Method for manufacturing light-emitting element

By forming a protective layer and annealing the semiconductor wafer to reduce resistance, the method addresses leakage current issues in light emitting devices, enhancing their efficiency and performance.

JP7590680B2Active Publication Date: 2024-11-27NICHIA CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024024363
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2016-12-16
Filing Date
2024-02-21
Publication Date
2024-11-27
Estimated Expiration
2037-09-07

AI Technical Summary

Technical Problem

Existing light emitting devices suffer from high leakage current due to damage during the wafer division process, which affects their performance and efficiency.

Method used

A manufacturing method that includes forming a protective layer on the p-side nitride semiconductor layer at the planned dividing line, annealing to reduce resistance in unprotected regions, and using laser irradiation to minimize damage, thereby reducing leakage current and increasing the light emitting area.

Benefits of technology

The method results in a light emitting device with reduced leakage current and increased light emitting area, improving luminous efficiency and forward voltage performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590680000001
    Figure 0007590680000001
  • Figure 0007590680000002
    Figure 0007590680000002
  • Figure 0007590680000003
    Figure 0007590680000003
Patent Text Reader

Abstract

To provide a method for manufacturing a light-emitting element, which can reduce the occurrence of leak current.SOLUTION: A method for manufacturing a light-emitting element comprises the steps of: preparing a semiconductor wafer having a substrate, an n-side nitride semiconductor layer including an n-type impurity, and a p-side nitride semiconductor layer including a p-type impurity from its downside toward the upside in turn; applying a laser beam to the substrate, thereby forming each processed and modified portion in the substrate; and dividing the semiconductor wafer with the processed and modified portions formed in the substrate to obtain a plurality of light-emitting elements. The method further comprises the steps of: forming a protection layer in a region including boundaries of regions, which make the plurality of light-emitting elements, in an upper face of the p-side nitride semiconductor layer; and annealing the semiconductor wafer, thereby lowering the resistance of the p-side nitride semiconductor layer in a region where the protection layer is not formed in turn, provided that the steps are arranged between the step of preparing the semiconductor wafer and the step of forming the processed and modified portion in the substrate.SELECTED DRAWING: Figure 5B
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for manufacturing a light-emitting device. [Background technology]

[0002] The light-emitting element can be obtained by dividing a semiconductor wafer including a substrate and a semiconductor portion having an n-side nitride semiconductor layer and a p-side nitride semiconductor layer in this order from the upper surface side of the substrate. As a method for dividing these semiconductor wafers, a method is known in which a laser beam is irradiated into the substrate to form a processing-affected portion and then the substrate is divided. In this case, the n-side nitride semiconductor layer is exposed by removing an area of ​​the semiconductor portion that overlaps with the planned dividing line of the semiconductor wafer from above by etching, and a protective layer may be formed on the surface of the removed portion. This can prevent the debris generated when dividing the semiconductor wafer from adhering to the surface exposed by etching, and therefore can prevent leakage current from flowing through the debris. (For example, Patent Document 1) [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent Publication No. 2005-166728 Summary of the Invention [Problem to be solved by the invention]

[0004] In the light-emitting element of Patent Document 1, there is room for further reduction in the occurrence of leakage current. [Means for solving the problem]

[0005] A method for manufacturing a light-emitting element, comprising the steps of: preparing a semiconductor wafer having, in order from bottom to top, a substrate, an n-side nitride semiconductor layer containing an n-type impurity, and a p-side nitride semiconductor layer containing a p-type impurity; forming a processed-altered portion in the substrate by irradiating the substrate with a laser beam; and obtaining a plurality of light-emitting elements by dividing the semiconductor wafer having the processed-altered portion formed in the substrate, the method for manufacturing a light-emitting element comprising the steps of: forming a protective layer in a region including boundaries between regions that will become the plurality of light-emitting elements on an upper surface of the p-side nitride semiconductor layer; and annealing the semiconductor wafer to reduce the resistance of the p-side nitride semiconductor layer in a region where the protective layer is not formed, between the steps of preparing the semiconductor wafer and forming the processed-altered portion in the substrate. Effect of the Invention

[0006] According to such a manufacturing method, a light emitting device in which the occurrence of leakage current is reduced can be manufactured, and a light emitting device in which the occurrence of leakage current is reduced can be provided. [Brief description of the drawings]

