Piezoelectric single crystal M3RE(PO4)3 and its growth method and application
The growth of piezoelectric single crystals with non-centrosymmetric structures addresses the lack of research on yttrium strontium phosphate crystals, enabling high-quality crystals for nonlinear optical and piezoelectric applications with high melting points and stable chemical properties.
Patent Information
- Application Number
- JP2021568831
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-06-14
- Filing Date
- 2020-06-10
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-06-10
AI Technical Summary
There is a lack of research on yttrium strontium phosphate single crystals, particularly in the development of piezoelectric single crystals with non-centrosymmetric structures, which are essential for advanced opto-electrical functional devices.
The growth method involves using the pulling method to develop piezoelectric single crystals with non-centrosymmetric structures, belonging to the cubic ~43m point group, utilizing alkaline earth metals like Ba, Ca, or Sr, and rare earth elements like Y, La, or Yb, ensuring high light transmittance, wide absorption edges, and no phase transitions from room temperature to melting points.
The method produces high-quality piezoelectric single crystals with excellent mechanical properties, suitable for nonlinear optical and piezoelectric applications, featuring high melting points, stable chemical properties, and no deliquescence, facilitating their use in high-temperature piezoelectricity and nonlinear optics.
Smart Images

Figure 0007589999000001 
Figure 0007589999000002 
Figure 0007589999000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a piezoelectric single crystal M3RE(PO4)3, its growth method and applications, and belongs to the technical field of optoelectronic functional crystals. [Background technology]
[0002] Optoelectronic functional crystal materials are highly regarded around the world as key materials in various high-tech fields, including microelectronics, optoelectronics, communications, aerospace, and modern military technology. The development of lasers and optoelectronics has further promoted the development and application of functional crystals. China is at the forefront of the world in the research and application of optoelectronic functional crystals, especially inorganic nonlinear optical crystals. Nevertheless, international competition in the field of optoelectronic functional crystals is becoming increasingly fierce, and Chinese crystal material researchers continue to strive to develop new crystal materials.
[0003] There are many types of optoelectronic functional crystals, mainly classified by function as nonlinear optical crystals, piezoelectric crystals, laser crystals, scintillation crystals, etc. Currently, the available optoelectronic functional crystal materials are limited, and it is urgent to explore new functional crystal materials to develop new optoelectronic devices and expand new applications. Research on compounds with the M3RE(PO4)3 structure is currently focused on the synthesis and luminescence properties of nanophosphor powders doped with different rare earth ions. For example, in 2008, Xu Shuai et al. from Tongji University synthesized Eu 3+ , Tb 3+ , Ce 3+ In another example, in 2013, Guo Ning et al. of the Changchun Institute of Applied Chemistry synthesized cubic bismuthite-type Ba3Gd(PO4)3 phosphor powder by a high-temperature solid-phase method, and did not dope with Eu. 2+ , Mn 2+(Non-Patent Document 2: Chem Phys Chem 2013, 14, 192-197). Although several M3RE(PO4)3 type compound powders have been successfully prepared, there are few reports on single crystals with M3RE(PO4)3 type structures and growth techniques.
[0004] So far, no research has been reported on strontium yttrium phosphate crystals. The few studies on Sr3Y(PO4)3 have been limited to Sr3Y(PO4)3 nanophosphor powders doped with different rare earth ions. Regarding the synthesis of Sr3Y(PO4)3 powder, in 2008, Xu Shuai et al. from Tongji University synthesized Eu by solution-gel method to study the luminescence properties of rare earth ion-doped nanophosphor powders. 3+ , Tb 3+ , Ce 3+ However, no research was conducted on the growth of single crystals and their photoelectric properties and applications (Non-Patent Document 3: Journal of Optoelectronics And Advanced Materials Vol. 10, No. 10, October 2008, p. 2727-2731). Therefore, the applicant proposed the present invention in order to develop a new piezoelectric single crystal. [Prior art documents] [Non-patent literature]
[0005] [Non-Patent Document 1] Journal of Optoelectronics And Advanced Materials Vol.10,No10, October 2008,p2727~2731 [Non-Patent Document 2] Chem Phys Chem 2013,14,192~197 [Non-Patent Document 3] Journal of Optoelectronics And Advanced Materials Vol.10,No10, October 2008,p2727~2731 Summary of the Invention [Problem to be solved by the invention]
[0006] In view of the problems associated with the prior art, the present invention provides a piezoelectric single crystal having the general formula M3RE(PO4)3 and a method for growing the same.
[0007] The present invention also provides a single crystal of yttrium strontium phosphate.
[0008] The present invention also provides applications of the yttrium strontium phosphate single crystal.
[0009] Definitions of terms: The following provides definitions of terms used in this specification.
[0010] "Single crystal of strontium yttrium phosphate" refers to the chemical formula Sr3Y(PO4)3, commonly used in the field as SYP. In the present invention, Sr3Y(PO4)3 and SYP have the same meaning.
[0011] "Room temperature" has the meaning commonly known in the art, and generally refers to 25±5°C.
[0012] "Crystal separation" refers to separating the pulled crystal from the melt. [Means for solving the problem]
[0013] This invention is the first to grow M3RE(PO4)3 piezoelectric single crystals with a non-centrosymmetric structure using the pulling method. M3RE(PO4)3 piezoelectric single crystals belong to the ~43m point group of the cubic crystal system. Not only do they have high optical transmittance and a wide absorption edge, but they also have no phase transition from room temperature to the melting point, and have piezoelectric activity and nonlinear frequency conversion properties, which are expected to be applied in the field of optoelectronic functional devices.
[0014] The present invention has been made to solve the above problems as follows: The technical solution of the present invention is as follows:
[0015] A piezoelectric single crystal having the general formula M3RE(PO4)3 is provided.
[0016] The single crystal has a non-centrosymmetric structure and belongs to the cubic crystal system 43m point group, where M represents an alkaline earth metal and RE represents a rare earth element.
[0017] According to the invention, preferably the alkaline earth metal is Ba, Ca or Sr.
[0018] According to the invention, preferably the rare earth element is Y, La, Gd or Yb.
[0019] The rare earth element of the present invention is not limited to the four metals Y, La, Gd or Yb, but can be applied to other rare earth elements, which have similarly excellent mechanical properties, are not easily deliquesced, and have uniform melting properties. Due to its non-centrosymmetric structure, it is suitable for use as a non-linear optical crystal or a piezoelectric crystal. The advantages of its application as a non-linear optical crystal or a piezoelectric crystal are that the crystal has a high melting point, there is no phase transition from room temperature to the melting point, the chemical properties are stable, and it does not deliquesce. As a compound with a non-centrosymmetric structure and a high melting point, it has obvious advantages in the fields of high temperature piezoelectricity and wide temperature range non-linear optics.
[0020] Preferably, the M3RE(PO4)3 piezoelectric single crystal is selected from the following single crystals:
[0021] Ba3Y(PO4)3 single crystal, Ba3La(PO4)3 single crystal, Ba3Yb(PO4)3 single crystal, Ca3Gd(PO4)3 single crystal, Sr3Y(PO4)3 single crystal, Sr3La(PO4)3 single crystal, Sr3Gd(PO4)3 single crystal; the corresponding chemical names are, respectively, yttrium barium phosphate single crystal, barium lanthanum phosphate single crystal, barium ytterbium phosphate single crystal, calcium gadolinium phosphate single crystal, yttrium strontium phosphate single crystal, lanthanum strontium phosphate single crystal, and gadolinium strontium phosphate single crystal.
[0022] Furthermore, the structural parameters of the single crystal are as follows:
[0023] Ba3Y(PO4)3 single crystal: cubic ~43m point group; space group I~43d; lattice constant a=b=c=10.4655Å, density=4.553g / cm3;
[0024] Ba3La(PO4)3 single crystal: cubic ~43m point group; space group I~43d; lattice constant a=b=c=10.521Å, density=4.77g / cm 3 ;
[0025] Ba3Yb(PO4)3 single crystal: cubic ~43m point group; space group I~43d; lattice constant a=b=c=10.459Å, density=5.149g / cm 3 ;
[0026] Ca3Gd(PO4)3 single crystal: cubic ~43m point group; space group I~43d; lattice constant a=b=c=9.857Å, density=3.9g / cm 3 ;
[0027] Sr3Y(PO4)3 single crystal: cubic ~43m point group; space group I~43d; lattice constant a=b=c=10.0814Å, Mitsudo=4.093g / cm 3 ;
[0028] Sr3La(PO4)3 single crystal: cubic ~43m point group; space group I~43d; lattice constant a=b=c=10.192Å, density=4.3g / cm3 ;
[0029] Sr3Gd(PO4)3 single crystal: cubic ~43m point group; space group I~43d; lattice constant a=b=c=10.114Å, density=4.526g / cm 3 .
