Ternary cathode material coated with nitride / graphitized carbon nanosheets and its manufacturing method
The in-situ formation of graphitized carbon nanosheets during nitride coating addresses the complexity and lattice damage issues of existing methods, resulting in improved rate characteristics and cycle stability for ternary cathode materials.
Patent Information
- Application Number
- JP2023565576
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-10-29
- Filing Date
- 2022-07-28
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2042-07-28
AI Technical Summary
The existing vapor deposition coating method for ternary positive electrode materials is complicated, and the one-step mixed sintering method damages the lattice structure, affecting material performance.
A method involving a ternary positive electrode material coated with nitride/graphitized carbon nanosheets, where graphitized carbon is formed in situ during the nitride coating process, using a process that includes wet coating, mixing, sintering, and sieving to create a dense conductive network.
The method results in improved rate characteristics and cycle stability with a simple process flow suitable for industrial production, enhancing the electrical properties of the ternary cathode material.
Abstract
Description
[Technical field]
[0001] The present invention relates to the technical field of lithium batteries, in particular to a ternary positive electrode material coated with nitride / graphitized carbon nanosheets and a method for preparing the same. [Background technology]
[0002] Lithium-ion batteries, as a new type of energy storage and conversion device, have been widely used in portable consumer electronics, new energy vehicles, energy storage grids and other fields due to their advantages such as high working voltage, high energy density, high Coulombic efficiency, no memory effect, long cycle life and environmental friendliness. The positive electrode material of lithium-ion batteries determines the overall performance of the battery. Among the currently mainstream positive electrode materials, the ternary positive electrode material LiNi x Co y M 1-x-y O2 (M=Mn or Al) has been the focus of research due to its high energy / power density and low temperature performance.
[0003] With the increase of Ni content in the ternary material, the material capacity increases, but the bond energy of Ni-O bond weakens and the stability of crystal structure deteriorates, resulting in poor structural stability. In particular, during the charge and discharge process, the oxidation-reduction reaction between the highly active interface and the electrolyte generates an inactive rock salt phase structure, and the electrolyte decomposes and releases a large amount of heat at the same time, which causes a series of problems such as gas expansion of the cell, deterioration of safety performance, attenuation of discharge capacity, and deterioration of cycle stability. At present, one of the main technical means to solve this problem is coating, which can not only effectively avoid the direct contact between the highly active positive electrode interface and the electrolyte to reduce the occurrence of side reactions, but also function as a fast ionic conductor to provide a good channel for the diffusion and transmission of lithium ions, thereby further improving the rate characteristics. At present, the coating agents are mainly oxides such as Al2O3, TiO2, ZrO2, B2O3, and SiO2, and this oxide coating agent can improve the above-mentioned interface stability problem, but most of the oxides belong to semiconductors and have low electronic conductivity, which cannot meet the requirements of large current charging and discharging. Compared with oxides, nitrides have superior chemical corrosion resistance, electronic conductivity, and thermal stability, and can be used as coatings to maximize the electrical properties of ternary materials.
[0004] Among the currently existing nitride coating technologies, as disclosed in Chinese Patent Application Publication No. CN113097459A, a vapor deposition coating method is used, but its vapor phase reaction process is complicated and difficult to mass-produce. In the method disclosed in Chinese Patent Application Publication No. CN112174222A, the ternary positive electrode material to be coated, the titanium source, and the nitrogen-containing compound are mixed and sintered in one step to produce a ternary positive electrode material coated with titanium nitride. This method has a simple process and is easy for industrial production, but during the manufacturing process, the reducing gas of the nitrogen-containing compound may directly react with the ternary material, which will destroy the lattice structure of the main material of the ternary positive electrode and affect the electrical properties of the material. Summary of the Invention [Problem to be solved by the invention]
[0005] In view of the above, it is necessary to provide a ternary positive electrode material coated with nitride / graphitized carbon nanosheets and a method for producing the same, which solves the technical problems that the process flow of the vapor deposition coating method in the prior art is complicated and the one-step mixing and sintering method is prone to destroying the lattice structure of the main material of the ternary positive electrode, thereby affecting the material performance. [Means for solving the problem]
[0006] A first aspect of the present invention provides a ternary positive electrode material comprising a ternary positive electrode material substrate and a coating layer, the coating layer being composed of a nitride and graphitized carbon, the graphitized carbon being coated with nitride / graphitized carbon nanosheets formed in situ during the nitride coating process.
