Intermediate liner for roll-bonded brazing sheets
By using an intermediate liner with optimized compositions of Si, Mn, and Zn, the multilayer braze sheets achieve enhanced bonding and corrosion resistance, addressing bonding and corrosion issues in corrosive environments.
Patent Information
- Application Number
- JP2021562360
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-04-24
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2039-04-24
AI Technical Summary
Existing multilayer braze sheets face challenges in bonding due to significant differences in flow stress between layers, leading to issues like delamination and corrosion, particularly in corrosive environments, and existing intermediate liners fail to provide adequate corrosion resistance while maintaining bondability.
Incorporating an intermediate liner with specific compositions of Si, Mn, Mg, and Zn, along with controlled flow stress adjustments, to enhance bonding and corrosion resistance, using aluminum alloys with 2XXX, 3XXX, 5XXX, or 6XXX as the core, 4XXX as the braze liner, and an intermediate liner with optimized elemental additions.
The solution improves roll bondability and maintains corrosion resistance, reducing liquid film migration and delamination, ensuring the multilayer sheets perform well in corrosive conditions.
Smart Images

Figure 0007587522000005 
Figure 0007587522000006 
Figure 0007587522000007
Abstract
Description
[Technical field]
[0001] The present invention relates to brazing sheet material, heat exchangers and methods for making the same, and more particularly to a multi-layer aluminum alloy brazing sheet formed by roll bonding. [Background technology]
[0002] For example, roll-bonded multi-layer brazing sheet materials are known in which multiple layers of different aluminum alloys to form a core, brazing liner, and intermediate liner are stacked and passed through a rolling mill. Typically, the stack of layers is preheated and the rolling mill exerts high pressure on the stack, reducing the cumulative thickness of the stack as well as the thickness of the individual layers. The rolling process and thickness reduction also bond the individual layers together, reducing the thickness of the single composite sheet with multiple layers. Intermediate liners / intermediate liner layers can be used in the multi-layer brazing sheet to reduce element migration between the core and brazing liner during brazing, for example, which leads to reduced corrosion resistance. In low pH environments such as EGR (exhaust gas recirculation)-related CAC (charge air cooler), the core material can be easily susceptible to corrosion, such as intergranular corrosion, without the protection of the intermediate liner. Known intermediate liners, such as alloy 0140 or AA1145 available from Arconic, Inc. of Pittsburgh, Pa., USA, can present difficulties in bonding to adjacent layers when roll bonded to form a laminate. Notwithstanding known methods, materials, and apparatus, alternative methods, apparatus, and materials for making multi-layer roll bonded brazed heating elements remain desirable. Summary of the Invention
[0003] The disclosed subject matter relates to a multi-layer sheet material having a core of one of a 2XXX, 3XXX, 5XXX, or 6XXX aluminum alloys, a brazed liner of a 4XXX aluminum alloy, and an intermediate liner, the intermediate liner having a composition by weight including 0.31-1.0 Si, <0.1 Mg, 0.25-1.0 Mn, max 5.0 Zn, max 0.3 Fe, max 0.2 Cu, max 0.125 Zr, other elements each ≦0.05 wt% and total ≦0.15 wt%, balance Al.
[0004] In another embodiment, the intermediate liner contains 0.34-0.5 wt.% Si, <0.05 wt.% Mg and 0.25-0.35 wt.% Mn, ≦0.05 wt.% Zn, ≦0.3 wt.% Fe, and ≦0.05 wt.% Cu.
[0005] In another embodiment, an intermediate liner is disposed between the braze liner and the core.
[0006] In another embodiment, the intermediate liner contains 0.4-0.5 wt. % Si.
[0007] In another embodiment, the intermediate liner contains 0.25 to 0.34 wt. % Mn.
[0008] In another embodiment, the intermediate liner further comprises 0.05 to 5.0 wt. % Zn.
[0009] In another embodiment, the increase in flow stress in the intermediate liner due to the presence of at least one of Mg and Mn is in the range of 20% to 52% relative to the flow stress in the intermediate liner without the presence of at least one of Mg and Mn.
[0010] In another embodiment, the core is a 3003 aluminum alloy.
[0011] In another embodiment, the core comprises 0.1-1.0 wt.% Si, up to 0.5 wt.% Fe, 0.2-1.0 wt.% Cu, 1.0-1.5 wt.% Mn, 0.2-0.3 wt.% Mg, up to 0.05 wt.% Zn, and 0.1-0.2 wt.% Ti.
[0012] In another embodiment, the braze liner comprises 6.8-8.2 wt.% Si, max. 0.8 wt.% Fe, max. 0.25 wt.% Cu, max. 0.1 wt.% Mn, and max. 0.2 wt.% Zn.
[0013] Another embodiment further includes another liner disposed on the core distal to the intermediate liner and the brazed liner.
[0014] In another embodiment, the other liner includes a second braze liner and a second intermediate liner, the second intermediate liner being disposed between the core and the second braze liner.
[0015] In another embodiment, the intermediate liner contains 0.34-0.5 wt.% Si, max. 0.1 wt.% Zn, max. 0.3 wt.% Fe, max. 0.2 wt.% Cu, balance Al, and further includes other elements each <0.05 wt.% totaling 0.15 wt.%.