[0030] According to the present invention, when the piezoelectric single crystal of M3RE(PO4)3 is measured by spectrum analysis for Ba3Y(PO4)3 single crystal, Ba3La(PO4)3 single crystal, Ba3Yb(PO4)3 single crystal, Ca3Gd(PO4)3 single crystal, Sr3La(PO4)3 single crystal, and Sr3Gd(PO4)3 single crystal, all of the above single crystals show an optical transmittance of more than 70% in the 325 nm to 4302 nm band.
[0031] According to the present invention, the piezoelectric single crystals of M3RE(PO4)3 are measured by impedance method respectively for Ba3Y(PO4)3 single crystal, Ba3La(PO4)3 single crystal, Ba3Yb(PO4)3 single crystal, Ca3Gd(PO4)3 single crystal, Sr3La(PO4)3 single crystal, and Sr3Gd(PO4)3 single crystal, and all of the above single crystals show effective piezoelectric constant deff>6pC / N and have piezoelectric activity.
[0032] It is a strontium yttrium phosphate single crystal with the chemical formula Sr3Y(PO4)3, a non-centrosymmetric structure, belonging to the cubic crystal system in the ~43m point group with lattice constants a=10.0814Å, b=10.0814Å, c=10.0814Å, α=β=γ=90°, and no phase transition from room temperature to the melting point.
[0033] Furthermore, the melting point of the yttrium strontium phosphate single crystal is basically 1850° C., and there is no phase transition from room temperature to the melting point.
[0034] Furthermore, when the yttrium strontium phosphate single crystal is measured by spectral analysis, it exhibits a light transmittance of more than 80% in the band of 480 nm to 4100 nm.
[0035] Furthermore, when the yttrium strontium phosphate single crystal is measured by an impedance method, the effective piezoelectric constant is d14=6 to 10 pC / N.
[0036] Furthermore, when the yttrium strontium phosphate single crystal is measured and calculated by an impedance method, the effective electromechanical coupling coefficient k14 is 10 to 30%.
[0037] The present invention provides a method for growing the M3RE(PO4)3 piezoelectric single crystal, comprising the following steps (1) to (3):
[0038] Step (1) in the synthesis of polycrystalline materials, according to the general formula M3RE(PO4)3, the raw materials MCO3, RE2O3 and phosphorus-containing compounds are accurately weighed according to the stoichiometric ratio, and the phosphorus-containing compound is in excess of 1.5-10% of the total mass (based on the stoichiometric ratio of the phosphorus compound in the formula);
[0039] The weighed raw materials are uniformly crushed and mixed, and then sintered once, preferably in a ceramic crucible, at a sintering temperature of 800 o C~950 o C, and the temperature is kept constant for 10-15 hours, then the temperature is lowered, the raw materials for the primary sintering are crushed and refined, mixed uniformly, and pressed into a round cake-like block for secondary sintering, and the sintering temperature is 1200 o C~1400 o C, and keep it at a constant temperature for 20-40 hours to obtain M3RE(PO4)3 polycrystalline material through solid-state reaction;
[0040] In step (2) melting the polycrystalline material, the M3RE(PO4)3 polycrystalline material synthesized in step (1) is placed in an iridium crucible in a single crystal growth furnace, the furnace is evacuated and filled with nitrogen or argon as a protective gas, and the M3RE(PO4)3 polycrystalline material is heated and melted by intermediate frequency induction heating. After the polycrystalline material is completely melted, the temperature is lowered and condensed, and then the temperature is raised again to melt the entire material. This is repeated several times to remove any bubbles generated in the melt, and then the melt is cooled for 10 o C~20 oC After heating and keeping the temperature constant for 0.5 to 2 hours, a homogeneous melt of M3RE(PO4)3 is obtained;
[0041] Step (3) In the crystal growth by the pulling method, an iridium rod or M3RE(PO4)3 single crystal is used as a seed crystal, the seed crystal is immersed in the M3RE(PO4)3 melt, and the lower end of the seed crystal is vertical and just in contact with the melt to start the single crystal growth; the technical conditions for single crystal growth are as follows: growth temperature is 1800 oC At 1950°C, the seed crystal is pulled at a rate of 1-5 mm / h during neck growth, reduced to 0.2-1 mm / h during shoulder growth, and 0.5-1 mm / h during constant diameter growth. When the crystal grows to the desired size, it is separated from the melt.
[0042] More preferably, the pulled and separated crystal is kept at a constant temperature in a temperature field for 0.5 to 1 hour, and then cooled to room temperature at a rate of 5 to 30°C / h to obtain M3RE(PO4)3 crystal.
[0043] Furthermore, after removing the M3RE(PO4)3 crystal from the single crystal growth furnace, it is annealed at a temperature of 1200 to 1400°C. Preferably, the annealing time is in the range of 24 to 48 hours, so that the thermal stress generated during the M3RE(PO4)3 piezoelectric single crystal growth is completely released. Preferably, the M3RE(PO4)3 piezoelectric single crystal is annealed in a high-temperature muffle furnace.
[0044] According to the present invention, preferably, in step (1), the phosphorus-containing compound is NH4H2PO4 or P2O5. More preferably, the phosphorus-containing compound is in excess of 3-6% of its total mass. According to the present invention, in step (1), all of the raw materials are made of high-purity raw materials with a purity of more than 99.9%; these raw materials can be purchased by conventional methods.
[0045] According to the present invention, preferably, in step (1), the primary sintering and secondary sintering of the raw material are carried out in a ceramic crucible, where the purpose of the primary sintering is to decompose and remove CO2, NH3 and H2O, and improve the purity of the synthesized polycrystalline material.
[0046] In the present invention, when a molten liquid pulling method is used to grow a single crystal and an iridium crucible is used, in order to prevent oxidation of iridium at high temperatures, it is necessary to grow the crystal in an inert gas atmosphere such as nitrogen or argon, and in particular, the volume fraction of nitrogen or inert gas is 90% to 95%.
[0047] According to the present invention, in step (2), after melting the polycrystalline material, the temperature is lowered, condensed and heated, and melted repeatedly, and then the bubbles generated in the melt are completely discharged, and the crystal growth defects (bubbles, inclusions, etc.) are reduced, thereby improving the quality of the crystal growth. It is recommended that the temperature lowering-condensation-heating-melting cycle be repeated three to four times.
[0048] According to the present invention, preferably, in step (3), the crystal growth process includes four steps, namely, neck growth, shoulder growth, constant diameter growth, and separation of the pulled crystal from the melt; in the neck growth, the pulling speed is 1-8 mm / h, and when the seed crystal diameter is narrowed to 0.5-2.0 mm, the temperature is slowly lowered at a rate of 0.5-5 ° C / h to grow the shoulder; in the shoulder growth, the pulling speed is lowered to 0.2-1 mm / h; when the shoulder diameter of the crystal reaches the desired size, the temperature is raised or lowered at a rate of 0.5-5 ° C / h, and the temperature is maintained at 1800-1950 ° C to grow the constant diameter; when the crystal grows to the desired size, the pulled crystal is separated from the melt.
[0049] More preferably, the method for separating the pulled crystal from the melt is as follows: slowly increase the temperature at a rate of 10 to 50°C / h, and if the lower end of the crystal has a tendency to shrink inward, increase the pulling speed to 5 to 20 mm / h, and pull up the crystal to separate it from the melt.
[0050] According to the present invention, the size of the single crystal growth is preferably generally 15-30 mm in diameter and 20-50 mm in height. The growth of M3RE(PO4)3 piezoelectric single crystal of this size usually takes 4-7 days. The crystal size refers to the typical diameter and total height of the crystal.
[0051] According to the present invention, the yttrium strontium phosphate single crystal is grown by a pulling method, and the key to this technology lies in the blending ratio of raw materials, especially the use of excess phosphate raw materials, synthesizing polycrystalline materials, and obtaining single crystals of high optical quality under the conditions of suitable temperature and specific temperature field to meet the application needs of nonlinear optical and piezoelectric functional materials.
