Composition for souvenirs, souvenirs, method of using souvenirs, and multi-layered warming pocket warmer

A souvenir composition using waste-derived materials with controlled warmth and emotional connection addresses safety and environmental concerns, offering long-lasting warmth and emotional benefits.

JP7588338B2Active Publication Date: 2024-11-22CONTRACT CO MATUBA
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020101476
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-11-01
Filing Date
2020-06-11
Publication Date
2024-11-22
Estimated Expiration
2040-06-11

AI Technical Summary

Technical Problem

Conventional hand warmers pose safety risks due to sudden chemical reactions, are disposable and uneconomical, lack diversity, and do not address social issues like waste management or emotional connections.

Method used

A souvenir composition using waste-derived, natural-derived, or animal-derived materials like sodium chloride and aluminosilicate components, combined with a water-permeable and sealable packaging, to provide controlled warmth and emotional connection.

Benefits of technology

The composition provides safe, long-lasting warmth, evokes memories, and promotes emotional healing while effectively utilizing waste materials, reducing environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588338000016
    Figure 0007588338000016
  • Figure 0007588338000017
    Figure 0007588338000017
  • Figure 0007588338000018
    Figure 0007588338000018
Patent Text Reader

Abstract

To provide a memento composition which becomes familiar with the body by proper warmth, with the warmth lasting for an extended period, which snuggles up a user's thought, reminds memory and heals, and which has an effect of giving happy feeling for a while, and to provide a memento and usage instruction thereof.SOLUTION: Provided is a memento 10, with a memento composition wrapped with a permeable material 2 and housed in a nonpermeable bag 4 that is hermetically sealable with a sealing part (zipper) 3. The nonpermeable bag 4 is in an outer bag 6. The memento composition contains sodium chloride and more than one or two kinds of materials derived from waste, nature or animals. Also, by adding a starch glue, it can be used as a molded object, or otherwise by evenly atomizing water of 0.5-5 weight % relative to the total weight, it may be used as a thermal body warmer.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a keepsake composition, a keepsake, a method of using a keepsake, and a multi-layered heated pocket warmer. [Background technology]

[0002] Conventional pocket warmers can be broadly divided into those that use the heat of reaction generated by an oxidation-reduction reaction that occurs between iron powder and activated charcoal via salt water, and those that use far-infrared radiation generated by exciting the crystalline water contained in salt crystals using a microwave oven or the like, but the former have the problem of low-temperature burns due to sudden chemical reactions, etc., and require special care when used by the elderly, disabled, infants, diabetics, etc. In addition, many of them are disposable, which is uneconomical, wastes resources, and has the problem of lacking diversity.

[0003] A thermal insulation device has been disclosed in which a thermal insulation material made by adding glycerin, montmorillonite, calcium carbonate, and salt is wrapped in one or more films such as polyethylene, polyvinyl chloride, and polyvinyl acetate, and placed on a part of the body that dissipates heat to prevent the dissipation of heat from said part (Patent Document 1). However, this thermal insulation device uses the heat emitted by the user as its heat source and is not intended to be used as a souvenir.

[0004] A far-infrared hot zone has been disclosed that contains rock salt as a hygroscopic heating substance and gravel made of granular porous andesite and basalt, the main component of which is silicon, as a far-infrared emitting substance (Patent Document 2). However, this far-infrared hot zone uses special gravel called silica high gray, and does not use aluminosilicate-containing components derived from waste or nature selected from sea sand, crushed ceramics, or jewel waste. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Jpn. Jpn. Published Examination No. 61-24248 [Patent Document 2] Japanese Patent Application Publication No. 11-197175 [Non-patent literature]

[0006] [Non-Patent Document 1] AdverTimes column, "The true meaning of 'From things to experiences' ~ What is behind experience branding (Part 2)" (URL: https: / / www.advertimes.com / 20180406 / article266418 / ) Summary of the Invention [Problem to be solved by the invention]

[0007] However, unlike the era when the products described above in the background art were proposed, today's daily necessities require new perspectives, such as an attitude to face the various social problems that have recently become apparent and selling experiences rather than things. Pocket warmers are no exception, and for example, they are perspectives that make effective use of industrial waste materials, foster compassion and mercy for the elderly and infants, remind people of their travels and hometowns, and provide an opportunity to remember important people and pets who have passed away, and are perspectives that are close to the feelings of the people who purchase the product, evoke memories, provide healing, and give a momentary sense of happiness (Non-Patent Document 1). Without these perspectives, future understanding of consumer consumption behavior will be insufficient, and the industry cannot be expected to develop.

[0008] All conventional pocket warmers are completely lacking in an approach that addresses the wide variety of social issues that have come to light in recent years and an approach that is considerate of people's feelings.

[0009] In view of the current situation as described above, the present invention aims to provide a souvenir composition that provides moderate warmth that fits the body and maintains that warmth for a long period of time, and more preferably a souvenir composition that is in tune with the user's feelings, evokes memories, provides healing, and gives a momentary sense of happiness, as well as a souvenir and a method for using the same. [Means for solving the problem]

[0010] One aspect of the present invention made to achieve the above object is a composition for a memorial product containing sodium chloride and one or more waste-derived, natural or animal-derived materials selected from waste-derived, natural or animal-derived silicate-containing components, waste-derived or natural aluminosilicate-containing components selected from sea sand, crushed ceramics or jewel waste, waste-derived, natural or animal-derived calcium carbonate-containing components, and waste-derived, natural or animal-derived calcium phosphate-containing components. According to the above configuration, by using waste-derived, natural or animal-derived materials, the viewpoints of effective use of waste materials, memorialization of deceased people or pets, and shaping memories of travels and hometowns can be incorporated into the memorial product, which can be close to the user's thoughts, recall memories, provide healing, and give a momentary sense of happiness. Furthermore, by appropriately selecting or appropriately combining one or more of the above waste-derived, natural-derived or animal-derived materials, the temperature immediately after heating and the resistance to cooling can be adjusted according to the material and thickness of the bag used for the outer cover, so that a keepsake that is moderately warm and fits the body and maintains its warmth for a long time can be obtained, and it can also be used at home when sleeping. In this specification, the outer cover refers to anything that surrounds the composition, and is not limited to the outer bag, but is a term that comprehensively refers to a non-permeable bag and a permeable material.

