Superconducting joint structure between Nb3Sn superconducting wire and NbTi wire, its manufacturing method, and nuclear magnetic resonance apparatus using the same

The superconducting connection structure using an M-doped Nb alloy strip effectively connects Nb3Sn and NbTi wires, ensuring high critical current performance in strong magnetic fields without hazardous materials, addressing the limitations of conventional technologies.

JP7587889B2Active Publication Date: 2024-11-21NAT INST FOR MATERIALS SCI
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023527578
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-06-08
Filing Date
2022-05-11
Publication Date
2024-11-21
Estimated Expiration
2042-05-11

AI Technical Summary

Technical Problem

Conventional superconducting connection technologies between Nb3Sn superconducting wire and NbTi wire contain environmentally hazardous substances like Pb and Cd, and there is a lack of effective methods for connecting dissimilar superconducting materials without these substances, especially for high-precision nuclear magnetic resonance (NMR) applications requiring strong magnetic fields.

Method used

A superconducting connection structure using an Nb alloy strip doped with an M element (such as Hf, Ta, Zr, or W) to increase the recovery and recrystallization temperature of Nb, allowing for diffusion bonding with Nb3Sn and mechanical connection with NbTi wire, without using hazardous materials, through a process involving exposure, bundling, crimping, and heat treatment.

Benefits of technology

The method enables stable superconducting connections between Nb3Sn and NbTi wires, maintaining high critical current properties even in magnetic fields of 0.5-1.0 T, suitable for NMR applications, without using environmentally harmful substances and reducing manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587889000001
    Figure 0007587889000001
  • Figure 0007587889000002
    Figure 0007587889000002
  • Figure 0007587889000003
    Figure 0007587889000003
Patent Text Reader

Abstract

The present invention addresses the problem of providing: a superconducting connection structure of an Nb3Sn superconducting wire rod and an NbTi wire rod, the superconducting connection structure comprising no environmental load substances such as Pb and Cd; a method for producing this superconducting connection structure; and a nuclear magnetic resonance apparatus which uses this superconducting connection structure. A superconducting connection structure according to the present invention is provided with: a connection strip that comprises an Nb alloy strip to which an element M is added (wherein the element M is an element which increases the recovery temperature and the recrystallization temperature of Nb); an Nb3Sn superconducting wire rod that comprises an Nb3Sn superconducting core material; and an NbTi wire rod that comprises an NbTi core material. With respect to this superconducting connection structure, one end of the connection strip is connected to the Nb3Sn superconducting wire rod by having the Nb alloy strip and the Nb3Sn superconducting core material in contact with each other by the intermediary of an Nb3Sn superconducting layer; and the other end of the connection strip is connected to the NbTi wire rod by having a newly formed surface of the Nb alloy strip and a newly formed surface of the NbTi core material in contact with each other.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention is 3 The present invention relates to a superconducting connection structure between an Sn superconducting wire and an NbTi wire, a method for manufacturing the same, and an NMR analyzer using the same. [Background technology]

[0002] In nuclear magnetic resonance (NMR) spectrometers, it is desirable to operate the magnets for orienting the spins of atomic nuclei in a state of persistent current in order to achieve high-precision NMR measurements. To achieve this, in addition to using superconducting wire with zero electrical resistance, a technology is required to connect superconducting wires of a limited length with zero resistance, i.e., so-called superconducting connection technology.

[0003] In particular, in medium-sized NMR devices that require a magnetic field of 10T (tesla) or more, it is necessary to use NbTi superconducting wires as well as Nb 3 Superconducting connections between dissimilar superconducting materials using Sn superconducting wires are essential.

[0004] NbTi is an alloy in which Ti is dissolved in a body-centered cubic lattice of Nb, and is therefore ductile and tough, and it is known that it is possible to realize a superconducting connection by mechanical pressure welding (see, for example, Patent Document 1). 3 Sn is an A15 type compound crystal composed of Nb atoms and Sn atoms in a 3:1 ratio, and is hard and brittle with no ductility, making it impossible to join by mechanical methods.

[0005] Therefore, instead of joining by mechanical methods, a superconducting connection technique using low melting point superconducting solder has been developed (see, for example, Patent Document 2 and Non-Patent Document 1). According to Patent Document 2, NbTi and Nb 3At the end of the Sn multifilamentary wire, the Cu matrix in which the superconducting filaments are embedded is melted with molten Sn or Sn alloy, and the filaments are coated with Sn. Next, the ends of both wires are immersed in molten Pb-Bi to replace the Sn with Pb-Bi. Finally, the ends of both wires are immersed in a cup filled with Pb-Bi to form a joint, resulting in a NbTi-Nb 3 This method realizes superconducting joints between Sn wires. 3 The surface of the Sn filament is not exposed to the atmosphere, and NbTi and Nb 3 Since the Sn can be bonded to the superconducting Pb-Bi without mechanical deformation, a good NbTi-Nb alloy can be obtained by using the Pb-Bi superconductivity. 3 A superconducting joint between Sn wires is obtained. The superconducting properties of this joint depend on the properties of Pb-Bi, and it is usually used in a magnetic field environment of 0.5 to 1.0 T.

[0006] Non-Patent Document 1 discloses superconducting joining technology using Wood Metal (50%Bi-24%Pb-14%Sn-12%Cd), Pb-In, and Sn-In as another low-melting point superconducting solder, but most of the solders with relatively high critical magnetic fields that can be used practically contain Pb and Cd, which are environmentally hazardous substances.

[0007] However, Pb and Cd are now strictly regulated as environmentally hazardous substances, and there is a strong demand for new environmentally friendly joining technologies that do not contain these substances.

[0008] On the other hand, recently, Nb 3 In relation to research into Sn structure control, it has been reported that Hf increases the recovery and recrystallization temperature of Nb (see, for example, Non-Patent Document 2). According to FIG. 1 of Non-Patent Document 2, it has been reported that an Nb-4 at% Ta-1 at% Hf alloy, which contains 1 at% Hf and 4 at% Ta, remained dense even after heat treatment at 900°C. Furthermore, according to FIG. 2 of Non-Patent Document 2, it has been reported that when the recovery and recrystallization temperature of an Nb-Hf alloy containing only Hf was investigated, the recovery temperature was found to be significantly higher than 600°C. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] U.S. Pat. No. 3,422,529 [Patent Document 2] U.S. Pat. No. 4,907,338 [Non-patent literature]

[0010] [Non-Patent Document 1] GD Brittles et al.,Supercond.Sci.Technol.,28,2015,093001 [Non-Patent Document 2] N. Banno et al., Scripta Materialia, 199, 2021, 113822 Summary of the Invention [Problem to be solved by the invention]

[0011] As mentioned above, in superconducting joint technology using low melting point superconducting solder, Nb 3 Conventional superconducting joint technologies between Sn superconducting wires and NbTi wires (for example, Patent Document 2 and Non-Patent Document 1) contain environmentally hazardous substances such as Pb and Cd. In addition, Non-Patent Document 2 states that Nb 3 The research has been limited to the simple structure control of Sn itself, and has not been focused on superconducting connections between different superconducting materials (e.g., Nb 3 The present application did not provide any teaching or suggestion regarding the superconducting joint between Sn superconducting wire and NbTi wire. The objective of this invention is to develop a completely new Nb alloy that does not contain environmentally hazardous substances such as Pb and Cd, which goes beyond conventional ideas. 3 The present invention provides a superconducting connection structure between an Sn superconducting wire and an NbTi wire, a method for manufacturing the same, and a nuclear magnetic resonance apparatus using the same. [Means for solving the problem]