[0052] The present invention provides a method for growing the yttrium strontium phosphate single crystal, which comprises the steps of:
[0053] Mix and sinter the raw materials of Sr-containing compound, Y-containing compound and P-containing compound to synthesize yttrium strontium phosphate polycrystalline material, raise the temperature to melt the yttrium strontium phosphate polycrystalline material, and repeat the cooling, condensation, heating and melting several times to obtain a uniformly melted yttrium strontium phosphate melt;
[0054] According to the chemical formula Sr3Y(PO4)3, the Sr-containing compound, the Y-containing compound and the P-containing compound in the raw materials are mixed according to a stoichiometric ratio, and the P-containing compound is in an excess of 2.5-7.5% by mass;
[0055] Using an iridium rod or a yttrium strontium phosphate single crystal as a seed crystal, the lower end of the seed crystal is just in contact with the yttrium strontium phosphate melt to grow a single crystal by a pulling method, the growth temperature of the single crystal is 1700-1850°C, the pulling speed of the seed crystal is 2-5mm / h during neck growth, reduced to 0.2-2mm / h during shoulder growth, and 0.2-1mm / h during constant diameter growth; when the crystal grows to a desired size, it is pulled up and separated from the melt, and kept at a constant temperature in a temperature field for 0.5-1 hour, and then cooled to room temperature at a rate of 30°C / h or less to obtain a yttrium strontium phosphate single crystal.
[0056] Preferably, the Sr-containing compound, the Y-containing compound and the P-containing compound are independently selected from at least one of the corresponding oxides, carbonates, rinates, halides, nitrates, oxalates and borates, and the compounds containing Sr, Y and P elements cannot be halides at the same time.
[0057] More preferably, the Sr-containing compound is selected from the corresponding oxide, carbonate, halide, sulfate or nitrate compound, the Y-containing compound is selected from the corresponding oxide, nitrate or nitrate salt, and the P-containing compound is selected from the corresponding oxide or phosphate. Most preferably, the Sr-containing compound is SrCO3, the Y-containing compound is Y2O3, and the P-containing compound is NH4H2PO4 or P2O5.
[0058] More preferably, among the raw materials, the Sr-containing compound, the Y-containing compound and the P-containing compound are mixed based on a stoichiometric ratio, and the P-containing compound is in excess by a mass percentage of 3 to 5%.
[0059] According to the present invention, preferably, in preparing the yttrium strontium phosphate polycrystalline material, after the raw materials are mixed, high-temperature sintering is carried out twice to ensure the growth quality of the single crystal. The mixing and sintering of the raw materials should be carried out in the following manner: the weighed raw materials are crushed, uniformly mixed, and sintered once, and the sintering temperature is 800°C.o C~950 o C, the temperature is kept constant for 10-15 hours, CO2, NH3 and H2O are decomposed and removed; then it is cooled down to room temperature, the raw materials for primary sintering are completely crushed, refined, mixed uniformly, pressed into a round cake-like block and sintered twice, the sintering temperature is 1200 o C~1400 o C, the temperature is kept constant for 20 to 40 hours, and the raw materials undergo a solid-state reaction to obtain a yttrium strontium phosphate polycrystalline material. More preferably, the sintering is carried out in a sintering furnace by putting the raw materials into a ceramic crucible.
[0060] According to the present invention, preferably, after the yttrium strontium phosphate polycrystalline material is melted, the cooling, condensation, heating, and melting are repeated 3 to 4 times. The reason for repeating the heating, melting, cooling, and condensation of the polycrystalline material multiple times is to completely expel bubbles generated in the molten liquid, reduce crystal growth defects (bubbles, inclusions, etc.), and improve the quality of the crystal growth. Furthermore, after the yttrium strontium phosphate polycrystalline material is melted and the cooling, condensation, heating, and melting are repeated several times, the molten liquid is then cooled for 10 o C~20 o C Heat and maintain at a constant temperature for 0.5 to 2 hours to melt evenly.
[0061] According to the present invention, preferably, when an iridium crucible is used, in order to prevent oxidation of iridium at high temperatures, it is necessary to grow the single crystal in an inert gas atmosphere such as nitrogen or argon, in which the volume fraction of nitrogen or the inert gas is 90% to 95%.
[0062] The melting point of yttrium strontium phosphate single crystal is higher than that of platinum (1772°C), so when growing yttrium strontium phosphate single crystal for the first time, it is necessary to use iridium, which has a higher melting point, as a seed crystal; after the yttrium strontium phosphate single crystal is obtained, yttrium strontium phosphate can be used as a seed crystal.
[0063] According to the present invention, the crystal growth process includes four steps, namely, neck growth, shoulder growth, constant diameter growth, and separation of the pulled crystal from the melt; preferably, in the neck growth, the pulling speed is 2-5 mm / h, and when the seed crystal diameter is narrowed to 0.5-2.0 mm, the temperature is slowly lowered at a rate of 0.5-5°C / h to grow the shoulder; in the shoulder growth, the pulling speed is lowered to 0.2-2 mm / h, and when the shoulder diameter of the crystal reaches the desired size, the temperature is raised or lowered at a rate of 0.5-5°C / h to grow the constant diameter, and the pulling speed during the constant diameter growth is 0.4-0.7 mm / h, and the rotation speed is 6-8 r / min; when the crystal grows to the desired size, the pulled crystal is separated from the melt.
[0064] More preferably, the method for separating the pulled crystal from the melt is as follows: slowly increase the temperature at a rate of 10 to 50°C / h, and if the lower end of the crystal has a tendency to shrink inward, increase the pulling speed to 5 to 20 mm / h and separate the pulled crystal from the melt.
[0065] According to the present invention, the yttrium strontium phosphate single crystal growth method of the present invention preferably includes an annealing step, the annealing step being as follows: After the yttrium strontium phosphate single crystal growth is completed, the yttrium strontium phosphate single crystal is taken out and placed in a high-temperature muffle furnace for annealing at a temperature of 1200-1400°C for 24-48 hours, so as to completely release the thermal stress generated during the Sr3Y(PO4)3 single crystal growth.
[0066] According to actual needs, the size of the Sr3Y(PO4)3 single crystal grown in the present invention is generally 20-50mm in height and 15-30mm in diameter. It usually takes 4-5 days to grow the Sr3Y(PO4)3 single crystal with this size. Here, the size of the single crystal refers to the normal diameter and total height of the crystal.
[0067] In one preferred embodiment, there is provided a method for growing the yttrium strontium phosphate single crystal, comprising the following steps (1) to (5).
[0068] In step (1) weighing the raw materials, according to the chemical formula of yttrium strontium phosphate Sr3Y(PO4)3, the raw materials SrCO3, Y2O3 and NH4H2PO4 are weighed using a stoichiometric ratio, and further, NH4H2PO4 is weighed in excess of 3 to 7% of the total mass of the phosphate.
[0069] In step (2) of polycrystalline material synthesis, the raw materials weighed in step (1) are uniformly crushed and mixed, then placed in a ceramic crucible and sintered once at a sintering temperature of 800 o C~950 o C, and the temperature is kept constant for 10-15 hours, then cooled to room temperature, the raw materials for the primary sintering are crushed and refined, mixed uniformly, pressed into a round cake-like block, and then placed in a ceramic crucible for secondary sintering, and the sintering temperature is 1200 o C~1400 o C, and keep the temperature constant for 20-40 hours, thus obtaining pure yttrium strontium phosphate polycrystalline material through solid-state reaction;
[0070] In step (3) melting the polycrystalline material, the yttrium strontium phosphate polycrystalline material synthesized in step (2) is placed in an iridium crucible in a single crystal growth furnace, the furnace is evacuated and filled with a protective gas of nitrogen or argon, and the yttrium strontium phosphate polycrystalline material is heated and melted by intermediate frequency induction heating. After the polycrystalline material is completely melted, the temperature is lowered and condensed, and then the temperature is raised again to melt the entire material. This process is repeated several times to remove any bubbles generated in the melt, and then the melt is cooled for 10 oC ~20 oC After heating and keeping the temperature constant for 0.5 to 2 hours, a homogeneously molten yttrium strontium phosphate melt is obtained;
[0071] In step (4) of growing the crystal by the pulling method, an iridium rod or a single crystal of yttrium strontium phosphate is used as a seed crystal, and the seed crystal is placed in the melt of yttrium strontium phosphate obtained in step (3), and the lower end of the seed crystal is vertical and just in contact with the melt to start the growth of the single crystal, and the growth temperature of the single crystal is 1700-1850°C; the crystal growth process includes four steps, namely, neck growth, shoulder growth, constant diameter growth, and separation of the pulled crystal from the melt; the pulling speed during neck growth is 2-5mm / h, and when the diameter of the seed crystal is narrowed to 0.5-2.0mm, the temperature is slowly lowered at a rate of 0.5-5°C / h to grow the shoulder; in shoulder growth, the pulling speed is lowered to 0.2-2mm / h, and when the diameter of the shoulder of the crystal reaches the desired size, the temperature is lowered to 0-5°C / h; The crystal is raised or lowered at a rate of 5 to 30 °C / h to grow the constant diameter section; when the crystal has grown to the desired size, the pulled crystal is separated from the melt. The separated crystal is kept at a constant temperature in the temperature field for 0.5 to 1 hour, and then cooled to room temperature at a rate of 5 to 30 °C / h to obtain yttrium strontium phosphate single crystals.