[0007] [Figure 1A] 5A to 5C are schematic plan views for explaining a manufacturing method of a light emitting device according to the embodiment. [Figure 1B] FIG. 1B is a schematic cross-sectional view taken along line AA in FIG. 1A. [Figure 2A] 5A to 5C are schematic plan views for explaining a manufacturing method of a light emitting device according to the embodiment. [Figure 2B] FIG. 2B is a schematic cross-sectional view taken along line AA in FIG. 2A. [Figure 3A] 5A to 5C are schematic plan views for explaining a manufacturing method of a light emitting device according to the embodiment. [Figure 3B] FIG. 3B is a schematic cross-sectional view taken along line AA in FIG. 3A. [Figure 4A] 5A to 5C are schematic plan views for explaining a manufacturing method of a light emitting device according to the embodiment. [Figure 4B] FIG. 4B is a schematic cross-sectional view taken along line AA in FIG. 4A. [Figure 5A] 5A to 5C are schematic plan views for explaining a manufacturing method of a light emitting device according to the embodiment. [Figure 5B] FIG. 5B is a schematic cross-sectional view taken along line AA in FIG. 5A. [Figure 6A] 5A to 5C are schematic plan views for explaining a manufacturing method of a light emitting device according to the embodiment. [Figure 6B] FIG. 6B is a schematic cross-sectional view taken along line AA in FIG. 6A. [Figure 7A] 11A to 11C are schematic plan views for explaining a manufacturing method for a light-emitting element according to a comparative example. [Figure 7B] FIG. 7B is a schematic cross-sectional view taken along line AA in FIG. 7A. [Figure 8] 4 is a graph showing the results of measuring the reverse current value of the light-emitting element according to Example 1. [Figure 9] 13 is a graph showing the results of measuring the reverse current value of the light-emitting element according to Example 2. [Figure 10] 13 is a graph showing the results of measuring the reverse current value of the light-emitting element according to Example 3. [Figure 11] 11 is a graph showing the results of measuring the reverse current value of a light-emitting element according to a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Hereinafter, the embodiments and examples of the present invention will be described with reference to the drawings. However, the embodiments and examples shown below are merely illustrative of configurations for embodying the technical ideas of the present invention, and do not specify the present invention. Furthermore, in the following description, the same names and symbols indicate the same or similar components, and detailed descriptions will be omitted as appropriate.

[0009] [Embodiment 1] In the manufacturing method of the light emitting device 100 according to the present embodiment, first, as shown in FIG. 1A and FIG. 1B, a semiconductor wafer 1 having a substrate 11, an n-side nitride semiconductor layer 12n containing an n-type impurity, and a p-side nitride semiconductor layer 12p containing a p-type impurity in this order from bottom to top is prepared (hereinafter, a region including the "n-side nitride semiconductor layer 12n" and the "p-side nitride semiconductor layer 12p" provided on the substrate 11 is referred to as a "semiconductor portion 12"). Next, as shown in FIG. 3A and FIG. 3B, a protective layer 14 is formed in a region including a boundary between regions that will become a plurality of light emitting devices 100 on the upper surface of the p-side nitride semiconductor layer 12p (hereinafter, the boundary between regions that will become a plurality of light emitting devices 100 is also referred to as a "planned division line 13"). Note that the protective layer for maintaining the p-side nitride semiconductor layer 12p with high resistance, indicated by the reference numeral 14, is referred to as a "first protective layer 14", and the protective layer for protecting the upper surface of the light emitting device 100, indicated by the reference numeral 18 described later, is sometimes referred to as a "second protective layer 18". In addition, in FIG. 3A, in order to simplify the description in the drawings, the regions of the semiconductor wafer 1 that will later become the four light emitting elements 100 are described. This point is the same in the schematic plan views in FIG. 2A to FIG. 5A and FIG. 7A. Next, as shown in FIG. 4A and FIG. 4B, the semiconductor wafer 1 is annealed (heat treated) to reduce the resistance of the p-side nitride semiconductor layer 12p in the region where the first protective layer 14 is not formed. In the region of the p-side nitride semiconductor layer 12p where the first protective layer 14 is not formed, hydrogen that inactivates the p-type impurity is separated from the p-type impurity by annealing, whereas in the region of the p-side nitride semiconductor layer 12p where the first protective layer 14 is formed, hydrogen that inactivates the p-type impurity is less likely to be separated from the p-type impurity. Therefore, it is presumed that the resistance of the p-side nitride semiconductor layer 12p can be reduced in the region where the first protective layer 14 is not formed, while the resistance of the p-side nitride semiconductor layer 12p is kept high in the region where the first protective layer 14 is formed. 5A and 5B, a laser beam L is irradiated onto the substrate 11 to form a processed and altered portion in the substrate 11. Then, the semiconductor wafer 1 in which the processed and altered portion is formed in the substrate 11 is divided to obtain a plurality of light-emitting elements 100 as shown in FIGS. 6A and 6B.

[0010] 6A and 6B, a high-resistance portion 12x corresponding to a part of the p-side nitride semiconductor layer 12p is disposed on the side surface of the obtained light-emitting element 100, so that even if debris generated when dividing the semiconductor wafer 1 adheres to the side surface of the light-emitting element 100, it is possible to reduce biased flow of current, which should flow more or less evenly throughout the entire low-resistance p-side nitride semiconductor layer 12p and the n-side nitride semiconductor layer 12n located immediately below it, through the debris. Note that, hereinafter, biased flow of current, which should flow more or less evenly throughout a certain region of the semiconductor portion 12, in a specific region such as a damaged region, is referred to as "a leakage current occurs" or "a current leaks".

[0011] Since the energy of the laser light L is larger as it approaches the optical axis of the laser light L, typically, damage by the laser light L is likely to occur in the region overlapping the planned division line 13. However, in this embodiment, since the high resistance portion 12x is disposed in the region overlapping the planned division line 13, even if damage occurs in that region, the possibility of leakage current due to the damage is low.

