Manufacturing method of ceramic green sheet

A release film with a specific composition and structure addresses the issue of deteriorating peelability in ceramic green sheets, ensuring stable and easy peeling, thereby enhancing the production of multilayer ceramic products.

JP7588282B1Active Publication Date: 2024-11-21MITSUI CHEM ICT MATERIA INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024555407
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-22
Publication Date
2024-11-21
Estimated Expiration
2044-03-22

AI Technical Summary

Technical Problem

Conventional methods for producing ceramic green sheets face issues with easy peelability deteriorating over time, leading to difficulties in peeling the sheets from the release film, which can result in defects such as pinholes and uneven thickness, especially in multilayer ceramic products.

Method used

A release film with a specific composition and structure, including a base material and a release agent layer, is used to maintain stable easy peelability over time. The release agent layer is formulated with a predetermined bromonaphthalene contact angle change and water contact angle change within specific ranges, ensuring consistent peeling performance.

Benefits of technology

The method enables easy and stable peeling of ceramic green sheets, reducing defects and improving productivity in multilayer ceramic products like capacitors and substrates, with minimal changes in peelability over extended periods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588282000002
    Figure 0007588282000002
  • Figure 0007588282000001
    Figure 0007588282000001
Patent Text Reader

Abstract

To provide a method for producing a ceramic green sheet using a release film for producing a ceramic green sheet having a substrate and a release agent layer, which allows easy peeling of the green sheet, and exhibits little change in peelability over time, so that excellent peelability can be stably achieved even after a long period of time has passed since the coating of the green sheet. The object is to provide a method for producing a ceramic green sheet, comprising: a) a step of applying a ceramic slurry onto a release film for producing a ceramic green sheet, b) a step of forming a ceramic green sheet from the ceramic slurry applied in the step a), and c) a step of peeling the ceramic green sheet formed in the step b) from the release film for producing a ceramic green sheet, wherein the release film for producing a ceramic green sheet has a substrate and a release agent layer provided on at least one side of the substrate, and the bromonaphthalene contact angle BCA1 of the surface of the release agent layer opposite to the substrate and the bromonaphthalene contact angle BCA2 of the surface of the release agent layer opposite to the substrate are: The problem is solved by the above-mentioned method for producing a ceramic green sheet, in which a ceramic slurry containing A) 45 mass% barium titanate particles, B) 3.6 mass% polyvinyl butyral, C) 0.9 mass% dibutyl phthalate, D) 25 mass% toluene, and E) 25 mass% ethanol is applied to the surface of the release agent layer opposite the substrate, dried, and then stored for one week in a constant temperature and humidity environment of 23±2°C x 50±5% RH. After peeling, the difference from the bromonaphthalene contact angle BCA2, δBCA=BCA2-BCA1, is within the range of -1.5° to 1.0°.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a release film for producing ceramic green sheets, and more specifically, to a method for producing ceramic green sheets which allows easy peeling of the green sheets, undergoes little change in peelability over time, and can stably achieve excellent peelability even long periods of time after the green sheet is applied, and is particularly suitable for use in producing various ceramic products such as multilayer ceramic capacitors and multilayer ceramic substrates. [Background technology]

[0002] In the manufacture of sheet-like ceramic members, a method for manufacturing a ceramic green sheet using a release film for manufacturing a ceramic green sheet has been conventionally adopted. For example, in the manufacture of multilayer ceramic products such as multilayer ceramic capacitors and multilayer ceramic substrates, a method is used in which a ceramic green sheet is formed on a release film for manufacturing a ceramic green sheet, and a plurality of the obtained ceramic green sheets are stacked and fired. In recent years, with the miniaturization and high performance of electronic devices, multilayer ceramic capacitors and multilayer ceramic substrates have become smaller and more multilayered. To achieve multilayering, ceramic green sheets are required to be thinner, and from the viewpoint of preventing defects such as pinholes and uneven thickness in thin ceramic green sheets and effectively suppressing breakage when thin ceramic green sheets are peeled off from a release film, a release film for producing ceramic green sheets has been proposed, which has a substrate and a release agent layer of a specific component, and in which the arithmetic mean roughness (Ra) and maximum projection height (Rp) on the surface of the release agent layer opposite the substrate are each equal to or less than a predetermined value, and the arithmetic mean roughness (Ra) and maximum projection height (Rp) on the surface of the substrate opposite the release agent layer are each within a predetermined numerical range (see, for example, Patent Document 1).

[0003] In the production of various ceramic products such as multilayer ceramic capacitors and multilayer ceramic substrates, it is required that the ceramic green sheet formed on the release film for producing the ceramic green sheet be easily peeled off from the standpoint of the quality and productivity of the ceramic products. However, in the conventional ceramic green sheet manufacturing methods, even if the ceramic green sheet is easy to peel immediately after it is formed by coating the slurry, the peelability may decrease, for example, when the sheet is stored for about one week after coating. In addition, the sheet may become difficult to peel due to storage, or the ceramic green sheet may break when peeled off after storage. Thus, improvements in this area were needed. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2013 / 145865 A1 Brochure Summary of the Invention [Problem to be solved by the invention]

[0005] In view of the above technical background, the present invention aims to provide a method for producing a ceramic green sheet using a release film for producing a ceramic green sheet having a base material and a release agent layer, which allows the green sheet to be easily peeled off, has little change in releasability over time, and can stably achieve excellent releasability even long periods of time have passed since the green sheet was applied. [Means for solving the problem]

[0006] As a result of intensive research, the inventors have found that in a release film for producing a ceramic green sheet having a substrate and a release agent layer provided on at least one side of the substrate, by using a release film for producing a ceramic green sheet in which the change in bromonaphthalene contact angle on the surface of the release agent layer before and after coating, drying, and peeling of a ceramic slurry of a predetermined composition is within a predetermined numerical range, and by applying this to a method for producing a ceramic green sheet having specific steps, it is possible to stabilize the easy releasability over time at a high level that exceeds the limits of conventional technology, and have thus completed the present invention. That is, the present invention provides: [1] a) applying a ceramic slurry onto a release film for producing a ceramic green sheet; b) forming a ceramic green sheet from the ceramic slurry applied in the a) step; and c) peeling the ceramic green sheet formed in the b) step from the release film for producing the ceramic green sheet; A method for producing a ceramic green sheet comprising the steps of: The release film for producing a ceramic green sheet has a base material and a release agent layer provided on at least one side of the base material, a bromonaphthalene contact angle BCA1 on the surface of the release agent layer opposite to the substrate; On the surface of the release agent layer opposite to the substrate A) 45% by weight of barium titanate particles, B) 3.6% by weight of polyvinyl butyral, C) 0.9% by mass of dibutyl phthalate, D) 25% by weight of toluene, and E) 25% ethanol by mass A ceramic slurry containing the above is coated, dried, and stored for one week in a constant temperature and humidity environment of 23±2°C x 50±5%RH, and then peeled off. The difference in contact angle between the ceramic slurry and bromonaphthalene BCA2, δBCA=BCA2-BCA1, is within the range of -1.5° to 1.0°. The present invention relates to a method for producing the ceramic green sheet.

