Cement composition for repair material and repair material using same
The cement composition for repair materials addresses the issues of integrity and construction cycle by controlling viscosity, carbonation resistance, and water absorption, resulting in improved durability and crack resistance.
Patent Information
- Application Number
- JP2020165737
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-30
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2040-09-30
AI Technical Summary
Existing repair materials for concrete structures, such as those described in Patent Document 1, lack integrity with the concrete structure and have issues with construction cycles.
A cement composition for repair materials is developed with controlled viscosity, carbonation resistance, and low water absorption, incorporating cement, fibrous materials, and specific additives to enhance integrity and construction cycle performance.
The cement composition improves the integrity and construction cycle of repair materials by ensuring low water absorption, carbonation resistance, and low-temperature curing properties, thereby enhancing durability and crack resistance.
Smart Images

Figure 0007588491000001 
Figure 0007588491000002 
Figure 0007588491000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a cement composition for a repair material, and a repair material using the same. [Background technology]
[0002] Various repair materials for use in repairing concrete structures have been developed to date. One such technique is described in Patent Document 1. Patent Document 1 describes a repair material that contains alumina cement and a shrinkage reducing agent that is a polyoxyalkylene compound. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent Publication No. 2006-044960 Summary of the Invention [Problem to be solved by the invention]
[0004] However, as a result of investigations by the present inventors, it has become clear that the repair material described in the above Patent Document 1 has room for improvement in terms of its integration with the concrete framework and its construction cycle. [Means for solving the problem]
[0005] As a result of further investigation, the inventors have found that by using the three properties of low water absorption, carbonation resistance, and low-temperature hardening property as indicators and appropriately controlling these indicators, it is possible to realize a cement composition for repair material that can improve the integration of the repair material with the concrete structure and the construction cycle, and have thus completed the present invention.
[0006] According to the present invention, A cement composition for repair material comprising cement and a fibrous material, The viscosity measured by procedure A below is 200 mPa s or more and 10,000 mPa s or less, The degree of accelerated carbonation measured by the procedure B below is 6.0 mm or less, and The water absorption rate measured by the procedure C below is 8.0% or less. A repair material cement composition is provided. (Step A) The cement composition for repair material is sieved to remove the fibrous material, and the sieved fraction is obtained. Water is added to the sieved fraction so that the water content is 36% by mass relative to 100% by mass of cement, and the mixture is kneaded to prepare a test sample A. The viscosity of the obtained test sample A is measured using a B-type viscometer at 25°C and a rotation speed of 100 rpm. (Step B) A test sample B is prepared by mixing the cement composition for repair material with 36 mass % water relative to 100 mass % cement. Using the obtained test sample B, a specimen measuring 4 cm x 4 cm x 16 cm is prepared. The obtained specimens were cured in water for 2 days, and then cured at 20°C and 60% RH for 7 to 28 days. Then, they were cured at 30°C, 60% RH, and CO 2 The specimen is placed in a 5% concentration accelerated carbonation device, and after 28 days, the specimen is split, and a 1% phenolphthalein ethyl alcohol solution is sprayed onto the split surface in accordance with JIS A 1152 "Method of measuring carbonation depth of concrete," and the carbonation depth (mm) to the point where the concrete turns reddish purple is measured with a caliper. This carbonation depth is the degree of accelerated carbonation (mm). (Step C) Prepare a 4 cm x 4 cm x 16 cm test specimen in the same manner as in Measurement Procedure B for Accelerated Carbonation Degree above. The obtained specimens are cured underwater after 2 days, and then cured at 20°C and 60% RH for 7 to 28 days. After drying at 80°C for 2 days, the mass W1 (g) of the specimen is measured. After that, the specimen is immersed in water at 20°C for 2 days, and the mass W2 (g) of the specimen is measured. Based on the obtained formula (W2-W1) / W1 x 100, the water absorption rate (%) is calculated from the change in mass before and after immersion in water.
[0007] Further, according to the present invention, There is provided a repair material comprising the above-mentioned cement composition for repair material and water. Effect of the Invention
[0008] According to the present invention, there are provided a cement composition for repair material which can realize a repair material having excellent integrity with the concrete framework and a short construction cycle, and a repair material using the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The cement composition for repair material of this embodiment will be outlined.
[0010] The cement composition for repair material contains cement and a fibrous material, and is configured to satisfy the following requirements: a viscosity, measured by procedure A below, of 200 mPa s or more and 10,000 mPa s or less; an accelerated carbonation degree, measured by procedure B below, of 6.0 mm or less; and a water absorption, measured by procedure C below, of 8.0% or less.
