Resist underlayer film forming composition

The resist underlayer film forming composition with a specific copolymer and optional additives addresses filling and thermal issues, providing a flat, antireflective film for semiconductor manufacturing.

JP7590696B2Active Publication Date: 2024-11-27NISSAN CHEM CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2021504993
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-12
Filing Date
2020-03-05
Publication Date
2024-11-27
Estimated Expiration
2040-03-05

AI Technical Summary

Technical Problem

Conventional resist underlayer film forming compositions face issues with poor pattern filling due to increased viscosity during heating, thermal shrinkage, and reflection from the substrate, leading to distorted patterns and image defects in semiconductor manufacturing.

Method used

A resist underlayer film forming composition containing a copolymer with specific repeating structural units and an organic solvent, optionally with a photocrosslinking agent and surfactant, is applied and cured through heating or a combination of heating and exposure, allowing for high reflow properties and antireflection effects.

Benefits of technology

The composition achieves improved pattern filling, thermal stability, and antireflection, resulting in a flat film formation with enhanced manufacturing efficiency and reduced defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590696000001
    Figure 0007590696000001
  • Figure 0007590696000002
    Figure 0007590696000002
  • Figure 0007590696000003
    Figure 0007590696000003
Patent Text Reader

Abstract

[Problem] The present invention addresses the problem of providing a resist underlayer film formation composition that is capable of exhibiting high reflow properties through a step for applying the composition on a substrate and heating the composition, and that can be flatly applied even on a multilevel substrate so as to enable formation of a planarized film. [Solution] The resist underlayer film formation composition according to the present invention contains an organic solvent and a copolymer having a repeating structural unit represented by formula (1) and / or a repeating unit represented by formula (2). (In formula (1) and formula (2), R1 represents a functional group represented by formula (3), in formula (3), Q1 and Q2 each independently represent a hydrogen atom or an alkyl group having 1-5 carbon atoms, * represents an end of a bond with an oxygen atom, and in formula (2), X1 represents an organic group having 1-50 carbon atoms, and i and j each independently represent 0 or 1.)
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resist underlayer film-forming composition for forming a planarizing film for filling in steps on a substrate having steps and flattening the substrate, and a method for producing a planarized resist underlayer film using the resist underlayer film-forming composition. [Background technology]

[0002] In recent years, there has been a demand for semiconductor integrated circuit devices to be able to be processed according to finer design. In order to form finer resist patterns using photolithography technology, it is necessary to shorten the exposure wavelength. However, since the depth of focus decreases as the exposure wavelength becomes shorter, it is necessary to further improve the planarization of the coating film formed on the substrate. In other words, in order to manufacture semiconductor devices with fine design, it is becoming important to establish a planarization technology that can form a high-level planarization film, especially on a stepped substrate.

[0003] As a method for forming a planarizing film, for example, a method for forming a resist underlayer film by photocuring the resist underlayer film has been disclosed. A resist underlayer film-forming composition containing a polymer having an epoxy group or an oxetane group in a side chain and a photocationic polymerization initiator, or a resist underlayer film-forming composition containing a polymer having a radically polymerizable ethylenically unsaturated bond and a photoradical polymerization initiator has been disclosed (see Patent Document 1).

[0004] In addition, a resist underlayer film-forming composition has been disclosed that contains a silicon-based compound having a cationic polymerizable reactive group such as an epoxy group or a vinyl group, a photocationic polymerization initiator, and a photoradical polymerization initiator (see Patent Document 2). Also disclosed is a method for manufacturing a semiconductor device using a resist underlayer film containing a polymer having a crosslinkable functional group (such as a hydroxyl group) in the side chain, a crosslinking agent, and a photoacid generator (see Patent Document 3).

[0005] Further, although they are not photocrosslinkable resist underlayer films, resist underlayer films having unsaturated bonds in the main chain or side chain have been disclosed (see Patent Documents 4 and 5). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] International Publication No. 2006 / 115044 Brochure [Patent Document 2] International Publication No. 2007 / 066597 Brochure [Patent Document 3] International Publication No. 2008 / 047638 Brochure [Patent Document 4] International Publication No. 2009 / 008446 Brochure [Patent Document 5] Special table 2004-533637 Summary of the Invention [Problem to be solved by the invention]

[0007] Conventionally, when a resist underlayer film-forming composition containing, for example, a polymer having a thermally crosslinkable functional group such as a hydroxyl group, a crosslinking agent, and an acid catalyst (acid generator) is used as a photocrosslinkable material, when the composition is heated to fill an uneven pattern (e.g., a hole or trench structure) formed on a substrate, a crosslinking reaction progresses, causing an increase in viscosity, resulting in insufficient filling of the inside of the pattern. Furthermore, when the heating temperature for forming a conventional resist underlayer film is 180° C. or higher, the resist underlayer film-forming composition gradually hardens due to heat, resulting in poor reflow properties.