[0011] In the above-mentioned souvenir composition, the sodium chloride is preferably a salt derived from seawater. Since salt derived from seawater generally has a high water content, it is likely to become hot immediately after being removed from a microwave oven or a heater.

[0012] The above-mentioned souvenir composition preferably contains 70 to 85% by weight of sodium chloride and 15 to 30% by weight of one or more waste-derived, natural or animal-derived materials relative to the total weight of the composition. If the composition is within the above range, the temperature immediately after removal from a microwave oven or heater does not become too high, and the composition is more resistant to cooling.

[0013] Another aspect of the present invention, which has been made to achieve the above object, is a keepsake in which the above-mentioned composition for keepsake is wrapped in a water-permeable material. Water can be slowly supplied to the composition through the water-permeable material, making the keepsake suitable for repeated use.

[0014] The commemorative item is preferably stored in a sealable, water-impermeable bag. If the pocket warmer wrapped in a water-permeable material is sprayed with water while it is inside the water-impermeable bag, the surrounding area will not get wet and it is easy to manage. In addition, spraying an excess amount of water will allow the excess water to permeate and replenish the water-permeable material as appropriate, maintaining the properties of the pocket warmer, and the sealability will prevent water from leaking out.

[0015] It is preferable that the souvenir is the sealable water-impermeable bag stored in an outer bag. Since the outer bag is required to have fewer functional characteristics, there are many variations, and it can be made to look cute and fashionable. Also, by changing the material and thickness of the outer bag, it is possible to reduce or increase the sensible temperature.

[0016] It is preferable that the souvenir has a heat-retaining material between the outer bag and the sealable water-impermeable bag, since this will maintain the warming effect.

[0017] Another aspect of the present invention made to achieve the above object is a method of using the keepsake, which includes spraying water on the surface of the keepsake to the extent that the center of the keepsake does not get wet, and heating or keeping warm in a microwave oven or a heater. This prevents the deep temperature from reaching a plateau near the boiling point of water, and allows the temperature immediately after removal from the microwave oven or heater to be raised to 100°C or higher, so that the warming effect can be maintained for a long time even if the composition has the property of cooling down somewhat easily.

[0018] The method of using the commemorative item preferably involves spraying water evenly in an amount of 0.5 to 5% by weight based on the total weight of the composition for the commemorative item. If the amount of water sprayed is within the above range, even if the commemorative item contains a composition whose properties have deteriorated due to repeated use, the property of the temperature being 100°C or higher immediately after being removed from a microwave oven or a heater can be immediately restored, and the commemorative item can be used repeatedly about 2 to 3 times.

[0019] Another aspect of the present invention made to achieve the above object is a keepsake composition containing 70-85% by weight of sodium chloride and 15-30% by weight in total of one or more components selected from calcium carbonate, calcium phosphate and silicate, based on the total weight of the composition. The above composition results in a keepsake composition that is comfortable to the body with moderate warmth and maintains that warmth for a long period of time.

[0020] Another aspect of the present invention, which has been made to achieve the above object, is a commemorative item obtained by adding water and starch paste to the above-mentioned composition for commemorative items, mixing and shaping the composition. When the commemorative item is placed in water, it dissolves easily and leaves no residue. In addition, if the composition is made of naturally derived ingredients, it does not pollute the environment even when it dissolves.

[0021] Another aspect of the present invention, which has been made to achieve the above object, is a souvenir in which the above-mentioned composition for souvenirs is stored in a bag. This souvenir can be used as a talisman, for example, after appropriate purification or other treatment.

[0022] Another aspect of the present invention made to achieve the above object is a multi-layered warming pocket warmer in which one or more waste-, natural- or animal-derived materials selected from waste-, natural- or animal-derived silicate-containing components, waste-, natural- or animal-derived aluminosilicate-containing components selected from sea sand, crushed ceramics or gemstone rubbish, waste-, natural- or animal-derived calcium carbonate-containing components, and waste-, natural- or animal-derived calcium phosphate-containing components are surrounded by a heat-resistant material and sandwiched between the above-mentioned keepsake. When arranged in layers in this way, the heat storage effect of the waste-, natural- or animal-derived materials allows the warmth to last for a long time.

[0023] From the viewpoint of preventing scorching, the above heat-resistant material is preferably carbonized fiber, carbon fiber, aluminum fiber, urethane rubber, a glass fiber sheet, a composite material of silicone rubber and linen cloth, silicone rubber, a composite material of silicone rubber and an aramid fiber sheet, or a polyester sheet. Effect of the Invention

[0024] According to the present invention, by incorporating the viewpoints of effective use of waste materials, memorialization of deceased people and pets, and shaping memories of travels and hometowns into the commemorative item, it is possible to evoke memories, heal, and give a momentary sense of happiness to the user. In addition, according to the composition for commemorative items and the commemorative items and the method for using the same of the present invention, the temperature immediately after heating is not too high and the heat retention is relatively high, so that low-temperature burns can be prevented and the commemorative items can be used at home when sleeping. [Brief description of the drawings]

