Methods and wet chemical compositions for forming diffusion barriers - Patents.com
The wet deposition of manganese oxide barrier layers on dielectric and semiconductor substrates enhances adhesion and conductivity, overcoming the inefficiencies of dry vacuum methods by reducing processing time and equipment needs.
Patent Information
- Application Number
- JP2023547619
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-02-08
- Filing Date
- 2022-02-07
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-02-07
AI Technical Summary
Conventional dry vacuum methods for depositing diffusion barrier layers on dielectric and semiconductor materials are costly, time-consuming, and face challenges in achieving uniform coverage and conductivity, leading to issues with copper interconnects due to void formation and electromigration.
A wet process for depositing manganese oxide barrier layers on dielectric or semiconductor substrates, involving a pretreatment with an aqueous solution containing manganese compounds and inorganic pH buffers, followed by optional heat treatment, which enhances adhesion and conductivity.
The wet process significantly reduces processing time, eliminates the need for vacuum equipment, and improves interconnect conductivity while maintaining effective barrier properties, addressing the limitations of dry vacuum methods.
Smart Images

Figure 0007589431000012 
Figure 0007589431000013 
Figure 0007589431000014
Abstract
Description
[Technical field]
[0001] The present invention relates generally to a wet method for forming diffusion barriers on dielectric and semiconductor materials for interconnect fabrication. [Background technology]
[0002] Integrated circuit devices typically include circuit elements such as transistors, capacitors, and resistors formed in or on a semiconductor substrate. Interconnect structures are used to electrically couple or connect the discrete circuit elements into functional circuits.
[0003] These interconnect structures can be fabricated from a variety of metals and metal alloys, including copper and cobalt. Copper as a metal is the second best conductor after silver and is often the most likely choice as the primary conductor metal for many IC metallization applications. Copper is also notoriously prone to diffusion and electromigration (EM), which can result in void formation and failure, and therefore needs to be fully encapsulated within a diffusion barrier. Thus, these interconnect structures typically include a barrier layer, such as tantalum or tantalum nitride, and combinations thereof (e.g., tantalum nitride / tantalum).
[0004] The material of the barrier layer must be carefully selected. If the barrier layer is too thick, it will occupy a portion of the copper wiring and increase the effective wiring resistance. On the other hand, if the barrier layer is too thin, it will not function as an efficient metal barrier layer, which may affect device performance and result in low reliability. Furthermore, as device sizes shrink, the barrier and cap layers for interconnect structures also shrink (i.e., become thinner) but must retain their barrier properties.
[0005] Metallization is a critical step in the manufacturing sequence of semiconductor devices. 2 , Si 3 N 4 , Six C y O Z The present invention is directed to processes and compositions that can be used to deposit diffusion barrier metals and / or metal oxides directly onto dielectric or semiconducting materials such as Si, Ge, GaAs, or other dielectric or semiconducting materials used in IC fabrication.
[0006] Traditionally, for the deposition of metals or metal oxides on dielectric or semiconductor materials, diffusion barrier layers are deposited using dry vacuum processes such as physical vapor deposition (PVD), chemical vapor deposition (CVD), or atomic layer deposition (ALD). However, these dry vacuum processing steps have several limitations and drawbacks, including:
[0007] Vacuum processes are significantly more expensive than wet deposition methods (such as electrochemical deposition (ECD) or electroless deposition (ELD)). Dry vacuum methods require highly specialized and sophisticated processing tools, specialized high purity gases, precursor materials, and high purity target materials with dedicated delivery infrastructure to perform and maintain these vacuum processes.
[0008] Vacuum metal deposition rates can be very low, and therefore vacuum processing times can be much longer for vacuum processes than for wet ECD / ELD processes, thereby reducing overall fab productivity.
[0009] As IC geometries are scaled down with each new technology node, the uniform coverage and thickness of the vacuum diffusion barrier in combination with the thickness of the conductive seed layer presents challenges and thus problems for the subsequent Cu ECD metallization gapfill process.
[0010] Vacuum diffusion barriers such as Ta and Ta nitride have a lower electrical conductivity than Cu, reducing the conductivity of the interconnect metal stack as these layers occupy volume that could otherwise be occupied by the much more conductive Cu.
[0011] Mn x S y O z Mn films deposited on Si by dry vacuum methods (CVD, PVD, and ALD) and heat treated to form Mn films have been reported to have excellent diffusion barrier properties against Cu diffusion. However, these dry vacuum methods require long processing times and the use of vacuum equipment.
[0012] It would therefore be desirable to develop a method for depositing manganese films to form diffusion barrier layers on dielectric or semiconductor substrates that overcomes the shortcomings of these dry vacuum methods. Summary of the Invention
[0013] It is an object of the present invention to provide a process for providing an improved barrier layer for metal interconnects on dielectric or semiconductor materials.
[0014] It is another object of the present invention to provide a process for preparing manganese oxide barrier layers for metal interconnects on dielectric or semiconducting materials that can be doped with one or more metals.
[0015] It is yet another object of the present invention to provide a wet process for depositing manganese oxide barrier layers for metal interconnects on dielectric or semiconductor materials.
[0016] It is yet another object of the present invention to provide a wet process for providing a manganese oxide barrier layer for a metallized layer, such as a metallized copper layer.