[0008] Furthermore, in general, a resist underlayer film-forming composition containing a polymer having a cationic polymerizable reactive group such as an epoxy group or a vinyl group and an acid generator is cured by a combination of light irradiation and heating, which is troublesome.

[0009] Furthermore, in the lithography process for manufacturing semiconductor devices, the shape of the pattern edge is distorted due to reflection of the exposure light onto the resist layer from the substrate, making it impossible to form a resist pattern of the desired shape, which causes fluctuations in the dimensions of the resist pattern and even poor resolution.

[0010] Therefore, an object of the present invention is to provide a resist underlayer film-forming composition for forming a planarizing film on a substrate, which has high pattern filling properties, does not cause thermal shrinkage, has good reflow properties, and is capable of forming a cured film having a reflective effect. [Means for solving the problem]

[0011] A first aspect of the present invention relates to a resist underlayer film-forming composition containing a copolymer having a repeating structural unit represented by formula (1) and / or a repeating unit represented by formula (2) and an organic solvent. [ka] (In formula (1) and formula (2), R 1 represents a functional group represented by formula (3), in which Q 1 and Q 2 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, * represents a bond end to an oxygen atom, and in formula (2), X 1 represents an organic group having 1 to 50 carbon atoms, and i and j each independently represent 0 or 1. As a second aspect, the present invention relates to the resist underlayer film forming composition according to aspect 1, wherein the functional group represented by formula (3) is a group represented by formula (4): [ka] (In formula (4), * represents the bond end with the oxygen atom.) In a third aspect, the present invention provides a repeating structural unit represented by the formula (2), 1represents a linear, branched or cyclic divalent hydrocarbon group having from 2 to 20 carbon atoms, represents a linear, branched or cyclic divalent organic group having from 2 to 20 carbon atoms having at least one sulfur atom or oxygen atom, or represents a divalent organic group containing at least one aromatic ring having from 6 to 20 carbon atoms or a heterocycle having from 3 to 12 carbon atoms, wherein the heterocycle has at least one sulfur atom or oxygen atom. In a fourth aspect, the present invention relates to the copolymer, 1 The resist underlayer film-forming composition according to any one of Aspects 1 to 3, wherein the composition contains 25% or more of a repeating structural unit formed from a monomer comprising the following: A fifth aspect of the present invention relates to the resist underlayer film-forming composition according to any one of Aspects 1 to 4, further comprising a photocrosslinking agent. As a sixth aspect, the present invention relates to the resist underlayer film-forming composition according to any one of Aspects 1 to 5, further comprising a compound represented by the following formula (5) and / or a compound represented by the following formula (6): [ka] (In the formula, X 2 represents a carbonyl group or a methylene group, l and m each independently represent an integer of 0 to 5 and satisfy the relational formula 3≦l+m≦10; R 3 represents an alkylene or alkenylene group having 1 to 4 carbon atoms or a single bond, k represents 0 or 1, and n represents an integer of 2 to 4. A seventh aspect of the present invention relates to the resist underlayer film forming composition according to any one of Aspects 1 to 6, further comprising a surfactant. In an eighth aspect, the present invention relates to a method for producing a resist underlayer film, comprising applying the resist underlayer film-forming composition according to any one of the first to seventh aspects to a substrate having a step, and then heating the composition to thermally cure it. The present invention relates, as a ninth aspect, to the method for producing a resist underlayer film according to the eighth aspect, wherein the heating temperature in the heating step is 200° C. to 300° C. The present invention relates to, as a tenth aspect, a method for producing a resist underlayer film according to the ninth aspect, further comprising an exposure step of exposing the resist to light. In an eleventh aspect, the present invention relates to a method for producing a resist underlayer film, comprising a heating step of applying the resist underlayer film-forming composition according to any one of Aspects 1 to 7 to a substrate having a step and thermally curing the composition at 250° C. or higher, without passing through an exposure step. Effect of the Invention

[0012] According to the resist underlayer film forming composition of the present invention, by applying the resist underlayer film forming composition to a substrate and heating it, high reflowability is exhibited, and a flat film can be formed even on a substrate having steps. In addition, the formed cured film has an appropriate antireflection effect. The resist underlayer film forming composition of the present invention contains a surfactant, which has the effect of improving the coatability onto a substrate. According to the method for producing a resist underlayer film of the present invention, the resist underlayer film forming composition of the present invention is applied to a substrate and then heated, whereby high reflowability is exhibited, and a flat film can be formed even on a substrate having a step. Furthermore, the formed cured film has an appropriate antireflection effect. Furthermore, according to the method for producing a resist underlayer film of the present invention, the resist underlayer film-forming composition of the present invention can be cured by combining two steps of heating and exposure. On the other hand, a planarized film having flatness can also be formed by curing the resist underlayer film-forming composition of the present invention only by heating at a high temperature without going through an exposure step, which has the effect of simplifying the production process and improving work efficiency. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] <Copolymer> The copolymer, which is an essential component of the resist underlayer film forming composition of the present invention, is preferably a copolymer having a repeating structural unit represented by the following formula (1) and / or a repeating structural unit represented by the following formula (2). [ka] (In formula (1) and formula (2), R 1 represents a functional group represented by formula (3), in which Q 1 and Q 2 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, * represents a bond end to an oxygen atom, and in formula (2), X 1 represents an organic group having 1 to 50 carbon atoms, and i and j each independently represent 0 or 1.