[0016] In another embodiment, the intermediate liner contains <0.05 wt.% Cu and further comprises up to 0.125 wt.% Zr.
[0017] In another embodiment, the sheet material has a total thickness of 0.1 mm to 3.0 mm, including a core thickness of 0.09 mm to 2.85 mm, the brazed liner has a clad ratio of 2.5% to 20%, and the intermediate liner has a clad ratio of 2.5% to 20%.
[0018] In another embodiment, the sheet material is O temper.
[0019] In another embodiment, the heat exchanger comprises:Sheet material included Tubes, fins, header plates, and Is % Mg, 0.25-1.0 wt. % Mn, ≦0.05 wt. % each and a total of ≦0.15 wt. % other elements, balance Al.
[0020] In another embodiment, the multi-layer sheet material has a core of one of a 2XXX, 3XXX, 5XXX, or 6XXX aluminum alloys, a brazed liner of a 4XXX aluminum alloy, and an intermediate liner, the intermediate liner having a composition by weight of 0.31-1.0 Si, 0.1-0.5 Mg, 0.05-0.3 Mn, up to 5.0 Zn, each ≦0.05 wt.% and totaling ≦0.15 wt.% other elements, balance Al.
[0021] In another embodiment, the intermediate liner contains 0.05 to 5.0 wt. % Zn.
[0022] In another embodiment, a method for making a brazing sheet comprises: % Si, <0.1 wt. % Mg, 0.25-1.0 wt. % Mn; providing a layer of core material selected from one of a 2XXX, 3XXX, 5XXX, or 6XXX aluminum alloy; providing a layer of brazing liner material of a 4XXX aluminum alloy; stacking the layer of intermediate liner, the layer of core material, and the layer of brazing liner material into a stack, the intermediate liner being disposed between the layer of core material and the layer of brazing liner material; and rolling the stack to form a joined multi-layer brazing sheet. [Brief description of the drawings]
[0023] For a more complete understanding of the present disclosure, reference is made to the following detailed description of exemplary embodiments taken in conjunction with the accompanying drawings.
[0024] [Figure 1] FIG. 2 is a diagram of a brazing sheet according to one embodiment of the present disclosure. [Diagram 2] FIG. 2 is a diagram of a brazing sheet according to another embodiment of the present disclosure. [Diagram 3] 1 is a graph of stress versus strain for several materials. [Figure 4] 1 is a graph of flow stress versus strain rate for several materials. [Diagram 5] 1 is a set of microstructural images of multiple post-braze multi-layer materials that were not pre-strained. [Figure 6] 1 is a set of microstructural images of a multi-layer material after multiple brazing subjected to pre-strain. [Figure 7] 1 is a graph of corrosion depth for several materials in response to a corrosion test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] One aspect of the present disclosure is the recognition that brazing sheets have several objectives, such as light weight, high strength, and corrosion resistance, and that these attributes are often in conflict. For example, the use of 3XXX aluminum alloys in the core layer of the brazing sheet contributes to the overall strength of the sheet material after brazing, while a typical 4XXX brazing liner causes severe liquid film migration (LFM) during brazing, resulting in reduced corrosion resistance. This is especially true for O-temper brazing sheets (or brazing sheets) using 3XXX cores and 4XXX brazing liners (also known as brazing layers). Intermediate liners (also known as interlayer or intermediate liner layers) made from high purity aluminum alloys such as Arconic alloys 0140 and AA1145 can be used as protective layers to provide improved corrosion resistance, but such intermediate liner materials sometimes result in roll bond defects and delamination (blistering) of all or part of the core and brazing layer at the intermediate liner interface.
[0026] One aspect of the present disclosure is the recognition that high purity intermediate liner alloys are soft, particularly relative to core alloys of the 2XXX, 3XXX, 5XXX, and 6XXX alloy series, such as 3003 aluminum alloy, and / or 4XXX brazing alloys, such as 4047, 4045, 4343, 4147, 4004, 4104 alloys, and derivatives of these alloys with zinc additions. Typical rolling temperatures for multi-layer brazed products range from 700 to 1000°F and can vary based on the specific manufacturing process and materials being rolled. During rolling in this temperature range, the large difference in flow stress of these alloys can cause the materials to deform distinctly, which presents a challenge to forming a bonded product. The flow stress of these layers at the rolling temperature defines their mechanical behavior and is related to rolling behavior and bondability.
[0027] One aspect of the present disclosure is the recognition that a smaller difference in flow stress of various layers of a roll-bonded multi-layer sheet, e.g., an intermediate liner relative to a core and / or brazed liner, may result in better bonding between the multiple layers, and that the bond produced by roll-bonding the multi-layer sheet is easier when the flow stress of the layers of the multi-layer roll-bonded sheet is closer in value. The term "bondability" can be used to refer to the property of adjacent layers that are bonded together by roll-bonding. For example, adjacent sheets with higher bondability will bond more easily and / or better to each other when roll-bonded, compared to adjacent sheets with lower bondability.
[0028] One aspect of the present application is the recognition that the flow stress of a relatively soft layer in a multi-layer roll-bonded brazing sheet can be adjusted by adding elements that strengthen the soft layer to more closely approach the flow stress of the other layers to which it is joined, and that this hardness adjustment will improve the bondability of the previously softer layers.
