Manufacturing method of aluminum member

An anodic oxide film with an amorphous and crystalline layer on aluminum members, formed via specific electrolytic treatment, addresses the balance of insulation, corrosion, and wear resistance, achieving superior performance across these properties.

JP7588369B2Active Publication Date: 2024-11-22HOKKAIDO UNIVERSITY +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020118492
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-07-09
Publication Date
2024-11-22
Estimated Expiration
2040-07-09

AI Technical Summary

Technical Problem

Existing anodic oxide films on aluminum members face challenges in balancing insulation, corrosion resistance, and wear resistance, with barrier type films being dense but hard to thicken, and plasma electrolytic films being porous and lacking insulation.

Method used

Forming an anodic oxide film with an amorphous layer of amorphous aluminum oxide and a crystalline layer of crystalline aluminum oxide on the surface of an aluminum member, achieved through anodizing treatment in an electrolytic solution with specific pH conditions, leading to dielectric breakdown and crystal layer formation.

Benefits of technology

The resulting film provides excellent insulation, corrosion resistance, and wear resistance, combining the benefits of both film types, with the amorphous layer ensuring density and the crystalline layer enhancing hardness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588369000003
    Figure 0007588369000003
  • Figure 0007588369000004
    Figure 0007588369000004
  • Figure 0007588369000005
    Figure 0007588369000005
Patent Text Reader

Abstract

To provide an aluminum member and a production method of the same, wherein the aluminum member has an anodic oxide film having excellent insulation, corrosion resistance, and wear resistance.SOLUTION: An aluminum member 1 comprises: a parent material 2 made of aluminum or an aluminum alloy; and an anodic oxide film 3 formed on a surface of the parent material 2. The anodic oxide film 3 has an amorphous layer 31 made of an amorphous aluminum oxide and formed on the parent metal 2, and a crystalline layer 32 made of a crystalline aluminum oxide and formed on the amorphous layer 31.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an aluminum member and a manufacturing method thereof. [Background technology]

[0002] Aluminum members have various applications, such as building materials, housings for electronic devices, machine parts, etc. The surfaces of the aluminum members may be provided with functional coatings for the purpose of imparting properties such as design, corrosion resistance, abrasion resistance, and insulation properties.

[0003] Anodized films are known as functional films formed on the surface of aluminum members. The properties of anodized films vary depending on the structure and manufacturing method of the anodized film. For example, Patent Document 1 describes a method for forming an anodized alumina film, which is characterized in that a substrate having exposed aluminum on its surface is immersed in a first electrolytic solution in which an electrolyte containing boron is dissolved to anodize the aluminum, and then the substrate is immersed in a second electrolytic solution in which an electrolyte not containing boron is dissolved to further anodize the aluminum.

[0004] Furthermore, Patent Document 2 describes a method for forming a ceramic coating, which comprises forming a ceramic coating containing aluminum oxide on the surface of an aluminum or aluminum alloy substrate by anode spark discharge in an aqueous electrolytic bath containing (a) a nitrogen atom-containing cation and (b) an aminocarboxylate anion having a stability constant of 9 or more for aluminum. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 10-107027 [Patent Document 2] JP 2003-171794 A Summary of the Invention [Problem to be solved by the invention]

[0006] According to the method of Patent Document 1, a type of anodized film called a barrier-type anodized film can be formed. The barrier-type anodized film is relatively dense and has excellent insulating properties and corrosion resistance. However, it is difficult to increase the thickness of the barrier-type anodized film, and therefore it has problems such as poor wear resistance and hardness.

[0007] According to the method of Patent Document 2, a type of anodic oxide film called a plasma electrolytic oxidation film can be formed. The plasma electrolytic oxidation film is made of crystalline aluminum oxide and can be easily thickened, so it has excellent abrasion resistance. However, the plasma electrolytic oxidation film has a problem of poor insulation because pores are easily formed.