[0017] To that end, in one embodiment, the present invention generally relates to a method for depositing a diffusion barrier layer on a dielectric or semiconductor substrate, the method comprising: 1. Treating a dielectric or semiconductor substrate with a pretreatment aqueous solution; 2. contacting the treated dielectric or semiconductor substrate with an aqueous deposition solution comprising a manganese compound and an inorganic pH buffer to deposit a diffusion barrier layer on the dielectric or semiconductor substrate, the diffusion barrier layer comprising manganese oxide; 3. Optionally, repeating step a) after step b) to further improve adhesion of the diffusion barrier layer to subsequently deposited copper. [Brief description of the drawings]
[0018] The invention will now be described with reference to the following drawings: [Figure 1] 1 shows a top-down SEM showing a dense MnO2 film on a dielectric surface according to Example 1. [Diagram 2] 13 shows a top-down SEM showing a dense MnO2 film on a dielectric surface according to Example 3. [Diagram 3] 1 shows a top-down SEM showing a dense MnO2 film on a bare silicon surface according to Example 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The present invention is directed to a method for depositing diffusion barrier layers for metal interconnects on dielectric and semiconductor materials based on a wet process. The wet process of the present invention offers several important advantages over conventional dry vacuum processes for forming diffusion barrier layers, including significantly shorter processing times and associated higher productivity, elimination of the need for vacuum equipment / disposables, and higher electrical conductivity of the interconnects.
[0020] The present invention is 2 A wet method for deposition is described, followed by an optional step of thermal treatment in vacuum, reducing atmosphere, or hydrogen plasma.
[0021] Manganese may be doped with one or more metals to improve its barrier performance, adhesion, continuity, nucleation density, and uniformity. Examples of doping metals include zinc, cobalt, ruthenium, palladium, zirconium, chromium, magnesium, titanium, tungsten, rhenium, tantalum, etc.
[0022] As used herein, "a," "an," and "the" refer to both singular and plural referents unless the context clearly dictates otherwise.
[0023] As used herein, the term "about" refers to a measurable value of a parameter, amount, duration, etc., and is meant to include no more than + / -15% variation, preferably no more than + / -10% variation, more preferably no more than + / -5% variation, even more preferably no more than + / -1% variation, and even more preferably no more than + / -0.1% variation of and from the specifically recited value, so long as such variations are appropriate to practice the invention described herein. It is further to be understood that the values referred to by the modifier "about" are themselves specifically disclosed herein.
[0024] As used herein, spatial terms such as "beneath," "below," "lower," "above," "upper," and the like, are used for ease of description to describe the relationship of one element or feature to another element or feature as shown in the figures. Spatially relative terms may be intended to encompass different orientations of the device in use or operation in addition to the orientation depicted in the figures. For example, if the device in the figures is turned over, an element described as "below" or "below" the other element or feature would then be oriented "above" the other element or feature. Thus, the exemplary term "below" may encompass both an orientation of above and below. The device may be otherwise oriented (rotated 90 degrees or in other orientations) and the spatially relative descriptors used herein may be interpreted accordingly. It is further understood that the terms "front" and "back" are not intended to be limiting and are intended to be interchangeable where appropriate.
[0025] As used herein, the terms "comprises" and / or "comprising" specify the presence of stated features, integers, steps, operations, elements, and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components, and / or groups thereof.
[0026] The present invention relates generally to a wet method for depositing a manganese oxide barrier layer on a dielectric or semiconductor substrate. x S y O z When formed, it can act as a diffusion barrier.
[0027] In one embodiment, the present invention generally relates to a method for depositing a diffusion barrier on a dielectric or semiconductor substrate, the method comprising: 1. Treating a dielectric or semiconductor substrate with a pretreatment aqueous solution; 2. contacting the treated dielectric or semiconductor substrate with an aqueous deposition solution comprising a manganese compound and an inorganic pH buffer to deposit a diffusion barrier layer on the dielectric or semiconductor substrate, the diffusion barrier layer comprising manganese oxide; 3. Optionally, repeating step a) after step b) to further improve adhesion of the diffusion barrier layer to the subsequently deposited metal (i.e., copper).
[0028] As described herein, the pretreatment aqueous solution includes one or more adsorptive promoting components capable of preparing a dielectric or semiconductor substrate for manganese oxide deposition thereon. In one embodiment, the one or more adsorptive promoting components include one or more nitrogen, silicon, and / or carbon (N, Si, and / or C) based cationic polymers. These nitrogen, silicon, and / or carbon based cationic polymers or oligomers typically have cationic functional groups containing nitrogen, silicon, and / or carbon atoms. In the case of nitrogen based cationic functional groups, they may be primary nitrogen atoms, secondary nitrogen atoms, tertiary nitrogen atoms, or quaternary nitrogen atoms. The nitrogen, silicon, and / or carbon based cationic polymers or oligomers may have an average molecular weight in the range of about 50 to about 1,000,000 Da, more preferably a weight average molecular weight in the range of about 400 to 10,000, as measured by size exclusion chromatography. In one embodiment, the cationic polymer or oligomer is a quaternary nitrogen based cationic polymer or oligomer, or a silicon based cationic polymer or oligomer.
[0029] The polymers are formed by polymerization of monomers containing nitrogen, silicon, and / or carbon-based cationic functional groups, which can be, for example, alkyleneimines having 2 to 12 carbon atoms, more preferably 2 to 8 carbon atoms, allylamines, diallyldimethylammonium salts, vinylpyridine, lysine, methylvinylpyridine, p-vinylpyridine, siloxanes, and combinations of one or more of the foregoing.
[0030] Examples of nitrogen-based cationic polymers and oligomers include amino-functional substituted polysiloxane polymers, polyethyleneimines, methylaminoethyl resins, alkyltrimethylammonium chlorides, and others. Esters of olefinic alcohols, aminoalkyl esters, esters of ether alcohols, cycloalkyl esters, and esters of halogenated alcohols and polyethylene oxides, such as materials available from Union Carbide Corp. under the trade names NSR N-10, NSR N3000, and NSR 301, can also be used in the practice of the present invention, as described, for example, in U.S. Patent No. 6,375,731 to Catano et al., the subject matter of which is incorporated herein by reference in its entirety.