[0007] Below, [2] to [7] are each a preferred aspect or embodiment of the present invention. [2] The method for producing a ceramic green sheet according to [1], wherein the coating amount of the ceramic slurry is 50 μm before drying, the drying conditions are 70° C. and 2 minutes, and the peeling is performed at an angle of 180°. [3] a water contact angle WCA1 of the surface of the release agent layer opposite to the substrate; The method for producing a ceramic green sheet according to [1] or [2], wherein the ceramic slurry is applied to a surface of the release agent layer opposite the substrate, the surface is dried, and the surface is stored in a constant temperature and humidity environment of 23±2°C x 50±5% RH for one week, after which the surface is peeled off. The difference between the water contact angle WCA2 and the water contact angle WCA1, δWCA=WCA2-WCA1, is within a range of -3.5° to 1.0°. [4] The method for producing a ceramic green sheet according to any one of [1] to [3], further comprising a step of printing internal electrodes on the ceramic green sheet between steps b) and c). [5] A method for producing a ceramic product, comprising the step of producing a ceramic green sheet by the method for producing a ceramic green sheet according to any one of [1] to [4]. [6] The method for producing a ceramic product according to [5], further comprising a step of firing the ceramic green sheet. [7] The method for producing a ceramic product according to [5] or [6], wherein the ceramic product is a multilayer ceramic capacitor or a multilayer ceramic substrate.

[0008] Furthermore, the following [4'] to [7'] are all examples of release films for producing ceramic green sheets that are preferably used in the present invention. [4'] A substrate and a release agent layer provided on at least one side of the substrate, a bromonaphthalene contact angle BCA1 on the surface of the release agent layer opposite to the substrate; On the surface of the release agent layer opposite to the substrate A) 45% by weight of barium titanate particles, B) 3.6% by weight of polyvinyl butyral, C) 0.9% by mass of dibutyl phthalate, D) 25% by weight of toluene, and E) 25% ethanol by mass A ceramic slurry containing the above is coated, dried, and stored for one week in a constant temperature and humidity environment of 23±2°C x 50±5%RH, and then peeled off. The difference in contact angle between the ceramic slurry and bromonaphthalene BCA2, δBCA=BCA2-BCA1, is within the range of -1.5° to 1.0°; a release agent layer comprising a cured product of a curable composition, the curable composition comprising at least one reactive compound (a) having at least one reactive functional group selected from the group consisting of a (meth)acryloyl group, a hydroxyl group, and an epoxy group, and the total amount of the reactive compound (a) is 50% or more by mass of the release agent layer. [5'] The release film for producing a ceramic green sheet according to [4'], wherein the curable composition contains, as the reactive compound (a), at least one reactive silicone (a1) having at least one reactive functional group selected from the group consisting of a (meth)acryloyl group, a hydroxyl group, and an epoxy group, and a siloxane skeleton, and at least one reactive compound (a2) having the same reactive functional group as the reactive silicone (a1) and having a reactive functional group equivalent of 2000 g / mol or less. [6'] The release film for producing a ceramic green sheet according to [5'], wherein the curable composition further contains a film-forming compound (a3) ​​having two or more (meth)acryloyl groups in one molecule. [7'] The release film for producing a ceramic green sheet according to any one of [4'] to [6'], wherein the arithmetic mean roughness (Ra) of the surface of the base material on the release agent layer side is 1 to 70 nm. Effect of the Invention

[0009] The method for producing a ceramic green sheet of the present invention realizes technical effects having high practical value at a high level that exceeds the limits of conventional techniques, such as easy peeling of a ceramic green sheet formed on a release film for producing a ceramic green sheet, small change in peelability over time, and stable excellent peelability even after a long period of time has passed since the green sheet was applied, and can be suitably used in the production of various ceramic products. For example, the productivity of various ceramic products such as multilayer ceramic capacitors and multilayer ceramic substrates is significantly improved, and the method can be particularly suitably used in the production of these products. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a schematic diagram showing one embodiment of a release film for producing a ceramic green sheet used in the production method of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention relates to a) applying a ceramic slurry onto a release film for producing a ceramic green sheet; b) forming a ceramic green sheet from the ceramic slurry applied in the a) step; and c) peeling the ceramic green sheet formed in the b) step from the release film for producing the ceramic green sheet; A method for producing a ceramic green sheet comprising the steps of: The release film for producing a ceramic green sheet has a base material and a release agent layer provided on at least one side of the base material, a bromonaphthalene contact angle BCA1 on the surface of the release agent layer opposite to the substrate; A ceramic slurry having the following composition is applied to the surface of the release agent layer opposite to the substrate, dried, and then stored for one week in a constant temperature and humidity environment of 23±2°C x 50±5%RH. After the layer is peeled off, the difference from the bromonaphthalene contact angle BCA2, δBCA=BCA2-BCA1, is within the range of -1.5° to 1.0°. A method for producing the ceramic green sheet. Here, the ceramic slurry is A) 45% by weight of barium titanate particles, B) 3.6% by weight of polyvinyl butyral, C) 0.9% by mass of dibutyl phthalate, D) 25% by weight of toluene, and E) A ceramic slurry containing 25% by weight of ethanol. That is, the release film for producing a ceramic green sheet used in the method for producing a ceramic green sheet of the present invention has a substrate and a release agent layer. The release film for producing a ceramic green sheet used in the method for producing a ceramic green sheet of the present invention only needs to have a substrate and a release agent layer, and may or may not have other layers. Therefore, the release film for producing a ceramic green sheet used in the method for producing a ceramic green sheet of the present invention may be composed of only a substrate (13) and a release agent layer (12) as shown in FIG. 1, or may have other layers such as an antistatic layer in addition to the substrate and the release agent layer. Each of the above layers will now be described.

[0012] Base material The substrate constituting the release film for producing ceramic green sheets used in the method for producing ceramic green sheets of the present invention is not particularly limited, and any substrate may be appropriately selected from those conventionally known as substrates in the technical field. Examples of such substrates include films made of plastics such as polyesters such as polyethylene terephthalate and polyethylene naphthalate, polyolefins such as polypropylene and polymethylpentene, polycarbonate, and ethylene-vinyl acetate copolymers, and may be a single layer or a multilayer of two or more layers of the same or different types. Among these, polyester films are preferred, polyethylene terephthalate films are particularly preferred, and biaxially stretched polyethylene terephthalate films are even more preferred. Polyethylene terephthalate films are less likely to generate dust during processing, use, etc., and therefore, for example, ceramic slurry coating defects due to dust, etc. can be effectively prevented.

[0013] In addition, this substrate may be subjected to a surface treatment such as an oxidation method or a primer treatment in order to improve adhesion to a release agent layer provided on at least one surface of the substrate. Examples of the oxidation method include corona discharge treatment, plasma discharge treatment, chromium oxidation treatment (wet), flame treatment, hot air treatment, ozone treatment, and ultraviolet irradiation treatment. These surface treatment methods are appropriately selected depending on the type of substrate film, but generally, corona discharge treatment is preferably used in terms of effectiveness and operability. There is no particular restriction on the thickness of the substrate, and the thickness may be set appropriately based on factors such as mechanical strength and ease of handling during production and use. The thickness is usually 10 to 300 μm, preferably 12 to 200 μm, and particularly preferably 15 to 125 μm.

[0014] The arithmetic mean roughness (Ra) of the surface of the substrate on the release agent layer side is preferably from 0.1 to 70 nm, and more preferably from 1 to 60 nm. The arithmetic mean roughness (Ra) of the surface of the substrate on the release agent layer side is preferably 0.1 to 70 nm in terms of handling of the substrate, suppression of poor electrical continuity, etc. In addition, substrates having a surface arithmetic mean roughness (Ra) of 1 to 70 nm are relatively easy and inexpensive to obtain, and are therefore also preferable in terms of availability and production costs of the release film for producing ceramic green sheets used in the production method of the present invention.