[0012] The superconducting joint structure of the present invention comprises a joint strip having an Nb alloy strip to which an element M is added, the element M being an element that increases the recovery temperature and recrystallization temperature of Nb, and a joint strip having an Nb alloy strip having an element M added thereto. 3 Nb with Sn superconducting core 3 The connecting strip is provided with a Sn superconducting wire and a NbTi wire having a NbTi core material, and one end of the connecting strip is connected to the Nb alloy strip and the Nb 3 Sn superconducting core material and Nb 3 The Nb 3 The connecting strip is connected to a Sn superconducting wire, and the other end of the connecting strip is connected to the NbTi wire by the newly formed surface of the Nb alloy strip and the newly formed surface of the NbTi core material coming into contact with each other, thereby solving the above-mentioned problem. The M element may be at least one selected from the group consisting of hafnium (Hf), titanium (Ti), tantalum (Ta), zirconium (Zr), and tungsten (W). The Nb alloy strip may be in any one shape selected from the group consisting of a core material, a sheet, and a pipe. In the present application, a strip refers to a long, thin belt-like material shaped like a core, sheet, or pipe. The M element may be added in a range of 0.2 at % to 10 at % (here, at % refers to the atomic % of the M element contained in the Nb alloy strip). The Nb alloy strip and the Nb 3 Sn superconducting core material and Nb 3 The portion where they come into contact via the Sn superconducting layer and the portion where the newly formed surface of the Nb alloy strip and the newly formed surface of the NbTi core material come into contact with each other may each be covered with a crimped tube made of at least one material selected from the group consisting of tantalum (Ta), niobium (Nb), copper-nickel alloy (CuNi), and stainless steel. The length of the covered portion may be in the range of 10 mm to 30 mm. The connecting strip is formed by covering and / or embedding the Nb alloy strip with a first stabilizing material, and the Nb 3 The Sn superconducting wire is 3 The Sn superconducting core material is coated and / or embedded in a second stabilizing material, and the NbTi wire material is coated and / or embedded in a third stabilizing material, and each of the first to third stabilizing materials may be at least one metal selected from the group consisting of copper metal, copper alloy, silver metal, and silver alloy. The method for producing the above superconducting joint structure of the present invention includes disposing one end of a joint strip having an Nb alloy strip to which an element M is added (wherein the element M is an element that increases the recovery temperature and recrystallization temperature of Nb) and a Nb 3 Nb with Sn superconducting core 3 The method includes a first connecting step of connecting an end of the connecting strip to a Sn superconducting wire and a second step of connecting the other end of the connecting strip to a NbTi wire having a NbTi core material, the first connecting step being a step of exposing the Nb alloy strip from one end of the connecting strip, and a step of connecting the NbTi wire having a NbTi core material embedded in a base material containing at least Cu and Sn. 3 A step of exposing the Nb core material from one end of a Sn superconducting precursor wire, a step of bundling the exposed Nb alloy strip and the exposed Nb core material, a step of crimping the bundled Nb alloy strip and the Nb core material, and a step of bonding the crimped Nb alloy strip and the connection strip including the Nb core material and the Nb core material. 3 and a step of heat treating the Sn superconducting precursor wire, and the second connecting step includes a step of exposing the Nb alloy strip from the other end of the connecting strip, a step of exposing the NbTi core material from one end of the NbTi wire, a step of bundling the exposed Nb alloy strip and the exposed NbTi core material, and a step of crimping the bundled Nb alloy strip and NbTi core material, thereby solving the above-mentioned problem. The step of exposing the Nb alloy strip in the first connecting step and the second connecting step may use chemical etching. The step of exposing the Nb core material in the first connecting step may use chemical corrosion. The step of exposing the Nb core material in the first connecting step may further include mechanical polishing. The step of exposing the NbTi core material in the second connecting step may use chemical corrosion. The steps of exposing the Nb alloy strip in the first connecting step and the second connecting step, the step of exposing the Nb core material in the first connecting step, and the step of exposing the NbTi core material in the second connecting step may each expose a length in the range of 10 mm or more and 30 mm or less. The pressing step in the first connecting step may expose new surfaces of the Nb alloy strip and the Nb core material, and bring the new surfaces of the Nb alloy strip and the Nb core material into close contact with each other. The crimping step in the first connecting step may involve covering the bundled Nb alloy strips and the Nb core material with a crimping tube made of at least one material selected from the group consisting of tantalum (Ta), niobium (Nb), copper-nickel alloy (CuNi), and stainless steel, and applying pressure in a direction perpendicular to the longitudinal direction of the bundled Nb alloy strips and the Nb core material. The pressure may be in the range of 100 MPa to 1 GPa. The heat treatment step in the first connecting step is performed by subjecting the connecting strip and the Nb 3 The Sn superconducting precursor wire may be heat-treated in a vacuum or in an inert gas atmosphere at a temperature in the range of 600° C. to 800° C. The heat treatment step in the first connecting step is performed by subjecting the connecting strip and the Nb 3 The Sn superconducting precursor wire may be heat-treated in a vacuum or in an inert gas atmosphere at a temperature range of 300°C to 500°C for 50 hours to 150 hours, and then at a temperature range of 600°C to 800°C for 50 hours to 150 hours. The pressing step in the second connecting step may expose fresh surfaces of the Nb alloy strip and the NbTi core material, and bring the fresh surfaces of the Nb alloy strip and the NbTi core material into close contact with each other. The crimping step in the second connecting step may include covering the bundled Nb alloy strips and the NbTi core material with a crimping tube made of a material selected from the group consisting of tantalum (Ta), niobium (Nb), copper-nickel alloy (CuNi), and stainless steel, and applying pressure in a direction perpendicular to the longitudinal direction of the bundled Nb alloy strips and the NbTi core material. The pressure may be in the range of 100 MPa to 1 GPa. In the present application, a new surface refers to a metal surface that is in an active state, does not have an oxide film or the like, and is not exposed to the atmosphere, as described below. The nuclear magnetic resonance apparatus of the present invention uses the above-mentioned superconducting connection structure, and solves the above-mentioned problems by using this (i.e., the nuclear magnetic resonance apparatus of the present invention including the above-mentioned superconducting connection structure). Effect of the Invention

[0013] The superconducting joint structure of the present invention uses a Nb alloy strip containing an M element. 3 The Sn superconducting wire is connected to the NbTi wire. The addition of the M element increases the recovery and recrystallization temperature of Nb, so high-temperature heat treatment (specifically, Nb 3 The superconducting properties of the Nb alloy strip do not deteriorate even after the heat treatment to form the Sn layer. 3 Through the Sn superconducting layer, Nb 3 The other end of the Nb alloy strip can be mechanically connected to the NbTi wire, so that the NbTi wire can be connected without deteriorating the properties of the NbTi wire. As a result, it is possible to produce NbTi alloy strips without using environmentally hazardous substances such as Pb and Cd, and still maintaining high superconducting properties. 3A superconducting connection structure of a Sn superconducting wire and a NbTi wire can be provided.