[0072] In step (5) annealing, the yttrium strontium phosphate single crystal is taken out of the single crystal furnace, and then it needs to be put into a high-temperature muffle furnace for annealing, the annealing temperature is 1200-1400°C, and the annealing time is 24-48 hours.
[0073] According to the present invention, it is further preferred that the pulling speed during the growth of the neck portion is 3 to 5 mm / h and the rotation speed is 8 to 15 r / min, the pulling speed during the growth of the shoulder portion is reduced to 0.3 to 0.8 mm / h and the rotation speed is 6 to 10 r / min, and the pulling speed during the growth of the constant diameter portion is 0.5 to 0.6 mm / h and the rotation speed is 8 r / min.
[0074] According to the present invention, preferably, all of the raw materials are high purity raw materials with a purity of more than 99.9%, and the raw materials required for single crystal growth can be purchased by conventional methods.
[0075] The strontium yttrium phosphate Sr3Y(PO4)3 provided by the present invention is a new type of piezoelectric single crystal, which belongs to the cubic crystal system's ~43m point group, has a non-centrosymmetric structure, excellent mechanical properties, and uniform melting properties. It is also not prone to deliquescence and can be grown into large single crystals in a short time by the pulling method; its non-centrosymmetric structure makes it suitable for use as a non-linear optical crystal or a piezoelectric crystal.
[0076] The present invention provides uses of the Sr3Y(PO4)3 single crystal as follows:
[0077] The present invention provides a method for producing a Sr3Y(PO4)3 single crystal, the method comprising the steps of: (1) providing a nonlinear optical crystal and a piezoelectric crystal; (2) providing a laser host crystal, a nonlinear frequency conversion crystal and a high-temperature piezoelectric crystal;
[0078] According to the present invention, the application of said Sr3Y(PO4)3 single crystal as a nonlinear optical crystal and a piezoelectric crystal is further described in detail as follows.
[0079] 1. In the application of nonlinear optical crystals, the crystal axis of Sr3Y(PO4)3 crystals is aligned using an X-ray alignment device. When the strontium yttrium phosphate single crystal is passed through a 2090 nm laser, a frequency doubling effect is observed, indicating that this single crystal can achieve effective frequency doubling of the 2090 nm wavelength laser. In the process, it is compared with AgGaS2 crystals, as shown in Figure 12.
[0080] 2. In the application as a piezoelectric single crystal, the effective piezoelectric constant of the single crystal is d14 = 6~10PC / N when measured by the impedance method. The effective electromechanical coupling coefficient of the single crystal obtained by measurement and calculation using the impedance analysis method is k14 = 10~30%. Sr3Y(PO4)3 single crystals cut by different methods are cut from room temperature to 1000 oIt is observed that the single crystal still has piezoelectric activity when it is raised to C. As shown in Figure 14, the single crystal shows potential applications in the field of piezoelectricity, especially in the field of high temperature piezoelectricity. The cutting direction of the Sr3Y(PO4)3 single crystal is XZ, XY or ZX, or XZ, XY, ZX, which are the single crystal cutting directions obtained by rotating around X, Y or Z, respectively.
[0081] Furthermore, the present invention provides the application of said Sr3Y(PO4)3 single crystal in nonlinear optical functional devices and piezoelectric devices.Preferably, said nonlinear optical functional devices include laser frequency converters, optical parametric amplifiers, optical parametric oscillators, or Raman frequency converters;preferably, said piezoelectric devices include piezoelectric resonators, oscillators, filters, piezoelectric transducers, piezoelectric pressure sensors, acoustic transducers, or ultrasonic sensors.
[0082] Anything not clearly defined in the above methods can be based on existing technology in this field. Effect of the Invention
[0083] 1. The inventor has found through research that M3RE(PO4)3 piezoelectric single crystal is different from other isomorphous compounds, its uniform melting zone is very narrow, and only by adding phosphate or diphosphorus pentoxide in excess of 1.5-10% of its total mass can the composition deviation caused by the volatilization of diphosphorus pentoxide during single crystal growth be compensated for, high-quality single crystal be obtained, and the technical conditions for high optical quality single crystal be met. In addition, the inventor has found that if the raw materials are mixed using the stoichiometric ratio, single crystal cannot be grown.
[0084] 2. In the method of the present invention, when preparing polycrystalline materials, after mixing the raw materials, high-temperature sintering is carried out twice, the first sintering is carried out at a temperature below the melting point to decompose and remove CO2, NH3 and H2O; then, the second sintering is carried out at the solid-state reaction temperature to prepare high-purity polycrystalline materials and ensure the quality of single crystal growth. Single crystal growth requires seed crystals to be inserted at the complete melting point. In order to obtain high-quality single crystals, the key is to control the pulling speed and rotation speed throughout the entire process of single crystal growth. The present invention can grow large-sized, high-quality photoelectric functional M3RE(PO4)3 single crystals in a short time using the pulling method.
[0085] 3. The new M3RE(PO4)3 piezoelectric single crystal series with photoelectric functionality provided by the present invention has excellent mechanical properties, is not easily deliquesced, and has uniform melting properties. Due to its non-centrosymmetric structure, it is suitable for use as a non-linear optical crystal or piezoelectric crystal. The advantages of its application as a non-linear optical crystal or piezoelectric crystal are that the crystal has a high melting point, no phase transition from room temperature to the melting point, stable chemical properties, and no deliquescing. As a rare compound with a non-centrosymmetric structure and high melting point, it has obvious advantages in the fields of high-temperature piezoelectricity and wide-temperature range non-linear optics. In addition, this single crystal series has a small melt viscosity, is easy to remove impurities during the single crystal growth process, and has a fast growth rate, so that high-quality single crystals can be easily obtained, which is advantageous for subsequent application research and development.
[0086] 4. The inventors accidentally discovered that yttrium strontium phosphate single crystals are different from other isomorphous compounds in that the homogeneous melting zone is very narrow. The present invention creatively adopts a method of adding excess P-containing compounds (phosphate or diphosphorus pentoxide) at 2.5-7.5% of the total mass, which can grow high-quality yttrium strontium phosphate single crystals that meet the technical conditions of high optical quality. Research shows that if raw materials are blended using the traditional stoichiometric ratio, yttrium strontium phosphate single crystals cannot be grown, and if the amount of excess phosphate or diphosphorus pentoxide added is too low, the quality of the obtained yttrium strontium phosphate single crystals does not meet the technical conditions of high optical quality.