[0031] In one embodiment, the one or more adsorption enhancing components may be selected from the group consisting of, but not limited to, Gelest N-(2-aminoethyl)-3-aminopropyltrimethoxysilane-propyltrimethoxysilane, N-[3-(trimethoxysilyl)propyl]ethylenediamine-(trimethoxysilyl)propane, oligomeric cohydrolyzates, Gelest Polysiloxanes including amino-substituted polysiloxanes such as N-3-[(amino(polypropyleneoxy)]aminopropyltrimethoxysilane, N-[3-(trimethoxysilyl)propyl]polypropyleneoxidediamine or 3-aminopropyltris(methoxyethoxyethoxy)silane, 3-[tris(methoxyethoxyethoxy)silyl]propylamine, 9,9-bis[2-(2-methoxyethoxy)ethoxy]-2,5,8-trioxa-9-siladodecane-12-amine; γ-aminopropyltris(methoxyethoxyethoxy)silane. One example of an amino-functional polysiloxane is available under the trade name Dynasylan® Hydrosil 1151 (aqueous 3-aminopropylsilane hydrolysate), available from Evonik Industries AG.
[0032] These adsorptive promoting components can be used alone or in combination with other components in the aqueous solution. In one embodiment, the pretreatment aqueous solution comprises one or more cationic nitrogen, silicon, and / or carbon-based polymers at a concentration of 1 to 500 g / L, more preferably 3 to 150 g / L, more preferably 25 to 125 g / L.
[0033] The one or more additional components may include one or more of an alkaline agent, an adsorption enhancer, an adhesion promoter, a dispersing agent, an emulsifying agent, a coupling agent, and / or a surfactant. Optionally, the aqueous pretreatment solution may also include a cupric ion and / or a chloride source.
[0034] An example of a pretreatment solution according to the present invention is one or more adsorption-promoting components, Alkaline agents, b. Adsorption enhancers; C. surfactants, d. a source of copper ions; e. one or more cationic nitrogen, silicon, and / or carbon based polymers or oligomers in combination with one or more of the following:
[0035] Suitable alkaline sources include, but are not limited to, alkanolamines, alkali metal hydroxides, alkali metal carbonates (e.g., sodium carbonate, potassium carbonate, sodium bicarbonate, potassium bicarbonate, sodium sesquicarbonate, potassium sesquicarbonate, etc., or combinations thereof), alkali metal borates (e.g., sodium borate, potassium borate, etc., or combinations thereof), alkali metal oxides (e.g., sodium oxide, potassium oxide, etc., or combinations thereof), etc., or combinations thereof. In one preferred embodiment, the alkaline source includes an alkanolamine.
[0036] In a preferred embodiment, the alkaline source may include ethanolamine and / or carbonate, which may be used alone or in combination. In a more preferred embodiment, the alkaline source may include monoethanolamine, diethanolamine, triethanolamine, 2-amino-2-methyl-1-propanol, monoisopropanolamine, diisopropanolamine, 2-(2-aminoethoxy)ethanol (DGA), and / or alkali metal carbonate. When used, the alkaline agent may be present in the pretreatment solution at a concentration in the range of 0.5 to 10 g / L, more preferably in the range of 2 to 8 g / L.
[0037] The adsorption enhancer is preferably selected from the group consisting of alkanolamines such as triethanolamine (TEA), diethanolamine (DEA), 3-amino-1-propanol, amino-2-propanol, and the like. In a preferred embodiment, the adsorption enhancer comprises a mixture of monoethanolamine and triethanolamine. As is readily apparent, triethanolamine and diethanolamine are alkanolamines and therefore can function as both an alkaline agent and an adsorption enhancer in the composition. When used in the pretreatment solution, the concentration of one or more adsorption enhancers can range from about 0.01 to about 5 g / L, more preferably from about 0.05 to about 0.5 g / L.
[0038] In one embodiment, the surfactant comprises a polyoxyalkylene alkyl ether. For example, the surfactant may comprise a surfactant represented by the following general formula (1): RO(CH2CH(CH3)O) x (CH2CH2O) y H (1)
[0039] In the general formula (1), R is an alkyl group having 3 to 20 carbon atoms, preferably an alkyl group having 12 carbon atoms, and x and y are values representing the degree of polymerization of the oxypropylene moiety and the oxyethylene moiety, respectively. In one embodiment, x has a value of about 1 to 20, more preferably about 3 to 10, and y has a value of about 1 to 20, more preferably about 3 to 10. Examples of commercially available polyoxyalkylene alkyl ether compounds include EMULGEN LS-106, EMULGEN LS-110, EMULGEN LS-114, and EMULGEN MS-110, all available from Kao Co., Ltd.
[0040] In one embodiment, the surfactant may act as an adhesion promoter, a dispersing agent, an emulsifying agent, and / or a coupling agent.
[0041] The pretreatment solution also optionally, but preferably, contains a copper source. In one embodiment, the copper source is copper sulfate pentahydrate or another suitable copper salt.
[0042] The pretreatment solution also optionally, but preferably, contains a chloride source, in one embodiment, the chloride source is selected from the group consisting of sodium chloride, potassium chloride, ammonium chloride, magnesium chloride, cupric chloride, or another commercially available chloride source.
[0043] The dielectric or semiconductor substrate is contacted with the pretreatment solution by immersing or contacting the dielectric substrate with the pretreatment solution for a time sufficient to pretreat the surface of the dielectric substrate. Adsorption is a very rapid process that results in an adsorption / desorption rate equilibrium. Once this adsorption / desorption equilibrium point is reached, the dielectric substrate can be removed from the pretreatment solution. In one embodiment, the dielectric substrate is contacted with the pretreatment solution for about 15 seconds to about 10 minutes, more preferably about 20 seconds to about 6 minutes, and most preferably about 30 seconds to about 4 minutes.
[0044] During contact of the dielectric substrate with the pretreatment solution, the temperature of the pretreatment solution is typically maintained in the range of about 20 to about 80° C., more preferably about 40 to about 50° C. After contact with the pretreatment solution, the dielectric substrate is preferably rinsed with water, more preferably deionized water, to remove excess pretreatment solution from the dielectric substrate.