[0014] The method for producing the above-mentioned superconducting joint structure of the present invention includes the steps of: (1) forming a joint strip having an Nb alloy strip containing an element M; 3 Nb with Sn superconducting core 3 The method includes a first connecting step of connecting the Sn superconducting wire to the connecting strip, and a second step of connecting the other end of the connecting strip to the NbTi wire having a NbTi core material. The Nb alloy strip is used, in which the recovery and recrystallization temperature of Nb is increased by the addition of the M element, and the properties of the Nb alloy strip are not deteriorated even by heat treatment, and the Nb 3 From Sn superconducting precursor wire to Nb 3 Sn superconducting wire can be produced, and Nb formed on the Nb alloy strip can be 3 Through the Sn superconducting layer, Nb alloy strip and Nb 3 The Nb alloy strip and the NbTi wire can be mechanically joined without using environmentally hazardous substances such as Pb and Cd. 3 A superconducting joint can be formed between a Sn superconducting wire and a NbTi wire. [Brief description of the drawings]

[0015] [Figure 1] 1 is a schematic diagram showing a superconducting connection structure of the present invention. [Diagram 2] 2A is a schematic diagram showing an exemplary form of the Nb alloy strip, in which Fig. 2(A) is a schematic diagram showing a case where the form of the Nb alloy strip is a core material, Fig. 2(B) is a schematic diagram showing a case where the form of the Nb alloy strip is a sheet, and Fig. 2(C) is a schematic diagram showing a case where the form of the Nb alloy strip is a pipe. [Diagram 3] 3A is a schematic diagram showing a cross section of a Nb3Sn superconducting wire and a NbTi wire, and FIG. 3B is a schematic diagram showing a cross section of a NbTi wire. [Figure 4]4 is a flowchart of a process for manufacturing a superconducting connection structure of the present invention. [Diagram 5] 5A is a schematic diagram of an exemplary Nb3Sn superconducting precursor wire used in the manufacture of a superconducting joint structure of the present invention. Here, Fig. 5A is an exemplary schematic diagram of an Nb3Sn superconducting precursor wire comprising an Nb core material, a Cu-Sn base material (i.e., a base material made of an alloy of Cu and Sn), a diffusion barrier layer, and a stabilizing material, in which the Nb core material is embedded in the Cu-Sn base material, and Fig. 5B is an exemplary schematic diagram of an Nb3Sn superconducting precursor wire comprising an Nb core material, a Cu base material, a Sn base material, a diffusion barrier layer, and a stabilizing material, in which the Nb core material is embedded only in the Cu base material. [Figure 6] 11 is a flowchart of a first connection step. [Figure 7] This is a procedure for the first connection step. [Figure 8] 11 is a flowchart of a second connection step. [Figure 9] This is a procedure for the second connection step. [Figure 10] FIG. 1 is a diagram showing the critical current characteristics of a NbTi wire (reference example) before and after a heat treatment. [Figure 11] FIG. 1 is a diagram showing the critical current characteristics before and after heat treatment of a Nb—Ta—Hf wire (reference example). [Figure 12] 12A and 12B are diagrams showing the results of electron microscope observation of a cross section of a joint part between a connection strip and a Nb3Sn superconducting wire of a superconducting connection structure, in which Fig. 12(A) is a diagram showing the results of electron microscope observation of a cross section of a connection part between a connection strip (i.e., a Nb-Ta-Hf wire) and a Nb3Sn superconducting core material, Fig. 12(B) is a diagram showing Nb mapping of the connection part, Fig. 12(C) is a diagram showing a backscattered electron image of the connection part, and Fig. 12(D) is a diagram showing Sn mapping of the connection part. [Figure 13] FIG. 2 is a diagram showing the critical current characteristics of the superconducting connection structure of Example 1. [Figure 14] FIG. 13 is a diagram showing the critical current characteristics of the superconducting connection structure of Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. Note that like elements are given like reference numerals and their description will be omitted.

[0017] FIG. 1 is a schematic diagram showing a superconducting connection structure of the present invention.

[0018] The superconducting joint structure 100 of the present invention comprises a joint strip 120 having a Nb alloy strip 110 to which an M element is added, and a Nb 3 The Sn superconducting wire 130 and the NbTi wire 140 are provided, and the Nb alloy strip 110 is used to form the Nb 3 The Sn superconducting wire 130 and the NbTi wire 140 are connected. The Nb alloy strip 110 is characterized in that the recovery temperature and recrystallization temperature of Nb are increased by adding the element M. The degree of increase is determined by the degree of increase in the recovery temperature and recrystallization temperature of Nb. 3 There is no particular restriction as long as the increase reaches the temperature at which Sn is formed (specifically, 600° C.) or higher.

[0019] In detail, Nb 3 Sn superconducting wire 130 is Nb 3 The NbTi wire 140 has a NbTi core 160. One end of the connecting strip 120 is connected to the Nb alloy strip 110 and the Nb 3 Sn superconducting core material 150 and Nb 3 By contacting through the Sn superconducting layer 170, Nb 3 The Nb 3 The Sn superconducting layer 170 is made of Nb 3 It may be a layer constituting the Sn superconducting core material 150, or it may be a layer formed on the surface of the Nb alloy strip 110.

[0020] The other end of the connecting strip 120 is connected to the NbTi wire 140 by contacting the newly formed surface of the Nb alloy strip 110 with the newly formed surface of the NbTi core material 160. Here, the newly formed surface refers to a metal surface in an active state that does not have an oxide film or the like and is not exposed to the atmosphere, and the contact between the newly formed surfaces can be evaluated from the critical current characteristics.

[0021] The inventors of the present application have found that by using the Nb alloy strip 110 having an increased recovery temperature and recrystallization temperature, it is possible to obtain Nb by the manufacturing method described below. 3 It has been found that it is possible to provide a superconducting connection structure 100 in which a Sn superconducting wire 130 and a NbTi wire 140 are connected.

[0022] Each component will be described in detail below. The M element is not particularly limited as long as it increases the recovery and recrystallization temperature of Nb, but is preferably at least one element selected from the group consisting of hafnium (Hf), titanium (Ti), tantalum (Ta), zirconium (Zr), and tungsten (W). Among them, Hf is preferable. Hf can increase the recovery and recrystallization temperature of Nb by 200° C., and is therefore advantageous in the manufacturing method described below.

[0023] The amount of the M element is not limited as long as it does not impair the superconducting properties of the Nb alloy, but is preferably in the range of 0.2 at% or more and 10 at% or less. If it is 0.2 at% or more, a critical magnetic field of 0.2 T or more can be obtained, which is advantageous for practical use, and is therefore preferable. If it is 10 at% or less, it is preferable because it is possible to avoid the difficulty of solid-solubilizing the Nb alloy. From the viewpoint of the recovery of Nb, the increase in the recrystallization temperature, and the critical magnetic field, the amount of the M element is more preferably in the range of 1 at% to 6 at%, and even more preferably in the range of 1.5 at% to 3 at%. When the M element is composed of multiple elements, the total amount of each element added may be within the above range. The content of the M element in the Nb alloy is measured by energy dispersive X-ray spectroscopy (EDS).

[0024] The connecting strip 120 preferably includes a first stabilizing material 210 (FIG. 2) covering the Nb alloy strip 110. The first stabilizing material is made of a normal metal material and can easily divert and stabilize the electric current even when subjected to a thermal disturbance or the like.

[0025] The first stabilizing material 210 may be preferably made of a material selected from the group consisting of copper metal, copper alloy, silver metal, and silver alloy. All of these are known as normal conductive metal materials. Among them, copper metal is preferable from the viewpoint of cost and workability.

[0026] FIG. 2 is a schematic diagram showing an exemplary morphology of the Nb alloy strip.

