Forged Steel Roll
A forged steel roll with a tailored chemical composition and grain boundary length effectively addresses crack issues in cold rolling, improving crack resistance and reducing consumption rates by suppressing crack initiation and propagation.
Patent Information
- Application Number
- JP2024554714
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-02-01
- Filing Date
- 2023-10-30
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2043-10-30
AI Technical Summary
Forged steel rolls used in cold rolling applications experience surface roughness decrease over time, leading to slip and seizure, which causes thermal shock, cracks, and spalling, increasing roll consumption rates.
A forged steel roll with a specific chemical composition (C: 0.70~1.50%, Si: 0.20~1.50%, Mn: 0.20~1.50%, P: 0.030% or less, S: 0.0200% or less, Al: 0.050% or less, N: 0.2000% or less, O: 0.0050% or less, Cr: 2.80~8.00%, Mo: 0.40~3.00%, Cu: 0.100% or less, B: 0.0100% or less, Ni: 0~1.20%, V: 0~2.00%, Nb: 0~0.50%, Fe and impurities) and an average high-angle grain boundary length of 2500 to 9000 mm in the surface layer to suppress crack initiation and propagation due to thermal shock.
The solution effectively suppresses crack occurrence and propagation, enhancing crack resistance and reducing roll consumption, with improved high-temperature hardness and wear resistance.
Smart Images

Figure 0007590689000004 
Figure 0007590689000005 
Figure 0007590689000006
Abstract
Description
[Technical field]
[0001] The present disclosure relates to forged steel rolls, and more particularly, to forged steel rolls suitable for cold rolling applications. [Background technology]
[0002] Forged steel rolls are used as rolling rolls, typically cold rolling rolls. When forged steel rolls are used for cold rolling over a long period of time, the surface roughness of the forged steel roll gradually decreases with the long-term use. If the surface roughness of the forged steel roll decreases, slippage may occur between the forged steel roll and the material being rolled. If slippage occurs, poor engagement may occur. Also, seizure may occur between the forged steel roll and the material being rolled during rolling.
[0003] When slippage and / or seizure occurs, a thermal shock is applied to the roll surface. This thermal shock may cause a crack to occur in the surface layer of the forged steel roll. If the forged steel roll in which a crack has occurred continues to be used, the crack will gradually grow. If the crack continues to grow, a part of the surface layer of the roll may peel off. This phenomenon is called spalling.
[0004] When a crack is found in a forged steel roll, the roll surface is ground according to the depth of the crack to prevent spalling from occurring, and the crack is removed. If the crack is deep, the amount of roll grinding required to remove the crack increases. If the amount of roll grinding increases, the roll consumption rate (kg / ton) deteriorates. Therefore, there is a demand for a forged steel roll that can prevent the occurrence and progression of cracks due to thermal shock. Hereinafter, in this specification, the ability to prevent the occurrence and progression of cracks due to thermal shock is also referred to as "excellent crack resistance."
[0005] Techniques for improving resistance to thermal shock in forged steel rolls have been proposed in JP-A-2-185928 (Patent Document 1), JP-A-1-234548 (Patent Document 2), JP-A-5-086439 (Patent Document 3), JP-A-5-132738 (Patent Document 4), and JP-A-2010-242166 (Patent Document 5).
[0006] In the method for manufacturing a forged steel roll disclosed in Patent Document 1, the surface layer of a forged steel material containing 0.7-1.0% C, 0.15-1.5% Si, 0.15-1.5% Mn, 3.0-6.0% Cr, 3.0-5.0% Mo, and 1.2% or less V is quenched. The quenched forged steel material is subjected to sub-zero treatment. The forged steel material after the sub-zero treatment is tempered at a temperature of 180°C or higher. In Patent Document 1, the tempering temperature is increased by 40°C or higher than the conventional temperature by increasing the tempering softening resistance. This increases the resistance to cracking.
[0007] The forged steel roll disclosed in Patent Document 2 contains, by weight, C: 0.45-0.95%, Mn: 1.0% or less, Cr: 4.5-6.0%, Mo: 0.3-0.7%, Ni: 0.6-2.0%, with the balance being Fe and impurities, and further, the Si content is suppressed to less than 0.1%. In Patent Document 2, the Si content as an impurity is suppressed to less than 0.1%, and the Ni content is set to 0.6-2.0%, thereby improving the spalling resistance and thermal shock crack resistance of the forged steel roll.
[0008] The forged steel roll disclosed in Patent Document 3 contains C: 0.90-1.10wt%, Si: 0.5-1.0wt%, Mn: 0.1-1.0wt%, Cr: 4.0-6.0wt%, Mo: 3.0-6.0wt%, V: 0.5-2.0wt%, Co: 1.0-3.0wt%, and the balance is Fe and impurities. In Patent Document 3, the forged steel roll has the above-mentioned chemical composition, thereby improving the thermal shock resistance of the forged steel roll.
[0009] The forged steel roll disclosed in Patent Document 4 is composed of, by weight, 0.7-1.4% C, 0.8-2.5% Si, 0.8-2.5% Mn, 0.5-2.5% Ni, 2.5-6.5% Cr, 2.5-8.5% Mo, 0.3-3.0% W, 0.5-4.5% V, and the balance being Fe and impurities. This forged steel roll contains more than 15% to 40% of retained austenite due to subzero post-tempering. In Patent Document 4, the retained austenite is contained to suppress the propagation of cracks.
[0010] The forged steel roll disclosed in Patent Document 5 contains, in mass%, C: 0.6-1.2%, Si: 0.4-0.8%, Mn: 0.4-1.0%, Ni: 0.4-1.0%, Cr: 3.0-6.0%, Mo: 0.2-0.5%, and the balance is Fe and impurities. In this forged steel roll, the average particle size of the carbides dispersed in the metal structure of the roll surface layer within 50 mm from the roll surface is 1 μm or less. Furthermore, the area fraction of the dispersed carbides is 5-30%. In Patent Document 5, the occurrence of cracks is suppressed by dispersing the above-mentioned carbides in the roll surface layer. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] Japanese Patent Application Publication No. 2-185928 [Patent Document 2] Japanese Patent Application Publication No. 1-234548 [Patent Document 3] Japanese Patent Application Publication No. 5-086439 [Patent Document 4] Japanese Patent Application Publication No. 5-132738 [Patent Document 5] JP 2010-242166 A Summary of the Invention [Problem to be solved by the invention]
[0012] However, it may be possible to suppress both the occurrence and propagation of cracks due to thermal shock by a means different from the means described in Patent Documents 1 to 5.