[0014] Preferably, Q in formula (3) 1 and Q 2 each independently represents a hydrogen atom. That is, the functional group represented by formula (3) becomes a group represented by formula (4) below. [ka] (In formula (4), * represents the bond end with the oxygen atom.)

[0015] Preferably, in the copolymer, R 1 The content of repeating structural units formed from a monomer containing the formula (I) is 25% or more, and more preferably 50% or more.

[0016] Preferably, the group X in formula (2) 1 represents a linear, branched or cyclic divalent hydrocarbon group having 2 to 20 carbon atoms, represents a linear, branched or cyclic divalent organic group having 2 to 20 carbon atoms having at least one sulfur atom or oxygen atom, or represents a divalent organic group containing at least one aromatic ring having 6 to 20 carbon atoms or a heterocycle having 3 to 12 carbon atoms, and the heterocycle has at least one sulfur atom or oxygen atom. Examples of the aromatic ring include a benzene ring, a naphthalene ring, an anthracene ring, a phenanthrene ring, a naphthacene ring, a triphenylene ring, a pyrene ring, and a chrysene ring, and preferably a benzene ring or a naphthalene ring. Examples of the heterocyclic ring include a triazine ring, a cyanuric ring, a pyrimidine ring, an imidazole ring, and a carbazole ring.

[0017] The compound represented by the formula below is an example of a monomer that corresponds to the repeating unit represented by formula (1) in the copolymer. [ka]

[0018] The compound represented by the following formula is an example of a monomer that corresponds to the repeating unit represented by formula (2) in the copolymer. [ka]

[0019] [ka]

[0020] Examples of the copolymer having the repeating structural unit represented by the above formula (1) and the repeating structural unit represented by the above formula (2) include copolymers having repeating structural units represented by the following formulas (1a) to (1k). [ka]

[0021] [ka]

[0022] The resist underlayer film forming composition of the present invention may contain, as an optional component, a compound represented by formula (5) and / or a compound represented by formula (6). [ka] In the formula, X 2 represents a carbonyl group or a methylene group, l and m each independently represent an integer of 0 to 5 and satisfy the relational formula 3≦l+m≦10; R 3represents an alkylene or alkenylene group having 1 to 4 carbon atoms or a single bond, k represents 0 or 1, and n represents an integer of 2 to 4.

[0023] Examples of the compound represented by formula (5) include compounds represented by the following formulas (5-1) to (5-20). [ka]

[0024] Examples of the compound represented by formula (6) include compounds represented by the following formulas (6-1) to (6-31). [ka]

[0025] The resist underlayer film forming composition of the present invention can contain the compound represented by formula (5) and / or the compound represented by formula (6) in an amount of, for example, 0.01 to 60 parts by mass, preferably 0.1 to 20 parts by mass, relative to 100 parts by mass of the copolymer.

[0026] <Photocrosslinking agent> The resist underlayer film forming composition of the present invention does not require a thermal crosslinking agent, and a photocrosslinking agent can be added as necessary.

[0027] Examples of the photocrosslinking agent include glycidyl ether compounds, glycidyl ester compounds, glycidyl group-containing isocyanurates, epoxycyclohexyl compounds, epoxy group-substituted cyclohexyl compounds, and resins thereof. Examples of the photocrosslinking agent used in the present invention include the following. [ka] The compound represented by formula (C-1) is available from Nissan Chemical Industries, Ltd. under the trade name TEPIC-SS. Formula (C-2) is available from Shikoku Chemical Industries Co., Ltd. under the trade name MA-DGIC. The compound represented by formula (C-3) is available from Nagase Chemtec Corporation under the trade name EX-411. The compound represented by formula (C-4) is available from Nagase Chemtec Corporation under the trade name EX-521. The compound represented by formula (C-7) is available from Nippon Kayaku Co., Ltd. under the trade name RE810-NM. The compound represented by formula (C-8) is available from Showa Denko KK under the trade name BATG. Compound (C-9) is available from Nagase Chemtec Corporation under the trade name EX-711. Formula (C-10) is available from DIC Corporation under the trade name YD-4032D. Compound (C-11) is available from DIC Corporation under the trade name HP-4770. The compound represented by formula (C-12) is available from Nippon Steel & Sumikin Chemical Co., Ltd. under the trade name YH-434L. Formula (C-13) is available from DIC Corporation under the trade name EPICLON HP-4700. The compound represented by formula (C-14) is available from Asahi Yukizai Kogyo Co., Ltd. under the trade name TEP-G. The formula (C-15) is Epolead GT401 (trade name) manufactured by Daicel Corporation, and a, b, c, and d are each 0 or 1, and a+b+c+d=1. The compound represented by formula (C-16) is available from Daicel Corporation under the trade name EHPE-3150. Compound (C-17) is available from DIC Corporation under the trade name HP-7200L. Compound (C-18) is available from Nippon Kayaku Co., Ltd. under the trade name EPPN-201. Formula (C-19) is available from Asahi Kasei Epoxy Corporation under the trade name ECN-1229. Compound (C-20) is available from Nippon Kayaku Co., Ltd. under the trade name EPPN-501H. The compound represented by formula (C-21) is available from Nippon Kayaku Co., Ltd. under the trade name NC-2000L. Compound (C-22) is available from Nippon Kayaku Co., Ltd. under the trade name NC-3000L. Compound (C-23) is available from Nippon Kayaku Co., Ltd. under the trade name NC-7000L. Compound (C-24) is available from Nippon Kayaku Co., Ltd. under the trade name NC-7300L. Compound (C-25) is available from Nippon Kayaku Co., Ltd. under the trade name NC-3500. Compound (C-26) is available from DIC Corporation under the trade name EPICLON HP-5000. Compound (C-27) is available from Nippon Kayaku Co., Ltd. under the trade name FAE-2500. Compound (C-28) is available from Nippon Kayaku Co., Ltd. under the trade name NC-6000.