[0027] Fig. 2(A) shows the case where the form of the Nb alloy strip is a core material 110a, but the form of the Nb alloy strip is not limited to a core material (multi-core wire). As shown in Fig. 2(B), the form of the Nb alloy strip may be a sheet 110b, and as shown in Fig. 2(C), the form of the Nb alloy strip may be a pipe 110c. Fig. 2 shows how the Nb alloy strip of each shape (form) is covered with the first stabilizing material 210.

[0028] If the Nb alloy strip is in the form of a core material 110a as shown in FIG. 2(A), it is advantageous to suppress the thermal runaway phenomenon called magnetic flux jump, which is specific to superconductors. If the Nb alloy strip is in the form of a sheet 110b as shown in FIG. 2(B), it is advantageous to suppress the thermal runaway phenomenon called magnetic flux jump, which is specific to superconductors, in the manufacturing process described later. 3 This is advantageous because the Nb core material that becomes the Sn superconducting core material 150 can be bundled by folding it with the sheet 110b. If the Nb alloy strip is in the form of a pipe 110c as shown in FIG. 2(C), the Nb 3 This is advantageous because the Nb core materials that become the Sn superconducting core materials 150 can be bundled simply by passing them through the pipe 10c.

[0029] Figure 3 shows the Nb 3 FIG. 2 is a schematic diagram showing a Sn superconducting wire and a NbTi wire.

[0030] Figure 3(A) and (B) show the results of Nb 3 The cross sections of the Sn superconducting wire and the NbTi wire are shown. 3 The Sn superconducting wire 130 is a multi-core wire of Nb 3 The Sn superconducting core material 150 may be covered by and / or embedded in the second stabilizing material 310. In the present invention, Nb 3 The Sn superconducting wire 130 is made of Nb 3 The commonly used Nb is obtained by heat treatment from Sn precursor wire. 3 The second stabilizer 310 may be a Sn superconducting wire. Again, the second stabilizer 310 may be made of a normal metal material, preferably a material selected from the group consisting of copper metal, copper alloy, silver metal, and silver alloy.

[0031] Nb 3 The Sn superconducting wire 130 may include a diffusion barrier layer 320. The diffusion barrier layer 320 is made of Nb 3 This can prevent element diffusion during production from the Sn precursor wire by heat treatment. Such a diffusion barrier layer 320 may be made of tantalum (Ta), niobium (Nb), or an alloy thereof. These materials more preferably suppress the diffusion of Sn and Nb.

[0032] The NbTi wire 140 may have a multi-core NbTi core 160 covered by and / or embedded in a third stabilizing material 330. Again, the third stabilizing material 330 may be made of a normal metal material, preferably a material selected from the group consisting of copper metal, copper alloy, silver metal, and silver alloy. The first to third stabilizing materials may be different or the same.

[0033] The NbTi core material 160 may be a commonly used and available NbTi core material, but preferably, the Ti composition in the NbTi alloy satisfies the range of 8 at% to 90 at%. This range allows wire drawing and maintains higher properties. The Ti composition in the NbTi alloy more preferably satisfies the range of 50 at% to 70 at%.

[0034] According to the superconducting joint structure 100 of the present invention, preferably, the Nb alloy strip 110 and the Nb 3 Sn superconducting core material 150 and Nb 3 The contact portion between the Sn superconducting layer 170 and the newly formed surface of the Nb alloy strip 110 and the newly formed surface of the NbTi core material 160 may be covered with a crimping tube 180 as shown in FIG. 3 Bonding with the Sn superconducting core 150 as well as bonding between the Nb alloy strip 110 and the NbTi core 160 can be promoted.

[0035] The crimping tube 180 is not particularly limited as long as it has a Vickers hardness of 60 Hv or more, but is illustratively made of a material selected from the group consisting of tantalum (Ta), niobium (Nb), copper-nickel alloy (CuNi), and stainless steel. These materials have a Vickers hardness of 60 Hv or more and 300 Hv or less. Furthermore, the Nb alloy strip 110 and the Nb 3 In the joint with the Sn superconducting core material 150, the crimped tube 180 and Nb 3 In a situation where the crimping tube 180 comes into contact with the Sn superconducting core material 150, the material of the crimping tube 180 is preferably tantalum (Ta) in order to suppress reactions during heat treatment.

[0036] According to the superconducting joint structure 100 of the present invention, the Nb alloy strip 110 and the Nb 3The length of the portion where the Sn superconducting core material 150 is in contact with and covered by the Nb alloy strip 110 and the NbTi core material 160 is in contact with and covered by the NbTi core material 160 (specifically, the length of the crimped tube 180) is preferably in the range of 10 mm to 30 mm. In this range, sufficient contact is obtained, and good superconducting properties are obtained. More preferably, the length of the contacting and covered portion is in the range of 10 mm to 20 mm and 15 mm to 25 mm, respectively.

[0037] In this way, the superconducting connection structure 100 of the present invention does not use environmentally hazardous substances such as Pb and Cd, and maintains a high critical current even in a magnetic field environment of 0.5 T to 1.0 T. 3 Since the Sn superconducting wire 130 and the NbTi wire 140 are connected, it can also be used in high magnetic field nuclear magnetic resonance (NMR) devices. In particular, since the superconducting connection structure 100 of the present invention does not use any environmentally hazardous substances, there is no need to apply for exemption under the RoHS Directive (Restriction of Hazardous Substances Directive). This also makes it possible to significantly reduce the manufacturing costs of NMR. The superconducting connection structure of the present invention preferably satisfies critical current characteristics of at least 50 A in a magnetic field environment of 0.6 T at 4.2 K.

[0038] Next, a manufacturing process for the superconducting connection structure 100 of the present invention will be described. FIG. 4 is a flow chart of the process for producing a superconducting connection structure of the present invention.

[0039] Step S410: One end of the connecting strip is provided with a Nb alloy strip containing an M element, and Nb 3 Nb with Sn superconducting core 3 Connect to Sn superconducting wire. Step S420: Connect the other end of the connecting strip to a NbTi wire having a NbTi core. The superconducting connection structure 100 of the present invention is manufactured by a first connection step in step S410 and a second connection step in step S420.

[0040] Here, the connection strip having the Nb alloy strip to which the M element is added, and the NbTi wire having the NbTi core material have already been described with reference to FIG. 1, and therefore description thereof will be omitted.

[0041] In order to use a Nb alloy strip in which the recovery and recrystallization temperature of Nb is increased by adding the M element, the Nb 3 The properties of the Nb alloy strip are not deteriorated by the heat treatment for Sn generation, and the Nb alloy strip is 3 From Sn superconducting precursor wire (Fig. 5) to Nb 3 Sn superconducting wire can be produced, and Nb formed on the Nb alloy strip can be 3 Through the Sn superconducting layer, Nb alloy strip and Nb 3 In the second joining step, the Nb alloy strip and the NbTi wire are mechanically joined, so that the Nb alloy strip and the NbTi wire are free of environmentally hazardous substances such as Pb and Cd. 3 A superconducting joint can be formed between a Sn superconducting wire and a NbTi wire.

[0042] In the manufacture of the superconducting joint structure of the present invention, Nb 3 Sn superconducting precursor wire is used, but Nb 3 The Sn superconducting precursor wire is a Nb core embedded in a matrix containing at least Cu and Sn. 3 Sn superconducting precursor wire can be used, and such Nb 3 Sn superconducting precursor wire is commercially available.

[0043] FIG. 5 shows an exemplary Nb alloy for use in fabricating a superconducting joint structure of the present invention. 3 FIG. 2 is a schematic diagram of a Sn superconducting precursor wire.

