OVD forming medium and its manufacturing method
The use of two-dimensional material particles in an OVD forming medium addresses the challenges of vacuum-based processes by providing a cost-effective, precise, and durable optical functional layer with controlled thickness and versatile visual effects.
Patent Information
- Application Number
- JP2021019983
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-10
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-02-10
AI Technical Summary
Existing OVD forming media require expensive vacuum processes and equipment, leading to potential deformation of base materials and material loss, with challenges in controlling metal layer thickness and quality variations.
A base material with a relief structure and an optical functional layer containing particles of a two-dimensional material, such as MXene, is formed using a simple process that does not require vacuum deposition, allowing for precise control of layer thickness and functionality.
The OVD forming medium achieves optical functions like light reflection and transmission with high precision and durability, avoiding the need for expensive equipment and reducing material waste, while enabling various visual effects based on viewing conditions.
Smart Images

Figure 0007590204000004 
Figure 0007590204000005 
Figure 0007590204000006
Abstract
Description
[Technical field]
[0001] The present invention relates to an OVD forming medium and a method for making the same. The present invention also relates to articles comprising the OVD forming medium. [Background technology]
[0002] An OVD (Optical Variable Device) is a device that can exhibit optical changes that can be recognized by the naked eye and / or other suitable means. OVDs are used as security technologies to prevent counterfeiting and imitation, and are also used for a variety of purposes due to their high design and decorative properties.
[0003] There are various types of media on which OVDs are formed (referred to as "OVD-formed media" in this specification). Conventionally, as an example of a surface relief type OVD-formed medium, there is known one having a transparent base material having a relief structure on its surface and a light reflecting layer covering a part of the relief structure (see, for example, Patent Documents 1 and 2). Such an OVD-formed medium covers a part of the relief structure with a light reflecting layer and allows light to pass through the remaining part of the relief structure, so that it can present different visual effects depending on the viewing conditions. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2008-107483 A [Patent Document 2] International Publication No. 2010 / 049676 Summary of the Invention [Problem to be solved by the invention]
[0005] In the OVD forming medium of Patent Document 1, a metal layer formed by vacuum deposition or sputtering is used as a light reflecting layer. When forming a metal layer by such a method, there is a drawback that vacuum deposition or sputtering requires a vacuum process, and a complicated process must be carried out using expensive equipment for vacuum deposition or sputtering. In particular, in the case of vacuum deposition, there is a risk that the substrate may be deformed by heat.
[0006] More specifically, Patent Document 1 discloses two methods for forming a metal layer as a light-reflecting layer that covers a part of a relief structure. In the first method, a metal is vacuum-deposited on a region of a substrate facing a metal source while the substrate is inclined with respect to the metal source, thereby forming a metal layer (see FIG. 18 of Patent Document 1). In the second method, a mask member having an opening slit is used, and a metal is vacuum-deposited on a region of the substrate corresponding to the opening slit through the mask member, thereby forming a metal layer (see FIG. 19 of Patent Document 1). In the first method, since the metal source is usually fixed, when a metal layer is formed on a substrate with a large area, the distance and angle from the metal source to the deposition position are different, which may cause quality variations in the metal layer, and further, the vacuum volume needs to be increased, which leads to a problem of an increase in the size of the device. The second method has the problem that the metal adhering to the mask member is discarded, resulting in material loss (increasing material prices and causing a large environmental burden). Furthermore, it is necessary to fabricate a mask member with a specified opening slit and align the mask member with the substrate, which results in a further increase in equipment costs.
[0007] On the other hand, in the OVD forming medium of Patent Document 2, a metal layer as a light reflecting layer that covers a part of the relief structure is formed by printing in a pattern form. More specifically, in Patent Document 2, a metal layer is formed by printing an ink containing flake- or plate-shaped metal particles and a binder in the form of a pattern on a transparent high refractive index layer. Patent Document 2 describes that the thickness (plate thickness) of the flake- or plate-shaped metal particles is in the range of 10 nm to 100 nm, but for application to holographic or diffractive structures, the preferred thickness is in the range of 15 nm to 100 nm, and specifically, aluminum flakes with a thickness of 25 nm are described. However, it is actually extremely difficult to obtain metal particles in a controlled sheet shape with a thickness of, for example, 20 nm or less, especially less than 10 nm.
[0008] Also, Patent Document 2 describes that the metal ink layer can be opaque or translucent depending on whether the information underneath is visible or not, but does not disclose a specific configuration for achieving this. Patent Document 2 discloses controlling the thickness of the transparent high refractive index layer below the metal layer, but does not disclose controlling the thickness of the metal layer. As described in Patent Document 2, when the metal layer is formed by printing an ink containing metal particles such as flake-shaped or plate-shaped particles and a binder, it is difficult to strictly control the thickness of the metal layer.
[0009] The present inventors have sought to move away from the use of metal layers and realize an entirely new OVD forming medium having optically functional layers that are not limited to only light reflecting layers.
[0010] An object of the present invention is to provide an OVD forming medium having an optically functional layer that can be formed with a strictly controlled thickness by a simple process without requiring expensive equipment. [Means for solving the problem]
[0011] As a result of extensive research, the present inventors independently discovered that a layer containing particles of a two-dimensional material can exhibit optical functions, and thus completed the present invention.
[0012] According to one aspect of the present invention, A substrate having a relief structure on a surface thereof; an optical functional layer covering the relief structure; wherein the optically functional layer comprises particles of a two-dimensional material.
[0013] In one embodiment of the invention, said two-dimensional material is a layered material comprising one or more layers, said one or more layers having the following formula: M m X n (wherein M is at least one Group 3, 4, 5, 6, or 7 metal; X is a carbon atom, a nitrogen atom, or a combination thereof; n is 1 to 4, m is greater than n and less than or equal to 5) and a modification or termination T (T is at least one selected from the group consisting of a hydroxyl group, a fluorine atom, a chlorine atom and an oxygen atom) present on the surface of the layer body.
[0014] In one embodiment of the present invention, the content of the particles of the two-dimensional material in the optical functional layer may be 50% by volume or more.
[0015] In one embodiment of the present invention, the optically functional layer may have a thickness of 3 μm or less.
[0016] In one embodiment of the present invention, the optical functional layer can function as a light reflecting layer or a light transmitting layer either constantly or depending on the viewing conditions.
[0017] In one embodiment of the present invention, the optical functional layer may include a first portion and a second portion, and the thickness of the second portion may be smaller than the thickness of the first portion.
[0018] According to another aspect of the invention, there is provided an article comprising the OVD forming medium of the invention.
[0019] According to yet another aspect of the present invention, 1. A method for producing an OVD forming medium, comprising: (a) providing a substrate having a relief structure thereon; (b) applying a liquid comprising particles of a two-dimensional material and a liquid medium onto the relief structure to form an optically functional layer covering the relief structure and comprising particles of the two-dimensional material; A method of manufacture is provided, comprising:
[0020] In one embodiment of the present invention, the (b) is (b1) applying the liquid material onto the relief structure by spraying the liquid material onto the substrate to form a precursor of the optical functional layer; and (b2) drying the precursor. may include.
[0021] In one embodiment of the present invention, in (b1), the liquid material may be sprayed in a discharge direction at an angle of less than 90 degrees to the substrate.
