Hardening composition

The combination of branched and linear polyoxyalkylene polymers with hydrolyzable silyl groups addresses the flexibility and viscosity issues in silicone-based compositions, resulting in a cured product with enhanced water-resistant adhesion and handleability.

JP7590749B2Active Publication Date: 2024-11-27SEKISUI FULLER CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020088707
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-05-21
Publication Date
2024-11-27
Estimated Expiration
2040-05-21

AI Technical Summary

Technical Problem

Modified silicone-based curable compositions face issues with reduced flexibility and increased viscosity when high molecular weight polymers are used, leading to poor handleability and water-resistant adhesion.

Method used

A curable composition comprising a polyoxyalkylene polymer with a branched main chain and hydrolyzable silyl group at the molecular end, combined with a linear polyoxyalkylene polymer having a hydrolyzable silyl group, in a specific mass ratio, to enhance flexibility and water-resistant adhesion while maintaining low viscosity.

Benefits of technology

The composition achieves a cured product with excellent flexibility, water-resistant adhesion, and improved handleability, reducing molecular gaps and swelling due to water absorption, while maintaining toughness and normal adhesion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590749000001
    Figure 0007590749000001
  • Figure 0007590749000002
    Figure 0007590749000002
Patent Text Reader

Abstract

To provide a curable composition enabling formation of a cured object excellent in water proof adhesive property while maintaining handleability and flexibility of a modified silicone curable composition.SOLUTION: A curable composition contains: a polyoxyalkylene-based polymer (A) whose main chain has a branched chain and which has a hydrolysis silyl group on a molecular terminal thereof; and (B) a polyoxyalkylene-based polymer whose main chain is linear and which has a hydrolysis silyl group on a molecular terminal thereof. A ratio of a content of the polyoxyalkylene polymer (A) and a content of the polyoxyalkylene polymer (B) (pts.mass of the polyoxyalkylene polymer (A) / pts.mass of the polyoxyalkylene polymer (B)) is 1 or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a curable composition. [Background technology]

[0002] Modified silicone-based curable compositions containing a polyoxyalkylene polymer having a hydrolyzable silyl group are safe in that they do not generate toxic substances during curing, and the cured products obtained by curing have excellent flexibility (elasticity), and therefore are widely used as sealants and adhesives.

[0003] Modified silicone-based curable compositions are often used outdoors, and therefore require durability and water-resistant adhesion.

[0004] In general, modified silicone-based curable compositions tend to have poor water-resistant adhesion, and therefore Patent Documents 1 and 2 disclose techniques in which an epoxy resin or an isocyanate compound is blended therein. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 5226314 [Patent Document 2] JP 2009-155407 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, the curable compositions disclosed in Patent Documents 1 and 2 have the problem that the cured product tends to be too hard, reducing the flexibility (elasticity) that is a characteristic of modified silicone-based curable compositions.

[0007] In view of this, it has been proposed to use a high molecular weight polymer in order to improve the elasticity of the cured product of the curable composition. However, when a high molecular weight polymer is used, the viscosity of the curable composition increases, which causes another problem of reduced handleability in applications such as adhesives that are applied manually.

[0008] The present invention provides a curable composition that can produce a cured product with excellent water-resistant adhesion while maintaining the handleability and flexibility of a modified silicone-based curable composition. [Means for solving the problem]

[0009] The curable composition of the present invention comprises A polyoxyalkylene polymer (A) having a branched main chain and a hydrolyzable silyl group at a molecular end; (B) a polyoxyalkylene polymer having a linear main chain and a hydrolyzable silyl group at a molecular end, The ratio of the content of the polyoxyalkylene polymer (A) to the content of the polyoxyalkylene polymer (B) [parts by mass of polyoxyalkylene polymer (A) / parts by mass of polyoxyalkylene polymer (B)] is 1 or more.

[0010] [Polyoxyalkylene polymer (A)] The curable composition contains a polyoxyalkylene polymer (A) whose main chain has a branched chain and whose molecular terminal has a hydrolyzable silyl group. The polyoxyalkylene polymer (A) may be used alone or in combination of two or more kinds. In the present invention, the "main chain" of a polyoxyalkylene polymer refers to the longest molecular chain in the molecule. The polyoxyalkylene polymer (A) whose main chain has a branched chain and whose molecular terminal has a hydrolyzable silyl group may be simply referred to as "polyoxyalkylene polymer (A)".

[0011] The polyoxyalkylene polymer (A) has a branched main chain. The branched main chain of the polyoxyalkylene polymer (A) causes the branched chains to become entangled in the cured product of the curable composition, reducing the gap between molecules, thereby reducing the water absorption of the cured product. In this way, the water absorption of the cured product is reduced, preventing the cured product from swelling due to water absorption, and improving the water-resistant adhesion of the cured product.