[0028] <Surfactant> The resist underlayer film forming composition of the present invention may contain a surfactant as an optional component to improve the coating property on the substrate. Examples of the surfactant include polyoxyethylene alkyl ethers such as polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene cetyl ether, and polyoxyethylene oleyl ether, polyoxyethylene alkyl allyl ethers such as polyoxyethylene octylphenol ether and polyoxyethylene nonylphenol ether, polyoxyethylene-polyoxypropylene block copolymers, sorbitan fatty acid esters such as sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan monooleate, sorbitan trioleate, and sorbitan tristearate, polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate ... nonionic surfactants such as polyoxyethylene sorbitan fatty acid esters, such as polyoxyethylene sorbitan nostearate, polyoxyethylene sorbitan trioleate, and polyoxyethylene sorbitan tristearate; fluorosurfactants such as F-TOP (registered trademark) EF301, EF303, and EF352 (manufactured by Mitsubishi Materials Electronic Chemicals Co., Ltd.), Megafac (registered trademark) F171, F173, R-30, R-30N, and R-40-LM (manufactured by DIC Corporation), Fluorad FC430 and FC431 (manufactured by 3M Japan Ltd.), Asahiguard (registered trademark) AG710, Surflon (registered trademark) S-382, SC101, SC102, SC103, SC104, SC105, and SC106 (manufactured by AGC Corporation); and organosiloxane polymer KP341 (manufactured by Shin-Etsu Chemical Co., Ltd.). These surfactants may be added alone or in combination of two or more kinds.

[0029] When the above surfactant is used, the content of the surfactant is, for example, 0.01 to 5 parts by mass, and preferably 0.1 to 3 parts by mass, per 100 parts by mass of the copolymer.

[0030] <Organic solvent> The resist underlayer film forming composition of the present invention can be prepared by dissolving the above-mentioned components in a suitable organic solvent, and is used in the form of a homogeneous solution. Examples of such organic solvents include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monomethyl ether acetate, propylene glycol propyl ether acetate, toluene, xylene, methyl ethyl ketone, cyclopentane, etc. Examples of the organic solvent that can be used include cyclohexanone, ethyl 2-hydroxypropionate, ethyl 2-hydroxy-2-methylpropionate, ethyl ethoxyacetate, ethyl hydroxyacetate, methyl 2-hydroxy-3-methylbutanoate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, ethyl 3-ethoxypropionate, methyl 3-ethoxypropionate, methyl pyruvate, ethyl pyruvate, ethyl acetate, butyl acetate, ethyl lactate, butyl lactate, N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone. These organic solvents can be used alone or in combination of two or more. Furthermore, these organic solvents can be used by mixing them with high-boiling organic solvents such as propylene glycol monobutyl ether and propylene glycol monobutyl ether acetate.

[0031] <Method for Producing a Resist Underlayer Film> Next, a method for producing a resist underlayer film using the resist underlayer film forming composition of the present invention will be described. The resist underlayer film forming composition is applied onto a substrate (e.g., a transparent substrate such as a silicon / silicon dioxide-coated substrate, a glass substrate, or an ITO substrate) used in the production of precision integrated circuit elements by a suitable application method such as a spinner or coater, and then baked (heated) on a hot plate to form a resist underlayer film. That is, the method for producing a resist underlayer film includes a heating step in which the resist underlayer film forming composition is applied onto a substrate and then heated at a high temperature. The resist underlayer film forming composition of the present invention does not thermally cure even at high temperatures up to 250° C., but is thermally cured by heating at high temperatures of 250° C. or higher to form a flat resist underlayer film.

