Membrane structure
A sea-island structured film with controlled conductive filler distribution in fluororesin provides a smooth and conductive surface, addressing the issue of poor appearance in composite materials.
Patent Information
- Application Number
- JP2020150673
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-08
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2040-09-08
AI Technical Summary
Molded bodies made from composite materials of conductive fillers and fluororesins exhibit poor surface smoothness and appearance despite achieving sufficient conductivity.
A film structure is formed using a composite material of fluororesin and conductive filler with a sea-island structure, where the conductive filler is present in the sea part, and the sea and island portions contain the same fluororesin as the main component, with a surface roughness of 5 μm or less.
The film structure achieves excellent conductivity and appearance by ensuring a smooth surface with a sea-island structure and controlled distribution of conductive fillers.
Smart Images

Figure 0007588485000003 
Figure 0007588485000004 
Figure 0007588485000005
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a coating structure. [Background technology]
[0002] It has been reported that molded articles made using a composite material of a conductive filler such as carbon nanotubes and a fluororesin exhibit electrical conductivity while maintaining the heat resistance, chemical resistance, and other properties of the fluororesin (Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2014-034591 A Summary of the Invention [Problem to be solved by the invention]
[0004] The inventors used the above-mentioned composite material of conductive filler and fluororesin as a paint ingredient and coated a substrate with the paint containing the composite material to form a coating. They found that although sufficient conductivity was obtained with the use of a very small amount of conductive filler, the surface condition of the resulting coating was poor in smoothness and had a poor appearance (see Figure 2).
[0005] An object of the present disclosure is to provide a coating structure having excellent electrical conductivity and excellent appearance, and a method for producing the same. [Means for solving the problem]
[0006] The present disclosure includes the following aspects. [1] A coating structure comprising a fluororesin and a conductive filler, The surface of the coating structure has an island-sea structure, A coating structure, wherein a conductive filler is present in the sea portion of the sea-island structure. [2] The coated structure according to the above [1], wherein the sea portion and the island portion of the sea-island structure contain the same fluororesin as a main component. [3] The coated structure according to the above [1] or [2], wherein the conductive filler is a carbon nanotube. [4] The coated structure according to any one of the above [1] to [3], wherein the surface roughness (Ra) of the surface of the coated structure is 5 μm or less. [5] A coated member comprising a substrate and the coated structure according to any one of the above [1] to [4] provided on a surface of the substrate. [6] A method for producing a coated member having a substrate and a coating structure provided on a surface of the substrate, comprising: A mixing step of mixing a first raw material containing a first fluororesin with a second raw material which is a composite resin material containing a second fluororesin and a conductive filler to obtain a coating mixture; A coating step of coating the coating mixture onto a substrate to form a coating structure; A method for producing a coated member comprising the steps of: [7] The method for producing a coated member according to [6] above, wherein the coating step includes a heating step of heating to a melting point or higher of the first fluororesin and the second fluororesin. [8] The method for producing a coated member according to the above [6] or [7], wherein the coating step is a rotatory lining step. Effect of the Invention
[0007] According to the present disclosure, it is possible to obtain a coating structure having excellent electrical conductivity and excellent appearance. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 shows SEM images of evaluation samples in the examples and comparative examples. [Diagram 2] FIG. 2 is a photograph showing the appearance of the evaluation sample in Comparative Example 2. [Diagram 3] FIG. 3 is a photograph showing the appearance of the evaluation sample in Example 3. [Figure 4]FIG. 4 is a photograph showing the appearance of the pipe after the roto-lining coating in Example 8. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] <Coated structure> The coating structure of the present disclosure contains a fluororesin and a conductive filler, and the surface of the coating structure has a sea-island structure, with the conductive filler being present in the sea portion of the sea-island structure.