[0007] A second aspect of the present invention provides a method for producing a ternary cathode material coated with nitride / graphitized carbon nanosheets, comprising: Providing a ternary positive electrode material substrate; A step of obtaining an intermediate product by wet coating a surface of a ternary positive electrode material substrate with one or more coating elements selected from Al, Si, Ti, Zr, Ta, and Nb; uniformly mixing the intermediate product with the carbon-nitrogen-containing compound, and sintering, grinding, sieving, and removing iron to obtain a ternary positive electrode material coated with nitride / graphitized carbon nanosheets. Effect of the Invention
[0008] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0009] In the present invention, in the process of coating the surface layer of a ternary positive electrode material with a nitride, a graphitized carbon layer structure is generated in situ. Compared with the physical mixing method, the carbon layer generated in situ is more closely connected to the substrate material and the conductive network is more dense, so that the rate performance of the material can be maximized. The ternary positive electrode material has excellent rate performance and cycle stability, and the manufacturing method thereof has a simple process flow and can be easily realized in industrial production. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] In order to clarify the object, technical means and advantages of the present invention, the present invention will be described in more detail with reference to the following examples. It should be understood that the specific examples described herein are only used for the purpose of explaining the present invention, and are not intended to limit the present invention.
[0011] The first aspect of the present invention provides a ternary positive electrode material comprising a ternary positive electrode material substrate and a coating layer, the coating layer being composed of nitride and graphitized carbon, the graphitized carbon being coated with nitride / graphitized carbon nanosheets formed in situ during the nitride coating process. Compared with amorphous carbon, the graphitized carbon material has better electrical conductivity, which further contributes to improving the rate characteristics.
[0012] In the present invention, the ternary positive electrode material substrate is one or more of nickel-cobalt-manganese ternary positive electrode materials or nickel-cobalt-aluminum ternary positive electrode materials, whose structural formula is LiNi x Co y M 1-x-y O2 (M=Mn or Al). In some particular embodiments of the invention, x≧0.8.
[0013] In the present invention, the nitride is one or more of aluminum nitride, silicon nitride, titanium nitride, zirconium nitride, tantalum nitride, and niobium nitride.
[0014] In the present invention, the coating layer has a thickness of 1 to 100 nm.
[0015] A second aspect of the present invention provides a method for producing a ternary cathode material coated with nitride / graphitized carbon nanosheets, comprising: S1: Providing a ternary positive electrode material substrate; S2: A step of obtaining an intermediate product by wet coating one or more coating elements selected from Al, Si, Ti, Zr, Ta, and Nb on the surface of the ternary positive electrode material substrate; S3: uniformly mixing the intermediate product and the carbon-nitrogen-containing compound, and sintering, grinding, sieving, and removing iron to obtain a ternary positive electrode material coated with nitride / graphitized carbon nanosheets.
[0016] In the present invention, the nitrogen element in the carbon / nitrogen-containing compound reacts with the transition metal oxide coated on the surface layer of the intermediate product under high temperature environment to generate transition metal nitride, while the carbon element generates graphitized carbon nanosheets in situ under the catalytic graphitization action of the transition metal, and finally forms a ternary positive electrode material coated with nitride / graphitized carbon nanosheets.
[0017] In the present invention, the step of providing a ternary positive electrode material substrate specifically includes uniformly mixing a ternary positive electrode material precursor and a lithium source, and then calcining, grinding and sieving to obtain a ternary positive electrode material substrate.