[0025] [Figure 1] A graph of deep heat dissipation when the ratio of coral sand, silica sand, and calcium phosphate to salt is kept constant. [Diagram 2] A graph of deep heat dissipation when the ratio of coral sand to salt is changed. [Diagram 3] A photo of a keepsake made of nonwoven fabric with four sides fused together. [Figure 4]A keepsake photo layered with laminated fabric on the outside and a ziplock bag on the inside. [Figure 5a] A souvenir photo showing the fusion margin between the zipper bag and the outer bag. [Figure 5b] A photo of the inside of the keepsake with the felt sandwiched between the outer bag and the ziplock bag. [Figure 5c] A photo of the inside of the keepsake, cut open to show the layering of the impermeable bag and felt. [Figure 5d] A keepsake photo showing the fusion of the zipper bag, felt, and outer bag. [Figure 6] Photographs showing heat dissipation experiments using nonwoven fabric with various compositions. [Figure 7] A photograph showing the measurement of a heat dissipation experiment in which various compositions were placed in a beaker. [Figure 8] A front view of a beaker wrapped four times with food shelf cushion sheet. [Figure 9] A flat photo of a beaker wrapped four times with food storage cushion sheet. [Figure 10] A photograph showing an experiment measuring the relationship between the surface temperature and deep temperature of nonwoven fabric. [Figure 11] A photo showing an experiment to measure the relationship between the deep temperature of nonwoven fabric and body sensation. [Figure 12] A photo showing an example of a sculpture made with salt and granite powder. [Figure 13] A photo of a multi-layered heated pocket warmer containing a keepsake and a piece of coral surrounded by heat-resistant material. [Figure 14] A photo of each element of the multi-layered warmer separated. [Figure 15] Coral surrounded by heat-resistant material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS An embodiment of the present invention will be described below with reference to the drawings. The composition for a souvenir according to the present invention contains sodium chloride and one or more waste-derived, natural-derived or animal-derived materials. In this specification, the term "souvenir composition" refers to a composition used for a souvenir. In this specification, the term "souvenir" refers to an item that is close to the user's thoughts, evokes memories, heals, and gives a momentary sense of happiness. Examples of such items include items that are used as souvenirs at travel destinations, items containing special products from travel destinations or hometowns, and items containing ingredients derived from humans or animals with whom the user has some kind of relationship, regardless of whether they are related by blood or not, and these include warm pocket warmers, amulets, and sculptures. In this specification, unless otherwise specified, the term "warm pocket warmer" includes a multi-layer warm pocket warmer that combines two or more warm pocket warmers.

[0027] The sodium chloride may be either rock salt or salt derived from seawater, but it is more preferable that it contains moisture equivalent to about 1% by weight of humidity. As such, salt derived from seawater is preferably used, and examples of such salt include those commercially available as solar salt, heavenly salt, and coarse salt. Note that salt derived from seawater may contain a small amount of bittern components and impurities. As for the sodium chloride, a bulky sodium chloride with a porosity of about 50% to 90% is preferably used. The preferred range of the angle of repose of sodium chloride is 40° to 70°.

[0028] As one or more waste-derived, natural or animal-derived materials, for example, one or more selected from the group consisting of waste-derived, natural or animal-derived silicate-containing components such as seagrass, silica sand, quartz, etc., waste-derived or natural aluminosilicate-containing components selected from beach sand (sea sand) from around the world or Japan, crushed ceramics or rubbish gemstones, waste-derived, natural or animal-derived porous or non-porous calcium carbonate-containing components such as coral sand, coral fragments, shells, rubbish (true) pearls, pearl powder, etc., and waste-derived, natural or animal-derived calcium phosphate-containing components such as human or animal bones (powder), teeth (powder), horns (powder), etc., can be selected and mixed and used. In this specification, the aluminosilicate-containing component is a component containing a compound having a structure in which some of the silicon atoms in silicate are replaced with aluminum atoms, and is conceptually distinguished from the silicate-containing component. However, the silicate-containing component may contain a trace amount of aluminum to the extent that it does not affect the composition formula.

[0029] The composition for keepsake according to the present invention, particularly when used in a warm pocket warmer, preferably contains 70 to 85% by weight of sodium chloride and 15 to 30% by weight of one or more waste-derived, natural or animal-derived materials based on the total weight of the composition. A more preferred lower limit of sodium chloride is 73% by weight.

[0030] The souvenir composition according to the present invention, particularly when used for a shaped object, preferably contains 70-93% by weight of sodium chloride and 7-30% by weight of one or more waste-derived, natural or animal-derived materials relative to the total weight of the composition. A more preferred lower limit for sodium chloride is 80% by weight. A more preferred upper limit for the one or more waste-derived, natural or animal-derived materials is 20% by weight.

[0031] Specific combinations of components of the souvenir composition of the present invention are not particularly limited, and include salt / coral flakes / coral sand, salt / coral sand / bone powder (bone ash), salt / quartz / bone powder, salt / seagrass / shell powder / bone powder, salt / pearl powder / coral sand, salt / coral sand / quartz sand, salt / coral sand / quartz sand / bone powder, salt / jewelry, and the like. Of these, from the standpoint of water retention and heat retention, a two-component, three-component, or four-component composition containing salt and coral sand is preferred.

[0032] The porosity of sodium chloride and one or more waste-derived, natural-derived or animal-derived materials can be said to be an index of the content of air layers with low thermal conductivity, but when spraying water and heating it, the heat stored in the water has a greater effect on the heat retention, so the porosity does not affect the heat retention so much. Therefore, the range of the porosity is not particularly limited, but can be 50% to 90%. The preferred lower limit is 60%, the preferred upper limit is 88%, and the upper limit can be 80% or less. When multiple components are used, it is preferable that the porosity of each component is approximately the same from the viewpoint of improving the mixability. The porosity in this specification is a value calculated by the ratio of the bulk density to the true density.

[0033] When a mixture of coarse salt (sodium chloride) and bone ash (containing calcium phosphate), silica sand (containing silicate), or coral sand (containing calcium carbonate) is heated in a microwave oven and the temperature immediately after removal and how quickly it cools are compared, the following trends may be observed depending on the conditions. (1) In terms of how long it takes for foods to cool down when mixed in the same ratio, the order is calcium phosphate >> silica sand > coral sand, and the temperature immediately after removing the food from the microwave when mixed in the same ratio generally tends to be coral sand > silica sand > calcium phosphate (Figure 1). (2) Mixtures of sodium chloride and silica sand tend to have the same difficulty in cooling over a relatively wide range of silica sand mixing ratios, from 10% to 25% by weight. (3) Mixtures of sodium chloride and coral sand have the property of being particularly slow to cool, especially those with a mixture ratio of 80 parts salt and 20 parts coral or 75 parts salt and 25 parts coral (Figure 2). (4) A mixture of sodium chloride and calcium phosphate tends to become more difficult to cool as the proportion of calcium phosphate increases.