[0045] This pretreatment step prepares the surface of the dielectric or semiconductor substrate for manganese oxide deposition. Without the pretreatment steps described herein, manganese oxide deposition will generally be much less effective.
[0046] After contacting the dielectric or semiconductor substrate with the pretreatment solution and then rinsing, the pretreated dielectric or semiconductor substrate is contacted with a manganese oxide deposition solution described herein.
[0047] The manganese oxide deposition solution preferably contains a suitable manganese compound and an inorganic pH buffer.
[0048] In one embodiment, the manganese compound is an oxidizing agent. For example, the manganese compound may include manganese salts such as sodium permanganate, potassium permanganate, or magnesium permanganate, or combinations thereof. Although sodium permanganate is the most soluble, its presence in significant concentrations is undesirable in damascene processes. Therefore, alternative permanganates such as magnesium permanganate or zinc permanganate are preferred.
[0049] For example, in the case of zinc permanganate, the concentration is preferably within the range of about 0.1 to about 5 g / L.
[0050] The manganese deposition solution also includes an inorganic pH buffer, which may be boric acid, a borate salt, phosphoric acid, or a phosphate salt. In one embodiment, the inorganic pH buffer is boric acid, which is highly stable to oxidation in hot permanganate solutions. Another inorganic pH buffer that may be used in the compositions of the present invention is a phosphate salt. In contrast to the buffers described herein, many prior art buffers are organic and therefore vulnerable to oxidation. The saturation point of boric acid in permanganate is about 15 g / L, so the preferred concentration of boric acid in the solution is in the range of about 5-15 g / L, more preferably 8-12 g / L.
[0051] A variety of dielectric substrates can be used for interconnect fabrication. However, it can be difficult to achieve high adhesion to some of them, including, for example, SiCO-based low-k dielectric substrates. Therefore, in some embodiments, co-deposition of a doping compound or metal with manganese is beneficial to improve the adhesion of manganese oxide films.
[0052] Examples of these doping metals include, but are not limited to, zinc, cobalt, nickel, chromium, molybdenum, tungsten, rhenium, palladium, rhodium, platinum, iridium, osmium, ruthenium, titanium, zirconium, tantalum, magnesium, and other similar metals, which may be used alone or in combination with each other. In a preferred embodiment, the co-deposited doping metals include one or more of zinc, cobalt, nickel, chromium, rhenium, palladium, ruthenium, tungsten, titanium, zirconium, tantalum, or magnesium.
[0053] Depending on the nature of the co-deposited doping metal, its position in the electromotive series, and the relative stability of its oxidation states, some or all of it may be in the form of an oxide, and in some embodiments, both the manganese and the doping metal oxide may be reduced to the metal by annealing in forming gas or hydrogen plasma.
[0054] Optionally, the doping metal can be deposited in a separate subsequent step, which can be through a wet reduction step based on aminoborane, hydrazine, borohydride, hypophosphite, or other reducing solutions, or a dry reduction step using forming gas or hydrogen plasma.
[0055] Other doping metals that may be included in the manganese deposition solution include MnO 2 To more carefully control the thickness of the film, metals that can modify the nucleation rate and grain size to improve continuity, uniformity, and reduce roughness, which is important due to the geometry of the features, include doping metals such as, but not limited to, molybdenum, germanium, indium, hafnium, and / or vanadium.
[0056] Alternatively, the doping metal may be added to the manganese deposition solution as a doping compound. Examples of these doping compounds include, but are not limited to, cobalt chloride, cobalt sulfate, hexafluorozirconate, zirconium sulfate, chromium sulfate, hexafluorotitanate, magnesium sulfamate, magnesium chloride, palladium chloride, palladium bromide, palladium sulfate, ammonium tungstate, nickel sulfamate, nickel chloride, nickel sulfate, ruthenium chloride, tantalum chloride, ammonium molybdate, aluminum sulfate, gallium nitrate, indium sulfate, hafnium acetate, vanadyl sulfate, and the like. In another embodiment, the doping compound is a fluoride salt, such as titanium(4+) dihydrogen hexafluoride.
[0057] Optionally, the manganese oxide deposition solution may include an acrylic block copolymer, such as a polyacrylate / methacrylate block copolymer.
[0058] The pH of the manganese oxide deposition solution is very important since it controls the manganese redox potential and therefore determines the equilibrium between the various manganese oxidation states, which in turn affects manganese oxide uptake. In one embodiment, the pH of the manganese oxide deposition solution is preferably from about 2 to about 7, more preferably from about 3 to about 6, more preferably from about 3.5 to about 5.5. The deposition time is from about 0.5 to about 10 minutes, more preferably from about 2 to about 6 minutes. The temperature of the manganese oxide deposition solution is preferably in the range of from about 70 to about 100°C, more preferably from about 80 to about 90°C.
[0059] After deposition, the manganese oxide layer is rinsed with water. In one embodiment, if the manganese oxide and the second codeposited metal are deposited in separate steps, the oxide layer may be rinsed with water after each step.
[0060] In one embodiment, the substrate may be, but is not limited to, silicon oxide (SiO 2 ), silicon nitride (e.g., Si 3 N 4 The dielectric substrate may include a dielectric material, including silicon-based low-k dielectrics (e.g., k<about 4.0), hydrogenated silicon oxycarbide (SiCOH), SiCH, SiCNH, other dielectric and semiconductor materials, or other types of silicon-based low-k dielectrics (e.g., k<about 4.0), porous dielectrics, or known ULK (ultra-low dielectric constant) dielectric materials (k<about 2.5). The thickness of the dielectric layer defines the vertical height (or thickness) of the metallization formed within the dielectric layer and will vary depending on the application. In another embodiment, the substrate is a semiconductor material, which may be selected from the group consisting of silicon, germanium, and gallium arsenide. Other dielectric and semiconductor materials may also be treated using the wet processes described herein to form a diffusion barrier layer thereon.