[0044] Nb shown in FIG. 3The Sn superconducting precursor wire 500a may have an Nb core material 510 embedded in a Cu-Sn matrix 520a. The Cu-Sn matrix 520a is made of an alloy of Cu and Sn, and the Sn content is preferably in the range of 5 at% to 10 at%. If the Sn content is within this range, the Nb core material 510 reacts with the Nb core material 510 to produce Nb. 3 The Sn superconducting core material 150 (FIG. 1) is produced and has the ability to be processed into a core wire.

[0045] Nb 3 The Sn superconducting precursor wire 500a may preferably include a diffusion barrier layer 530 around the Cu-Sn matrix 520a. This can suppress diffusion of Nb from the Nb core material 510 and Sn from the Cu-Sn matrix 520a during heat treatment, which will be described later. The diffusion barrier layer 530 may be made of tantalum (Ta), niobium (Nb), or an alloy thereof.

[0046] Nb 3 The Sn superconducting precursor wire 500a may preferably include a stabilizing material 540 around the Cu-Sn base material 520a. This prevents the Nb 3 Even if the Sn superconducting core returns to a normal conducting state, the current can be easily diverted. The stabilizing material 540 is the same material as the second stabilizing material 310 described above.

[0047] Nb shown in FIG. 3 The Sn superconducting precursor wire 500b includes a Cu matrix 520b and a Sn matrix 550, and the Nb core material 510 is embedded only in the Cu matrix 520b. This is the same as the Nb core material 510 in FIG. 3The wire is different from the Sn superconducting precursor wire 500a. In the present specification, even when the base material in which the Nb core material is embedded is divided into a Cu base material and a Sn base material, the Nb core material is considered to be embedded in the base material containing Cu and Sn. In other words, the embodiment of the "base material containing at least Cu and Sn" in the present specification includes, in addition to the embodiment in which at least Cu and Sn are contained in the same base material as in FIG. 5(A) (i.e., the base material containing Cu and the base material containing Sn are the same), for example, the embodiment in which the base material containing at least Cu and the base material containing Sn are separated as in FIG. 5(B). Therefore, examples of the embodiment in which "the Nb core material is embedded in a base material containing at least Cu and Sn" include an embodiment in which the Nb core material is embedded in a Cu-Sn base material made of an alloy of Cu and Sn as shown in FIG. 5(A), an embodiment in which the Nb core material is embedded only in the base material made of Sn in a base material in which a base material made of Cu and a base material made of Sn are separated as shown in FIG. 5(B), and an embodiment in which the Nb core material is embedded only in the base material made of Cu in a base material in which a base material made of Cu and a base material made of Sn are separated as shown in FIG. 5(B). In the case of FIG. 5(B) in which the base material in which the Nb core material is embedded is separated into a Cu base material and a Sn base material, the Sn base material 550 preferably satisfies the range of 10 at % or more and 60 at % or less with respect to the total of the Cu base material 520b and the Sn base material 550. If it is within this range, it preferably reacts with the Nb core material 510 and Nb 3 The Sn superconducting core material 150 (FIG. 1) is produced and has the ability to be processed into a core wire.

[0048] Nb 3 The Sn superconducting precursor wire 500b is made of Nb 3 Similar to the Sn superconducting precursor wire 500a, a stabilizer 540 may be provided around the Cu base material 520b.

[0049] Nb shown in Fig. 5 3 The Sn superconducting precursor wire is merely an example. In addition, for example, Nb 3A Sn superconducting precursor wire can also be applied. From this viewpoint, the Nb core material 510 may be embedded in a base material containing at least Cu and Sn, but the base material (Cu base material, Sn base material, or Cu-Sn base material) may further contain zinc (Zn), germanium (Ge), gallium (Ga), magnesium (Mg), aluminum (Al), and titanium (Ti).

[0050] The first connecting step and the second connecting step will be described in detail below. FIG. 6 is a flowchart of the first connection step. FIG. 7 shows the procedure of the first connection step.

[0051] Here, the connecting strip 120 shown in FIG. 1 is used as the connecting strip, and Nb 3 The Sn superconducting precursor wire is Nb 3 The first joining step (S410) in FIG. 4 will be described in detail assuming that the Sn superconducting precursor wire 500a is used.

[0052] Step S411: The Nb alloy strip (core material) 110a is exposed from one end of the connection strip 120 in which the Nb alloy strip (core material) 110a is covered with the first stabilizing material 210. The method of exposure is not particularly limited, but it is performed by chemical corrosion, mechanical polishing, or a combination of these. The exposed length is preferably in the range of 10 mm to 30 mm. In this range, when bundling with the Nb core material 510 described later, good superconducting characteristics can be obtained due to sufficient contact. The exposed length is more preferably in the range of 10 mm to 20 mm.

[0053] Step S412: The Nb core material 510 is embedded in a base material (Cu-Sn base material 520a) containing at least Cu and Sn. 3 The Nb core material 510 is exposed from one end of the Sn superconducting precursor wire 500a. The method for exposing the Nb core material 510 is not particularly limited, but it can be performed by chemical corrosion, mechanical polishing, or a combination of these. Preferably, the chemical corrosion and mechanical polishing are performed in this order. As a result, the Nb3 This also facilitates exposure when the Sn superconducting precursor wire 500a has a diffusion barrier layer 530. The exposed length is preferably in the range of 10 mm to 30 mm. In this range, sufficient contact is achieved when bundling with the Nb alloy strip 110a exposed in step S411, resulting in good superconducting properties. The exposed length is more preferably in the range of 10 mm to 20 mm. At this time, care must be taken not to completely remove the base material containing Cu and Sn. The remaining Cu-Sn is mixed with Nb. 3 This is because it is essential for the formation of the Sn layer.

[0054] Step S413: Bundle the exposed Nb alloy strips 110a and the exposed Nb core material 510. There is no limitation on the method of bundling, but they may be joined, twisted, entangled, wrapped, or the like.

[0055] Step S414: The Nb alloy strips 110a and the Nb core material 510 bound in step S413 are pressed together. The pressing is performed by applying pressure to the bound Nb alloy strips 110a and the Nb core material 510, exposing their respective newly formed surfaces, and bonding them together. This allows Nb to be bonded to the newly formed surfaces by a heat treatment, which will be described later. 3 A Sn superconducting layer may be produced and bonded.

[0056] Preferably, the bundled portion is covered with the crimping tube 180, and then pressure is applied in a direction perpendicular to the longitudinal direction of the bundled Nb alloy strips 110a and the Nb core material 510 to crimp them. This allows the newly formed surfaces to adhere to each other. The crimping tube 180 is as already described with reference to FIG. 1. The pressure to be applied is preferably in the range of 100 MPa to 1 GPa. This range can promote adhesion between the newly formed surfaces. The pressure to be applied is more preferably in the range of 300 MPa to 500 MPa. This range can promote adhesion between the newly formed surfaces without breaking the wire.

[0057] Step S415: The Nb alloy strip and the connecting strip 120 including the Nb core material and the Nb3 The Sn superconducting precursor wire 500a is heat-treated. 3 Sn superconducting precursor wire 500a Nb 3 This may be a normal heat treatment for forming a Sn superconducting wire. As a result, the Nb core material 510 reacts with the Cu-Sn base material 520a, and Nb 3 The resulting superconducting core material is Sn 150, and the newly formed surfaces of the bundled Nb alloy strips and the Nb core material are treated with Nb 3 A Sn superconducting layer 170 can be formed. In the present invention, the Nb alloy strip is used in which the recovery temperature and recrystallization temperature of Nb are increased by adding the M element, so that the superconducting properties of the Nb alloy strip are not deteriorated even by conventional heat treatment.