[0015] The arithmetic mean roughness (Ra) of the surface of the substrate opposite to the release agent layer side is preferably from 5 to 70 nm, and particularly preferably from 10 to 60 nm. When the arithmetic mean roughness (Ra) of the surface of the substrate opposite to the release agent layer side is not less than the above lower limit, blocking during winding of the release film for producing a ceramic green sheet used in the production method of the present invention can be effectively suppressed, while when it is not more than the above upper limit, it becomes easy to smooth the surface of the release agent layer.

[0016] Release agent layer There are no particular limitations on the material of the release agent layer constituting the release film for producing a ceramic green sheet used in the manufacturing method of the present invention, and any material can be used as long as the following condition is satisfied: the difference between the bromonaphthalene contact angle BCA1 of the release agent layer on the surface opposite the substrate and the bromonaphthalene contact angle BCA2 obtained by applying a ceramic slurry of the specific composition described above to the surface opposite the substrate, drying it, storing it in a constant temperature and humidity environment of 23±2°C x 50±5%RH for one week, and then peeling it off, δBCA=BCA2-BCA1, is within the range of -1.5° to 1.0°. From the viewpoint of ease of production of the release film for producing a ceramic green sheet and appropriate control of the bromonaphthalene contact angle, water contact angle, etc., it is preferable to form the release agent layer by coating a curable composition on a substrate and curing it, and it is particularly preferable to form the release agent layer by coating a photocurable and / or thermosetting curable composition and curing it. That is, it is preferable that the release agent layer in the release film for producing a ceramic green sheet used in the production method of the present invention contains a cured product of the curable composition.

[0017] curable composition The curable composition preferably used for forming the release agent layer in the release film for producing a ceramic green sheet used in the production method of the present invention preferably contains at least one reactive compound (a) having at least one reactive functional group selected from the group consisting of a (meth)acryloyl group, a hydroxyl group, and an epoxy group. By using a curable composition containing at least one reactive compound (a) having at least one reactive functional group selected from the group consisting of a (meth)acryloyl group, a hydroxyl group, and an epoxy group, it is possible to easily form a release agent layer of the release film for producing a ceramic green sheet used in this embodiment with good controllability of the surface free energy, etc.

[0018] The curable composition may contain only one reactive compound (a) having at least one reactive functional group selected from the group consisting of (meth)acryloyl group, hydroxyl group, and epoxy group, or may contain two or more reactive compounds (a) having at least one reactive functional group selected from the group consisting of (meth)acryloyl group, hydroxyl group, and epoxy group. From the viewpoint of controlling various properties such as curability, releasability, and surface free energy of the release agent layer, it is preferable to use two or more reactive compounds (a) in combination, and it is particularly preferable to use a combination of the reactive silicone (a1) and the crosslinkable compound (a2) described below, and further preferably to combine the film-forming compound (a3) ​​described below.

[0019] The curable composition may be composed of only a reactive compound (a) having at least one reactive functional group selected from the group consisting of a (meth)acryloyl group, a hydroxyl group, and an epoxy group, or may contain other components such as a solvent, a radical initiator, a cationic initiator, a leveling agent, an antistatic agent, a dye, and a pigment. The amount of reactive compound (a) having at least one reactive functional group selected from the group consisting of a (meth)acryloyl group, a hydroxyl group, and an epoxy group used is preferably 50 mass% or more, particularly preferably 60 to 96 mass%, of the mass of the release agent layer.

[0020] Reactive Compound (a) The reactive compound (a) preferably used for forming the release agent layer in the release film for producing a ceramic green sheet used in the production method of the present invention has at least one reactive functional group selected from the group consisting of a (meth)acryloyl group, a hydroxyl group, and an epoxy group. By having at least one reactive functional group selected from the group consisting of a (meth)acryloyl group, a hydroxyl group, and an epoxy group, it is possible to impart photocurability and / or thermosetting property to the curable composition.

[0021] The reactive compound (a) may have one or more reactive functional groups, but from the viewpoint of photocurability and / or thermosetting property, it preferably has two or more reactive functional groups, more preferably has 2 to 15 reactive functional groups, and particularly preferably has 2 to 10 reactive functional groups. When the reactive compound (a) has two or more reactive functional groups, it may have two or more of the same type of reactive functional groups, or may have a combination of two or more different types of reactive functional groups in total. From the viewpoint of curability, etc., when active energy rays are used, it is preferable that the reactive compound (a) has a (meth)acryloyl group. When heat curing is also used, a material containing a hydroxyl group or an epoxy group can be appropriately selected.

[0022] Preferred examples of the reactive compound (a) include reactive silicone (a1) having at least one reactive functional group selected from the group consisting of a (meth)acryloyl group, a hydroxyl group, and an epoxy group, and a siloxane skeleton, reactive compound (a2) having the same reactive functional group as the reactive silicone (a1) and having a reactive functional group equivalent of 2000 g / mol or less, and film-forming compound (a3) ​​having two or more (meth)acryloyl groups in one molecule. In the curable composition, it is preferable to use a combination of the reactive silicone (a1) and the reactive compound (a2), and it is further preferable to use a combination of the film-forming compound (a3).

[0023] Reactive Silicone (a1) The curable composition preferably contains, as the reactive compound (a), at least one reactive functional group selected from the group consisting of a (meth)acryloyl group, a hydroxyl group, and an epoxy group, and a reactive silicone (a1) having a siloxane skeleton. By using the reactive silicone (a1), the desired releasability can be imparted to the surface of the release agent layer, making it easier to peel off the ceramic green sheet. In addition, the bromonaphthalene contact angle, water contact angle, etc. can be appropriately controlled. The reactive silicone (a1) is not limited as long as it has at least one reactive functional group selected from the group consisting of a (meth)acryloyl group, a hydroxyl group, and an epoxy group, and has a siloxane skeleton. By having at least one reactive functional group selected from the group consisting of (meth)acryloyl group, hydroxyl group, and epoxy group, the reactive functional group reacts by irradiation with active energy rays or by a separate reaction step (for example, a heating step), and the siloxane skeleton is incorporated into a crosslinked structure and fixed. This makes it possible to more effectively control the releasability, bromonaphthalene contact angle, water contact angle, etc. of the release agent layer. As the reactive functional group, an epoxy group is particularly preferred.

[0024] The reactive functional group may be introduced into one end of the siloxane skeleton, may be introduced into both ends, or may be introduced into a side chain. At least one reactive functional group selected from the group consisting of (meth)acryloyl group, hydroxyl group, and epoxy group is preferably introduced into one molecule of the reactive silicone (a1). When having two or more reactive functional groups, it may have two or more of the same type of reactive functional groups, or may have a combination of two or more different reactive functional groups in total. In addition to the reactive functional group selected from the group consisting of a (meth)acryloyl group, a hydroxyl group, and an epoxy group, it may further have a vinyl group, a maleimide group, a carboxyl group, an isocyanate group, or the like.

[0025] There is no particular restriction on the molecular weight of the reactive silicone (a1), but from the viewpoints of appropriate releasability and controllability of the bromonaphthalene contact angle, water contact angle, etc., it is preferably from 5,000 to 100,000, and particularly preferably from 10,000 to 70,000.