[0022] In one embodiment of the invention, the angle may be less than or equal to 45 degrees. Effect of the Invention
[0023] The OVD forming medium of the present invention includes a substrate having a relief structure on its surface and an optical functional layer covering the relief structure, the optical functional layer including particles of a two-dimensional material. Although not limiting the present invention, the optical functional layer can be formed by applying a liquid including particles of a two-dimensional material and a liquid medium onto the relief structure, and the thickness of the optical functional layer can be strictly controlled depending on the application conditions. Thus, according to the present invention, an OVD forming medium having an optical functional layer that can be formed with a strictly controlled thickness by a simple process without requiring expensive equipment, an article including such an OVD forming medium, and a method for manufacturing such an OVD forming medium are provided. [Brief description of the drawings]
[0024] [Figure 1] FIG. 1 is a diagram illustrating an OVD-forming medium in one embodiment of the present invention, in which (a) shows a schematic cross-sectional view of the OVD-forming medium, (b) shows a schematic cross-sectional view of an optical functional layer on a substrate, and (c) shows a schematic oblique view of a two-dimensional material in the optical functional layer. [Diagram 2] 1A and 1B are schematic cross-sectional views showing MXene, a two-dimensional material that can be used in one embodiment of the present invention, where (a) shows a single-layer MXene and (b) shows a multi-layer (illustratively two-layer) MXene. [Diagram 3] FIG. 2 is a schematic diagram illustrating a method for producing an OVD-forming medium in one embodiment of the present invention. [Figure 4] FIG. 13 is a diagram illustrating an OVD-forming medium in a modified example of one embodiment of the present invention, where (a) shows a schematic cross-sectional view of the OVD-forming medium, and (b) shows a schematic top view of the OVD-forming medium. [Diagram 5] FIG. 2 is a schematic diagram illustrating a method for producing an OVD-forming medium in a modified example of one embodiment of the present invention. [Figure 6] 1 is a schematic top view of an article in one embodiment of the present invention. FIG. [Figure 7] FIG. 1 is a schematic top view of a base layer (paper with a lattice pattern drawn thereon) used in evaluating partial transmittance in Examples 7 to 10. [Figure 8]FIG. 4(a) shows the appearance (schematic top view) of the OVD-forming medium arranged on the underlayer in the evaluation of partial transmittance in Example 10, when the OVD-forming medium was viewed along the C direction in FIG. [Figure 9] FIG. 4(a) shows the appearance (schematic top view) of the OVD-forming medium arranged on the underlayer in the evaluation of partial transmittance in Example 10, when the OVD-forming medium was viewed along the C' direction in FIG. [Figure 10] As a modified example of Examples 9 to 10, the appearance (schematic top view) of the OVD-forming medium placed on the underlayer when the material and / or thickness t2 of the optical functional layer is changed is shown when viewed along the C' direction in Figure 4(a). [Figure 11] (a) and (b) show the appearance (schematic top view) of the OVD-forming medium arranged on the underlayer when the material and / or thickness t1 of the optical functional layer is changed as a modified example of Examples 9 to 10, when viewed along the C direction and the C' direction in Figure 4(a), respectively. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] An OVD-forming medium and a method for producing the same, as well as an article containing the OVD-forming medium, in one embodiment of the present invention will be described in detail below, but the present invention is not limited to this embodiment.
[0026] Referring to FIGS. 1(a) to 1(c), the OVD forming medium 20 of this embodiment is: A substrate 11 having a relief structure on a surface 11a (also called a "relief surface"); an optical functional layer 15 covering the relief structure; and the optically functional layer 15 comprises particles 10 of a two-dimensional material.
[0027] In the OVD forming medium 20, the optical function layer 15 exhibits optical functions (reflection, transmission, refraction, diffusion, absorption, blocking, etc. of light) and exhibits the OVD function together with the relief structure of the surface 11a of the substrate 11 (and possibly the printing layer, etc., described later). The OVD function means the ability to exhibit optical changes that can be recognized by the naked eye and / or other appropriate means. The OVD function is typically the ability to exhibit different appearances depending on the viewing conditions, and more specifically, the ability to display a three-dimensional image or change the color and / or image depending on the viewing conditions (e.g., the viewing direction / angle) by utilizing phenomena such as light diffraction, interference, and / or reflection.
[0028] The relief structure is also called a (fine) concave-convex structure, and its shape, dimensions, pattern, design, etc. may vary depending on the OVD function desired for the OVD forming medium 20. When a visual effect is desired as the OVD function, the structural period p of the concave-convex can be, for example, in the range of 500 nm to 50 μm, and the depth (height difference between the concaves and convexities) d can be, for example, in the range of 0.1 μm to 20 μm, and can be 0.5 μm or more as desired. Note that in the illustrated embodiment, a relief structure (also called a prism structure type) that is sawtooth-shaped in cross section and extends in stripes parallel to the Y axis when viewed from the A direction side (top side) is shown, but is not limited thereto, and other relief structures such as a sine wave or comb-tooth-shaped in cross section may also be used.
[0029] The substrate 11 may be made of any suitable material depending on the application of the OVD-forming medium 20, etc., as long as it has a relief structure on the surface 11a. The substrate 11 may be made of a single body consisting of only a relief structure forming layer, or may be made of a laminate including a carrier film (and optionally a release layer disposed thereon) and a relief structure forming layer (constituting the surface 11a) disposed thereon. Although not essential to this embodiment, the OVD-forming medium 20 may further include an overcoat layer 17 that covers the optical functional layer 15. If present, the overcoat layer 17 may be made of any suitable material depending on the application of the OVD-forming medium 20, etc.
[0030] The OVD-forming medium 20 may have either the A-direction side (upper surface side) or the B-direction side (lower surface side) in FIG. 1(a) as the viewing side. When the A-direction side is the viewing side and the overcoat layer 17 is present, the overcoat layer 17 is transparent. When the B-direction side is the viewing side, the substrate 11 (more specifically, the relief structure forming layer) is transparent. When the optical functional layer 15 in the OVD-forming medium 20 can function as a light transmitting layer, the OVD-forming medium 20 may further include a printing layer (not shown) on the side opposite the viewing side with respect to the optical functional layer 15. In some cases, the OVD-forming medium 20 may further include an adhesive layer (or a bonding layer, not shown) or the like on the side opposite the viewing side.
[0031] The OVD forming medium 20 is characterized in that the optically functional layer 15 comprises particles 10 of a two-dimensional material.
[0032] In the present invention, a two-dimensional material refers to a layered material having a two-dimensional extent, with a thickness of one layer being less than 10 nm, and hereinafter, the surface having a two-dimensional extent of each layer may be referred to as a two-dimensional sheet surface. A two-dimensional material can be understood as a layered material (or a layered compound in some cases) having a two-dimensional bond structure in its atomic structure. The thickness of one layer of a two-dimensional material can typically be 0.3 nm or more and 3 nm or less. A two-dimensional material can have a single layer structure consisting of one layer, or a multilayer structure in which multiple layers are superimposed. In either case, the cross section of the optical functional layer 15 is observed in three or more fields of view with a transmission electron microscope (TEM), the thicknesses of multiple (e.g., 40 or more) layers randomly selected on the observation surfaces are measured, and the number average of the thicknesses is obtained to determine the thickness of one layer of the two-dimensional material.
[0033] Examples of 2D materials include MXene (discussed in more detail below), graphene, transition metal dichalcogenides (TMDs, e.g., molybdenum disulfide, niobium diselenide, etc.), metal oxides, metal hydroxides, layered double hydroxides (LDHs), graphene oxide, boron nitride (hexagonal boron nitride: h-BN), silicone, germanene, and other materials with planar structures similar to any of these.
[0034] The two-dimensional material particles 10 may be particles having a single-layer structure with a thickness of one layer less than 10 nm, particles having a multi-layer structure with a thickness of one layer less than 10 nm, or a mixture thereof, and in either case, may be in the form of a thin sheet having exposed surfaces facing each other. The thickness of the two-dimensional material particles 10 may be, for example, 20 nm or less, preferably less than 10 nm, and may be, for example, 0.3 nm or more, although the lower limit is not particularly essential. The dimension of the two-dimensional material particles 10 in the direction along the exposed surface (or the direction perpendicular to the thickness direction) (hereinafter referred to as "in-plane dimension" in this specification) may be, for example, 0.1 μm or more, preferably 1 μm or more, and may be, for example, 100 μm or less, preferably 20 μm or less. The in-plane dimension of the two-dimensional material particles 10 is preferably 1 / 4 or less of the structural period p of the unevenness in the relief structure.
[0035] In most (usually most) of the two-dimensional material particles 10, the thickness direction of the two-dimensional material particles coincides with the thickness direction of the layer of the two-dimensional material, and the exposed surfaces of the two-dimensional material particles facing each other are two-dimensional sheet surfaces of the two-dimensional material and have high surface smoothness. Even if such two-dimensional material particles 10 are extremely thin particles, for example, having a thickness of 20 nm or less, preferably less than 10 nm, they can be more strictly controlled to have a sheet-like shape than, for example, metal particles ("flake-like or plate-like metal particles" as described in Patent Document 2).
[0036] The two-dimensional material is preferably MXene, which is defined herein as follows: 1. A layered material comprising one or more layers, the one or more layers comprising a compound represented by the following formula: M m X n where M is at least one group 3, 4, 5, 6, 7 metal and may include at least one selected from the group consisting of so-called early transition metals, such as Sc, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo and Mn; X is a carbon atom, a nitrogen atom, or a combination thereof; n is 1 or more and 4 or less, m is greater than n and less than or equal to 5) and a modification or termination T (T is at least one selected from the group consisting of a hydroxyl group, a fluorine atom, a chlorine atom, and an oxygen atom) present on the surface of the layer body (more specifically, on at least one of the two opposing surfaces of the layer body). m X n T s ", where s is any number, and conventionally, x is sometimes used in place of s). Typically, n can be 1, 2, 3, or 4, but is not limited thereto.
[0037] In the above formula for MXene, M is preferably at least one selected from the group consisting of Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, and Mn, and more preferably at least one selected from the group consisting of Ti, V, Cr, and Mo.