[0034] The composition for souvenirs according to the present invention is not limited to waste-derived, natural-derived or animal-derived materials as described above, and may contain 70-85% by weight of sodium chloride and 15-30% by weight of one or more components selected from calcium carbonate, calcium phosphate and silicate, based on the total weight of the composition. In the case of a three-component or four-component composition, the composition preferably contains 70-85% by weight of sodium chloride, 10-18% by weight of porous calcium carbonate, and 5-12% by weight of calcium phosphate and / or silicate, based on the total weight of the composition. Here, if the proportion of silicate is increased, the temperature immediately after heating becomes higher, and if the proportion of calcium phosphate is increased, the composition tends to be slow to cool, so it is preferable to adjust the temperature by the outer covering.

[0035] In one embodiment, the commemorative item of the present invention is obtained by wrapping the above-mentioned composition for commemorative items in a water-permeable material. The water-permeable material is sufficient if it can withstand heating and heat-retaining conditions using a microwave oven or a heater, has a heat-resistant temperature of 100°C or higher, preferably 120°C or higher, more preferably 150°C or higher, measured according to JIS S 2029, and can supply moisture (water) of 0.8% by weight to 5% by weight based on the total weight of the composition for commemorative items to the surface of the composition for commemorative items, which is the content, by spraying within an allowable time limit. Representative inexpensive materials include polyester nonwoven fabric and polypropylene nonwoven fabric. In this embodiment, Soft Bag LL with Fancy Wrapping Flower (manufactured by Cando Co., Ltd., material: polypropylene nonwoven fabric, JAN code: 4542804042672) is used as the water-permeable material. Such a commemorative item can be produced by sandwiching the above-mentioned commemorative composition between two larger pieces of nonwoven fabric, heat sealing the four sides of the composition with a sealer, and cutting off the excess fused portions, as shown in Figure 3.

[0036] It is useful if the memento wrapped in the water-permeable material is stored in a sealable water-impermeable bag. As the sealable water-impermeable bag, a plastic zipper bag can be used because of its flexibility and the possibility of integration with an outer bag. A representative example is Ziploc (registered trademark). However, heat resistance is required for long-term storage such as 3 to 4 months in a heating device or repeated heating in a microwave oven, etc. Therefore, when repeatedly heating in a microwave oven, etc., it is recommended to take out the memento wrapped in the water-permeable material, heat it, and return it to the bag for use, or to use other heat-resistant water-impermeable bags such as those made of polypropylene or silicone rubber.

[0037] The souvenir 10 shown in FIG. 4 is made by wrapping the above-mentioned souvenir composition in a water-permeable material 2 and storing it in a water-impermeable bag 4 that can be sealed with a sealing portion (zipper) 3, and the water-impermeable bag 4 is contained in an outer bag 6. The outer bag 6 is not limited to what is generally called a bag, and can be anything that wraps the outside, including stuffed toys, belly warmers, charms, pillowcases, etc. There is no particular limit to the material of the outer bag, but when a plastic zipper bag is used as the water-impermeable bag, a laminated cloth that can be fused to the zipper bag is preferably used. In this case, it is preferable that the outside of the laminated cloth is treated with a water-repellent treatment to prevent dirt. In addition, when importance is placed on softness to the touch, silk, gauze, double gauze, etc. can also be used.

[0038] The outer bag 6 and the sealable non-water-permeable bag 4 may or may not be integrated. If they are integrated, they can be produced by covering both sides with laminated cloth with the sealing portion (zipper) closed, and heat fusing the laminated cloth together on three sides of the sealing portion excluding the opening edge 5, leaving a fusing allowance 7 of about 5 mm to 10 mm at the edge of the sealing portion, as shown in Figure 5a.

[0039] As shown in Figures 5b and 5c, a heat-retaining material 8 may be provided between the outer bag 6 and the sealable water-impermeable bag 4. Examples of the heat-retaining material 8 include felt, double gauze, and plastic cushion sheets for food shelves.

[0040] When the heat retaining material 8 is sandwiched between the outer bag 6 and the sealable water-impermeable bag 4, it is preferable to heat seal the heat retaining material 8 together, since this will prevent the heat retaining material 8 from shifting out of position. As a result of heat sealing, the state shown in Fig. 5d is obtained. In this embodiment, a tabletop sealer (T-130 model, manufactured by Fuji Impulse Sealer Co., Ltd.) is used as the sealer for heat sealing.

[0041] The method of using the commemorative item of the present invention includes spraying water on the surface of the commemorative item wrapped in the water-permeable material to the extent that the center does not become wet, and heating or keeping warm in a microwave oven or a heater. The amount of water sprayed here is preferably 0.5 to 5% by weight based on the total weight of the composition for the commemorative item. A more preferred upper limit is 3% by weight, and an even more preferred upper limit is 2.5% by weight. When the total weight of the composition is just under 100g, the microwave oven is typically heated for 1 minute 30 seconds to 2 minutes at 500W, or 40 seconds to 1 minute 30 seconds at 900W. As the heater, a hand towel heater, generally called a hot cabinet or towel warmer, is preferably used.

[0042] As shown in Figs. 13 and 14, the multi-layered warming pocket warmer 11 of the present invention is a cloth storage bag 12 having three pockets formed by two partition cloths 14a and 14b inside, in which a souvenir 20 is stored in the first pocket 13 and the third pocket 15, and a coral 22 surrounded by a heat-resistant material 18 is stored in the second pocket 17. The heat-resistant material shown in Fig. 15 refers to a packaging material for coral used to prevent the coral from burning the surroundings when heated in a microwave oven and becoming hot, and in this embodiment, a spatter sheet for curing made of carbonized fiber is used. Other heat-resistant materials include, for example, urethane rubber, glass fiber sheet, silicone rubber, a composite material of silicone rubber and linen cloth, a composite material of silicone rubber and aramid fiber sheet, and polyester sheet. The partition cloth is not essential as long as it can stabilize the state in which the heat-resistant material surrounding the coral is sandwiched between the souvenirs.

[0043] In one embodiment, the commemorative item of the present invention is obtained by adding water and starch paste to the above-mentioned composition for commemorative items, mixing them, and shaping them. The amount of starch paste added is 0.75 to 1.25 times the total weight of the components other than sodium chloride in the composition for commemorative items. The amount of water added is 3% to 12% times the total weight of the sodium chloride in the composition for commemorative items. If the composition for commemorative items contains a silicate-containing component, particularly silica sand, the resulting shaped object will be denser and more firmly packed.