[0032] In the present invention, the heating temperature in the heating step is preferably 200°C to 300°C.

[0033] When heated at a high temperature of 250° C. or higher, the resist underlayer film forming composition is thermally cured, and a resist underlayer film can be formed without going through an exposure step.

[0034] In the present invention, there is also a method in which, for an underlayer film-forming composition that is not thermally cured in a heating step, an exposure step of irradiating the composition with ultraviolet light using an ultraviolet irradiation device is added after the composition is heated, thereby photocuring the resist underlayer film-forming composition. The light for exposure is actinic radiation such as near ultraviolet, far ultraviolet, or extreme ultraviolet (e.g., EUV, wavelength 13.5 nm), and light with wavelengths of, for example, 248 nm (KrF laser light), 193 nm (ArF laser light), 172 nm (xenon excimer light), 157 nm (F2 laser light), etc. The exposure wavelength may be ultraviolet light of 150 nm to 248 nm, with the wavelength of 172 nm being preferred. This exposure causes crosslinking of the resist underlayer film. The exposure dose in the exposure step is 10 mJ / cm 2 ~3000mJ / cm 2 Within this range of exposure dose, a photoreaction occurs, crosslinking is formed, and solvent resistance is achieved. EXAMPLES

[0035] Specific examples of the resist underlayer film forming composition of the present invention will be described below using the following examples, but the present invention is not limited thereto.

[0036] The apparatus used to measure the weight average molecular weight of the reaction products obtained in the following synthesis examples is shown below. Equipment: Tosoh Corporation HLC-8320GPC GPC column: TSKgel Super-MultiporeHZ-N (2 columns) Column temperature: 40℃ Flow rate: 0.35ml / min Eluent:THF Standard sample: polystyrene

[0037] The abbreviations used in the following examples have the following meanings. PGME: Propylene glycol monomethyl ether RE810-NM: Diallyl bisphenol A type epoxy resin (formula (A) below) BPA-CA: 2,2-bis(3-allyl-4-hydroxyphenyl)propane (formula (B) below) Ex-216L: Cyclohexanedimethanol diglycidyl ether (formula (C) below) Ex-252: Hydrogenated bisphenol A diglycidyl ether (formula (D) below) Cis-1,2-Cyclohexanedicarboxylic Acid PGMEA: Propylene glycol monomethyl ether acetate EHPE-3150: 1,2-epoxy-4-(2-oxiranyl)cyclohexane adduct of 2,2-bis(hydroxymethyl)-1-butanol [ka]

[0038] <Synthesis Example 1> 26.00 g of RE810-NM (manufactured by Nippon Kayaku Co., Ltd.), 20.81 g of BPA-CA (manufactured by Konishi Chemical Co., Ltd.), 2.18 g of ethyltriphenylphosphonium bromide as a catalyst, and 0.32 g of hydroquinone as a radical trapping agent were added to 72.46 g of PGME, and the mixture was reacted at 140 ° C. for 24 hours to obtain a solution containing a reaction product. After diluting to a 20 wt% solution with PGME, 147.90 g of anion exchange resin (product name: Dowex [registered trademark] MONOSPHERE [registered trademark] 550A, Muromachi Technos Co., Ltd.) and 147.90 g of cation exchange resin (product name: Amberlyst [registered trademark] 15JWET, Organo Co., Ltd.) were added, stirred at 60 ° C. for 4 hours, and then filtered. The reaction product obtained was analyzed by GPC and found to have a weight average molecular weight of 18,000 in terms of standard polystyrene. The reaction product obtained is presumed to be a copolymer having a structural unit represented by the following formula (7). [ka]

[0039] <Synthesis Example 2> 48.10 g of PGME was added with 9.00 g of RE810-NM (manufactured by Nippon Kayaku Co., Ltd.), 14.98 g of BPA-CA (manufactured by Konishi Chemical Co., Ltd.), 6.28 g of Ex-216L (manufactured by Nagase ChemteX Co., Ltd.), 1.57 g of ethyltriphenylphosphonium bromide as a catalyst, and 0.23 g of hydroquinone as a radical trapping agent, and the mixture was reacted at 140°C for 24 hours to obtain a solution containing the reaction product. The mixture was reprecipitated using methanol (320 g, manufactured by Kanto Chemical Co., Ltd.). The obtained precipitate was filtered and dried in a vacuum dryer at 60°C for 24 hours to obtain the target polymer. After adjusting the solution to a 20 wt% solution with PGME, 11.83 g of anion exchange resin (product name: Dowex [registered trademark] MONOSPHERE [registered trademark] 550A, Muromachi Technos Co., Ltd.) and 11.81 g of cation exchange resin (product name: Amberlyst [registered trademark] 15JWET, Organo Corporation) were added, stirred at 25 to 30°C for 4 hours, and then filtered. The reaction product was analyzed by GPC and found to have a weight average molecular weight of 13,700 in terms of standard polystyrene. The reaction product was presumed to be a copolymer having a structural unit represented by the following formula (8). [ka]