[0029] One aspect of the present disclosure is the recognition that strengthening the soft layers in a multi-layer roll-bonded brazing sheet results in an increase in flow stress. Furthermore, the roll-bonding is facilitated when adjacent layers have flow stress values close to each other. For example, Arconic alloy 0140 (Table 2, IL0For an intermediate liner layer made from 0.01, 0.1, and 1 / sec strain rates, respectively, at 900°F, the alloy can be observed to have flow stresses of 1.25, 1.91, and 3.15 ksi (see Table 4 below). In comparison, the flow stresses of 3XXX core alloys, such as 3003, have flow stresses of 2.09, 3.19, and 5.16 ksi (see Table 4 below) at strain rates of 0.01, 0.1, and 1 / sec, respectively, and 4XXX braze liners, such as 4343, have flow stresses of 1.7, 2.62, and 4.55 ksi (see Table 4 below) at strain rates of 0.01, 0.1, and 1 / sec. By adding 0.2-0.3 wt. % Mn to 0140 aluminum alloys (IL4, IL5, and IL6 in Table 2), the flow stresses are increased to 1.0, 1.0, and 1.0 ksi (see Table 4 below) at strain rates of 0.01, 0.1, and 1 / sec. In IL4, 1.72, 2.35, and 3.78ksi respectively , in IL6, 1.9, 2.6, and 3.87 ksi, representing an increase in flow stress of 20% to 52%. Further additions of 0.1 to 0.4 wt.% Mg to the 0140 aluminum alloys (IL7, IL8, and IL10 alloys in Table 4) can increase the flow stress of the resulting alloys to higher levels. A good roll bond to multiple aluminum alloy layers requires that all surface aluminum oxides be simultaneously broken down so that the aluminum underneath can be metallurgically bonded. When a softer intermediate liner is used to create a multi-layer material, it can be deformed more easily, but both the harder braze liner and core alloys have a relatively low amount of deformation. The lower deformation of the braze liner and core is less effective at breaking down surface oxides, making the formation of a good metallurgical bond with the intermediate liner more difficult. According to the present disclosure, a smaller flow stress difference between the layers is preferred to promote good bonding. A closer match of flow stresses between the intermediate liner and the braze liner is beneficial for the roll bond and helps prevent blistering that is often seen between the braze liner and intermediate liner alloys in multi-layer brazing sheets.
[0030] Figure 1 shows a brazing sheet material 10 including an aluminum alloy core 12 of a 3XXX series aluminum alloy, e.g., Core B alloy, Arconic alloy 0359, in Table 1 below, with the compositions shown. In one embodiment, the core has a composition of ≦0.2 wt.% Si, ≦0.35 wt.% Fe, 0.4-0.6 wt.% Cu, 1.0-1.3 wt.% Mn, 0.2-0.3 wt.% Mg, ≦0.05 wt.% Zn, 0.1-0.2 wt.% Ti, with the balance being Al and unavoidable impurities. The brazing sheet 10 of Figure 1 includes a brazing liner (layer) 14 having a base composition of a 4XXX (4000) series aluminum alloy, e.g., 4343. In one embodiment, the brazing liner 14 has a composition of 6.8-8.2 wt.% Si, ≦0.8 wt.% Fe, ≦0.25 wt.% Cu, ≦0.1 wt.% Mn, ≦0.2 wt.% Zn, with the balance being Al and unavoidable impurities. The intermediate liner (intermediate liner layer) 16 is located between the core 12 and the brazing liner 14. In one embodiment, the intermediate liner 16 (IL0,0140 in Table 2) has a composition of 0.34-0.5 wt.% Si, <0.3 wt.% Fe, <0.05 wt.% Cu, <0.1 wt.% Mn and <0.05 wt.% Mg, <0.1 wt.% Zn. This may be described as a modified 1XXX series aluminum alloy in view of the presence of Mn and / or Mg in the intermediate liner 16. In one embodiment, the 0140 aluminum alloy can be modified by adding up to 0.10-0.30 wt% Mn, or 0.10-0.40 wt% Mg, either alternatively or in combination. Additions up to 0.2 wt% Cu, and up to 0.125 wt% Zr have also been investigated for their strengthening effect. In another embodiment, the intermediate liner has 0.31-1.0 wt% Si, up to 0.1 wt% Mg, and 0.25-1.0 wt% Mn.
[0031] The brazing sheet material 10 has a thickness range of 0.1-3mm, the core has a thickness of 0.1-2.85mm, the brazing liner has a thickness of 0.005-0.6mm, or a clad ratio of 2.5-20%, and the intermediate liner has a thickness of 0.005-0.6mm (clad ratio of 2.5-20%).