[0013] An object of the present invention is to provide a forged steel roll which is capable of suppressing the occurrence of cracks due to thermal shock and also suppressing the propagation of the cracks. [Means for solving the problem]
[0014] The forged steel roll of the present disclosure is Chemical composition, in mass%, C: 0.70-1.50%, Si: 0.20-1.50%, Mn: 0.20-1.50%, P: 0.030% or less, S: 0.0200% or less, Al: 0.050% or less, N: 0.2000% or less, O: 0.0050% or less, Cr: 2.80~8.00%, Mo: 0.40-3.00%, Cu: 0.100% or less, B: 0.0100% or less, Ni: 0-1.20%, V: 0~2.00%, Nb: 0 to 0.50%, and The balance is composed of Fe and impurities. The surface layer of the forged steel roll is 1 mm 2 The length of the high angle grain boundary per unit area is 2500-9000 mm. Effect of the Invention
[0015] In the forged steel roll according to the present invention, the occurrence of cracks due to thermal shock can be suppressed, and the propagation of the cracks can also be suppressed. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a diagram showing the configuration of a drop-weight frictional thermal shock tester used in the crack resistance evaluation tests in the examples. [Diagram 2] FIG. 2 is a schematic diagram of the contact area obtained in a crack resistance evaluation test using the drop weight type frictional thermal shock tester of FIG. [Diagram 3] FIG. 3 is a cross-sectional view of the contact area shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The present inventors first conducted a study on a forged steel roll having excellent crack resistance from the viewpoint of chemical composition. As a result, the present inventors considered that if the forged steel roll has a chemical composition containing, in mass%, C: 0.70 to 1.50%, Si: 0.20 to 1.50%, Mn: 0.20 to 1.50%, P: 0.030% or less, S: 0.0200% or less, Al: 0.050% or less, N: 0.2000% or less, O: 0.0050% or less, Cr: 2.80 to 8.00%, Mo: 0.40 to 3.00%, Cu: 0.100% or less, B: 0.0100% or less, Ni: 0 to 1.20%, V: 0 to 2.00%, and Nb: 0 to 0.50%, with the balance being Fe and impurities, excellent crack resistance may be obtained.
[0018] Therefore, the present inventors further investigated and examined the mechanism of crack generation and crack growth when a thermal shock is applied to the surface layer of a forged steel roll satisfying the above-mentioned chemical composition.
[0019] Here, the inventors paid attention to the grain boundary length in the surface layer of the forged steel roll. The inventors considered that the grain boundary length in the surface layer has an effect on the initiation and propagation of cracks. Therefore, the inventors investigated the initiation and propagation of cracks due to thermal shock and the grain boundary length in the surface layer within 1 mm 2 The inventors conducted an investigation and study on the relationship between the length of high-angle grain boundaries per unit area and the orientation difference between adjacent crystal grains of 15° or more. As a result of the investigation and study, the inventors have obtained the following findings.
[0020] 1mm 2The high angle grain boundary length per mm affects both the occurrence and propagation of cracks due to thermal shock. Specifically, if the high angle grain boundary length is too small, the propagation of cracks is suppressed, but the frequency of crack occurrence increases. On the other hand, if the high angle grain boundary length is too large, the frequency of crack occurrence is suppressed, but the cracks tend to propagate. Therefore, in order to suppress the occurrence of cracks due to thermal shock and also to suppress the propagation of cracks in a forged steel roll having the above-mentioned chemical composition, it is necessary to set the high angle grain boundary length per mm to 1 mm. 2 It is effective to adjust the length of the high angle grain boundary per unit area within an appropriate range.
[0021] Based on the above findings, the present inventors have further investigated. As a result, in the forged steel rolls satisfying the above-mentioned chemical composition, 2 The inventors have found that, when the high angle grain boundary length per unit area is 2500 to 9000 mm, even if a thermal shock is applied during use, the occurrence of cracks can be suppressed and the propagation of the cracks can also be suppressed, thereby obtaining excellent crack resistance. The forged steel roll of this embodiment, which has been completed based on the above findings, has the following configuration.
[0022] The forged steel roll of the first configuration is Chemical composition, in mass%, C: 0.70-1.50%, Si: 0.20-1.50%, Mn: 0.20-1.50%, P: 0.030% or less, S: 0.0200% or less, Al: 0.050% or less, N: 0.2000% or less, O: 0.0050% or less, Cr: 2.80~8.00%, Mo: 0.40-3.00%, Cu: 0.100% or less, B: 0.0100% or less, Ni: 0-1.20%, V: 0~2.00%, Nb: 0 to 0.50%, and The balance is composed of Fe and impurities. The surface layer of the forged steel roll is 1 mm 2 The length of the high angle grain boundary per unit area is 2500-9000 mm.
[0023] The second configuration of forged steel rolls is A forged steel roll of a first configuration, The above chemical composition is Ni: 0.01 to 1.20%, V: 0.01 to 2.00%, and Nb: 0.01 to 0.50%.
[0024] The third configuration of forged steel rolls is Forged steel rolls of first and second configurations, The N content is 0.0200% or less by mass.
[0025] The fourth configuration of forged steel rolls is A forged steel roll having any one of the first to third configurations, The Si content is 0.40 to 1.50% by mass, The above chemical composition satisfies formula (1), The Vickers hardness at 400℃ is 400HV or more. 4.50≦Cr+Mo+V+Nb≦13.50 (1) Here, each element symbol in the formula is substituted with the content of the corresponding element in mass%. If an element is not contained, the corresponding element symbol is substituted with "0".
[0026] The forged steel roll of this embodiment will be described in detail below. "%" for elements means mass % unless otherwise specified.
[0027] [Features of the forged steel roll of this embodiment] The forged steel roll of this embodiment satisfies the following features 1 and 2. (Feature 1) The chemical composition, in mass%, is C: 0.70 to 1.50%, Si: 0.20 to 1.50%, Mn: 0.20 to 1.50%, P: 0.030% or less, S: 0.0200% or less, Al: 0.050% or less, N: 0.2000% or less, O: 0.0050% or less, Cr: 2.80 to 8.00%, Mo: 0.40 to 3.00%, Cu: 0.100% or less, B: 0.0100% or less, Ni: 0 to 1.20%, V: 0 to 2.00%, and Nb: 0 to 0.50%, with the remainder being Fe and impurities. (Feature 2) 1mm of the surface of the forged steel roll 2 The length of the high angle grain boundary per unit area is 2500-9000 mm. Features 1 and 2 will be explained below.
[0028] [(Feature 1) Chemical composition] The chemical composition of the forged steel roll of this embodiment contains the following elements.
[0029] C: 0.70-1.50% Carbon (C) increases the hardness of the surface layer of the forged steel roll. If the C content is less than 0.70%, the above effect cannot be sufficiently obtained. On the other hand, if the C content exceeds 1.50%, coarse carbides are generated. In this case, sufficient hardness may not be obtained in the surface layer of the forged steel roll. Therefore, the C content is 0.70 to 1.50%. The lower limit of the C content is preferably 0.75%, more preferably 0.80%, still more preferably 0.85%, and still more preferably 0.90%. The upper limit of the C content is preferably 1.45%, more preferably 1.40%, more preferably 1.35%, more preferably 1.20%, more preferably 1.15%, more preferably 1.10%, and more preferably 1.05%.
[0030] Silicon: 0.20 to 1.50% Silicon (Si) deoxidizes steel at the molten steel stage. Si also enhances the hardenability of steel. If the Si content is less than 0.20%, the above effects are not sufficiently obtained. On the other hand, if the Si content exceeds 1.50%, the toughness of the forged steel roll decreases. Therefore, the Si content is 0.20 to 1.50%. The lower limit of the Si content is preferably 0.25%, more preferably 0.30%, more preferably 0.40%, more preferably 0.45%, more preferably 0.50%, more preferably 0.55%, more preferably 0.60%, more preferably 0.65%, more preferably 0.70%, and more preferably 0.75%. When the Si content is 0.40% or more, a sufficient amount of dissolved Si can be obtained. In this case, the high-temperature hardness can be increased in the surface layer of the forged steel roll, provided that the formula (1) described below is satisfied. Therefore, the crack resistance is further improved. The upper limit of the Si content is preferably 1.45%, more preferably 1.40%, more preferably 1.35%, more preferably 1.30%, more preferably 1.25%, more preferably 1.20%, and more preferably 1.15%.