[0040] <Synthesis Example 3> 48.10 g of PGME was added with 9.00 g of RE810-NM (manufactured by Nippon Kayaku Co., Ltd.), 14.98 g of BPA-CA (manufactured by Konishi Chemical Co., Ltd.), 8.76 g of Ex-252 (manufactured by Nagase ChemteX Co., Ltd.), 1.57 g of ethyltriphenylphosphonium bromide as a catalyst, and 0.23 g of hydroquinone as a radical trapping agent, and the mixture was reacted at 140°C for 24 hours to obtain a solution containing the reaction product. The mixture was reprecipitated using methanol (320 g, manufactured by Kanto Chemical Co., Ltd.). The obtained precipitate was filtered and dried in a vacuum dryer at 60°C for 24 hours to obtain the target polymer. After adjusting the solution to a 20 wt% solution with PGME, 15.03 g of anion exchange resin (product name: Dowex [registered trademark] MONOSPHERE [registered trademark] 550A, Muromachi Technos Co., Ltd.) and 15.16 g of cation exchange resin (product name: Amberlyst [registered trademark] 15JWET, Organo Corporation) were added, stirred at 25 to 30°C for 4 hours, and then filtered. The reaction product obtained was analyzed by GPC and found to have a weight average molecular weight of 11,300 in terms of standard polystyrene. The reaction product obtained is presumed to be a copolymer having a structural unit represented by the following formula (9). [ka]

[0041] <Comparative Synthesis Example 1> To 148.30 g of PGME, 40.00 g of YX4000 (manufactured by Mitsubishi Chemical Corporation), 19.54 g of Cis-1,2-Cyclohexanedicarboxylic Acid (manufactured by Tokyo Chemical Industry Co., Ltd.), and 4.01 g of ethyltriphenylphosphonium bromide as a catalyst were added, and the mixture was reacted at 140° C. for 24 hours to obtain a solution containing a reaction product. 64.00 g of anion exchange resin (product name: Dowex [registered trademark] MONOSPHERE [registered trademark] 550A, Muromachi Technos Co., Ltd.) and 64.00 g of cation exchange resin (product name: Amberlyst [registered trademark] 15JWET, Organo Co., Ltd.) were added, and the mixture was stirred at 25° C. to 30° C. for 4 hours and then filtered. The reaction product obtained was subjected to GPC analysis and found to have a weight average molecular weight, calculated in terms of standard polystyrene, of 2,000. The reaction product obtained is presumed to be a copolymer having a structural unit represented by the following formula (10). [ka]

[0042] <Comparative Synthesis Example 2> 17.67g of PGMEA, 5.00g of EHPE-3150 (manufactured by Daicel Corporation), 3.11g of 9-anthracene carboxylic acid, 2.09g of benzoic acid, and 0.62g of ethyl triphenylphosphonium bromide were added to 7.57g of PGME, and the mixture was heated under reflux for 13 hours under a nitrogen atmosphere. 16g of a cation exchange resin (product name: Amberlyst [registered trademark] 15JWET, Organo Corporation) and 16g of anion exchange resin (product name: Dowex [registered trademark] MONOSPHERE [registered trademark] 550A, Muromachi Technos Corporation) were added to the resulting solution, and the mixture was stirred at 25°C to 30°C for 4 hours and then filtered. The reaction product obtained was subjected to GPC analysis and found to have a weight average molecular weight, calculated in terms of standard polystyrene, of 4,700. The reaction product obtained is presumed to be a copolymer having a structural unit represented by the following formula (11). [ka]

[0043] [Preparation of resist underlayer film-forming composition] <Example 1> 8.49g of PGME, 5.65g of PGMEA, and 0.12g of a 1wt% PGME solution of a surfactant (manufactured by DIC Corporation, product name: R-30N) were mixed with 5.74g of a solution containing 1.16g of the copolymer obtained in Synthesis Example 1 (solvent was the PGME used in the synthesis, solid content was 20.18wt%) to prepare a 5.8wt% solution. The solution was filtered using a polytetrafluoroethylene microfilter having a pore size of 0.2μm to prepare a resist underlayer film forming composition.

[0044] <Example 2> 7.06g of PGME, 5.61g of PGMEA, and 0.13g of a 1wt% PGME solution of a surfactant (manufactured by DIC Corporation, product name: R-30N) were mixed with 7.20g of a solution containing 1.30g of the copolymer obtained in Synthesis Example 2 (solvent was the PGME used in the synthesis, solid content was 18.05wt%) to prepare a 6.5wt% solution. The solution was filtered using a polytetrafluoroethylene microfilter having a pore size of 0.2μm to prepare a resist underlayer film forming composition.

[0045] <Example 3> 7.19g of PGME, 5.61g of PGMEA, and 0.13g of a 1 wt% PGME solution of a surfactant (manufactured by DIC Corporation, product name: R-30N) were mixed with 7.07g of a solution containing 1.30g of the copolymer obtained in Synthesis Example 3 (solvent was the PGME used in the synthesis, solid content was 18.38wt%) to prepare a 6.5 mass% solution. The solution was filtered using a polytetrafluoroethylene microfilter having a pore size of 0.2μm to prepare a resist underlayer film forming composition.