[0044] In one embodiment, the souvenir of the present invention is a souvenir in which the above-mentioned souvenir composition is contained in a bag. EXAMPLES

[0045] Example 1 (Table Salt) Put 220 g of edible salt into a Tupperware (12 cm long x 8 cm wide x 3 cm high), filling it to the brim, and put it in the Tupperware to a height of about 3 cm (bulk density 0.76 g / cm 3 , true density: 2.16g / cm 3 The mixture was spread over the surface until the salt reached a thickness of 100 ml (porosity: 64.8%), and the surface was sprayed with water 50 times using a spray bottle (amount sprayed: 10 cc, 4.5% by weight of the edible salt), and then heated in a 900 W microwave for 2 minutes. After that, with the lid of the Tupperware open, the temperature was measured over time using a commercially available digital thermometer (DRETEC O-274IV cooking thermometer), with the center temperature measured at a depth of about 2 cm from the surface and the surface temperature measured at a depth of about 1 cm from the surface. The results are shown in Table 1.

[0046] Example 2 (Coral Sand 1) Instead of salt, use 220g of coral sand, whose main component is calcium carbonate, so that the height of the container is about 2.6cm (bulk density 0.88g / cm 3 , true density: 2.7~2.9g / cm 3 The coral sand was then sprayed with water 50 times (10 cc in terms of spray amount, 4.5% by weight relative to the weight of the coral sand), and the temperature change over time was measured in the same manner as in Example 1. The results are shown in Table 1.

[0047] Example 3 (Coral Sand 2) Instead of salt, 220 g of coral sand was spread to a height of about 2.6 cm inside the Tupperware, and water was sprayed over 200 times to moisten the entire surface. The temperature change over time was measured in the same manner as in Example 1. The results are shown in Table 1.

[0048] Example 4 (Silica Sand) Instead of salt, 220 g of beach sand collected from Yoron Island was used, with a height of about 2.8 cm (bulk density 0.82 g / cm 3 , true density: 2.5g / cm 3 The temperature change over time was measured in the same manner as in Example 1, except that the mixture was sprayed with water. The results are shown in Table 1.

[0049] [Table 1]

[0050] As can be seen from Table 1, it was found that the salt of Example 1 had little difference in temperature between the center and the surface. In addition, the temperature of the center of Coral 1 of Example 2 dropped by 36 degrees in a single go in 5 minutes after the start of measurement, but the rate of temperature drop thereafter was the slowest among the three types. The center temperature of the sand of Example 4 dropped by 39 degrees in a single go in 5 minutes after the start of measurement, just like Coral 1, and was the lowest among the three types. In addition, in a comparison between Example 2 and Example 3, it was expected that the temperature would naturally rise if Coral Sand 2, which was in a state of retaining moisture, was placed in a microwave oven, but it did not rise as much as expected, and the inside of Coral 1, which should have been almost dry, had a higher temperature. In addition, in a comparison between Example 2 (Coral 1) and Example 4 (Quartz Sand), although the porosity in the dry state was almost the same, there was a large difference in heat retention, so it was inferred that the influence of the material and the water retention derived therefrom was greater than the porosity.

[0051] Visual observation of the properties revealed that salt produced the highest temperature when heated while retaining moisture, but if it was kept too hot it would harden, so it was found that salt that contained too much water was unsuitable for use as a pocket warmer.

[0052] Example 5 Using coral sand 3 with a "beach-like" texture, which had a higher moisture content than coral sand 2 in Example 3 and was obtained by pouring water directly over the coral sand instead of using a spray bottle and then draining the water, we measured the temperature immediately after removing the sand from a 900W microwave oven after varying the heating time. The results are shown in Table 2.

[0053] [Table 2]

[0054] According to Table 2, regardless of the heating time, the deeper part of Coral Sand 3 was warmer than the surface, indicating that heat was being transferred from the deeper part to the surface. In addition, the temperature of the deeper part of Coral Sand 3 peaked out near the boiling point of water after 1 minute 30 seconds, indicating that the added energy was being used as latent heat when the water that had fallen to the deeper part due to gravity evaporated. From the results of Examples 2 and 3 and Table 2, it was found that if coral sand is too moist, the temperature does not rise easily, and if the moisture is removed, the temperature does not rise any more, so it is important to spray water on the surface of the warmer just enough to prevent the center of the warmer from getting wet. This result is advantageous because it is easier to spray less frequently. Considering the results of Example 5, in Example 2, the reason why the surface reached near the boiling point of water immediately after removing the microwave, while the deeper layers rose above the boiling point of water, is thought to be that when there was almost no water in the deeper layers, the specific heat of calcium carbonate and air (limestone has a value of 920 J / Kg / ℃, and air is about 1000 J / Kg / ℃) was about one-quarter of the specific heat of water (4189 J / Kg / ℃), resulting in a rapid temperature rise.

[0055] Taking all of the above into consideration, it was speculated that because the internal temperature of the salt when its surface was moist and the internal temperature of Coral 1 when its surface was moist were high, a mixture of salt and coral sand that retained a slight amount of moisture might be suitable for a pocket warmer.

[0056] Example 6-1 (Calcium phosphate) As a calcium phosphate-containing component, commercially available natural bone ash (manufacturer: Takesho Seiko Co., Ltd., product code: TO804013) was placed in a Tupperware (length 12 cm x width 8 cm x height 3 cm) at a weight of 110 g, with a height of approximately 2.5 cm (bulk density 0.46 g / cm 3 , true density: 3.14g / cm 3 The container was then covered with a layer of 1000g of tar, with a porosity of 85.4%, and the surface was sprayed with water 50 times (Example 6-1) or 230 times (Example 6-2) using a mister, after which it was heated in a 900W microwave for 2 minutes. After that, with the lid of the Tupperware open, a commercially available digital thermometer (DRETEC O-274IV cooking thermometer) was inserted near the center and the surface to measure the change in temperature T over time, and the properties were visually observed. The results are shown in Table 3. The change in temperature over time was provisionally curve-fitted using the least squares method with the following model formula, with T0 and B as variables. (Unless otherwise specified below, T0 is the deep layer temperature immediately after removing the container from the microwave, T ∞ is the indoor temperature controlled to a constant value, B is the coefficient of the following formula, and σ 2 is the error variance.) B was used as an index of how hard it is to cool. T=T ∞ +(T0-T ∞ )exp(-Bt) Example 6-2 The surface was sprayed with water 230 times with a spray bottle to wet the deep layers, but the same procedure as in Example 6-1 was followed to measure the temperature change over time and visually observe the properties. The results are shown in Table 3. Example 6-3 The same procedure as in Example 6-1 was followed except that the surface was not sprayed with mist, and the temperature change over time was measured and the properties were visually observed. The results are shown in Table 3.