[0012] The main chain of the polyoxyalkylene polymer (A) is preferably a polymer containing a repeating unit represented by the general formula (1). -(OR 1 ) n - (1) (In the formula, R 1 represents an alkylene group having 1 to 14 carbon atoms, and n is the number of repeating units and is a positive integer.

[0013] The main chain of the polyoxyalkylene polymer (A) may consist of only one type of repeating unit, or may consist of two or more types of repeating units.

[0014] Examples of the main chain skeleton of the polyoxyalkylene polymer (A) include polyoxyethylene, polyoxypropylene, polyoxybutylene, polyoxytetramethylene, polyoxyethylene-polyoxypropylene copolymer, and polyoxypropylene-polyoxybutylene copolymer, and polyoxypropylene is preferred because it improves the flexibility of the cured product of the curable composition.

[0015] The polyoxyalkylene polymer (A) has a branched chain in the main chain. A "branched chain" refers to a molecular chain having two or more carbon atoms. Therefore, methyl groups are not included in the branched chain.

[0016] As described above, the branched chain in the main chain of the polyoxyalkylene polymer (A) is intended to reduce the gap between molecules due to the entanglement of the molecular chains in the cured product of the curable composition, so it is necessary to have a certain molecular chain length. Therefore, the branched chain has a carbon number of 2 or more. The carbon number of the branched chain is preferably 14 or less, more preferably 13 or less, and more preferably 12 or less, because it can reduce the viscosity of the curable composition and improve the handleability.

[0017] The branched chain in the main chain of the polyoxyalkylene polymer (A) is not particularly limited as long as it has two or more carbon atoms. However, a polyoxyalkylene chain is preferred because it improves compatibility with the polyoxyalkylene polymer (B), improves the handleability of the curable composition, and improves the flexibility and water-resistant adhesion of a cured product of the curable composition.

[0018] The branched chain in the main chain of the polyoxyalkylene polymer (A) is preferably a polymer containing a repeating unit represented by the general formula (2). -(OR 2 ) m - (2) (In the formula, R 2 represents an alkylene group having 1 to 14 carbon atoms, and m is the number of repeating units and is an integer of 2 or more.

[0019] The branched chain in the main chain of the polyoxyalkylene polymer may be composed of only one type of repeating unit, or may be composed of two or more types of repeating units.

[0020] Examples of the branched chain skeleton in the main chain of the polyoxyalkylene polymer (A) include polyoxyethylene, polyoxypropylene, polyoxybutylene, polyoxytetramethylene, polyoxyethylene-polyoxypropylene copolymer, and polyoxypropylene-polyoxybutylene copolymer. Polyoxypropylene is preferred because the cured product of the curable composition has excellent water-resistant adhesion while maintaining excellent flexibility.

[0021] In the polyoxyalkylene polymer (A), the main chain skeleton structure having a branched chain preferably contains a structure represented by general formula (3).

[0022] [ka] (In the formula, R 3 , R 4 and R 5 R each represents an alkylene group having 1 to 14 carbon atoms. 6 R is an alkylene group having 1 to 6 carbon atoms. 3 , R 4 , R 5 and R 6 may be the same or different. x and y are the numbers of repeating units and are positive integers. z is the number of repeating units and is an integer of 2 or more.

[0023] The polyoxyalkylene polymer (A) has a hydrolyzable silyl group at the molecular end. The hydrolyzable silyl group is preferably bonded to only one of the two ends of the main chain, or to both ends. When the hydrolyzable silyl group is bonded to the end of the main chain, the cured product of the curable composition can maintain excellent flexibility and can be imparted with excellent normal adhesion, while also being imparted with excellent water-resistant adhesion. When the polyoxyalkylene polymer (A) has a plurality of hydrolyzable silyl groups in the molecule, the hydrolyzable silyl groups may be the same or different from each other.

[0024] The hydrolyzable silyl group refers to a group that undergoes a condensation reaction in the presence of moisture or a crosslinking agent, and if necessary, using a catalyst, such as a silicon-containing group or a silanol group having a hydrolyzable group bonded to a silicon atom. Note that a silanol group refers to a functional group in which a hydroxyl group is directly bonded to a silicon atom (≡Si-OH).

[0025] The hydrolyzable group of the hydrolyzable silyl group is not particularly limited, and examples thereof include a hydrogen atom, a halogen atom, an alkoxy group, an acyloxy group, a ketoximate group, an amino group, an amide group, an acid amide group, an aminooxy group, a mercapto group, and an alkenyloxy group.

[0026] Among these, the hydrolyzable silyl group is preferably an alkoxysilyl group, since it can impart excellent water-resistant adhesion while maintaining the flexibility of the cured product of the curable composition and imparting excellent normal adhesion.