[0018] Further, the ternary positive electrode material precursor is one or more of oxides, hydroxides, and oxyhydroxides of nickel-cobalt-manganese or nickel-cobalt-aluminum, the lithium source is a mixture of one or more of lithium carbonate, lithium oxide, and lithium hydroxide, the molar ratio of the ternary positive electrode material precursor to the lithium source is 1:1 to 1.15, the ternary positive electrode material precursor and the lithium source are uniformly mixed in a high-speed mixer, the rotation speed of the high-speed mixer is 100 to 1500 rpm, and further 1000 rpm, the mixing treatment time is 0.5 to 5 hours, and further 1 hour, the firing is performed in an oxygen atmosphere, and the volume concentration of the oxygen atmosphere passed through is 99% or more, the firing temperature is 500 to 1200°C, and further 650 to 850°C, and further 750°C, and the firing time is 5 to 24 hours, and further 10 to 14 hours, and further 12 hours.
[0019] In addition, during the manufacturing process of the ternary positive electrode material substrate, a dopant is also added to improve the structural stability of the positive electrode material. For example, the dopant may be zirconium dioxide, aluminum trioxide, titanium dioxide, magnesium oxide, etc., but the present invention is not limited thereto. Furthermore, the molar ratio of the dopant to the ternary positive electrode material precursor is 0.0001-0.1:1.
[0020] In the present invention, the mass ratio of the coating element to the ternary positive electrode material substrate is 0.0001 to 0.005:1, preferably 0.0004 to 0.003:1, and more preferably 0.0008 to 0.001:1.
[0021] In the present invention, the wet coating step specifically includes: adding a ternary cathode material substrate to a first solvent to form a solution I; adding a compound containing a coating element to a second solvent to form a solution II; The method includes the steps of slowly adding solution II to solution I, maintaining the temperature constant to carry out the reaction, and obtaining an intermediate product by solid-liquid separation and drying.
[0022] Furthermore, the compound containing the coating element is an alkoxide containing the coating element. In some specific embodiments of the present invention, the compound containing the coating element is one or more of aluminum triethoxide, tetraethyl orthosilicate, tetrabutyl titanate, titanium isopropoxide, zirconium isopropoxide, tantalum pentaethoxide, niobium pentaethoxide, and the first solvent and the second solvent are one or more of water, methanol, ethanol, isopropyl alcohol, and ethylene glycol.
[0023] Furthermore, in solution I, the dosage ratio of the ternary positive electrode material substrate to the solvent is 1-20 g:100 ml, further 10-20 g:100 ml, and in solution II, the dosage ratio of the compound containing the coating element to the solvent is 0.01-10 g:100 ml, further 0.04-1 g:100 ml, further 0.1-0.6 g:100 ml, further 0.2 g:100 ml.
[0024] Furthermore, the temperature at which the reaction is carried out while maintaining the temperature constant is 30 to 80°C, and further 60°C, the time at which the reaction is carried out while maintaining the temperature constant is 0.5 to 5 hours, and further 1 to 2 hours, the drying temperature is 80 to 120°C, and the drying time is 5 to 20 hours.
[0025] In the present invention, the carbon-nitrogen-containing compound is one or more of amino acids, melamine, and urea. Furthermore, the mass ratio of the carbon-nitrogen-containing compound to the intermediate product is 5-20:100, and if the mass ratio is too high, the surface coating layer (nitride or graphitized carbon) will be too much, which will affect the material capacity, and if the mass ratio is too low, the coating layer will be too little, and the coating effect cannot be achieved, and it is further 6-17:100, and further 10:100. The carbon-nitrogen-containing compound and the intermediate product are uniformly mixed in a high-speed mixer, and the rotation speed of the high-speed mixer is 1000-4000 rpm, and further 2000 rpm, the mixing treatment time is 1-8 hours, and further 2 hours, and the sintering is carried out under the protection of an inert gas (such as argon gas or nitrogen gas), the sintering temperature is 500-1000 ° C, and further 800 ° C, and the sintering time is 3-12 hours, and further 6 hours.