[0026] In the curable composition, the reactive silicone (a1) may be used alone or in combination of two or more kinds. The content of the reactive silicone (a1) in the curable composition is not particularly limited, but is preferably from 0.1 to 20 mass %, and particularly preferably from 0.2 to 15 mass %, based on the total mass of the release agent layer.

[0027] Reactive compound (a2) (crosslinking compound (a2)) The curable composition preferably contains, as the reactive compound (a), a reactive compound (a2) having the same reactive functional group as the reactive silicone (a1) and having a reactive functional group equivalent of 2000 g / mol or less. It is particularly preferable to use the reactive compound (a2) in combination with the reactive silicone (a1). The reactive compound (a2) functions as a crosslinking agent for the reactive silicone (a1) and the like, promotes the effect of the curable composition, and can incorporate and fix the reactive silicone (a1) and the like into the crosslinked structure. This makes it possible to prevent contamination of the ceramic green sheet, and to further improve the performance of stability over time due to the effect of the crosslinked structure promoting curing. In consideration of its function as a crosslinking agent, the reactive compound (a2) is also referred to as the "crosslinkable compound (a2)" in this specification.

[0028] The reactive functional group equivalent of the reactive compound (a2) is 2000 g / mol or less, preferably 1800 g / mol or less, particularly preferably 1700 g / mol or less. By having a reactive functional group equivalent of 2000 g / mol or less, the polymer has a sufficient number of (meth)acryloyl groups, hydroxyl groups, and / or epoxy groups to achieve suitable crosslinking performance. The reactive compound (a2) preferably has a total of 1 or more reactive functional groups ((meth)acryloyl groups, hydroxyl groups, and / or epoxy groups), preferably 2 to 15, and particularly preferably 2 to 6. When the number of reactive functional groups is within the above range, more appropriate crosslinking performance can be achieved.

[0029] The molecular weight of the crosslinkable compound (a2) is not particularly limited, but from the viewpoint of crosslinking performance, it is preferably from 150 to 4,000, and particularly preferably from 150 to 3,000. The crosslinkable compound (a2) may have a siloxane skeleton. In this case, by introducing a sufficient amount of siloxane skeleton into the release agent layer together with the siloxane skeleton of the reactive silicone (a1), more preferable release performance can be achieved.

[0030] In the curable composition, the crosslinkable compound (a2) may be used alone or in combination of two or more kinds. The content of the crosslinkable compound (a2) in the curable composition is not particularly limited, but is preferably 0.08 to 99 mass%, more preferably 0.4 to 50 mass%, even more preferably 0.7 to 30 mass%, and particularly preferably 1.0 to 15 mass%, based on the total mass of the release agent layer. Also, based on the amount of reactive silicone (a1) used, it is preferably 81 to 9900 mass parts, and particularly preferably 85 to 1000 mass parts, based on 100 mass parts of reactive silicone (a1).

[0031] It is also preferable to use a compound having excellent film-forming properties as the reactive compound (a) in the curable composition. The compound having excellent film-forming properties may be either a compound having a (meth)acryloyl group or a compound having a hydroxyl group, but it is preferable to use a film-forming compound (a3) ​​having two or more (meth)acryloyl groups in one molecule. Film-forming compound (a3) The curable composition preferably contains, as the reactive compound (a), a film-forming compound (a3) ​​having two or more (meth)acryloyl groups in one molecule. By including the film-forming compound (a3) ​​having two or more (meth)acryloyl groups in one molecule, the curable composition can be cured by irradiation with active energy rays. The film-forming compound (a3) ​​may be any one of a monomer, an oligomer, or a polymer, or may be a mixture thereof. The film-forming compound (a3) ​​is preferably a (meth)acrylic acid ester. Here, the (meth)acrylic acid ester means both an acrylic acid ester and a methacrylic acid ester. The same applies to other similar terms.

[0032] The (meth)acrylic acid ester is preferably at least one selected from polyfunctional (meth)acrylate monomers and (meth)acrylate oligomers, particularly preferably at least one selected from difunctional or higher (meth)acrylate monomers and (meth)acrylate oligomers, and more preferably a trifunctional or higher (meth)acrylate monomer. By being difunctional or higher, more preferably trifunctional or higher, the curability of the curable composition is excellent, and the surface of the obtained release agent layer also has excellent releasability.

[0033] There is no particular restriction on the (meth)acryloyl group equivalent of the film-forming compound (a3), and film-forming compounds (a3) ​​having a wide range of (meth)acryloyl group equivalents can be used as long as the ΔBCA condition specified in the present invention is satisfied. From the viewpoint of achieving even better peelability and controllability of the bromonaphthalene contact angle, water contact angle, etc., the (meth)acryloyl group equivalent of the film-forming compound (a3) ​​is preferably 300 g / mol or less, and particularly preferably 260 g / mol or less.

[0034] Examples of polyfunctional (meth)acrylate monomers include 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, neopentyl glycol adipate di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, dicyclopentanyl di(meth)acrylate, caprolactone-modified dicyclopentenyl di(meth)acrylate, ethylene oxide-modified phosphoric acid di(meth)acrylate, allylated cyclohexyl di(meth)acrylate, and isocyanurate di(meth)acrylate. acrylate, trimethylolpropane tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, dipentaerythritol tetra(meth)acrylate, propionic acid modified dipentaerythritol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, propylene oxide modified trimethylolpropane tri(meth)acrylate, tris((meth)acryloxyethyl)isocyanurate, propionic acid modified dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, caprolactone modified dipentaerythritol hexa(meth)acrylate, and the like. These may be used alone or in combination of two or more.

[0035] Examples of the polyfunctional (meth)acrylate oligomer include polyester acrylate oligomers, epoxy acrylate oligomers, urethane acrylate oligomers, polyether acrylate oligomers, polybutadiene acrylate oligomers, and silicone acrylate oligomers.

[0036] The polyester acrylate oligomer can be obtained, for example, by esterifying the hydroxyl groups of a polyester oligomer having hydroxyl groups at both ends, which is obtained by condensation of a polycarboxylic acid and a polyhydric alcohol, with (meth)acrylic acid, or by esterifying the terminal hydroxyl groups of an oligomer obtained by adding an alkylene oxide to a polycarboxylic acid, with (meth)acrylic acid.

[0037] The epoxy acrylate oligomer can be obtained, for example, by reacting (meth)acrylic acid with the oxirane ring of a relatively low molecular weight bisphenol epoxy resin or novolac epoxy resin to esterify it. In addition, a carboxyl-modified epoxy acrylate oligomer obtained by partially modifying an epoxy acrylate oligomer with a dibasic carboxylic acid anhydride can also be used.

[0038] The urethane acrylate oligomer can be obtained, for example, by esterifying a polyurethane oligomer obtained by reacting a polyether polyol or polyester polyol with a polyisocyanate with (meth)acrylic acid.

[0039] The polyether acrylate oligomer can be obtained by esterifying the hydroxyl groups of a polyether polyol with (meth)acrylic acid.

[0040] In the curable composition, the film-forming compound (a3) ​​may be used alone or in combination of two or more kinds. The content of the film-forming compound (a3) ​​in the curable composition is not particularly limited, but is preferably 50 to 90 mass %, and particularly preferably 60 to 85 mass %, based on the total mass of the release agent layer.