[0032] FIG. 2 shows a multi-layer (four or five layer) brazing sheet 20 having a brazing liner 64, an intermediate liner 66, a core 62, another brazing liner 68, and another intermediate liner 70. The brazing liners 64 and 68 may be made of 4XXX series aluminum alloys, such as 4343, 4045, and 4047 alloys. The core 62 may be made of 2XXX, 3XXX, and 6XXX alloys, such as 3003 alloy. As mentioned above, the intermediate liners 66 and 70 may be made of high purity aluminum alloys, including an amount of Mn and / or Mg. The brazing liner 64 may typically be used to form the outer surface of the structure formed from the brazing sheet 20, interposed between the intermediate liner 66 and the outer environment O. The intermediate liner 70 may be used to interpose between the core 62 and the inner environment I of the structure formed from the brazing sheet 20, in the absence of the optional additional brazing liner 68. When present, the braze liner 68 will form the inner surface of the structure interposed between the intermediate liner 70 and the internal environment I. Amounts of 0.25-1.0 wt.% or 0.25-0.35 wt.% Mn in the intermediate liners 66, 70 have shown dramatic increases in flow stress at rolling temperatures. The addition of 0.2 wt.% Mn also shows an effective increase in flow stress compared to high purity intermediate liners such as intermediate liner alloy IL0 (Table 2 below). In another embodiment, Si may be present in an amount of 0.4-0.5 wt.%.
[0033] In another embodiment, small amounts, i.e., 0.10-0.5 wt.% Mg, with or potentially without 0.05-0.3 wt.% Mn, may provide similar beneficial effects as the presence of 0.25-1.0 wt.% Mn, as discussed above.
[0034] In another embodiment, additions of up to 5 wt. % zinc may be added to the interliner alloys in accordance with the present disclosure to aid in corrosion resistance without changing the flow stress and LFM behavior of the braze liner and interliner alloys herein. In one example, the internal environment I may be exhaust gas from an internal combustion engine and the external environment O may be air or a coolant.
[0035] One aspect of the present disclosure is the recognition that when an intermediate liner is used in brazing sheets containing high strength aluminum alloys such as the 3XXX series alloys, the intermediate liner tends to experience significant liquid film migration (LFM) during brazing, which can adversely affect corrosion resistance. This is especially true for O-temper materials. Brazing sheets are often supplied in O-temper, i.e., after being fully annealed. O-temper brazing sheets exhibit good formability, allowing the sheets to be formed into the required shapes required to make components such as EGR-type CAC (charge air cooler) and heat exchanger parts, e.g., tubes, end plates, manifolds, collector tanks, etc. It is important to maintain the corrosion protection function of the intermediate liner when components made of these multi-layer materials are exposed to corrosive environments. By forming multi-layer sheet materials, where O-temper is preferred, the forming process may create residual strain in the material within the formed shape. It is known that multi-layer brazing sheets including 3XXX interliners with low residual strain (i.e., <10%) in O temper can experience severe LFM during brazing by reacting with the braze filler material. For this reason, high purity interliner alloys, such as 0140, are preferred as they recrystallize early during the brazing cycle and can prevent LFM. An aspect of the present disclosure is the identification of strengthening elements and their concentration limits to achieve higher flow stress for improved roll bonding and also much less impact of LFM on corrosion resistance than, for example, 3XXX alloy interliners. A further aspect of the present disclosure is to achieve improved roll bondability while minimizing LFM without reducing corrosion resistance. The interliner 16 according to the present disclosure promotes roll bonding through the brazing liner 14 while retaining good resistance to LFM, corrosion resistance, and brazeability. If the midliner 16 contains strengthening elements such as Mn greater than 0.34 wt. % and experiences a small amount of distortion from the forming process prior to brazing, LFM can change the microstructure and chemical composition of the midliner layer.This is generally not favorable for brazed heat exchangers or other components and is exemplified by IL8 shown in FIG. 6, which exhibited severe LFM.
[0036] The brazing sheet material 10 shown in Figure 1 may be particularly suitable as a material used to make heat exchangers used in corrosive environments, such as EGR-type CACs and evaporator heat exchangers. In these applications, the brazing sheet material must be corrosion resistant to withstand exposure to applicable internal and external fluids, such as air, coolants, and exhaust gases, without corrosion over a commercially acceptable period of normal use. Additionally, the resulting heat exchanger HE must be strong and lightweight.
[0037] <Manufacturing method - composition> Various examples of cores, mid-liners, and braze liners having various compositions were prepared. The compositions of the core alloys are shown in Table 1, the compositions of the mid-liners in Table 2, and the compositions of the braze liners in Table 3. The alloys identified as "0359" (Table 1) and "0611" (Table 2) are alloys sold by Arconic, Inc., Pittsburgh, Pennsylvania, USA. [Table 1] [Table 2] [Table 3]
[0038] In each of the core, braze liner, and intermediate liner compositions disclosed herein, the composition is an aluminum alloy, expressed in weight percent of each, with aluminum and impurities listed as the balance of the composition, i.e., each being ≦0.05 and totaling ≦0.15 weight percent. The composition ranges of elements are as expressed literally herein, including all intermediate values. For example, in the above composition, Mn in the range of 0.1-0.3 weight percent includes 0.01, 0.02, 0.03, 0.04..., 0.28, 0.29, and 0.30 weight percent, and all intermediate values such as 0.11, 0.24 weight percent, etc., in increments of 0.01 weight percent.