[0026] <Example 1> (1) Nickel-cobalt-manganese hydroxide ternary positive electrode material precursor, Ni 0.83 Co 0.12 Mn 0.05 2500g of (OH), 240g of lithium hydroxide (LiOH·H2O), and 1.5g of zirconium dioxide nanoparticles (ZrO2) were weighed out, transferred to a high-speed mixer, and mixed at 1000 rpm for 1 hour, then removed. Then, transferred to a muffle furnace for firing and sintering at 750℃ in an oxygen atmosphere for 12 hours. After the sintering was completed, the material was removed, crushed, and sieved to obtain a ternary positive electrode material substrate.
[0027] (2) 400 g of the ternary positive electrode material substrate is weighed and transferred to 3000 ml of ethanol solvent to form solution I. 2 g of titanium isopropoxide coating agent is weighed and transferred to 1000 ml of ethanol solvent to form solution II. After stirring each solution for 10 minutes, solution II is slowly added to solution I, stirring is continued, the water bath is heated to 60 ° C, the temperature is kept constant for 1 hour, the mixed solution is press filtered, and a filter cake is obtained by solid-liquid separation. It is then transferred to the inside of a 100 ° C oven to dry, and the temperature is kept constant for 10 hours to obtain a dried intermediate product.
[0028] (3) 300 g of the intermediate product and 30 g of melamine are weighed and mixed, then transferred to a high-speed mixer and stirred at high speed at 2000 rpm for 2 hours, and then transferred to a muffle furnace in an argon gas atmosphere and sintered at 800°C for 6 hours in an argon gas atmosphere. After sintering is complete, the resulting material is crushed, sieved, and iron is removed to finally produce a ternary positive electrode material coated with nitride / graphitized carbon nanosheets.
[0029] Button cell testing: The obtained nitride / graphitized carbon nanosheet-coated ternary cathode material (LiNi 0.83 Co 0.12 Mn 0.05), acetylene black, and PVDF were mixed in a ratio of 94:4:4, and NMP was used as a solvent to mix uniformly. The mixture was then applied to aluminum foil to produce a 2032 button battery, which was then subjected to electrochemical performance testing. The test voltage range was 2.8~4.3V, and the first cycle was charged and discharged at 0.1C / 0.1C, and then cycle testing was performed at 1C / 1C for 50 cycles. Final test results: 0.1C discharge capacity was 210mAh / g, 1C discharge capacity was 199mAh / g, and the cycle capacity retention rate for 50 cycles was 98.6%.
[0030] <Example 2> (1) Nickel-cobalt-manganese hydroxide ternary positive electrode material precursor, Ni 0.83 Co 0.12 Mn 0.05 2500g of (OH), 240g of lithium hydroxide (LiOH·H2O), and 1.5g of zirconium dioxide nanoparticles (ZrO2) were weighed out, transferred to a high-speed mixer, and mixed at 1000 rpm for 1 hour, then removed. Then, transferred to a muffle furnace for firing and sintering at 750℃ in an oxygen atmosphere for 12 hours. After the sintering was completed, the material was removed, crushed, and sieved to obtain a ternary positive electrode material substrate.
[0031] (2) 400 g of the ternary positive electrode material substrate is weighed and transferred to 3000 ml of ethanol solvent to form solution I. 0.4 g of titanium isopropoxide coating agent is weighed and transferred to 1000 ml of ethanol solvent to form solution II. After stirring each solution for 10 minutes, solution II is slowly added to solution I, stirring is continued, the water bath is heated to 60 ° C, the temperature is kept constant for 1 hour, the mixed solution is press filtered, and a filter cake is obtained by solid-liquid separation. Then, it is transferred to the inside of a 100 ° C oven to dry, and the temperature is kept constant for 10 hours to obtain a dried intermediate product.