[0008] The present invention has been made in view of the above background, and has an object to provide an aluminum member having an anodized coating that is excellent in insulation properties, corrosion resistance, and abrasion resistance, and a method for producing the same. [Means for solving the problem]

[0009] One aspect of the present invention reference The embodiment includes a base material made of aluminum or an aluminum alloy, and an anodic oxide film formed on the surface of the base material, The anodized coating is an amorphous layer formed on the base material and made of amorphous aluminum oxide; The aluminum member has a crystalline layer made of crystalline aluminum oxide and formed on the amorphous layer.

[0010] The present invention one The present invention relates to a method for producing an aluminum member according to the above embodiment, The method for producing an aluminum member includes anodizing the base material in an electrolyte containing boron atoms and having a pH of 7.0 or more and 12.0 or less, thereby forming the anodic oxide film. Effect of the Invention

[0011] The surface of the aluminum member has an anodized coating including the amorphous layer and the crystalline layer. The amorphous layer is made of a relatively dense amorphous aluminum oxide, and therefore can provide the aluminum member with excellent insulation properties and corrosion resistance. The crystalline layer is made of a relatively hard crystalline aluminum oxide, and therefore can provide the aluminum member with excellent wear resistance.

[0012] In this way, the anodized film combines the excellent insulation and corrosion resistance of a barrier-type anodized film with the excellent wear resistance of a plasma electrolytic oxidation film, and therefore the aluminum member has excellent insulation, corrosion resistance and wear resistance.

[0013] In the method for manufacturing an aluminum member, the base material is anodized in the specific electrolyte. By using the specific electrolyte as the electrolyte, the amorphous layer can be formed in the early stage of the anodization. When the anodization proceeds and the thickness of the amorphous layer becomes thick to a certain degree, dielectric breakdown occurs on the surface of the amorphous layer, and discharge accompanied by light emission is likely to occur. This allows the crystalline layer to be formed on the amorphous layer.

[0014] Therefore, according to the method for producing an aluminum member, the anodized film can be formed on the base material by a simple method.

[0015] As described above, according to the above-described embodiment, it is possible to provide an aluminum member having an anodized coating that is excellent in insulation properties, corrosion resistance, and abrasion resistance, and a method for manufacturing the same. [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is a cross-sectional view of an aluminum member in an embodiment. [Diagram 2]FIG. 2 is an electron microscope image of a fracture surface of the anodized coating of test material B in the example. [Diagram 3] FIG. 3 is an X-ray diffraction chart of test material B in the example. [Figure 4] FIG. 4 is an electron microscope image of the surface of the anodized film of test material L in the example. [Diagram 5] FIG. 5 is an explanatory diagram of a method for measuring the maximum width of a pore. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] (Aluminum parts) The aluminum member has a base material and an anodized coating formed on the surface of the base material. The shape of the aluminum member is not particularly limited, and may be an appropriate shape depending on the application of the aluminum member. The anodized coating may be provided on the entire surface of the base material, or may be provided on only a part of the surface of the base material.

[0018] The material of the base material of the aluminum member is not particularly limited as long as it is aluminum or an aluminum alloy. For example, the base material may be high-purity aluminum, JIS A1000 series aluminum, A2000 series alloys, A3000 series alloys, A4000 series alloys, A5000 series alloys, A6000 series alloys, A7000 series alloys, and A8000 series alloys.

[0019] For example, when the base material is a relatively high-strength aluminum alloy such as an A5000 series alloy or an A6000 series alloy, the strength of the aluminum member can be increased, and therefore, an aluminum member having a base material made of an A5000 series alloy or an A6000 series alloy is suitable for applications requiring high strength, such as automotive materials and structural materials.

[0020] Furthermore, for example, when the base material is A1000 series aluminum or A3000 series alloy, the coloring of the anodized film can be suppressed, and the color tone of the aluminum member can be made closer to white. Such an aluminum member can be used in applications where a white appearance is required. Furthermore, the closer the color tone of the aluminum member is to white, the easier it is to color the surface of the aluminum member to a desired color. Therefore, an aluminum member having a base material made of A1000 series aluminum or A3000 series alloy is suitable for applications where design is required, such as exterior materials and electronic device housings.