[0011] According to the findings of the present inventors, it has been found that by using the three properties of a cement composition for use as a repair material, namely, low water absorption, carbonation resistance, and low-temperature hardening property, as indicators and appropriately controlling these indicators, it is possible to realize a repair material that can inhibit early deterioration and improve the construction cycle by using the cement composition for use as a repair material. Although the detailed mechanism is unclear, it is thought that this is because the low water absorption, carbonation resistance, and low-temperature hardening properties provide anti-rust effects for reinforcing bars, and also provide good crack resistance.
[0012] According to this embodiment, it is possible to realize a cement composition for repair material that can realize a repair material that is excellent in integration with the concrete framework and in the construction cycle.
[0013] The repair material contains the above-mentioned cement composition for repair material and water, and may be any of cement paste, mortar, and concrete. This repair material is obtained by mixing the above-mentioned cement composition for repair material with water.
[0014] The repair material is used to repair concrete structures. The repair material makes it possible to carry out various types of repairs, such as cross-sectional repair of concrete, roads, sidewalks, asphalt pavement, and concrete pavement.
[0015] Repairs using repair materials can be carried out using a variety of methods, including spraying and troweling.
[0016] Hereinafter, each component of the cement composition for repair material of the present embodiment will be described in detail.
[0017] The repair material cement composition contains cement. As the cement, any of the commercially available cements may be used, including ordinary Portland cement, high-early-strength Portland cement, moderate-heat Portland cement, white Portland cement, ultra-high-early-strength Portland cement, low-heat (belite) cement, and sulfate-resistant Portland cement, as well as mixed cements made by mixing silica powder, blast furnace slag powder, and fly ash, and which already contain an appropriate amount of gypsum. These may be used alone or in combination of two or more types.
[0018] The repair cement composition includes a fibrous material. The fiber material may be either bundled or non-bundled, and either may be used. Examples of fibrous materials include alkali-resistant glass fibers, carbon fibers, aramid fibers, vinylon fibers, polypropylene fibers, polyethylene fibers, acrylic fibers, etc. These may be used alone or in combination of two or more.
[0019] The fiber length of the fibrous material is, for example, 3 mm to 30 mm, preferably 4 mm to 20 mm. By making it equal to or greater than the lower limit, the effect of preventing cracks from occurring can be obtained. On the other hand, by making it equal to or less than the upper limit, kneadability and workability can be improved. In this specification, the symbol "to" indicates that the upper and lower limits are included, unless otherwise specified.
[0020] The upper limit of the moisture content in the fibrous material may be, for example, 1.0% or less, 0.8% or less, and preferably 0.5% or less, calculated on a weight basis, which can enhance the storage stability of the cement composition for repair material and improve the workability in on-site construction. The lower limit of the moisture content in the fiber material is not particularly limited, but may be 0% or more.
[0021] The content of the fibrous material is, for example, preferably 0.05% by weight to 5% by weight, more preferably 0.1% by weight to 3% by weight, based on 100% by weight of cement. By making the content equal to or greater than the lower limit, the effect of preventing cracks from occurring in the hardened body of the repair material can be obtained. On the other hand, by making the content equal to or less than the upper limit, the kneadability and workability of the repair material can be improved.
[0022] The cement composition for repair material may contain one or more selected from the group consisting of an accelerator, an aggregate, a plasticizer, a water reducing agent, and an antifoaming agent.
[0023] The cement composition for repair material may include a (setting) accelerator. The accelerator may include a carboxylate.
[0024] In the carboxylate, for example, formic acid, lactic acid, acetic acid, etc. are used as the carboxylic acid, and for example, calcium, potassium, etc. are used as the salt. These may be used alone or in combination of two or more. Among them, calcium carboxylate may be used, and carboxylates such as potassium formate and calcium formate may be used.
[0025] The carboxylate may be in powder form. The upper limit of the water content in the carboxylate may be, for example, 1.0% or less, 0.8% or less, preferably 0.5% or less, calculated by weight. This enhances the storage stability of the cement composition for repair material and improves the on-site construction workability. The lower limit of the water content in the carboxylate is not particularly limited, and may be 0%, but may be 0.01% or more.
[0026] The moisture content of an object is calculated by drying it by placing it in a dryer at 110°C for three days, using the formula: change in weight of the object before and after drying / weight of the object before drying × 100%.
[0027] The content of the carboxylate is, for example, 0.5 to 10% by weight, preferably 1 to 5% by weight, calculated as solid content, relative to 100% by weight of cement. By making the content equal to or more than the lower limit, the setting property of the repair material can be improved. By making the content equal to or less than the upper limit, the usable time of the repair material can be secured.
[0028] The repair material cement composition may contain aggregate. As the aggregate, natural aggregates such as river sand, sea sand, silica stone and limestone, recycled fine aggregates, and inactive inorganic powders such as silica stone fine powder, limestone fine powder and recycled fine powder can be used. This is expected to improve the fluidity of the repair material and the durability of the hardened body of the repair material.