[0038] Such MXenes can be synthesized by selectively etching (removing and optionally phase-separating) the A atoms (and optionally some of the M atoms) from the MAX phase. The MAX phase has the following formula: M m AX n (wherein M, X, n and m are as defined above, and A is at least one Group 12, 13, 14, 15, 16 element, usually a Group A element, typically Group IIIA and Group IVA, and more particularly may include at least one element selected from the group consisting of Al, Ga, In, Tl, Si, Ge, Sn, Pb, P, As, S and Cd, and is preferably Al). and M m X n(each X may have a crystal lattice in which it is located in the octahedral array of M) between which a layer composed of A atoms is located. In the MAX phase, typically when m=n+1, one layer of X atoms is arranged between each of the n+1 layers of M atoms (collectively referred to as "M m X n The MAX phase has a repeating unit in which a layer of A atoms (also referred to as an "A layer") is arranged as a layer next to the n+1th layer of M atoms, but is not limited thereto. The A atoms (and sometimes a part of the M atoms) are selectively etched (removed and sometimes layer separated) from the MAX phase, thereby removing the A atom layer (and sometimes a part of the M atoms) to expose the M m X n The surface of the layer is modified by hydroxyl groups, fluorine atoms, chlorine atoms, oxygen atoms, etc. present in the etching solution (usually, an aqueous solution of fluorine-containing acid is used, but is not limited to this) to terminate the surface. - The etching may be carried out using an etching solution containing, for example, a method using a mixture of lithium fluoride and hydrochloric acid, or a method using hydrofluoric acid. Thereafter, any suitable post-treatment (e.g., ultrasonic treatment, hand shaking, automatic shaker, etc.) may be used to promote layer separation of MXene (delamination, separation of multi-layer MXene into single-layer MXene). Note that ultrasonic treatment may destroy MXene due to excessive shear force, so when it is desired to obtain MXene with a two-dimensional shape having a larger aspect ratio (preferably single-layer MXene), it is preferable to apply an appropriate shear force by hand shaking or an automatic shaker, etc.
[0039] MXene is a compound represented by the above formula: m X n However, it is known that it can be expressed as follows: Sc2C, Ti2C, Ti2N, Zr2C, Zr2N, Hf2C, Hf2N, V2C, V2N, Nb2C, Ta2C, Cr2C, Cr2N, Mo2C, Mo 1.3 C, Cr 1.3 C, (Ti,V)2C, (Ti,Nb)2C, W2C, W1.3 C, Mo2N, Nb 1.3 C, Mo 1.3 Y 0.6 C (in the above formula, "1.3" and "0.6" mean approximately 1.3 (= 4 / 3) and approximately 0.6 (= 2 / 3), respectively), Ti3C2, Ti3N2, Ti3(CN), Zr3C2, (Ti,V)3C2, (Ti2Nb)C2, (Ti2Ta)C2, (Ti2Mn)C2, Hf3C2, (Hf2V)C2, (Hf2Mn)C2, (V2Ti)C2, (Cr2Ti)C2, (Cr2V)C 2, (Cr2Nb)C2, (Cr2Ta)C2, (Mo2Sc)C2, (Mo2Ti)C2, (Mo2Zr)C2, (Mo2Hf)C2, (Mo2V)C2, (Mo2Nb)C2, (Mo2Ta)C2, (W2Ti)C2, (W2Zr)C2, (W2Hf)C2, Ti4N3, V4C3, Nb4C3, Ta4C3, (Ti,Nb)4C3, (Nb,Zr)4C3, (Ti2Nb2)C3, (Ti2Ta2)C3, (V2Ti2)C3, (V2Nb2)C3, (V2Ta2)C3, (Nb2Ta2)C3, (Cr2Ti2)C3, (Cr 2V2)C3, (Cr2Nb2)C3, (Cr2Ta2)C3, (Mo2Ti2)C3, (Mo2Zr2)C3, (Mo2Hf2)C3, (Mo2V2)C3, (Mo2Nb2)C3, (Mo2Ta2)C3, (W2Ti2)C3, (W2Zr2)C3, (W2Hf2)C3
[0040] Typically, in the above formula, M can be titanium or vanadium, and X can be a carbon atom or a nitrogen atom. For example, the MAX phase is Ti3AlC2, and MXene is Ti3C2T s (In other words, M is Ti, X is C, n is 2, and m is 3). That is, the above formula: M m X n However, it is Ti3C2.
[0041] In the present invention, MXene may contain a relatively small amount of residual A atoms, for example, 10% by mass or less of the original A atoms. The amount of residual A atoms may be preferably 8% by mass or less, more preferably 6% by mass or less. However, even if the amount of residual A atoms exceeds 10% by mass, there may be cases where there is no problem depending on the application and use conditions of the OVD forming medium.
[0042] The MXene (particle) thus synthesized may be a layered material comprising one or more MXene layers 7a, 7b, as shown diagrammatically in FIG. 2 (examples of the MXene (particle) include, but are not limited to, one layer of MXene 10a in FIG. 2(a) and two layers of MXene 10b in FIG. 2(b)). More specifically, the MXene layers 7a, 7b may be a layered material comprising one or more MXene layers 7a, 7b, as shown diagrammatically in FIG. 2(a). m X n The layer body (M m X n The MXene layers 7a, 7b have "M m X n T s ", where s is any number. The MXene particles may be those in which the MXene layers are individually separated and present as one layer (single layer structure shown in FIG. 2(a), so-called single layer MXene10a), or may be a laminate in which multiple MXene layers are stacked at a distance from each other (multilayer structure shown in FIG. 2(b), so-called multilayer MXene10b), or a mixture thereof. The MXene (particles) may be aggregate particles (which may also be referred to as powder or flakes) composed of single layer MXene10a and / or multilayer MXene10b. In the case of multilayer MXene, two adjacent MXene layers (e.g. 7a and 7b) do not necessarily have to be completely separated, and may be partially in contact.
[0043] Without being limiting to this embodiment, the thickness of each MXene layer (corresponding to the above-mentioned MXene layers 7a and 7b) is, for example, 0.8 nm or more and 5 nm or less, particularly 0.8 nm or more and 3 nm or less (which may vary mainly depending on the number of M atomic layers contained in each layer), and the maximum dimension in a plane parallel to the layer (two-dimensional sheet surface) (which may correspond to the "in-plane dimension" of the particle) is, for example, 0.1 μm or more, particularly 1 μm or more, for example 200 μm or less, particularly 40 μm or less.
[0044] When the MXene is a laminate (multilayer MXene), for each individual laminate, the interlayer distance (or gap dimension, shown as Δd in Figure 2(b)) is, for example, 0.8 nm or more and less than 10 nm, particularly 0.8 nm or more and 5 nm or less, more particularly about 1 nm, and the maximum dimension in a plane perpendicular to the stacking direction (the two-dimensional sheet surface) (which may correspond to the "in-plane dimension" of the particle) is, for example, 0.1 μm or more, particularly 1 μm or more, for example 100 μm or less, particularly 20 μm or less.
[0045] The total number of MXene layers may be 1 or 2 or more, for example, 1 to 20, and the thickness in the stacking direction (which may correspond to the "thickness" of the particle) is, for example, 0.8 to 20 nm.
[0046] When the MXene is a laminate (multilayer MXene), it is preferably an MXene with a small number of layers. The term "small number of layers" refers to, for example, an MXene having 6 or less laminated layers. In addition, the thickness in the lamination direction of a multilayer MXene with a small number of layers is preferably less than 10 nm. In this specification, this "multilayer MXene with a small number of layers" is also referred to as a "few-layer MXene."
[0047] In this embodiment, the MXene is preferably a particle (which may also be referred to as a nanosheet) composed mostly of monolayer MXene and / or few-layer MXene. In this specification, monolayer MXene and few-layer MXene may be collectively referred to as "monolayer / few-layer MXene".
[0048] In other words, the average thickness of the MXene particles is preferably less than 10 nm. This average thickness is more preferably 7 nm or less, and even more preferably 5 nm or less. On the other hand, considering the thickness of a single layer of MXene, the lower limit of the thickness of the MXene particles may be 0.8 nm. Thus, the average thickness of the MXene particles may be about 1 nm or more.
[0049] From another perspective, the proportion of particles with a thickness of less than 10 nm in the stacking direction (single-layer MXene and / or few-layer MXene) in all MXene particles is preferably 90 vol. % or more, and more preferably 95 vol. % or more.
[0050] The above dimensions may be determined as number-average dimensions (e.g., number-average of at least 40 particles) based on photographs taken with a scanning electron microscope (SEM), a transmission electron microscope (TEM), or an atomic force microscope (AFM), or as distances in real space calculated from the position in reciprocal space of the (002) plane measured by X-ray diffraction (XRD).