[0058] The heat treatment conditions are preferably in a vacuum or in an inert gas atmosphere such as argon (Ar) or helium (He) at a temperature range of 600° C. to 800° C. This allows the Nb alloy strip to maintain its high superconducting properties while improving the Nb 3 Sn superconducting core material 150 and Nb on the nascent surface 3 The heat treatment time can promote the formation of the Sn superconducting layer 170. 3 The time varies depending on the length of the Sn superconducting precursor wire 500a and the number of multifilamentary wires, but is illustratively in the range of 5 hours or more and 300 hours or less.

[0059] More preferably, the heat treatment may be performed in two stages within the above temperature range. For example, the heat treatment may be performed in a vacuum or in an inert gas atmosphere at a temperature range of 300°C to 500°C for 50 hours to 150 hours, and then at a temperature range of 600°C to 800°C for 50 hours to 150 hours. By such a two-stage heat treatment, it is possible to obtain homogeneous Nb alloy strip while maintaining the high superconducting properties of the Nb alloy strip. 3 Sn superconducting core material 150 and Nb on the nascent surface 3 This can promote the formation of the Sn superconducting layer 170.

[0060] In FIG. 6, the process is described as being performed in the order of step S411, then step S412, but the process may be performed in the order of step S412, then step S411.

[0061] FIG. 8 is a flowchart of the second connection step. FIG. 9 shows the procedure of the second connection step.

[0062] Step S421: The Nb alloy strip 110a is exposed from the other end of the connection strip 120 where the Nb alloy strip 110a is covered with the first stabilizing material 210. Step S421 may be the same exposure method as step S411. The exposed length is preferably in the range of 10 mm to 30 mm. In this range, when bundling with the NbTi core material 160 described later, good superconducting properties can be obtained due to sufficient contact. The exposed length is more preferably in the range of 15 mm to 25 mm. Here, the other end of the connection strip 120 is exposed from the other end of the Nb alloy strip 110a covered with the first stabilizing material 210 by the above-mentioned first connection step. 3 It is joined to the Sn superconducting wire 130 .

[0063] Step S422: The NbTi core material 160 is exposed from one end of the NbTi wire 140. The method of exposure is not particularly limited, but may be chemical corrosion, mechanical polishing, or a combination of these. The exposed length is preferably in the range of 10 mm to 30 mm. In this range, when bundling with the Nb alloy strip 110a exposed in step S421, sufficient contact is achieved to obtain good superconducting properties. The exposed length is more preferably in the range of 15 mm to 25 mm.

[0064] Step S423: The exposed Nb alloy strips 110a and the exposed NbTi core material 160 are bundled together. There is no limitation on the method of bundling, and they may be combined, twisted, entangled, wrapped around, or the like.

[0065] Step S424: The Nb alloy strips and the NbTi core material bundled in step S423 are pressed together. The pressing is performed by applying pressure to the bundled Nb alloy strips 110a and the NbTi core material 160, exposing their newly formed surfaces, and bonding them together. This allows the Nb alloy strips and the NbTi core material to be bonded together at their newly formed surfaces.

[0066] Preferably, the bundled portion is covered with a crimping tube 180, and then pressure is applied in a direction perpendicular to the longitudinal direction of the bundled Nb alloy strips 110a and NbTi core material 160 to crimp them. This allows the newly formed surfaces to adhere to each other. The pressure to be applied is preferably in the range of 100 MPa to 1 GPa. This range can promote adhesion between the newly formed surfaces. The pressure to be applied is more preferably in the range of 300 MPa to 500 MPa. This range can promote adhesion between the newly formed surfaces without breaking the wire. In this manner, the superconducting connection structure 100 of the present invention is obtained.

[0067] The present invention will now be described in detail with reference to specific examples, but it should be noted that the present invention is not limited to these examples. EXAMPLES

[0068] [Reference example] The change in the critical current characteristics before and after heat treatment of an NbTi wire (National Bureau of Standards (NBS) standard sample) with a wire diameter of 0.5 mm and 180 NbTi cores embedded in a Cu base material was investigated. The heat treatment conditions were 685°C in a vacuum for 100 hours. The Ti composition in the NbTi core was 60at%. The wire was immersed in liquid helium, and the critical current was measured when an external magnetic field was applied. The results are shown in Figure 10.

[0069] FIG. 10 is a diagram showing the critical current characteristics of the NbTi wire before and after the heat treatment.

[0070] According to Fig. 10, the critical current of the NbTi wire before heat treatment was high, but the Nb3 Heat treatment exceeding 600°C, which corresponds to the Sn formation temperature, caused the critical magnetic field of the NbTi wire to drop sharply, and the critical current also dropped. The critical current of the NbTi wire after heat treatment was less than 100A, even in a magnetic field of 0.2T. This is because the heat treatment causes the nanostructures, such as dislocation cells, in the NbTi core material to disappear, and the nanoscale ribbon-like α-Ti that acts as the flux pinning points to aggregate, causing the flux pinning force to be lost. As a result, the critical current drops.

[0071] Next, we investigated the change in critical current before and after heat treatment of Nb alloy wires with 19 cores of Nb-2at%Hf and Nb-4at%Ta-1at%Hf embedded in Cu matrix with a linear length of 1 mm. The Nb alloy wires were manufactured as follows.

[0072] Nb-2at%Hf alloy and Nb-4at%Ta-1at%Hf alloy produced by arc melting were processed into rods of just under 6 mm by swaging, and inserted into Cu tubes with outer / inner diameters of 8mm / 6mm, respectively. These were then subjected to swaging and die drawing to produce Cu / Nb-Hf single-core wires and Cu / Nb-Ta-Hf single-core wires with outer diameters of 1mm. Next, 19 of these single-core wires were bundled together, inserted into a Cu tube with outer / inner diameters of 7.5mm / 5.1mm, and again subjected to swaging and die drawing to prepare Cu / Nb-Hf wires and Cu / Nb-Ta-Hf wires with outer diameters of 1mm.

[0073] The change in the critical current characteristics of Cu / Nb-Hf wire and Cu / Nb-Ta-Hf wire before and after heat treatment was investigated. The heat treatment conditions were in vacuum at 685°C for 100 hours. The results are shown in Figure 11.

[0074] Fig. 11 is a diagram showing the critical current characteristics before and after the heat treatment of the Nb-Ta-Hf wire (Nb-4at%Ta-1at%Hf wire). In Fig. 11, the Nb-Ta-Hf wire is called Nb-4Ta-1Hf. Note that the critical current characteristics before and after the heat treatment of the Nb-Hf wire are not shown.

[0075] According to Fig. 11, the critical current of the Nb-Ta-Hf wire is 3 Even after heat treatment exceeding 600°C, which corresponds to the Sn generation temperature, the critical current only decreased slightly, and a high critical current was still maintained even at 0.5 T. Although not shown in the figure, it was confirmed that the Nb-Hf wire also maintained a high critical current at 0.8 T after heat treatment. In this way, the Nb alloy wire to which elements such as Hf and Ta are added as M elements has an increased Nb recovery temperature and recrystallization temperature, so that the Nb 3 It was found that the high critical current was maintained even after heat treatment above the Sn formation temperature. This shows that the Nb alloy with the M element added has a high critical current. 3 It was shown to be effective for connecting strips with Sn superconducting precursor wires.