[0021] An anodic oxide film is formed on the base material. The anodic oxide film has an amorphous layer formed on the base material and a crystalline layer formed on the amorphous layer.

[0022] The amorphous layer is composed of amorphous aluminum oxide. As described above, the amorphous layer is relatively dense, and therefore can provide the aluminum member with insulating properties and corrosion resistance. The composition of the aluminum oxide constituting the amorphous layer is determined according to the material of the base material. That is, the amorphous layer is mainly composed of aluminum atoms and oxygen atoms. In addition to aluminum atoms and oxygen atoms, the amorphous layer may also contain alloy elements contained in the base material.

[0023] Whether or not an amorphous layer is formed in the anodized coating can be determined based on an X-ray diffraction chart obtained by X-ray crystal structure analysis. That is, if a broad peak having an apex in the diffraction angle range of 20° to 40° appears in the X-ray diffraction chart, it can be determined that an amorphous layer made of amorphous aluminum is formed in the anodized coating.

[0024] The thickness of the amorphous layer may be, for example, 0.05 μm or more and 1.0 μm or less. In this case, the effect of further reducing defects in the amorphous layer and improving the insulation and corrosion resistance of the aluminum member can be more reliably achieved. From the viewpoint of more reliably obtaining such an effect, the thickness of the amorphous layer is preferably 0.10 μm or more and 0.90 μm or less, and more preferably 0.20 μm or more and 0.80 μm or less.

[0025] The thickness of the amorphous layer is a value calculated by the following method. That is, first, an electron microscope image is obtained by observing the cross section of the aluminum member using a scanning electron microscope or the like. Ten measurement positions are randomly selected from the amorphous layer in the electron microscope image. Then, the arithmetic average value of the thicknesses of the amorphous layer at these measurement positions is taken as the thickness of the amorphous layer.

[0026] A crystal layer made of crystalline aluminum oxide is laminated on the amorphous layer. As described above, the crystal layer made of crystalline aluminum oxide is relatively hard, and therefore can impart wear resistance to the aluminum member. The crystal layer is made of crystalline aluminum oxide such as α-Al2O3 or γ-Al2O3. More specifically, the crystal layer may be made of α-Al2O3 or γ-Al2O3. The crystal layer may also be made of α-Al2O3 and γ-Al2O3. Furthermore, the crystal layer may contain alloy elements contained in the base material in addition to these aluminum oxides.

[0027] Whether or not a crystal layer is formed on the anodized film can be determined based on an X-ray diffraction chart obtained by X-ray crystal structure analysis. That is, when a diffraction peak derived from a crystalline aluminum oxide such as α-Al2O3 or γ-Al2O3 appears in the X-ray diffraction chart, it can be determined that a crystal layer is formed on the anodized film.

[0028] The thickness of the crystal layer may be, for example, 1.0 μm or more. In this case, the crystal layer is sufficiently thick, and the effect of improving the wear resistance can be more reliably achieved. From the viewpoint of more reliably obtaining such an effect, the thickness of the crystal layer is preferably 2.0 μm or more, and more preferably 3.0 μm or more.

[0029] The thickness of the crystal layer is preferably 5.0 μm or more and 15.0 μm or less, more preferably 6.0 μm or more and 14.0 μm or less, and even more preferably 7.0 μm or more and 13.0 μm or less. In this case, the color tone of the aluminum member can be made closer to white. As a result, the design of the aluminum member can be further improved.

[0030] The method for measuring the thickness of the crystalline layer is the same as the method for measuring the thickness of the amorphous layer described above. That is, first, an electron microscope image is obtained by observing the cross section of the aluminum member using a scanning electron microscope or the like. Ten measurement positions are randomly selected from the crystalline layer in this electron microscope image. Then, the arithmetic average value of the thicknesses of the crystalline layer at these measurement positions is taken as the thickness of the crystalline layer described above.