[0032] (3) 300 g of the intermediate product and 15 g of melamine are weighed and mixed, then transferred to a high-speed mixer and stirred at high speed at 2000 rpm for 2 hours, and then transferred to a muffle furnace in an argon gas atmosphere and sintered at 800°C for 6 hours in an argon gas atmosphere. After sintering is complete, the resulting material is crushed, sieved, and iron is removed to finally produce a ternary positive electrode material coated with nitride / graphitized carbon nanosheets.
[0033] Button cell testing: The obtained nitride / graphitized carbon nanosheet-coated ternary cathode material (LiNi 0.83 Co 0.12 Mn 0.05 ), acetylene black, and PVDF were mixed in a ratio of 94:4:4, and NMP was used as a solvent to mix uniformly. The mixture was then applied to aluminum foil to produce a 2032 button battery, which was then subjected to electrochemical performance testing. The test voltage range was 2.8~4.3V, and the first cycle was charged and discharged at 0.1C / 0.1C, and then cycle testing was performed at 1C / 1C for 50 cycles. Final test results: 0.1C discharge capacity was 208mAh / g, 1C discharge capacity was 194mAh / g, and the cycle capacity retention rate for 50 cycles was 93.7%.
[0034] <Example 3> (1) Nickel-cobalt-manganese hydroxide ternary positive electrode material precursor, Ni 0.83 Co 0.12 Mn 0.05 2500g of (OH), 240g of lithium hydroxide (LiOH·H2O), and 1.5g of zirconium dioxide nanoparticles (ZrO2) were weighed out, transferred to a high-speed mixer, and mixed at 1000 rpm for 1 hour, then removed. Then, transferred to a muffle furnace for firing and sintering at 750℃ in an oxygen atmosphere for 12 hours. After the sintering was completed, the material was removed, crushed, and sieved to obtain a ternary positive electrode material substrate.
[0035] (2) 400 g of the ternary positive electrode material substrate is weighed and transferred to 3000 ml of ethanol solvent to form solution I. 1 g of titanium isopropoxide coating agent is weighed and transferred to 1000 ml of ethanol solvent to form solution II. After stirring each solution for 10 minutes, solution II is slowly added to solution I, stirring is continued, the water bath is heated to 60 ° C, the temperature is kept constant for 2 hours, the mixed solution is press filtered, and a filter cake is obtained by solid-liquid separation. Then, it is transferred to the inside of a 100 ° C oven to dry, and the temperature is kept constant for 10 hours to obtain a dried intermediate product.
[0036] (3) 300 g of the intermediate product and 20 g of melamine are weighed and mixed, then transferred to a high-speed mixer and stirred at high speed at 2000 rpm for 2 hours, and then transferred to a muffle furnace in an argon gas atmosphere and sintered at 800°C for 6 hours in an argon gas atmosphere. After sintering is complete, the resulting material is crushed, sieved, and iron is removed to finally produce a ternary positive electrode material coated with nitride / graphitized carbon nanosheets.
[0037] Button cell testing: The obtained nitride / graphitized carbon nanosheet-coated ternary cathode material (LiNi 0.83 Co 0.12 Mn 0.05 ), acetylene black, and PVDF were mixed in a ratio of 94:4:4, and NMP was used as a solvent to mix uniformly. The mixture was then applied to aluminum foil to produce a 2032 button battery, which was then subjected to electrochemical performance testing. The test voltage range was 2.8~4.3V, and the first cycle was charged and discharged at 0.1C / 0.1C, and then cycle testing was performed at 1C / 1C for 50 cycles. Final test results: 0.1C discharge capacity was 209mAh / g, 1C discharge capacity was 196mAh / g, and the cycle capacity retention rate for 50 cycles was 97.9%.