[0031] Mn: 0.20 to 1.50% Manganese (Mn) improves the hardenability of steel. If the Mn content is less than 0.20%, the above effect cannot be sufficiently obtained. On the other hand, if the Mn content exceeds 1.50%, the toughness of the forged steel roll decreases. Therefore, the Mn content is 0.20 to 1.50%. The lower limit of the Mn content is preferably 0.25%, more preferably 0.30%, further preferably 0.35%, and further preferably 0.40%. The upper limit of the Mn content is preferably 1.45%, more preferably 1.40%, still more preferably 1.35%, still more preferably 1.30%, and still more preferably 1.25%.
[0032] P:0.030% or less Phosphorus (P) is an impurity. P segregates at grain boundaries and reduces the toughness of forged steel rolls. Therefore, the P content is 0.030% or less. The P content is preferably as low as possible. However, excessive reduction in the P content increases the production cost. Therefore, in consideration of normal industrial production, the lower limit of the P content is preferably more than 0%, more preferably 0.001%, and even more preferably 0.002%. The upper limit of the P content is preferably 0.025%, and more preferably 0.020%.
[0033] S: 0.0200% or less Sulfur (S) is an impurity. S segregates at grain boundaries and reduces the toughness and hot workability of forged steel rolls. Therefore, the S content is 0.0200% or less. The S content is preferably as low as possible. However, excessive reduction in the S content increases the production cost. Therefore, in consideration of normal industrial production, the preferred lower limit of the S content is more than 0%, more preferably 0.0001%, more preferably 0.0002%, and even more preferably 0.0003%. The upper limit of the S content is preferably 0.0050%, more preferably 0.0040%, and further preferably 0.0030%.
[0034] Al: 0.050% or less Aluminum (Al) deoxidizes steel during the molten steel stage. However, if the Al content exceeds 0.050%, coarse Al nitrides are formed. In this case, the toughness of the steel material decreases. Therefore, the Al content is 0.050% or less. The lower limit of the Al content is preferably more than 0%, more preferably 0.001%, more preferably 0.002%, more preferably 0.005%, and even more preferably 0.010%. The upper limit of the Al content is preferably 0.040%, more preferably 0.035%, further preferably 0.030%, and further preferably 0.025%. In this specification, the Al content means the total Al content in the steel.
[0035] N: 0.2000% or less Nitrogen (N) increases the strength of the forged steel roll through solid solution strengthening. In particular, it increases the high temperature hardness of the forged steel roll. However, if the N content exceeds 0.2000%, coarse nitrides are formed. In this case, the toughness of the forged steel roll decreases. Therefore, the N content is 0.2000% or less. The lower limit of the N content is preferably more than 0%, more preferably 0.0001%, more preferably 0.0005%, more preferably 0.0010%, more preferably 0.0025%, more preferably 0.0035%, and more preferably 0.0045%. The upper limit of the N content is preferably 0.1900%, more preferably 0.1800%, more preferably 0.1500%, more preferably 0.1200%, more preferably 0.1000%, more preferably 0.0500%, more preferably 0.0200%, more preferably 0.0150%, and more preferably 0.0100%.
[0036] O: 0.0050% or less Oxygen (O) is an impurity. O forms oxides and reduces the toughness of forged steel rolls. Therefore, the O content is 0.0050% or less. The O content is preferably as low as possible. However, excessive reduction in the O content increases the production cost. Therefore, in consideration of normal industrial production, the lower limit of the O content is preferably more than 0%, more preferably 0.0001%, more preferably 0.0005%, more preferably 0.0007%, and more preferably 0.0010%. The upper limit of the O content is preferably 0.0040%, more preferably 0.0035%, and further preferably 0.0030%.
[0037] Cr: 2.80~8.00% Chromium (Cr) forms carbides to increase the wear resistance of the forged steel roll. Furthermore, Cr increases the tempering softening resistance of steel through solid solution, and increases the high-temperature hardness of the surface layer of the forged steel roll. If the Cr content is less than 2.80%, the above effects cannot be sufficiently obtained. On the other hand, if the Cr content exceeds 8.00%, coarse carbides are generated. In this case, the grindability and toughness of the forged steel roll decrease. Therefore, the Cr content is 2.80 to 8.00%. The lower limit of the Cr content is preferably 2.85%, more preferably 3.00%, further preferably 3.50%, and further preferably 4.00%. The upper limit of the Cr content is preferably 7.50%, more preferably 7.00%, more preferably 6.50%, more preferably 6.00%, and even more preferably 5.50%.
[0038] Mo: 0.40-3.00% Molybdenum (Mo) forms carbides to increase the wear resistance of the forged steel roll. Mo also increases the high-temperature hardness of the surface layer of the forged steel roll by solid solution. If the Mo content is less than 0.40%, the above effect cannot be sufficiently obtained. On the other hand, if the Mo content exceeds 3.00%, coarse carbides are generated. In this case, the grindability and toughness of the forged steel roll are reduced. Therefore, the Mo content is 0.40 to 3.00%. The lower limit of the Mo content is preferably 0.45%, more preferably 0.50%, and further preferably 0.55%. The upper limit of the Mo content is preferably 2.80%, more preferably 2.60%, more preferably 2.40%, more preferably 2.20%, more preferably 2.00%, more preferably 1.90%, more preferably 1.80%, more preferably 1.70%, and more preferably 1.60%.
[0039] Cu:0.100% or less Copper (Cu) is an impurity. Cu reduces the hot workability of steel. Therefore, the Cu content is 0.100% or less. The Cu content is preferably as low as possible. However, excessive reduction in the Cu content increases the manufacturing cost. Therefore, in consideration of normal industrial production, the preferred lower limit of the Cu content is more than 0%, more preferably 0.001%, more preferably 0.005%, more preferably 0.010%, and more preferably 0.015%. The upper limit of the Cu content is preferably 0.095%, more preferably 0.090%, more preferably 0.085%, more preferably 0.080%, more preferably 0.075%, and more preferably 0.070%.
[0040] B: 0.0100% or less Boron (B) is an impurity. B reduces the toughness of forged steel rolls. Therefore, the B content is 0.0100% or less. The B content is preferably as low as possible. However, excessive reduction in the B content increases the manufacturing cost. Therefore, in consideration of normal industrial production, the preferred lower limit of the B content is more than 0%, more preferably 0.0001%, more preferably 0.0005%, more preferably 0.0010%, more preferably 0.0015%, and more preferably 0.0020%. The upper limit of the B content is preferably 0.0090%, more preferably 0.0085%, and further preferably 0.0080%.
[0041] The balance of the chemical composition of the forged steel roll according to the present embodiment is composed of Fe and impurities. Here, the impurities refer to substances that are mixed in from raw materials such as ore and scrap, or from the manufacturing environment, during industrial production of the forged steel roll, and are permissible within a range that does not adversely affect the forged steel roll of the present embodiment.
[0042] [About optional elements] The chemical composition of the forged steel roll of this embodiment further includes, instead of a part of Fe, Ni: 0-1.20%, V: 0 to 2.00%, and Nb: 0 to 0.50%. The optional elements in each group will be described below.
[0043] [Group 1: Ni] Ni: 1.20% or less Nickel (Ni) is an optional element and may not be contained. In other words, the Ni content may be 0%. When contained, that is, when the Ni content is more than 0%, Ni enhances the hardenability of the steel. Even if even a small amount of Ni is contained, the above effect can be obtained to some extent. However, when the Ni content exceeds 1.20%, excessive retained austenite is formed. In this case, the hardness of the forged steel roll decreases. Therefore, the Ni content is 0 to 1.20%, and when contained, the Ni content is 1.20% or less. The lower limit of the Ni content is preferably 0.01%, more preferably 0.05%, more preferably 0.10%, more preferably 0.15%, and more preferably 0.20%. The upper limit of the Ni content is preferably 1.15%, more preferably 1.10%, more preferably 1.05%, more preferably 1.00%, more preferably 0.95%, more preferably 0.90%, more preferably 0.85%, more preferably 0.80%, more preferably 0.75%, and more preferably 0.70%.