[0010] The fluororesin may be a commercially available product that is generally known, and is not particularly limited as long as the coating structure of the present invention can be obtained. Specific examples include at least one selected from polytetrafluoroethylene (PTFE), modified polytetrafluoroethylene (modified PTFE), tetrafluoroethylene / perfluoroalkyl vinyl ether copolymer (PFA), tetrafluoroethylene / hexafluoropropylene copolymer (FEP), ethylene / tetrafluoroethylene copolymer (ETFE), ethylene / chlorotrifluoroethylene copolymer (ECTFE), polychlorotrifluoroethylene (PCTFE), polyvinylidene fluoride (PVDF) and polyvinyl fluoride (PVF), preferably tetrafluoroethylene / perfluoroalkyl vinyl ether copolymer (PFA), tetrafluoroethylene / hexafluoropropylene copolymer (FEP), ethylene / tetrafluoroethylene copolymer (ETFE) or ethylene / chlorotrifluoroethylene copolymer (ECTFE), and particularly preferably tetrafluoroethylene / perfluoroalkyl vinyl ether copolymer (PFA) or ethylene / tetrafluoroethylene copolymer (ETFE). The above fluororesin may be used alone or in combination of two or more kinds, but in a preferred embodiment, the coating structure of the present disclosure contains one kind of fluororesin.
[0011] The melting point of the fluororesin may be preferably 170° C. or higher, more preferably 200° C. or higher.
[0012] The melt flow rate of the fluororesin is preferably 5 to 60 g / 10 min, more preferably 20 to 40 g / 10 min. If it is in this range, it is particularly suitable for use in the rotor lining technique.
[0013] The conductive filler is not particularly limited as long as it is a filler having electrical conductivity, but a preferred example is a carbon nanomaterial.
[0014] The carbon nanomaterial is typically a material having a six-membered carbon ring structure, and specific examples include carbon nanotubes, carbon nanofibers, carbon nanohorns, carbon nanocoils, graphene, fullerene, acetylene black, Ketchon black, carbon black, and carbon fibers, with carbon nanotubes being preferred.
[0015] The average length of the carbon nanomaterial is not particularly limited, but may be, for example, 10 to 600 μm. By making the average length of the carbon nanomaterial 10 μm or more, the electrical conductivity of the coating structure is improved. By making the average length of the carbon nanomaterial 600 μm or less, the dispersibility or supportability of the carbon nanomaterial in the fluororesin is improved. The average length of the carbon nanomaterial can be measured, for example, by observation with a scanning electron microscope described later.
[0016] The content of the carbon nanomaterial is preferably 0.001 to 2.0 mass%, more preferably 0.005 to 1.5 mass%, further preferably 0.01 to 1.0 mass%, and particularly preferably 0.05 to 1.0 mass%, based on the total mass of the coating structure. By setting the content of the carbon nanomaterial in the coating structure to the range of 0.001 to 2.0 mass%, a better conductive path can be formed, and the conductivity is further improved.
[0017] In a preferred embodiment, the carbon nanomaterial is a carbon nanotube.
[0018] The carbon nanotubes are not particularly limited as long as the coating structure of the present disclosure can be obtained, and may be either a single-walled SWCNT (single wall carbon nanotube) or a multiwalled MWCNT (multiwall carbon nanotube) having two or more walls. Commercially available carbon nanotubes can be used, and the carbon nanotubes can be used alone or in combination of two or more kinds.
[0019] The average length of the carbon nanotubes is not particularly limited, but is preferably 40 μm or more, more preferably 50 μm or more, even more preferably 70 to 250 μm, even more preferably 100 to 200 μm, and particularly preferably 150 to 200 μm. By making the average length of the carbon nanotubes 40 μm or more, conductive paths are easily connected, and the conductivity of the coating structure is improved.
[0020] In this specification, the average length of the carbon nanomaterial refers to the average length obtained from an image taken by a SEM (scanning electron microscope). That is, a part of the coating structure is heated to 300°C to 600°C and incinerated to obtain a residue (a sample for SEM photography). An SEM image of the residue is taken. The length of each carbon nanomaterial contained in the SEM image is obtained by image processing. The average value of the lengths obtained by the image processing is calculated, and this average value is called the average length of the carbon nanomaterial.
[0021] The coating structure of the present disclosure has an islands-in-a-sea structure on its surface.
[0022] In this specification, the sea-island structure refers to a structure that is roughly composed of a low region (hereinafter also referred to as "sea part") and a high region (hereinafter also referred to as "island part"). In the sea-island structure, the sea part does not necessarily have to surround the island part, and may be surrounded by the island part.