[0039] Mechanical and thermal methods used in the preparation of the brazing sheet Fabrication experiments include, but are not limited to, casting ingots of high strength core alloy, 4XXX braze liner alloy, and intermediate liner alloy in a three-layer structure as shown in FIG. 1. In some embodiments, the intermediate liner ingot may be subjected to preheating or homogenization at a temperature ranging from 450°C to 550°C for a soak time of up to 24 hours before rolling into the intermediate liner layer. The high strength core ingot may also be subjected to a similar heat treatment. In some embodiments, the ingot is not subjected to heat treatment before rolling. In some embodiments, the high strength core ingot is not subjected to heat treatment before hot rolling. The three-layer braze sheet has a braze liner, an intermediate liner, and a core. The braze liner and the intermediate liner may each contribute 5-30% of the total thickness of the sheet.
[0040] In some embodiments, the stackup / composite consists of three layers that are subjected to a hot rolling reheat process. The hot rolling temperature ranges from 400°C to 520°C.
[0041] In some embodiments, the resulting multi-layered composite is cold rolled to an intermediate gauge and then passes through an intermediate anneal at a temperature ranging from 340°C to 420°C for a soak time of up to 8 hours. After the intermediate anneal, the composite is cold rolled again to a light or final gauge of 0.1 to 3 mm. In some embodiments, the material may be subjected to two or more intermediate anneals, then rolled to a light gauge and then subjected to another intermediate anneal. In some embodiments, at the final gauge, the material is subjected to a final partial or full anneal at a temperature ranging from 150°C to 420°C for a soak time of up to 8 hours.
[0042] In some embodiments, the composite is cold rolled directly to final gauge without an intermediate anneal and then subjected to a final partial anneal or full anneal at a temperature ranging from 150° C. to 420° C. for a soak time of up to 8 hours.
[0043] <Experimental Results> A series of experimental intermediate liner alloys (listed in Table 2) were cast into ingots with dimensions 14" x 10" x 2" with the addition of strengthening elements such as Mn, Mg, Cu, and Zr. Cylindrical coupons (10 mm diameter and 15 mm length) were prepared from the ingot material after preheat treatment. These coupons were measured for flow stress at these representative rolling temperatures. The core alloy, braze liner 4343, and baseline high purity intermediate liner (IL0) were also measured for comparison. The compositions of the core alloy and braze liner are listed in Tables 1 and 3 above, respectively. According to one embodiment of the present disclosure, the smaller difference in flow stress at rolling temperature between these layers facilitates roll bonding, especially for the soft intermediate liner layer. Flow stress testing was performed using a Gleeble thermo-mechanical simulator. Testing was performed at a temperature of 900°F (482°C), which is representative of the rolling temperature range of the multi-layer brazing sheet (400-520°C). Three strain rates were applied for flow stress measurements: 0.01, 0.1, and 1 / sec. These strain rates were selected to cover a wide range of typical reductions for brazing sheet rolling operations. Table 4 below lists the flow stress of relevant alloys at 900°F measured at strain rates of 0.01, 0.1, and 1 / sec, respectively. The flow stress values at each strain rate were calculated by averaging the values of true strains between 0.2 and 0.7 from compression tests using a Gleeble thermomechanical simulator. [Table 4]
[0044] The results recorded in Table 4 are shown in Figure 3, which shows the flow stress curves for the alloys tested at 900°F and a strain rate of 1 / sec, with the flow stress averaged over strain values of 0.2 to 0.7.
[0045] FIG. 4 shows the flow stress of the alloys tested at strain rates of 0.01, 0.1, and 1 / sec at 900°F. The flow stress is averaged by the 0.2-0.7 strain values from the tests shown in FIG. 3. The flow stress of the intermediate liner alloys according to the present disclosure at lower strain rates such as 0.01 / sec and 0.1 / sec is similar to the flow stress of brazing liner alloy 4343, which promotes good bonding in slow reduction processes such as those used for roll bonding of multi-layer brazing sheets. Higher strain rates are often used to reduce the thickness of the stackup at later stages of the rolling process after bonding has already been completed. Reduce Applies.
[0046] During roll bonding, IL0 High purity intermediate liners such as (0140 alloy) deform more easily compared to braze layers such as 4343 (alloy B) and core alloys such as 3003 / 0359 (core alloys A and B), which can often cause delamination, blistering, and bowing of the multi-layer ingot / plate assembly. IL0 The measured flow stresses of the IL4 (0.2Mn), IL6 (0.3Mn), IL7 (0.1Mn 0.1Mg 0.125Zr), IL8 alloys (0.2Mn 0.2Cu 0.15Mg), and IL10 (0.4Mg) alloys are shown in Figure 3 along with some other materials for comparison. A summary of the flow stress values for all experimental alloys is shown in Table 4. The intermediate liners IL4 (0.2Mn), IL6 (0.3Mn), IL7 (0.1Mn 0.1Mg 0.125Zr), IL8 alloys (0.2Mn 0.2Cu 0.15Mg), and IL10 (0.4Mg) are shown in Figure 3. IL0 According to one embodiment of the present disclosure, the intermediate liner containing additional strengthening elements exhibits increased flow stress and improved roll bondability. It is believed that the highest flow stress of the intermediate liner alloy mentioned above provides the best performance for roll bonding. However, according to the present disclosure, the LFM phenomenon associated with the higher content of strengthening elements is also considered, as shown by the evaluation of corrosion in the tests described below.
