be, for example, an image display device having a camera function. In that case, for example, as described above, the transparent layer in the optical film of the present invention may be a transparent layer for a camera hole of the image display device. According to the present invention, as described above, an optical film can be provided without impairing the transparency of the transparent layer, and therefore, for example, an image display device can be provided without impairing the image quality of a camera image. EXAMPLES

[0098] Next, examples of the present invention will be described together with comparative examples, although the present invention is not limited to the following examples and comparative examples.

[0099] In the following examples and comparative examples, the number of parts of a substance is by mass (parts by weight) unless otherwise specified.

[0100] [Measurement method (light transmittance)] In the following Examples and Comparative Examples, the light transmittance was measured as follows: Using a microspectroscopic system (product name LvmicroZ2, manufactured by LambdaVision), a 5x objective lens, and a 100 μm pinhole unit, the light transmittance was measured at a wavelength of 550 nm under the measurement conditions of an air temperature of 23°C and a humidity of 50%.

[0101] [Measurement method (thickness)] In the following examples and comparative examples, the thickness (film thickness) was measured using a three-dimensional surface roughness measuring device (Kosaka Laboratory Co., Ltd.) under an atmosphere of 23°C and 30% RH. This measuring device is a stylus type measuring device, and the film thickness and step can be measured by tracing the surface of the measurement sample with a needle. In the thickness measurement of the transparent layer (clear hard coat layer in the following examples and comparative examples. Hereinafter, it may be referred to as "clear HC" or "HC"), the measurement sample was attached to glass after the transparent layer forming process and the mask material removing process, and before the non-transparent layer (anti-glare layer in the following examples and comparative examples. Hereinafter, it may be referred to as "AG") forming process. Specifically, after peeling (removing) the mask material from the substrate, the HC part was traced from the substrate part, and the film thickness difference between the substrate surface and the clear HC part was measured. When measuring the HC thickness of a finished optical film (antiglare film in the following Examples and Comparative Examples), the cross section of the optical film can be observed with a SEM (Scanning Electron Microscope) to measure the HC thickness as well as the thicknesses of the substrate and AG. In the following Examples and Comparative Examples, the measurement conditions using the above-mentioned measuring device are as follows. Measurement speed: 500μm / s Stylus tip R: 0.5μmR Measurement pressure: 100μN

[0102] [Measurement method (water contact angle)] In the following Examples and Comparative Examples, the water contact angle of HC was measured as follows. That is, first, a water droplet of about 2.8 μL was dropped on the center of clear HC by the sessile drop method in an atmosphere of temperature 23° C. and humidity 30% RH using a water contact angle measuring device (trade name "DM700", manufactured by Kyowa Interface Science Co., Ltd.). Then, the angle formed by the tangent line of the end of the dropped water droplet and the adherend surface 1 second after the drop was measured and recorded as the "water contact angle (°)".

[0103] [Measurement method (transparency)] In the following examples and comparative examples, the transparency (clearness) of the HC was measured and evaluated as follows. That is, a laser microscope (product name "VK-X1000 / 1100", manufactured by Keyence Corporation) was used to observe a measurement sample under an atmosphere of 23°C temperature and 30% RH humidity, and the transparency (clearness) was evaluated. As the measurement sample, an anti-glare film after the non-transparent layer forming step was used. The measurement sample was observed using a 5x magnification lens, and a sample with no AG cured product (non-transparent part) of 500 μm or more in the HC part was marked as ◯, a sample with one or more AG cured products of 500 μm to 1 mm in size was marked as △, and a sample with an AG cured product of 1 mm or more in size was marked as ×.

[0104] [Example 1] The method for producing an optical film of the present invention was carried out as described below, and an optical film of the present invention was produced.