[0051] Referring again to Figures 1(a) to (c), the particles 10 of the two-dimensional material can be densely present in the optical functional layer 15. In the optical functional layer 15, the particles 10 of the two-dimensional material can be present in an oriented state with respect to the surface 11a (relief surface) of the substrate 11 (Figure 1(b)), and the particles 10 of the two-dimensional material can also be present in an oriented (preferably parallel) state with each other (Figures 1(b) and (c)). Note that, for convenience, Figure 1(b) is rotated as a whole so that the surface 11a of the substrate 11 is parallel to the horizontal direction (width direction) of the paper.
[0052] Therefore, it is considered that the two-dimensional material particles 10 contact each other and the two-dimensional material particles 10 contact the surface 11a (relief surface) over a relatively large area. Furthermore, since the two-dimensional material particles 10 have high surface smoothness on the exposed surfaces facing each other, high adhesion is obtained at the contact surfaces between the two-dimensional material particles 10 and between the two-dimensional material particles 10 and the surface 11a. As a result, a large adhesion force (or adhesive force or bonding force) is obtained, and an optical functional layer 15 with high film strength (hard to peel off) is obtained. Such adhesion force can be enhanced by van der Waals forces and, if applicable, hydrogen bonds depending on the surface state of the two-dimensional material particles 10.
[0053] Due to the large adhesion, the binder content in the optical functional layer 15 can be reduced, and preferably the optical functional layer 15 can be binderless, for example, composed only of the two-dimensional material particles 10. The binder content in the optical functional layer 15 can be, for example, 50 vol.% or less, preferably 25 vol.% or less, and more preferably substantially 0 vol.%. The content of the two-dimensional material particles 10 in the optical functional layer 15 can be, for example, 50 vol.% or more, preferably 75 vol.% or more, and more preferably substantially 100 vol.%. When the optical function of the optical functional layer 15 can be ensured by the two-dimensional material particles 10, it is preferable that the binder content in the optical functional layer 15 is low, since the optical function of the optical functional layer 15 can be reduced / prevented from being impaired by the binder. When present, the binder can be, for example, any suitable organic material, more specifically, a resin material such as polyurethane or nitrocellulose.
[0054] The optical functional layer 15 containing the particles 10 of the two-dimensional material can be formed as a layer with a strictly controlled thickness. The thickness of the optical functional layer 15 can be, for example, 3 μm or less (3.0 μm or less when strictness is required), particularly 1.5 μm or less, more particularly 1 μm or less (1.0 μm or less when strictness is required). The thickness of the optical functional layer 15 is preferably smaller than the depth d of the unevenness in the relief structure. The lower limit of the thickness of the optical functional layer 15 is not particularly required, but can be, for example, 0.05 μm or more.
[0055] The optical function layer 15 can be adjusted in optical function by forming it with its thickness strictly controlled, and can be preferably transparent, semi-transparent, or opaque. The optical function layer 15 can function as a light reflecting layer or a light transmitting layer at all times or depending on the viewing conditions (e.g., the direction / angle of observation). For example, the reflectance of light can be increased at all times (irrespective of the viewing conditions) by increasing the thickness of the optical function layer 15, and the transmittance of light can be increased at all times by decreasing the thickness of the optical function layer 15. In addition, since the particles 10 of the two-dimensional material are present in an oriented state in the optical function layer 15, even if the thickness of the optical function layer 15 is extremely thin, it is possible to efficiently exhibit the optical function (e.g., reflection or transmission of light). The thickness of the optical function layer 15 may be substantially uniform over the entire surface of the optical function layer 15, or may be different among the multiple parts constituting the optical function layer 15. By designing the thickness of the optical functional layer 15 (or the thickness distribution that varies depending on the part) in combination with the shape, dimensions, pattern, design, etc. of the relief structure of the substrate 11 and forming these precisely, it is possible to realize a variety of OVD functions (e.g., difficult to counterfeit / imitate and easy to visually determine authenticity, or highly design / decorative) according to the viewing conditions (e.g., the observation direction / angle).
[0056] Among two-dimensional materials, MXene has a metallic luster and can provide high reflectance. In addition, MXene has a modification or terminal T (T is at least one selected from the group consisting of hydroxyl, fluorine, chlorine, and oxygen), and such modification or terminal T can have high activity, and the hydroxyl / oxygen atom can form hydrogen bonds, so that an optical functional layer 15 with sufficiently high film strength (hard to peel off) can be obtained with a small amount of binder or preferably binderless.
[0057] The optical functional layer 15 as described above can be formed with a strictly controlled thickness by a simple process without requiring expensive equipment for vacuum deposition or sputtering.
[0058] An example of a method for manufacturing the OVD-forming medium 20 of this embodiment will be described in detail below.
[0059] The method for manufacturing the OVD forming medium 20 includes the following steps: (a) providing a substrate 11 having a relief structure on a surface 11a; (b) applying a liquid comprising particles 10 of a two-dimensional material and a liquid medium onto the relief structure to form an optically functional layer 15 covering the relief structure and comprising particles 10 of the two-dimensional material; More specifically, the following:
[0060] ·Process (a) First, a substrate 11 having a relief structure on its surface 11a is prepared. The relief structure may be formed by any appropriate method depending on the material constituting the surface 11a of the substrate 11, and may be formed, for example, as follows.
[0061] The material constituting the surface 11a of the substrate 11 (material of the relief structure forming layer) may be, for example, a resin material such as a thermoplastic resin, a thermosetting resin, or a radiation (ultraviolet ray, electron beam, etc.) curable resin. Examples of the thermoplastic resin include an acrylic resin, an epoxy resin, a cellulose resin, and a vinyl resin. Examples of the thermosetting resin include a urethane resin, a melamine resin, and a phenol resin crosslinked by adding a polyisocyanate as a crosslinking agent to an acrylic polyol or a polyester polyol having a reactive hydroxyl group. Examples of the radiation (ultraviolet ray, electron beam, etc.) curable resin include a (meth)acrylic resin.
[0062] Such a resin material may be applied to a carrier film (not shown) by a known method such as gravure printing or microgravure printing.
[0063] Then, a master plate (or a replica plate) is used to form a relief structure (embossed structure) on the applied resin material. When the resin material is a thermoplastic resin, the master plate is pressed against it, the resin material is plasticized by heating, and the resin material is cooled in this state, thereby forming a relief structure. Alternatively, when the resin material is a thermosetting resin or a radiation curable resin, the master plate is pressed against the uncured (or semi-cured) resin material, and the resin material is cured in this state, thereby forming a relief structure. Note that continuous molding is facilitated by using a roll-shaped master plate.
[0064] The original plate is prepared, for example, by using an electron beam lithography device. Usually, the concave-convex portion of the original plate is transferred to prepare an inverted plate, and the concave-convex structure of the inverted plate is transferred to prepare a duplicate plate. Then, as necessary, the duplicate plate is used as the original plate to prepare an inverted plate, and the concave-convex structure of the inverted plate is transferred to prepare a duplicate plate. The duplicate plate thus obtained is usually used for forming the actual concave-convex structure.
[0065] ·Process (b) A liquid comprising particles 10 of the two-dimensional material and a liquid medium is then applied onto the relief structure to form an optically functional layer 15 covering the relief structure and comprising particles 10 of the two-dimensional material.
[0066] This step is understood as a wet process, and is a simple process that does not require expensive equipment such as vacuum deposition or sputtering. Unlike vacuum deposition, this process can form an optical function layer without exposure to high temperatures, so that even a material that may be deformed by heat can be selected as the material of the substrate 11, and further, thermal deformation of the relief structure can be prevented, and the desired OVD function can be expressed with high precision even in a relief structure with an extremely fine design.
[0067] The liquid medium may be either an aqueous medium or an organic medium. The aqueous medium is typically water, and may contain a relatively small amount of other liquid substances in addition to water (for example, 30 mass % or less, preferably 20 mass % or less based on the total aqueous medium). The organic medium is not particularly limited, and may be, for example, a protic solvent such as alcohol, or an aprotic solvent, or a mixed solvent of two or more of these, but is preferably one that does not easily remain in the optical functional layer 15.
[0068] The liquid containing the particles 10 of the two-dimensional material and the liquid medium is preferably a dispersion in which the particles 10 of the two-dimensional material are dispersed in the liquid medium. The liquid may optionally contain a dispersant.