[0046] <Example 4> 3.74 g of PGME, 2.72 g of PGMEA, and 0.07 g of a 1 wt % PGMEA solution of a surfactant (manufactured by DIC Corporation, product name: R-30N) were mixed with 3.47 g of a solution containing 0.70 g of the copolymer obtained in Synthesis Example 1 (solvent was the PGME used in the synthesis, solid content was 20.18 wt %). The solution was filtered using a polytetrafluoroethylene microfilter having a pore size of 0.2 μm to prepare a resist underlayer film forming composition.

[0047] <Example 5> 1.73 g of a solution containing 0.35 g of the copolymer obtained in Synthesis Example 1 (solvent was the PGME used in the synthesis, solid content was 20.18 wt%) was mixed with 1.18 g of a 29.68 wt% PGMEA solution of GT-401 (manufactured by Daicel Corporation, product name: Epolead GT401), 5.13 g of PGME, 1.69 g of PGMEA, and 0.28 g of a 1 wt% PGMEA solution of a surfactant (manufactured by DIC Corporation, product name: R-30N). The solution was filtered using a polytetrafluoroethylene microfilter having a pore size of 0.2 μm to prepare a resist underlayer film forming composition.

[0048] <Example 6> 0.88 g of a 29.68 wt % PGMEA solution of GT-401 (manufactured by Daicel Corporation, product name: Epolead GT401), 6.65 g of PGME, 3.36 g of PGMEA, and 0.21 g of a 1 wt % PGMEA solution of a surfactant (manufactured by DIC Corporation, product name: R-30N) were mixed with 3.90 g of a solution containing 0.79 g of the copolymer obtained in Synthesis Example 1 (solvent was the PGME used in the synthesis, solid content was 20.18 wt %). The solution was filtered using a polytetrafluoroethylene microfilter having a pore size of 0.2 μm to prepare a resist underlayer film forming composition.

[0049] <Comparative Example 1> 4.89g of PGME, 2.76g of PGMEA, and 0.060g of a 1 wt% PGME solution of a surfactant (manufactured by DIC Corporation, product name: R-30N) were mixed with 2.29g of a solution containing 0.60g of the copolymer obtained in Comparative Synthesis Example 1 (solvent was the PGME used in the synthesis, solid content was 26.18wt%) to prepare a 6.0 mass% solution. The solution was filtered using a polytetrafluoroethylene microfilter having a pore size of 0.2μm to prepare a resist underlayer film forming composition.

[0050] <Comparative Example 2> 19.52 g of the solution containing 4.51 g of the copolymer obtained in Comparative Synthesis Example 2 (solvent is the PGME / PGMEA mixed solvent used in the synthesis, solid content is 23.26 wt%) was mixed with 1.14 g of tetramethoxymethylglycoluril (product name: POWDERLINK [registered trademark] 1174, manufactured by Nippon Cytec Industries Co., Ltd.), 3.41 g of a 1 wt% PGME solution of pyridium p-toluenesulfonate, 50.68 g of PGME, 14.80 g of PGMEA, and 0.45 g of a 1 wt% PGME solution of a surfactant (manufactured by DIC Co., Ltd., product name: R-30) to obtain a 6.35 mass% solution. The solution was filtered using a polytetrafluoroethylene microfilter with a pore size of 0.2 μm to prepare a resist underlayer film forming composition.

[0051] [Photoresist solvent elution test] The resist underlayer film forming compositions prepared in Examples 1 to 3, Comparative Example 1, and Comparative Example 2 were each applied onto a silicon wafer using a spinner. Then, the wafer was baked on a hot plate for 1 minute at the temperature shown in Table 1 below to form a resist underlayer film (film thickness: 0.2 μm). These resist underlayer films were immersed in PGME and PGMEA, which are solvents used in photoresist solutions, and it was confirmed that they were insoluble in both solvents, and the results are shown in Table 1 below with "○". Comparative Example 1 was dissolved in both solvents, so no further testing was performed. In addition to the same tests as in Examples 1 to 3, Examples 4 to 6 were baked at the temperatures shown in Table 1 below, and then irradiated with 500 mJ / cm2 ultraviolet light using an ultraviolet light irradiation device using a UV irradiation unit (wavelength 172 nm) manufactured by Ushio Inc. to form a resist underlayer film (film thickness 0.2 μm). Then, tests similar to those in Examples 1 to 3 were carried out. Since the photocurable material is a material that is not cured by heat at the temperatures shown in Table 1 but is cured by light, it was confirmed that it tends to dissolve in the photoresist solution after baking and become insoluble after light irradiation.