[0012] Furthermore, the inventors have found, as a result of intensive research, that when the region of the semiconductor portion 12 overlapping with the planned dividing line 13 is removed by etching as in the conventional technology shown in Figs. 7A and 7B, the laser light L is likely to concentrate on the corners and their vicinity (hereinafter referred to as "corners, etc. 21") defined by the side of the recess 20 of the semiconductor portion 12 formed by etching and the upper surface of the semiconductor portion 12. Although the detailed reason why the energy of the laser light L is concentrated on the corners, etc. 21 is unclear, it is considered that the laser light L is likely to be concentrated on the corners, etc. 21 when the recess 20 is formed in the semiconductor portion 12 due to reflection and refraction. In other words, when the recess 20 is formed in the semiconductor portion 12 as in the conventional technology, if the region of the semiconductor portion 12 to be removed is not sufficiently large, the corners, etc. 21 of the semiconductor portion 12 may be damaged, and current may leak. However, in this embodiment, the recess 20 is not formed in the semiconductor portion 12. In other words, in this embodiment, the upper surface of the semiconductor portion 12 is substantially flat and the semiconductor portion 12 does not have corners 21, so there is no risk of damage occurring at the corners 21 and current leaking due to that damage.

[0013] Also, in the conventional technology, if the area where the semiconductor part 12 is removed is made sufficiently large, the corners 21 etc. are not damaged, but the light emitting area in one semiconductor wafer is reduced. However, in this embodiment, since the corners 21 etc. do not exist, the light emitting area in one semiconductor wafer 1 can be made larger. Therefore, in this embodiment, when the size of one light emitting element is made the same as in the conventional technology, the light emitting area in one light emitting element 100 can be made larger, so that the light emission output can be increased and the forward voltage (hereinafter also referred to as "Vf") can be reduced. Also, in the case where the size of the light emitting area in one light emitting element is made the same as in the conventional technology, the area that does not contribute to light emission can be reduced in this embodiment, so that the number of light emitting elements 100 that can be taken from one semiconductor wafer 1 can be increased.

[0014] Each step will be described below in order.

[0015] (Semiconductor wafer preparation process) First, as shown in Figs. 1A and 1B, a semiconductor wafer 1 is prepared which has, in order from bottom to top, a substrate 11, an n-side nitride semiconductor layer 12n containing n-type impurities, and a p-side nitride semiconductor layer 12p containing p-type impurities. Hereinafter, a case where an active layer 12a is provided between the n-side nitride semiconductor layer 12n and the p-side nitride semiconductor layer 12p will be described. Hereinafter, the n-side nitride semiconductor layer 12n, the active layer 12a, and the p-side nitride semiconductor layer 12p may be collectively referred to as the semiconductor section 12. Each layer constituting the semiconductor section 12 may include, for example, In X Al Y Ga 1-X-Y A nitride semiconductor such as N (0≦X, 0≦Y, X+Y≦1) can be used. As the n-type impurity, for example, Si can be used, and as the p-type impurity, for example, Mg can be used. As the substrate 11, an insulating substrate such as sapphire, or a conductive substrate such as GaN, SiC, ZnS, ZnO, GaAs, or Si can be used. On the upper surface of the substrate 11, a low-temperature grown buffer layer or the like may be formed as an underlayer.

[0016] In this specification, based on the interface between the p-side nitride semiconductor layer 12p and the n-side nitride semiconductor layer 12n or the active layer 12a, the side of the semiconductor portion 12 on which the p-electrode is provided is referred to as the p-side nitride semiconductor layer 12p, and the side of the semiconductor portion 12 on which the n-electrode is provided is referred to as the n-side nitride semiconductor layer 12n.

[0017] 2A and 2B, from the state shown in FIG. 1A and FIG. 1B, a part of the semiconductor portion 12 is etched from the p-side nitride semiconductor layer 12p side to expose the n-side nitride semiconductor layer 12n, thereby forming a region for providing the n-pad electrode 16 in a later process. At this time, a region of the p-side nitride semiconductor layer 12p that overlaps with the planned dividing line 13 of the semiconductor wafer 1 is not etched. When a part of the semiconductor part 12 is etched from the side of the p-side nitride semiconductor layer 12p to expose the n-side nitride semiconductor layer 12n, a potential difference occurs on the upper surface of the light emitting element 100. Therefore, when the semiconductor part 12 is etched and then the current diffusion layer 15 described below is formed, migration may occur due to the potential difference depending on the material of the current diffusion layer 15 (e.g., Ag, etc.). Therefore, when such a material is used as the current diffusion layer 15, it is preferable to etch the semiconductor part 12 after forming the current diffusion layer 15. This allows, for example, the semiconductor part 12 to be removed after the current diffusion layer 15 is covered with a cover layer, so that migration of the current diffusion layer 15 due to the potential difference can be suppressed.

[0018] (Protective layer forming process) Next, as shown in FIG. 3A and FIG. 3B, a first protective layer 14 is formed on the upper surface of the p-side nitride semiconductor layer 12p in an area overlapping the planned dividing lines 13 of the semiconductor wafer 1. The planned dividing lines 13 of the semiconductor wafer 1 may be extended so that the light emitting element 100 has an arbitrary shape when the semiconductor wafer 1 is divided in a later step, and typically, as shown in FIG. 3A, the planned dividing lines 13 may be formed in a lattice shape when viewed from above. By forming the planned dividing lines 13 of the semiconductor wafer 1 in a lattice shape, the light emitting element 100 having a rectangular shape when viewed from above can be obtained. As another shape of the light emitting element 100, a hexagonal shape when viewed from above can be used. The first protective layer 14 may have any shape as long as it is formed in an area overlapping the planned dividing lines 13 of the semiconductor wafer 1, but when the planned dividing lines 13 of the semiconductor wafer 1 are lattice-shaped, the first protective layer 14 can also be formed in a lattice shape so as to overlap these lattice-shaped planned dividing lines 13. This makes it possible to suppress leakage current from flowing on all side surfaces of the rectangular light emitting element 100.