[0076] In addition, as shown in Fig. 4, Nb 3 The connecting strip and Nb, which require heat treatment above the Sn formation temperature, 3 It was shown that it is essential to perform the connection with the Sn superconducting precursor wire (step S410) and then the connection strip and the NbTi wire (step S420) in that order.

[0077] [Example 1] In Example 1, the Nb-Ta-Hf (specifically, Nb-4 at% Ta-1 at% Hf) wire used in the reference example was used as the connection strip, and Nb 3 A superconducting joint structure was produced by joining a Sn superconducting wire and a NbTi wire.

[0078] Nb 3 The Sn precursor wire has a structure in which Nb cores are embedded in a base material in which Cu and Sn are separated, as shown in Figure 5(B). 3 A Sn precursor wire was prepared. A diffusion barrier layer made of Nb was provided between the region containing Cu, Sn, and Nb and the outermost Cu. The composition of Sn in the base material was 14 at%, the Nb core diameter was 11 μm, and the thickness of the diffusion barrier layer was 15 μm. The NbTi wire was the same as the NbTi wire used in the reference example.

[0079] The Nb-Ta-Hf wire as a connecting strip, and the Nb 3 The Nb-Ta-Hf wire was connected to a Sn superconducting wire (step S410 in FIG. 4). Specifically, the Nb-Ta-Hf wire was cut to a length of 8 cm, and the Nb-Ta-Hf core material was exposed from one end as a Nb alloy strip (step S411 in FIG. 6 and FIG. 7). A 15 mm portion of the end of the Nb-Ta-Hf wire was immersed in nitric acid to remove the Cu (copper) base material used as a stabilizing material. Next, the Nb 3 The Nb core material was exposed from one end of the Sn superconducting precursor wire (step S412 in FIG. 6 and FIG. 7). 3 The outermost Cu was removed from the end of the Sn superconducting precursor wire at a length of 15 mm using nitric acid, and the diffusion barrier layer was then mechanically polished with sandpaper to remove it. It was confirmed that the Cu and Sn base materials around the Nb core were not completely removed.

[0080] Next, the exposed Nb-Ta-Hf core material and the exposed Nb core material were bundled by twisting them together (step S413 in Fig. 6 and Fig. 7). The bundled portion was crimped (step S414 in Fig. 6 and Fig. 7). The bundled portion was inserted into a tantalum (Ta) tube with an outer diameter / inner diameter of 3.6 mm / 2.5 mm as a crimping tube, and a pressure of 400 MPa was applied using a hydraulic press. Next, the Nb-Ta-Hf wire material including the crimped portion and the Nb 3 The Nb superconducting precursor wire was heat-treated (FIG. 6, step S415 in FIG. 7). The heat treatment conditions were 390° C., 100 hours in a vacuum, and then 685° C., 100 hours. 3 The Nb superconducting precursor wire is 3 The Nb-Ta-Hf wire and the Nb 3 Sn superconducting wire and Nb 3 The connection was made via a Sn superconducting layer.

[0081] Next, the other end of the Nb-Ta-Hf wire was connected to the NbTi wire having an NbTi core (step S420 in FIG. 4). Specifically, the Nb-Ta-Hf core was exposed from the other end of the Nb-Ta-Hf wire (step S421 in FIG. 8 and FIG. 9). The end of the Nb-Ta-Hf wire, 20 mm long, was immersed in nitric acid to remove the Cu base material (third stabilizing material). Next, the NbTi core was exposed from one end of the NbTi wire (step S422 in FIG. 8 and FIG. 9). The end of the NbTi wire, 20 mm long, was immersed in nitric acid to remove the Cu base material.

[0082] Next, the exposed Nb-Ta-Hf core material and the exposed NbTi core material were bundled by twisting them together (step S423 in FIG. 8 and FIG. 9). The bundled part was crimped (step S424 in FIG. 8 and FIG. 9). The bundled part was inserted into a tantalum (Ta) tube with an outer diameter / inner diameter of 3.6 mm / 2.5 mm as a crimping tube, and a pressure of 400 MPa was applied using a hydraulic press. In this way, the Nb-Ta-Hf wire material and the NbTi wire material were connected by bringing their newly formed surfaces into close contact with each other. A superconducting connection structure was obtained using the connection strip obtained in this way.

[0083] The superconducting joint structure of Example 1 was observed and element mapping was examined using a scanning electron microscope (SEM, manufactured by JEOL Ltd.) equipped with an energy dispersive X-ray analyzer (EDS). The results are shown in FIG.

[0084] FIG. 12 shows the connection strips of the superconducting connection structure and the Nb 3 FIG. 2 is a diagram showing the results of electron microscope observation of a cross section of a joint portion with a Sn superconducting wire.

[0085] According to FIG. 12(A), it can be seen that the core material is tightly adhered to the connection part by the crimping (step S414 in FIG. 6). According to FIG. 12(C), Nb 3 Nb in Sn superconducting wire 3 The Sn superconducting core material is a multifilamentary wire, in close contact with each other, and the Nb-Ta-Hf core material of the connecting strip and the Nb 3 It was found that the Sn superconducting core material was in close contact with the material.

[0086] According to Fig. 12(B) and (C), the Nb-Ta-Hf core material and the Nb 3 Sn superconducting core material is Nb 3 Sn superconducting layer (in the figure, Nb 3 It was found that the contact was made via the Sn layer.

[0087] The critical current characteristics of the superconducting joint structure of Example 1 were examined in the same manner as in the reference example, and the results are shown in FIG. FIG. 13 is a diagram showing the critical current characteristics of the superconducting joint structure of Example 1. In FIG. 13, the superconducting joint structure (NbTi-Nb-4at%Ta-1at%Hf-Nb 3 Sn superconducting joint structure) 3 This is called a Sn superconducting joint structure. 13, the superconducting joint structure of Example 1 exhibited a high critical current exceeding 150 A even when 0.55 T was applied. This shows that the superconducting joint structure of Example 1 can maintain high superconducting properties without using environmentally hazardous substances such as Pb and Cd. 3 It was confirmed that a superconducting connection structure between a Sn superconducting wire and a NbTi wire was provided.

[0088] [Example 2] In Example 2, a superconducting junction structure was manufactured in the same manner as in Example 1, except that the Nb-Hf (Nb-2at%Hf) wire used in the reference example was used as the connection strip. The superconducting junction structure of Example 2 was observed by SEM to examine the critical current characteristics. The results are shown in FIG.

[0089] FIG. 14 is a diagram showing the critical current characteristics of the superconducting joint structure of Example 2. In FIG. 14, the superconducting joint structure (NbTi—Nb-2at%Hf—Nb 3 Sn superconducting joint structure) 3 This is called a Sn superconducting joint structure.