[0031] The crystal layer may have a plurality of pores that open to the surface of the aluminum member. In this case, the crystal layer sufficiently scatters external light that enters the anodized film, and the transparency of the anodized film can be further reduced. By reducing the transparency of the anodized film, the color tone of the base material that is the base material can be effectively concealed. As a result, the color tone of the aluminum member can be made closer to white, and the design can be further improved.

[0032] In order to ensure that such an effect is achieved, the crystal layer preferably has pores with an average diameter of 1 μm or more and 20 μm or less.

[0033] The average diameter of the pores present in the crystal layer is a value calculated by the following method. That is, first, an electron microscope image is obtained by observing the surface of the crystal layer using a scanning electron microscope or the like. In this electron microscope image, 10 pores to be measured are randomly selected. Next, the maximum width of the pores to be measured, that is, the width of the pores from various directions, is measured, and the largest width value among the obtained values ​​is determined. The arithmetic average value of the maximum widths of the 10 pores determined in this way is taken as the average diameter of the pores.

[0034] The arithmetic mean roughness Ra of the surface of the anodized film is preferably 0.5 μm or more and 1.5 μm or less. In this case, the external light incident on the anodized film is sufficiently scattered on the surface, and the transparency of the anodized film can be further reduced. By reducing the transparency of the anodized film, the color tone of the base material, which is the base material, can be effectively concealed. As a result, the color tone of the aluminum member can be made closer to white, and the design can be further improved. The arithmetic mean roughness Ra of the surface of the anodized film is a value measured by a method conforming to JIS B0601:2013.

[0035] The L* value in the CIE 1976 L*a*b* color space, obtained by measuring the color tone of the surface having the anodized film of the aluminum member, is preferably 70.0 or more. The L* value in the CIE 1976 L*a*b* color space ranges from 0 to 100, with a higher value indicating a higher lightness of the color.

[0036] By setting the L* value of the surface of the aluminum component having the specific configuration within the specific range, the color tone of the surface of the aluminum component when viewed with the naked eye can be made closer to white. As described above, an aluminum component having a surface color tone close to white can be suitably used in applications where a white appearance is required.

[0037] Furthermore, when the surface of a white aluminum component is colored chromatically by painting or the like, the color tone of the colored component is less likely to be influenced by the color tone of the base material, making it easier to achieve the desired chromatic color.

[0038] Thus, an aluminum member having an L* value within the above-mentioned specific range has excellent designability because it can easily realize a desired color tone. From the viewpoint of further improving the designability of the aluminum member, the L* value in the CIE 1976 L*a*b* color space is preferably 75 or more, and more preferably 80 or more. From the viewpoint of further improving the designability of the aluminum member, the closer the L* value is to the upper limit of 100, the more preferable it is.

[0039] (Method of manufacturing aluminum components) The method for producing an aluminum member includes a step of anodizing a base material in an electrolyte containing boron atoms and having a pH of 7.0 to 12.0. When anodizing is performed on a base material made of aluminum or an aluminum alloy using the specific electrolyte, an amorphous layer made of amorphous aluminum oxide is formed on the surface of the base material in the early stage of the anodizing.

[0040] As the anodization process progresses, the thickness of the amorphous layer increases, and the electrical insulation of the amorphous layer increases accordingly. When the electrical insulation of the amorphous layer increases and the anodic reaction does not easily occur on the surface of the base material, minute and irregular discharges called micro-arcs occur intermittently on the surface of the amorphous layer. The micro-arcs cause the surface of the amorphous layer to repeatedly melt and solidify, forming a crystalline layer on the surface of the amorphous layer.

[0041] As described above, by performing anodizing treatment using the specific electrolyte, it is possible to easily form an anodized coating having an amorphous layer laminated on a base material and a crystalline layer laminated on the amorphous layer.

[0042] In the method for manufacturing an aluminum member, the base material may be subjected to pretreatment such as degreasing and polishing, if necessary, before the base material is anodized. As the degreasing, for example, an alkaline degreasing treatment using an alkaline cleaning solution can be used. By performing the degreasing treatment, the gloss value of the aluminum member obtained after the anodizing treatment can be reduced, and an aluminum member with no gloss can be easily obtained.

[0043] In addition, the polishing treatment can be, for example, a chemical polishing treatment, a mechanical polishing treatment, an electrolytic polishing treatment, or the like. By performing the polishing treatment, the gloss value of the aluminum member obtained after the anodizing treatment can be increased, and a glossy aluminum member can be easily obtained. From the viewpoint of increasing the gloss value of the aluminum member, it is preferable to perform an electrolytic polishing treatment on the base material.

[0044] The electrolyte used in the anodization treatment may be a liquid containing boron atoms and having a pH of 7.0 to 12.0. For example, an aqueous solution of one or more electrolytes selected from the group consisting of boric acid and borates may be used. Specific examples of the electrolyte used in the electrolyte include salts of boric acid and ammonia, such as ammonium tetraborate and ammonium pentaborate, and salts of boric acid and alkali metal elements, such as sodium tetraborate.

[0045] From the viewpoint of more easily forming an anodic oxide film having the specific structure, the electrolytic solution is preferably an aqueous solution of an electrolyte containing ammonium tetraborate.

[0046] The concentration of the electrolyte can be appropriately set within the range of, for example, 0.1 mol / L or more and 1.0 mol / L or less. The concentration of the electrolyte in the anodizing treatment is preferably 0.2 mol / L or more and 0.9 mol / L or less. In this case, the growth of the anodized film during the anodizing treatment can be further promoted. As a result, the thickness of the anodized film can be more easily increased.

[0047] The temperature of the electrolytic solution in the anodizing treatment can be appropriately set within the range of, for example, 283 K or more and 343 K or less. The temperature of the electrolytic solution in the anodizing treatment is preferably 303 K or more and 343 K or less. In this case, the concentration of the electrolytic solution can be appropriately increased, and the growth of the anodized film during the anodizing treatment can be further promoted. As a result, the thickness of the anodized film can be more easily increased.

[0048] In anodizing, 10A / m 2 More than 200A / m 2 It is preferable to carry out constant current electrolysis at the following current density. By carrying out the anodizing treatment under such current conditions, the growth of the anodized film during the anodizing treatment is further promoted and the anodized film can be grown more uniformly.

[0049] The treatment time in the anodizing treatment can be, for example, 5 minutes or more. By setting the treatment time in the anodizing treatment to 5 minutes or more, it is possible to more easily form an anodized coating in which a crystalline layer is laminated on an amorphous layer. In addition, the longer the treatment time in the anodizing treatment, the thicker the crystalline layer can be, and the more the wear resistance of the aluminum member can be improved. From this viewpoint, the treatment time in the anodizing treatment is preferably 10 minutes or more, more preferably 20 minutes or more, and even more preferably 30 minutes or more. EXAMPLES

[0050] An embodiment of the aluminum member and a manufacturing method thereof will be described with reference to Fig. 1 to Fig. 4. As shown in Fig. 1, the aluminum member 1 of this embodiment has a base material 2 made of aluminum or an aluminum alloy, and an anodized coating 3 formed on the surface of the base material 2. The anodized coating 3 has an amorphous layer 31 made of amorphous aluminum oxide and formed on the base material 2, and a crystalline layer 32 made of crystalline aluminum oxide and formed on the amorphous layer 31.

[0051] The aluminum member 1 of this example can be produced by the following method. First, a base material 2 made of high-purity aluminum with an Al purity of 99.99% by mass is prepared. The base material 2 is a square plate with each side measuring 20 mm. The surface of the base material 2 is ultrasonically cleaned using ethanol to perform a degreasing process, and then electrolytic polishing is performed.

[0052] One side of the base material 2 that has been pretreated in this manner is subjected to anodizing treatment in an electrolyte containing boron atoms and having a pH of 7.0 or more and 12.0 or less, thereby forming an anodized film 3 on the surface of the base material 2.

[0053] In the anodizing treatment, for example, the electrolyte and treatment conditions shown in Table 1 can be used. A more detailed configuration of the aluminum member 1 will be described below using test materials A to K shown in Table 1 as examples. Note that test materials L to N shown in Table 1 are test materials for comparison with test materials A to K. Test materials L to N can be produced in the same manner as test materials A to K, except that the electrolyte and treatment conditions are changed as shown in Table 1.

[0054] ·Anodized film structure The structure of an anodic oxide film can be evaluated by combining cross-sectional observation using a field emission scanning electron microscope (FE-SEM) and identification of the constituent materials using an X-ray diffraction device.

[0055] When performing the cross-sectional observation, first, each of the test materials A to N is V-bent so that the anodized surface is on the outside, and the anodized film is broken. The layered structure of the anodized film can be evaluated by observing the fractured surface of the anodized film using FE-SEM. If the anodized film is composed of a single layer as a result of the cross-sectional observation, it is recorded as "single layer" in the "Layered structure" column of Table 2, and if it is a two-layer structure, it is recorded as "two layers" in the same column. If no anodized film is formed, it is recorded as "-" in the same column.

[0056] In addition, in identifying the constituent substances, an X-ray diffraction device (Rigaku Corporation, "RINT2500") is used to irradiate the anodized coatings of test materials A to N with X-rays to obtain X-ray diffraction charts. Then, by comparing the diffraction peaks appearing in the X-ray diffraction charts with the diffraction patterns of known substances, the substances corresponding to the diffraction peaks appearing in the X-ray diffraction charts can be identified. In addition, if a broad peak having an apex in the diffraction angle range of 20° to 40° appears in the X-ray diffraction chart, it can be determined that the anodized coating contains an amorphous substance.

[0057] The "Constituent Substances" column in Table 2 shows the substances contained in test materials A to N.

[0058] As shown in Table 2, the anodized films 3 of the test materials A to K all have a two-layer structure. More specifically, like the test material B shown in FIG. 2 as an example, the anodized films 3 of the test materials A to K have a layer of relatively uniform thickness formed on the base material 2 with few defects, and a layer formed on the above layer that contains pores, discharge marks, melt marks, etc.

[0059] As an example, an X-ray diffraction chart of test material B is shown in Fig. 3. The vertical axis of Fig. 3 represents the diffraction intensity, and the horizontal axis represents the diffraction angle 2θ (°). Although not shown in the figure, the X-ray diffraction charts of test material A and test materials C to K are similar to that of test material B. As shown in Table 2, these results show that the anodized coatings 3 of test materials A to K are composed of crystalline aluminum oxides α-Al2O3 and γ-Al2O3, and amorphous aluminum oxide.

[0060] On the other hand, in test material L, which had a shorter anodizing treatment time than test materials A to K, a single-layer anodized coating made of amorphous aluminum oxide is formed, as shown in Table 2. From a comparison of test materials A to K with test material L, it can be seen that the layer formed on base material 2 in test materials A to K is amorphous layer 31 made of amorphous aluminum oxide, and a crystalline layer 32 is formed on amorphous layer 31.

[0061] Because the electrolyte in the test material M is a sodium hydroxide solution, the dissolution rate of the anodized film and the base material is faster than the growth rate of the anodized film during the anodizing treatment. Therefore, it is difficult to form an anodized film on the surface of the test material M.

[0062] Since the electrolyte for test material N is an aqueous sulfuric acid solution, no dielectric breakdown occurs during the anodizing process. Therefore, a single-layer anodized film made of amorphous aluminum and having fine pores is formed on the surface of test material N.