[0038] <Example 4> (1) Nickel-cobalt-manganese hydroxide ternary positive electrode material precursor, Ni 0.83 Co 0.12 Mn 0.052500g of (OH), 240g of lithium hydroxide (LiOH·H2O), and 1.5g of zirconium dioxide nanoparticles (ZrO2) were weighed out, transferred to a high-speed mixer, and mixed at 1000 rpm for 1 hour, then removed. Then, transferred to a muffle furnace for firing and sintering at 750℃ in an oxygen atmosphere for 12 hours. After the sintering was completed, the material was removed, crushed, and sieved to obtain a ternary positive electrode material substrate.
[0039] (2) 400 g of the ternary positive electrode material substrate is weighed and transferred to 3000 ml of ethanol solvent to form solution I. 6 g of titanium isopropoxide coating agent is weighed and transferred to 1000 ml of ethanol solvent to form solution II. After stirring each solution for 10 minutes, solution II is slowly added to solution I, stirring is continued, the water bath is heated to 60 ° C, the temperature is kept constant for 2 hours, the mixed solution is press filtered, and a filter cake is obtained by solid-liquid separation. Then, it is transferred to the inside of a 100 ° C oven to dry, and the temperature is kept constant for 10 hours to obtain a dried intermediate product.
[0040] (3) 300 g of the intermediate product and 50 g of melamine are weighed and mixed, then transferred to a high-speed mixer and stirred at high speed at 2000 rpm for 2 hours, and then transferred to a muffle furnace in an argon gas atmosphere and sintered at 800°C for 6 hours in an argon gas atmosphere. After sintering is complete, the resulting material is crushed, sieved, and iron is removed to finally produce a ternary positive electrode material coated with nitride / graphitized carbon nanosheets.
[0041] Button cell testing: The obtained nitride / graphitized carbon nanosheet-coated ternary cathode material (LiNi 0.83 Co 0.12 Mn 0.05), acetylene black, and PVDF were mixed in a ratio of 94:4:4, and NMP was used as a solvent to mix uniformly. The mixture was then applied to aluminum foil to produce a 2032 button battery, which was then subjected to electrochemical performance testing. The test voltage range was 2.8~4.3V, and the first cycle was charged and discharged at 0.1C / 0.1C, and then cycle testing was performed at 1C / 1C for 50 cycles. Final test results: 0.1C discharge capacity was 207mAh / g, 1C discharge capacity was 193mAh / g, and the cycle capacity retention rate for 50 cycles was 97.4%.
[0042] <Example 5> (1) Nickel-cobalt-manganese hydroxide ternary positive electrode material precursor, Ni 0.83 Co 0.12 Mn 0.05 2500g of (OH), 240g of lithium hydroxide (LiOH·H2O), and 1.5g of zirconium dioxide nanoparticles (ZrO2) were weighed out, transferred to a high-speed mixer, and mixed at 1000 rpm for 1 hour, then removed. Then, transferred to a muffle furnace for firing and sintering at 750℃ in an oxygen atmosphere for 12 hours. After the sintering was completed, the material was removed, crushed, and sieved to obtain a ternary positive electrode material substrate.
[0043] (2) 400 g of the ternary positive electrode material substrate is weighed and transferred to 3000 ml of ethanol solvent to form solution I. 10 g of titanium isopropoxide coating agent is weighed and transferred to 1000 ml of ethanol solvent to form solution II. After stirring each solution for 10 minutes, solution II is slowly added to solution I, stirring is continued, the water bath is heated to 60 ° C, the temperature is kept constant for 2 hours, the mixed solution is press filtered, and a filter cake is obtained by solid-liquid separation. Then, it is transferred to the inside of a 100 ° C oven to dry, and the temperature is kept constant for 10 hours to obtain a dried intermediate product.