[0087] 5. The present invention provides a new type of piezoelectric single crystal, Sr3Y(PO4)3. When applied as a nonlinear optical crystal or piezoelectric crystal, Sr3Y(PO4)3 single crystal has the advantages of having a melting point of over 1800℃, no phase transition from room temperature to the melting point, stable chemical properties, and no deliquescence. As a rare compound with a non-centrosymmetric structure and high melting point, it has significant advantages in the fields of high-temperature piezoelectricity and wide-temperature range nonlinear optics. In addition, this single crystal series has a low melt viscosity, is easy to remove impurities during the single crystal growth process, and has a fast growth rate, so high-quality single crystals can be easily obtained, which is advantageous for subsequent application research and development. [Brief description of the drawings]
[0088] [Figure 1] This is the XRD phase diagram of the M3R(PO4)3 single crystal series. [Diagram 2] This is a photograph of the Ba3Y(PO4)3 single crystal grown in Example 1. [Diagram 3] 1 is a photograph of a Ba3Y(PO4)3 single crystal grown in Example 2. [Figure 4] 1 is a photograph of a Ca3Gd(PO4)3 single crystal grown in Example 3. [Diagram 5] 1 is a transmission spectrum of the Ba3Y(PO4)3 single crystal of Example 1. [Figure 6] 1 is a dielectric spectrum of the Ba3Y(PO4)3 single crystal of Example 1. [Figure 7] 1 is a photograph of Ba3Y(PO4)3 polycrystals grown according to the stoichiometric ratio of Comparative Example 1. [Figure 8] FIG. 1 is a photograph of a low optical quality Ca3Gd(PO4)3 single crystal obtained in Comparative Example 2. [Figure 9] 1 is a photograph of the Sr3Y(PO4)3 single crystal grown in Example 5. [Figure 10] This is an X-ray diffraction spectrum of a single crystal of Sr3Y(PO4)3. [Figure 11] 1 is a photograph of the product obtained by the method of Comparative Example 3. [Figure 12]This is the 2090 nm frequency doubling data of the Sr3Y(PO4)3 single crystal in Example 5. For comparison, AgGaS2 single crystal is used. The horizontal axis is the grain size of the yttrium strontium phosphate single crystal and the AgGaS2 single crystal powder sample, and the vertical axis is the relative intensity. [Figure 13] 13 is a transmission spectrum of the Sr3Y(PO4)3 single crystal of Example 5. [Figure 14] 13 is a dielectric spectrum of the Sr3Y(PO4)3 single crystal in the XY cutting direction of Example 7. [Figure 15] 13 is an impedance phase angle spectrum of the piezoelectric effect of the Sr3Y(PO4)3 single crystal in the ZX cutting direction of Example 9. [Figure 16] This is the Sr3Y(PO4)3 single crystal grown in Comparative Example 4. [Figure 17] 1 is a photograph of a Ba3Yb(PO4)3 single crystal grown in Example 11. [Figure 18] 1 is an X-ray diffraction pattern of the Ba3Yb(PO4)3 single crystal grown in Example 11. [Figure 19] 1 is a dielectric spectrum of the Ba3Yb(PO4)3 single crystal of Example 11. [Figure 20] 1 is a resistivity plot of Ba3Yb(PO4)3 single crystal of Example 11. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0089] Hereinafter, the embodiments of the present invention will be described with reference to the drawings, but the present invention is not limited to the following examples. Among the examples, the purity of the raw materials in Examples 1 to 6 exceeds 99.9%. EXAMPLES
[0090] The method for growing a barium yttrium phosphate single crystal includes the following steps (1) to (5):
[0091] In step (1), BaCO3, Y2O3 and NH4H2PO4 are used as raw materials, and the raw materials are mixed in a stoichiometric ratio according to the chemical formula of barium yttrium phosphate Ba3Y(PO4)3, with the proviso that the phosphate is in excess of 5% of the total mass of ammonium dihydrogen phosphate;
[0092] In step (2), the raw materials prepared in step (1) are mixed uniformly and then placed in an alumina crucible and sintered in a muffle furnace for the first time. The sintering temperature is 850±50°C and the temperature is kept constant for 12 hours to remove CO2, NH3 and H2O from the raw materials; After cooling, the raw materials for the first sintering are crushed and refined, then mixed uniformly again, pressed into a block shape using a cylindrical mold, and then placed in an alumina crucible for solid-state reaction. The sintering temperature is 1350°C and kept constant for 40 hours to obtain the polycrystalline yttrium barium phosphate mentioned above;
[0093] In step (3), the polycrystal of yttrium barium phosphate synthesized in step (2) is placed in an iridium crucible in a single crystal furnace, the furnace is evacuated and filled with nitrogen as a protective gas, the polycrystal is heated and melted by intermediate frequency induction heating, and after the polycrystal material is completely melted, the temperature is lowered to condense it, and then the temperature is raised again to melt it all. This process is repeated three times to remove any bubbles that have formed in the melt. The melt is then cooled for 20 oC After heating and keeping the temperature constant for 0.5 to 2 hours, a uniformly molten yttrium barium phosphate melt is obtained;
[0094] In step (4), a polycrystalline rod of yttrium barium phosphate is used as a seed crystal and slowly dipped into the polycrystalline melt of step (3) so that the top end of the seed crystal is vertical and just in contact with the melt to initiate the growth of a single crystal; The technical conditions for single crystal growth are as follows: temperature is 1850±50°C; the seed crystal pulling speed is 5mm / h during neck growth, and when the diameter of the seed crystal shrinks to about 1mm, the temperature is slowly lowered at a rate of 1-4°C / h to grow the shoulder; the pulling speed during shoulder growth is reduced to 0.5-1mm / h. When the diameter of the crystal shoulder grows to the desired size of about 22mm, the temperature is again raised and lowered at a rate of 1-4°C / h to grow the constant diameter part. The pulling speed during constant diameter growth is 0.5-0.7mm / h. When the crystal grows to the desired size of about 40mm, the temperature is first raised slowly at a rate of 15-20°C / h, and when the lower end of the crystal appears to shrink inward as the temperature increases, the pulling speed is increased to 10-15mm / h to separate the crystal from the melt. The separated crystals were kept at a constant temperature in a temperature field for 45 minutes, and then o C / h to room temperature to obtain barium yttrium phosphate crystals.
[0095] In step (5), the crystal is taken out and then placed in a high-temperature electric resistance furnace to be annealed at a temperature of 1300°C for 24 hours, so that the thermal stress generated during the Ba3Y(PO4)3 crystal growth is completely released.
[0096] As shown in FIG. 2, the Ba3Y(PO4)3 single crystal has high optical quality. EXAMPLES
[0097] The method for growing a barium lanthanum phosphate single crystal includes the following steps (1) to (5):
[0098] In step (1), BaCO3, La2O3 and NH4H2PO4 are used as raw materials, and the raw materials are mixed in a stoichiometric ratio according to the chemical formula of barium lanthanum phosphate Ba3La(PO4)3, and NH4H2PO4 is in excess of 5% of the total mass of the phosphate;
[0099] In step (2), the raw materials prepared in step (1) are mixed uniformly, then placed in an alumina crucible and sintered in a muffle furnace at a sintering temperature of 900o C and keep the temperature constant for 10 hours to decompose and remove CO2, H2O and NH3; After cooling, the primary sintering raw materials are crushed and refined, then mixed uniformly again, pressed into a block shape, and placed in an alumina ceramic crucible for solid-state reaction. The sintering temperature is 1400°C and kept constant for 30 hours to obtain the polycrystalline lanthanum barium phosphate mentioned above;
[0100] In step (3), the polycrystal of lanthanum barium phosphate synthesized in step (2) is placed in an iridium crucible in a single crystal furnace, the furnace is evacuated, and nitrogen is filled as a protective gas to prevent oxidation of the iridium crucible. The polycrystal is heated and melted by intermediate frequency induction heating, and after the polycrystal material is completely melted, the temperature is lowered and condensed, and then the temperature is raised again to melt it all. This process is repeated 2 to 4 times to remove any bubbles that have formed in the melt. The melt is then cooled for 15 minutes. o C and keep at a constant temperature for 1 hour to obtain a homogeneously molten lanthanum barium phosphate melt;
[0101] In step (4), an iridium rod is used as a seed crystal and slowly dipped into the polycrystalline melt of step (3) so that the top end of the seed crystal is vertical and just in contact with the melt to initiate the growth of a single crystal; The technical conditions for single crystal growth are as follows: temperature is 1850±50°C; the seed crystal pulling speed is 6mm / h during neck growth, and when the diameter of the seed crystal shrinks to about 1.5mm, the temperature is slowly lowered at a rate of 5°C / h to grow the shoulder; the pulling speed during shoulder growth is reduced to 0.3mm / h. When the diameter of the crystal shoulder grows to the desired size of about 30mm, the temperature is again raised and lowered at a rate of 0-5°C / h to grow the constant diameter part. The pulling speed during constant diameter growth is 0.6mm / h. When the crystal grows to the desired size of about 50mm, the temperature is first raised slowly at a rate of 20°C / h, and when the lower end of the crystal appears to shrink inward as the temperature increases, the pulling speed is increased to 15mm / h to separate the crystal from the melt.
[0102] In step (5), the separated crystal is kept at a constant temperature in a temperature field for 1 hour, and then o C / h to room temperature to obtain barium lanthanum phosphate single crystal. As shown in Figure 3, the Ba3La(PO4)3 single crystal has high optical quality.