[0029] The aggregate preferably includes aggregate having a grain size of, for example, 5 mm or less. Particle size is an index indicated by the mass fraction passing through a sieve having a given mesh size. A mixture of aggregates having two or more different grain sizes may be used, with 50% to 100% by weight of aggregates having grain sizes of 5 mm, 2.5 mm, or 1.2 mm, 25% to 65% by weight of aggregates having grain sizes of 0.6 mm or less, 10% to 35% by weight of aggregates having grain sizes of 0.3 mm or less, and 2% to 15% by weight of aggregates having grain sizes of 0.15 mm or less. For example, aggregates having grain sizes of 1.2 mm or less to over 0.6 mm and aggregates having grain sizes of 0.6 mm or less may be used. Commercially available grain size-controlled silica sand may also be combined. By keeping the maximum aggregate particle size at 5mm or less, fluidity and workability can be improved.
[0030] The content of the aggregate is, for example, preferably 80% by weight to 300% by weight, more preferably 90% by weight to 200% by weight, based on 100% by weight of cement. By making the content equal to or greater than the lower limit, the occurrence of cracks in the hardened body of the repair material can be suppressed. On the other hand, by making the content equal to or less than the upper limit, sufficient fluidity of the repair material can be ensured.
[0031] The repair material cement composition may contain a plasticizer. By adding a plasticizer, the mixed mortar can be made more plastic. For example, when repairing a pothole on a slope, the mortar can be prevented from flowing out of the slope, making it possible to finish the slope smoothly.
[0032] The plasticizer may be in powder form, and examples thereof include clay minerals such as kaolinite, bentonite, sepiolite containing magnesium silicate hydrate, zeolite, etc. These may be used alone or in combination of two or more kinds.
[0033] The content of the plasticizer is, for example, 0.1% by weight to 10% by weight, preferably 0.2% by weight to 5% by weight, based on 100% by weight of cement. By making the content equal to or greater than the lower limit, the plasticity of the mortar can be increased. On the other hand, by making the content equal to or less than the upper limit, the viscosity of the mortar during mixing can be appropriately adjusted.
[0034] The repair material cement composition may contain a defoamer. The addition of an antifoaming agent reduces the amount of air entrapped when the powdered cement composition for repair material is mixed, and improves the compressive and bending strength of the hardened repair material.
[0035] The defoaming agent may be in a powder form, and for example, a lower alcohol-based defoaming agent, a higher alcohol-based defoaming agent, an oil-based defoaming agent, a surfactant-based defoaming agent, a silicone-based defoaming agent, etc. can be used. Specifically, examples of the powdered defoaming agent include "ADEKANATE B-115F" manufactured by Asahi Denka Kogyo Co., Ltd. and "SN DEFOAMER 14HP" manufactured by San Nopco Co., Ltd. These may be used alone or in combination of two or more kinds.
[0036] The content of the defoaming agent is, for example, 0.01% by weight to 0.50% by weight, preferably 0.02% by weight to 0.30% by weight, based on 100% by weight of cement. By making the content equal to or greater than the lower limit, a defoaming effect can be obtained. On the other hand, by making the content equal to or less than the upper limit, material separation caused by foam generation can be suppressed.
[0037] The repair material cement composition may contain a water reducing agent. By adding a water reducing agent, the unit water content in the mortar can be reduced while maintaining the fluidity of the mortar.
[0038] The water reducing agent can be used in either powder or liquid form.
[0039] Examples of the water reducing agent include polyalkylarylsulfonate-based high performance water reducing agents, aromatic aminosulfonate-based high performance water reducing agents, melamine formalin resin sulfonate-based high performance water reducing agents, and polycarboxylate-based high performance water reducing agents. Specific examples of the water reducing agent include polyalkylarylsulfonate-based high performance water reducing agents, such as "Cellflow 110P" manufactured by Daiichi Kogyo Seiyaku Co., Ltd. and "IPC" manufactured by Idemitsu Petrochemical Co., Ltd., and aromatic aminosulfonate-based high performance water reducing agents, such as "Mighty 100" manufactured by Kao Corporation and "Sanyo Revellon P" manufactured by Sanyo Chemical Industries Co., Ltd., and melamine formalin resin sulfonate-based high performance water reducing agents, such as "Sikament FF86 / 100" manufactured by Sika Corporation, and polycarboxylate-based high performance water reducing agents, such as "Melflux AP101F" manufactured by BASF Pozzolith Co., Ltd. and "Mighty 21PZ" manufactured by Kao Corporation. These may be used alone or in combination of two or more.