[0044] [Group 2: V and Nb] V:2.00% or less Vanadium (V) is an optional element and may not be contained. In other words, the V content may be 0%. When vanadium is contained, that is, when the V content is more than 0%, V forms carbides to increase the wear resistance of the forged steel roll. V also increases the high-temperature hardness of the forged steel roll by solid solution. If even a small amount of V is contained, the above effects can be obtained to some extent. However, if the V content exceeds 2.00%, coarse carbides are generated. In this case, the grindability and toughness of the forged steel roll are reduced. Therefore, the V content is 0 to 2.00%, and when contained, the V content is 2.00% or less. The lower limit of the V content is preferably 0.01%, more preferably 0.05%, more preferably 0.10%, more preferably 0.15%, more preferably 0.20%, and more preferably 0.25%. The upper limit of the V content is preferably 1.80%, more preferably 1.60%, more preferably 1.50%, more preferably 1.40%, more preferably 1.30%, and more preferably 1.20%.
[0045] Nb: 0.50% or less Niobium (Nb) is an optional element and may not be contained. That is, the Nb content may be 0%. When it is contained, that is, when the Nb content is more than 0%, Nb forms carbides to increase the wear resistance of the forged steel roll. Nb further increases the high-temperature hardness of the forged steel roll by solid solution. If even a small amount of Nb is contained, the above effect can be obtained to some extent. However, if the Nb content exceeds 0.50%, coarse carbides are generated. In this case, the grindability and toughness of the forged steel roll are reduced. Therefore, the Nb content is 0 to 0.50%, and when it is contained, the Nb content is 0.50% or less. The lower limit of the Nb content is preferably 0.01%, more preferably 0.05%, more preferably 0.10%, more preferably 0.15%, more preferably 0.20%, and more preferably 0.25%. The upper limit of the Nb content is preferably 0.45%, more preferably 0.42%, still more preferably 0.40%, still more preferably 0.38%, and still more preferably 0.36%.
[0046] (Feature 2) Surface 1mm 2 [Length of high angle grain boundaries per unit area] In the forged steel roll of this embodiment, the surface layer of 1 mm 2 The length of a high-angle grain boundary per unit area is 2500 to 9000 mm. Here, the "length of a high-angle grain boundary" means the length of a grain boundary where the difference in orientation between adjacent crystal grains is 15° or more.
[0047] 1mm 2 When the high angle grain boundary length per unit area exceeds 9000 mm, the high angle grain boundary length is too long. In this case, the resistance to grain boundary slippage increases. Therefore, the frequency of cracks along the grain boundaries is suppressed. However, at the moment when a crack occurs, the accumulated excessive energy is released, causing the grain boundaries to slip significantly. As a result, the crack becomes excessively deep, and crack resistance decreases.
[0048] On the other hand, 1mm 2 When the high angle grain boundary length per unit area is less than 2500 mm, the high angle grain boundary length is too short. In this case, the propagation of cracks is suppressed. However, the resistance to slippage of the grain boundaries is small, so the frequency of crack occurrence increases. As a result, excessive cracks occur, and crack resistance decreases.
[0049] The surface 1mm 2 If the high angle grain boundary length per unit area is 2500 to 9000 mm, the frequency of crack occurrence is sufficiently suppressed, and even if a crack occurs, the crack growth is sufficiently suppressed, resulting in sufficient crack resistance.
[0050] 1mm 2 The lower limit of the high angle grain boundary length per unit area is preferably 3000 mm, more preferably 3200 mm, more preferably 3300 mm, more preferably 3400 mm, and even more preferably 3500 mm. 1mm 2 The upper limit of the high angle grain boundary length per unit area is preferably 8800 mm, more preferably 8600 mm, more preferably 8400 mm, more preferably 8300 mm, more preferably 8200 mm, more preferably 8100 mm, and more preferably 8000 mm.
[0051] [1mm of the surface 2 Measurement method for high angle grain boundary length per unit area] The surface layer of the forged steel roll of this embodiment is 1 mm 2 The length of the high angle grain boundary per unit area is determined by the following method.
[0052] Five test pieces are taken from the surface of the barrel of the forged steel roll, each of which is located at a depth of 1 mm. The surface of each test piece that is located at a depth of 1 mm from the surface of the forged steel roll is defined as the observation surface. The observation surface of each test piece is mirror-polished with diamond paste. After mirror polishing, the observation surface is chemically polished with colloidal silica liquid to remove any process-affected layers introduced during mirror polishing.
[0053] The observation field of the polished observation surface, which corresponds to a depth position of 1 mm from the surface of the forged steel roll, is observed at 5000x magnification using SEM / EBSD / OIM. The observation field is 20 μm x 20 μm, and the measurement interval between adjacent measurement points is 0.03 μm. The acceleration voltage for EBSD measurement is 25 kV.
[0054] Using EBSD analysis software, the crystal orientation for each measurement in the observation field is obtained. Based on the crystal orientation of each measurement point, a grain boundary where the crystal orientation difference between adjacent crystal grains is 15° or more is defined as a "high-angle grain boundary". The total length of the high-angle grain boundaries in the observation field is measured. Based on the observation field area and the measured total length of the high-angle grain boundaries, a 1 mm 2 The arithmetic mean of the high angle boundary lengths obtained for five test pieces was calculated for each 1 mm 2 This is defined as the high angle grain boundary length (mm) per unit area.
[0055] The EBSD analysis software may be any known software. For example, a known EBSD analysis software is OIM Analysis, a product name of TSL Solutions Co., Ltd. In order to eliminate the influence of measurement errors due to noise on the data, cleanup processing is not performed, and data with an image quality (IQ value) of 11,000 or less, which is also measured, is excluded from the analysis.
[0056] [Effects of the forged steel roll of this embodiment] The forged steel roll of this embodiment satisfies Features 1 and 2. Therefore, the forged steel roll of this embodiment has excellent crack resistance. Specifically, when the forged steel roll is used, the frequency of crack occurrence is sufficiently suppressed, and even if a crack occurs, the growth of the crack is sufficiently suppressed. As a result, excellent crack resistance is obtained.
[0057] [Preferable form of the forged steel roll of this embodiment] The forged steel roll of the present embodiment preferably further satisfies the following feature 3. (Feature 3) In the chemical composition, the Si content is 0.40 to 1.50% by mass, satisfying formula (1). Furthermore, the Vickers hardness at 400°C is 400HV or more. 4.50≦Cr+Mo+V+Nb≦13.50 (1) Here, each element symbol in the formula is substituted with the content of the corresponding element in mass%. If an element is not contained, the corresponding element symbol is substituted with "0".
[0058] If the forged steel roll of this embodiment satisfies not only Features 1 and 2 but also Feature 3, the high-temperature hardness of the surface layer of the forged steel roll is further increased. As a result, the frequency of crack occurrence during use of the forged steel roll is further suppressed, and the crack resistance is further improved. Feature 3 includes the following three requirements. (Requirement 1) The Si content is 0.40 to 1.50% by mass. (Requirement 2) The chemical composition satisfies formula (1). 4.50≦Cr+Mo+V+Nb≦13.50 (1) Here, each element symbol in the formula is substituted with the content of the corresponding element in mass%. If an element is not contained, the corresponding element symbol is substituted with "0". When the chemical composition of the forged steel roll does not contain the optional elements V and Nb, that is, when the chemical composition of the forged steel roll is composed only of essential elements, formula (1) is defined as follows. 4.50≦Cr+Mo≦13.50 (1) Here, each element symbol in the formula is substituted with the content of the corresponding element in mass %. (Requirement 3) The Vickers hardness at 400°C is 400HV or more. Requirements 1 to 3 of Feature 3 will be explained below.