[0103] The annealing treatment of the crystal was the same as in Example 1. EXAMPLES
[0104] The method for growing calcium gadolinium phosphate single crystals includes the following steps (1) to (4):
[0105] In step (1), CaCO3, Gd2O3 and NH4H2PO4 are used as raw materials, and the raw materials are mixed in a stoichiometric ratio according to the chemical formula of calcium gadolinium phosphate, Ca3Gd(PO4)3, with the proviso that the phosphate is in excess of 3.5% of the total mass of ammonium dihydrogen phosphate;
[0106] In step (2), the raw materials prepared in step (1) are mixed uniformly and then placed in an alumina crucible and subjected to primary sintering in a muffle furnace. The sintering temperature is 900°C and the temperature is kept constant for 13 hours to remove CO2, H2O and NH3; After cooling, the primary sintering raw materials are crushed and refined, then mixed uniformly again, pressed into a block shape using a cylindrical mold, and then placed in an alumina crucible for solid-state reaction. The sintering temperature is 1350°C and kept constant for 30 hours to obtain the above-mentioned gadolinium calcium phosphate polycrystal;
[0107] In step (3), the gadolinium calcium phosphate polycrystal synthesized in step (2) is placed in an iridium crucible in a single crystal furnace, the furnace is evacuated and filled with nitrogen as a protective gas, the polycrystal is heated and melted by intermediate frequency induction heating, and after the polycrystal material is completely melted, the temperature is lowered to condense it, and then the temperature is raised again to melt it all. This process is repeated three times to remove any bubbles that have formed in the melt. The melt is then cooled for 20 oC and keep at a constant temperature for 0.5 hours to obtain a homogeneously molten calcium gadolinium phosphate melt;
[0108] In step (4), an iridium rod is used as a seed crystal and slowly dipped into the polycrystalline melt of step (3) so that the top end of the seed crystal is vertical and just in contact with the melt to initiate the growth of a single crystal; The technical conditions for single crystal growth are as follows: temperature is 1850±50°C; the seed crystal pulling speed is 5mm / h during neck growth, and when the diameter of the seed crystal shrinks to about 1mm, the temperature is slowly lowered at a rate of 3°C / h to grow the shoulder; the pulling speed during shoulder growth is reduced to 0.3-1mm / h. When the diameter of the crystal shoulder grows to the desired size of about 15-25mm, the temperature is again raised and lowered at a rate of 1-4°C / h to grow the constant diameter part. The pulling speed during constant diameter growth is 0.5mm / h. When the crystal grows to the desired size of about 30-50mm, the temperature is first raised slowly at a rate of 25°C / h, and when the lower end of the crystal appears to shrink inward as the temperature increases, the pulling speed is increased to 15-20mm / h to separate the crystal from the melt. The separated crystals were kept at a constant temperature in a temperature field for 45 minutes, and then o C / h to room temperature to obtain calcium gadolinium phosphate crystals. As shown in Figure 4, the Ca3Gd(PO4)3 single crystals have high optical quality.
[0109] The annealing treatment of the crystal was the same as in Example 1. EXAMPLES
[0110] The method for growing a lanthanum strontium phosphate single crystal includes the following steps (1) to (4).
[0111] In step (1), SrCO3, La2O3 and NH4H2PO4 are used as raw materials, and the raw materials are mixed in a stoichiometric ratio according to the chemical formula of lanthanum strontium phosphate Sr3La(PO4)3, with the proviso that the phosphate is in excess of 3% of the total mass of ammonium dihydrogen phosphate;
[0112] In step (2), the raw materials prepared in step (1) are mixed uniformly, then placed in an alumina crucible and sintered in a muffle furnace at a sintering temperature of 850 o C and keep the temperature constant for 15 hours to remove CO2, H2O and NH3; After cooling, the raw materials for the first sintering are crushed and refined, then mixed uniformly again, pressed into a block shape using a cylindrical mold, and placed in an alumina crucible for solid-state reaction. The sintering temperature is kept constant at 1300-1400°C for 20-30 hours to obtain the above-mentioned lanthanum strontium phosphate polycrystals;
[0113] In step (3), the lanthanum strontium phosphate polycrystal synthesized in step (2) is placed in an iridium crucible in a single crystal furnace, the furnace is evacuated and filled with nitrogen as a protective gas, and the polycrystal is heated and melted by intermediate frequency induction heating. After the polycrystal is completely melted, the temperature is lowered to condense it, and then the temperature is raised again to melt it completely. This process is repeated three times to remove any bubbles that have formed in the melt. The melt is then cooled for 20 o C After heating and keeping the temperature constant for 0.5 hours, a homogeneous melt of lanthanum strontium phosphate is obtained;
[0114] In step (4), an iridium rod is used as a seed crystal and slowly dipped into the polycrystalline melt of step (3) so that the top end of the seed crystal is vertical and just in contact with the melt to initiate the growth of a single crystal; The technical conditions for single crystal growth are as follows: the temperature is 1800-1900°C; the seed crystal pulling speed is 6mm / h during neck growth, and when the diameter of the seed crystal shrinks to about 1mm, the temperature is slowly lowered at a rate of 1-3°C / h to grow the shoulder; the pulling speed during shoulder growth is reduced to 0.4mm / h. When the diameter of the crystal shoulder grows to the desired size of 15-25mm, the temperature is again raised and lowered at a rate of 1-4°C / h to grow the constant diameter part. The pulling speed during constant diameter growth is 0.6mm / h. When the crystal grows to the desired size of 20-35mm, the temperature is first raised slowly at a rate of 20°C / h, and when the lower end of the crystal appears to shrink inward as the temperature increases, the pulling speed is increased to 10-15mm / h to separate the crystal from the melt. The separated crystals were kept at a constant temperature in a temperature field for 45 minutes, and then o C / h to room temperature to obtain lanthanum strontium phosphate single crystals.
[0115] The annealing treatment of the crystal was the same as in Example 1.
[0116] Comparative Example 1 This is a method for growing yttrium barium phosphate single crystals by mixing in a stoichiometric ratio. The same as in Example 1 above, except that in step (1), BaCO3, Y2O3 and NH4H2PO4 are used as raw materials for crystal growth, and are mixed in a stoichiometric ratio according to the chemical formula of barium yttrium phosphate Ba3Y(PO4)3, and NH4H2PO4 is not excessive. The results show that after the barium yttrium phosphate raw material is melted, composition deviation and stratification occur, and when the seed crystal is pulled up, it does not grow into a Ba3Y(PO4)3 single crystal. The product is Ba3Y(PO4)3 polycrystal, as shown in Figure 7.
[0117] Comparative Example 2 This is a method for growing calcium gadolinium phosphate single crystals using a 0.5% excess of NH4H2PO4. The method is the same as in Example 3 above, except that in step (1), the raw materials CaCO3, Gd2O3 and NH4H2PO4 are mixed in a stoichiometric ratio according to the chemical formula Ca3Gd(PO4)3, and NH4H2PO4 is in excess by mass percentage of 0.5%. The resulting single crystal has poor quality, as shown in Figure 8. Research has shown that in this example, the phosphate is only 0.5% excess, which cannot compensate for the composition deviation caused by the volatilization of phosphorus during the growth of the single crystal, resulting in low crystallinity of calcium gadolinium phosphate single crystal. EXAMPLES
[0118] The method for growing an yttrium strontium phosphate single crystal includes the following steps (1) to (5):
[0119] In step (1), SrCO3, Y2O3 and NH4H2PO4 are used as raw materials for crystal growth, and are mixed in a stoichiometric ratio according to the chemical formula of yttrium strontium phosphate Sr3Y(PO4)3, and NH4H2PO4 is in excess of 3% of the total mass of the phosphate;
[0120] In step (2), the raw materials prepared in step (1) are mixed uniformly and then placed in an alumina crucible for primary sintering. The sintering temperature is 900°C and the temperature is kept constant for 10 hours to decompose and remove CO2, H2O and NH3; After cooling, the raw materials for primary sintering are crushed and refined, then mixed uniformly again, pressed into a block shape, and subjected to solid-state reaction in an alumina ceramic crucible. The sintering temperature is 1250°C, and the temperature is kept constant for 48 hours to obtain the polycrystalline yttrium strontium phosphate;
[0121] In step (3), the polycrystal of yttrium strontium phosphate obtained in step (2) is placed in an iridium crucible in a single crystal furnace, the furnace is evacuated and nitrogen is filled as protective gas to prevent oxidation of the iridium crucible, the polycrystal is heated and melted by intermediate frequency induction heating, and after the polycrystal is completely melted, the temperature is lowered to condense, and then the temperature is raised again to melt it completely, and this is repeated three times to remove bubbles generated in the melt. Then, the melt is heated to about 20°C and kept at a constant temperature for 1 hour to obtain a uniformly melted yttrium strontium phosphate melt;
[0122] In step (4), use an iridium rod as a seed crystal and slowly dip it into the polycrystalline melt of step (3) so that the top end of the seed crystal is vertical and just in contact with the melt to initiate the growth of a single crystal; The technical conditions for single crystal growth are as follows: the growth temperature is 1800°C; the pulling speed during the growth of the neck part of the seed crystal is 3-3.5mm / h, and the rotation speed is 8-15r / min; when the seed crystal diameter is narrowed to 1mm, the temperature is slowly lowered at a rate of 0.5°C / h to grow the shoulder part; the pulling speed during the growth of the shoulder part is lowered to 0.3-0.4mm / h, and the rotation speed is 6-8r / min; when the diameter of the crystal shoulder reaches the desired size of 20mm, the temperature is raised and lowered again at a rate of 0.3°C / h to grow the constant diameter part; the pulling speed during the growth of the constant diameter part is 0.5mm / h, and the rotation speed is 8r / min. When the crystal grows to a height of about 36mm, the temperature is raised at a rate of 20°C / h, and when the lower end of the crystal appears to shrink inward with the rise in temperature, the pulling speed is increased to 5mm / h to separate the crystal from the melt. The separated crystal is kept at a constant temperature in a temperature field for 1 hour, and then cooled to room temperature at a rate of 10° C. / h to obtain a single crystal of yttrium strontium phosphate.