[0047] Figures 5 and 6 show the microstructures of the multilayer material with no prestrain and with 4% prestrain, respectively, after a typical CAB brazing cycle. The brazing cycle includes heating at 35°C / min to 577°C, then heating at 12°C / min to 600°C with a 2 minute step at 600°C. Cooling then occurred in a furnace at about -125°C / min to 250°C, then air cooled. In Figure 6, the top and bottom of the mid-liner are indicated by double arrows. As shown in Figure 5, all mid-liner alloys without prestrain before brazing were fully recrystallized during the brazing cycle and no LFM was observed. At 4% prestrain, LFM can be observed in some experimental materials with various levels of severity in Figure 6. IL0 Intermediate liner alloys IL10 and IL10 did not exhibit LFM because the material was fully recrystallized to prevent LFM from occurring. IL10 had a 0.4Mg content, which may increase flow stress due to simple roll bonding. Alloys IL4, IL6, and IL7 (with 0.2Mn, 0.3Mn, and 0.1Mn, 0.1Mg, 0.125Zr, respectively) exhibited LFM, but it was mainly limited to less than 50% of the original thickness of the intermediate liner IL. The more highly alloyed IL8 exhibited more severe LFM, which affected nearly the entire IL layer. It is important to maintain the corrosion protection function of the intermediate liner when components made of these materials are exposed to corrosive environments. From this perspective, higher alloy contents such as IL8 are not preferred. One aspect of the present disclosure is the recognition that there is a limit to the strengthening elements that can be added to intermediate liner alloys such as 0140 to increase flow stress while maintaining a limited effect of LFM. The selection criterion for the intermediate liner alloys of the present disclosure is corrosion resistance.
[0048] The corrosion test used to evaluate the interliner alloys in Table 2 used a solution that was a mixture of sulfuric, nitric, formic, and acetic acids with a pH of 2.4 and 50 mg / L sodium chloride. The solution was to simulate an exhaust gas recirculation (EGR) type environment. For this test method, alternating dry (16 hours in air) and wet (8 hours in solution) cycles were used, with aeration applied to the solution during the wet cycle to accelerate corrosion.
[0049] Figure 7 shows the measurement of corrosion pit count and depth after 60 days of testing using this method. All materials were treated with 4% pre-strain prior to the brazing cycle to simulate significant LFM conditions. The corrosion depth shown in Figure 7 was measured from the top location of the intermediate liner (just below the brazed liner) to the deepest location of any corrosion site. IL4, 6, and 7 all show similar corrosion resistance compared to IL0 and IL10, both of which did not have any LFM effects. IL8, which showed the most significant LFM, showed deteriorated corrosion resistance. The results show that the optimized composition increased the flow stress and also maintained excellent corrosion resistance, as well as the high purity intermediate liner ( IL0 It has been demonstrated that it is possible to provide
[0050] As shown in FIG. 1, the multi-layer brazing sheet includes a layer of brazing liner, an intermediate liner alloy, and a core alloy. The brazing liner can be made of 4XXX series aluminum alloys, such as 4343, 4045, and 4047 alloys. The core alloy can be made of 2XXX, 3XXX, and 6XXX alloys, such as 3003 alloy. As mentioned above, the intermediate liner alloy can be made of high purity aluminum alloys with optimal amounts of Mn and / or Mg. Experiments have shown that addition of up to 0.4 wt.% of 0.15 wt.% Mg, with or without a small amount of Mn, can be made to the same effect as 0.3 wt.% Mn. Up to 5 wt.% zinc can be added to these alloys for potential corrosion resistance improvement, since up to 5 wt.% zinc does not change the flow stress and LFM behavior of the brazing liner and intermediate liner alloys herein.
[0051] This disclosure utilizes standard abbreviations for elements that appear in the Periodic Table of the Elements, e.g., Mg (magnesium), O (oxygen), Si (silicon), Al (aluminum), Bi (bismuth), Fe (iron), Zn (zinc), Cu (copper), Mn (manganese), Ti (titanium), Zr (zirconium), F (fluorine), K (potassium), Cs (cesium).
[0052] The figures constitute a part of this specification, include exemplary embodiments of the present disclosure, and illustrate various objects and their features. In addition, any measurements, specifications, etc. shown in the figures are intended to be illustrative and not limiting. Thus, specific structural and functional details disclosed herein should not be construed as limiting, but merely as a representative basis for teaching those skilled in the art how to use the present invention in various ways.
[0053] Detailed embodiments of the invention are disclosed herein; however, it should be understood that the disclosed embodiments are merely illustrative of the invention, which may be embodied in various forms. Moreover, the examples given in connection with the various embodiments of the invention are intended to be illustrative and not limiting.
[0054] Throughout the specification and claims, the following terms shall take the meanings expressly associated therewith, unless the context clearly dictates otherwise. As used herein, the phrases "in one embodiment" and "in some embodiments" do not necessarily refer to the same embodiment, but may. Additionally, as used herein, the phrases "in another embodiment" and "in some other embodiments" do not necessarily refer to different embodiments, but may. Thus, as described below, various embodiments of the present invention may be readily combined without departing from the scope and spirit of the subject matter of the present invention.