[0059] [(Requirement 1) Regarding Si content] If the Si content is 0.40% or more, the amount of solid-solubilized Si in the forged steel roll increases. As a result, the high-temperature hardness of the forged steel roll increases. In this case, the frequency of cracks occurring in the surface layer of the forged steel roll is further suppressed. Therefore, the preferred Si content is 0.40 to 1.50%.
[0060] [Regarding formula (1) (Requirement 2)] Let F1 be defined as follows: F1 = Cr + Mo + V + Nb F1 is an index of high-temperature hardness of the forged steel roll. When the chemical composition of the forged steel roll does not contain optional elements V and Nb, that is, when the chemical composition of the forged steel roll is composed of only essential elements, F1 is defined as follows: F1=Cr+Mo
[0061] Cr, Mo, V and Nb form carbides to increase the wear resistance of the forged steel roll. Cr, Mo, V and Nb further form a solid solution to increase the high-temperature hardness of the forged steel roll. That is, Cr, Mo, V and Nb increase the wear resistance by forming carbides and increase the high-temperature hardness by forming a solid solution.
[0062] If F1 is 4.50 or more, Cr, Mo, V and Nb are not only distributed among the carbide forming elements but also among the solid solution elements. Therefore, if F1 is 4.50 or more, the high temperature hardness of the forged steel roll is further increased. As a result, the frequency of cracks occurring during use of the forged steel roll is further suppressed, and the crack resistance is further increased.
[0063] On the other hand, if F1 is equal to or less than 13.50, which is the total of the upper limits of the Cr, Mo, V and Nb contents, coarsening of carbides of Cr, Mo, V and Nb is sufficiently suppressed, and therefore sufficient grindability and toughness are maintained in the forged steel roll.
[0064] The more preferred lower limit of F1 is 4.70, more preferably 4.90, more preferably 5.10, more preferably 5.30, more preferably 5.50, more preferably 5.60, more preferably 5.70, more preferably 5.80, and more preferably 5.90. The more preferred upper limit of F1 is 13.40, more preferably 13.30, more preferably 13.20, more preferably 13.10, more preferably 13.00, more preferably 12.90, more preferably 12.80, more preferably 12.70, and more preferably 12.60.
[0065] When F1=Cr+Mo, the upper limit is more preferably 11.00, even more preferably 10.80, and even more preferably 10.50.
[0066] [(Requirement 3) Vickers hardness at 400℃] In conventional forged steel rolls, when the temperature rises from room temperature, the hardness drops sharply at around 400°C. As a result, sufficient crack resistance is not obtained. If the hardness at 400°C is high, the frequency of crack occurrence in the surface layer of the forged steel roll is further suppressed. In the case of a forged steel roll that satisfies Features 1 and 2, if it satisfies Requirements 1 and 2 and further has a Vickers hardness of 400HV or more at 400°C (i.e., if it satisfies Feature 3), the high-temperature hardness of the forged steel roll is further increased. As a result, the frequency of crack occurrence is further suppressed and crack resistance is further improved.
[0067] The lower limit of the Vickers hardness at 400° C. is preferably 405 HV, more preferably 410 HV, more preferably 415 HV, more preferably 420 HV, and even more preferably 425 HV. The upper limit of the Vickers hardness at 400° C. is not particularly limited. The upper limit of the Vickers hardness at 400° C. is preferably 600 HV, more preferably 550 HV, more preferably 520 HV, and even more preferably 500 HV. In this case, the toughness of the forged steel roll is further increased.
[0068] [Method of measuring Vickers hardness at 400℃] The Vickers hardness of the forged steel roll at 400°C is determined by the following method. A test piece is taken that includes the area from the surface of the forged steel roll to a depth of 1 mm. The size of the test piece is 5 mm x 5 mm x 10 mm, and the measurement surface is 5 mm x 10 mm. The measurement surface is a cross section perpendicular to the surface of the forged steel roll, and includes the surface of the forged steel roll and a depth of 1 mm from the surface. The test piece with the thermocouple attached and the indenter are placed in a vacuum (3 x 10 -5The specimen is heated from room temperature to 400°C at a pressure of 10 Torr and held at 400°C for 5 minutes. After holding, the Vickers hardness of the surface of the specimen in the surface layer region is determined by a high-temperature Vickers hardness test method conforming to JIS Z 2252:1991. Specifically, the Vickers hardness is measured at five arbitrary points 1 mm deep from the surface of the forged steel roll on the measurement surface of the specimen. The test force is 300 gf. The arithmetic average of the five obtained Vickers hardness values is regarded as the Vickers hardness (unit: HV) at 400°C.
[0069] [Regarding the microstructure of the surface layer of the forged steel roll of this embodiment] The microstructure of the surface layer of the forged steel roll of this embodiment is mainly composed of martensite and / or bainite. "Mainly composed of martensite and / or bainite" means that the total area ratio of martensite and bainite is 85% or more. In the microstructure, structures other than martensite and bainite include, for example, retained austenite and carbides.
[0070] [Method for measuring the total area ratio of martensite and bainite in the surface layer of a forged steel roll] The total area ratio of martensite and bainite in the surface layer of the forged steel roll of this embodiment is determined by the following method. A test piece is taken from the surface of the barrel of the forged steel roll, including a position 1 mm deep from the surface. The surface of the test piece including a position 1 mm deep from the surface of the forged steel roll is defined as the observation surface. The observation surface is mirror-polished. After mirror-polishing, the observation surface is etched using 2% nitric acid alcohol (Nital etching solution). Of the etched observation surface, five arbitrary observation fields (400 μm x 600 μm) 1 mm deep from the surface of the barrel of the forged steel roll are observed with a 200x optical microscope.
[0071] Each observation field is etched with Murakami's reagent. Murakami's reagent colors the carbides in the observation field. This makes it easy to distinguish the carbides from other phases by contrast. Then, the carbides are identified in each observation field. The area ratio of the carbides is calculated based on the total area of the carbides identified in all observation fields and the total area of all observation fields.
[0072] Furthermore, the area ratio of the retained austenite is determined by the following X-ray diffraction method. A test piece including a depth position of 1 mm from the surface of the barrel of the forged steel roll is taken. The size of the test piece is not particularly limited, but is, for example, 15 mm x 15 mm x 10 mm thick. In this case, the thickness direction of the test piece is the radial direction of the forged steel roll. Using the obtained test piece, the X-ray diffraction intensity of each of the (200) plane of the α phase, the (211) plane of the α phase, the (220) plane of the α phase, the (200) plane of the γ phase, the (220) plane of the γ phase, and the (311) plane of the γ phase is measured, and the integrated intensity of each plane is calculated. In the measurement of the X-ray diffraction intensity, the target of the X-ray diffraction device is Co (CoKα ray), and the output is 40 kV-135 mA. After the calculation, the volume ratio Vγ (%) of the retained austenite is calculated using formula (I) for each combination (3 x 3 = 9 pairs) of each plane of the α phase and each plane of the γ phase. The average value of the nine sets of volume fractions of retained austenite Vγ is defined as the volume fraction of retained austenite (%). Vγ=100 / {1+(Iα×Rγ) / (Iγ×Rα)} (I) Here, Iα is the integral intensity of the α phase. Rα is the crystallographic theoretical calculation value of the α phase. Iγ is the integral intensity of the γ phase. Rγ is the crystallographic theoretical calculation value of the γ phase. In this specification, Rα on the (200) plane of the α phase is 9.9, Rα on the (211) plane of the α phase is 20.4, Rα on the (220) plane of the α phase is 9.3, Rγ on the (200) plane of the γ phase is 23.8, Rγ on the (220) plane of the γ phase is 12.5, and Rγ on the (311) plane of the γ phase is 17.2. The volume fraction of the retained austenite is rounded off to the first decimal place of the obtained value. In the measurement of the X-ray diffraction intensity, X-rays are irradiated to a position on the test piece corresponding to a depth position of 1 mm from the surface of the barrel of the forged steel roll.