[0057] [Table 3]

[0058] According to Table 3, it was found that in Example 6-2, the deep layer temperature was highest in the first 20 minutes, while in Example 6-3, the deep layer temperature was highest after the last 20 minutes. It was also found that in Example 6-1, the surface temperature decreased quickly, while in Example 6-2, the surface temperature was highest in the first 20 minutes. Overall, it was found that the temperature immediately after heating was high in Example 6-2, which retained moisture, while the temperature of powdered Example 6-3 tended to be slightly slower to cool.

[0059] Generally, the air layer (thermal conductivity 0.025 to 0.030 W / m / K) has the highest heat retention effect, and thermos flasks create a vacuum by eliminating the air layer, creating an insulating effect and retaining heat. In light of this, it is expected that a dry material with high porosity will have air between the particles, creating air layers, and therefore high heat retention, meaning that the temperature at the center will be high, but the air layer keeps the heat in and makes it difficult for heat to be transmitted to the outside, so the temperature felt by the body will not be as hot, and this characteristic was clearly evident in Example 6-3.

[0060] On the other hand, the reason why the deep layer temperature in the first 20 minutes of Example 6-2 is highest when it contains a lot of moisture is thought to be because, unlike Example 6-3, the inherent water retention of the material and the property of water to store heat are utilized to retain heat. Looking at the results of Example 6-1 in Table 3, although the porosity is higher than that of coral or sand, the heat dissipation in the deep layer was significant, and it was speculated that factors such as the material and water retention have a greater impact than the porosity when spraying water for heating.

[0061] Furthermore, it was found that calcium phosphate hardens when it absorbs moisture, so this point must be taken into consideration when blending it.

[0062] Example 7 (measurement with different ratios of salt and calcium phosphate) A total of 100g of coarse salt (origin: Setouchi coarse salt, manufacturer: Salt Company, Inc.) and calcium phosphate were placed into a nonwoven fabric measuring approximately 17cm in length and 11.5cm in width, folded in half lengthwise (approximately 8.5cm in length and 11.5cm in width), and heated in a 900W microwave for 1 minute. As shown in Figure 6, the fabric was removed and placed on top of a newspaper, the folded part was then returned to its original position, and a thermometer was inserted. The measurement results of the temperature change over time are shown in Table 4.

[0063] [Table 4]

[0064] From Table 4, when the calcium phosphate ratio was 85%, the temperature and heat retention immediately after removal from the microwave were the highest. This suggests that when making a composition of multiple components, it is necessary to consider the possibility of an appropriate blend ratio. Also, since moisture oozed out of the nonwoven fabric immediately after heating, it was suggested that when using it as a warming hand warmer, it would be appropriate to place the nonwoven fabric bag containing the composition in another water-repellent, heat-resistant bag.

[0065] Example 8 (measurement with different salt and coral ratios) A total of 100g of salt and coral was placed in a nonwoven fabric measuring approximately 17cm in length and 11.5cm in width, sprayed with water 50 times, folded in half lengthwise (approximately 8.5cm in length and 11.5cm in width), and heated in a 500W microwave for 1 minute and 30 seconds. As shown in Figure 6, the fabric was removed and placed on top of a newspaper, then the folded part was returned to its original position and a thermometer was inserted. The measurement results of the change in temperature over time are shown in Table 5. The ambient environment was a room temperature of 25°C and a humidity of 51%.

[0066] [Table 5]

[0067] From Table 5, it was found that as the proportion of coral increases, it becomes harder to cool, while the temperature immediately after removing from the microwave becomes lower. As an overall trend, in the first 30 minutes, the 10% coral component had better heat retention than the 30% coral component. Taking Examples 7 and 8 together, it was suggested that when making a composition of multiple components whose surface does not harden, there is a possibility that an appropriate blending ratio exists within the range containing 5 to 20 weight percent of waste-derived, natural-derived, or animal-derived materials, regardless of the material or porosity.

[0068] Example 9 (Beaker / Coral) 100g of pure coral sand or a composition obtained by thoroughly mixing coarse salt and coral sand in a specified ratio was placed in a 150cc beaker to a total of 100g, and heated for 1 minute in a 900W microwave oven with two paper plates placed on top of each other. After heating, a cooking thermometer (DAISO C008, made of glass, indicator: kerosene) was inserted upright in the center as shown in Figure 7, and the beaker was turned over so that it fit into the spout of the beaker. The gap in the content that was created when the thermometer was turned over was filled by covering it. This operation ensured that the position of the thermometer did not change, the thermometer was set in almost the same position, moisture did not bleed into the nonwoven fabric, and it was possible to observe without moving it even a millimeter. The measurement results of the temperature change over time are shown in Table 6. The surrounding environment was set to an air conditioner temperature of 22 degrees and humidity of 35%.

[0069] [Table 6]

[0070] From Table 6, it was found that the mixture ratio of 80% salt and 20% coral or 75% salt and 25% coral has a particularly hard-to-cool property. This tendency was also seen in Example 8, which used nonwoven fabric, suggesting that this property is derived from the mixed composition, regardless of whether the outer container is nonwoven fabric or a beaker.

[0071] Example 10 (Beaker / Calcium Phosphate) The temperature change over time was observed in the same manner as in Example 9, except that calcium phosphate powder was used instead of coral sand. The results are shown in Table 7. The surrounding environment was an air conditioner with an air conditioner set at 22 degrees and a humidity of 35%.