[0041] The release agent layer can be formed by applying the raw material of the release agent layer, preferably the above-mentioned curable composition, to at least one surface of the substrate, and then drying as necessary and curing by irradiation with active energy rays such as light. If the reactive functional group of the reactive compound (a) is one that reacts with heat, the reaction can be caused by drying at this time, and the reactive compound (a) preferably having a siloxane skeleton can be incorporated into the crosslinked structure. There is no particular limitation on the coating method of the curable composition, and for example, gravure coating method, bar coating method, spray coating method, spin coating method, knife coating method, roll coating method, die coating method, etc. can be used.

[0042] As the active energy ray, ultraviolet rays, electron beams, etc. are usually used. The irradiation amount of the active energy ray varies depending on the type of energy ray. For example, in the case of ultraviolet rays, the light amount is 10 to 1000 mJ / cm. 2 is preferred, particularly from 20 to 500 mJ / cm 2 In the case of electron beams, the dose is preferably about 0.1 to 50 kGy.

[0043] In the release film for producing a ceramic green sheet used in the manufacturing method of the present invention, the difference δBCA=BCA2-BCA1 between the bromonaphthalene contact angle BCA1 of the surface of the release agent layer opposite the substrate and the bromonaphthalene contact angle BCA2 obtained by coating the surface of the release agent layer opposite the substrate with a ceramic slurry of a specific composition (A) containing 45% by mass of barium titanate particles, B) 3.6% by mass of polyvinyl butyral, C) 0.9% by mass of dibutyl phthalate, D) 25% by mass of toluene, and E) 25% by mass of ethanol, drying the ceramic slurry, storing it for one week in a constant temperature and humidity environment of 23±2°C x 50±5% RH, and then peeling it off, is within the range of -1.5° to 1.0°. Since the δBCA is within the range of -1.5° to 1.0°, in combination with other technical features of the present invention, the method for producing a ceramic green sheet of the present invention using the release film for producing a ceramic green sheet makes it easy to peel off the ceramic green sheet formed thereon, and changes in releasability over time are small, so that excellent easy releasability can be stably achieved even long periods of time after the green sheet is coated. This achieves technical effects of great practical value at a high level that exceeds the limits of conventional technology. The mechanism by which a δBCA within the range of -1.5° to 1.0° achieves excellent ceramic green sheet ease of releasability and suppression of its deterioration over time is not entirely clear, but it is estimated that the hardness of the release agent layer affects the interaction at the ceramic green sheet interface, and as a result, there is a range of the contact angle change δBCA of bromonaphthalene that corresponds to an optimal surface state for preventing migration of release agent components and transfer of green sheet components and for achieving easy releasability and suppression of its deterioration over time, and specifically, the contact angle change δBCA of bromonaphthalene is in the range of -1.5° to 1.0°.

[0044] The bromonaphthalene contact angles BCA1 and BCA2 of the surface of the release agent layer opposite to the substrate of the release film for producing a ceramic green sheet used in the production method of the present invention can be measured by a method conventionally known in the art, for example, by an automatic contact angle meter, etc. More specifically, they can be measured by the method described in the examples of the present specification. The conditions for coating, drying, and peeling the ceramic slurry during the measurement of the bromonaphthalene contact angles BCA1 and BCA2 are usually as follows: the ceramic slurry coating thickness is 50 μm before drying, the drying conditions are 70° C., 2 minutes, and the peel angle is 180°. The composition of the ceramic slurry is as described above. The change in the bromonaphthalene contact angle, ΔBCA, can be calculated from the BCA1 and BCA2 measured above according to the formula ΔBCA=BCA2−BCA1.

[0045] The change δBCA in the bromonaphthalene contact angle of the release agent layer on the surface opposite the substrate of the release film for producing a ceramic green sheet used in the manufacturing method of the present invention is preferably from -1.2° to 0.8°, more preferably from -1.0° to 0.6°, and particularly preferably from -0.8° to 0.5°. There is no particular restriction on the initial bromonaphthalene contact angle BCA1 of the surface of the release agent layer opposite the substrate, but from the viewpoints of facilitating peeling of the green sheet and facilitating keeping the value of δBCA within a specified range, it is preferably 55° to 85°, and particularly preferably 60° to 80°.

[0046] The initial bromonaphthalene contact angle BCA1 of the surface of the release agent layer opposite the substrate, the bromonaphthalene contact angle BCA2 after a ceramic slurry of a specific composition is applied, dried, stored for one week in a constant temperature and humidity environment of 23±2°C x 50±5%RH and then peeled off, and the change in the bromonaphthalene contact angle δBCA can be appropriately adjusted by adjusting the type and amount of the material constituting the release agent layer, the amount of the release agent layer applied, and curing conditions such as the drying temperature and the amount of active energy ray irradiation. In particular, the reactive functional group equivalent and the amount used of the reactive compound (a) having at least one reactive functional group selected from the group consisting of a (meth)acryloyl group, a hydroxyl group, and an epoxy group, particularly the reactive compound (a2) having the same reactive functional group as the reactive silicone (a1) and having a reactive functional group equivalent of 2000 g / mol or less, or the film-forming compound (a3) ​​having two or more (meth)acryloyl groups in one molecule, can be appropriately adjusted by adjusting the reactive functional group equivalent and the amount used.

[0047] The release film for producing a ceramic green sheet used in the manufacturing method of the present invention may have a difference, δBCA=BCA2-BCA1, between the bromonaphthalene contact angle BCA1 of the surface of the release agent layer opposite the substrate and the bromonaphthalene contact angle BCA2 obtained by applying a ceramic slurry of a specific composition to the surface of the release agent layer opposite the substrate, drying the same, storing the same for one week in a constant temperature and humidity environment of 23±2°C×50±5%RH, and then peeling the same, and no other restrictions are imposed. However, it is preferable that the difference, δWCA=WCA2-WCA1, between the water contact angle WCA1 of the surface of the release agent layer opposite the substrate and the water contact angle WCA2 obtained by applying a ceramic slurry of a specific composition to the surface of the release agent layer opposite the substrate, drying the same, storing the same for one week in a constant temperature and humidity environment of 23±2°C×50±5%RH, and then peeling the same, is within the range of -3.5° to 1.0°. In addition to the above δBCA, by using a release film for producing a ceramic green sheet having a δWCA in the range of -3.5° to 1.0°, in combination with other technical features of the present invention, the method for producing a ceramic green sheet of this embodiment can achieve an even higher level of technical effects with high practical value, such as easy peeling of the ceramic green sheet formed on the release film for producing a ceramic green sheet, small change in releasability over time, stable achievement of excellent easy peelability even long periods of time after coating of the green sheet, and suppression of charging when peeling the green sheet.

[0048] The mechanism by which the use of a release film for producing a ceramic green sheet having a δWCA in the range of -3.5° to 1.0° can achieve better ease of releasability of the ceramic green sheet, suppression of changes over time, and suppression of charging when the green sheet is peeled off is not necessarily clear, but it is believed that there is a range of the water contact angle change δWCA that corresponds to an optimal surface state for ease of releasability and suppression of changes over time, in which the hardness of the release agent layer affects the interaction at the ceramic green sheet interface, and as a result, the migration of release agent components and the transfer of green sheet components are suppressed, and specifically, the water contact angle change δWCA is estimated to be in the range of -3.5° to 1.0°.