[0061] As discussed above, in one embodiment, an aqueous pretreatment solution is subsequently applied to the dielectric or semiconductor substrate after the diffusion barrier is deposited to further improve adhesion of the diffusion barrier layer to a subsequently deposited metal layer, which may be copper.
[0062] In one embodiment, an additional adhesion promotion step using an adhesion promotion composition may be performed. If used, this step may be performed before the pretreatment step, before the manganese deposition step, or after the manganese deposition step. If used, the adhesion promotion composition includes a polyacrylate copolymer and a surfactant. Suitable surfactants include, but are not limited to, polyether polyols, polyacrylates, alcohol ethoxylates, EO / PO block copolymers, aminopropionates, sulfosuccinates, lauramine oxide, and other similar compounds, which may be used alone or in combination. The concentration of the polyacrylate copolymer may range from about 0.5 to about 10 g / L, more preferably from about 0.5 to about 5 g / L. The concentration of the surfactant may range from about 0.1 to about 10 g / L, more preferably from about 0.5 to about 3.0 g / L.
[0063] The diffusion barrier layer may also be subjected to a step of heat treating the diffusion barrier layer, the heat treating step being carried out by annealing in forming gas. x S y O z Convert to.
[0064] The present invention also generally relates to a two-part kit for treating a dielectric or semiconductor substrate to form a manganese oxide barrier layer thereon, the kit comprising: a) an aqueous pretreatment solution comprising one or more adsorption-promoting components capable of preparing a substrate for deposition of manganese oxide thereon; b) a manganese oxide deposition solution, the manganese oxide deposition solution comprising a manganese compound and an inorganic pH buffer.
[0065] In addition, as discussed above, the manganese oxide deposition solution may also include one or more codeposited doping metals or their oxides, or one or more doping compounds.
[0066] The invention will now be described with reference to the following non-limiting examples.
[0067] Example 1: A. A pretreatment solution was prepared according to Table 1 below, and a manganese oxide deposition solution was prepared according to Table 2 below.
[0068] [Table 1]
[0069] [Table 2]
[0070] The dielectric substrate was processed according to the following process sequence. Process sequence: A) Surface treatment solution #1, 4 min, 50°C B) Deionized water (DIW) rinse C) MnO 2 Deposition solution, 4 min, 85 °C D) DIW Rinse E)N 2 Drying
[0071] Sample surface analysis: Wafer coupon samples were stripped in 10 mL of stripping solution containing 10% (v / v) sulfuric acid with 5% (v / v) hydrogen peroxide. Inductively coupled plasma (ICP) atomic emission spectroscopy detected 0.5300 mg / L Mn, while a blank control sample detected less than 0.0500 mg / L Mn.
[0072] Thus, the process described in Example 1 produced a manganese oxide layer on the surface of the dielectric layer. 2 1 shows a top-down SEM image showing the membrane.
[0073] This example was repeated using bare silicon coupons instead of the dielectric wafer coupons. After processing, the silicon coupons were subjected to Cu deposition and annealing at 400° C. The coupons were then inspected for copper silicide formation on the backside. The manganese oxide film was found to function as an effective diffusion barrier.
[0074] Example 2: The pretreatment solution was prepared according to Table 3 below, and the manganese oxide deposition solution was prepared according to Table 2 in Example 1.
[0075] [Table 3]
[0076] The process sequence described in Example 1 was followed to process the dielectric substrate.
[0077] Wafer coupon samples were stripped in 10 mL of stripping solution containing 10% (v / v) sulfuric acid with 5% (v / v) hydrogen peroxide as in Example 1. 0.0500 mg / L Mn was detected by ICP, while <0.0500 mg / L Mn was detected in the blank control sample.
[0078] This example was repeated using bare silicon coupons instead of the dielectric wafer coupons. After processing, the silicon coupons were subjected to Cu deposition and annealing at 400° C. The coupons were then inspected for backside copper silicide formation. The manganese oxide film was found to function as an effective diffusion barrier.
[0079] Example 3: The pretreatment solution was prepared according to Table 4 below, and the manganese oxide deposition solution was prepared according to Table 2 in Example 1.
[0080] [Table 4]
[0081] The dielectric substrate was processed according to the following process sequence. Process sequence: A) Surface treatment solution, 1 min, RT B) Deionized water (DIW) rinse, 20 seconds C) MnO 2 Deposition solution, 4 min, 85 °C D) Light DIW Rinse E) Curing, 10 minutes, 80℃
[0082] Wafer coupon samples were stripped in 10 mL of stripping solution containing 10% (v / v) sulfuric acid with 5% (v / v) hydrogen peroxide as in Example 1. 0.1100 mg / L Mn was detected by ICP, while <0.0500 mg / L Mn was detected in the blank control sample.
[0083] Figure 2 shows the MnO 2 1 shows a top-down SEM image showing the membrane.
[0084] This example was repeated using bare silicon coupons instead of the dielectric wafer coupons. After processing, the silicon coupons were subjected to Cu deposition and annealing at 400° C. The coupons were then inspected for copper silicide formation on the backside. The manganese oxide film was found to function as an effective diffusion barrier.
[0085] Example 4: Wafer coupon samples were also prepared on bare silicon substrates. The wafer coupon samples were stripped in 10 mL of stripping solution containing 10% (v / v) sulfuric acid with 5% (v / v) hydrogen peroxide as in Example 1. 0.2300 mg / L Mn was detected by ICP, while <0.0500 mg / L Mn was detected in the blank control sample.
[0086] The described process is capable of depositing an effective manganese oxide barrier layer onto both dielectric and semiconductor substrates for depositing metal layers thereon.
[0087] Figure 3 shows the MnO 2 1 shows a top-down SEM image showing the membrane.
[0088] Example 5: The pretreatment solution was prepared according to Table 5 below, and the manganese oxide deposition solution was prepared according to Table 2 in Example 1.