[0105] [1. Masking material coating process] A masking material (PET film, thickness 9 μm) in which a through hole for forming a transparent layer (circular, diameter 2.5 mm) was formed was attached to one side of a TAC substrate (product name "KC8UA", manufactured by Konica Minolta, Inc., thickness 80 μm). This masking material is a masking material in which a 5 μm thick adhesive layer is formed on one side of a 4 μm thick PET film. The thickness of this masking material (9 μm) is the combined thickness of the PET film and the adhesive layer. Since this masking material had a uniform thickness, the minimum thickness T2 (μm) of the masking material on the periphery of the through hole for forming a transparent layer is equal to the thickness (9 μm) of the entire masking material. If it is necessary to measure the minimum thickness T2 (μm) of the masking material, it can be measured using the above-mentioned three-dimensional surface roughness measuring instrument or SEM.

[0106] [2. Transparent layer formation process] The following components (1) to (4) were prepared and all mixed together to prepare a transparent layer forming liquid. The solids concentration of this transparent layer forming liquid (content of components other than the following solvent (4)) was 50 mass %. (1) 67 parts by mass of polyfunctional acrylate containing nanosilica (product name "NC035", manufactured by Arakawa Chemical Industries, Ltd.) (2) 33 parts by mass of multifunctional acrylate (product name "Binder A", manufactured by Arakawa Chemical Industries, Ltd.) (3) Antifouling agent (product name "KY-1203", manufactured by Shin-Etsu Chemical Co., Ltd.) 2 parts by weight (4) Dilution solvent: Butyl acetate

[0107] The transparent layer forming liquid obtained by mixing all of the components (1) to (4) was applied to the surface of the TAC substrate covered with the mask material (PET film) after the "1. Mask material covering step", and then dried in an oven at 60°C for 60 seconds to form a coating film. After that, ultraviolet light having a wavelength of 365 nm was irradiated to the coating film from a high-pressure mercury lamp at an integrated irradiation dose of 300 mJ / cm. 2 The coating film was cured by irradiating the coating film in the transparent layer-forming through-holes. This resulted in the coating film being cured to form a transparent layer (HC). The thickness of the center (thinnest part) of this HC layer was measured by the above-mentioned measuring method and was 7 μm.

[0108] [3. Masking material removal process] After the "2. Transparent layer forming process", the mask material (PET film) was peeled off together with the unnecessary layer (the cured dried coating film of the transparent layer forming liquid) formed thereon, and removed from the TAC substrate.

[0109] [4. Non-transparent layer formation process] The following components (11) to (17) were prepared and mixed to prepare a non-transparent layer forming liquid. The solid content of this non-transparent layer forming liquid (content of components other than the following solvent (17)) was 45 mass %. (11) Nanosilica-containing polyfunctional acrylate (product name "NC035", manufactured by Arakawa Chemical Industries, Ltd.) 67 parts by mass (12) Polyfunctional acrylate (product name "Binder A", manufactured by Arakawa Chemical Industries, Ltd.) 33 parts by mass (13) Polymethyl methacrylate particles (product name "Techpolymer", average particle size 3 μm, refractive index 1.525, manufactured by Sekisui Chemical Co., Ltd.) 10 parts by mass (14) Thixotropy imparting agent (trade name "Lucentite SAN", a synthetic smectite which is an organic clay, manufactured by Co-op Chemical Co., Ltd.) 1.5 parts by mass (15) Photopolymerization initiator (product name "OMNIRAD907", manufactured by BASF) 3 parts by mass (16) Leveling agent (product name "LE303", manufactured by Kyoeisha Chemical Co., Ltd.) 0.15 parts by mass (17) Diluent: Toluene

[0110] The non-transparent layer forming liquid obtained by mixing all of the components (11) to (17) was applied to the surface of the TAC substrate on which the transparent layer (HC) had been formed after the "3. Masking material removal step", and then dried in an oven at 60°C for 60 seconds to form a coating film. After that, the coating film was irradiated with ultraviolet light having a wavelength of 365 nm from a high-pressure mercury lamp at an integrated irradiation dose of 300 mJ / cm. 2The coating film was cured by irradiating the coating film so that the coating film was cured to form a non-transparent layer (AG). The total haze value of the non-transparent layer (AG) was measured and found to be 40%.

[0111] [Examples 2 to 14, Comparative Examples 1 to 4] Anti-glare films (optical films of the present invention) were produced in the same manner as in Example 1, except that the production conditions were changed as shown in Tables 1 to 3 below.