[0040] The content of the water reducing agent is, for example, preferably 0.01% by weight to 5% by weight, more preferably 0.05% by weight to 2% by weight, calculated as solid matter, relative to 100% by weight of cement. By making the content equal to or greater than the lower limit, good fluidity can be obtained for the repair material. By making the content equal to or greater than the upper limit, setting delay of the repair material can be suppressed.
[0041] The cement composition for repair material may contain, as necessary, within the scope of the purpose, a hardening agent, an expansive agent, a shrinkage reducing agent, a pozzolanic substance such as fly ash or silica fume, an anti-rust agent, an underwater non-separating admixture such as methylcellulose, a thickener, a water-retaining agent, a waterproofing agent, a foaming agent, an antifreeze agent, a subsidence inhibitor, an antibacterial agent, a coloring agent, etc. These may be used alone or in combination of two or more kinds.
[0042] The cement composition for repair material may be configured so as not to contain at least one of a hardening agent and a shrinkage reducing agent, preferably both. The hardening agent may be calcium aluminate. The shrinkage reducing agent may be polyoxyalkylene monoalkyl ether. This configuration can improve the carbonation resistance.
[0043] The cement composition for repairing material may be composed of a powder composition. That is, each component contained in the cement composition for repairing material may be in a powder form, not in a liquid form. This can improve the on-site workability of the cement composition for repairing material.
[0044] The cement composition for repair material of the present embodiment has the following properties, which are indicated by the following viscosity, accelerated carbonation degree, and water absorption rate. By setting the viscosity, accelerated carbonation degree, and water absorption rate within the following numerical ranges, it is possible to improve the integration of the repair material using the cement composition for repair material with the concrete framework and the application cycle.
[0045] The lower limit of the viscosity is 200 mPa·s or more, preferably 300 mPa·s or more, and more preferably 350 mPa·s or more, while the upper limit of the viscosity is 10,000 mPa·s or less, preferably 9,000 mPa·s or less, and more preferably 8,000 mPa·s or less.
[0046] The upper limit of the accelerated carbonation degree is 6.0 mm or less, preferably 5.0 mm or less, and more preferably 4.0 mm or less. The lower limit of the accelerated carbonation degree is not particularly limited, but may be 0 mm or more, or 0.1 mm or more.
[0047] The water absorption is 8.0% or less, preferably 7.0% or less, and more preferably 6.0% or less. The lower limit of C is not particularly limited, but may be 0% or more, or 0.1% or more.
[0048] (Step A) The cement composition for repair material is sieved to remove fibrous material, and the sieved fraction is obtained. Water is added to the sieved fraction so that the water content is 36% by mass relative to 100% by mass of cement, and the mixture is kneaded to prepare a test sample A. The viscosity of the obtained test sample A is measured using a B-type viscometer at 25°C and a rotation speed of 100 rpm.
[0049] (Step B) Water is added to the cement composition for repair material so that the water content is 36 mass% relative to 100 mass% of cement, and the mixture is kneaded to prepare a test sample B. Using the obtained repair material, a test specimen measuring 4cm x 4cm x 16cm is prepared. The obtained specimens were cured in water for 2 days, and then cured at 20°C and 60% RH for 7 to 28 days. Then, they were cured at 30°C, 60% RH, and CO 2 The specimen is placed in a 5% concentration accelerated carbonation device, and after 28 days, the specimen is split, and a 1% phenolphthalein ethyl alcohol solution is sprayed onto the split surface in accordance with JIS A 1152 "Method of measuring carbonation depth of concrete," and the carbonation depth (mm) to the point where the concrete turns reddish purple is measured with a caliper. This carbonation depth is the degree of accelerated carbonation (mm).
[0050] (Step C) Prepare a 4 cm x 4 cm x 16 cm test specimen in the same manner as in Measurement Procedure B for Accelerated Carbonation Degree above. The obtained specimens are cured underwater after 2 days, and then cured at 20°C and 60% RH for 7 to 28 days. After drying at 80°C for 2 days, the mass W1 (g) of the specimen is measured. After that, the specimen is immersed in water at 20°C for 2 days, and the mass W2 (g) of the specimen is measured. Based on the obtained formula (W2-W1) / W1 x 100, the water absorption rate (%) is calculated from the change in mass before and after immersion in water.
[0051] The viscosity value at 5 revolutions measured by procedure D below is η5, the viscosity value at 50 revolutions is η50, the viscosity value at 100 revolutions is η100, η5 / η50=TI1, and η50 / η100=TI2. TI1 is, for example, 0.1 or more and 10 or less, preferably 2.0 or more and 9.0 or less, and more preferably 4.0 or more and 8.0 or less. TI2 is, for example, 0.1 or more and 10 or less, preferably 0.2 or more and 5.0 or less, and more preferably 0.5 or more and 3.0 or less. By setting at least one of TI1 and TI2 within the above numerical range, a repair material that is excellent in integration with the concrete structure and in the construction cycle can be realized.