[0123] In step (5), the crystal is taken out and then placed in a high-temperature electric resistance furnace for annealing at a temperature of 1300°C for 24 hours, which completely releases the thermal stress generated during the growth of the Sr3Y(PO4)3 single crystal.
[0124] An actual photograph of the obtained Sr3Y(PO4)3 single crystal is shown in Figure 9. The X-ray diffraction spectrum of the obtained Sr3Y(PO4)3 single crystal shows characteristic peaks at 2θ = 27.88°, 33.13°, and 45.74°, as shown in Figure 10.
[0125] The frequency doubling effect of the obtained Sr3Y(PO4)3 single crystal was observed when 2090 nm light was passed through it, indicating that the single crystal can realize effective frequency doubling of the 2090 nm wavelength laser. As shown in Figure 12, when compared with AgGaS2 single crystal, it shows that the Sr3Y(PO4)3 single crystal can realize effective frequency doubling in the infrared band.
[0126] The transmission spectrum of the Sr3Y(PO4)3 single crystal is shown in Figure 13. In the band of 480nm~4100nm, the transmittance is more than 80%, indicating that the optical uniformity of the grown single crystal is good and the absorption cut-off edge is less than 180nm, indicating the potential application of the single crystal in the deep ultraviolet band. EXAMPLES
[0127] The method for growing a gadolinium strontium phosphate single crystal includes the following steps (1) to (5).
[0128] In step (1), SrCO3, Gd2O3 and P2O5 are used as crystal growth raw materials, which are mixed in a stoichiometric ratio according to the chemical formula of strontium gadolinium phosphate Sr3Gd(PO4)3, and P2O5 is in excess of 5% of the total mass;
[0129] In step (2), the raw materials prepared in step (1) are mixed uniformly, then placed in an alumina crucible and subjected to primary sintering at a sintering temperature of 900 o C and keep at a constant temperature for 15 hours to decompose and remove CO2 and H2O; The temperature is lowered, the primary sintered raw materials are crushed and refined, then mixed uniformly again, pressed into a block shape, and placed in an alumina ceramic crucible for solid-state reaction. The sintering temperature is 1300 oC and maintaining the temperature at a constant level for 48 hours to obtain the gadolinium strontium phosphate polycrystals;
[0130] In step (3), the gadolinium strontium phosphate polycrystal obtained in step (2) is placed in an iridium crucible in a single crystal furnace, the furnace is evacuated, and nitrogen is filled as protective gas to prevent oxidation of the iridium crucible. The polycrystal is heated and melted by intermediate frequency induction heating. After the polycrystal is completely melted, it is cooled and condensed, and then heated again to melt it completely. This process is repeated three times to remove bubbles generated in the melt. The melt is then heated to about 20°C and kept at a constant temperature for 1 hour to obtain a uniformly melted gadolinium strontium phosphate melt;
[0131] In step (4), a yttrium strontium phosphate single crystal is used as a seed crystal and slowly immersed in the polycrystalline melt from step (3) so that the top end of the seed crystal is vertical and just in contact with the melt to initiate the growth of the single crystal; The technical conditions for single crystal growth are as follows: the growth temperature is 1800°C; the pulling speed during the seed crystal neck growth is 4-4.5mm / h, and the rotation speed is 8-15r / min; when the seed crystal diameter shrinks to 1mm, the temperature is slowly lowered at a rate of 0.8°C / h to grow the shoulder; the pulling speed during the shoulder growth is lowered to 0.4-0.5mm / h, and the rotation speed is 6-8r / min; when the diameter of the crystal shoulder reaches the desired size of 20mm, the temperature is again raised and lowered at a rate of 0.2°C / h to grow the constant diameter part; the pulling speed during the constant diameter part growth is 0.6mm / h, and the rotation speed is 8r / min. When the crystal grows to a height of 30mm, the temperature is raised at a rate of 20°C / h, and when the lower end of the crystal appears to shrink inward with the temperature increase, the pulling speed is increased to 6mm / h to separate the crystal from the melt. The separated crystal is kept at a constant temperature in a temperature field for 1 hour, and then cooled to room temperature at a rate of 15°C / h to obtain a gadolinium strontium phosphate single crystal.
[0132] In step (5), the single crystal is taken out and then placed in a high-temperature electric resistance furnace at a temperature of 1300 oC, and the annealing time is 24 h, so that the thermal stress generated during the growth of Sr3Gd(PO4)3 single crystal is completely released.
[0133] The obtained Sr3Gd(PO4)3 single crystal has a diameter of 20 mm and a height of 30 mm; a frequency doubling effect is observed when 2090 nm light passes through it. Tests show that the single crystal has a transmittance of over 80% in the 480 nm to 4100 nm band, and has high optical uniformity.
[0134] Comparative Example 3 The same as in Example 5 above, except that in step (1), the raw materials SrCO3, Y2O3 and NH4H2PO4 are mixed in a stoichiometric ratio according to the chemical formula Sr3Y(PO4)3, and NH4H2PO4 is not in excess. The results show that after the yttrium strontium phosphate raw material is melted, composition deviation and stratification occur, and the seed crystal cannot be pulled up to grow into a Sr3Y(PO4)3 single crystal. The actual product is shown in Figure 3, which is a polycrystalline Sr3Y(PO4)3.
[0135] Comparative Example 4 The procedure is the same as in Example 5 above, except that in step (1), the raw materials SrCO3, Y2O3 and NH4H2PO4 are mixed in a stoichiometric ratio according to the chemical formula Sr3Y(PO4)3, and NH4H2PO4 is in excess of 0.5%.
[0136] The resulting single crystals are of poor quality and irregular in shape, as shown in Figure 8. Research has shown that in this example, the phosphate in excess of only 0.5% cannot compensate for the composition deviation caused by the phosphorus volatilization during the growth of the single crystal, resulting in low crystallinity of the yttrium strontium phosphate single crystal. EXAMPLES
[0137] The Sr3Y(PO4)3 single crystal grown in Example 5 is oriented based on the physical piezoelectric axis, and then the crystal plate is machined along the X and Y directions of the physical axis with the X direction as the thickness, the Y direction as the length, and the Z direction as the width. The dimensions of the crystal plate are thickness x width x length = 1.2 mm x 3.5 mm x 10.0 mm, and the crystal surface in the thickness direction is plated with a conductive electrode. When the crystal plate sample is tested with an impedance analyzer, piezoelectric resonance and anti-resonance peaks are detected, indicating that the single crystal has a piezoelectric effect in the cutting direction. In particular, even when the temperature is increased to 1000°C, the piezoelectric resonance and anti-resonance peaks are still observed, indicating that the single crystal can be applied as a high-temperature piezoelectric crystal. Please refer to Figure 14. EXAMPLES
[0138] The Sr3Y(PO4)3 single crystal grown in Example 6 is oriented based on the physical piezoelectric axis, and then processed into a crystal plate along the X and Y directions of the physical axis, with the X direction being the thickness, the Y direction being the length, and the Z direction being the width. The dimensions of the crystal plate are thickness x width x length = (0.5-1.5) mm x (3.0-4.0) mm x (8.0-12.0) mm, and a conductive electrode is plated on the crystal surface in the thickness direction.
[0139] When the crystal plate sample is tested with an impedance analyzer, the piezoelectric resonance and anti-resonance peaks are detected, indicating that the single crystal has a piezoelectric effect in the cutting direction. Similar to Example 5, when the temperature is increased to 1000°C, the piezoelectric resonance and anti-resonance peaks are still observed, indicating that the single crystal can be applied as a high-temperature piezoelectric crystal. The resonant and anti-resonant frequencies of the sample appear at 881.8kHz and 887.8kHz, respectively. EXAMPLES
[0140] The Sr3Y(PO4)3 single crystal grown in Example 5 is oriented based on the physical piezoelectric axis, and then the crystal plate is processed along the X and Y directions of the physical axis, with the Z direction being the thickness, the X direction being the length, and the Y direction being the width. The dimensions of the crystal plate are thickness x width x length = 1.0 mm x 3.5 mm x 10.0 mm, and a conductive electrode is plated on the crystal surface in the thickness direction.