[0049] The water contact angles WCA1 and WCA2 of the surface of the release agent layer opposite the substrate of the release film for producing a ceramic green sheet can be measured by a method conventionally known in the art, for example, by an automatic contact angle meter, etc. More specifically, they can be measured by the method described in the examples of the present specification. The conditions for coating, drying, and peeling the ceramic slurry between the measurements of the water contact angles WCA1 and WCA2 are usually as follows: the ceramic slurry coating thickness is 50 μm before drying, the drying conditions are 70° C., 2 minutes, and the peel angle is 180°. The composition of the ceramic slurry is as described above. The change in water contact angle ΔWCA can be calculated from the above measured WCA1 and WCA2 according to the formula ΔWCA=WCA2-WCA1.

[0050] The change in water contact angle ΔWCA of the surface of the release agent layer opposite the substrate of the release film for producing a ceramic green sheet used in the method for producing a ceramic green sheet of this embodiment is preferably from −3.3° to 0.8°, and particularly preferably from −3.2° to 0.6°. There is no particular restriction on the initial water contact angle WCA1 of the surface of the release agent layer opposite the substrate, but from the viewpoints of making it easier to peel off the green sheet and making it easier to keep the δWCA value within a specified range, it is preferably 85° to 115°, and particularly preferably 90° to 110°.

[0051] The initial water contact angle WCA1 of the surface of the release agent layer opposite to the substrate, the water contact angle WCA2 after coating a ceramic slurry of a specific composition, drying, and storing it in a constant temperature and humidity environment of 23±2°C x 50±5%RH for one week and then peeling it off, and the change in water contact angle δWCA can be appropriately adjusted by adjusting the type and amount of material constituting the release agent layer, the coating amount of the release agent layer, and curing conditions such as drying temperature and active energy ray irradiation amount. In particular, the reactive compound (a) having at least one reactive functional group selected from the group consisting of (meth)acryloyl group, hydroxyl group, and epoxy group, especially the reactive compound (a2) having the same reactive functional group as the reactive silicone (a1) and having a reactive functional group equivalent of 2000g / mol or less, and the film-forming compound (a3) ​​having two or more (meth)acryloyl groups in one molecule, can be appropriately adjusted by adjusting the reactive functional group equivalent and amount used.

[0052] The thickness of the release agent layer is preferably 0.05 to 2 μm, and particularly preferably 0.2 to 1.5 μm. The thickness of the release agent layer is preferably 0.05 μm or more from the viewpoint of smoothness of the surface of the release agent layer and suppression of pinholes and thickness unevenness of the ceramic green sheet. The thickness of the release agent layer is preferably 2 μm or less from the viewpoint of suppressing curling caused by cure shrinkage of the release agent layer. It is also preferable from the viewpoint of suppressing blocking and charging.

[0053] Other layers The release film for producing a ceramic green sheet used in the production method of the present invention may have layers other than the above-mentioned substrate and release agent layer, such as a protective layer, an adhesive layer, an antistatic layer, etc. The substrate and the release agent layer may be laminated directly to each other, or may be laminated via another layer such as an adhesive layer.

[0054] Release film for ceramic green sheet manufacturing The method for producing a ceramic green sheet of the present invention uses the release film for producing a ceramic green sheet described above, and in combination with other technical features of the present invention, it is possible to easily peel off the ceramic green sheet formed on the release film, with little change in releasability over time, and excellent easy releasability can be stably achieved even long periods of time after the green sheet was applied, thereby achieving technical effects of high practical value at a high level that exceeds the limitations of conventional technology. Therefore, the method can be suitably used in the production of ceramic green sheets used in various ceramic products, for example, in the production of ceramic green sheets used for multilayer ceramic capacitors or multilayer ceramic substrates.

[0055] Manufacturing method of ceramic green sheet The method for producing a ceramic green sheet of the present invention is a production method including the following steps a) to c). a) A step of applying a ceramic slurry onto the release film for producing a ceramic green sheet described above in detail. b) forming a ceramic green sheet from the ceramic slurry applied in the a) step; c) peeling the ceramic green sheet formed in the b) step from the release film for producing the ceramic green sheet. By using the specific release film for producing ceramic green sheets as described above in detail, and by having the specific steps a) to c) described above, the method for producing a ceramic green sheet of the present invention can easily peel off the ceramic green sheet from the release film, and at the same time, can achieve technical effects of high practical value at a high level that exceeds the limitations of conventional technology, such as small change in releasability over time and stable achievement of excellent releasability even long periods of time after the green sheet is applied.

[0056] a) Ceramic slurry coating In step a) of the method for producing a ceramic green sheet of the present invention, for example, a technique that has been conventionally used in this technical field for applying a ceramic slurry onto a release film for producing a ceramic green sheet can be appropriately used, and for example, the following technique can be used.

[0057] Ceramic Slurry There is no particular limitation on the ceramic slurry used in step a) of the production method of the present invention, and for example, any ceramic slurry that has been conventionally used in the present technical field for producing ceramic green sheets can be used as appropriate.

[0058] The ceramic slurry used in step a) may be the same as or different from a ceramic slurry of a specific composition (A) containing 45% by mass of barium titanate particles, B) 3.6% by mass of polyvinyl butyral, C) 0.9% by mass of dibutyl phthalate, D) 25% by mass of toluene, and E) 25% by mass of ethanol) that is coated on a release film for producing a ceramic green sheet between the measurements of δBCA=BCA2-BCA1, which characterizes the release film for producing a ceramic green sheet used in the manufacturing method of the present invention. In other words, the method for producing a ceramic green sheet of the present invention is not limited to a method for producing a ceramic green sheet using a ceramic slurry of the above-mentioned specific composition, but also includes a method for producing a ceramic green sheet using a ceramic slurry of a wide range of other compositions.

[0059] The ceramic slurry preferably contains ceramic particles and a solvent, and the ceramic particles are preferably dispersed in the solvent. As the ceramic particles, inorganic compound particles capable of forming ceramics by sintering can be used. Examples of inorganic compounds include oxides, nitrides, oxynitrides, borides, etc. of metals or semimetals. More specific examples of inorganic compounds include perovskite compounds such as barium titanate (BaTiO3), calcium titanate (CaTiO3), strontium titanate (SrTiO3), calcium zirconate (CaZrO3), strontium zirconate (SrZrO3), etc. When these inorganic compounds are used as the main component of the ceramic particles, they may contain Mn, Mg, Si, Co, Ni, rare earth elements, etc. as a minor component with a content less than that of the main component.

[0060] The primary particle size of the ceramic particles is desirably 1 μm or less.

[0061] The solvent may be an organic solvent or an inorganic solvent such as a water-based solvent, but is preferably an organic solvent from the viewpoint of ease of solvent removal when forming a ceramic green sheet in the step b) described later. As the organic solvent, a general one can be used, and it can be appropriately selected depending on the drying temperature when forming the green sheet and the type of binder used. Generally, aromatic, alcohol, ester, ketone, and hydrocarbon-based solvents are used, and they can also be used in combination. The boiling point of the solvent is not particularly limited, but is preferably from 60 to 130°C, and particularly preferably from 70 to 130°C.