[0052] (Step D) The cement composition for repair material is sieved to remove fibrous material, and the sieved fraction is obtained. Water is added to the sieved fraction so that the water is 60% by mass relative to 100% by mass of cement, and the mixture is mixed for 1 minute, allowed to stand for 10 minutes, and then mixed again for 1 minute to prepare test sample D. The viscosity of the obtained test sample D is measured using a B-type viscometer at 25°C and rotation speeds of 5 rpm, 50 rpm, and 100 rpm, and the viscosity value 1 minute after the start of measurement is obtained.
[0053] In this embodiment, it is possible to control the viscosity, accelerated carbonation degree, and water absorption rate by appropriately selecting the type and amount of each component contained in the cement composition for repair material, the preparation method of the cement composition for repair material, etc. Among these, for example, the use of a carboxylate and its amount, not using a hardener or shrinkage reducing agent, etc. are listed as elements for setting the viscosity, accelerated carbonation degree, and water absorption rate in the desired numerical range.
[0054] The repair material of the present embodiment can be obtained by mixing the above-mentioned cement composition for repair material with water.
[0055] The amount of water used is appropriately selected depending on whether it is a cement paste, mortar, or concrete, but in the case of a mortar repair material, for example, 5 to 50 parts is preferable, and 10 to 30 parts is more preferable, per 100 parts of the cement composition for repair material. By setting it to the above lower limit value or more, sufficient fluidity as a mortar can be obtained. By setting it to the above upper limit value or less, sufficient durability can be obtained in the hardened mortar.
[0056] The repair material may contain a polymer for cement admixture. The polymer for cement admixture can be mixed with water and used as a polymer dispersion. By adding the polymer for cement admixture, it is possible to improve the material separation resistance, the adhesion to the concrete structure, and the low water absorption. In addition, by using a polymer dispersion and not using powdered resin that has been dried, drying shrinkage can be reduced. Also, the fluctuation of air entrainment when mixing powdered resin can be suppressed, resulting in a repair material with excellent manufacturing stability.
[0057] Polymers for mixing with cement are systems in which fine particles of polymer are dispersed in water (dispersions), and examples of such systems include rubber latex and resin emulsions.
[0058] Examples of the rubber component in rubber latex include synthetic rubbers such as acrylonitrile-butadiene rubber, styrene-butadiene rubber, and chloroprene rubber, natural rubber, rubber asphalt, etc. In addition to the rubber component and water, rubber latex may contain stabilizers and defoamers as necessary. Among these, water-dispersible styrene-butadiene copolymer latexes mainly composed of styrene, styrene-acrylic emulsions, methyl methacrylate-butadiene latexes copolymerized with styrene, ethylene-acrylic emulsions, and the like may be used.
[0059] Examples of the resin component in the resin emulsion include ethylene-vinyl acetate copolymers, polyacrylic esters, vinyl acetate-vinyl versatate copolymers, styrene-acrylic ester copolymers, acrylic ester copolymers such as acrylonitrile-acrylic ester, epoxy resins, unsaturated polyester resins, etc. In addition to the resin component and water, the resin emulsion may contain a stabilizer and / or an antifoaming agent, if necessary.
[0060] In the polymer dispersion, the particle size of the polymer fine particles may be, for example, 100 to 300 nm, or 60 to 100 nm, which provides appropriate dispersibility.
[0061] The repair material may be prepared by adding water and a polymer for cement admixture to a premixed powder composition in which all the components constituting the above-mentioned cement composition for repair material are mixed in advance, and the premixed powder composition is used by simply adding water and mixing on-site. This can improve the workability on-site. Alternatively, the method for producing the repair material may be a method in which the components constituting the above-mentioned cement composition for repair material, i.e., cement, carboxylate, aggregate, fibrous material, etc., are mixed at the site of use, and water and a polymer for mixing with cement are added to the obtained powdery mixture to prepare the repair material.