[0112] In the following Tables 1 to 3, the substrate is the same TAC substrate (thickness 80 μm) as in Example 1, and "KC8UA" is a product name of Konica Minolta, Inc., as described above.

[0113] In the following Tables 1 to 3, "HC antifouling agent" means the antifouling agent in the transparent layer (HC) forming liquid. As described above, the antifouling agent "KY-1203" in the following Tables 1 to 3 is the product name of Shin-Etsu Chemical Co., Ltd., and "LE-303" is the product name of Kyoeisha Chemical Co., Ltd. The composition of the transparent layer forming liquid in Examples 2 to 14 and Comparative Examples 1 to 4 was the same as that of Example 1, except that the antifouling agent in the table was used instead of "KY-1203" in Example 1 as the antifouling agent.

[0114] In Tables 1 to 3 below, "AG liquid" refers to a liquid for forming a non-transparent layer (AG). "With silica" in Tables 1 to 3 below means that a non-transparent layer forming liquid of the same composition as in Example 1 was used. "Without silica" means that a non-transparent layer forming liquid of the same composition as in Example 1 was used, except that 100 parts by mass of component (12) multifunctional acrylate was used instead of 67 parts by mass of component (11) nanosilica-containing multifunctional acrylate and 33 parts by mass of component (12) multifunctional acrylate in Example 1 (i.e., component (11) was not used but was replaced with the same mass of component (12)).

[0115] In the following Tables 1 to 3, "mask material thickness (T2)" refers to the thickness T2 (μm) of the mask material (PET film) used in each Example and Comparative Example. The mask materials used in each Example and Comparative Example all had a uniform thickness throughout. Therefore, the thickness of the entire mask material was considered to be equal to the minimum thickness T2 (μm) of the mask material on the periphery of the transparent layer-forming through hole.

[0116] In the following Tables 1 to 3, "HC center thickness (T1)" refers to the thickness T1 (μm) of the center (thinnest part) of the transparent layer (HC) measured by the above-mentioned measurement method.

[0117] In the following Tables 1 to 3, "HC water contact angle" represents the water contact angle of the transparent layer (HC) measured by the above-mentioned measurement method.

[0118] In Tables 1 to 3 below, "HC shape" represents the shape and dimensions of the transparent layer (HC). These shapes and dimensions are approximately equal to the shape and dimensions of the transparent layer-forming through-holes formed in the mask material. "○" represents that the transparent layer was circular. "□" represents that the transparent layer was square. "△" represents that the transparent layer was equilateral triangular. "Diameter" and the numerical value represent the major axis R1 (mm) of the transparent layer. "Side" and the numerical value represent the length (mm) of one side of the transparent layer. The length of one side of an equilateral triangle is equal to the major axis.

[0119] In the following Tables 1 to 3, "HC transparency evaluation" indicates the evaluation result of the transparency (clearness) of the transparent layer (HC) measured and evaluated by the above-mentioned measurement method, and "clear part transmittance" indicates the light transmittance of the transparent layer (HC) measured by the above-mentioned measurement method.

[0120] [Table 1]

[0121] [Table 2]

[0122] [Table 3]

[0123] As shown in Tables 1 to 3, in all of Examples 1 to 14, the ratio T2 / T1 of the minimum thickness T2 (μm) of the mask material at the periphery of the transparent layer-forming through hole to the thickness T1 (μm) of the thinnest part of the transparent layer was 3 or less. As a result, in all of Examples 1 to 14, the evaluation result of the transparency (clearness) of the transparent layer (HC) was ○ or △, and it was confirmed that the transparency was not impaired. In contrast, in all of Comparative Examples 1 to 4, the T2 / T1 was greater than 3. As a result, in all of Comparative Examples 1 to 4, the evaluation result of the transparency (clearness) of the transparent layer (HC) was ×, and the transparency was impaired. [Industrial Applicability]

[0124] As described above, according to the present invention, it is possible to provide a method for manufacturing an optical film, an optical film, an optical member, an image display device, a method for manufacturing an optical member, and a method for manufacturing an image display device that do not impair the transparency of a transparent layer. The present invention is suitable for use in, for example, an image display device having a camera hole, and can provide, for example, an image display device without impairing the image quality of a camera image. However, the present invention is not limited to this use and can be used in a wide range of uses. [Explanation of symbols]