[0073] The volume fraction (%) of the retained austenite obtained by the above-mentioned X-ray diffraction method is regarded as the area fraction (%) of the retained austenite. Then, the total area fraction of martensite and bainite in the surface layer of the forged steel roll is calculated by the following formula. Total area ratio of martensite and bainite in the surface layer of the forged steel roll = 100.0 - (area ratio of carbide + area ratio of retained austenite)
[0074] [Applications of the forged steel roll according to this embodiment] The forged steel roll of this embodiment is widely applicable as a roll for rolling. The forged steel roll of this embodiment is particularly suitable as a roll for cold rolling of thin steel sheets. The roll for cold rolling is, for example, a work roll for a cold tandem rolling mill or a cold reverse rolling mill, or a work roll for skin pass (temper rolling).
[0075] [Manufacturing method of forged steel rolls] An example of a method for manufacturing the forged steel roll of the present embodiment will be described. The forged steel roll of the present embodiment may be manufactured by a manufacturing method other than the manufacturing method described below. However, the manufacturing method described below is a preferred example of the method for manufacturing the forged steel roll of the present embodiment.
[0076] An example of a method for manufacturing a forged steel roll according to the present embodiment includes the following steps. (Process 1) Steelmaking process (Process 2) Hot forging process (Step 3) Annealing step (Process 4) Rough processing process (Step 5) Quenching process (Process 6) Tempering process (Step 7) Finishing process Each step will be described below.
[0077] [(Process 1) Steelmaking process] In the steelmaking process, molten steel satisfying Feature 1 or molten steel satisfying Feature 1, Requirement 1, and Requirement 2 is used to produce an ingot by a known casting method. An example of the known casting method is the bottom pouring ingot casting method. An electroslag remelting (ESR) method or the like may be carried out using the cast ingot as an electrode.
[0078] [(Process 2) Hot forging process] In the hot forging process, first, an ingot is heated in a heating furnace. Then, the heated ingot is subjected to hot forging to produce a roll blank having a rough shape (hereinafter, referred to as an intermediate blank). In the hot forging process, the following essential condition 1 and essential condition 2 are satisfied. (Requirement 1) Ingot temperature just before the start of hot forging T1: 1100-1200℃ (Requirement 2) Forging ratio S: 1.3~3.2 Each of the required conditions will be explained below.
[0079] [(Requirement 1) Regarding the ingot temperature T1 just before the start of hot forging] The temperature T1 of the ingot immediately before the start of hot forging is set to 1100 to 1200°C. If the temperature T1 is less than 1100°C, the temperature T1 is too low. In this case, cracks may occur in the ingot during hot forging. If the temperature T1 exceeds 1200°C, cracks may occur in the ingot during hot forging. Therefore, the temperature T1 is set to 1100 to 1200°C.
[0080] [(Requirement 2) Forging ratio S] In the hot forging process, the forging ratio S is set to 1.3 to 3.2. In this specification, the forging ratio S means the forging ratio in solid forging. The forging ratio S is defined by the following formula. Forging ratio S = Cross-sectional area of ingot before hot forging / Cross-sectional area of intermediate material body after hot forging Here, the cross-sectional area of the ingot before hot forging means the cross-sectional area of the ingot in a cross section perpendicular to the longitudinal direction, and the cross-sectional area of the trunk part of the intermediate preform after hot forging means the cross-sectional area of the trunk part of the intermediate preform in a cross section perpendicular to the longitudinal direction.
[0081] The forging ratio S is the thickness of the forged steel roll after manufacture. 2 If the forging ratio S is less than 1.3, the length of the large angle grain boundary per mm of the forged steel roll after manufacture 2 On the other hand, if the forging ratio S exceeds 3.2, the length of the high angle grain boundary per unit area of the forged steel roll after manufacture becomes too short. 2If the forging ratio S is set to 1.3 to 3.2, the length of the high angle grain boundary per unit area becomes too long. 2 The length of the high-angle grain boundary per unit area can be adjusted to an appropriate size.
[0082] [Preferable conditions for hot forging process (optional conditions)] Preferably, the hot forging step further satisfies the following conditions: These conditions are optional. (Optional condition 1) Heating temperature T0: 1200~1300℃ (Optional condition 2) Holding time at heating temperature T0: 10 hours or more (Optional condition 3) Temperature difference ΔT = heating temperature T0 - ingot temperature just before the start of hot forging T1: 50 to 150°C Optional Conditions 1 to 3 will now be described.
[0083] [(Optional Condition 1 and Optional Condition 2) Heating temperature T0 and holding time t0] If the heating temperature T0 is set to 1200 to 1300°C and the holding time t0 is set to 10 hours or more, the Si precipitates such as Si carbides in the intermediate preform are sufficiently dissolved in the subsequent annealing process. Therefore, a sufficient amount of dissolved Si can be secured in the manufactured forged steel roll. As a result, the Vickers hardness of the forged steel roll at 400°C is 400HV or more.
[0084] [(Optional condition 3) Temperature difference ΔT] Furthermore, if the temperature difference ΔT obtained by subtracting the temperature T1 of the ingot immediately before the start of hot forging from the heating temperature T0 is within a range of 50 to 150°C, Si precipitates such as Si carbides in the intermediate preform are sufficiently dissolved in the subsequent annealing process. Therefore, a sufficient amount of dissolved Si can be secured in the manufactured forged steel roll. As a result, the Vickers hardness of the forged steel roll at 400°C is 400HV or more. A more preferable temperature difference ΔT is 60 to 100°C.
[0085] When the temperature of the steel material during hot forging drops to 900°C, the steel material is heated again in a heating furnace. Then, hot forging is resumed for the reheated steel material. The heating temperatures T0 and T1 when reheating and resuming hot forging both satisfy essential condition 1. Furthermore, preferably, the holding time t0 satisfies 1 to 10 hours. When the steel material during hot forging is heated again in a heating furnace, the temperature difference ΔT means the temperature difference in the first heating, and the temperature difference ΔT from the second heating onwards does not have to satisfy optional condition 3.
[0086] [(Step 3) Annealing process] In the annealing process, the intermediate blank produced in the hot forging process is annealed. By carrying out the annealing process, the intermediate blank is easier to grind in the next rough processing process. The annealing may be carried out under well-known conditions using an electric furnace or a gas furnace. The annealing temperature is, for example, 500 to 1000°C. The holding time is, for example, 10 to 50 hours.
[0087] [(Process 4) Rough processing process] In the rough processing step, the intermediate blank after the annealing step is subjected to rough processing to further roughly process the intermediate blank into a shape close to the final roll shape. The rough processing is, for example, grinding. The rough processing may be performed under well-known conditions.