[0069] When the two-dimensional material particle 10 is MXene (particle), the liquid medium is preferably an aqueous medium. MXene has a modification or terminal T (T is at least one selected from the group consisting of a hydroxyl group, a fluorine atom, a chlorine atom, and an oxygen atom), and due to the effect of the modification or terminal T, it is easy to disperse in an aqueous medium, and a dispersion with a relatively high particle concentration can be prepared while preventing particle aggregation. In particular, single-layer and small-layer MXene is preferable because it has higher dispersibility in an aqueous medium. For example, the solid concentration (particle concentration) of the MXene (particle)-aqueous dispersion can reach 100 mg / mL (about 10 mass%) even without a dispersant while preventing aggregation of MXene. Therefore, when the two-dimensional material particle 10 is MXene (particle), other components that may remain in the optical function layer 15 and impair its optical function can be eliminated, and an optical function layer 15 that can exhibit high optical function can be formed at low raw material cost.
[0070] The method of applying the liquid containing the two-dimensional material particles 10 and the liquid medium onto the relief structure is not particularly limited, and may be, for example, a method such as spraying, printing, inkjet, dispenser, etc. In these methods, by adjusting the application conditions, the optical functional layer 15 can be formed at a strictly controlled thickness at low cost.
[0071] In the case of spraying, more specifically: (b1) applying said liquid onto the relief structure by spraying said liquid onto the substrate 11 to form a precursor of the optical functional layer 15; and (b2) drying the precursor (at least partially removing the liquid medium); In this way, the optical function layer 15 can be formed.
[0072] The above steps (b1) and (b2) can be repeated until a desired thickness is obtained in the optical functional layer 15. This allows the optical functional layer 15 to be formed with a strictly controlled thickness at low cost.
[0073] In the case where the two-dimensional material particles 10 are MXene (particles) and the liquid medium is an aqueous medium, when the liquid medium is at least partially removed, high adhesion is obtained between the two-dimensional material particles 10 and between the two-dimensional material particles 10 and the surface 11 of the substrate 11 due to the effect of the MXene modification or the terminal T. This makes it possible to form an optical functional layer 15 with high film strength.
[0074] Thereafter, if desired, an overcoat layer 17 may be formed by any suitable method.
[0075] In this manner, the OVD forming medium 20 of this embodiment is manufactured. When the A direction side (upper surface side) of FIG. 1(a) is the viewing side, the optical functional layer 15 has a structural period p and a depth d similar to the relief structure. When the B direction side (lower surface side) of FIG. 1(a) is the viewing side, the optical functional layer 15 has a structural period p' and a depth d'. The structural period p' and the depth d' may vary depending on the thickness of the optical functional layer 15.
[0076] In the OVD forming medium 20 of this embodiment, the optical functional layer 15 may have a substantially uniform thickness over the entire surface of the optical functional layer 15, or may have a different thickness depending on the relief structure. More specifically, the optical functional layer 15 may include a first portion and a second portion depending on the relief structure, and the thickness t1 of the first portion and the thickness t2 of the second portion may be the same, or the thickness t2 of the second portion may be smaller than the thickness t1 of the first portion. In the illustrated embodiment, when the portion covering the inclined upper surface of the relief structure is the first portion (thickness t1) and the portion covering the wall surface of the relief structure is the second portion (thickness t2), t1 ≧ t2 may be satisfied.
[0077] As shown in FIG. 1(a), the OVD forming medium 20 of this embodiment can have a uniform thickness that does not cause significant differences in optical function, and the ratio of the thickness of the second portion to the thickness of the first portion (defined as t2 / t1×100(%), hereinafter also referred to simply as the "thickness ratio") can be relatively large, for example, 80% or more, particularly 85% or more, and 100% or less. The larger the thickness ratio is and the closer it is to 100%, the more homogeneous the optical function layer 15 can be obtained.
[0078] The optical functional layer 15 having such a relatively large thickness ratio can be formed in the above step (b1) by spraying the above liquid material from the nozzle 21 in a discharge direction E (preferably vertical) at an angle of 90 degrees (preferably vertical) to the substrate 11, as shown in Fig. 3. Note that in Fig. 3, the substrate 11 is illustrated without showing the relief structure present on the surface 11a (relief surface).
[0079] The discharge direction E can be determined based on the shape of the discharge portion of the nozzle 21, and means the direction in which the mist M of the liquid material is discharged most vigorously and / or in the greatest amount. The angle of the discharge direction E can be the angle θa with respect to the imaginary (for example, average) main surface of the surface 11a having the relief structure, but if the back surface 11b of the substrate 11 is flat, it may be the angle θb with respect to the back surface 11b. If the relief structure is large relative to the discharge area (spray area) on the surface 11a of the mist M of the liquid material discharged from the nozzle 21, or if there is a possibility of variation in the amount of the mist M of the liquid material adhering to the relief structure, the optical function layer 15 can be formed with uniform quality by moving (sliding) either one or both of the nozzle 21 and the substrate 11 relative to each other parallel to the XY plane. (These explanations also apply to the modified example shown in FIG. 5.)
[0080] Alternatively, it is also possible to intentionally reduce the thickness ratio to produce a difference in optical function between a first portion having a relatively large thickness and a second portion having a relatively small thickness in the optical function layer.
[0081] FIG. 4 shows an OVD-forming medium 20' in a modified example of this embodiment. In the OVD-forming medium 20', the optical functional layer 15' includes a first portion and a second portion according to the relief structure, and the thickness t2 of the second portion is smaller than the thickness t1 of the first portion. In the illustrated embodiment, if the portion covering the inclined upper surface of the relief structure is the first portion (thickness t1) and the portion covering the wall surface of the relief structure is the second portion (thickness t2), t1>t2 can be satisfied. Also, if desired, t2 can be zero, i.e., the optical functional layer 15' can be composed of only the portion covering the inclined upper surface of the relief structure (first portion), and the portion covering the wall surface of the relief structure (second portion) can be omitted.
[0082] In the OVD forming medium 20' of the modified example of this embodiment, the ratio of the thickness of the second portion to the thickness of the first portion (thickness ratio = t2 / t1 x 100 (%)) is relatively small, for example, less than 80%, particularly 50% or less, more particularly 20% or less, and may be 0% or more. The smaller the thickness ratio is and the closer it is to 0%, the more difference (e.g., anisotropy) can be generated in the optical function of the optical function layer 15.
[0083] The optical functional layer 15' having such a relatively small thickness ratio can be formed in the above step (b1) by spraying the liquid from the nozzle 21 in a discharge direction E that is less than 90 degrees, preferably 50 degrees or less, more preferably 45 degrees or less, with respect to the substrate 11, as shown in FIG. 5. The angle of the discharge direction E can be selected according to the inclined upper surface of the relief structure. For example, as shown in FIG. 4(a)-(b), in the case of a relief structure (also called a prism structure type) that is sawtooth-shaped in cross section and extends in stripes parallel to the Y axis when viewed from the A direction side (upper surface side), the nozzle 21 can be preferably rotated around the Y axis and angled as shown in FIG. 5. In FIG. 5, the substrate 11 is illustrated without the relief structure present on the surface 11a (relief surface).
[0084] When the angle of the discharge direction E with respect to the substrate 11 is less than 90 degrees, preferably 50 degrees or less, more preferably 45 degrees or less, the smaller the angle, the more the optical functional layer 15 has a different thickness depending on the relief structure. In the case of the OVD forming medium 20' shown in FIG. 4, the smaller the angle, the smaller the thickness ratio (=t2 / t1×100(%)) becomes in the optical functional layer 15'. If desired, the angle of the discharge direction E with respect to the substrate 11 may be made very small, so that t2 is zero (substantially zero). However, there is no particular problem even if the particles 10 of the two-dimensional material wrap around and t2 cannot be made completely zero.
[0085] For example, by setting the angle to 50 degrees or less, preferably 45 degrees or less, a difference in optical function can be generated between the first part (thickness t1) covering the inclined upper surface of the optical function layer 15' and the second part (thickness t2) covering the wall surface of the relief structure. As a result, different visual effects can be presented depending on the viewing conditions. For example, as shown in Figures 4(a) to (b), in the case of a relief structure (also called a prism structure type) that is sawtooth-shaped in cross section and extends in stripes parallel to the Y axis when viewed from the A direction side (top side), a base layer (not shown) with a predetermined pattern drawn thereon is placed under the OVD forming medium 20', and observed from the A direction side (top side) of Figure 4(a). Referring to FIG. 4(a), when the viewing direction is a direction C that rotates from the direction A to the positive direction of the X-axis around the Y-axis and forms an angle θ with respect to the substrate 11, the pattern of the underlayer (not shown) cannot be viewed through the optical functional layer 15' (the optical functional layer 15' is not transparent in the direction C). In this case, the viewing direction crosses the first portion having a relatively large thickness t1, and the pattern of the underlayer cannot be viewed. However, referring to FIG. 4(a), when the viewing direction is a direction C' that rotates from the direction A to the negative direction of the X-axis around the Y-axis and forms an angle θ' with respect to the substrate 11, the pattern of the underlayer (not shown) can be viewed through the optical functional layer 15' (the optical functional layer 15' is transparent in the direction C'). In this case, the viewing direction can cross the second portion having a relatively small thickness t2, and the pattern of the underlayer can be viewed. The design is not particularly limited and may be a pattern or color, or a combination of these, and may be, for example, a picture, a letter, a number, a design / pattern (e.g., a geometric pattern), or the like, either alone or in combination of two or more. Although not limiting this embodiment, by checking (identifying) such a design, it is possible to reliably distinguish the OVD forming medium of this embodiment from other counterfeit / imitation products or similar products.