[0052] [Optical parameter testing] The resist underlayer film forming compositions prepared in Examples 1 to 6 and Comparative Example 2 were applied onto a silicon wafer by a spinner. Then, the resist underlayer film was baked on a hot plate for 1 minute at the temperature shown in Table 1 below to form a resist underlayer film (film thickness 0.2 μm). In Examples 4 to 6, the resist underlayer films were cured by irradiating 500 mJ / cm2 of ultraviolet light using an ultraviolet light irradiation device using a UV irradiation unit (wavelength 172 nm) after baking at a predetermined temperature. The refractive index (n value) and attenuation coefficient (k value) of these resist underlayer films at a wavelength of 193 nm were measured using an optical ellipsometer (JA Woollam, VUV-VASE VU-302). The results are shown in Table 1 below. In order for the resist underlayer film to have a sufficient antireflection function, it is desirable for the k value at a wavelength of 193 nm to be 0.1 or more.

[0053] [Table 1]

[0054] [Coating test for stepped substrate] For the evaluation of planarization, a comparison was made between the coating thickness of a trench pattern area (TRENCH) with a trench width of 50 nm and a pitch of 100 nm and an open area (OPEN) with no pattern formed on a 230 nm thick SiO2 substrate. The resist underlayer film forming compositions of Examples 1 to 6 and Comparative Example 2 were applied to the substrate in a thickness of 200 nm, and then baked on a hot plate at the temperature shown in Table 1 for 1 minute to form a resist underlayer film (thickness 0.2 μm). In addition, in Examples 4 to 6, the compositions were cured by irradiating 500 mJ / cm2 of ultraviolet light using an ultraviolet light irradiation device using a UV irradiation unit (wavelength 172 nm) after baking at a predetermined temperature. The step coverage of this substrate was observed using a scanning electron microscope (S-4800) manufactured by Hitachi High-Technologies Corporation, and the step coverage was evaluated by measuring the film thickness difference between the trench area (patterned area) and the open area (no patterned area) of the step substrate (the coating step between the trench area and the open area, which is called Bias). The film thickness and coating step values ​​in each area are shown in Table 2. In the flattening evaluation, the smaller the bias (coating step) value, the higher the flattening property.

[0055] [Table 2] Comparing the planarization properties, the results of Examples 1 to 6 show that the coating step difference between the pattern area and the open area is smaller than the result of Comparative Example 2, and therefore it can be said that the resist underlayer films obtained from the resist underlayer film forming compositions of Examples 1 to 6 have good planarization properties. Furthermore, although the materials of Examples 1 and 4 have the same composition, it is possible to improve the planarization properties of the same material by utilizing photocuring. [Industrial Applicability]

[0056] The resist underlayer film-forming composition of the present invention exhibits high reflowability by heating after being applied to a substrate, and can be applied evenly even on a substrate having steps to form a flat film. In addition, since the composition has an appropriate antireflection effect, it is useful as a resist underlayer film-forming composition.

Claims

1. A resist underlayer film forming composition comprising: a copolymer composed of a repeating structural unit represented by the following formula (1a), or a copolymer having at least one repeating structural unit selected from the group consisting of a repeating structural unit represented by the following formula (1a) and repeating structural units represented by the following formulas (1b) to (1k); and an organic solvent. 【Chemistry 1】 【Chemistry 2】

2. The resist underlayer film forming composition according to claim 1 , further comprising a photocrosslinking agent.

3. The resist underlayer film forming composition according to claim 1 or 2, further comprising a compound represented by the following formula (5) and / or a compound represented by the following formula (6): 【Chemistry 3】 (In the formula, X 2 represents a carbonyl group or a methylene group, l and m each independently represent an integer of 0 to 5 and satisfy the relational formula 3≦l+m≦10; R 3 represents an alkylene or alkenylene group having 1 to 4 carbon atoms or a single bond, k represents 0 or 1, and n represents an integer of 2 to 4.

4. The resist underlayer film forming composition according to claim 1 , further comprising a surfactant.

5. 5. A method for producing a resist underlayer film, comprising the steps of applying the resist underlayer film forming composition according to claim 1 to a substrate having a step, and then heating the composition to thermally cure it.

6. The method for producing a resist underlayer film according to claim 5, wherein the heating temperature in the heating step is 200°C to 300°C.

7. The method for producing a resist underlayer film according to claim 6 , further comprising an exposure step of exposing the resist to light.

8. A method for producing a resist underlayer film without an exposure step, comprising the steps of applying the resist underlayer film forming composition according to any one of claims 1 to 4 to a substrate having a step and thermally curing the composition at 250°C or higher.

Citation Information

Patent Citations

  • Antireflective coating composition with improved spin bowl compatibility

    JP2004533637A

  • Liquid resin composition and semiconductor device using the same

    JP2008088278A

  • Laminate and patterning method

    JP2018063382A

  • Composition for resist underlayer film formation for forming photocrosslinking cured resist underlayer film

    WO2006115044A1

  • Silicon-containing resist underlying layer film forming composition for formation of photocrosslinking cured resist underlying layer film