[0055] Additionally, as used herein, the term "or" is an inclusive "or" and is equivalent to "and / or" unless the context clearly dictates otherwise. The term "based on" is not exclusive and may be based on additional unstated factors unless the context clearly dictates otherwise. Additionally, throughout this specification, the meanings of "a," "an," and "the" include plural references. The meaning of "in" includes "in" and "on."
[0056] Aspects of the present invention will now be described with reference to the following numbered clauses.
[0057] 1. A multi-layer sheet material comprising: an aluminum alloy core of one of the following aluminum alloys: 2XXX, 3XXX, 5XXX, or 6XXX; A brazed liner made of 4XXX aluminum alloy; and an intermediate liner, the intermediate liner comprising: 0.31 to 1.0 wt% Si; <0.1 wt.% Mg; 0.25 to 1.0 wt.% Mn; Zn up to 5.0 wt.%; Fe up to 0.3 wt.%; up to 0.125 wt.% Zr; % each and in the sum of ≦0.15 wt.% other elements, the balance being Al.
[0058] 2. Intermediate liner 0.34 to 0.5 wt.% Si; <0.05 wt.% Mg; 0.25 to 0.35 wt.% Mn; ≦0.05 wt.% Zn; ≦0.05 wt.% Cu.
[0059] 3. The sheet material of clause 1 or 2, wherein an intermediate liner is disposed between the brazed liner and the core.
[0060] 4. The sheet material according to claim 2 or 3, wherein the intermediate liner contains 0.4 to 0.5 wt. % Si.
[0061] 5. The sheet material according to any one of clauses 2 to 4, wherein the intermediate liner contains 0.25 to 0.34 wt. % Mn.
[0062] 6. The sheet material of any one of clauses 1 to 5, wherein the intermediate liner further comprises 0.05 to 5.0 wt.% Zn.
[0063] 7. The sheet material of any one of clauses 1 to 6, wherein the increase in flow stress in the intermediate liner due to the presence of at least one of Mg and Mn is in the range of 20% to 52% relative to the flow stress in the intermediate liner without the presence of at least one of Mg and Mn.
[0064] 8. The sheet material of any one of clauses 1 to 7, wherein the core is a 3003 aluminum alloy.
[0065] 9. The sheet material of any one of clauses 1 to 7, wherein the core comprises 0.1-1.0 wt.% Si, maximum 0.5 wt.% Fe, 0.2-1.0 wt.% Cu, 1.0-1.5 wt.% Mn, 0.2-0.3 wt.% Mg, maximum 0.05 wt.% Zn, and 0.1-0.2 wt.% Ti.
[0066] 10. The sheet material of any one of clauses 1-9, wherein the braze liner comprises 6.8-8.2 wt.% Si, max. 0.8 wt.% Fe, max. 0.25 wt.% Cu, max. 0.1 wt.% Mn, and max. 0.2 wt.% Zn.
[0067] 11. The sheet material of any one of clauses 1-10, further comprising another liner disposed on the core distal to the intermediate liner and the brazed liner.
[0068] 12. The sheet material of claim 11, wherein the other liner includes a second brazed liner and a second intermediate liner, the second intermediate liner being disposed between the core and the second brazed liner.
[0069] 13. The sheet material according to clause 1, wherein the intermediate liner contains 0.34-0.5 wt.% Si and up to 0.1 wt.% Zn.
[0070] 14. The sheet material of clause 13, wherein the intermediate liner contains <0.05 wt.% Cu.
[0071] 15. The sheet material of any one of clauses 1 to 14, wherein the sheet material has a total thickness of 0.1 mm to 3.0 mm, including a core thickness of 0.09 mm to 2.85 mm, the brazed liner has a clad ratio of 2.5% to 20%, and the intermediate liner has a clad ratio of 2.5% to 20%.
[0072] 16. The sheet material according to any one of clauses 1 to 15, wherein the sheet material is O temper.
[0073] 17. The sheet material according to any one of claims 1 to 16 is included.Tubes, fins, header plates, and Is at least one of the heat exchangers.
[0074] 18. A multi-layer sheet material comprising: an aluminum alloy core of one of the following aluminum alloys: 2XXX, 3XXX, 5XXX, or 6XXX; A brazed liner made of 4XXX aluminum alloy; and an intermediate liner, the intermediate liner comprising: 0.31 to 1.0 wt% Si; 0.1 to 0.5 wt.% Mg; 0.05 to 0.3 wt.% Mn; Zn up to 5.0 wt.%; % each and in the sum of ≦0.15 wt.% other elements, the balance being Al.
[0075] 19. The sheet material according to claim 18, wherein the intermediate liner contains 0.05 to 5.0 wt. % Zn.
[0076] 20. A method for making a brazing sheet, comprising: providing an interliner layer, the interliner layer comprising: 0.31-1.0 wt.% Si, <0.1 wt.% Mg, 0.25-1.0 wt.% Mn; providing a layer of core material selected from one of a 2XXX, 3XXX, 5XXX, or 6XXX aluminum alloy; providing a layer of a braze liner material of a 4XXX aluminum alloy; stacking a layer of an intermediate liner, a layer of core material, and a layer of brazing liner material into a stack, the intermediate liner being disposed between the layer of core material and the layer of brazing liner material; and rolling the stack to form a bonded multi-layer brazing sheet. While some embodiments of the present invention have been described, it should be understood that these embodiments are merely illustrative and not limiting, and that many modifications may become apparent to those skilled in the art. It is further understood that the various steps may be performed in any desired order (and any desired steps may be added and / or any desired steps may be eliminated). All such variations and modifications are intended to be included within the scope of the appended claims.