[0027] The alkoxysilyl group is -SiR 7 j (OR 8 ) 3-j Preferably, the compound has a structure represented by the formula: 7 R represents an alkyl group having 1 to 20 carbon atoms which may have a substituent, or a hydrogen atom. 8 represents an alkyl group having a carbon number of 1 to 6. j represents an integer of 0 to 2.

[0028] Examples of the alkoxysilyl group include trialkoxysilyl groups such as trimethoxysilyl group, triethoxysilyl group, triisopropoxysilyl group, and triphenoxysilyl group; dialkoxysilyl groups such as propyldimethoxysilyl group, methyldimethoxysilyl group, and methyldiethoxysilyl group; and monoalkoxysilyl groups such as dimethylmethoxysilyl group and dimethylethoxysilyl group. Among them, dialkoxysilyl groups are preferred, and dimethoxysilyl groups are more preferred, since they can maintain the flexibility of the cured product of the curable composition, impart excellent normal adhesion, and impart excellent water-resistant adhesion.

[0029] In the polyoxyalkylene polymer (A), the average number of hydrolyzable silyl groups in one molecule is preferably from 1 to 3, and more preferably from 1 to 2. When the number of hydrolyzable silyl groups in the polyoxyalkylene polymer (A) is within the above range, the flexibility of the cured product of the curable composition is improved.

[0030] In the present invention, the average number of hydrolyzable silyl groups per molecule in the polyoxyalkylene polymer is 1 It can be calculated based on the concentration of hydrolyzable silyl groups in the polyoxyalkylene polymer determined by H-NMR and the number average molecular weight of the polyoxyalkylene polymer determined by GPC.

[0031] The polyoxyalkylene polymer (A) is preferably a polyoxypropylene polymer having a main chain skeleton which is polyoxypropylene and has branched chains, and having a dimethoxysilyl group as a hydrolyzable silyl group at the end of the main chain skeleton, because the cured product of the curable composition maintains excellent flexibility and has excellent water-resistant adhesion.

[0032] As the polyoxypropylene-based polymer having a polyoxypropylene main chain skeleton, a branched chain, and a dimethoxysilyl group as a hydrolyzable silyl group at the end of the main chain skeleton, a commercially available product can be used. The commercially available product can be one sold by AGC under the trade names "Exestar 6250" and "Exestar 3430."

[0033] In the present invention, the polyoxyalkylene polymer having a hydrolyzable silyl group can be produced, for example, by reacting a polyoxyalkylene polymer having a functional group such as a hydroxyl group at its terminal with an organic compound having an active group and an unsaturated group that are reactive with the functional group, and then allowing a hydrosilane having a hydrolyzable group to act on the resulting reaction product to carry out hydrosilylation.

[0034] The number average molecular weight of the polyoxyalkylene polymer (A) is preferably 18000 or less, more preferably 17000 or less, and more preferably 15000 or less. The number average molecular weight of the polyoxyalkylene polymer (A) is preferably 5000 or more, more preferably 6000 or more, and more preferably 7000 or more. When the number average molecular weight of the polyoxyalkylene polymer (A) is 18000 or less, the water-resistant adhesion of the cured product of the curable composition is improved, and the viscosity of the curable composition can be kept low, improving the handleability of the curable composition and imparting excellent coatability to the curable composition. When the number average molecular weight of the polyoxyalkylene polymer (A) is 5000 or more, the excellent flexibility of the cured product of the curable composition can be maintained, and excellent normal adhesion can be imparted to the cured product.

[0035] In the present invention, the number average molecular weight and weight average molecular weight of the polyoxyalkylene polymer are values ​​measured by GPC (gel permeation chromatography) and converted into polystyrene. Specifically, 6 to 7 mg of the polyoxyalkylene polymer is collected, the collected polyoxyalkylene polymer is fed to a test tube, and then an o-DCB (orthodichlorobenzene) solution containing 0.05% by mass of BHT (dibutylhydroxytoluene) is added to the test tube to dilute the polyoxyalkylene polymer to a concentration of 1 mg / mL to prepare a diluted solution.

[0036] The dilution solution is shaken at 25 rpm at 145° C. for 1 hour using a dissolution filter to dissolve the polyoxyalkylene polymer in the o-DCB solution containing BHT to obtain a measurement sample. The number average molecular weight and weight average molecular weight of the polyoxyalkylene polymer can be measured by the GPC method using this measurement sample.