[0090] 14, the superconducting joint structure of Example 2 exhibited a high critical current exceeding 150 A even when a higher magnetic field (0.9 T) was applied than the superconducting joint structure of Example 1. Although not shown, SEM observation showed that the Nb-Hf core material and the Nb 3 Sn superconducting core material and Nb 3 It was confirmed that the contact was made via the Sn superconducting layer. This confirmed that the Nb 3 It was confirmed that a superconducting joint structure between a Sn superconducting wire and a NbTi wire was provided. It was also shown that Hf is preferable as the M element. [Industrial Applicability]

[0091] According to the present invention, Nb 3 The connection structure of Sn superconducting wire and NbTi wire is connected without using environmentally harmful substances such as Pb and Cd, has excellent properties, and can be used in a magnetic field environment of 0.5T to 1.0T, so it is used as a superconducting connection for nuclear magnetic resonance (NMR) magnets. [Explanation of symbols]

[0092] 100 Superconducting joint structure 110 Nb alloy strip 110a core material 110b sheet 110c pipe 120 Connection Strips 130 Nb 3 Sn superconducting wire 140 NbTi wire 150 Nb 3 Sn superconducting core material 160 NbTi core material 170 Nb 3 Sn superconducting layer 180 Crimp tube 210 First Stabilizer 310 Secondary Stabilizer 320, 530 Diffusion Barrier Layer 330 Third Stabilizer 500a, 500b Nb3 Sn superconducting precursor wire 510 Nb core material 520a Cu-Sn base material 520b Cu base material 540 Stabilizing material 550 Sn base material

Claims

1. a connecting strip having an Nb alloy strip with an added M element, said M element being an element that increases the recovery and recrystallization temperatures of Nb; Nb 3 Nb with Sn superconducting core 3 A Sn superconducting wire; NbTi wire having a NbTi core material; Equipped with One end of the connecting strip is connected to the Nb alloy strip and the Nb 3 Sn superconducting core material and Nb 3 The Nb 3 It is connected to a Sn superconducting wire, A superconducting connection structure, wherein the other end of the connection strip is connected to the NbTi wire by contacting a fresh surface of the Nb alloy strip with a fresh surface of the NbTi core material.

2. 2. The superconducting connection structure according to claim 1, wherein the M element is at least one selected from the group consisting of hafnium (Hf), titanium (Ti), tantalum (Ta), zirconium (Zr), and tungsten (W).

3. 2. The superconducting connection structure according to claim 1, wherein the Nb alloy strip is in any one shape selected from the group consisting of a core material, a sheet, and a pipe.

4. 2. The superconducting connection structure according to claim 1, wherein the M element is added in an amount ranging from 0.2 at % to 10 at %.

5. The Nb alloy strip and the Nb 3 Sn superconducting core material and Nb 3 2. The superconducting connection structure according to claim 1, wherein the contact portion via the Sn superconducting layer and the contact portion between the newly formed surface of the Nb alloy strip and the newly formed surface of the NbTi core material are each covered with a crimp tube made of at least one material selected from the group consisting of tantalum (Ta), niobium (Nb), copper-nickel alloy (CuNi), and stainless steel.

6. 6. The superconducting connection structure according to claim 5, wherein the length of the covered portion is in the range of 10 mm to 30 mm.

7. The connecting strip is formed by coating and / or embedding the Nb alloy strip with a first stabilizing material, The Nb 3 The Sn superconducting wire is 3 The Sn superconducting core material is covered and / or embedded in a second stabilizing material, The NbTi wire is formed by covering and / or embedding the NbTi core material with a third stabilizing material, 2. The superconducting connection structure according to claim 1, wherein each of the first to third stabilizing materials is at least one metal selected from the group consisting of copper metal, copper alloy, silver metal, and silver alloy.

8. One end of a connecting strip having an Nb alloy strip with an added M element, where the M element is an element that increases the recovery temperature and recrystallization temperature of Nb, and 3 Nb with Sn superconducting core 3 a first connecting step of connecting the Sn superconducting wire; a second connecting step of connecting the other end of the connecting strip to a NbTi wire having a NbTi core; Inclusive of The first connecting step includes: exposing the Nb alloy strip from one end of the connecting strip; The Nb core material is embedded in a base material containing at least Cu and Sn. 3 exposing the Nb core material from one end of the Sn superconducting precursor wire; bundling the exposed Nb alloy strip and the exposed Nb core; crimping the bundled Nb alloy strips and the Nb core; The Nb alloy strip and the Nb core material-containing connecting strip and the Nb alloy strip are joined together. 3 A step of heat treating the Sn superconducting precursor wire; Inclusive of The second connecting step includes: exposing the Nb alloy strip from the other end of the connecting strip; exposing the NbTi core material from one end of the NbTi wire; bundling the exposed Nb alloy strip and the exposed NbTi core; crimping the bundled Nb alloy strips and the NbTi core; A method for producing the superconducting connection structure according to any one of claims 1 to 7, comprising:

9. 9. The method of claim 8, wherein the step of exposing the Nb alloy strip in the first and second connecting steps uses chemical etching.

10. The method of claim 8 , wherein the step of exposing the Nb core in the first connecting step uses chemical etching.

11. The method according to claim 10 , wherein the step of exposing the Nb core material in the first connecting step further comprises mechanical polishing.

12. The method of claim 8 , wherein the step of exposing the NbTi core in the second connecting step uses chemical etching.

13. 9. The method according to claim 8, wherein the steps of exposing the Nb alloy strip in the first connecting step and the second connecting step, exposing the Nb core material in the first connecting step, and exposing the NbTi core material in the second connecting step each expose a length in the range of 10 mm or more and 30 mm or less.

14. The method according to claim 8, wherein the pressing step in the first connecting step exposes the new surfaces of the Nb alloy strip and the Nb core material, and brings the new surfaces of the Nb alloy strip and the new surfaces of the Nb core material into close contact with each other.

15. 15. The method according to claim 14, wherein the crimping step in the first connecting step is to cover the bundled Nb alloy strips and the Nb core material with a crimping tube made of at least one material selected from the group consisting of tantalum (Ta), niobium (Nb), copper-nickel alloy (CuNi), and stainless steel, and apply pressure in a direction perpendicular to the longitudinal direction of the bundled Nb alloy strips and the Nb core material.

16. The method of claim 15, wherein the pressure is in the range of 100 MPa to 1 GPa.

17. The heat treatment step in the first connecting step is performed by subjecting the connecting strip and the Nb 3 The method according to claim 8, wherein the Sn superconducting precursor wire is heat-treated in a vacuum or in an inert gas atmosphere at a temperature in the range of 600° C. to 800° C.

18. The heat treatment step in the first connecting step is performed by subjecting the connecting strip and the Nb 3 The method according to claim 17, wherein the Sn superconducting precursor wire is heat-treated in a vacuum or in an inert gas atmosphere at a temperature range of 300° C. to 500° C. for 50 hours to 150 hours, and then at a temperature range of 600° C. to 800° C. for 50 hours to 150 hours.

19. The method according to claim 8, wherein the pressing step in the second connecting step exposes the new surfaces of the Nb alloy strip and the NbTi core material, and brings the new surfaces of the Nb alloy strip and the new surfaces of the Nb core material into close contact with each other.

20. 20. The method according to claim 19, wherein the crimping step in the second connecting step is to cover the bundled Nb alloy strips and the NbTi core material with a crimping tube made of a material selected from the group consisting of tantalum (Ta), niobium (Nb), copper-nickel alloy (CuNi), and stainless steel, and apply pressure in a direction perpendicular to the longitudinal direction of the bundled Nb alloy strips and the NbTi core material.

21. 21. The method of claim 20, wherein the pressure is in the range of 100 MPa to 1 GPa.

22. A nuclear magnetic resonance apparatus comprising the superconducting connection structure according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Superconducting joint of niobium-tin superconducting wire and niobium-titanium superconducting wire and preparation method of superconducting joint

    CN111243818A

  • Different kind superconducting wire connecting method

    JP1994005345A

  • Nb3sn superconductive wire material

    JP1996138460A

  • Superconducting connection structure and manufacturing method of the same

    JP2004193019A