Claims
1. 1. A multi-layer sheet material comprising: a core of one of 2XXX, 3XXX, 5XXX, or 6XXX aluminum alloys; a brazed liner of 4xxx aluminum alloy; and an intermediate liner, the intermediate liner comprising: 0.31 to 1.0 wt.% Si, less than 0.1% by weight of Mg, 0.2 to 0.35 wt.% Mn, max. 0.1 wt.% Zn, max 0.3 wt.% Fe, Maximum 0.2 wt.% Cu, Maximum 0.05 wt.% Ti; Optionally, up to 0.125 wt.% Zr; an alloy of the balance Al and other elements each not exceeding 0.05% by weight and not exceeding 0.15% by weight in total;
2. The intermediate liner is 0.34 to 0.5 wt.% Si; less than 0.05 wt.% Mg; 0.25 to 0.35 wt.% Mn; Zn up to 0.05 wt.%; % Cu. 0.05 wt. % max.
3. The sheet material of claim 2, wherein the intermediate liner contains 0.4 to 0.5 wt. % Si.
4. The sheet material of claim 2, wherein the intermediate liner contains 0.25 to 0.34 wt. % Mn.
5. 2. The sheet material of claim 1, wherein the intermediate liner contains 0.05 to 0.1 wt. % Zn.
6. 10. The sheet material of claim 1, wherein the core is 3003 aluminum alloy.
7. 2. The sheet material of claim 1, wherein the core comprises: 0.1-1.0 wt.% Si; max. 0.5 wt.% Fe; 0.2-1.0 wt.% Cu; 1.0-1.5 wt.% Mn; 0.2-0.3 wt.% Mg; max. 0.05 wt.% Zn; and 0.1-0.2 wt.% Ti.
8. 2. The sheet material of claim 1, wherein the braze liner comprises 6.8-8.2 wt.% Si, max. 0.8 wt.% Fe, max. 0.25 wt.% Cu, max. 0.1 wt.% Mn, max. 0.2 wt.% Zn.
9. The sheet material of claim 1 further comprising another liner disposed on the core distal to the intermediate liner and the braze liner.
10. 10. The sheet material of claim 9, wherein the another liner includes a second braze liner and a second intermediate liner, the second intermediate liner being disposed between the core and the second braze liner.
11. 2. The sheet material of claim 1, wherein the intermediate liner contains 0.34-0.5 wt. % Si.
12. 12. The sheet material of claim 11, wherein the intermediate liner contains less than 0.05 wt.% Cu.
13. 2. The sheet material of claim 1, wherein the sheet material has a total thickness of 0.1 mm to 3.0 mm including a core thickness of 0.09 mm to 2.85 mm, the braze liner has a clad ratio of 2.5% to 20%, and the intermediate liner has a clad ratio of 2.5% to 20%.
14. The sheet material of claim 1 , wherein the sheet material is O-tempered.
15. A heat exchanger comprising at least one of a tube, fin, header plate, or tank comprising the sheet material of claim 1.
16. 1. A multi-layer sheet material comprising: a core of one of 2XXX, 3XXX, 5XXX, or 6XXX aluminum alloys; a brazed liner of 4xxx aluminum alloy; and an intermediate liner, the intermediate liner comprising: 0.31 to 1.0 wt.% Si, 0.1 to 0.5% by weight of Mg, 0.05 to 0.3 wt. % Mn, max. 0.1 wt.% Zn, max 0.3 wt.% Fe, Maximum 0.2 wt.% Cu, Maximum 0.05 wt.% Ti; Optionally, up to 0.125 wt.% Zr; the balance being an alloy of Al and other elements each not exceeding 0.05% by weight and not exceeding 0.15% by weight in total.
17. The sheet material of claim 16, wherein the intermediate liner contains 0.05 to 0.1 wt. % Zn.
18. A method for making a brazing sheet, comprising the steps of: providing a layer of an intermediate liner according to any one of claims 1, 2, 3, 4, 5, 11, 12, 16 or 17; providing a layer of a core material selected from one of a 2XXX, 3XXX, 5XXX, or 6XXX aluminum alloy; providing a layer of 4xxx aluminum alloy braze liner material; stacking the layer of intermediate liner, the layer of core material, and the layer of braze liner material into a stack, the intermediate liner being disposed between the layer of core material and the layer of braze liner material; and rolling the stack to form a bonded multi-layer brazing sheet.
Citation Information
Patent Citations
Brazing sheet for heat exchanger, excellent in corrosion resistance and strength after brazing
JP1999140574A
Aluminum alloy clad material for heat exchanger
JP2001269794A
Aluminum alloy brazing sheet
JP2007152421A
Method for producing aluminum alloy brazing sheet
JP2007152422A
Aluminum alloy-clad material for heat exchanger and brazing sheet
JP2008240084A