[0023] The presence or absence of the above-mentioned sea-island structure is judged based on the surface condition of the coating structure observed at a magnification of 75 times using a SEM (scanning electron microscope).
[0024] The conductive filler is present mainly in the sea portion of the above-mentioned sea-island structure.
[0025] In a preferred embodiment, the islands of the sea-island structure are substantially free of conductive filler, where "substantially" means that the conductive filler is present in an amount of 0.01 mass % or less relative to the islands.
[0026] In one embodiment, the sea portion and the island portion of the sea-island structure contain different fluororesin as main components. In this specification, the main component refers to the fluororesin contained in the largest amount among the fluororesin in the sea portion or the island portion, and is typically contained in an amount exceeding 50 mass% of the total fluororesin in the sea portion or the island portion.
[0027] In the above embodiment, the amount of the fluororesin contained as a main component in each of the sea part and the island part of the sea-island structure is preferably 90 mass % or more, more preferably 95 mass % or more, even more preferably 98 mass % or more, and most preferably substantially 100 mass %, based on the total amount of the fluororesin contained in said parts.
[0028] In a preferred embodiment, the sea portion and the island portion of the sea-island structure contain the same fluororesin as a main component.
[0029] In the above sea-island structure, the area ratio of the sea part to the island part (sea part:island part) is not particularly limited, but is preferably 99:1 to 1:99, more preferably 90:10 to 10:90, even more preferably 70:30 to 20:80, and even more preferably 60:40 to 20:80. By setting the area ratio of the sea part to the island part in the above range, the electrical conductivity and the appearance of the coating structure are improved.
[0030] The volume resistivity of the coating structure is not particularly limited as long as it has electrical conductivity, but is preferably 1×10 8 Ω cm or less, preferably 1×10 5 Ω cm or less, especially preferably 1×10 3 The lower limit of the volume resistivity is not particularly limited, but may be, for example, 1×10-1 It can be Ω·cm.
[0031] The volume resistivity is measured according to JIS K6911 using a resistivity meter (for example, "Loresta" manufactured by Mitsubishi Chemical Analytech).
[0032] The surface roughness (Ra: arithmetic surface roughness) of the coating structure may be preferably 5 μm or less, more preferably 3 μm or less, even more preferably 2 μm or less, and even more preferably 1 μm or less. The lower limit of the surface roughness (Ra) is not particularly limited, but may be, for example, 0.05 μm.
[0033] The surface roughness (Rz: maximum height) of the coating structure is preferably 15 μm or less, more preferably 10 μm or less, even more preferably 8 μm or less, even more preferably 5 μm or less, and particularly preferably 4 μm or less. The lower limit of the surface roughness (Rz) is not particularly limited, but may be, for example, 0.5 μm.
[0034] The surface roughness (Ra and Rz) is measured in accordance with ISO 4284:1997 using a surface roughness measuring device (for example, "Surfcorder SE3500" manufactured by Kosaka Laboratory Co., Ltd.).
[0035] The thickness of the coated structure of the present disclosure is not particularly limited, but may be, for example, 20 μm to 10 mm, and preferably 50 μm to 5 mm.
[0036] The coating structure of the present disclosure is provided on the surface of a substrate to constitute a coated member. That is, the present disclosure provides a coated member having a substrate and the coating structure of the present disclosure provided on the surface of the substrate.
[0037] The substrate is not particularly limited as long as it can support the coated structure of the present disclosure, and examples thereof include metals such as iron, aluminum, stainless steel, other metals, or alloys of several of these metals, inorganic compounds such as quartz glass and ceramics, and plastics such as polyimide resins and polyamideimide resins, and may be metals and inorganic compounds. The shape, size, etc. of the substrate are not particularly limited, and may be, for example, a plate, rod, cylinder, cone, comb-like, etc., and the shape and size can be appropriately selected depending on the application.
[0038] The coated member may be produced by forming a coated structure directly on a substrate, or by attaching a separately produced coated structure onto a substrate.
[0039] The present disclosure provides a method for producing the coated structure and coated member of the present disclosure.
[0040] The coated member of the present disclosure has a substrate and a coating structure provided on a surface of the substrate, A mixing step of mixing a first raw material containing a first fluororesin with a second raw material which is a composite resin material containing a second fluororesin and a conductive filler to obtain a coating mixture; A coating step of coating the coating mixture onto a substrate to form a coating structure; Includes.