[0044] (3) 300 g of the intermediate product and 60 g of melamine are weighed and mixed, then transferred to a high-speed mixer and stirred at high speed at 2000 rpm for 2 hours, and then transferred to a muffle furnace in an argon gas atmosphere and sintered at 800°C for 6 hours in an argon gas atmosphere. After sintering is complete, the resulting material is crushed, sieved, and iron is removed to finally produce a ternary positive electrode material coated with nitride / graphitized carbon nanosheets.
[0045] Button cell testing: The obtained nitride / graphitized carbon nanosheet-coated ternary cathode material (LiNi 0.83 Co 0.12 Mn 0.05 ), acetylene black, and PVDF are mixed in a ratio of 94:4:4, and NMP is used as a solvent to mix uniformly. The mixture is then applied to aluminum foil to produce a 2032 button battery, which is then subjected to electrochemical performance testing. The test voltage range is 2.8~4.3V, and the first cycle is charged and discharged at 0.1C / 0.1C, and then cycle testing is performed at 1C / 1C for 50 cycles. Final test results: 0.1C discharge capacity is 198mAh / g, 1C discharge capacity is 176mAh / g, and the cycle capacity retention rate for 50 cycles is 97.5%.
[0046] <Comparative Example 1> (1) Nickel-cobalt-manganese hydroxide ternary positive electrode material precursor, Ni 0.83 Co 0.12 Mn 0.05 2500g of (OH), 240g of lithium hydroxide (LiOH·H2O), and 1.5g of zirconium dioxide nanoparticles (ZrO2) were weighed out, transferred to a high-speed mixer, and mixed at 1000 rpm for 1 hour, then removed. Then, transferred to a muffle furnace for firing and sintering at 750℃ in an oxygen atmosphere for 12 hours. After the sintering was completed, the material was removed, crushed, and sieved to obtain a ternary positive electrode material substrate.
[0047] (2) 400 g of the ternary positive electrode material substrate is weighed and transferred to 3000 ml of ethanol solvent to form solution I. 2 g of titanium isopropoxide coating agent is weighed and transferred to 1000 ml of ethanol solvent to form solution II. After stirring each solution for 10 minutes, solution II is slowly added to solution I, stirring is continued, the water bath is heated to 60 ° C, the temperature is kept constant for 1 hour, the mixed solution is press filtered, and a filter cake is obtained by solid-liquid separation. It is then transferred to the inside of a 100 ° C oven to dry, and the temperature is kept constant for 10 hours to obtain a dried intermediate product.
[0048] (3) 300 g of the intermediate product and 30 g of melamine are weighed and mixed, then transferred to a high-speed mixer and stirred at high speed at 2000 rpm for 2 hours, and then transferred to a muffle furnace in an oxygen atmosphere and sintered at 800°C in an oxygen atmosphere for 6 hours. After sintering is complete, the resulting material is crushed, sieved, and iron is removed to finally produce a ternary positive electrode material coated with nitride.
[0049] Button cell testing: The obtained nitride-coated ternary cathode material (LiNi 0.83 Co 0.12 Mn 0.05 ), acetylene black, and PVDF were mixed in a ratio of 94:4:4, and NMP was used as a solvent to mix uniformly. The mixture was then applied to aluminum foil to produce a 2032 button battery, which was then subjected to electrochemical performance testing. The test voltage range was 2.8~4.3V, and the first cycle was charged and discharged at 0.1C / 0.1C, and then cycle testing was performed at 1C / 1C for 50 cycles. Final test results: 0.1C discharge capacity was 206mAh / g, 1C discharge capacity was 190mAh / g, and the cycle capacity retention rate for 50 cycles was 97.0%.
[0050] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0051] (1) The process flow of the manufacturing method is simple, it is a pure solid-phase reaction process, the conditions are easy to control, and it is easy for large-scale industrial production.
[0052] (2) The whole coating process is divided into a wet pre-coating step and a subsequent high-temperature nitridation step. Compared with the one-time coating process, the pre-coating process can not only provide a precursor for the subsequent nitridation, but also protect the ternary positive electrode substrate material from the subsequent damage caused by the reducing gas containing carbon and nitrogen.