[0088] [(Step 5) Hardening process] In the quenching process, quenching is performed on the intermediate blank after the rough machining process. In the quenching process, the following essential conditions 3 to 5 are satisfied. (Requirement 3) Quenching temperature T2: 950~1100℃ (Requirement 4) Holding time at quenching temperature T2: 0.02 to 0.22 hours (Requirement 5) FA defined by the following formula: 5.00 to 12.00 FA = S / (T2 × (26 + log 10 (5×t2))×10 -5 ) Here, the forging ratio S is substituted for "S" in FA. The quenching temperature (℃) is substituted for "T2". The holding time (hours) is substituted for "t2". Essential conditions 3 to 5 will be explained below.
[0089] [(Requirements 3 and 4) Regarding quenching temperature T2 and holding time t2] The quenching temperature T2 and the holding time t2 affect the length of the large angle grain boundary of the manufactured forged steel roll. If the quenching temperature T2 is too low or the holding time t2 is too short, the length of the large angle grain boundary of the manufactured forged steel roll will be 2 On the other hand, if the quenching temperature T2 is too high or the holding time t2 is too long, the length of the high angle grain boundary per mm of the forged steel roll after manufacture becomes too long. 2 If the quenching temperature T2 is set to 950-1100°C and the holding time t2 is set to 0.02-0.22 hours, the length of the high angle grain boundary per mm of the manufactured forged steel roll will be too short. 2 The length of the high-angle grain boundary per unit area can be adjusted to an appropriate size.
[0090] [(Requirement 5) FA] The forging ratio S, the quenching temperature T2, and the holding time t2 are related to each other and are 2 When FA, which is the relation between the forging ratio S, the quenching temperature T2 and the holding time t2, is less than 5.00, the length of the large angle grain boundary per mm of the forged steel roll after manufacture is affected. 2 On the other hand, if FA exceeds 12.00, the length of the high angle grain boundary per mm of the manufactured forged steel roll becomes too short. 2 If FA is set to 5.00 to 12.00, the length of the high angle grain boundary per unit area becomes too long. 2 The length of the high-angle grain boundary per unit area can be adjusted to an appropriate size.
[0091] [Preferable conditions for the quenching process (optional conditions)] Preferably, the quenching step further satisfies the following conditions: (Optional condition 4) Cooling time CT from quenching temperature T2 to 800°C: 30 to 300 seconds If the cooling time CT from the quenching temperature T2 to 800°C is 30 to 300 seconds, the formation of solid-solubilized Si as Si precipitates can be sufficiently suppressed, and carbides made of alloys other than Si can be sufficiently formed, thereby increasing the high-temperature hardness of the forged steel roll.
[0092] After the quenching step and before the tempering step, the intermediate preform may be subjected to a sub-zero treatment. The cooling temperature in the sub-zero treatment may be in a known range, for example, -30 to -196°C.
[0093] [(Step 6) Tempering process] In the tempering process, the intermediate blank after the quenching process is tempered. The hardness of the surface layer of the forged steel roll is adjusted by tempering. The tempering temperature is, for example, 100 to 600°C.
[0094] [(Step 7) Finishing process] In the finish processing step, the intermediate preform after the tempering step is subjected to a finish processing. The finish processing is, for example, a grinding process using a grinding machine. The intermediate preform is processed into a final product shape by the finish processing. By the above steps, the forged steel roll of this embodiment can be manufactured.
[0095] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way. EXAMPLES
[0096] [Manufacturing of forged steel rolls] A forged steel roll having the chemical composition shown in Table 1 was manufactured by the following manufacturing method.
[0097] [Table 1]
[0098] Specifically, ingots were cast from molten steel by bottom pouring. The produced ingots were remelted by electroslag remelting (ESR) to produce ingots as materials. The produced ingots were subjected to a hot forging process. Table 2 shows essential condition 1 (forging temperature T1 (℃)), essential condition 2 (forging ratio S), optional condition 1 (heating temperature T0 (℃)), optional condition 2 (holding time t0 (hours)), and optional condition 3 (temperature difference ΔT (℃)). The hot forging process produced intermediate blanks in the shape of rolls with a roll barrel diameter of φ700 mm, barrel length of 2100 mm, and total length of 4100 mm for each test number.
[0099] [Table 2]
[0100] In the forging process, the ingot was heated and held at a heating temperature T0 and a holding time t0. Then, the ingot temperature was lowered to a forging temperature T1, and hot forging was performed. In all test numbers, the ingot temperature dropped to 900°C during hot forging. Therefore, hot forging was temporarily interrupted, and the ingot was heated again in a heating furnace (second heating). Hot forging was resumed for the ingot after reheating. Table 2 shows the first and second heating temperatures T0, holding time t0, temperature T1, and the first temperature difference ΔT.
[0101] The intermediate blanks after the hot forging process were subjected to an annealing process. In the annealing process, they were held at 900°C for 10 hours. After that, they were further held at 600°C for 15 hours. The intermediate blanks after the annealing process were subjected to a rough machining process. Specifically, for each test number, grinding was performed on the intermediate blanks to produce intermediate blanks in the shape of rolls with a roll barrel diameter of φ650 mm, barrel length of 2000 mm, and total length of 4000 mm.
[0102] The intermediate blank after the rough machining process was subjected to a quenching process. Essential condition 3 (quenching temperature T2 (℃)), essential condition 4 (holding time t2 (hours)), essential condition 5 (FA), and optional condition 4 (cooling time CT (seconds)) for the quenching process are shown in Table 2. In the quenching process, the intermediate blank was heated by induction heating and then water-cooled.
[0103] Sub-zero treatment was carried out on the intermediate preform after the quenching process. In the sub-zero treatment, the intermediate preform was cooled to -60 to -140°C. The intermediate preform after the sub-zero treatment was tempered at 100 to 600°C, and then a finishing process was carried out. In the finishing process, the intermediate preform was ground to finish the final roll shape with a roll barrel diameter of φ645 mm, a barrel length of 1950 mm, and a total length of 3950 mm. The forged steel rolls of each test number were manufactured by the above manufacturing process. The total area ratio of martensite and bainite in the surface layer of the forged steel roll of each test number was determined based on the method described in the above-mentioned [Method for measuring the total area ratio of martensite and bainite in the surface layer of a forged steel roll]. As a result, the total area ratio of martensite and bainite in the surface layer was 85% or more in the forged steel rolls of all test numbers.
[0104] [Evaluation test] The following evaluation tests were carried out using the forged steel rolls with each test number. (Test 1) 1mm 2 Measurement test of high angle grain boundary length (Test 2) Vickers hardness test at 400℃ (Test 3) Crack resistance evaluation test Tests 1 to 3 will be described below.
[0105] [(Test 1) 1mm 2 [Measurement test of high angle grain boundary length per unit area] The above-mentioned [surface 1 mm 2 In accordance with the method described in "Method of measuring the length of high angle grain boundaries per unit area," the surface of the forged steel roll with each test number was measured for 1 mm 2 Length of high angle grain boundary per unit (mm / mm 2 ) was obtained. 2The high angle grain boundary length per unit area is shown in Table 3 as "Length of high angle grain boundary (mm / mm 2 ) column.
[0106] [Table 3]
[0107] [(Test 2) Vickers hardness test at 400℃] The Vickers hardness (HV) of the forged steel roll of each test number at 400°C was determined according to the method described above in [Method of measuring Vickers hardness at 400°C]. The measurement was performed using a Nikon Corporation QM2 high temperature microscope hardness tester. The obtained Vickers hardness is shown in the "Vickers hardness (HV) at 400°C" column in Table 3.