[0062] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of the present invention are included in the present invention. Below, examples of reference forms are given. 1. A cement composition for repair comprising cement and a fibrous material, The viscosity measured by procedure A below is 200 mPa s or more and 10,000 mPa s or less, The degree of accelerated carbonation measured by the procedure B below is 6.0 mm or less, and The water absorption rate measured by the procedure C below is 8.0% or less. Cement composition for repair material. (Step A) The cement composition for repair material is sieved to remove the fibrous material, and the sieved fraction is obtained. Water is added to the sieved fraction so that the water content is 36% by mass relative to 100% by mass of cement, and the mixture is kneaded to prepare a test sample A. The viscosity of the obtained test sample A is measured using a B-type viscometer at 25°C and a rotation speed of 100 rpm. (Step B) A test sample B is prepared by mixing the cement composition for repair material with 36 mass % water relative to 100 mass % cement. Using the obtained test sample B, a specimen measuring 4 cm x 4 cm x 16 cm is prepared. The obtained specimens were cured in water for 2 days, and then cured at 20°C and 60% RH for 7 to 28 days. Then, they were cured at 30°C, 60% RH, and CO 2 The specimen is placed in a 5% concentration accelerated carbonation device, and after 28 days, the specimen is split, and a 1% phenolphthalein ethyl alcohol solution is sprayed onto the split surface in accordance with JIS A 1152 "Method of measuring carbonation depth of concrete," and the carbonation depth (mm) to the point where the concrete turns reddish purple is measured with a caliper. This carbonation depth is the degree of accelerated carbonation (mm). (Step C) Prepare a 4 cm x 4 cm x 16 cm test specimen in the same manner as in Measurement Procedure B for Accelerated Carbonation Degree above. The obtained specimens are cured underwater after 2 days, and then cured at 20°C and 60% RH for 7 to 28 days. After drying at 80°C for 2 days, the mass W1 (g) of the specimen is measured. After that, the specimen is immersed in water at 20°C for 2 days, and the mass W2 (g) of the specimen is measured. Based on the obtained formula (W2-W1) / W1 x 100, the water absorption rate (%) is calculated from the change in mass before and after immersion in water. 2. The cement composition for repair material according to 1., A cement composition for repair material, wherein the moisture content in the fibrous material is 1.0% or less. 3. A cement composition for repair material according to 1. or 2., When the viscosity value at 5 rpm is η5, the viscosity value at 50 rpm is η50, the viscosity value at 100 rpm is η100, η5 / η50=TI1, and η50 / η100=TI2, measured using the procedure D below, A cement composition for repair material, having TI1 and / or TI2 of 0.1 or more and 10 or less. (Step D) The cement composition for repair material is sieved to remove the fibrous material, and the sieved fraction is obtained. Water is added to the sieved fraction so that the water is 60% by mass relative to 100% by mass of cement, and the mixture is mixed for 1 minute, allowed to stand for 10 minutes, and then mixed again for 1 minute to prepare test sample D. The viscosity of the obtained test sample D is measured using a B-type viscometer at 25°C and rotation speeds of 5 rpm, 50 rpm, and 100 rpm, and the viscosity value 1 minute after the start of measurement is obtained. 4. A cement composition for repair material according to any one of 1. to 3., A cement composition for repair material comprising one or more selected from the group consisting of an accelerator, an aggregate, a plasticizer, a water reducing agent, and an antifoaming agent. 5. The cement composition for repair material according to 4., The cement composition for repair material, wherein the accelerator comprises a carboxylate. 6. The cement composition for repair material according to 5., A cement composition for repair material, wherein the water content in the carboxylate is 1.0% or less by weight. 7. A cement composition for repair material according to 5. or 6., The cement composition for repair material, wherein the carboxylate comprises calcium formate. 8. A cement composition for repair material according to any one of 1. to 7., A cement composition for repair material, which does not contain at least one of a hardening accelerator and a shrinkage reducing agent. 9. A cement composition for repair material according to any one of 1. to 8., A powdered cement composition for repair material. 10. A repair material comprising the cement composition for repair material according to any one of 1. to 9. and water. 11. The repair material according to claim 10, A repair material comprising a cement-mixing polymer. 12. The repair material according to 11., The repair material, wherein the cement-mixable polymer comprises a water-dispersible styrene-butadiene copolymer latex. EXAMPLES
[0063] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the descriptions of these examples.
[0064] <Preparation of cement composition for repair material> The raw materials shown in Table 1 below were mixed according to the mixing ratio in Table 1 to obtain a cement composition for repair material (powder product).