[0019] The first protective layer 14 can be made of SiO2, SiN, SiON, Al2O3, ZnO, ZrO2, TiO2, Nb2O5, Ta2O5, or the like, and typically made of SiO2. The first protective layer 14 can be formed by depositing a material to become the first protective layer 14 on the semiconductor wafer 1 using a CVD or sputtering device or the like.

[0020] The thickness of the first protective layer 14 is preferably 0.01 μm or more, and more preferably 0.2 μm or more. This can more reliably prevent the p-side nitride semiconductor layer 12p from becoming low-resistance in the region where the first protective layer 14 is formed. The thickness of the first protective layer 14 is preferably 1 μm or less, and more preferably 0.5 μm or less. This can prevent cracks from occurring in the first protective layer 14.

[0021] When viewed from above, the width in the short-side direction of the first protective layer 14 (the width in the direction perpendicular to the planned division lines 13) is preferably 1 μm or more, and more preferably 5 μm or more. This makes it possible to more reliably divide the semiconductor wafer 1 into a plurality of light-emitting elements 100 directly below the first protective layer 14. When viewed from above, the width in the short-side direction of the first protective layer 14 (the width in the direction perpendicular to the planned division lines 13) is preferably 50 μm or less, more preferably 20 μm or less, and even more preferably 15 μm or less. This makes it possible to ensure a large low-resistance region in the p-side nitride semiconductor layer 12p.

[0022] After the first protective layer 14 is formed, the current diffusion layer 15 can be formed in a region of the upper surface of the p-side nitride semiconductor layer 12p where the first protective layer 14 is not formed, including the vicinity of the region where the first protective layer 14 is formed. Here, after the first protective layer 14 is formed, the current diffusion layer 15 is provided on substantially the entire upper surface of the p-side nitride semiconductor layer 12p where the first protective layer 14 is not formed. Here, the vicinity of the region where the first protective layer 14 is formed refers to a region within 20 μm from the first protective layer 14. This can make the current density distribution in the plane of the light emitting element 100 more uniform, thereby improving the light emitting efficiency of the light emitting element 100. The timing of providing the current diffusion layer 15 may be, for example, before the first protective layer 14 is formed, or after a process of reducing the resistance of the p-side nitride semiconductor layer 12p described later.

[0023] By providing the current spreading layer 15 after the process of reducing the resistance of the p-side nitride semiconductor layer 12p, even if a specific material suppresses the reduction in resistance of the p-side nitride semiconductor layer 12p, it can be used as the current spreading layer 15.

[0024] The electrode diffusion layer can be made of a conductive metal oxide such as ITO, ZnO, or In2O3. When the current diffusion layer 15 is also used as a reflective layer, Ag or the like can be used. The current diffusion layer 15 can be provided by depositing a material to be the current diffusion layer 15 on the upper surface of the p-side nitride semiconductor layer 12p using, for example, a sputtering device.

[0025] In top view, the distance between the current diffusion layer 15 and the first protective layer 14 is preferably 0 μm or more, and more preferably 2 μm or more. By providing a certain distance between them, the absorption of light by the current diffusion layer 15 in the outer periphery of the light emitting element 100 that emits weak light can be reduced, and the light extraction efficiency can be improved. In top view, the distance between the current diffusion layer 15 and the first protective layer 14 is preferably 20 μm or less, and more preferably 10 μm or less. This allows the area of ​​the current diffusion layer 15 in the light emitting element 100 to be increased, and therefore Vf can be reduced.

[0026] (Process for reducing the resistance of the p-side nitride semiconductor layer) Next, the semiconductor wafer 1 is annealed to reduce the resistance of the p-side nitride semiconductor layer 12p in the region where the first protective layer 14 is not formed. As a result, the p-side nitride semiconductor layer 12p in the region where the first protective layer 14 is formed is maintained to have a high resistance, and forms the high resistance portion 12x. Therefore, even if debris scattered from the end face of the semiconductor wafer 1 adheres to the side surface of the light emitting element 100 when the semiconductor wafer 1 is divided along the planned division line 13, it is possible to suppress a current from flowing between the p-side nitride semiconductor layer 12p and the n-side nitride semiconductor layer 12n through the debris. In FIG. 4A and FIG. 4B, for ease of understanding, the region of the p-side nitride semiconductor layer 12p corresponding to the high resistance portion 12x that is maintained to have a high resistance is indicated by diagonal lines, and the same is true in FIG. 5A to FIG. 6B.

[0027] The annealing is preferably performed in an atmosphere substantially free of hydrogen. Typically, the annealing is preferably performed in a nitrogen atmosphere. The temperature at which the semiconductor wafer 1 is annealed is preferably 350° C. to 600° C. The time for which the semiconductor wafer 1 is annealed is preferably 10 minutes to 60 minutes. This allows the resistance of the p-side nitride semiconductor layer to be efficiently reduced.

[0028] Next, as shown in FIG. 5A and FIG. 5B, an n-pad electrode 16 and a p-pad electrode 17 are formed on the semiconductor portion 12. In this embodiment, the second protective layer 18 covers substantially the entire upper surface of the semiconductor wafer 1, except for a portion of the upper surfaces of the n-pad electrode 16 and the p-pad electrode 17. The second protective layer 18 can be formed so as to cover the first protective layer 14, or can be formed after removing the first protective layer 14. The second protective layer 18 can be made of SiO2, SiN, SiON, Al2O3, ZnO, ZrO2, TiO2, Nb2O5, Ta2O5, or the like, and typically, SiO2 can be used. The second protective layer 18 can be formed by depositing a material to be the second protective layer 18 on the semiconductor wafer 1 using a CVD or sputtering device, or the like.

[0029] (Laser light irradiation process) Next, as shown in Figures 5A and 5B, a region of the substrate 11 corresponding to the planned dividing line 13 is irradiated with laser light L. At this time, the laser light L is condensed and irradiated so as to be focused on the inside of the substrate 11. This makes it possible to generate a processing-affected portion in the substrate 11 that serves as a starting point for dividing the semiconductor wafer 1, making it easier to divide the semiconductor wafer 1 in a later process. In order to minimize damage to the semiconductor portion 12, it is preferable to irradiate the laser light L from the substrate 11 side of the semiconductor wafer 1, i.e., from the lower surface side of the semiconductor wafer 1.

[0030] The laser processing machine that emits the laser light L may be any machine capable of forming a processed altered portion. Specifically, a fiber laser, a CO2 laser, a YAG laser, or the like may be used. The wavelength of the laser light L may be 200 nm to 5000 nm, and preferably 360 nm to 2000 nm. The pulse width of the laser light L may be 10 fsec to 10 μsec, and preferably 100 fsec to 1 nsec. The output of the laser light L is preferably 0.01 W to 10 W.

[0031] In this embodiment, unlike the conventional method, the recess 20 is not formed in the semiconductor part 12 in the region overlapping with the planned division line 13 in top view, so that no corners or the like 21 exist. Therefore, when the width of the recess 20 in the direction perpendicular to the planned division line 13 when forming the recess 20 in the semiconductor part 12 as in the conventional method and the width of the first protective layer 14 in the direction perpendicular to the planned division line 13 when forming the first protective layer 14 without forming the recess 20 in the semiconductor part 12 as in this embodiment are the same, if the region to be irradiated with the laser light L is brought close to the semiconductor part 12 in the former (conventional method) and the latter (present embodiment), the latter (present embodiment) is less likely to be damaged than the former (conventional method). Therefore, in the latter (present embodiment), the irradiation position of the laser light L can be brought closer to the semiconductor part 12.

[0032] On the other hand, when dividing the semiconductor wafer 1, depending on the crystal orientation of the substrate 11, the semiconductor wafer 1 may be divided at an angle from the processing-affected portion formed by the laser light L, rather than perpendicular to the parallel upper and lower surfaces of the semiconductor wafer 1. In this case, depending on the degree of deviation from the planned dividing line 13, the obtained light-emitting device 100 may be a defective product.

[0033] However, as described above, in this embodiment, the region of the substrate 11 to be irradiated with the laser light L, i.e., the region where the processed-altered portion is to be formed, can be brought closer to the semiconductor portion 12 than in the conventional case. The region where the processed-altered portion is to be formed can be, for example, a region above half the thickness of the substrate 11. This can reduce deviation from the planned dividing line 13, and is expected to improve the yield.

[0034] The position where the processed-altered portion is formed on the substrate 11 (the position in the thickness direction of the substrate 11) does not have to be one, and the processed-altered portion can be formed at multiple positions. In this way, the semiconductor wafer 1 can be divided relatively easily even if the substrate 11 is thick. When the processed-altered portions are formed at multiple positions on the substrate 11, the deviation from the planned dividing line 13 can be reduced if, for example, the processed-altered portion closest to the semiconductor portion 12 is in a region above half the thickness of the substrate 11. Furthermore, by bringing the region where the processed-altered portion is formed closer to the semiconductor portion 12, it is possible to make the light emitted from the semiconductor portion 12 toward the substrate 11 reach the processed-altered portion relatively quickly when the light-emitting element 100 is caused to emit light. This allows more light to be reflected by the processed-altered portion, the surface of which has been roughened by the laser light L, thereby improving the amount of light extracted from the light-emitting element 100. At this time, when the process-altered portion is formed at a plurality of positions on the substrate 11 in the depth direction, the first process-altered portion is formed and the second process-altered portion is formed above the first process-altered portion. For example, the first process-altered portion is formed by irradiating the substrate 11 with the laser light L at a first pulse energy and a first pitch, and the second process-altered portion is formed by irradiating the substrate 11 with the laser light L at a second pulse energy smaller than the first pulse energy and a second pitch wider than the first pitch. As a result, the process-altered portion is formed close to the semiconductor portion 12, thereby improving the amount of light extraction and suppressing damage to the semiconductor portion 12 caused by the laser light L. In other words, in order to form a process-altered portion large enough to fracture the semiconductor wafer 1, it is necessary to irradiate the substrate 11 with the laser light L at a relatively large pulse energy and a relatively small pitch, but if such a process-altered portion is formed at a position relatively close to the semiconductor portion 12, there is a risk that the semiconductor portion 12 will be damaged. Therefore, by irradiating the substrate 11 with the laser light L at a second pulse energy smaller than the first pulse energy and a second pitch wider than the first pitch, damage to the semiconductor portion 12 caused by the laser light L can be suppressed compared to the case where the second processed-altered portion is formed with the same pulse energy and pitch as the first pulse energy and first pitch used to form the first processed-altered portion. When forming the first process-altered portion and the second process-altered portion, the first process-altered portion can be formed in a region below half the thickness of the substrate 11, and the second process-altered portion can be formed in a region above half the thickness of the substrate 11. This allows the process-altered portion to be formed closer to the semiconductor portion 12, thereby further improving the amount of light extracted, while further suppressing damage to the semiconductor portion 12 caused by the laser light L.