[0089] [Table 5]
[0090] The process sequence described in Example 1 was followed to process the dielectric substrate.
[0091] Wafer coupon samples were stripped in 10 mL of stripping solution containing 10% (v / v) sulfuric acid with 5% (v / v) hydrogen peroxide as in Example 1. 0.0946 mg / L Mn was detected by ICP, while <0.0500 mg / L Mn was detected in the blank control sample.
[0092] This example was repeated using bare silicon coupons instead of the dielectric wafer coupons. After processing, the silicon coupons were subjected to Cu deposition and annealing at 400° C. The coupons were then inspected for backside copper silicide formation. The manganese oxide film was found to function as an effective diffusion barrier.
[0093] Example 6. Wafer coupon samples were pretreated with the solutions described in Table 1 from Example 1 and then treated with the manganese oxide deposition solutions described in Table 2 from Example 1 with the addition of codeposited metal compounds. The codeposited metals tested included the following: 1. Zn, 2. Co, 3. Ti, 4. Zr, 5. Pd, 6. Blank dielectric control sample with no deposition
[0094] The process sequence described in Example 1 was followed to process the dielectric substrate.
[0095] ICP detected Mn in the Zn, Co, Ti, Zr, and Pd spiked samples with values of 0.171 mg / L, 0.292 mg / L, 0.396 mg / L, 0.458 mg / L, and 0.31 mg / L, respectively. The blank control sample had an ICP result of <0.05 mg / L Mn.
[0096] Four wafer coupon samples were analyzed using X-ray photoelectron spectroscopy (XPS). Two of them were pretreated with the solution described in Table 1 from Example 1 and then treated with the manganese deposition solution described in Table 2 from Example 1 with added Zn, and the other two were blank dielectric control samples with no deposition. One sample study with a co-deposited MnZn film showed 13.7 at% Mn and 0.9 at% Zn, and the other MnZn sample showed 14.4 at% Mn and 1.2 at% Zn.
[0097] This example was repeated using bare silicon coupons instead of the dielectric wafer coupons. After processing, the silicon coupons were subjected to Cu deposition and annealing at 400° C. The coupons were then inspected for backside copper silicide formation. The manganese oxide film was found to function as an effective diffusion barrier.
[0098] Example 7: Wafer coupon samples were pretreated with the solutions described in Table 4 from Example 3, except that the concentration of HS-1151 was reduced from 30 g / L to 15 g / L. The wafer coupon samples were then treated with manganese oxide deposition solutions. The deposition solutions tested are described below in Tables 6 and 7.
[0099] [Table 6]
[0100] [Table 7]
[0101] The process sequence described in Example 3 was followed to process the dielectric substrate.
[0102] Wafer coupon samples were stripped in 10 mL of stripping solution containing 10% (v / v) sulfuric acid with 5% (v / v) hydrogen peroxide as in Example 1. The ICP values of Mn detected for the samples treated with copolymer (1) and copolymer (2) were 0.2070 mg / L and 0.1570 mg / L, respectively. The blank control sample had an ICP result of Mn of <0.0500 mg / L.
[0103] The described process can deposit a manganese oxide barrier layer that is effective for depositing a metal layer thereon. The wet process described herein improves adhesion between the dielectric / semiconductor substrate and the manganese oxide barrier layer.
[0104] This example was repeated using bare silicon coupons instead of the dielectric wafer coupons. After processing, the silicon coupons were subjected to Cu deposition and annealing at 400° C. The coupons were then inspected for copper silicide formation on the backside. The manganese oxide film was found to function as an effective diffusion barrier.
[0105] Example 8: Wafer coupon samples were pretreated with the solutions described in Table 4 from Example 3, except that the concentration of HS-1151 was reduced from 30 g / L to 15 g / L. The wafer coupon samples were then treated with the manganese oxide deposition solutions described in Table 8 below.
[0106] [Table 8]
[0107] Suitable metal salts can be found in Example 6.
[0108] The process sequence described in Example 3 was followed to process the dielectric substrate.
[0109] Wafer coupon samples were stripped in 10 mL of stripping solution containing 10% (v / v) sulfuric acid with 5% (v / v) hydrogen peroxide as in Example 1. ICP analysis detected 0.156 mg / L Mn in the sample. A blank control sample had an ICP result of <0.0500 mg / L Mn.
[0110] The described process can deposit a manganese oxide barrier layer that is effective for depositing a metal layer thereon. The wet process described herein improves adhesion between the dielectric / semiconductor substrate and the manganese oxide barrier layer.
[0111] This example was repeated using bare silicon coupons instead of the dielectric wafer coupons. After processing, the silicon coupons were subjected to Cu deposition and annealing at 400° C. The coupons were then inspected for copper silicide formation on the backside. The manganese oxide film was found to function as an effective diffusion barrier.
[0112] Example 9: Wafer coupon samples were pretreated with the solutions described in Table 4 from Example 3, except that the concentration of HS-1151 was reduced from 30 g / L to 15 g / L. The wafer coupon samples were then treated with the manganese oxide deposition solutions described in Table 2. Additional steps that can be applied either before the pretreatment, before the deposition step, or after the deposition step are described below in Table 9.
[0113] [Table 9]
[0114] This additional adhesion promotion step was applied for 1 minute at ambient temperature. After applying this additional adhesion promotion step, the coupons were rinsed with DI water.
[0115] The surfactants tested are listed below. 1. Ethylenediamine-initiated polyether polyols 2. Polyacrylate surfactants 3. Alcohol EO / PO 4. Aminopropionates 5. Sulfosuccinate 6. Lauramine oxide
[0116] Wafer coupon samples were stripped in 10 mL of stripping solution containing 10% (v / v) sulfuric acid with 5% (v / v) hydrogen peroxide as in Example 1. TCP analysis on samples where this additional adhesion promotion step was applied before the pretreatment step detected 0.170 mg / L Mn. ICP analysis on samples where this additional adhesion promotion step was applied before the deposition step detected 0.116 mg / L Mn. ICP analysis on samples where this additional adhesion promotion step was applied after the deposition step detected 0.188 mg / L Mn. Blank control samples had ICP results of <0.0500 mg / L Mn.