[0041] In the method of the present disclosure, first, a first raw material containing a first fluororesin and a second raw material which is a composite resin material containing a second fluororesin and a conductive filler are prepared.
[0042] The first and second fluororesins may be the same as the fluororesin contained in the coated structure. The first and second fluororesins may be the same or different, but are preferably the same.
[0043] The first fluororesin is a fluororesin contained as a main component in the island portion of the coated structure.
[0044] The second fluororesin is a fluororesin contained as a main component in the sea portion of the coated structure.
[0045] The first raw material includes a first fluororesin, and preferably consists of the first fluororesin.
[0046] The first raw material containing the first fluororesin is preferably in a particulate form.
[0047] The average particle size of the particles of the first raw material may be preferably 1 to 500 μm, more preferably 5 to 300 μm, and particularly preferably 10 to 250 μm.
[0048] In this specification, the average particle size refers to the median diameter (D) which means the particle size at 50% of the cumulative value in the particle size distribution obtained by a laser diffraction / scattering method. 50 ) and is measured using a laser diffraction / scattering particle size distribution analyzer.
[0049] The second raw material is a composite resin material containing a second fluororesin and a conductive filler, and is preferably composed of the second fluororesin and the conductive filler.
[0050] The conductive filler may be the same as the conductive filler contained in the coated structure, and is preferably carbon nanotubes.
[0051] The content of the conductive filler in the second raw material is preferably 0.001 to 4.0 mass%, more preferably 0.005 to 3.0 mass%, even more preferably 0.010 to 2.0 mass%, still more preferably 0.020 to 1.0 mass%, and particularly preferably 0.020 to 0.10 mass%, based on the entire second raw material. By setting the content of the conductive filler within the above range, the conductivity and appearance of the coating structure are improved.
[0052] The composite resin material used as the second raw material is a fluororesin composition having a mixed layer in which a part or all of the conductive filler is embedded or fixed in a dispersed state in a surface layer of a second fluororesin. An example of the composite resin material used as the second raw material is a fluororesin composition obtained by the method disclosed in JP 2015-030821 A.
[0053] The average particle size of the composite resin material particles is preferably 5 to 500 μm, more preferably 10 to 250 μm, even more preferably 10 to 100 μm, even more preferably 10 to 50 μm, and particularly preferably 15 to 30 μm. By setting the average particle size of the composite resin material to the above upper limit or less, it is easy to increase the dispersibility of the conductive filler in the coating structure, and it is easy to uniformly increase the antistatic property and / or conductivity, which is preferable. By setting the average particle size of the composite resin material to the above lower limit or more, it is preferable from the viewpoint of ease of production of the composite resin material.
[0054] The shape of the second raw material is not particularly limited, and may be, for example, liquid or particulate, and is preferably particulate. In the case of liquid, the composite resin material can be obtained by dispersing it in a solvent that is usually used in making paint, such as water or alcohol.
[0055] Next, the first and second raw materials are mixed to obtain a coating mixture. The mixing method is not particularly limited as long as the two raw materials are mixed uniformly.
[0056] The mixing ratio of the first raw material to the second raw material (first raw material:second raw material) may be preferably 1:5 to 5:1, more preferably 1:2 to 4:1, and further preferably 1:1 to 3:1. By setting the mixing ratio of the first raw material to the second raw material within the above range, the smoothness of the surface of the coated structure is improved, resulting in a coated structure with excellent appearance.
[0057] Next, the coating mixture obtained above is applied to a substrate to form a coating structure.
[0058] The coating method is not particularly limited and can be appropriately selected depending on the application and shape of the coated member. Examples of the coating method include spray coating, electrostatic powder coating, roto-lining, piling, applicator coating, etc., and roto-lining is preferred.
[0059] In a preferred embodiment, the coating step includes a heating step of heating the first fluororesin and the second fluororesin to a melting point or higher, which improves the appearance and mechanical properties of the coated member.
[0060] The temperature in the heating step is equal to or higher than the melting points of the first fluororesin and the second fluororesin, and can be, for example, 150 to 400°C, and preferably 200 to 380°C.