[0072] [Table 7]

[0073] Table 7 shows that as the proportion of calcium phosphate increases, the temperature tends to become slower to cool.

[0074] Example 11 (Beaker / Silica Sand) The temperature change over time was observed in the same manner as in Example 9, except that silica sand was used instead of calcium phosphate powder. The results are shown in Table 8. The surrounding environment was an air conditioner with an air conditioner set at 22 degrees and a humidity of 35%.

[0075] [Table 8]

[0076] From Table 8, we can see that the mixture of salt and silica sand has the same cooling effect over a relatively wide range of silica sand mixing ratios, from 10% by weight to 25% by weight, but that the higher the silica sand ratio, the lower the temperature immediately after removing the food from the microwave. However, when only silica sand (11) is used, the temperature drops dramatically immediately after removing the food from the microwave. This is thought to be due to the lack of moisture in the silica sand itself.

[0077] Taking the results of Examples 9 to 11, which were carried out under the moisture conditions of coarse salt, into account, with the same mixing ratio, in terms of how difficult it is to cool, the order is calcium phosphate >> silica sand > coral sand, and it was found that, with the same mixing ratio, the temperature immediately after removing the food from the microwave generally tends to be coral sand > silica sand > calcium phosphate.

[0078] Example 12 (Beaker / 3, 4 components) Based on the results of the studies of Examples 9 to 11 above, heat dissipation tests were carried out under the same conditions as in Example 9 using the ternary and quaternary compositions shown in Table 9. The results are shown in Table 9. The surrounding environment was an air conditioner with a set temperature of 22°C and a humidity of 35%.

[0079] [Table 9]

[0080] From Table 9, it is difficult to say which of (23) and (24) is better in terms of how long it takes to cool down, but the temperature after one hour differed depending on the temperature immediately after taking it out. Comparing (23) and (25), it was found that by replacing all of the calcium phosphate with silica sand, the temperature immediately after taking it out of the microwave rose dramatically.

[0081] Example 13 (Cushion-surrounded beaker / 3, 4 components) As shown in Figures 8 and 9, a heat dissipation test was conducted under the same conditions as in Example 12, except that a polyethylene food shelf cushion sheet was wrapped around the product four times. The results are shown in Table 10. The surrounding environment was an air conditioner with an air conditioner set at 22 degrees and a humidity of 35%.

[0082] [Table 10]

[0083] From Table 10, the σ 2 The value of was reduced, indicating that blocking heat radiation from the beaker glass had brought the experiment closer to an ideal environment. With the three and four components (27), (28), (29), and (31), the temperature immediately after removing from the microwave was low, but they all tended to be slow to cool, while with the composition (30) of coarse salt, coral, and silica sand, the temperature was high immediately after removing from the microwave, but it cooled somewhat quickly, a tendency similar to that of Example 12. Also, a comparison with the B value in Table 9 indicates that the compositions generally tended to be slower to cool.

[0084] Example 14 (Study of the amount of water required until the performance of coarse salt is lost) Two patterns were used: a normal beaker 1 containing a total of 100 g of coarse salt in a 150 cc beaker, and a beaker 2 wrapped in a polyethylene food shelf cushion sheet. These were heated for 1 minute in a 900 W microwave oven with two paper plates laid on top. After heating, as shown in Figure 7, a cooking thermometer (DAISO C008, made of glass, indicator: kerosene) was inserted upright in the center and the beaker was turned over so that it fit into the spout of the beaker. The gap in the contents that was created when the thermometer was turned over was filled with a cover, and the temperature change over time was measured. Here, the coarse salt that had not been treated was used as the "wet" sample, and the salt that had been heated in a microwave oven at 900 W for 1 minute four times, after which 1% of the moisture had been removed and the weight was 99 g, was used as the "dry" sample. The results are shown in Table 11. The surrounding environment was an air conditioner set at 22 degrees and humidity at 35%.

[0085] [Table 11]

[0086] Comparing the B values ​​of beaker 2 in (34) and (35) in Table 11, it is believed that even if 1% of the water is lost from the coarse salt, there is no significant change in the resistance to cooling, but the temperature immediately after removing it from the microwave drops significantly, and it is no longer possible to obtain satisfactory characteristics as a pocket warmer. Conversely, it is suggested that as long as the salt component always retains 1% moisture, sufficient characteristics can be maintained.

[0087] Example 15 (Study of the amount of water required to restore the performance of coarse salt) 99g of dry coarse salt was placed in 150cc beakers 1 and 2, and the temperature immediately after removing the salt from the microwave was compared between spraying it 5 times (equivalent to 1cc) and spraying it 10 times (equivalent to 2cc). The results are shown in Table 12. The surrounding environment was an air conditioner with a set temperature of 22 degrees and a humidity of 35%.

[0088] [Table 12]

[0089] Table 12 shows that the properties of the coarse salt can be restored by spraying it five times, but even if it is sprayed ten times, there is almost no change in the temperature immediately after removing it from the microwave. This suggests that if a pocket warmer is placed in a non-permeable bag beforehand and an excess amount of spray is sprayed, it is possible to heat the salt in the microwave several times.

[0090] Example 16 (Cushion-surrounded beaker / 3, 4 components) A heat dissipation test was carried out under the same conditions as in Example 13. The results are shown in Table 13. The surrounding environment was an air conditioner with a set temperature of 22 degrees and a humidity of 35%.

[0091] [Table 13]

[0092] From Table 13, it can be seen that the temperature immediately after (41) is lower than that of (40), but there is no significant difference after 5 minutes, so (41) is considered to be safer to use.

[0093] Example 17 (Comparison of temperature changes between surface temperature and deep temperature of nonwoven fabric) A nonwoven bag was packed with 100g of salt, coral sand, calcium phosphate, and silica sand, and heated for 1 minute in a 900W microwave oven with two paper plates placed inside. After heating, the bag was immediately removed and a cooking thermometer (DAISO C008, glass, indicator: kerosene) was inserted into the center of the nonwoven as shown in Figure 10, while another thermometer was placed on the surface of the nonwoven and fixed in place with packing tape. The nonwoven was then placed over the thermometer on the surface and a heat dissipation test was performed. The results are shown in Table 14. The surrounding environment was an air conditioner with an air conditioner set to 22°C and a humidity of 35%.