[0086] According to this modified example, an optical functional layer 15' that can provide different visual effects according to viewing conditions can be formed using a simple process without variation in quality or loss of material.
[0087] The OVD forming medium and its manufacturing method of this embodiment may be modified without departing from the scope of the present invention. For example, depending on the two-dimensional material used, the optically functional layer may absorb or block light instead of / in addition to reflecting light.
[0088] The OVD forming medium 20 of this embodiment may exist alone or may form some kind of article together with other members.
[0089] The article 30 of this embodiment is described in more detail below.
[0090] Referring to FIG. 6, the article 30 of this embodiment is Object 25; An OVD forming medium 20 attached to an object 25; may include.
[0091] The object 25 may vary depending on the use and / or purpose of the OVD forming medium 20. For example, the OVD forming medium may be used for security purposes such as preventing counterfeiting / imitation, or for the purpose of adding design / decoration. The object 25 is not particularly limited, and may be, for example, a credit card, an ID card, a bill, a computer software package, a music software package, a video software package, an electronic component package (for example, an electronic component package in which a tape containing multiple electronic components is wound in a reel shape), etc. (FIG. 6 exemplarily shows a case in which the object 25 is a credit card.)
[0092] The method of attaching the OVD-forming medium 20 to the object 25 is not particularly limited, and any appropriate method may be used. For example, an adhesive layer (or a bonding layer, not shown) may be provided on the side of the OVD-forming medium 20 opposite to the viewing side, and the adhesive layer may be brought into contact with the object 25, so that the OVD-forming medium 20 may be attached to the object via the adhesive layer.
[0093] Typically, the OVD-forming medium 20 can be attached to the object 25 by transfer. In this case, the B direction side in FIG. 1(a) is the viewing side. More specifically, first, a release layer (a layer that promotes the release of the carrier film) and a transparent relief structure forming layer are formed in this order on a carrier film as the substrate 11. Then, an optical function layer 15 that covers the relief structure (surface 11a) of the relief structure forming layer, an overcoat layer 17, and an adhesive layer (not shown) are formed in this order on the substrate 11 obtained in this way. The laminate obtained in this way is attached so that the adhesive layer contacts the object 25, and then the carrier film is peeled off. As a result, the OVD (more specifically, the OVD-forming medium 20 excluding the carrier film) is transferred to the object 25 so that the release layer is located on the outermost surface on the viewing side.
[0094] However, the article 30 of this embodiment may be in any other suitable form as long as it includes the OVD-forming medium 20. In addition, the OVD-forming medium 20 of this embodiment is not limited to constituting the article 30, and may be distributed on the market by itself (in a state before being attached to the object 25, for example, with the above-mentioned carrier film). EXAMPLES
[0095] (Examples 1 to 6) Examples 1 to 6 relate to an embodiment in which an optical functional layer is formed by spraying in a discharge direction E at an angle of 90 degrees to the substrate as shown in FIG.
[0096] [Preparation of MXene-water dispersion A] As described in detail below, (1) preparation of precursor (MAX), (2) etching of the precursor, (3) cleaning, (4) delamination, (5) ultrasonic cleaning, and (6) concentration adjustment were carried out in that order to prepare MXene-aqueous dispersion A.
[0097] (1) Preparation of precursor (MAX) TiC powder, Ti powder, and Al powder (all manufactured by Kojundo Chemical Laboratory Co., Ltd.) were mixed in a molar ratio of 2:1:1 in a ball mill containing zirconia balls for 24 hours. The mixed powder was sintered at 1350°C for 2 hours in an Ar atmosphere. The sintered body (block) was pulverized with an end mill to a maximum dimension of 40 μm or less. As a result, Ti3AlC2 particles were obtained as the precursor (MAX).
[0098] (2) Etching of Precursor Using the Ti3AlC2 particles (powder) prepared by the above method, etching was carried out under the following etching conditions to obtain a solid-liquid mixture (slurry) containing solid components derived from the Ti3AlC2 powder. (Etching conditions) Precursor: Ti3AlC2 (passed through a 45μm sieve) Etching solution composition: A mixture of 3g of LiF and 30mL of hydrochloric acid (9 mol / L). Precursor input: 3.0g Etching container: 100mL Eyeboy Etching temperature: 35℃ Etching time: 24h Stirrer speed: 400 rpm
[0099] (3) Cleaning The above slurry was divided into three parts and placed in three 50 mL centrifuge tubes, and centrifuged at a relative centrifugal force (RCF) of 3500G (which causes the clay to settle), after which the supernatant was separated and removed (discarded). 40 mL of pure water was added to each centrifuge tube (containing the remainder after the supernatant was separated and removed), and centrifuged again at 3500G to separate and remove the supernatant. This operation was repeated 11 times. Finally, MXene (Ti3C2T s )-water medium clay was obtained.
[0100] (4) Delamination The above MXene (Ti3C2T s)-Water medium clay was added with 40 mL of pure water, stirred for 15 minutes on a shaker, centrifuged at 3500 G, and the supernatant was separated into single-layer and single-layer MXene (Ti3C2T s )-containing liquid was recovered.
[0101] (5) Ultrasonic cleaning The above single-layer and small-layer MXene (Ti3C2T s The resulting solution was subjected to ultrasonic cleaning for 10 minutes in an ultrasonic cleaner.
[0102] (6) Density adjustment Then, the single-layer and few-layer MXene (Ti3C2T s The MXene-containing liquid was diluted with pure water so that the concentration of the particles as solid content was adjusted to 10 mg / mL (approximately 1 mass %), thereby obtaining an MXene-aqueous dispersion A.
[0103] [Preparation of MXene-aqueous dispersion B] MXene-aqueous dispersion B was prepared in the same manner as for preparing MXene-aqueous dispersion A, except that (5) ultrasonic cleaning was not performed.
[0104] [MXene (particles) contained in MXene-aqueous dispersions A and B] The MXene (particles) contained in MXene-aqueous dispersions A and B were investigated. s The thickness of each layer is about 1.0 nm.
[0105] The thickness of MXene (particles) contained in MXene-aqueous dispersions A and B was measured as follows. The MXene-aqueous dispersion was applied onto a silicon substrate and dried to remove water (solvent). The MXene (particles) remaining on the substrate were then observed with an atomic force microscope (AFM) to measure the thickness of multiple particles, and the number average of these was taken as the "thickness" of the two-dimensional particles. A Dimension-FastScan (manufactured by Bruker Japan Co., Ltd.) was used for the AFM. The measurement conditions were a viewing angle of 30 μm × 30 μm and a scanning speed of 18 μm / s-0.3 Hz. The measurement was performed in five or more fields of view in which at least one particle was present, and the thickness of all particles present in one field of view (excluding particles that were crushed and difficult to measure) was measured (thus, the thickness of particles was measured for at least five particle samples).
[0106] The in-plane dimensions of MXene (particles) contained in MXene-aqueous dispersions A and B were measured as follows. The MXene-aqueous dispersion was applied onto a silicon substrate and dried to remove the water (solvent). The MXene (particles) remaining on the substrate were then observed with a scanning electron microscope (SEM) at a viewing angle of about 30 μm to about 100 μm, the maximum dimensions of multiple randomly selected particles were measured, and the number average of these was taken as the "in-plane dimensions" of the two-dimensional particles. A JSM-6390LV (manufactured by JEOL Ltd.) was used for the SEM. The measurement conditions were 2000x magnification, accelerating voltage of 5 kV, 3 or more visual fields, and a total of 40 or more particles were measured.
[0107] The results are shown in Table 1.
[0108] [Table 1]
[0109] Ti3C2T used as MXene s uses Ti as the metal, and is expected to have a higher light reflectance than other two-dimensional materials, such as graphene and graphene oxide.