[0061] The heating time in the heating step is not particularly limited, but may be preferably 10 to 150 minutes, more preferably 30 to 120 minutes.
[0062] The coated member of the present disclosure can be produced in the manner described above. After the production of the coated member, the substrate can be removed to obtain a single coated structure.
[0063] The coated structure and the coated member produced as described above have a sea-island structure on their surface, and the conductive filler is present in the sea part of the sea-island structure. In addition, the smoothness of the surface of the coated structure is improved, resulting in a coated structure with excellent appearance. EXAMPLES
[0064] The present invention will be specifically described below with reference to examples, but the scope of the present invention is not limited thereto.
[0065] [First raw material] As the first raw material, ETFE powder, Neoflon (registered trademark) EC-6820 and EC-6510 (manufactured by Daikin Industries, Ltd.), were prepared. M1-1: Neoflon (registered trademark) EC-6820 M1-2: Neoflon (registered trademark) EC-6510
[0066] [Second raw material (CNT composite resin material)] A composite resin material (manufactured by Taiyo Nippon Sanso Corporation; hereinafter referred to as "CNT composite resin material") in which a predetermined amount of carbon nanotubes (hereinafter referred to as "CNT") having an average length of 100 μm is supported on Neoflon (registered trademark) EC-6820 or EC-6510 as a second fluororesin was prepared as follows. M2-1: 0.025% by mass CNT-supported Neoflon (registered trademark) EC-6820 M2-2: 0.05% by mass CNT-supported Neoflon (registered trademark) EC-6820 M2-3: 0.10% by mass CNT-supported Neoflon (registered trademark) EC-6820 M2-4: 0.20% by mass CNT-supported Neoflon (registered trademark) EC-6820 M2-5: 0.10% by mass CNT-supported Neoflon (registered trademark) EC-6510
[0067] [Mixed material for coating] The first raw material and the CNT composite resin material (second raw material) obtained above were stirred and mixed in the ratio shown in the table below to obtain a coating mixture.
[0068] [Table 1]
[0069] [Examples 1 to 6, Comparative Examples 1 and 2: Preparation of Coating Structure Samples for Pile Coating] An iron frame of 50×100 mm size was placed on an iron plate that had been sandblasted and coated with a release agent, and the above-obtained coating mixture materials Mx1 to 9 were filled into the frame so that the film thickness after baking would be 3 mm. The mixture was then baked in an electric furnace at 280° C. for 1 hour, and the iron frame and coating structure were removed from the iron plate to obtain evaluation samples for each coating structure of Examples 1 to 6 (Mx1, 2, 4, 5, 7, and 8 were used, respectively) and Comparative Examples 1 and 2 (Mx3 and 6 were used, respectively). The surface condition, surface roughness, volume resistivity, and appearance of all or part of the obtained evaluation samples were measured or observed by the methods described below. The results are shown in FIGS. 1 to 3 and Table 2.
[0070] [Example 7 Preparation of a coating structure sample related to applicator coating] The coating mixture Mx9 (150 g) obtained above was dispersed and mixed in ethylene glycol (225 g) to prepare a dispersion, and the dispersion was applied to a SUS plate (50 x 100 mm) coated with a release agent to a thickness of 200 μm using a baker applicator. After baking in an electric furnace at 280 ° C for 1 hour, the coating structure was removed from the SUS plate to obtain an evaluation sample related to the coating structure of Example 7. The surface condition, surface roughness, and volume resistivity of the obtained evaluation sample were measured or observed by the methods described below. The results are shown in Figure 1 and Table 2.
[0071] [Surface condition] Using a scanning electron microscope FlexSEM 1000 (Hitachi High-Tech Corporation), the surface condition of the evaluation sample was confirmed at an applied voltage of 10 to 15 KV and a magnification of 75 times.
[0072] [Surface roughness (Ra and Rz)] Surface roughness (arithmetic mean roughness (Ra); maximum height (Rz)) was measured using a Surfcorder SE3500 (manufactured by Kosaka Laboratory Co., Ltd.) in accordance with ISO 4287:1997.