[0141] When the crystal plate sample is tested with an impedance analyzer, the piezoelectric resonance and anti-resonance peaks are detected, indicating that the single crystal has a piezoelectric effect in the cutting direction. Even when the temperature is increased to 1000℃, the single crystal still has piezoelectric activity, which shows that it can be used as a high-temperature piezoelectric single crystal. The piezoelectric activity of Sr3Y(PO4)3 single crystal does not change regardless of the cutting direction when the temperature is increased from room temperature to 1000℃. The impedance analysis diagram is shown in Figure 15. EXAMPLES
[0142] The Sr3Y(PO4)3 single crystal grown in Example 6 was oriented based on the physical piezoelectric axes X, Y, and Z, and then rotated by θ degrees (θ=0 to 180°) along the X, Y, and Z axes. o ) to process it into Sr3Y(PO4)3 single crystals with different cutting directions. Next, the crystal plate is processed with reference to Example 5. The dimensions of the crystal plate are thickness x width x length = (0.5-1.5) mm x (3.0-4.0) mm x (8.0-12.0) mm, and the crystal face in the thickness direction is plated with a conductive electrode.
[0143] When the above Sr3Y(PO4)3 single crystal plate samples with different cutting directions are tested with an impedance analyzer, piezoelectric resonance and anti-resonance peaks are detected in all samples, indicating that this single crystal has a piezoelectric effect in all directions in space. The piezoelectric activity of the single crystal does not change even at a temperature of 1000℃ regardless of the cutting direction, so it can be used as a high-temperature piezoelectric crystal. EXAMPLES
[0144] The method for growing a barium ytterbium phosphate single crystal includes the following steps (1) to (5):
[0145] In step (1), BaCO3, Yb2O3 and NH4H2PO4 are used as crystal growth materials, which are mixed in a stoichiometric ratio according to the chemical formula of barium ytterbium phosphate Ba3Yb(PO4)3, and NH4H2PO4 is in excess of 5% of the total mass of the phosphate;
[0146] In step (2), the raw materials prepared in step (1) are mixed uniformly and then placed in an alumina crucible for primary sintering. The sintering temperature is 900°C and kept constant for 10 hours to decompose and remove CO2, H2O and NH3; The temperature is lowered, the primary sintered raw material is crushed, refined, mixed uniformly again, pressed into a block shape, and subjected to solid-state reaction in an alumina ceramic crucible. The sintering temperature is 1250°C and kept at a constant temperature for 48 hours to obtain the above-mentioned barium ytterbium phosphate polycrystal;
[0147] In step (3), the barium ytterbium phosphate polycrystal obtained in step (2) is placed in an iridium crucible in a single crystal furnace, the furnace is evacuated, and nitrogen is filled as protective gas to prevent the iridium crucible from oxidizing. The polycrystal is heated and melted by intermediate frequency induction heating. After the polycrystal is completely melted, the temperature is lowered to condense it, and then the temperature is raised again to melt it completely. This is repeated three times to remove bubbles generated in the melt. Then, the melt is heated to about 20°C and kept at a constant temperature for 1 hour to obtain a uniformly melted barium ytterbium phosphate melt;
[0148] In step (4), use an iridium rod as a seed crystal and slowly dip it into the polycrystalline melt obtained in step (3) so that the top end of the seed crystal is vertical and just in contact with the melt, thereby initiating the growth of a single crystal; The technical conditions for single crystal growth are as follows: the growth temperature is 1800°C; the pulling speed during the seed crystal neck growth is 1-3.5mm / h, and the rotation speed is 6-12r / min; when the seed crystal diameter shrinks to 1mm, the temperature is slowly lowered at a rate of 0.5°C / h to grow the shoulder; during the shoulder growth, the pulling speed is lowered to 0.3-0.5mm / h, and the rotation speed is 6-8r / min; when the diameter of the crystal shoulder grows to the desired size of 15mm, the temperature is again raised and lowered at a rate of 0.3°C / h to grow the constant diameter section; the pulling speed during the constant diameter section growth is 0.5mm / h, and the rotation speed is 5r / min. When the crystal grows to a height of about 30mm, the temperature is raised at a rate of 15°C / h, and when the lower end of the crystal appears to shrink inward with the temperature rise, the crystal is pulled up at a rate of 5mm / h to separate it from the melt. The separated crystal is kept at a constant temperature in a temperature field for 1 hour, and then cooled to room temperature at a rate of 10 to 30°C / h to obtain a barium ytterbium phosphate single crystal.
[0149] In step (5), after the single crystal is taken out, it is annealed in a high-temperature electric resistance furnace at a temperature of 1300°C, and the annealing time is 48 hours, so that the thermal stress generated during the growth of Ba3Yb(PO4)3 single crystal is completely released.
[0150] An actual photograph of the obtained Ba3Yb(PO4)3 single crystal is shown in Figure 17. The X-ray diffraction spectrum of the obtained Ba3Yb(PO4)3 single crystal shows characteristic peaks at 2θ = 26.93°, 31.99°, and 44.10°, as shown in Figure 18.
[0151] The dielectric spectrum and resistivity characteristics of the Ba3Yb(PO4)3 single crystal are shown in Figures 19 and 20. The dielectric loss is low (<1.1) at 900℃, and the resistivity is high (ρ>107 (Ohm·cm)), indicating the possibility of application in the high temperature piezoelectric field.
Claims
1. General formula M 3 RE (PO 4 ) 3 (wherein M represents an alkaline earth metal and RE represents a rare earth element), has a non-centrosymmetric structure, is in the cubic crystal system and belongs to the 43m point group; the rare earth element is Y, La, Gd or Yb; The alkaline earth metal is Ba, Ca or Sr; Light transmittance in the 325nm to 4302nm band exceeds 70% A piezoelectric single crystal characterized by:
2. The above M 3 RE (PO 4 ) 3 The piezoelectric single crystal is Ba 3 Y (PO 4 ) 3 Single crystal, Ba3La(PO 4 ) 3 Single crystal, Ba 3 Yb(PO 4 ) 3 Single crystal, Ca 3 Gd(PO 4 ) 3 Single crystal, Sr 3 Y (PO 4 ) 3 Single crystal, Sr 3 La (PO 4 ) 3 Single crystal, Sr 3 Gd(PO 4 ) 3 It is one of the single crystals The piezoelectric single crystal according to claim 1 .
3. The structural parameters of each of the piezoelectric single crystals are: Ba 3 Y (PO 4 ) 3 Single crystal: cubic system ~ 43m point group; space group I ~ 43d; lattice constant a = b = c = 10.4655 Å, density = 4.553 g / cm 3 ; Ba3La(PO 4 ) 3Single crystal: cubic system ~43m point group; space group I~43d; lattice constant a = b = c = 10.521 Å, density = 4.77 g / cm 3 ; Ba 3 Yb(PO 4 ) 3 Single crystal: cubic system ~43m point group; space group I~43d; lattice constant a = b = c = 10.459 Å, density = 5.149 g / cm 3 ; Ca 3 Gd(PO 4 ) 3 Single crystal: cubic system ~43m point group; space group I~43d; lattice constant a = b = c = 9.857 Å, density = 3.9 g / cm 3 ; Sr 3 Y (PO 4 ) 3 Single crystal: cubic system ~43m point group; space group I~43d; lattice constant a = b = c = 10.0814 Å, density = 4.093 g / cm 3 ; Sr 3 La (PO 4 ) 3 Single crystal: cubic system ~43m point group; space group I~43d; lattice constant a = b = c = 10.192 Å, density = 4.3 g / cm 3 ; Sr 3 Gd(PO 4 ) 3 Single crystal: cubic system ~43m point group; space group I~43d; lattice constant a = b = c = 10.114 Å, density = 4.526 g / cm 3 is The piezoelectric single crystal according to claim 2 .
4. Chemical formula Sr 3 Y (PO 4 ) 3 In a yttrium strontium phosphate single crystal having It has a non-centrosymmetric structure, is a cubic crystal system, belongs to the 43m point group, has lattice constants a = 10.0814 Å, b = 10.0814 Å, c = 10.0814 Å, α = β = γ = 90°, and does not have a phase transition from room temperature to the melting point.
1. A yttrium strontium phosphate single crystal comprising: