Laminated core, rotating electric machine, and method of manufacturing laminated core
The laminated core with controlled magnetic domain structure and annealing in a magnetic field effectively reduces iron loss, enhancing the efficiency of rotating electrical machines, particularly for electric vehicles.
Patent Information
- Application Number
- JP2024541778
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-03-15
- Filing Date
- 2024-03-07
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2044-03-07
AI Technical Summary
Existing methods for annealing laminated cores made of amorphous alloy ribbons in a magnetic field do not effectively reduce iron loss due to differences in magnetic flux direction between the core back and teeth, leading to insufficient iron loss reduction.
A laminated core configuration with annular flakes of Fe-based amorphous alloy, annealed in a magnetic field along the circumferential direction, featuring a magnetic domain structure with controlled magnetic domain width and angle, and an adhesive layer to enhance magnetic properties.
The method results in a laminated core with significantly reduced iron loss, improving the efficiency of rotating electrical machines by enhancing magnetic properties and reducing iron loss, suitable for applications in electric vehicles.
Smart Images

Figure 0007590686000002 
Figure 0007590686000003 
Figure 0007590686000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminated core, a rotating electric machine, and a method for manufacturing a laminated core. This application claims priority based on Japanese Patent Application No. 2023-040773, filed on March 15, 2023, the contents of which are incorporated herein by reference. [Background technology]
[0002] In recent years, electric vehicles have been attracting attention, and rotating electric machines, which are the driving sources of electric vehicles, have been actively developed. Rotating electric machines for electric vehicles are required to exhibit high efficiency over a wide range of rotation speeds and / or a wide range of torque in order to obtain appropriate output according to various driving conditions.
[0003] Conventionally, stator cores using amorphous alloys have been proposed (see, for example, Patent Documents 1 to 4). In particular, Patent Documents 3 and 4 propose a method of annealing a stator core using an amorphous alloy in a magnetic field. Specifically, Patent Document 3 describes an apparatus for annealing a wound core formed by winding a thin plate of an amorphous alloy in a magnetic field. Patent Document 4 describes a method of annealing an amorphous alloy ribbon made of a high magnetic permeability amorphous alloy applicable to the iron cores of transformers and motors at a temperature equal to or lower than the crystallization temperature in a magnetic field. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2020 / 044745 [Patent Document 2] Japanese Patent No. 6656429 [Patent Document 3] Japanese Patent Application Publication No. 5-21774 [Patent Document 4] Japanese Patent Publication No. 3-10052 Summary of the Invention [Problem to be solved by the invention]
[0005] However, the device described in Patent Document 3 is not intended for laminated cores. Moreover, Patent Document 4 merely suggests the application of amorphous alloy ribbons annealed in a magnetic field to motor cores, but does not specifically disclose the annealing of laminated cores in a magnetic field. The laminated core has an annular core back and a plurality of teeth formed to protrude inward from the core back, but the direction of magnetic flux flow within the plane of the laminated core is different between the core back and the teeth. Therefore, when annealing a laminated core made of an amorphous alloy ribbon in a magnetic field, even if the techniques disclosed in Patent Documents 3 and 4 are applied, there are cases in which the effect of reducing iron loss is not sufficiently obtained.
[0006] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a laminated core made of an amorphous alloy ribbon with reduced iron loss, a rotating electric machine including a laminated core with reduced iron loss, and a method for manufacturing the laminated core. [Means for solving the problem]
[0007] In order to solve the above problems, the present invention employs the following configuration. [1] A laminated core according to one embodiment of the present invention is formed by stacking a plurality of annular thin flakes made of an Fe-based amorphous alloy having an amorphous structure in the thickness direction, and the ratio (Wθ / Wr) of iron loss Wθ in the circumferential direction θ of the flakes to iron loss Wr in the radial direction perpendicular to the circumferential direction θ and the thickness direction is less than 1.0. [2] The laminated core described in [1] above may be provided with an annular core back portion and a plurality of teeth portions protruding from the core back portion in the radial direction and arranged at intervals in the circumferential direction θ, and a ratio (Wc / Wr) of the iron loss Wθ to the iron loss Wr in the core back portion may be less than 1.0. [3] In the laminated core described in [1] above, the Fe-based amorphous alloy may have an amorphous structure as a whole and may not contain a crystalline structure. [4] In the laminated core described in [1] above, an oxide film may be formed on the surface of the thin pieces. [5] The laminated core described in [1] above may have an adhesive layer between the laminations. [6] The laminated core described in [2] above may have at least one magnetic domain in the core back portion between adjacent teeth among the plurality of teeth, the magnetic domain width being 0.3 mm or more and 3.0 mm or less, and the angle between the magnetic domain wall and a tangent to the circumferential direction θ being less than 10°. [7] In the laminated core described in [2] above, in the core back portion between adjacent teeth portions among the plurality of teeth portions, the magnetic domain width may be 0.3 mm or more and 3.0 mm or less, and the angle between the magnetic domain wall and a tangent to the circumferential direction θ of less than 10° may account for 50% or more of the magnetic domains in terms of area percentage. [8] A rotating electric machine according to an aspect of the present invention includes the laminated core according to any one of the above [1] to [7]. [9] A method for manufacturing a laminated core according to one embodiment of the present invention includes a magnetic field annealing process for annealing a laminate formed by stacking a plurality of annular thin pieces made of an Fe-based amorphous alloy along its thickness direction in a magnetic field, in which the laminate is annealed at an annealing temperature lower than the Curie point Tc (°C) of the Fe-based amorphous alloy and equal to or higher than (Tc-100)°C while a magnetic field is applied in a circumferential direction θ of the laminate.
[10] In the method for manufacturing a laminated core described in [9] above, the annealing temperature in the magnetic field annealing step may be in the range of (Tc-20)°C or less and (Tc-90)°C or more.
[11] In the method for manufacturing a laminated core described in [9] above, the annealing temperature in the magnetic field annealing step may be in the range of (Tc-40)°C or less and (Tc-70)°C or more.
[12] In the method for manufacturing a laminated core described in [9] above, the magnitude of a magnetic field applied to the laminate may be in the range of 100 to 10,000 A / m inside the laminate.
[13] In the method for manufacturing a laminated core described in [9] above, the magnitude of a magnetic field applied to the laminate may be in the range of 400 to 7500 A / m inside the laminate.
[14] In the method for producing a laminated core according to the above [9], the magnetic field annealing step comprises: A first step of applying a magnetic field to the laminate along the circumferential direction θ; A second step of heating the laminate to which the magnetic field has been applied up to the annealing temperature; A third step of annealing the laminate to which the magnetic field has been applied by holding the laminate at the annealing temperature for 1 to 8 hours; A fourth step of cooling the laminate to which the magnetic field has been applied to a temperature of 200° C. or lower; a fifth step of stopping application of the magnetic field to the laminate after the fourth step; The present invention may also include:
[15] In the method for producing a laminated core according to the above
[14] , in the second step, an average heating rate may be 1 to 10° C. / min. Effect of the Invention
[0008] According to the present invention, it is possible to provide a laminated core made of an amorphous alloy ribbon with reduced iron loss, a rotating electrical machine including a laminated core with reduced iron loss, and a method for manufacturing the laminated core. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of a rotating electric machine according to this embodiment. [Diagram 2] FIG. 2 is a schematic plan view showing an example of a stator core (stacked core) provided in the rotating electric machine according to this embodiment. [Diagram 3] FIG. 3 is a schematic cross-sectional view showing an example of a stator core (stacked core) provided in the rotating electric machine according to this embodiment. [Figure 4] FIG. 4 is a schematic plan view illustrating an example of magnetic field annealing for a stator core (stacked core) provided in the rotating electric machine according to this embodiment. [Diagram 5] FIG. 5 is a schematic plan view illustrating another example of magnetic field annealing for a stator core (stacked core) provided in the rotating electric machine according to this embodiment. [Figure 6]FIG. 6 is a schematic plan view illustrating another example of magnetic field annealing for a stator core (stacked core) provided in the rotating electric machine according to this embodiment. [Figure 7] FIG. 7 is a graph showing losses in the rotating electrical machine according to this embodiment. [Figure 8] FIG. 8 is a graph showing the relationship between the core loss of a wound core made of an Fe-based amorphous alloy and the holding temperature of annealing in a magnetic field. [Figure 9] FIG. 9 is a graph showing the effect of improving magnetic properties when a ribbon of an Fe-based amorphous alloy is annealed in a magnetic field. [Figure 10] FIG. 10 is a schematic diagram illustrating the positions at which test pieces for measuring magnetic properties were cut out. [Figure 11] FIG. 11 is a schematic perspective view showing an example in which a wound core is applied to a stator core of a rotating electrical machine. [Figure 12A] FIG. 12A is a schematic perspective view showing another example in which a wound core is applied to a stator core of a rotating electrical machine. [Figure 12B] FIG. 12B is a partially enlarged view of FIG. 12A. [Figure 13] FIG. 13 is an example of an image obtained by observing, by Kerr effect microscopy, an area of 10 mm length×10 mm width on the surface of a sample taken from a stator core (stacked iron core) provided in the rotating electric machine of this embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS A laminated core, a rotating electrical machine including the laminated core, and a method for manufacturing the laminated core according to embodiments of the present invention will be described with reference to the drawings.
[0011] In the following description, the rotating electric machine will be described as an electric motor, specifically an AC motor, more specifically a synchronous motor, and even more specifically a permanent magnet field type motor, which is suitable for use in, for example, electric vehicles.
[0012] 1 to 3, a rotating electric machine 10 of this embodiment includes a stator 20, a rotor 30, a case 50, and a rotating shaft 60. The stator 20 and the rotor 30 are housed in the case 50. The stator 20 is fixed to the case 50.
[0013] In this embodiment, an inner rotor type rotating electric machine 10 is used in which the rotor 30 is located inside the stator 20. However, an outer rotor type rotating electric machine 10 in which the rotor 30 is located outside the stator 20 may also be used. The rotating electric machine 10 of this embodiment is a three-phase AC motor with 12 poles and 18 slots. However, for example, the number of poles, the number of slots, the number of phases, etc. can be changed as appropriate.
[0014] The stator 20 includes a stator core 21, which is an example of a laminated core of the present embodiment, and a winding (not shown). As shown in Fig. 4, the stator core 21 is configured by laminating thin pieces 40 made of an Fe-based amorphous alloy in the thickness direction. The stator core 21 includes an annular core back portion 22 and a plurality of teeth portions 23. Hereinafter, the axial direction of the stator core 21 (core back portion 22), i.e., the direction of the central axis O of the stator core 21, is referred to as the axial direction t. The radial direction of the stator core 21 (core back portion 22), i.e., the direction perpendicular to the central axis O of the stator core 21, is referred to as the radial direction r. The circumferential direction of the stator core 21 (core back portion 22), i.e., the direction going around the central axis O of the stator core 21, is referred to as the circumferential direction θ.
[0015] The core back portion 22 is formed in an annular shape when the stator 20 is viewed in a plan view from the axial direction t.
[0016] The multiple teeth portions 23 protrude inward in the radial direction r from the core back portion 22. Specifically, the multiple teeth portions 23 protrude toward the central axis O of the core back portion 22 along the radial direction r. The multiple teeth portions 23 are arranged at equal intervals in the circumferential direction θ. In this embodiment, 18 teeth portions 23 are provided at central angle intervals of 20 degrees about the central axis O. The multiple teeth portions 23 are formed to have the same shape and size as one another.
[0017] The winding is wound around the teeth portion 23. The winding may be concentrated winding or distributed winding.
[0018] The rotor 30 is disposed on the inside in the radial direction r with respect to the stator 20 (the stator core 21). The rotor 30 includes a rotor core 31 and a plurality of permanent magnets 32.
[0019] Rotor core 31 is formed in an annular (circular) shape and arranged coaxially with stator 20. A rotating shaft 60 is arranged inside rotor core 31. Rotor core 31 is a ferromagnetic body. Rotor core 31 may be formed by stacking a plurality of steel pieces cut from an electromagnetic steel sheet in the thickness direction. Rotor core 31 may also be formed by stacking a plurality of thin pieces cut from a ribbon of Fe-based amorphous alloy in the thickness direction.
[0020] The multiple permanent magnets 32 are fixed to the rotor core 31. In this embodiment, a pair of the permanent magnets 32 forms one magnetic pole. The multiple pairs of permanent magnets 32 are arranged at equal intervals in the circumferential direction θ. In this embodiment, 12 pairs (24 in total) of permanent magnets 32 are provided at central angle intervals of 30 degrees around the central axis O.
[0021] In this embodiment, an interior magnet motor is used as the permanent magnet field type motor. The rotor core 31 is formed with a plurality of through holes 33 penetrating the rotor core 31 in the axial direction t. The plurality of through holes 33 are provided corresponding to the plurality of permanent magnets 32. Each permanent magnet 32 is fixed to the rotor core 31 while being disposed in the corresponding through hole 33. Each permanent magnet 32 can be fixed to the rotor core 31, for example, by bonding the outer surface of the permanent magnet 32 to the inner surface of the through hole 33 with an adhesive. Note that a surface permanent magnet motor may be used as the permanent magnet field type motor instead of the embedded permanent magnet motor.
[0022] The lamination thickness of each of the stator core 21 and the rotor core 31 is, for example, 30 mm. The outer diameter of stator core 21 is, for example, 150 mm. The inner diameter of stator core 21 is, for example, 100 mm. The outer diameter of rotor core 31 is, for example, 98.4 mm. However, these values are merely examples, and the lamination thickness, outer diameter, and inner diameter of stator core 21 and the lamination thickness and outer diameter of rotor core 31 are not limited to these values. Here, the reference for the inner diameter of stator core 21 is the tip of teeth portion 23 in stator core 21. The inner diameter of stator core 21 is the diameter of an imaginary circle inscribed in the tips of all teeth portions 23.
[0023] The flakes 40 made of the Fe-based amorphous alloy constituting the laminated core of this embodiment are formed, for example, by punching, cutting, or wire discharge machining of the Fe-based amorphous alloy ribbon as the base material. Alternatively, a plurality of Fe-based amorphous alloy ribbons that have not been subjected to shaping may be laminated, and then processed into a predetermined shape by wire discharge machining to form a plurality of flakes 40 at once.
[0024] The Fe-based amorphous alloy may contain, for example, 70 mass% or more of Fe, and may further contain one or more of Si, P, B, and C. The Fe-based amorphous alloy may contain, in addition to the above elements, one or more of Al, Ge, Se, W, Mo, V, Nb, Ta, Ti, Hf, Mn, and Cu. A part of Fe may be replaced with Co or Ni. It is preferable that the Fe-based amorphous alloy has an amorphous structure as a whole and does not contain a crystalline structure. The absence of a crystalline structure can be confirmed by observing no clear diffraction peaks by X-ray diffraction measurement.
[0025] The Fe-based amorphous alloy can be obtained, for example, by quenching a molten alloy containing Fe and the above-mentioned elements using, for example, a single-roll type liquid quenching device, and casting the molten alloy. The Fe-based amorphous alloy thus produced is obtained in the form of a thin ribbon.
[0026] The magnetic properties of the as-quenched Fe-based amorphous alloy are preferably such that the saturation magnetic flux density is 1.2 T or more, for example.
[0027] The thickness of the flake 40 made of the ribbon of the Fe-based amorphous alloy thus obtained is preferably, for example, 10 μm or more and 100 μm or less.
[0028] The surface of the flakes 40 made of the Fe-based amorphous alloy ribbon may have an oxide film having a thickness of, for example, about 20 nm. This oxide film is a natural oxide film formed on the surface of the ribbon when the Fe-based amorphous alloy ribbon is manufactured by quenching the molten alloy. Since this oxide film has insulating properties, it can insulate the flakes 40 constituting the laminated core from each other, suppressing eddy currents and reducing iron loss.
[0029] The multiple laminations 40 forming the stator core 21 may be bonded together by an adhesive layer 41 . The adhesive may be, for example, a thermosetting adhesive based on polymerization bonding. The adhesive composition may be, for example, (1) an acrylic resin, (2) an epoxy resin, (3) a composition containing an acrylic resin and an epoxy resin, or (4) a natural or synthetic varnish. The type of adhesive is not limited to the above.
[0030] In order to obtain a stable and sufficient adhesive strength, the thickness of the adhesive layer 41 is preferably 1 μm or more. On the other hand, if the thickness of the adhesive layer 41 exceeds 100 μm, the adhesive strength is saturated. In addition, as the adhesive layer 41 becomes thicker, the space factor of the flakes 40 decreases, and magnetic properties such as iron loss decrease. Therefore, the thickness of the adhesive layer 41 is more preferably 1 μm or more and 100 μm or less, and even more preferably 1 μm or more and 10 μm or less. The thickness of the adhesive layer 41 means the average thickness of the adhesive layer 41. In addition, since the adhesive layer 41 has insulating properties, together with the oxide film on the surface of the flakes, the flakes 40 constituting the laminated core can be insulated from each other, suppressing eddy currents and reducing iron loss.
[0031] The stator core 21 (laminated core) according to this embodiment is annealed in a magnetic field. The stator core 21 that has been annealed in a magnetic field has significantly improved iron loss. In addition, the stator core 21 that has been annealed in a magnetic field has anisotropy in iron loss. In other words, it has the characteristic that the iron loss in the direction in which the magnetic field is applied during annealing is lower than the iron loss in other directions.
[0032] In addition, in the stator core 21 that has been annealed in a magnetic field, the surfaces of the flakes 40 are discolored in a mottled manner, so whether or not the stator core 21 has been annealed in a magnetic field can be determined based on the presence or absence of discoloration. That is, the stator core 21 of this embodiment is formed by laminating the flakes 40 along the thickness direction, and at least one discolored portion is observed on the surface of the flakes 40 located on the outermost side of the stator core 21. The discolored portion is formed by annealing in a magnetic field and corresponds to what is called a temper color. The discolored portion refers to a portion where the color tone or color of the surface is different from that of the other portions when the surface of the flakes 40 located on the outermost side of the stator core 21 is observed with the naked eye or a magnifying glass.
[0033] The discolored portion caused by magnetic field annealing can also be confirmed by observing the side surface of stator core 21. That is, the end faces of laminated flakes 40 are exposed on the side surface of stator core 21, and discolored portions are also formed on these end faces by magnetic field annealing. The discolored portion refers to a portion whose surface color tone or color is different from the other portions when the side surface of stator core 21 is observed with the naked eye or a magnifying glass.
[0034] Moreover, whether or not the material has been annealed in a magnetic field can also be determined by checking the anisotropy of core loss.
[0035] In the stator core 21 of this embodiment, the ratio (Wθ / Wr) of the iron loss Wθ in the circumferential direction θ of the laminate to the iron loss Wr in the radial direction r of the laminate is less than 1.0. The radial direction r of the laminate is a direction perpendicular to the circumferential direction θ and the axial direction t (thickness direction of the laminate). More specifically, in the stator core 21 of this embodiment, the ratio (Wθ / Wr) of the iron loss Wθ to the iron loss Wr in the core back portion 22 is less than 1.0.
[0036] The iron loss ratio (Wθ / Wr) is measured as follows. First, a test piece S is cut out from the stator core 21. The shape of the test piece S is, for example, 20 mm in length, 20 mm in width, and 0.5 mm in thickness, that is, a square shape when viewed from above. However, the shape and dimensions of the test piece S are not limited to the above. The test piece S may be cut out so as to include the surface of the slice. Moreover, the above thickness of the test piece S is along the thickness direction of the slice.
[0037] When cutting out the test piece S from the stator core 21, as shown in FIG. 10, one of the length and width of the test piece S is aligned with the circumferential direction θ of the stator core 21, and the thickness direction of the test piece S is aligned with the axial direction t of the stator core 21. The cut-out position of the test piece S is the core back portion 22 of the stator core 21, as shown in FIG. 10. The test piece S may be taken, for example, from the core back portion 22 in the vicinity of the teeth portion 23, or from the core back portion 22 corresponding to a space between two adjacent teeth portions. If the shape of the test piece S is square, it is possible to use the same test piece for measuring the iron loss Wr in the radial direction r and the iron loss Wθ in the circumferential direction θ. However, if only a rectangular test piece S can be taken, a test piece for measuring the iron loss Wr in the radial direction r of the laminate and a test piece for measuring the iron loss Wθ in the circumferential direction θ are prepared separately.
[0038] The obtained test piece S is then measured using an SST (Single Strip Tester). The iron loss measurement conditions are a magnetic flux density of 1.0 T and a frequency of 50 Hz. The iron loss Wθ in the circumferential direction θ of the laminate is measured by applying a magnetic field in the direction of the side of the test piece S corresponding to the circumferential direction θ (the circumferential direction θ of the stator core 21). The iron loss Wr in the radial direction r of the laminate is measured by applying a magnetic field in the direction of the side of the test piece corresponding to the radial direction r (the radius r of the stator core 21). The iron loss ratio (Wθ / Wr) is then calculated from the obtained iron losses Wθ and Wr. The iron loss measurement is in accordance with the measurement method described in JIS H 7152:1996 (Method of testing magnetic properties of amorphous metal single sheet).
[0039] As described above, the stator core 21 according to this embodiment is annealed in a magnetic field. This allows a magnetic domain structure that is effective in reducing iron loss to be imparted to the stator core 21. Specifically, in the core back portion 22 between the teeth portions 23, there is at least one magnetic domain whose magnetic domain width is 0.3 mm or more and 3.0 mm or less, and whose angle between the magnetic domain wall and the circumferential direction θ is less than 10°.
[0040] The magnetic domain structure can be controlled by the magnitude of the magnetic field applied during magnetic annealing and the annealing temperature. In particular, the effect of the applied magnetic field is large, and when the magnetic field is weak, the magnetic domain width is narrow and the angle between the magnetic domain wall and the circumferential direction θ is large. On the other hand, when the magnetic field is strong, the magnetic domain width is wide and the angle between the magnetic domain wall and the circumferential direction θ is small. In particular, in the case of a laminated core for motor use, the inventors have found that it is possible to effectively reduce iron loss by appropriately controlling the magnitude of the magnetic field applied during magnetic annealing and the annealing temperature so that the magnetic domain structure has a magnetic domain width of 0.3 mm to 3.0 mm and an angle between the magnetic domain wall and the circumferential direction θ of less than 10°.
[0041] The inventors have also found that iron loss can be reduced more effectively in the case of a laminated core having many magnetic domains with a magnetic domain width of 0.3 mm to 3.0 mm and an angle between the magnetic domain wall and the circumferential direction θ of less than 10° as described above. Specifically, in the core back portion 22 between the teeth portions 23, if the proportion of magnetic domains with a magnetic domain width of 0.3 mm to 3.0 mm and an angle between the magnetic domain wall and the tangent to the circumferential direction θ of less than 10° is 50% to 100% by area, iron loss can be further reduced.
[0042] The magnetic domain structure can be observed by the Bitter method, the Kerr effect microscope, the Lorentz microscope, an observation method using a magneto-optical sensor, etc., and there is no particular limitation on the observation method. In this embodiment, the magnetic domain structure is observed by the Kerr effect microscope.
[0043] A specific method for observing the magnetic domain structure is as follows. Samples for observing the magnetic domain structure are taken from the stator core shown in Fig. 2. Specifically, the annular stator core in Fig. 2 is viewed in plan, and samples are taken from the core back portions 22 corresponding to 0°, 45°, 90°, and 135°.
[0044] Next, the magnetic domain structure is observed by Kerr effect microscopy in a region of 10 mm length × 10 mm width on the surface of each sample. Figure 13 shows an example of an image obtained by observing a region of 10 mm length × 10 mm width on the surface of a sample taken from the stator core of this embodiment using the Kerr effect microscope.
[0045] The white or black contrast in Figure 13 is a magnetic domain, and each magnetic domain has a curved shape along the circumferential direction θ. The boundary between the white and black contrast (i.e., the boundary between the magnetic domains) is a magnetic domain wall. The magnetic domain structure of each sample (four in total) corresponding to 0°, 45°, 90°, and 135° of the stator core is observed, and the "magnetic domain width" and "angle between the magnetic domain wall and the tangent to the circumferential direction θ" for each sample are determined. Here, "magnetic domain width" refers to the average value of the widths (length along the radial direction r) of three randomly selected magnetic domains in each magnetic domain.
[0046] Next, the area ratio of the magnetic domain structure having a magnetic domain width of 0.3 mm to 3.0 mm and an angle between the magnetic domain wall and the tangent of the circumferential direction θ of less than 10° is obtained. The area ratio of the magnetic domain structure (area %) is defined as the ratio of the total magnetic domain width of the magnetic domains having a magnetic domain width of 0.3 mm to 3.0 mm to the total magnetic domain width of all the magnetic domains observed. For example, in the case of the image shown in FIG. 13, the total magnetic domain width of the magnetic domains having a magnetic domain width of 0.3 mm to 3.0 mm is 2.15+1.67=3.82 μm, and the total magnetic domain width of all the magnetic domains is 6.99 μm, so the area ratio is 3.82 μm / 6.99 μm=54.6%. Note that for magnetic domains whose both ends (both magnetic domain walls) in the radial direction r cannot be confirmed in the observation image, the magnetic domain width cannot be measured, so they are excluded from the calculation of the "magnetic domain width" and the "area ratio (%) of the magnetic domain structure". In addition, in each image obtained in this embodiment, the "area ratio of magnetic domain structures having a magnetic domain width of 0.3 mm or more and 3.0 mm or less and an angle between the magnetic domain wall and the tangent to the circumferential direction θ of less than 10°" is the average value of the area ratios of each image.
[0047] If no magnetic field is applied during annealing, a magnetic domain structure with an unclear contrast between white and black is observed. This suggests that the magnetic domain structure has no anisotropy, and effective iron loss reduction cannot be expected. Furthermore, when annealing in a magnetic field as shown in FIG. 4, which will be described later, the magnetic field is applied concentrically, but in the teeth portion 23, the magnetic field is hardly applied due to the presence of gaps (slots) in the circumferential direction. Therefore, the magnetic domain structure of the teeth portion 23 is the same as when annealing is performed without a magnetic field. Therefore, the magnetic domains are random (no anisotropy) other than in the core back portion 22 (i.e., in the teeth portion 23).
[0048] Next, a method for manufacturing the laminated core of this embodiment will be described. The manufacturing method of the laminated core of this embodiment includes a magnetic field annealing step of annealing an annular laminate formed by stacking a plurality of annular thin pieces made of an Fe-based amorphous alloy along the thickness direction in a magnetic field. The magnetic field annealing step is a step of annealing the laminate in a temperature range (annealing temperature) lower than the Curie point Tc (°C) of the Fe-based amorphous alloy and equal to or higher than (Tc-100)°C while applying a magnetic field in the circumferential direction θ of the laminate.
[0049] The magnetic field annealing step of this embodiment may include the following steps. That is, the magnetic field annealing step of this embodiment includes: A first step of applying a magnetic field to the laminate along the circumferential direction θ; A second step of heating the laminate to which the magnetic field has been applied up to the annealing temperature; A third step of annealing the laminate to which the magnetic field has been applied by holding the laminate at the annealing temperature for 1 to 8 hours; A fourth step of cooling the laminate to which the magnetic field has been applied to a temperature of 200° C. or lower; a fifth step of stopping application of the magnetic field to the laminate after the fourth step; The present invention may also include: The magnetic field annealing step will be described in detail below.
[0050] The annular laminate to be annealed in the magnetic field is obtained by, for example, cutting out a plurality of slices from a ribbon made of an Fe-based amorphous alloy and stacking them in the thickness direction. The planar shape of the slices cut out from the ribbon is, for example, the planar shape of the stator core 21 shown in FIG. 2. The slices may be cut out by, for example, punching the ribbon or by wire discharge machining of the ribbon. When stacking a plurality of slices, an adhesive layer may be interposed between the slices. In this way, an annular laminate having the shape of a stator core as shown in FIG. 2 is obtained.
[0051] The annular laminate may be obtained, for example, by laminating ribbons made of an Fe-based amorphous alloy in the thickness direction and then processing the laminate of the ribbons. When laminating the ribbons, an adhesive layer may be interposed between the ribbons. The processing method for obtaining the laminate from the laminate of the ribbons may be, for example, punching or wire discharge processing. By carrying out such processing, an annular laminate having the shape of a stator core as shown in FIG. 2 is obtained.
[0052] The magnetic field annealing of the laminate is carried out by heating the laminate in a temperature range lower than the Curie point Tc (° C.) of the Fe-based amorphous alloy and equal to or higher than (Tc−100)° C. while applying a magnetic field to the laminate.
[0053] When performing magnetic field annealing, a magnetic field is applied to a laminate having the shape of a stator core along the circumferential direction θ, and the laminate is heated to the annealing temperature, and then annealed by holding it for a certain period of time. That is, a magnetic field is applied to the laminate along the circumferential direction θ (first step), and then the laminate to which the magnetic field has been applied is heated to the annealing temperature (second step). Next, the laminate to which the magnetic field has been applied is held at the annealing temperature for a certain period of time to perform magnetic field annealing (third step). The method of applying the magnetic field will be described in detail later.
[0054] In addition, the first step and the second step may be interchanged so long as the temperature is in a range of 200° C. or less. That is, as described above, the third step may be performed after applying a magnetic field and heating to the annealing temperature, or the laminate may be heated to 200° C., and then a magnetic field may be applied to the laminate and the laminate may be heated from 200° C. to the annealing temperature.
[0055] The magnitude of the magnetic field applied to the laminate is preferably within the range of 100 to 10,000 A / m, more preferably 400 to 7,500 A / m, and even more preferably 400 to 5,000 A / m. By setting the magnitude of the magnetic field applied to the laminate within the above range, it is possible to significantly reduce the iron loss of the stator core.
[0056] The average heating rate up to the annealing temperature may be 1 to 10°C / min. If the average heating rate up to the annealing temperature exceeds 10°C / min, the temperature difference occurring within the laminate increases. If the temperature difference within the laminate increases, the thermal distortion caused by the temperature difference also increases, and the magnetic properties may deteriorate. Therefore, the average heating rate up to the annealing temperature is preferably 10°C / min or less. On the other hand, if the average heating rate up to the annealing temperature is less than 1°C / min, the temperature rise time becomes long, which is not preferable from the viewpoint of productivity.
[0057] The laminate to which the magnetic field has been applied is then annealed by holding it at the annealing temperature for 1 to 8 hours (third step). The annealing temperature (holding temperature) is preferably equal to or higher than (Tc-100) (°C) and lower than Tc (°C). The annealing temperature may be (Tc-90)(°C) or more, (Tc-70)(°C) or more, or (Tc-60)(°C) or more. The annealing temperature may be (Tc-20)(°C) or less, or (Tc-40)(°C) or less. By setting the annealing temperature to (Tc-100)(°C) or more and less than Tc(°C), the iron loss of the stator core can be significantly improved and anisotropy of the iron loss can be imparted. If the annealing temperature is lower than (Tc-100)(°C), the improvement effect of the iron loss is reduced. Also, if the annealing temperature is higher than the Curie point Tc(°C), the Fe-based amorphous alloy will crystallize, the magnetic properties will be significantly reduced, and the improvement effect of the iron loss will be reduced, which is not preferable.
[0058] There are two ways to increase the efficiency of rotating electrical machines: reducing iron loss and reducing magnetizing force, but there is a trade-off between the two. Fe-based amorphous alloys have an extremely good start-up in BH characteristics compared to electromagnetic steel sheets. In other words, the current (magnetizing force) required to obtain the same magnetic flux density is small, and the copper loss is small, so it is thought that reducing iron loss will have a greater effect in improving the efficiency of rotating electrical machines such as motors. For example, minimizing iron loss and minimizing magnetizing force require different structures depending on the purpose, so the annealing temperature changes. To minimize magnetizing force, it is possible to crystallize only a portion of the material, but to improve iron loss, it is better to have no crystallization and have an amorphous structure.
[0059] The annealing time (holding time) is preferably in the range of 1 to 8 hours. Holding time exceeding 8 hours results in a long annealing time, which is undesirable from the viewpoint of productivity. Therefore, the annealing time is preferably 8 hours or less. More preferably, it is 4 hours. On the other hand, if the holding time is less than 1 hour, the effect of fixing the magnetization by annealing in a magnetic field may not be sufficient, and a magnetic domain structure effective in reducing iron loss may not be obtained. Therefore, the annealing time is 1 hour or more.
[0060] The annealing time can be determined by the Larson-Miller parameter LMP below. The relationship between the annealing temperature and the annealing time is determined by the Larson-Miller parameter LMP using the holding temperature T [K] and holding time t [hr] during annealing in a magnetic field. If the value of this LMP is the same, the effect of the heat treatment will be the same. Therefore, for example, when changing the annealing temperature, the LMP is calculated from the annealing temperature and annealing time before the change using the following formula, and then the calculated LMP and the planned annealing temperature are input into the following formula to calculate the planned changed annealing time.
[0061] LMP = T(C + logt)
[0062] Here, C is a value [hr] determined by the material.
[0063] If the Curie point Tc (℃) of an Fe-based amorphous alloy is unknown, it is necessary to measure and determine it. The Curie point Tc (℃) can be measured using a general measurement method. For example, the Curie point Tc (℃) can be identified by using a vibrating sample magnetometer (VSM) to extrapolate the asymptote of the temperature change of magnetization on the low temperature side to magnetic polarization 0.
[0064] After the annealing in the magnetic field, the laminate with the magnetic field applied is cooled to 200° C. or less (fourth step), and then the application of the magnetic field to the laminate is stopped (fifth step). In the fourth step, it is preferable to slowly cool the laminate to a temperature range of 200° C. or less by natural cooling or the like. By the above steps, the laminate can be annealed in a magnetic field, and a laminated core having a Wθ / Wr within a desired range can be obtained.
[0065] Next, a magnetic field annealing step (a method of applying a magnetic field) in which the laminate having the shape of the stator core 21 is annealed in a magnetic field will be described in detail with reference to FIGS.
[0066] The first magnetic field application method will be described below. First, as shown in FIG. 4, a rod-shaped exciting electrode 101 is inserted into the hollow portion of the laminate. The rod-shaped exciting electrode 101 is inserted into the hollow portion along the axial direction t of the laminate so as not to come into contact with the laminate. Next, a current is passed through the rod-shaped exciting electrode 101 to generate an induced magnetic field around the rod-shaped electrode 101, and a magnetic field is applied along the circumferential direction θ of the laminate. Then, annealing is performed with a magnetic field applied inside the laminate.
[0067] The laminated body having the shape of a stator core is composed of an annular core back portion 22 and a plurality of teeth portions 23 protruding toward the central axis of the stator core 23. The core back portion 22 is continuous along the circumferential direction θ of the stator core 21. On the other hand, the teeth portions 23 are divided along the circumferential direction θ and are discontinuous because of gaps (slots) between the teeth portions 23. Therefore, when a magnetic field is applied in the circumferential direction θ of the stator core 21, the magnetic field ψ is concentrated and applied to the core back portion 22, and the magnetic field is hardly applied to the teeth portions 23. Therefore, in the first method shown in FIG. 4, magnetic field annealing is mainly performed on the core back portion 22. In the first method, magnetic field annealing can be completed in a relatively short time.
[0068] Next, the second method of applying a magnetic field will be described below. First, as shown in FIG. 5, the winding 102 is wound around the laminate. The winding 102 is insulated from the laminate. The winding 102 is wound so as to pass alternately through the hollow portion of the laminate and the outer periphery of the laminate. When the winding 102 is inserted into the hollow portion of the laminate, the winding is disposed at a position corresponding to the tip of the teeth portion 23 or between the teeth portion 23. In this manner, an excitation coil made of the winding 102 is formed. Next, a magnetic field ψ is applied to the laminate along the circumferential direction θ by passing a current through the excitation coil. Annealing is then performed with the magnetic field applied.
[0069] In the second method, the magnetic field ψ is also applied intensively to the core back portion 22, and is hardly applied to the teeth portion 23. Therefore, in the second method shown in Fig. 5, the magnetic field annealing is mainly performed on the core back portion 22 of the laminate. In the second method, the magnetic field annealing can be completed in a relatively short time.
[0070] Next, as a third method of applying a magnetic field, as shown in Fig. 6, a winding 103 is wound independently around each tooth 23 of the laminate, and an auxiliary core 104 made of a ferromagnetic material is inserted into the hollow portion of the laminate. The winding 103 is insulated from the laminate. By inserting the auxiliary core 104 into the hollow portion, a closed magnetic circuit is formed between the teeth 23, the core back portion 22, and the auxiliary core 104 when a magnetic field is generated by passing a current through the winding 103.
[0071] When applying a current to the winding 103, a direct current is passed through the U-phase coil, V-phase coil, and W-phase coil, which are arranged at a central angle of 120 degrees each with respect to the teeth portion 23, at a current ratio of, for example, U-phase coil:V-phase coil:W-phase coil = 2:-1:-1. This applies a magnetic field to the laminate. Annealing is then performed with the magnetic field applied. During annealing, the coils to which current is passed are switched in sequence. Note that the current ratios for the U-phase coil, V-phase coil, and W-phase coil are merely examples, and may deviate slightly from the above ratios. A negative current ratio indicates a direction opposite to the positive direction.
[0072] As shown in Fig. 6, the magnetic field ψ applied to the teeth portion 23 is applied in the radial direction r of the laminate, while the magnetic field ψ applied to the core back portion 22 is applied in the circumferential direction θ of the laminate. Therefore, in the third method shown in Fig. 6, magnetic field annealing is performed on both the core back portion 22 and the teeth portion 23. In the third method, the processing time is longer than in the first and second methods, but magnetic field annealing can be performed on both the core back portion 22 and the teeth portion 23.
[0073] As described above, magnetic field annealing is performed on a laminate having the shape of a stator core 21 made of an Fe-based amorphous alloy while applying a magnetic field along the circumferential direction θ. This can improve the magnetic properties of the core back portion, which has a larger area than the teeth portion, in the stator core, and can reduce the iron loss of the stator core 21 as a whole. By improving the magnetic properties of the core back portion, which has a larger area than the teeth portion, the magnetic properties of the stator core 21 as a whole can be improved even if the magnetic property improvement effect of the teeth portion is small. Therefore, by configuring a rotating electric machine with such a stator core 21, it is possible to achieve high efficiency over a wide range of rotation speeds and / or a wide range of torque. That is, a rotating electric machine equipped with such a stator core 21 has lower iron loss than a rotating electric machine configured with a stator core that has not been annealed in a magnetic field as described above, and can be suitably used as a rotating electric machine for electric vehicles.
[0074] 1, a pair of permanent magnets 32 form one magnetic pole, but this embodiment is not limited to this. For example, one permanent magnet 32 may form one magnetic pole, or three or more permanent magnets 32 may form one magnetic pole. In addition, in the above embodiment, a permanent magnet field type motor has been used as an example of a rotating electric motor, but the structure of the rotating electric motor is not limited to this, as exemplified below, and various well-known structures not exemplified below can also be adopted. In the above embodiment, a permanent magnet field type motor is used as an example of a rotating electric machine, but the present embodiment is not limited to this. For example, the rotating electric machine may be a reluctance type motor or an electromagnetic field type motor (wound field type motor). In the above embodiment, a synchronous motor is used as an example of an AC motor, but the present embodiment is not limited to this. For example, the rotating electric machine may be an induction motor. In the above embodiment, an AC motor is used as an example of a rotating electric machine, but the present embodiment is not limited to this. For example, the rotating electric machine may be a DC motor. In the above embodiment, an electric motor is used as an example of a rotating electric machine, but the present embodiment is not limited to this. For example, the rotating electric machine may be a generator. In the above embodiment, the stacked core according to the present embodiment is applied to a stator core, but it can also be applied to a rotor core.
[0075] Furthermore, the wound core according to this embodiment is not limited to those described in the above embodiments, and may be a wound core having a shape shown in Fig. 11 or Fig. 12A. The wound core shown in Fig. 11 or Fig. 12A is preferably used as the stator core of the rotating electric machine of this embodiment.
[0076] A perspective view of the wound core is shown in Fig. 11. A portion of the wound core 121 shown in Fig. 11 has been removed for the purpose of explanation, and a cross section of the removed portion is shown.
[0077] The wound core 121 shown in Fig. 11 can be obtained, for example, by the following method. First, an Fe-based amorphous alloy ribbon is wound spirally, either directly or after slitting the Fe-based amorphous alloy ribbon to adjust its width, into a toroidal core shape. Then, for example, by wire discharge machining, multiple recesses that are approximately rectangular in plan view are provided along the circumferential direction θ on the inner periphery of the spiral structure to form the teeth portion 123. In this way, the wound core 121 is obtained.
[0078] That is, the wound core 121 shown in Fig. 11 is composed of a core back portion 122 and teeth portions 123. The core back portion 122 is composed of an Fe-based amorphous alloy ribbon or a ribbon with an adjusted width wound in a spiral shape. The teeth portions 123 are composed of Fe-based amorphous alloy ribbons or ribbons with an adjusted width stacked one on top of the other. The multiple teeth portions 123 are disposed at equal intervals in the circumferential direction θ. The multiple teeth portions 123 are formed to have the same shape and size as each other.
[0079] 12A and 12B is formed by spirally winding an Fe-based amorphous alloy ribbon, either directly or after slitting the Fe-based amorphous alloy ribbon to adjust its width, into a toroidal core shape, and then forming grooves 222a on the inner periphery by, for example, electric discharge wire machining, and attaching teeth 223 to the grooves 222a. The shape of the grooves 222a is not limited to the V-shaped grooves shown in FIGS. 12A and 12B.
[0080] 12A shows a state in which rotor 230 is inserted into the hollow portion of wound core 221. Rotor 230 has, for example, rotor core 231 made of laminated electromagnetic steel sheets formed into a predetermined shape, and permanent magnets 232 provided in rotor core 231. At both longitudinal ends of permanent magnet 232, gaps 233 are provided for controlling the flow of magnetic flux of permanent magnet 232. Rotor core 231 may be made of an Fe-based amorphous alloy ribbon.
[0081] 12A and 12B is composed of a core back portion 222 and a plurality of teeth portions 223. The core back portion 222 is composed of an Fe-based amorphous alloy ribbon or a ribbon with an adjusted width wound in a spiral shape. The teeth portions 223 are formed so as to protrude from the inner peripheral surface of the core back portion 222 toward the center of the wound core 221. Each of the teeth portions 223 is attached to the core back portion 222 by being inserted into a groove portion 222a provided on the inner peripheral surface of the core back portion 222.
[0082] Each of the teeth 223 is formed by laminating thin pieces made of Fe-based amorphous alloy ribbons in the height direction of the wound core 221.
[0083] The teeth portion 223 can be manufactured by forming an Fe-based amorphous alloy ribbon into a thin piece having the same shape as the planar shape of the teeth portion 223, and stacking the thin piece in the height direction of the wound core 221. The forming process for the Fe-based amorphous alloy ribbon may be a punching process or a wire discharge process, and is not particularly limited.
[0084] The teeth portion 223 can be manufactured by processing the Fe-based amorphous alloy ribbon into rectangular or circular pieces, stacking the pieces in the thickness direction to form a laminate, and subjecting the laminate to a forming process. The forming process for the laminate may be a punching process or an electric discharge wire processing, and is not particularly limited.
[0085] The plurality of teeth 223 thus obtained may be attached to the core back portion 222 to form the wound core 221. When attaching the teeth 223 to the core back portion 222, the teeth 223 on which a winding has been applied in advance may be attached to the core back portion 222. This can increase the occupation rate of the winding.
[0086] The wound cores 121, 221 shown in Figures 11 and 12A can be suitably used as the stator core of the rotating electric machine of this embodiment. In particular, the wound core 221 shown in Figures 12A and 12B can have the windings wound on the teeth 223 in advance, which increases the occupancy rate of the windings, thereby improving the rotational torque of the rotating electric machine and reducing copper loss.
[0087] In addition, within the scope of the invention, the components in the above-described embodiments may be replaced with well-known components, and the above-described modified examples may be combined as appropriate. EXAMPLES
[0088] Example 1 A verification test was carried out to confirm the effect of reducing iron loss in rotating electrical machines. This verification test was carried out by simulation using software. The software used was JMAG, a finite element method electromagnetic field analysis software made by JSOL Corporation.
[0089] The test material was an Fe-based amorphous alloy (chemical composition: Fe 78 Si9B 12A ribbon made of Fe-based amorphous alloy (C1 (atomic %)) was experimentally produced by a liquid quenching method using a single roll device. The ribbon was an Fe-based amorphous alloy ribbon with a width of 170 mm and a thickness of 25 μm. The Curie point Tc of this Fe-based amorphous alloy was 400°C. Using this Fe-based amorphous alloy ribbon, the rotating electric machine shown below was designed.
[0090] Stator core: Outer diameter φ150mm, inner diameter φ100mm Rotor core: Outer diameter φ98.4mm ·Stacking thickness (both stator core and rotor core)…30mm Number of poles and slots: 12 poles, 18 slots Winding method: concentrated winding - Revolution speed, torque: 2000rpm, 12Nm
[0091] The inventive examples were stator cores that had been annealed in a magnetic field, and the comparative examples were stator cores that had not been annealed in a magnetic field. As shown in Fig. 4, the inventive examples were annealed in a magnetic field at 340°C for 2 hours by inserting an excitation electrode into a hollow portion of the stator core and passing current through the excitation electrode to apply a magnetic field of 800 A / m in the circumferential direction θ of the stator core. The strength of the magnetic field was the strength at the center of the core-back portion in the radial direction r.
[0092] The copper loss and iron loss of the stator core of the invention example and the stator core of the comparative example were calculated by simulation. The ratio of the copper loss and iron loss of the stator core of the invention example to the copper loss and iron loss of the stator core of the comparative example was calculated. The results are shown in FIG.
[0093] As shown in FIG. 7, with the comparative example taken as a reference, the stator core made of the Fe-based amorphous alloy of the invention example had 68% of the iron loss and 85% of the total loss of the comparative example, and thus exhibited excellent characteristics.
[0094] In addition, the ratio (Wθ / Wr) of the iron loss Wθ in the circumferential direction θ to the iron loss Wr in the radial direction r of the core back portion of the stator core of the example was measured and confirmed to be less than 1.0. The measurement conditions were as described above.
[0095] In addition, when X-ray diffraction measurements were performed on the stator cores of the examples and comparative examples that had been annealed in a magnetic field, no clear diffraction peaks were observed in either the examples or the comparative examples. This meant that it could not be said that a crystalline phase had formed in the metal structure, and it was confirmed that the entire structure was amorphous.
[0096] Example 2 The magnetic field annealing conditions of Fe-based amorphous alloy ribbons were investigated. The same thin strip as in Example 1 was used as a test material.
[0097] The test material was cut to a length of 10 m and spirally wound around a quartz bobbin with an outer diameter of 60 mm to produce a wound core. After winding an excitation coil around this wound core, a magnetic field of 2000 A / m was applied to the wound core in the circumferential direction, and magnetic field annealing was performed with a holding time of 1 hour. The holding temperatures were the Curie point Tc (℃), (Tc-20) (℃), (Tc-40) (℃), (Tc-55) (℃), (Tc-70) (℃), and (Tc-100) (℃). In addition, a core that was not annealed in a magnetic field was also prepared. This was used as the reference.
[0098] The primary coil and secondary coil are wound around a wound core with 10 turns each, and the iron loss W is measured using a BH analyzer (Iwasaki Tsushin SY-8258) at a frequency of 50 Hz and a magnetic flux density of 1.0 T. 10 / 50 The results are shown in Figure 8.
[0099] As shown in FIG. 8, when the iron loss ratio of the wound core that was not annealed in a magnetic field was examined, the iron loss value decreased in the range of (Tc-20) (°C) to (Tc-100) (°C). On the other hand, although not shown in FIG. 8, when the annealing temperature was Tc (°C), the iron loss ratio was 1.23, and the iron loss increased compared to the unannealed case. More specifically, as shown in FIG. 8, by annealing in a magnetic field in which a magnetic field was applied in the circumferential direction θ of the laminate, the iron loss value decreased by about 30% compared to the unannealed case in the temperature range from (Tc-20)°C or lower to (Tc-90)°C or higher, and the iron loss value decreased by about 40% compared to the unannealed case in the range from (Tc-40)°C or lower to (Tc-70)°C or higher.
[0100] In addition, X-ray diffraction measurements were performed on the ribbons that constituted all of the wound cores used in the evaluation. No clear diffraction peaks were observed in any of the ribbons. This meant that it could not be said that a crystalline phase had formed in the metal structure, and it was confirmed that the entire structure was amorphous.
[0101] Example 3 In order to confirm the effect of improving the magnetic properties by annealing in a magnetic field, magnetic measurements were carried out under the following conditions. As test materials, Fe-based amorphous alloy ribbons having the chemical compositions shown in the following Table 1 were prepared. These Fe-based amorphous alloy ribbons were produced by a liquid quenching method using a single roll apparatus.
[0102] [Table 1]
[0103] The ribbons of Samples A to C were each cut into a square with a side length of 55 mm, and the core loss (W / kg) was measured according to the measurement method described in JIS H 7152:1996 (Method of testing magnetic properties of amorphous metal single sheet). The measurement was performed by annealing in a magnetic field under conditions of 800 A / m, 340°C, and 1 hour. The magnitude of the applied magnetic field is the magnetic field strength in the sample.
[0104] The iron loss was measured under the conditions of a magnetic flux density of 1.0 T and a frequency of 50 Hz. The direction of application of the magnetic field during magnetic annealing was defined as the circumferential direction θ, and the direction perpendicular to the circumferential direction θ, other than the thickness direction of the ribbon, was defined as the radial direction r. The iron losses Wθ and Wr were measured when the magnetic field was excited in each direction. When the ratios of Wθ and Wr (Wθ / Wr) were compared, the values were smaller than 1.0 in all of the samples A to C, as shown in FIG. 9. This indicates that the iron loss Wθ in the magnetic field application direction was smaller than the iron loss Wr perpendicular to the magnetic field application direction.
[0105] In addition, when X-ray diffraction measurements were performed on the ribbons of samples A to C after magnetic field annealing, no clear diffraction peaks were observed in any of them, so it could not be said that a crystalline phase was formed in the metal structure, and it was confirmed that the entire structure was amorphous. [Industrial Applicability]
[0106] The laminated core of the present disclosure has reduced core loss and therefore has high industrial applicability. [Explanation of symbols]
[0107] 10...Rotary electric machine 20…Stator 21...Stator core (laminated core) 22…Core back section 23…Teeth 30…Rotor 31...Rotor core 32...Permanent magnet 33...Through hole 40...Thin piece (Fe-based amorphous alloy), 41...adhesive layer 50…case 60…Rotation axis 101...rod electrode 102…Winding 103…Winding 104…Auxiliary core O…Central axis line r…Radial direction t…Axis direction θ…Circumferential direction ψ…magnetic field
Claims
1. A plurality of annular thin pieces made of an Fe-based amorphous alloy having an amorphous structure are laminated in the thickness direction, A laminated core, wherein a ratio (Wθ / Wr) of an iron loss Wθ in the circumferential direction θ of the thin pieces to an iron loss Wr in a radial direction perpendicular to the circumferential direction θ and the thickness direction of the thin pieces is less than 1.
0.
2. The laminated core is provided with an annular core back portion and a plurality of teeth portions protruding from the core back portion in the radial direction and arranged at intervals in the circumferential direction θ, The laminated core according to claim 1 , wherein a ratio (Wc / Wr) of the iron loss Wθ to the iron loss Wr in the core back portion is less than 1.
0.
3. 2. The laminated core according to claim 1, wherein the Fe-based amorphous alloy has an amorphous structure as a whole and does not contain a crystalline structure.
4. The laminated core according to claim 1 , wherein an oxide film is formed on the surface of said thin pieces.
5. 2. The laminated core according to claim 1, wherein an adhesive layer is provided between the laminae.
6. 3. The laminated core according to claim 2, wherein the core back portion between adjacent teeth among the plurality of teeth has at least one magnetic domain having a magnetic domain width of 0.3 mm or more and 3.0 mm or less, and an angle between a magnetic domain wall and a tangent to the circumferential direction θ of less than 10°.
7. 3. The laminated core according to claim 2, wherein in the core back portion between adjacent teeth among the plurality of teeth, magnetic domains having a magnetic domain width of 0.3 mm or more and 3.0 mm or less, and an angle between a magnetic domain wall and a tangent to the circumferential direction θ of less than 10°, account for 50% or more of the area.
8. A rotating electric machine comprising a stator core made of the laminated core according to any one of claims 1 to 7.
9. A magnetic field annealing process is provided in which a laminate formed by stacking a plurality of annular thin pieces made of an Fe-based amorphous alloy along the thickness direction is annealed in a magnetic field; The magnetic field annealing process is performed by applying a magnetic field in a circumferential direction θ of the laminated body, and annealing the laminated body at an annealing temperature lower than the Curie point Tc (°C) of the Fe-based amorphous alloy and equal to or higher than (Tc-100)°C. A manufacturing method for a laminated core.
10. 10. The method for manufacturing a laminated core according to claim 9, wherein the annealing temperature in the magnetic field annealing step is in the range of (Tc-20)°C or lower and (Tc-90)°C or higher.
11. 10. The method for manufacturing a laminated core according to claim 9, wherein the annealing temperature in the magnetic field annealing step is in the range of (Tc-40)°C or less and (Tc-70)°C or more.
12. The method for manufacturing a laminated core according to claim 9, wherein the magnitude of the magnetic field applied to the laminate is in the range of 100 to 10,000 A / m inside the laminate.
13. The method for manufacturing a laminated core according to claim 9, wherein the magnitude of the magnetic field applied to the laminate is in the range of 400 to 7500 A / m inside the laminate.
14. The magnetic field annealing step includes: A first step of applying a magnetic field to the laminate along the circumferential direction θ; A second step of heating the laminate to which the magnetic field has been applied up to the annealing temperature; A third step of annealing the laminate to which the magnetic field has been applied at the annealing temperature for 1 to 8 hours; A fourth step of cooling the laminate to which the magnetic field has been applied to a temperature of 200° C. or lower; a fifth step of stopping application of the magnetic field to the laminate after the fourth step; The method for manufacturing a laminated core according to claim 9, comprising:
15. In the second step, The method for producing a laminated core according to claim 14, wherein the average heating rate is 1 to 10° C. / min.
Citation Information
Patent Citations
Magnetic material and its manufacture
JP1987167840A
Stator
JP2006325295A
Exciter
JP2007202292A
Fe-BASED AMORPHOUS ALLOY HAVING EXCELLENT SOFT MAGNETIC CHARACTERISTICS AND PROCESSABILITY, Fe-BASED AMORPHOUS ALLOY THIN STRIP HAVING EXCELLENT SOFT MAGNETIC CHARACTERISTICS AND PROCESSABILITY, WOUND CORE, STACKED CORE AND ROTARY ELECTRIC MACHINE
JP2023107731A
Stator, electric motor, compressor, and refrigerating / air conditioning device
WO2018138864A1