[0108] [(Test 3) Crack resistance evaluation test] To evaluate the crack resistance, a thermal shock test was carried out using a drop-weight friction thermal shock tester 10 shown in Fig. 1. Specifically, a test piece 13 measuring 20 mm in the depth direction, 20 mm in the circumferential direction, and 30 mm in the longitudinal direction was taken from the surface at the longitudinal center position of the barrel of the forged steel roll of each test number.
[0109] A rod-shaped biting material 12 having a diameter of 5 mm and a length of 10 mm was attached to the outer periphery of the pinion 11 of the drop weight type frictional thermal shock tester 10. The biting material 12 was a soft steel wire SWRM6 standardized in JIS G 3505:2017. The tip of the biting material 12 was bent and the tip was embedded in the radial direction of the pinion 11 from the outer periphery of the pinion 11. As shown in FIG. 1, the surface 13A of the test piece 13 was brought into contact with the biting material 12. At this time, the biting material was arranged so that the part of the biting material 12 other than the tip part extended upward. The test piece 13 and the biting material were arranged so that the bent part of the biting material 12 contacted the upper part of the surface 13A. The surface 13A was 20 mm x 30 mm and was arranged so that the 30 mm side was vertical. The surface 13A was a surface corresponding to the surface of the forged steel roll. After the test piece 13 and the biting member 12 were arranged as described above, the pinion 11 was rotated using a weight to cause the biting member 12 to slide strongly on the surface 13A, thereby applying a thermal shock to the surface 13A.
[0110] Fig. 2 is a schematic diagram of the surface 13A after the biting material 12 has passed over the surface 13A. As shown in Fig. 2, a contact area 100, which is a portion where the biting material 12 has slid, was formed in the longitudinal direction on the surface 13A. Therefore, as shown in Fig. 2, the contact area 100 was cut at a plane CS including the longitudinal direction and normal direction of the surface 13A at approximately the center of the width.
[0111] The entire contact area 100 of the cut surface was observed with a 100x optical microscope, and the surface vicinity of the entire contact area 100 was continuously photographed to generate a plurality of continuous photographic images. FIG. 3 is a cross-sectional view showing a portion of the continuous photographic images. Using the continuous photographic images, the number of cracks 50 occurring in the entire contact area 100 and the maximum depth of the cracks 50 were confirmed. In each photographic image, the length NL of the crack 50 in the normal direction N of the surface 13A was recognized as the crack depth. If the crack depth was 10 μm or more, it was recognized as a crack. The number of recognized cracks was calculated. Furthermore, the maximum crack depth of the recognized cracks was calculated. The obtained maximum crack depth (μm) and number of cracks are shown in the "Maximum crack depth (μm)" and "Number of cracks (pieces)" columns in Table 3.
[0112] [Evaluation Results] With reference to Tables 1, 2 and 3, in test numbers 1 to 37, the chemical composition was appropriate and the essential conditions 1 to 5 in the manufacturing process were met. 2 The length of the high angle grain boundary per unit area was 2500 to 9000 mm. Therefore, these test numbers had excellent crack resistance. Specifically, in the crack resistance evaluation test, the maximum crack depth was suppressed to 400 μm or less, and the number of cracks was 30 or less.
[0113] Among test numbers 1 to 37, test numbers 6 to 10, 12, 14, 16, 18, and 19 further had a Si content of 0.40 to 1.50%, satisfying formula (1). Furthermore, the Vickers hardness at 400°C was 400HV or more. As a result, in the crack resistance evaluation test, the number of cracks was 20 or less, the frequency of crack occurrence was further suppressed, and further excellent crack resistance was obtained.
[0114] On the other hand, in test numbers 38 and 39, the forging ratio S was too low. 2 The length of the high angle grain boundary per unit area was too short. As a result, the number of cracks exceeded 30, and sufficient crack resistance was not obtained.
[0115] In test numbers 40 and 41, the forging ratio S was too high. 2 The length of the high angle grain boundary at the interface was too long. As a result, the maximum crack depth exceeded 400 μm, and sufficient crack resistance was not obtained.
[0116] In test numbers 42 and 43, the quenching temperature T2 was too low. 2 The length of the high angle grain boundary at the interface was too long. As a result, the maximum crack depth exceeded 400 μm, and sufficient crack resistance was not obtained.
[0117] In test numbers 44 and 45, the quenching temperature T2 was too high. 2 The length of the high angle grain boundary per unit area was too short. As a result, the number of cracks exceeded 30, and sufficient crack resistance was not obtained.
[0118] In test numbers 46 and 47, the holding time t2 at the quenching temperature was too short. 2 The length of the high angle grain boundary at the interface was too long. As a result, the maximum crack depth exceeded 400 μm, and sufficient crack resistance was not obtained.
[0119] In test numbers 48 and 49, the holding time t2 was too long. 2 The length of the high angle grain boundary per unit area was too short. As a result, the number of cracks exceeded 30, and sufficient crack resistance was not obtained.
[0120] In test numbers 50 and 51, the FA values were too low. 2 The length of the high angle grain boundary per unit area was too short. As a result, the number of cracks exceeded 30, and sufficient crack resistance was not obtained.
[0121] In test numbers 52 and 53, the FA value was too high. 2 The length of the high angle grain boundary at the interface was too long. As a result, the maximum crack depth exceeded 400 μm, and sufficient crack resistance was not obtained.
[0122] The embodiments of the present disclosure have been described above. However, the above-described embodiments are merely examples for implementing the present disclosure. Therefore, the present disclosure is not limited to the above-described embodiments, and can be implemented by appropriately modifying the above-described embodiments without departing from the spirit of the present disclosure.
Claims
1. A forged steel roll, The chemical composition, in mass%, is C: 0.70-1.50%, Si: 0.20-1.50%, Mn: 0.20-1.50%, P: 0.030% or less, S: 0.0200% or less, Al: 0.050% or less, N: 0.2000% or less, O: 0.0050% or less, Cr: 2.80-8.00%, Mo: 0.40-3.00%, Cu: 0.100% or less, B: 0.0100% or less, Ni: 0 to 1.20%, V: 0-2.00%, Nb: 0 to 0.50%, and The balance is composed of Fe and impurities. The surface layer of the forged steel roll is 1 mm 2 The length of the high angle grain boundary per unit area is 2500 to 9000 mm. Forged steel roll.
2. 2. The forged steel roll according to claim 1, The chemical composition is Ni: 0.01 to 1.20%, V: 0.01 to 2.00%, and Nb: 0.01 to 0.50%; Forged steel roll.
3. 2. The forged steel roll according to claim 1, The N content is 0.0200% or less by mass%, Forged steel roll.
4. 3. The forged steel roll according to claim 2, The N content is 0.0200% or less by mass%, Forged steel roll.
5. The forged steel roll according to any one of claims 1 to 4, further comprising: The Si content is 0.40 to 1.50% by mass, The chemical composition satisfies formula (1), The Vickers hardness at 400°C is 400HV or more. Forged steel roll. 4.50≦Cr+Mo+V+Nb≦13.50 (1) Here, each element symbol in the formula is substituted with the content of the corresponding element in mass %. When an element is not contained, the corresponding element symbol is substituted with "0."
Citation Information
Patent Citations
Forged steel roll for cold rolling and its manufacture
JP1987040346A
Production of operating roll for high-load cold rolling mill having great case depth
JP1989056826A
Highly wear resistant type roll for cold rolling
JP1997003603A
Steel material superior in spalling resistance for rolling roll for galvanized steel sheet, and rolling roll for galvanized steel sheet
JP2013127104A
Cold rolling roll
JP2019055419A