[0065] The information on the raw material ingredients in Table 1 is shown below. Cement: High early strength Portland cement Fine aggregate 1: limestone sand with a grain size of 1.2mm to 0.6mm Fine aggregate 2: limestone sand with a grain size of 0.6 mm or less Accelerator: Calcium formate (dry product, moisture content: 0.4% or less, moisture content measurement method: leave in a dryer at 110°C for 3 days, measure the moisture content in calcium formate based on the formula: weight change of calcium formate before and after drying / weight of calcium formate before drying x 100%) Plasticizer: Magnesium silicate hydrate (sepiolite) Defoamer: Powdered defoamer (non-ionic surfactant) Water reducing agent: Melamine formalin resin sulfonate-based high performance water reducing agent (main component is modified methylol melamine condensate) Fiber: Vinylon fiber (diameter 7 μm, fiber length 6 mm) Shrinkage reducer: Polyoxyalkylene monoalkyl ether
[0066] [Table 1]
[0067] (Preparation of repair materials) A polymer dispersion (liquid product) was prepared by dispersing water-dispersible styrene-butadiene copolymer latex (rubber solids: 45 wt%, viscosity: 25 mPa·s, pH: 8.5) in water. 100 parts by weight of the cement composition for repair material (powder product) obtained above was mixed with 8.3 parts by weight of polymer dispersion (liquid product) and 12.5 parts by weight of water, and the mixture was kneaded for 90 seconds to obtain a repair material (100% by weight of cement with 36% by weight of water).
[0068] The properties of the resulting cement composition for repair material and the repair material were measured and evaluated based on the following evaluation items.
[0069] (viscosity) The resulting cement composition for repair material (powder product) was sieved through a sieve with an opening of 90 μm to remove fibrous material and sand (fine aggregate). Water was added to the resulting powder that passed through the sieve so that the water content was 36 mass% relative to 100 mass% of cement, and the mixture was kneaded for 90 seconds to prepare test sample A. The viscosity (mPa·s) of the obtained test sample A was measured using a Brookfield viscometer at 25°C and a rotation speed of 100 rpm. Cases between 200 mPa·s and 10,000 mPa·s were rated as ○, and cases less than 200 mPa·s or more than 10,000 mPa·s were rated as ×.
[0070] (Accelerated Neutralization Degree) Water was added to the obtained cement composition for repair material so that the water content was 36 mass % relative to 100 mass % of cement, and the mixture was kneaded for 90 seconds to obtain a test sample B. Using the obtained test sample B, a test specimen measuring 4 cm x 4 cm x 16 cm was prepared. The obtained specimens were cured in water for 2 days, and then cured at 20°C and 60% RH for 7 to 28 days. Then, they were cured at 30°C, 60% RH, and CO2 The specimen was placed in a 5% concentration accelerated carbonation device, and after 28 days, the specimen was split open, and a 1% phenolphthalein ethyl alcohol solution was sprayed onto the split surface in accordance with JIS A 1152 "Method of measuring carbonation depth of concrete," and the carbonation depth (mm) to the point where the concrete turned reddish purple was measured with a caliper. This carbonation depth was defined as the degree of accelerated carbonation (mm). The case where the thickness was 6.0 mm or less was rated as ◯, and the case where the thickness exceeded 6.0 mm was rated as ×.
[0071] (Water absorption rate) Test specimens measuring 4 cm x 4 cm x 16 cm were prepared in the same manner as in the measurement of the accelerated carbonation degree described above. The obtained specimens were cured in water after 2 days, and then cured at 20°C and 60% RH for 7 to 28 days. After drying at 80°C for 2 days, the mass W1 (g) of the specimen was measured. Then, after immersion in water at 20°C for 2 days, the mass W2 (g) of the specimen was measured. The water absorption rate (%) was calculated from the change in mass before and after immersion in water based on the formula (W2-W1) / W1×100. The case of 8.0% or less was evaluated as ◯, and the case of more than 8.0% was evaluated as ×.
[0072] (Construction cycle) As an index of the construction cycle, a 30cm x 30cm x 6cm concrete slab conforming to JISA5371 was coated with 3cm of the cement composition for repair materials mixed with water to form a first layer, and then a 3cm layer was coated on the surface of the first layer. If the time it took for the first layer to not drip off was within 4 hours, it was evaluated as ◯, and if the time it took for the first layer to not drip off was more than 4 hours, it was evaluated as ×.
[0073] (Integrity with the concrete structure: durability) A 3cm thick layer of the cement composition for repair mixed with water was applied to a 30cm x 30cm x 6cm concrete plate conforming to JISA5371, and the bond strength was measured by the Construction Research Institute method after 7 days, and the bond strength with the concrete structure was determined. The bond strength was 1.0N / mm 2 Above 0, 1.0N / mm 2 Less than this was rated as x.
[0074] [Table 2]
[0075] (TI value: Thixotropy index) The cement composition for repair material of each Example was sieved through a sieve with a mesh size of 90 μm to remove fibrous material and sand (fine aggregate), and the sieved portion was obtained. Water was added to the obtained sieved powder so that the water was 60% by mass relative to 100% by mass of cement, and the mixture was mixed for 1 minute, allowed to stand for 10 minutes, and then mixed again for 1 minute to prepare a test sample D. The viscosity of the obtained test sample D was measured using a B-type viscometer at 25°C and rotation speeds of 5 rpm, 50 rpm, and 100 rpm, and the viscosity value 1 minute after the start of measurement was obtained. Based on the viscosity value η5 at 5 rpm, the viscosity value η50 at 50 rpm, and the viscosity value η100 at 100 rpm, η5 / η50=TI1 and η50 / η100=TI2 were calculated.