[0035] Furthermore, in this embodiment, since there are no corners 21, it is possible to irradiate the laser light L with stronger pulse energy than in the conventional case. This makes it easier to divide the semiconductor wafer 1 even if a relatively thick substrate 11 is used.

[0036] Specifically, the thickness of the substrate 11 can be set to 50 μm to 500 μm. The laser light L is preferably irradiated to a position 10 μm to 150 μm from the upper surface of the substrate 11, and more preferably 20 μm to 100 μm from the upper surface of the substrate 11. In other words, the process-affected portion is preferably formed at a position 10 μm to 150 μm from the upper surface of the substrate 11, and more preferably 20 μm to 100 μm from the upper surface of the substrate 11. This makes it possible to divide the semiconductor wafer 1 with high accuracy while suppressing damage to the semiconductor portion 12.

[0037] (Semiconductor wafer division process) Thereafter, the semiconductor wafer 1 is divided along the planned dividing lines 13 to obtain a plurality of light-emitting elements 100 as shown in Figures 6A and 6B. The semiconductor wafer 1 can be divided, for example, by pressing a roller, a blade, or the like against the lower surface of the substrate 11 to apply force.

[0038] [Embodiment 2] As shown in Fig. 6A and Fig. 6B, the light emitting device 100 according to this embodiment has a semiconductor structure including, in order from bottom to top, a substrate 11, an n-side nitride semiconductor layer 12n containing an n-type impurity, and a p-side nitride semiconductor layer 12p containing a p-type impurity. In the semiconductor structure, the p-side nitride semiconductor layer 12p side is the light extraction surface side, and the n-side nitride semiconductor layer 12n side is the mounting surface side. In other words, the light emitting device 100 is a face-up mounting type light emitting device. In addition, when viewed from above, the outer periphery of the p-side nitride semiconductor layer 12p has a higher resistance than the inside of the outer periphery of the p-side nitride semiconductor layer 12p. As a result, the high resistance portion 12x corresponding to a part of the p-side nitride semiconductor layer 12p is disposed on the side surface of the light emitting element 100, so that it is possible to suppress the occurrence of leakage current even if debris or the like that may be a leakage source is attached to the side surface of the light emitting element 100. Moreover, even if damage is caused to the high resistance portion 12x, it is possible to suppress the occurrence of leakage current due to the damage. In the light emitting device 100, the first protective layer 14 can be formed in a region of the upper surface of the p-side nitride semiconductor layer 12p corresponding to the outer periphery. When the semiconductor wafer 1 is annealed, the p-side nitride semiconductor layer 12p in the region where the first protective layer 14 is formed maintains high resistance, so that a high resistance portion 12x can be formed below the first protective layer 14. Note that the first protective layer 14 may be removed after the semiconductor wafer 1 is annealed. A second protective layer 18 can be formed above the semiconductor structure in a region including the upper surface of the first protective layer 14. This makes it possible to protect the upper surface of the light emitting element 100. A current diffusion layer 15 can be formed in a region of the upper surface of the p-side nitride semiconductor layer 12p that is inside the outer periphery and includes the vicinity of the outer periphery. Here, the current diffusion layer 15 is formed on substantially the entire upper surface of the p-side nitride semiconductor layer 12p in the region inside the outer periphery. Here, the vicinity of the outer periphery of the p-side nitride semiconductor layer 12p refers to a region that is 20 μm or less inward from the outer periphery. This makes it possible to make the current density distribution in the plane of the light emitting element 100 more uniform, thereby improving the light emitting efficiency of the light emitting element 100. In addition, the area through which the current flows in the plane of the light emitting element 100 can be relatively large, thereby improving the amount of light extracted from the light emitting element 100. A process-altered portion is formed on the side surface of the substrate 11. This allows the semiconductor wafer 1 to be easily divided, and therefore the light-emitting device 100 can be easily obtained. The process-altered portion can be formed above half the thickness of the substrate 11. This allows the deviation from the planned dividing line 13 when dividing the semiconductor wafer 1 to obtain the light-emitting device 100 to be reduced. Furthermore, by bringing the region where the process-altered portion is formed closer to the semiconductor portion 12, more light can be reflected by the process-altered portion, and therefore the amount of light extracted from the light-emitting device 100 can be improved. When the process-altered portions are formed at a plurality of positions on the substrate 11 in the depth direction, the process-altered portions can have a first process-altered portion formed at a first pitch and a second process-altered portion formed at a second pitch wider than the first pitch. The second process-altered portion can be formed above the first process-altered portion. This allows the process-altered portion to be formed closer to the semiconductor portion 12, thereby improving the amount of light extracted from the light-emitting element 100. In addition, the second process-altered portion is formed at a pitch wider than the pitch of the first process-altered portion, thereby suppressing damage to the semiconductor portion 12 caused by the laser light L. When the first process-altered portion and the second process-altered portion are formed, the first process-altered portion can be formed in a region below half the thickness of the substrate 11, and the second process-altered portion can be formed in a region above half the thickness of the substrate 11. This makes it possible to further improve the amount of light extracted by forming the process-altered portion closer to the semiconductor portion 12, while further suppressing damage to the semiconductor portion 12 caused by the laser light L. [Example 1] The present embodiment will be described with reference to FIGS. 1A to 6B.

[0039] First, as shown in FIG. 1A and FIG. 1B, an n-side nitride semiconductor layer 12n containing Si as an n-type impurity, an active layer 12a, and a p-side nitride semiconductor layer 12p containing Mg as a p-type impurity were laminated on a substrate 11 to obtain a semiconductor wafer 1. A sapphire substrate having a thickness of 800 μm was used as the substrate 11, and GaN, AlGaN, InGaN, or the like was formed as the n-side nitride semiconductor layer 12n, the active layer 12a, and the p-side nitride semiconductor layer 12p. Then, as shown in FIG. 2A and FIG. 2B, a part of the semiconductor part was etched from the side of the p-side nitride semiconductor layer 12p to expose the n-side nitride semiconductor layer 12n, thereby forming a region for providing an n-pad electrode 16 in a later process. In this etching of the p-side nitride semiconductor layer 12p, the region of the p-side nitride semiconductor layer 12p that overlaps with the planned dividing line 13 of the semiconductor wafer 1 was not etched.

[0040] Next, as shown in FIG. 3A and FIG. 3B, a first protective layer 14 made of SiO2 was formed to a thickness of about 0.3 μm on the upper surface of the p-side nitride semiconductor layer 12p in a region overlapping with the planned dividing lines 13 of the semiconductor wafer 1. The planned dividing lines 13 of the semiconductor wafer 1 were in a lattice shape when viewed from above, and the distance between adjacent planned dividing lines 13 was 650 μm. The width of the first protective layer 14 in the short direction was 20 μm. After that, ITO was formed as a current diffusion layer 15 to a thickness of about 0.1 μm on the substantially entire area of ​​the upper surface of the p-side nitride semiconductor layer 12p in the region where the first protective layer 14 was not formed. The distance between the current diffusion layer 15 and the first protective layer 14 was 6 μm.

[0041] Next, as shown in FIGS. 4A and 4B, the semiconductor wafer 1 was annealed in a nitrogen atmosphere at about 500° C. for 40 minutes to reduce the resistance of the p-side nitride semiconductor layer 12p in the region where the first protective layer 14 is not formed.

[0042] Next, as shown in FIG. 5A and FIG. 5B, a p-pad electrode 17 was formed on the current diffusion layer 15 formed on the upper surface of the p-side nitride semiconductor layer 12p, and an n-pad electrode 16 was formed on the exposed n-side nitride semiconductor layer 12n. As the p-pad electrode, Cr, Rh, Pt, and Au were laminated in this order. As the n-pad electrode, Ti, Al, Ti, Ru, Ti, Cr, Rh, Pt, and Au were laminated in this order. On almost the entire upper surface of the semiconductor wafer 1 except for the p-pad electrode 17 and the n-pad electrode 16, a second protective layer 18 made of SiO2 was formed to a thickness of about 0.2 μm. Then, the substrate 11 was polished from the lower surface side to a thickness of 150 μm.

[0043] 5A and 5B, a laser beam L was applied from the lower surface side of the substrate 11 to an area corresponding to the planned dividing lines 13 of the substrate 11. The laser beam L was applied to a position 100 μm from the upper surface of the substrate 11. As the laser beam L, a fiber laser having a wavelength of 1064 nm, a pulse width of about 1 psec, and an output of about 0.3 W was used.

[0044] Thereafter, the semiconductor wafer 1 was divided along the planned dividing lines 13 to obtain a plurality of light-emitting elements 100. The semiconductor wafer 1 was divided by applying a force along the planned dividing lines 13 of the semiconductor wafer 1 by pressing a roller against the lower surface side of the substrate 11.

[0045] As a result, 5,529 light-emitting elements 100 each having a rectangular shape with each side being 650 μm long were obtained, as shown in Figures 6A and 6B. A test was conducted on these light-emitting elements 100 to measure the current (hereinafter also referred to as "Ir") that flows when a voltage of 5 V is applied in the reverse direction. As a result, as shown in Figure 8, in Example 1, 39 light-emitting elements 100 had an Ir of 0.01 or more (occurrence rate 0.7%), and it was found that the leakage current was sufficiently suppressed.

[0046] [Example 2] 9 shows the test results of 5,542 light-emitting elements 100 according to Example 2, which were formed in the same manner as in Example 1, except that the width in the short side direction of the first protective layer 14 was set to 30 μm. As described above, in Example 2, 42 of the light-emitting elements 100 had Ir of 0.01 or more (incidence rate: 0.8%), demonstrating that the leakage current was sufficiently suppressed.

[0047] [Example 3] 10 shows the test results of the light emitting element 100 according to Example 3, which was formed in the same manner as in Example 1, except that the width in the short side direction of the first protective layer 14 was set to 40 μm. As described above, in Example 3, 36 light emitting elements 100 had Ir of 0.01 or more (incidence rate: 0.7%), and it was found that the leakage current was sufficiently suppressed.

[0048] [Comparative Example] As a comparative example, a light emitting device 200 was prepared which differed from Example 1 in that the region of the p-side nitride semiconductor layer 12p overlapping the planned dividing lines 13 of the semiconductor wafer 2 was etched. That is, in the semiconductor wafer 2, recesses 20 are formed in the semiconductor portion 12 by etching, and therefore corners and the like 21 are present.

[0049] 7A and 7B, in the comparative example, the width in the short direction of the recess 20 of the semiconductor portion is 50 μm. In other words, the outer periphery of the p-side nitride semiconductor layer 12p of the light emitting element 200 is etched by 25 μm.

[0050] In the comparative example, 4050 light-emitting elements 200 were fabricated, each of which was rectangular and had a side length of 650 μm. A test was conducted to measure the Ir that flowed when a voltage of 5 V was applied in the reverse direction to these light-emitting elements 200. As a result, as shown in Fig. 11, 599 of the light-emitting elements 200 in the comparative example had an Ir of 0.01 or more (occurrence rate: 14.8%), indicating that the leakage current was not sufficiently suppressed.

[0051] In the light emitting device 200 according to the comparative example, the width of the recess 20 in the short side direction is larger than the width of the first protective layer 14 in the short side direction in Examples 1 to 3. However, since the recess 20 is formed in the semiconductor portion 12 by etching, it is considered that the corners 21 of the semiconductor portion 12 are damaged by the laser light L, causing leakage current. On the other hand, in the light emitting device 100 in Examples 1 to 3, although the width of the protective layer 14 in the short side direction is smaller than the width of the recess 20 of the light emitting device 200 in the short side direction, the leakage current was sufficiently suppressed. [Explanation of symbols]

[0052] 1, 2 Semiconductor wafer 100, 200 light emitting elements 11 Substrate 12 Semiconductor Department 12n n-side nitride semiconductor layer 12a active layer 12p p-side nitride semiconductor layer 12x high resistance section 13 Dividing Line 14 1st protective layer 15 Current spreading layer 16 n-pad electrode 17 p pad electrode 18 Second protective layer 20 Recess 21 Corners etc. L Laser light

Claims

1. A semiconductor structure including, in order from bottom to top, a substrate, an n-side nitride semiconductor layer containing an n-type impurity, and a p-side nitride semiconductor layer containing a p-type impurity, the n-side nitride semiconductor layer having a region exposed from the p-side nitride semiconductor layer; a first protective layer provided only on an upper surface of a periphery of the p-side nitride semiconductor layer, among an upper surface of the p-side nitride semiconductor layer; a p-pad electrode located above the p-side nitride semiconductor layer and located inside the outer periphery in a plan view; the p-side nitride semiconductor layer side of the semiconductor structure is a light extraction surface side, and the n-side nitride semiconductor layer side of the semiconductor structure is a mounting surface side; 1. A light-emitting device, comprising: a p-side nitride semiconductor layer having a periphery having a higher resistance than an inside of the periphery of the p-side nitride semiconductor layer when viewed from above.

2. The light-emitting element as described in claim 1, wherein the outer side surface of the n-side nitride semiconductor layer and the outer side surface of the p-side nitride semiconductor layer are located on the same plane.

3. The p-side nitride semiconductor layer further includes a current spreading layer provided in a region of the upper surface of the p-side nitride semiconductor layer that is more inward than the upper surface of the outer periphery, 3. The light-emitting device according to claim 1, wherein the p-pad electrode is provided on the current spreading layer.

4. The light-emitting element according to claim 3 , further comprising a second protective layer formed above the semiconductor structure in a region including an upper surface of the first protective layer.

5. The light-emitting element described in claim 4, wherein the second protective layer is in contact with the first protective layer and the current spreading layer.

6. A light-emitting element as described in claim 1, further comprising an n-pad electrode, the n-pad electrode being located inside the outer peripheral side surface of the n-side nitride semiconductor layer in a planar view and being provided in an exposed region of the n-side nitride semiconductor layer exposed from the p-side nitride semiconductor layer.

Citation Information

Patent Citations

  • Semiconductor device and its production

    JP1997162441A

  • Gallium nitride compound semiconductor light emitting element and its manufacture

    JP2000353822A

  • Method of manufacturing nitride-based semiconductor element

    JP2005166728A

  • Method for preparing protective film with high transmittance and method for manufacturing semiconductor light emitting element

    JP2014045094A

  • Manufacturing method for light emission element

    JP2016184718A