[0125] 10 Optical Film 11 Base material 12 Non-transparent layer 12a Resin layer 12b particles 12d Non-transparent part 13 Transparent layer 13b Unnecessary layer 21 Masking material 21h Through hole for transparent layer formation

Claims

1. A method for producing an optical film having a non-transparent layer laminated on a substrate, comprising the steps of: the non-transparent layer has a through hole, and a transparent layer is formed in the through hole; The manufacturing method includes a mask material coating step, a transparent layer forming step, a mask material removing step, and a non-transparent layer forming step, In the mask material coating step, one surface of the base material is coated with a mask material having the transparent layer formation through hole formed therein; After the mask material coating step, in the transparent layer forming step, a transparent layer forming liquid is applied into the transparent layer forming through hole and solidified to form the transparent layer; After the transparent layer forming step, in the mask material removing step, the mask material is removed from the base material; After the mask material removing step, in the non-transparent layer forming step, a non-transparent layer forming liquid is applied onto the surface of the base material on which the transparent layer is formed to form the non-transparent layer; the transparent layer is a clear hard coat layer, A method for producing an optical film, wherein the thickness of the thinnest part of the transparent layer and the minimum thickness of the mask material on the outer periphery of the through hole for forming the transparent layer satisfy the relationship of the following mathematical formula (1). T2 / T1≦3(1) In the formula (1), T1 is the thickness (μm) of the thinnest portion of the transparent layer, and T2 is the minimum thickness (μm) of the mask material on the outer periphery of the transparent layer-forming through hole.

2. The method for producing an optical film according to claim 1 , wherein the transparent layer has a major axis R1 of 2.5 mm or more.

3. 3. The method for producing an optical film according to claim 1, wherein the transparent layer surface has a water contact angle of 85[deg.] or more.

4. The method for producing an optical film according to claim 1 , wherein the transparent layer has a thickness at its thinnest portion and a thickness at its thickest portion that satisfy the relationship of the following mathematical formula (2): H1 / T1≦3.5 (2) In the formula (2), T1 is the thickness (μm) of the thinnest part of the transparent layer, and H1 is the thickness (μm) of the thickest part of the transparent layer.

5. The method for producing an optical film according to claim 1 , wherein the transparent layer has a light transmittance of 80% or more at a wavelength of 550 nm.

6. The method for producing an optical film according to claim 1 , wherein the non-transparent layer has a light transmittance of less than 80% at a wavelength of 550 nm.

7. The method for producing an optical film according to claim 1 , wherein the non-transparent layer is an antiglare layer.

8. the substrate and the mask material are elongated, The method for producing an optical film according to claim 1 , wherein the mask material coating step, the transparent layer forming step, the mask material removing step, and the non-transparent layer forming step are continuously performed while the base material is being transported.

9. An optical film having a non-transparent layer laminated on a substrate, the non-transparent layer has a through hole, and a transparent layer is formed in the through hole; the transparent layer is a clear hard coat layer, the non-transparent layer is formed on the transparent layer-forming surface of the base material, The major axis R1 of the transparent layer is 2.5 mm or more, An optical film, wherein the transparent layer has a water contact angle of 85° or more on its surface.

10. An optical member comprising the optical film according to claim 9.

11. The optical member according to claim 10, which is a polarizing plate.

12. An image display device comprising the optical film according to claim 9 or the optical member according to claim 10 or 11.

13. A method for producing the optical member according to claim 10 or 11, comprising the step of producing the optical film according to claim 9 by the method according to any one of claims 1 to 8.

14. A method for producing an image display device according to claim 12, comprising the step of producing the optical film according to claim 9 by the method according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Method of manufacturing microlens array, method of manufacturing microlens and method of manufacturing display device

    JP2007206601A

  • Lens array

    JP2008040455A

  • Antiglare and Anti-newton film

    JP2009109683A

  • Light guide, light guide appratus, light guide system and method of manufacturing the same