[0110] Furthermore, the solids concentration of MXene-aqueous dispersions A and B was set to 10 mg / mL (approximately 1% by mass) in consideration of the ease of spraying and thickness controllability. At this concentration, the viscosity of the MXene-aqueous dispersion is very small (approximately 1 mPas), and the ease of spraying is high. However, even with a solids concentration of approximately 100 mg / mL (approximately 10% by mass) of the MXene-aqueous dispersion, the MXene is dispersed at the solids concentration without the addition of a dispersant while preventing aggregation.
[0111] [Manufacture of OVD forming medium] As described in detail below, OVD-forming media of Examples 1 to 6 were produced.
[0112] (a) Preparing a substrate having a relief structure on its surface A polyethylene terephthalate (PET) film was used as the carrier film. A thermoplastic resin was applied to one side of the carrier film to produce a coated film. Next, a separately prepared mold master having a concave-convex pattern was pressed against the thermoplastic resin of the coated film, and heat treatment (heating and cooling) was performed to transfer the concave-convex pattern to the thermoplastic resin.
[0113] This resulted in a substrate having a relief structure on its surface. The relief structure was sawtooth-shaped in cross section and extended in stripes when viewed from the A direction side (top side), as described above with reference to Figure 1. The structural period p of the relief structure was 10 μm, and the depth d was 5 μm.
[0114] (b) Application of MXene-water dispersion onto relief structures The surface of the base material having the relief structure prepared above was subjected to ultraviolet (UV) treatment for 15 minutes (hydrophilization treatment).
[0115] Then, the MXene-water dispersion A or B (solid concentration 10 mg / mL) prepared above was sprayed onto the relief structure of the above substrate using a commercially available airbrush (Tamiya Co., Ltd., Airbrush System No. 23, Spraywork HG Airbrush Wide (Trigger Type) 74523). The spraying was performed in a discharge direction E at an angle of 90 degrees to the substrate (vertically). After spraying, the substrate was dried by blowing hot air with a hand dryer (Panasonic Co., Ltd., EH5206P-A). The thickness of each precursor layer by spraying was several tens of nm. After spraying one layer of the precursor, the substrate was sufficiently dried by blowing hot air (the substrate temperature during drying was considered to be 40°C or higher, which effectively promoted drying). Such spraying and drying operations were repeated a total of 10 to 100 times. The substrate was then dried in a vacuum oven at 80°C for 16 hours.
[0116] This formed an optical functional layer that covered the relief structure and contained MXene (particles), and an OVD-forming medium was manufactured. In Examples 1 to 5, MXene-aqueous dispersion A was used, and optical functional layers of different thicknesses were formed by varying the number of times the above-mentioned spraying and drying were repeated. In Example 6, MXene-aqueous dispersion B was used to form an optical functional layer. Since no binder was added to either MXene-aqueous dispersion A or B, the optical functional layer did not contain a binder in all of the OVD-forming media of Examples 1 to 6.
[0117] [Evaluation of OVD forming media, etc.] For the OVD forming media of Examples 1 to 6 produced as described above, the thickness of the optical functional layer was measured, and further, peeling, color tone change, and transmittance were evaluated as follows.
[0118] (Thickness of optical function layer) For the substrate on which the optical functional layer was formed, FIB (focused ion beam) processing was performed at three locations in the first portion covering the inclined upper surface of the relief structure to expose the optical functional layer and the relief structure portion of the substrate below it. The cross sections of each location were observed with an SEM (scanning electron microscope) to obtain SEM observation images of a total of three fields of view. The thickness of the optical functional layer was measured at five or more locations per field of view, and the average value of these measurements was taken as the thickness t1 of the optical functional layer.
[0119] (peeling) After the optical functional layer was formed, it was visually observed whether the optical functional layer peeled off due to handling, simple contact, etc. In this evaluation, the absence of peeling means that the optical functional layer can withstand the process load from the formation of the optical functional layer until the formation of the overcoat layer.
[0120] (Color change) The OVD-forming medium was irradiated with light from the surface side (A direction side) and visual observation was performed to determine whether the appearance of the OVD-forming medium changed when the observation direction and / or angle were changed as the viewing conditions from the surface side of the OVD-forming medium. More specifically, a uniform color change was observed over the entire surface of the OVD-forming medium, and the area ratio of the area where the color change was not observed partially was 10% or less. A color change was observed, but the area ratio where the color change was not observed partially or where the color change was recognized as uneven was 10 to 50%. A color change was not observed over 50% or more of the surface. In this evaluation, the presence of a color change means that a change in the intensity of transmitted light and / or reflected light depending on the period and depth of the relief structure can be recognized by changing the observation direction and / or angle during visual observation.
[0121] (transparency) Light was irradiated from the back side (side along direction B) of the substrate, and visual observation was performed to check whether transmitted light could be confirmed from the front side (side along direction A) of the OVD-forming substrate (i.e., whether there was transparency).
[0122] The results are shown in Table 2.
[0123] [Table 2]
[0124] In all of the OVD forming media of Examples 1 to 6, no peeling occurred even though the optical functional layer was binderless and was composed substantially only of MXene particles (MXene particle content: 100%).
[0125] In the OVD-forming media of Examples 1 to 4, when observed from the surface side (A direction side) of the OVD-forming media, the relief structure caused shading. This means that a shading image can be displayed by designing the inclination of the relief structure based on an image prepared in advance. More specifically, in the OVD-forming media of Examples 1 to 4, when observed from the surface side (A direction side) of the OVD-forming media, the shading could be changed (within the range of ◯ to △, which is the criterion for judging color tone change) by changing the angle at which the OVD-forming media is observed (or by tilting the OVD-forming media while maintaining the observation angle).
[0126] In all the OVD-forming media of Examples 1 to 6, the structural period p of the relief structure was set to 10 μm and the depth d was set to 5 μm. In Examples 4 to 5, in which the thickness of the optical functional layer exceeded the depth of the relief structure of 5 μm, good color tone change was not obtained. This is believed to be because the unevenness was not properly maintained on the surface side of the optical functional layer. In addition, the OVD-forming media of Example 6, which was manufactured using MXene-aqueous dispersion B, did not obtain good color tone change. This is believed to be because the in-plane dimension of the MXene (particles), which is a particle of a two-dimensional material, was about 3 μm in the OVD-forming media of Example 6, which was relatively close to the structural period of the relief structure of 10 μm. On the other hand, the OVD-forming media of Examples 1 to 3, which were manufactured using MXene-aqueous dispersion A and in which the thickness of the optical functional layer was set to the depth of the relief structure of less than 5 μm, showed excellent color tone change. The reason for this is believed to be that in the OVD forming media of Examples 1 to 3, the in-plane dimensions of the MXene (particles), which is a two-dimensional material particle, were approximately 0.5 μm, which was less than 1 / 4 of the structural period of the relief structure of 10 μm, so that the optical functional layer could be formed along the recesses of the periodic structure with a thickness less than the depth of the relief structure, and the unevenness could be properly maintained on the surface side of the optical functional layer.
[0127] It was confirmed that the OVD-forming medium of Example 1, in which the thickness of the optical functional layer was extremely thin, had transparency. On the other hand, the OVD-forming media of Examples 2 to 6, in which the thickness of the optical functional layer was relatively thick, did not have transparency, but it was confirmed that they reflected light when light was irradiated from the front side (direction A side) of the OVD-forming medium.
[0128] (Examples 7 to 10) Examples 7 to 10 relate to embodiments in which an optical functional layer is formed by spraying in an ejection direction E at an angle of 90 degrees to the substrate as shown in FIG. 3, and in an ejection direction E at an angle of less than 90 degrees to the substrate as shown in FIG. 5.
[0129] [Preparation of MXene-water dispersion A] The above-mentioned MXene-water dispersion A was used.
[0130] [Manufacture of OVD forming medium] The OVD forming medium of Example 7 was manufactured in the same manner as in Example 2, with the optical functional layer having a thickness of about 1 μm. That is, in Example 7, similar to Example 2, spraying was performed in a discharge direction E at an angle of 90 degrees (vertically) with respect to the substrate.
[0131] The OVD forming media of Examples 8 to 10 were produced in the same manner as in Example 7, except that the spraying was performed with the discharge direction E at angles of 60 degrees, 45 degrees, and 30 degrees, respectively, relative to the substrate.
[0132] [Evaluation of OVD forming media, etc.] For the OVD forming media of Examples 7 to 10 produced as described above, the thickness of the optical functional layer was measured and further the partial transmittance was evaluated as follows.
[0133] (Thickness of optical function layer) For the substrate on which the optical functional layer was formed, FIB processing was performed at three locations in the first portion covering the inclined upper surface of the relief structure to expose the optical functional layer and the relief structure portion of the substrate below it. The cross sections of each location were observed with an SEM to obtain SEM observation images of a total of three fields of view, and the thickness of the optical functional layer was measured at five or more locations per field of view, and the average value of these measurements was defined as the thickness t1 of the optical functional layer.