[0063] Surface structure of the crystal layer The surfaces of the test materials A to K are observed using an FE-SEM to evaluate the surface structure of the crystal layer 32. As shown in an electron microscope image of the surface of the test material B in FIG. 4 as an example, a large number of pores 321 are present on the surface of the crystal layer 32.

[0064] The average diameter of the pores 321 present in the crystal layer 32 is calculated as follows. First, ten pores 321 to be measured are randomly selected from the pores 321 present in the electron microscope image. Next, as shown in an example in FIG. 5, the width W of the pores 321 to be measured is measured from various directions. Then, the maximum value of the widths W of the pores 321 measured from the various directions is taken as the maximum width W of the pore. max The maximum width W of the ten pores 321 thus obtained is max The arithmetic mean value of these is taken as the average diameter of the pores 321.

[0065] The average diameter of the pores 321 in the test materials A to K are shown in Table 2. Note that for the test materials L and M which do not have the crystal layer 32, there are no pores, so the symbol "-" is entered in the "average pore diameter" column in Table 2. The average diameter of the pores in the test material N can be calculated in the same manner as for the test materials A to K. The average diameter of the pores in the test material N is shown in Table 2.

[0066] As shown in Table 2, the average pore diameters of the test materials A to K are 1 μm or more and 20 μm or less.

[0067] Evaluation of arithmetic mean roughness Ra The arithmetic mean roughness Ra of the surface of the anodized film can be evaluated by a method conforming to JIS B0601:2013. Specifically, first, the anodized film is observed at a magnification of 50 times using a laser microscope (OLS-3000 manufactured by Olympus Corporation) to obtain a three-dimensional image including the height information of the surface of the anodized film. In the three-dimensional image thus obtained, the arithmetic mean roughness Ra of three randomly selected points is calculated. Then, the arithmetic mean value of the arithmetic mean roughness Ra of the surface of the anodized film is set as the arithmetic mean roughness Ra of the surface of the anodized film. The arithmetic mean roughness Ra of the surfaces of the anodized film of the test materials A to K and the test material N are the values ​​shown in Table 2. Note that the test materials L and M do not have the crystal layer 32, so it is not necessary to measure the arithmetic mean roughness Ra. Therefore, the symbol "-" is entered in the "arithmetic mean roughness Ra" column for these test materials.

[0068] Next, a method for evaluating the characteristics of the aluminum member 1 will be described.

[0069] Appearance characteristics The appearance characteristics of the aluminum member 1 can be evaluated based on the uniformity of the appearance of the anodized film 3 by visual inspection and SEM observation. The symbols given in the "Appearance characteristics" column in Table 2 have the following meanings. A: The appearance of the anodized film is uniform when observed visually and by SEM. B: The appearance of the anodized film is uniform when visually inspected, but SEM observation reveals a mixture of areas with and without discharge marks. C: The appearance of the anodized film is uneven when visually inspected, but there are areas where discharge marks have been formed when observed under SEM. D: The appearance of the anodized film is uneven when visually inspected, and no discharge marks are present when observed under SEM.

[0070] ·Design The design of the aluminum member 1 can be evaluated based on the color tone of the surface having the anodized film 3. The "Design" column in Table 2 shows the L* values ​​in the CIE (International Commission on Illumination) 1976 L*a*b* color space for test materials A to K and test material N. A spectrophotometer conforming to JIS Z8781-4:2013 (for example, the color meter "CC-iS" manufactured by Suga Test Instruments Co., Ltd.) can be used to measure the L* value. Note that the test material L does not have a crystal layer, so the symbol "-" is entered in the "Design" column. Also, the test material M does not have an anodized film, so the symbol "-" is entered in the "Design" column.

[0071] [Table 1]

[0072] [Table 2]

[0073] As shown in Table 1, the anodized coating 3 of test materials A to K has a two-layer structure in which a crystalline layer 32 is laminated on an amorphous layer 31. Therefore, as shown in Table 2, these test materials are expected to have both excellent insulation properties and corrosion resistance derived from the amorphous layer 31 and excellent wear resistance derived from the crystalline layer 32.