[0094] [Table 14]

[0095] From Table 14, it can be seen that after 5 minutes, the heat is gradually transferred from the inside to the nonwoven fabric, and the surface temperature becomes higher. The surface temperature immediately afterwards is 44°C-58°C, but it is thought to be higher. According to various literature, low-temperature burns can occur when touching a 44°C object for 3-4 hours, a 46°C object for 30 minutes-1 hour, or a 50°C object for 2-3 minutes. From this perspective, it was found that direct contact with (46), (47), (49), and (50), which contain silica sand, is not recommended in the early stages of heat dissipation, and that temperature adjustment with a cloth cover or the like is necessary, but it was found that there is little risk of low-temperature burns with products that do not contain silica sand.

[0096] Example 18 (Comparison of deep temperature and sensible temperature) A nonwoven bag was packed with 100g of salt, coral sand, calcium phosphate, and silica sand, and heated for 1 minute in a 900W microwave oven with two paper plates laid on top of each other. After heating, the bag was immediately taken out and a cooking thermometer (DAISO C008, made of glass, indicator: kerosene) was inserted into the center of the bag as shown in Figure 11. The opening of the bag and the thermometer were closed by squeezing them together in the hand, and the part containing the mixture was touched and the temperature and sensation were recorded. When touching the mixture, the hand that was least warm was used. The results are shown in Table 15. The surrounding environment was an air conditioner set at 22 degrees and humidity at 35%.

[0097] [Table 15]

[0098] From Table 15, it was found that when compared with the temperatures obtained in the experiment on deep temperature and surface temperature in Example 17, the deep temperature that felt lukewarm to the surface touch lasted for about 20 to 30 minutes.

[0099] Example 19 (Production of a sculpture containing salt and granite powder - Okijio) Salt (product name: "Nihonkaisui Table Salt" (Setouchi), manufactured by Nihonkaisui Co., Ltd., Ako Factory), granite powder (from Okazaki, obtained from a lantern shop in Okazaki), and starch glue (Fueki AB glue, manufactured by Fueki Glue Kogyo Co., Ltd.) were prepared. The salt was powdered in advance using a mill, and then mixed well in a ratio of 10 parts salt, 2 parts granite powder, 2 parts starch glue, and 0.4 parts water to create the sculpture. For the head, a straw was cut vertically to make a semicircular cross section, and pressed to draw eyes. After that, it was left to dry naturally for at least one day, and the cheeks were colored red with poster paint to obtain a sculpture (Jizo) as shown in Figure 12. The heart ornament held by Jizo was made of paper clay, dried, colored with poster paint, dried again, and attached with starch glue to the Jizo that had been dried for more than one day. It was found that this sculpture, apart from the paper clay, is light and does not use any glue or plaster, and therefore has the characteristic that it easily dissolves when placed in water.

[0100] Example 20 After drawing the face, I found that applying a mixture of 2 parts water and 1 part starch glue with a brush made the face firmer.

[0101] Example 21 (Modeling with salt and granite powder - Effect of adding silica sand) Salt (product name: "Nihonkaisui Table Salt" (Setouchi), manufactured by Nihonkaisui Co., Ltd. Ako Factory), granite powder (from Okazaki, obtained from a lantern shop in Okazaki), silica sand powder (from Gifu Prefecture, manufactured by Shirai Soap Co., Ltd., sold by Rakuraku Eco Shop Co., Ltd.), and starch paste (Fueki AB paste, manufactured by Fueki Glue Kogyo Co., Ltd.) were prepared, and the salt was first powdered in a mill, then mixed well in a ratio of 10 parts salt, 1 part granite powder, 0.1 parts silica sand powder, 1 part starch paste, and 1 part water, and shaped. Thereafter, a shaped object was obtained through the same process as in Example 19. The resulting shaped object had increased density and was firmly packed.

[0102] The present invention is not limited to the above-described embodiment, and not all of the configurations described in the above-described embodiment are essential requirements for the present invention. The present invention may be modified in various ways within the scope of the technical concept of the present invention. [Industrial Applicability]

[0103] The warming pocket warmer of the present invention can be used at home while sleeping by putting it in a belly warmer, or it can be provided to customers at beauty salons as a neck pillow during shampooing, at barber shops as a neck pillow during shaving, and at dental clinics as a neck pillow or belly warmer during waiting time or treatment. It can also be heated in a microwave oven and used in school health rooms. It can also be used in acupuncture and moxibustion clinics, esthetic salons, osteopathic clinics, and chiropractic clinics. In addition, since the manufacturing process of the warming pocket warmer itself is simple, it can be used in vocational centers to create jobs and be industrially useful. The amulet of the present invention uses pet bones and human bones as ingredients, providing a new form of hand-held memorial service for lost pets and deceased people. The shaped object of the present invention does not require a mold that is essential for the manufacture of "morishio", a traditional Japanese custom, and can save the effort of manufacturing morishio. In addition, by increasing the variety of shaped objects, this custom can be made more familiar. [Explanation of symbols]

[0104] 10, 20 Warm Pocket Warmer (souvenir) 2. Permeable materials 3 Sealing parts (zippers) 4 Impermeable bag 5 Opening Edge 6 Outer bag 7. Welding margin 8 Heat retention material 11 Multi-layered warming pocket warmer 12 Cloth storage bag 13 First Pocket 14a, 14b Partition cloth 15 3rd Pocket 17 Second Pocket 18 Heat-resistant materials 22 Coral

Claims

[Claim 1] A warming hand warmer using a composition consisting essentially of one or more materials selected from coral sand, coral pieces, shells, rubbish (true) pearls, pearl powder, and human or animal bone (powder), tooth (powder), or horn (powder), and sodium chloride, The warming pocket warmer contains 70 to 95% by weight of sodium chloride and 5 to 30% by weight of the one or more materials in total based on the total weight of the composition.

Citation Information

Patent Citations

  • JP1979131393U

  • Weather strip for a vehicle

    JP1986024248U

  • Production of granulated salt

    JP1992027361A

  • Amulet of okinawa

    JP1997238821A

  • Far infrared ray warm band

    JP1999197175A