[0073] [Volume resistivity] Conductivity evaluation of Examples 1 to 7 and Comparative Examples 1 and 2 The evaluation samples were cut into 30 × 30 mm test pieces, and the volume resistivity (Ω·cm) was measured using a resistivity meter (Loresta, manufactured by Mitsubishi Chemical Analytech) in accordance with JIS K6911.
[0074] Conductivity evaluation of Example 8 For the coated member produced in Example 8 described below, the surface resistivity (Ω / sq.) of the coated surface after roto-lining was measured using a resistivity meter (HIOKI EE "IR4054", 50 V applied) in accordance with JIS K6911, and the volume resistivity (Ω cm) was calculated according to the following equation. Volume resistivity (ρv) = surface resistivity (ρs) × thickness (t) [exterior] The appearance of the evaluation sample was visually observed.
[0075] [Table 2]
[0076] From the above table, it can be seen from the photograph in FIG. 1 that the surface states of Examples 1 to 7 included in the scope of the present invention all exhibit a sea-island structure, unlike the surface states of Comparative Examples 1 and 2. Furthermore, Examples 1 to 7 are not limited to their coating methods, and all have a surface roughness (Ra) of 5 μm or less and a volume resistivity of 1×10 8 2 and 3, it was confirmed that Example 3, which is within the scope of the present invention, has improved surface smoothness and is excellent in appearance, compared to Comparative Example 2, which is not within the scope of the present invention.
[0077] [Example 8: Preparation of coated member by rotolining] The coating mixture material Mx4 obtained above was applied to the inner surface of a pipe (base material: SS400, JIS 5K 25A flanged pipe 245L) at 280°C by roto-lining (lining coating using rotational molding technology) to obtain a roto-lining coated pipe (coating thickness 2 mm) as a coating component. Figure 4 shows a photograph of the obtained coated pipe. As shown in Figure 4, it can be seen that the coated surface has smoothness and excellent appearance. In addition, the volume resistivity calculated by the above-mentioned method was 4×10 3 It was confirmed that the electrical conductivity was sufficient, being Ω·cm (calculated value). [Industrial Applicability]
[0078] The coated structure of the present disclosure has excellent electrical conductivity and an excellent appearance, and therefore can be suitably used in various fields, such as the inner surface treatment of parts that come into contact with fluids in semiconductor manufacturing equipment and the like.
Claims
1. A coating structure including a fluororesin and a conductive filler, The surface of the coating structure has an island-sea structure, A conductive filler is present in the sea portion of the sea-island structure, The sea portion and the island portion of the sea-island structure contain, as a main component, a fluororesin made of the same fluororesin material. Coating structure.
2. The coating structure according to claim 1 , wherein the conductive filler is a carbon nanotube.
3. The coated structure according to claim 1 or 2, wherein the surface roughness (Ra) of the surface of the coated structure is 5 μm or less.
4. A coated member comprising a substrate and the coating structure according to any one of claims 1 to 3 provided on a surface of the substrate.
5. A method for producing a coated member having a substrate and a coating structure provided on a surface of the substrate, comprising the steps of: A mixing step of mixing a first raw material containing a first fluororesin with a second raw material which is a composite resin material containing a second fluororesin and a conductive filler to obtain a coating mixture; A coating step of coating the coating mixture onto a substrate to form a coating structure; Including, The first fluororesin and the second fluororesin are made of the same fluororesin material. A method for manufacturing a coated member.
6. The method for producing a coated member according to claim 5 , wherein the coating step includes a heating step of heating the first fluororesin and the second fluororesin to a melting point or higher of the first fluororesin and the second fluororesin.
7. The method for producing a coated member according to claim 5 or 6, wherein the coating step is a roto-lining step.
Citation Information
Patent Citations
Fluoroplastic-containing laminate
JP2005335184A
Method of manufacturing fluororesin molded body and fluororesin molded body formed by the manufacturing method
JP2011057868A
Method of manufacturing coating containing carbon nanotube, forming method of coating layer containing carbon nanotube, coating layer containing carbon nanotube, and laminate provided with the coating layer
JP2013231129A
Manufacturing method of composite resin material particles and manufacturing method of a composite resin molding
JP2014034591A
Carbon fiber composite material and method of producing carbon fiber composite material
JP2015078345A