[0134] In addition, FIB processing was performed at three locations on the second portion covering the wall surface of the relief structure of the substrate on which the optical functional layer was formed, to expose the optical functional layer and the relief structure portion of the substrate below it, and the cross sections of each location were observed with an SEM to obtain SEM observation images of a total of three fields of view. The thickness of the optical functional layer was measured at five or more locations per field of view, and the average value of these measurements was taken as the thickness t2 of the optical functional layer.
[0135] Furthermore, the thickness ratio was calculated as t2 / t1×100(%).
[0136] (partially transparent) As shown in FIG. 7, a paper with a lattice pattern drawn on it was used as a base layer 23, and an OVD-forming medium (see the OVD-forming medium 20' described above with reference to FIG. 4) was placed on top of it so that its back side was in contact with the paper surface with the lattice pattern drawn on it. Light was irradiated from the front side (A direction side) of the OVD-forming medium, and visual observation was performed to check whether the appearance of the lattice pattern under the OVD-forming medium changed when the observation direction and / or angle was changed as the viewing condition from the front side of the OVD-forming medium. When the lattice pattern was not visible, partial transmittance was "absent," and when the lattice pattern was visible or not depending on the observation direction and / or angle, partial transmittance was "present." In this evaluation, the presence of partial transmittance means that the optical functional layer functions as a light reflecting layer or a light transmitting layer by changing the observation direction and / or angle during visual observation.
[0137] The results are shown in Table 3.
[0138] [Table 3]
[0139] As can be seen from Table 3, the thickness ratio decreased as the spray discharge angle was reduced, and the thickness t2 of the second portion of the optical functional layer that covers the wall surface of the relief structure could be reduced. The reason for this is believed to be that the smaller the spray discharge angle, the less mist (and therefore particles) wraps around the wall surface of the relief structure. In the OVD forming media of Examples 9 and 10, the thickness t2 of the optical functional layer was 250 nm and 150 nm, respectively, which is extremely thin, and therefore partial transparency was obtained. The layer of MXene is very thin, and even if about 100 layers are deposited, the thickness is only several hundred nm, and light can be transmitted through it.
[0140] In particular, the OVD-forming medium of Example 10 (corresponding to the OVD-forming medium 20' described above with reference to FIG. 4) was able to present different visual effects depending on the viewing conditions (the direction and / or angle of observation). Specifically, when observed from the A direction side (top side) of FIG. 4(a) and the viewing direction was the C direction (angle θ=greater than 0 degrees and less than 90 degrees) shown in FIG. 4(a), the lattice pattern of the paper (underlying layer) present under the OVD-forming medium was not confirmed as shown in FIG. 8, and a metallic luster was observed over the entire surface due to the reflection of light by the optical function layer. On the other hand, when the viewing direction was the C' direction (angle θ'=greater than 0 degrees and less than about 45 degrees, preferably less than about 20 degrees) shown in FIG. 4(a), the lattice pattern of the paper (underlying layer) present under the OVD-forming medium was confirmed over the entire surface as shown in FIG. 9. That is, the optical function layer of the OVD-forming medium did not exhibit transparency in the C direction, but exhibited transparency in the C' direction. In addition, in Figures 8 and 9, for ease of understanding, the edge of the inclined upper surface of the relief structure corresponding to the structural period p' is shown by a solid line, as in Figure 4(b), but it should be noted that in reality, since the structural period p' is extremely small, such an edge is difficult to observe with the naked eye.
[0141] 9 shows an example in which the optical functional layer is colorless and transparent when viewed along the C' direction in Example 10. However, the examples of the present invention are not limited to such examples, and for example, as a modified example of Examples 9 to 10, the optical functional layer may be colored and transparent when viewed along the C' direction as shown in FIG. 10, depending on the material and / or thickness t2 of the optical functional layer.
[0142] In addition, in Example 10, when viewed along the C direction, the pattern (lattice pattern) of the underlayer was not confirmed because the thickness t1 of the optical functional layer was relatively thick (FIG. 8), and it was confirmed that the optical functional layer exhibited transparency only when viewed along the C' direction (FIG. 9). However, the examples of the present invention are not limited to such examples, and for example, as a modified example of Examples 9 to 10, the material and / or thickness t1 of the optical functional layer may be selected so that the optical functional layer exhibits transparency when viewed along the C direction (typically, the thickness t1 of the optical functional layer is suppressed to a value equal to or less than the size at which the optical functional layer exhibits transparency when viewed along the C direction, for example, about 0.5 μm or less), thereby producing an optical functional layer in which the transparency (transparency) of the pattern of the underlayer (lattice pattern in the illustrated example) differs depending on the viewing direction and / or viewing angle, as shown in FIG. 11(a)(b). Figure 11(a) shows a case where the optical functional layer is transmissive but has low transparency when viewed along the C direction, and Figure 11(b) shows a case where the optical functional layer is transmissive and has higher transparency when viewed along the C' direction.
[0143] Therefore, by appropriately designing the shape, dimensions, pattern, design, etc. of the relief structure and the thickness distribution of the optical function layer and forming them precisely, it is possible to realize a variety of OVD functions according to the viewing conditions (e.g., the observation direction / angle). [Industrial Applicability]
[0144] The OVD forming medium of the present invention can be used in security technologies such as forgery / anti-copying, and also can be used for various other purposes due to its high design / decorative properties. [Explanation of symbols]
[0145] 1a, 1b layer body (M m X n layer) 3a, 5a, 3b, 5b Modified or terminal T 7a, 7b MXene layers 10 2D materials 10a, 10b MXene (layered material) 11 Base material 11a Surface (relief surface) 11b Back side 15 Optical functional layer 17 Overcoat layer 20 OVD forming media 21 Nozzle 23 Base layer 25 Object 30 Goods
Claims
1. A substrate having a relief structure on a surface thereof; an optical functional layer covering the relief structure; 1. An OVD forming medium comprising: the two-dimensional material is a layered material comprising one or more layers; The one or more layers may have the following formula: M m X n wherein M is at least one Group 3, 4, 5, 6, or 7 metal; X is a carbon atom, a nitrogen atom, or a combination thereof; n is 1 or more and 4 or less, m is greater than n and is equal to or less than 5. and a modification or terminal T (T is at least one selected from the group consisting of a hydroxyl group, a fluorine atom, a chlorine atom, and an oxygen atom) present on the surface of the layer body, An OVD forming medium, wherein the optical functional layer includes a first portion and a second portion, the ratio of the thickness of the second portion to the thickness of the first portion is 20% or less (except when it is 0%), and the optical functional layer has partial transparency.
2. The OVD forming medium according to claim 1 , wherein the content of the particles of the two-dimensional material in the optical functional layer is 50% by volume or more.
3. 3. The OVD forming medium according to claim 1, wherein the optically functional layer has a thickness of 3 μm or less.
4. 4. The OVD forming medium according to claim 1, wherein the optical functional layer functions as a light reflecting layer or a light transmitting layer either constantly or depending on viewing conditions.
5. An article comprising an OVD forming medium according to any one of claims 1 to 4.
6. A method for producing an OVD forming medium, comprising the steps of: (a) providing a substrate having a relief structure thereon; (b) applying a liquid comprising particles of a two-dimensional material and a liquid medium onto the relief structure to form an optically functional layer covering the relief structure and comprising particles of the two-dimensional material; Including, the two-dimensional material is a layered material comprising one or more layers; The one or more layers may have the following formula: M m X n wherein M is at least one Group 3, 4, 5, 6, or 7 metal; X is a carbon atom, a nitrogen atom, or a combination thereof; n is 1 or more and 4 or less, m is greater than n and is equal to or less than 5. and a modification or terminal T (T is at least one selected from the group consisting of a hydroxyl group, a fluorine atom, a chlorine atom, and an oxygen atom) present on the surface of the layer body, The (b) is (b1) applying the liquid material onto the relief structure by spraying the liquid material with a discharge direction at an angle of 45 degrees or less with respect to the substrate to form a precursor of the optical function layer; and (b2) drying the precursor Including, A manufacturing method in which the optical functional layer includes a first portion and a second portion, the ratio of the thickness of the second portion to the thickness of the first portion is 20% or less (except when it is 0%), and the optical functional layer has partial transparency.
Citation Information
Patent Citations
OVD medium, information print having OVD medium attached thereto and manufacturing method of OVD medium
JP2008107483A
Display body and article with label
JP2009080201A
Color image print medium, article including the same, and printing method
JP2018120010A
Physical Forms of MXene Materials Exhibiting Novel Electrical and Optical Characteristics
US20170294546A1
Security device comprising a printed metal layer in form of a pattern and methods for its manufacture
WO2010049676A1