[0117] The described process can deposit a manganese oxide barrier layer that is effective for depositing a metal layer thereon. The wet process described herein improves adhesion between the dielectric / semiconductor substrate and the manganese oxide barrier layer.
[0118] This example was repeated using bare silicon coupons instead of the dielectric wafer coupons. After processing, the silicon coupons were subjected to Cu deposition and annealing at 400° C. The coupons were then inspected for backside copper silicide formation. The manganese oxide film was found to function as an effective diffusion barrier.
[0119] Example 10: Wafer coupon samples were pretreated with the solutions described in Table 4 from Example 3, except that the concentration of HS-1151 was reduced from 30 g / L to 15 g / L. The wafer coupon samples were then treated with the manganese oxide deposition solutions described in Table 10 below.
[0120] [Table 10]
[0121] The process sequence described in Example 3 was followed to process the dielectric substrate.
[0122] The wafer coupon sample was stripped in 10 mL of stripping solution containing 10% (v / v) sulfuric acid with 5% (v / v) hydrogen peroxide as in Example 1. The ICP value of Mn detected for this sample was 0.1940 mg / L. The blank control sample had an ICP result of Mn of <0.0500 mg / L.
[0123] The processes described therein can deposit a manganese oxide barrier layer that is effective for depositing a metal layer thereon. The wet process described herein improves adhesion between the dielectric / semiconductor substrate and the manganese oxide barrier layer.
[0124] This example was repeated using bare silicon coupons instead of the dielectric wafer coupons. After processing, the silicon coupons were subjected to Cu deposition and annealing at 400° C. The coupons were then inspected for backside copper silicide formation. The manganese oxide film was found to function as an effective diffusion barrier.
[0125] Example 11: Wafer coupon samples were pretreated with the solutions described in Table 4 of Example 3, except that the concentration of HS-1151 was reduced from 30 g / L to 15 g / L. The wafer coupon samples were then treated with the manganese oxide deposition solutions described in Table 11 below.
[0126] [Table 11]
[0127] The pH of the deposition solution was reduced to pH 3.5 using hydrochloric acid.
[0128] The process sequence described in Example 3 was followed to process the dielectric substrate.
[0129] Wafer coupon samples were stripped in 10 mL of stripping solution containing 10% (v / v) sulfuric acid with 5% (v / v) hydrogen peroxide as in Example 1. 0.1912 mg / L Mn was detected by ICP, while <0.0500 mg / L Mn was detected in the blank control sample.
[0130] This example was repeated using bare silicon coupons instead of the dielectric wafer coupons. After processing, the silicon coupons were subjected to Cu deposition and annealing at 400° C. The coupons were then inspected for copper silicide formation on the backside. The manganese oxide film was found to function as an effective diffusion barrier.
[0131] The samples produced according to Examples 1-11 were then subjected to a diffusion barrier performance evaluation. The samples were coated with copper deposited by PVD and electroplated with electrochemical deposition (ECD) copper. The Mn x S y O z The performance of the diffusion barrier was evaluated and poor diffusion barrier performance resulted in an increase in sheet resistance, indicating diffusion of copper from the surface into the bulk of the dielectric.
[0132] The results demonstrated that the Mn-based wet diffusion barrier films deposited by the processes described herein can exhibit excellent barrier performance.
[0133] Comparative Example 1 The wafer coupon samples were treated only with the manganese oxide deposition solution detailed in Table 2 of Example 1.
[0134] The dielectric substrate was processed according to the following process sequence. Process sequence: A.MnO 2 Deposition solution, 4 min, 85 °C B.DIW Rinse CN 2 Drying
[0135] Wafer coupon samples were stripped in 10 mL of stripping solution containing 10% (v / v) sulfuric acid with 5% (v / v) hydrogen peroxide as in Example 1. ICP values of Mn detected for treated samples were <0.0500 mg / L. Blank control samples had ICP results of Mn <0.0500 mg / L.
[0136] Copper silicide formation on the backside of the coupon indicated that the deposited film did not function as a diffusion barrier.
[0137] Therefore, without the additional pretreatment step, the process is not capable of depositing an effective manganese oxide barrier layer.
[0138] Comparative Example 2 The pretreatment solution was prepared according to Table 4 shown in Example 3. The manganese oxide deposition solution was prepared according to Table 2 in Example 1.
[0139] The dielectric substrate was processed according to the following process sequence. Process sequence: A) Surface treatment solution, 1 min, RT B) Deionized water (DIW) rinse, 20 seconds C) MnO 2 Deposition solution, 4 min, 85 °C D) Light DIW Rinse
[0140] Wafer coupon samples were stripped in 10 mL of stripping solution containing 10% (v / v) sulfuric acid with 5% (v / v) hydrogen peroxide as in Example 1. ICP values of Mn detected for treated samples were <0.0500 mg / L. Blank control samples had ICP results of Mn <0.0500 mg / L.
[0141] Copper silicide formation on the backside of the coupon indicated that the deposited film did not function as a diffusion barrier.
[0142] The process is not capable of depositing an effective manganese oxide barrier layer. In order to deposit a sufficient manganese barrier layer, the wafer coupon sample needs to be cured after the manganese oxide deposition step.
[0143] Thus, the processes described herein are capable of depositing an effective manganese oxide barrier layer onto which a metal layer can be deposited. As can be seen from the examples, manganese was detected by ICP in amounts of at least 0.05 mg / L, or at least 0.010 mg / L, or 0.20 mg / L, or even at least 0.50 mg / L in samples treated according to the processes described herein compared to untreated samples. The wet processes described herein require significantly shorter processing times and produce higher interconnect conductivity in contrast to conventional methods.