[0062] From the viewpoint of ease of handling of the ceramic green sheets, the ceramic slurry preferably contains a binder in addition to ceramic particles and a solvent. As the binder, various binders conventionally used in the present technical field for producing ceramic green sheets can be appropriately used, for example, polyvinyl butyral, urethane resin, polyvinyl acetate resin, acrylic resin, cellulose resin, etc. Among them, polyvinyl butyral, acrylic, etc. can be particularly preferably used. The amount of binder used is not particularly limited, but is preferably 3 to 20 parts by mass, and particularly preferably 5 to 15 parts by mass, per 100 parts by mass of ceramic particles.

[0063] The ceramic slurry may contain, in addition to the above-mentioned ceramic particles, solvent, and optional binder, other components such as a plasticizer, a surfactant, a dispersion stabilizer, and an antistatic agent. Suitable plasticizers include dibutyl phthalate, fatty acid esters, and the like.

[0064] The ceramic particles and organic solvent described above, as well as other components such as a binder and a plasticizer, if desired, are mixed with stirring to produce a ceramic slurry. The method of stirring and mixing is not particularly limited, and any method and device conventionally used in the present technical field for producing ceramic slurries can be used as appropriate, but for example, stirring and mixing can be performed using a ball mill. By using a ball mill, the particle size of the ceramic particles can be adjusted at the same time.

[0065] In step a), the method for applying the ceramic slurry can be appropriately selected depending on the viscosity of the ceramic slurry and the type and thickness of the ceramic green sheet to be formed in step b). For example, an applicator, on-roll die coater, reduced pressure die coater, off-roll die coater, slit coater, curtain coater, lift coater, knife coater, cast coater, reverse roll coater, blade coater, screen printing method, etc. can be appropriately used.

[0066] b) green sheet formation process; In step b), the solvent is removed from the ceramic slurry applied in step a) by drying or the like, thereby forming a ceramic green sheet on the release film. The temperature and time for drying in step b) are not particularly limited, but drying can be performed usually at 60 to 100° C., preferably 70 to 100° C., for usually 30 to 300 seconds, preferably 30 to 200 seconds.

[0067] By setting the drying time in step b) to 30 seconds or more, the particles in the sheet can be arranged uniformly and densely by the time drying is completed, thereby reducing voids in the green sheet. By setting the drying time in step b) to 200 seconds or less, the production efficiency in the manufacturing process of the ceramic green sheet can be improved.

[0068] By setting the drying temperature in step b) to 70°C or higher, substantially no solvent remains in the ceramic green sheet, and it is possible to prevent voids from occurring in the ceramic during the firing step. Also, by setting the drying temperature to 100°C or lower, it is possible to prevent swelling or dents on the surface of the green sheet caused by rapid evaporation of the solvent. Also, it is possible to have multiple drying zones and change the temperature for each drying zone.

[0069] c) Peeling process In step c), the ceramic green sheet formed in step b) is peeled off from the release film for producing the ceramic green sheet. The peeling method in step c) is not particularly limited and may be appropriately selected depending on the material and properties of the ceramic green sheet and the subsequent steps. For example, the ceramic green sheet can be peeled off by cutting the ceramic green sheet portion on the release film and then heating or deforming the release film. In the method for producing a ceramic green sheet of the present invention, the specific release film described above is used, so that the peeling force in step c) can be reduced (light peeling), which can effectively reduce breakage of the ceramic green sheet. The peeling force in the peeling step is preferably from 5 to 100 (mN / 50 mm), and particularly preferably from 10 to 50 (mN / 50 mm).

[0070] In the method for producing a ceramic green sheet of the present invention, by using the specific release film described in detail above, it is possible to maintain a peel force with little change from the initial green sheet peel force even if a long period of time has passed between steps a) and b) and step c). For example, even after storage at room temperature for one week from steps a) and b), the peel force in step c) is preferably 115% or less, and particularly preferably 110% or less, of the peel force when step c) is performed immediately after steps a) and b). If the peel force in step c) after storage at room temperature for one week from step b) is 115% or less, the problem of green sheet breakage can be more effectively suppressed.

[0071] Electrode printing process, half-cut process, punching process The method for producing a ceramic green sheet of the present invention may further include, in addition to the above steps a) to c), a step of performing electrode printing, half-cutting and / or punching after step b) and before step c).

[0072] By firing the ceramic green sheet obtained by the manufacturing method of the present invention, various ceramic products can be manufactured. According to the above embodiment having an electrode printing step after step b) and before step c), after electrode printing, a multilayer ceramic capacitor or a multilayer ceramic substrate can be manufactured through steps c) (peeling), lamination and pressure bonding, cutting and separation, firing, and external electrode formation.

[0073] By firing the ceramic green sheet obtained by the above-mentioned production method, various ceramic products can be produced. In manufacturing a multilayer ceramic capacitor, a step of printing internal electrodes on the green sheet is provided between the above steps b) and c), followed by step c) (peeling), lamination and pressure bonding, cutting and separation, firing, and external electrode formation steps to manufacture the multilayer ceramic capacitor. EXAMPLES

[0074] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0075] In the following Examples and Comparative Examples, the physical properties and characteristics were evaluated by the following methods. (water contact angle) The contact angle of water on the surface of the release agent layer was measured under the following conditions. Contact angle meter: Kyowa Interface Science Co., Ltd. DM-701 Fully automatic contact angle meter Contact angle meter analysis software: FAMAS made by the same company The contact angle θ was calculated by the sessile drop method according to the following procedure. i) The sample cut into a rectangular shape was set in the contact angle meter. ii) Approximately 6.1 μL of water droplets were ejected from the syringe pump. iii) Images of the droplets ejected onto the sample were taken. iv) The angle between the sample and the droplet was measured and this was taken as the contact angle (°) of water.

[0076] (Bromonaphthalene contact angle) The bromonaphthalene contact angle was measured in the same manner as in the above-mentioned method for measuring the water contact angle, except that 1-bromonaphthalene was used instead of water and the amount of 1-bromonaphthalene was 3.4 μL.

[0077] (peel strength) 1) Preparation of ceramic slurry Barium titanate (BT-01, manufactured by Sakai Chemical Industry Co., Ltd.), polyvinyl butyral (S-LEC BH-S, manufactured by Sekisui Chemical Co., Ltd.), dibutyl phthalate, toluene, and ethanol were mixed in a mass ratio of 45:3.6:0.9:25:25 to prepare a ceramic slurry as the raw material for the ceramic green sheets. 2) Formation of ceramic green sheets The ceramic slurry prepared in 1) above was applied to the release agent layer side of the release film sample for producing a ceramic green sheet with an applicator to a thickness of 50 μm, and dried at 70° C. for 2 minutes to form a ceramic green sheet with a thickness of 10 μm. 3) Measurement of peel strength of green sheet The release film sample and the ceramic green sheet formed thereon in the above step 2) were cut into strips of 50 mm x 200 mm, and the green sheet was peeled off from the release film at an angle of 180° using a Tensilon (A&D Co., Ltd.: RTG-1210) to measure the peel strength.