[0076] [Table 3]
[0077] The cement compositions for repair materials of Examples 1 to 3 can realize repair materials that are superior in integration with the concrete framework and in construction cycle compared to Comparative Example 1.
Claims
1. A cement composition for repair material comprising cement and a fibrous material, Contains a promoter, the accelerator comprises a carboxylate, the carboxylate comprises calcium formate; The moisture content of the fiber material is 1.0% or less, Does not contain any hardening materials. The viscosity measured by the following procedure A is 200 mPa·s or more and 10,000 mPa·s or less, The degree of accelerated carbonation measured by the following procedure B is 6.0 mm or less; and The water absorption rate measured by the following procedure C is 8.0% or less. Cement composition for repair material. (Procedure A) The cement composition for repair material is sieved to remove the fibrous material, and the sieved fraction is obtained. Water is added to the sieved fraction so that the water content is 36% by mass relative to 100% by mass of cement, and the mixture is kneaded to prepare a test sample A. The viscosity of the obtained test sample A is measured using a B-type viscometer at 25° C. and a rotation speed of 100 rpm. (Procedure B) A test sample B is prepared by mixing the cement composition for repair material with 36% water by mass relative to 100% cement by mass. Using the obtained test sample B, a test specimen of 4 cm x 4 cm x 16 cm is prepared. The obtained test specimens are cured in water after 2 days, and then cured at 20°C and 60% RH for 7 to 28 days. Then, they are cured at 30°C, 60% RH, CO 2 The specimen is placed in a 5% concentration accelerated carbonation device, and after 28 days, the specimen is split, and a 1% ethyl alcohol solution of phenolphthalein is sprayed onto the split surface in accordance with JIS A 1152 "Method of measuring carbonation depth of concrete," and the carbonation depth (mm) to the point where the concrete turns reddish purple is measured with a caliper. This carbonation depth is the degree of accelerated carbonation (mm). (Step C) A test specimen of 4 cm x 4 cm x 16 cm is prepared in the same manner as in the measurement procedure B for the (degree of accelerated carbonation) above. The obtained specimens are cured in water after 2 days, and then cured at 20°C and 60% RH for 7 to 28 days. After drying at 80°C for 2 days, the mass W1 (g) of the specimen is measured. After that, the specimen is immersed in water at 20°C for 2 days, and the mass W2 (g) of the specimen is measured. Based on the obtained formula (W2-W1) / W1 x 100, the water absorption rate (%) is calculated from the change in mass before and after immersion in water.
2. The cement composition for repair material according to claim 1, When the viscosity value at 5 rpm is η5, the viscosity value at 50 rpm is η50, the viscosity value at 100 rpm is η100, η5 / η50=TI1, and η50 / η100=TI2, measured by the following procedure D, A cement composition for repair material, having TI1 and / or TI2 of 0.1 or more and 10 or less. (Procedure D) The cement composition for repair material is sieved to remove the fibrous material, and the sieved fraction is obtained. Water is added to the sieved fraction so that the water is 60% by mass relative to 100% by mass of cement, and the mixture is mixed for 1 minute, allowed to stand for 10 minutes, and then mixed again for 1 minute to prepare a test sample D. The viscosity of the obtained test sample D is measured using a B-type viscometer at 25° C. and rotation speeds of 5 rpm, 50 rpm, and 100 rpm, and the viscosity value 1 minute after the start of the measurement is obtained.
3. The cement composition for repair material according to claim 1 or 2, A cement composition for repair material comprising one or more selected from the group consisting of aggregate, a plasticizer, a water reducing agent, and a defoaming agent.
4. The cement composition for repair material according to claims 1 to 3, A cement composition for repair material, wherein the water content in the carboxylate is 1.0% or less by weight.
5. The cement composition for repair material according to any one of claims 1 to 4, A powdered cement composition for repair material.
6. A repair material comprising the cement composition for repair material according to any one of claims 1 to 5 and water.
7. The repair material according to claim 6, A repair material comprising a cement-mixing polymer.
8. The repair material according to claim 7, The repair material, wherein the cement-compatible polymer comprises a water-dispersible styrene-butadiene copolymer latex.
Citation Information
Patent Citations
Compounding agent for cement mortar and / or concrete
JP1991257047A
Manufacture of super light weight concrete molding
JP1999048234A
Spraying material and spraying method
JP2002137953A
Hydraulic composition with improved wet adhesion
JP2006044960A
Cement composition for repairing and repairing method
JP2006117451A