[0144] Finally, it should also be understood that the following claims are intended to cover, subject to language considerations, all of the general and specific features of the invention described herein, and the full scope of the invention.
Claims
1. 1. A method for depositing a diffusion barrier layer on a dielectric or semiconductor substrate, the method comprising: a) treating the dielectric or semiconductor substrate with an aqueous pretreatment solution comprising one or more adsorption promoting components, the one or more adsorption promoting components comprising one or more cationic nitrogen, silicon, and / or carbon based polymers or oligomers; b) contacting the treated dielectric or semiconductor substrate with an aqueous deposition solution comprising a manganese compound and an inorganic pH buffer to deposit the diffusion barrier layer on the dielectric or semiconductor substrate, wherein the diffusion barrier layer comprises manganese oxide.
2. 10. The method of claim 1, wherein the dielectric or semiconductor substrate is treated with the aqueous pretreatment solution to prepare the substrate for deposition of the diffusion barrier layer thereon.
3. 10. The method of claim 1, wherein the aqueous pretreatment solution comprises one or more additional components, the one or more additional components being selected from the group consisting of an alkaline agent, an adsorption enhancer, an adhesion promoter, a dispersing agent, an emulsifying agent, a coupling agent, a surfactant, a copper source, a chloride source, and combinations of the foregoing.
4. The method further includes a heat treatment step of heat treating the diffusion barrier layer, the heat treatment step being performed by a step of annealing in forming gas, the step of annealing being performed by converting manganese oxide to Mn x S y O z The method of claim 1 , wherein
5. 10. The method of claim 1, wherein the substrate is a dielectric or semiconductor substrate selected from the group consisting of silicon oxide, silicon nitride, hydrogenated silicon oxycarbide, SiCH, SiCNH, other dielectric and semiconductor materials, silicon based low-k dielectrics, porous dielectrics, ultra-low-k dielectric materials, silicon, germanium, gallium arsenide, and combinations of one or more of the foregoing.
6. The method of claim 1 , wherein after contacting the substrate with the aqueous deposition solution, the substrate is rinsed with water.
7. 10. The method of claim 1 further comprising carrying out the adhesion promotion step using an adhesion promotion composition comprising a polyacrylate copolymer and a surfactant.
8. The method of claim 1 , wherein the manganese compound is an oxidizer comprising a permanganate compound.
9. 9. The method of claim 8, wherein the permanganate compound is selected from the group consisting of sodium permanganate, potassium permanganate, magnesium permanganate, zinc permanganate, and combinations of the foregoing.
10. 2. The method of claim 1, wherein the inorganic pH buffer is selected from the group consisting of boric acid, a borate salt, phosphoric acid, and a phosphate salt.
11. The method of claim 1, wherein the aqueous deposition solution has a pH of 2-7.
12. 2. The method of claim 1, wherein the aqueous deposition solution comprises a doping codeposited metal with manganese to improve adhesion, continuity and uniformity of the diffusion barrier layer, the doping codeposited metal comprising one or more metals selected from the group consisting of zinc, cobalt, nickel, chromium, molybdenum, tungsten, rhenium, palladium, rhodium, platinum, iridium, osmium, ruthenium, titanium, zirconium, tantalum, magnesium, and combinations of one or more of the foregoing.
13. The method of claim 1 further comprising depositing a metal layer over the diffusion barrier layer.
14. The method of claim 13 , wherein the metal layer comprises copper or a copper alloy.
15. 1. A two-part kit for treating a dielectric or semiconductor substrate to form a diffusion barrier layer thereon, said kit comprising: a) an aqueous pretreatment solution comprising one or more adsorption-promoting components capable of preparing the substrate for manganese oxide deposition thereon; b) a manganese deposition solution comprising a manganese compound and an inorganic pH buffer.
16. 16. The kit of claim 15, wherein the adsorption-promoting component comprises one or more nitrogen-, silicon-, and / or carbon-based cationic polymers or oligomers.
17. 16. The kit of claim 15, wherein the aqueous pretreatment solution comprises one or more additional components, the one or more additional components being selected from the group consisting of an alkaline agent, an adsorption enhancer, an adhesion promoter, a dispersing agent, an emulsifying agent, a coupling agent, a surfactant, a copper source, a chloride source, and combinations of the foregoing.
18. 16. The kit of claim 15, wherein the manganese deposition solution includes a doping metal along with manganese to improve adhesion, continuity, and uniformity of the diffusion barrier layer, the codeposited doping metal including one or more metals selected from the group consisting of zinc, cobalt, nickel, chromium, molybdenum, tungsten, rhenium, palladium, rhodium, platinum, iridium, osmium, ruthenium, titanium, zirconium, tantalum, magnesium, and combinations of one or more of the foregoing.
19. 1. An aqueous pretreatment solution for preparing a dielectric or semiconductor substrate for deposition of manganese oxide thereon, said aqueous pretreatment solution comprising one or more adsorptive promoting components, said one or more adsorptive promoting components comprising one or more nitrogen, silicon, and / or carbon based cationic polymers or oligomers, said aqueous pretreatment solution comprising: a. an alkaline agent, b. an adsorption enhancer; c. a surfactant; d. a source of copper ions, and e. a chloride source.
20. The method of claim 7, wherein the surfactant is selected from the group consisting of polyether polyols, polyacrylates, alcohol ethoxylates, EO / PO block copolymers, aminopropionates, sulfosuccinates, lauramine oxides, and one or more combinations thereof.
Citation Information
Patent Citations
Pretreatment liquid of through-hole plating using conductive polymer
JP1995288381A
Plating method, its device and plated structure
JP2000212754A
Semiconductor device and its manufacturing method
JP2005277390A
Method for manufacturing semiconductor device
JP2007165881A
Semiconductor device and method for manufacturing the same
JP2010283103A