[0078] Details of each of the constituent components such as resins used in the release agent layer in the examples and comparative examples are as follows. (a3) Multifunctional acrylate 1 Product name: NK Ester A-9300, manufactured by Shin-Nakamura Chemical Co., Ltd. Tris-(2-acryloxyethyl)isocyanurate (functional groups: 3) Acrylic equivalent: 141g / mol (a3) Multifunctional acrylate 2 Manufactured by Shin-Nakamura Chemical Co., Ltd. Product name: NK Ester A-TMM-3LM-N Pentaerythritol tri- and tetraacrylate (functional groups: 3 and 4) Acrylic equivalent: 93.7g / mol (a3) Multifunctional acrylate 3 Product name: NK Ester A-DCP, manufactured by Shin-Nakamura Chemical Co., Ltd. Tricyclodecane dimethanol diacrylate (functional groups: 2) Acrylic equivalent: 304g / mol (a3) Multifunctional acrylate 4 Manufactured by Shin-Nakamura Chemical Co., Ltd. Product name: NK Ester A-GLY-9E Ethoxylated glycerin triacrylate (functional groups: 3) Acrylic equivalent: 217g / mol (a1) Epoxy-modified silicone 1 Arakawa Chemical Industries, Ltd., Product name: Silicolyse UV POLY201 Dimethyl silicone, alicyclic epoxy silicone block copolymer (a2) Epoxy-modified silicone 2 Manufactured by Shin-Etsu Chemical Co., Ltd., Product name: Shin-Etsu Silicone KR-470 Alicyclic epoxy group-containing cyclic siloxane tetrafunctional oligomer Epoxy equivalent: 200g / mol (a2) Epoxy-modified silicone 3 Manufactured by Shin-Etsu Chemical Co., Ltd., Product name: Shin-Etsu Silicone X-22-169AS Both ends / alicyclic epoxy modified silicone oil Epoxy equivalent: 500g / mol (a2) Epoxy-modified silicone 4 Manufactured by Shin-Etsu Chemical Co., Ltd., Product name: Shin-Etsu Silicone X-22-169B Both ends / alicyclic epoxy modified silicone oil Epoxy equivalent: 1700g / mol Epoxy modified silicone 5 Manufactured by Shin-Etsu Chemical Co., Ltd., Product name: Shin-Etsu Silicone KF-102 Side chain type / alicyclic epoxy modified silicone oil Epoxy equivalent: 3600g / mol Cationic initiator 1 Sanshin Chemical Industry Co., Ltd. Product name: San-Aid SI-100 Radical initiator 1 Made by IGM RESINS Product name: Esacure ONE α-Hydroxyketone type photoinitiator

[0079] [Example 1] Multifunctional acrylate 1, epoxy modified silicone 1, epoxy modified silicone 2, cationic initiator 1, and radical initiator 1 were mixed in the mass ratio shown in Table 1 to prepare a curable composition for the release agent layer. A polyethylene terephthalate film having a thickness of about 30 μm and a surface arithmetic mean roughness (Ra) of about 20 nm was used as the substrate. The curable composition prepared above was applied to one surface of the substrate, and the substrate was dried at 100°C for 15 seconds, after which it was irradiated with ultraviolet light using a high-pressure mercury lamp (accumulated light amount: about 40 mJ / cm 2 ) and curing to form a release agent layer, thereby producing a release film having a substrate and a release agent layer provided on one side of the substrate. For the release layer surface of the produced release film, the water contact angle and the bromonaphthalene contact angle were measured by the above-mentioned method to obtain the initial water contact angle WCA1 and the initial bromonaphthalene contact angle BCA1. Next, 1) a ceramic slurry was prepared, and 2) a ceramic green sheet was formed by the above-mentioned methods, and then 3) the peel strength of the green sheet was measured to obtain the initial sheet peel strength. Using a separate unused release film sample and the ceramic slurry obtained in the above 1) preparation of ceramic slurry, the above 2) ceramic green sheet was formed, and after storing it for one week in a constant temperature and humidity environment of 23±2°C x 50±5%RH, the above 3) peeling force of the green sheet was measured to obtain the sheet peeling force after one week. Furthermore, for the release layer surface of the release film after measuring the sheet peeling force after one week (after peeling the green sheet), the water contact angle and bromonaphthalene contact angle were measured again by the above method to obtain the water contact angle after peeling WCA2 and the bromonaphthalene contact angle after peeling BCA2. The results are shown in Table 1.

[0080] [Examples 2 to 4 and Comparative Examples 1 to 3] A release film was produced in the same manner as in Example 1, except that the formulation of the curing agent composition for the release agent layer was changed to that shown in Table 1, and then evaluated. The results are shown in Table 1.

[0081] [Table 1] [Industrial Applicability]

[0082] The method for producing a ceramic green sheet of the present invention realizes technical effects of high practical value at a high level that goes beyond the limitations of conventional technology, such as easy peeling of a ceramic green sheet formed on a release film, small change in peelability over time, and stable achievement of excellent easy peelability even long periods of time after the green sheet was applied. Since the method can be suitably used for producing various ceramic products, it has high applicability in various fields of industry, including the electrical and electronics industry, electronic parts industry, machinery industry, and automotive industry. [Explanation of symbols]

[0083] 11: Release film for ceramic green sheet manufacturing 12: Release agent layer 13: Base material

Claims

1. a) applying a ceramic slurry onto a release film for producing a ceramic green sheet; b) forming a ceramic green sheet from the ceramic slurry applied in the a) step; and c) peeling the ceramic green sheet formed in the b) step from the release film for producing the ceramic green sheet; A method for producing a ceramic green sheet comprising the steps of: The release film for producing a ceramic green sheet has a base material and a release agent layer provided on at least one side of the base material, The bromonaphthalene contact angle (BCA) of the surface of the release agent layer opposite to the substrate 1 and, On the surface of the release agent layer opposite to the substrate A) 45% by weight of barium titanate particles, B) 3.6% by weight of polyvinyl butyral, C) 0.9% by weight of dibutyl phthalate, D) 25% by weight of toluene, and E) 25% by weight of ethanol A ceramic slurry containing the above was applied, dried, and stored for one week in a constant temperature and humidity environment of 23±2°C x 50±5% RH. After peeling, the bromonaphthalene contact angle BCA was measured. 2 The difference between δBCA and δBCA = BCA 2 -BCA 1 , is in the range of −1.5° to 1.0°; A method for producing the ceramic green sheet.

2. 2. The method for producing a ceramic green sheet according to claim 1, wherein the coating amount of the ceramic slurry is 50 μm before drying, the drying conditions are 70° C. and 2 minutes, and the peeling is performed at an angle of 180°.

3. Water contact angle (WCA) of the surface of the release agent layer opposite to the substrate 1 and, The ceramic slurry was applied to the surface of the release agent layer opposite to the substrate, dried, and stored for one week in a constant temperature and humidity environment of 23±2° C.×50±5% RH. After peeling, the water contact angle WCA was 2 The difference between δWCA and WCA 2 - W.C.A. 1 3. The method for producing a ceramic green sheet according to claim 1, wherein the angle .theta.

4. 3. The method for producing a ceramic green sheet according to claim 1, further comprising a step of printing an internal electrode on the ceramic green sheet between step b) and step c).

5. A method for producing a ceramic product, comprising the step of producing a ceramic green sheet by the method for producing a ceramic green sheet according to claim 1 or 2.

6. The method for producing a ceramic product according to claim 5, further comprising the step of firing the ceramic green sheet.

7. The method for producing a ceramic product according to claim 5, wherein the ceramic product is a multilayer ceramic capacitor or a multilayer ceramic substrate.

Citation Information

Patent Citations

  • Release film

    JP2002200721A

  • Mold release film and method for producing the same

    JP2013060555A

  • Release film for production of green sheet and method of producing release film for production of green sheet

    JP2014177094A

  • Mold-releasing film

    WO2018037991A1

  • Release sheet

    WO2018079337A1