[0074] In addition, the average diameter of the pores 321 present in the crystalline layer 32 of each of the test materials A to K and the arithmetic mean roughness Ra of each of the test materials A to K are within the above-mentioned specific ranges. Therefore, the appearance of each of the test materials A to K is white and opaque, and the test materials have excellent design properties.

[0075] Since the anodizing time of the test material L is shorter than that of the test materials A to K, no dielectric breakdown occurs on the surface of the amorphous layer 31 during the anodizing treatment. Therefore, it is difficult to form a crystalline layer on the amorphous layer 31 of the test material L.

[0076] Because the electrolyte in the test material M is a sodium hydroxide solution, the dissolution rate of the anodized film and the base material is faster than the growth rate of the anodized film during anodizing treatment. Therefore, it is difficult to form an anodized film on the surface of the test material M. Therefore, it is presumed that the test material M is inferior to the test materials A to K in terms of insulation, corrosion resistance, and wear resistance.

[0077] Since the electrolyte in the test material N is an aqueous sulfuric acid solution, no dielectric breakdown occurs during anodizing. Therefore, it is difficult to form a crystal layer on the surface of the test material N. Therefore, it is presumed that the test material N has inferior wear resistance compared to the test materials A to K. In addition, since the anodized film formed on the surface of the test material N is highly transparent, the appearance of the test material N tends to be close to the color tone of the base material.

[0078] As described above, specific aspects of the aluminum member and the manufacturing method thereof have been described based on the examples. However, the aluminum member and the manufacturing method thereof according to the present invention are not limited to the aspects of the above-mentioned examples, and the configuration can be appropriately changed within the scope that does not depart from the spirit of the present invention. [Explanation of symbols]

[0079] 1 Aluminum components 2 Base material 3 Anodized film 31 Amorphous layer 32 Crystal Layer

Claims

1. A base material made of aluminum or an aluminum alloy; and an anodic oxide film formed on the surface of the base material, The anodized coating is an amorphous layer formed on the base material and made of amorphous aluminum oxide; A method for producing an aluminum member having a crystalline layer made of crystalline aluminum oxide and formed on the amorphous layer, comprising: The method for producing an aluminum member includes anodizing the base material in an electrolyte solution containing boron atoms and having a pH of 7.0 or more and 12.0 or less, thereby forming the anodized coating.

2. The method for manufacturing an aluminum member according to claim 1 , wherein the crystal layer has pores having an average diameter of 1 μm or more and 20 μm or less.

3. The method for producing an aluminum member according to claim 1 or 2, wherein the arithmetic mean roughness Ra of the surface of the anodized film is 0.5 μm or more and 1.5 μm or less.

4. The method for producing an aluminum member according to any one of claims 1 to 3, wherein an L* value in CIE 1976 L*a*b* color space, obtained by measuring a color tone of a surface having the anodized coating on the aluminum member, is 70.0 or more.

5. The method for manufacturing an aluminum member according to any one of claims 1 to 4, wherein the electrolytic solution is an aqueous solution of ammonium tetraborate.

6. In the anodizing treatment, the temperature of the electrolyte is set to 283 K or more and 343 K or less, and the current is 10 A / m 2 More than 200A / m 2 The method for producing an aluminum member according to any one of claims 1 to 5, wherein constant current electrolysis is performed at a current density below 1000 kPa.

Citation Information

Patent Citations

  • Separation of catabolic hemoglobin

    JP1983000760A

  • Method for forming anodized alumina film

    JP1998107027A

  • Method for forming ceramic film on aluminum substrate surface

    JP2003171794A

  • Aluminum alloy member, and method for forming surface protective film of aluminum alloy

    JP2015025184A

  • Production method of metal compact having anodic oxide film, metal compact having anodic oxide film, piston, and internal combustion engine

    JP2020033591A