[0053] (3) The graphitized nanosheets are directly generated in situ through the catalytic action of transition metals, which leads to closer contact between the materials and more uniform distribution of the conductive carbon layer network compared with the physical mixing method, thus greatly improving the conductivity of the composite material and maximizing the rate capability of the ternary cathode material.
[0054] (4) As the nitrides are produced, a graphitized carbon coating layer is formed, improving both the ionic and electronic conductivity.
[0055] The above are merely preferred embodiments of the present invention, and the scope of protection of the present invention is not limited thereto. All modifications or replacements that can be easily thought of by those skilled in the art within the technical scope disclosed in the present invention should be included in the scope of protection of the present invention.
Claims
1. A ternary positive electrode material coated with a nitride / graphitized carbon nanosheet, comprising a ternary positive electrode material substrate and a coating layer, the coating layer being composed of a nitride and graphitized carbon, the graphitized carbon being formed in situ during a coating process of the nitride.
2. The nitride / graphitized carbon nanosheet-coated ternary positive electrode material according to claim 1, characterized in that the nitride is one or more of aluminum nitride, silicon nitride, titanium nitride, zirconium nitride, tantalum nitride, and niobium nitride, and the coating layer has a thickness of 1 to 100 nm.
3. The method for producing a ternary positive electrode material coated with a nitride / graphitized carbon nanosheet according to claim 1 or 2, Providing a ternary positive electrode material substrate; A step of obtaining an intermediate product by wet coating a surface of a ternary positive electrode material substrate with one or more coating elements selected from Al, Si, Ti, Zr, Ta, and Nb; and homogeneously mixing the intermediate product with a carbon / nitrogen-containing compound, and then sintering, grinding, sieving, and removing iron to obtain a ternary positive electrode material coated with a nitride / graphitized carbon nanosheet, wherein the sintering atmosphere is an inert gas.
4. The method for producing a ternary positive electrode material coated with a nitride / graphitized carbon nanosheet according to claim 3, characterized in that the mass ratio of the coating element to the ternary positive electrode material substrate is 0.0001-0.005:
1.
5. The wet coating step includes: adding a ternary cathode material substrate to a first solvent to form Solution I; adding a compound containing a coating element to a second solvent to form a solution II; The method for producing a ternary positive electrode material coated with nitride / graphitized carbon nanosheets according to claim 3, further comprising the steps of: slowly adding the solution II to the solution I, maintaining a constant temperature to carry out the reaction, and obtaining an intermediate product through solid-liquid separation and drying.
6. the compound containing a coating element is an alkoxide containing a coating element, The method for producing a ternary positive electrode material coated with a nitride / graphitized carbon nanosheet according to claim 5, wherein the first solvent and the second solvent are one or more of water, methanol, ethanol, isopropyl alcohol, and ethylene glycol.
7. The method for producing a ternary positive electrode material coated with a nitride / graphitized carbon nanosheet according to claim 5, characterized in that the temperature when the reaction is carried out while maintaining the temperature constant is 30 to 80°C, and the time when the reaction is carried out while maintaining the temperature constant is 0.5 to 5 hours.
8. The method for producing a ternary positive electrode material coated with a nitride / graphitized carbon nanosheet according to claim 3, characterized in that the carbon / nitrogen-containing compound is one or more of an amino acid, melamine, and urea.
9. The method for producing a ternary positive electrode material coated with a nitride / graphitized carbon nanosheet according to claim 3, wherein the mass ratio of the carbon / nitrogen-containing compound to the intermediate product is 5 to 20:
100.
10. The method for producing a ternary positive electrode material coated with a nitride / graphitized carbon nanosheet according to claim 3, characterized in that the sintering temperature is 500-1000°C, and the sintering time is 3-12 hours.
Citation Information
Patent Citations
Power-storage device
JP2015109227A
Electrode particles suitable for batteries
WO2021011647A1