[0037] The number average molecular weight and weight average molecular weight of the polyoxyalkylene polymer can be measured, for example, using the following measuring device and under the following measuring conditions. Measuring device: TOSOH product name "HLC-8121GPC / HT" Measurement conditions Column: TSKgelGMHHR-H(20)HT x 3 TSKguardcolumn-HHR(30)HT x 1 Mobile phase: o-DCB 1.0mL / min Sample concentration: 1mg / mL Detector: Bryce type refractometer Standard material: Polystyrene (TOSOH, molecular weight: 500-8420000) Elution conditions: 145℃ SEC temperature: 145℃

[0038] [Polyoxyalkylene polymer (B)] The curable composition contains a polyoxyalkylene polymer (B) having a linear main chain and a hydrolyzable silyl group at the molecular end. The polyoxyalkylene polymer (B) may be used alone or in combination of two or more kinds. The polyoxyalkylene polymer (B) having a linear main chain and a hydrolyzable silyl group at the molecular end may be simply referred to as "polyoxyalkylene polymer (B)".

[0039] The curable composition contains a polyoxyalkylene polymer (B) whose main chain is linear, and thus the cured product of the curable composition is given flexibility and excellent adhesion under normal conditions. Furthermore, the viscosity of the curable composition is reduced to improve the handling properties, and excellent coatability is given to the curable composition. The "linear" main chain means that the main chain does not have the above-mentioned branched chain.

[0040] The main chain of the polyoxyalkylene polymer (B) is preferably a polymer containing a repeating unit represented by the general formula (4). -(OR 9 )p- (4) (In the formula, R 9 represents an alkylene group having 1 to 14 carbon atoms, and p is the number of repeating units and is a positive integer.

[0041] The main chain of the polyoxyalkylene polymer (B) may consist of only one type of repeating unit, or may consist of two or more types of repeating units.

[0042] Examples of the main chain skeleton of the polyoxyalkylene polymer (B) include polyoxyethylene, polyoxypropylene, polyoxybutylene, polyoxytetramethylene, polyoxyethylene-polyoxypropylene copolymer, and polyoxypropylene-polyoxybutylene copolymer, and polyoxypropylene is preferred because it improves the flexibility of the cured product of the curable composition.

[0043] The polyoxyalkylene polymer (B) has a hydrolyzable silyl group at the molecular end. The hydrolyzable silyl group is preferably bonded to one or both ends of the main chain, and is preferably bonded to only one end of the main chain. When the hydrolyzable silyl group is bonded to the end of the main chain, the cured product of the curable composition can be imparted with excellent water-resistant adhesion while maintaining excellent flexibility and imparting excellent normal adhesion. When the hydrolyzable silyl group is bonded to only one of the two ends of the main chain, the water-resistant adhesion of the cured product of the curable composition is improved. In addition, when the polyoxyalkylene polymer (B) has a plurality of hydrolyzable silyl groups in the molecule, the hydrolyzable silyl groups may be the same or different from each other.

[0044] In the polyoxyalkylene polymer (B), the hydrolyzable silyl group is preferably bonded to the end of the main chain via an alkylene group having 1 to 25 carbon atoms (preferably an alkylene group having 1 to 6 carbon atoms). When the hydrolyzable silyl group is bonded via an alkylene group having 1 to 25 carbon atoms, the normal adhesion of the cured product of the curable composition is improved.

[0045] In the polyoxyalkylene polymer (B), the hydrolyzable silyl group may be bonded to the end of the main chain via a urethane bond. When the hydrolyzable silyl group is bonded to the end of the main chain via a urethane bond, the normal adhesiveness of the cured product of the curable composition is improved. Since the flexibility of the cured product of the curable composition is improved, it is preferable that the urethane bond and the hydrolyzable silyl group are bonded via an alkylene group (preferably an alkylene group having 1 to 25 carbon atoms).

[0046] The hydrolyzable silyl group in the polyoxyalkylene polymer (B) is the same as the hydrolyzable silyl group in the polyoxyalkylene polymer (A), and therefore a description of the same structure will be omitted. Note that the hydrolyzable silyl group in the polyoxyalkylene polymer (A) and the hydrolyzable silyl group in the polyoxyalkylene polymer (B) may be the same or different.

[0047] Examples of the alkoxysilyl group include trialkoxysilyl groups such as trimethoxysilyl group, triethoxysilyl group, triisopropoxysilyl group, and triphenoxysilyl group; dialkoxysilyl groups such as propyldimethoxysilyl group, methyldimethoxysilyl group, and methyldiethoxysilyl group; and monoalkoxysilyl groups such as dimethylmethoxysilyl group and dimethylethoxysilyl group. Among them, dialkoxysilyl group and trimethoxysilyl group are preferred, dialkoxysilyl group are more preferred, and dimethoxysilyl group is more preferred, because they can maintain the flexibility of the cured product of the curable composition, impart excellent normal adhesion, and impart excellent water-resistant adhesion.

[0048] In the polyoxyalkylene polymer (B), the average number of hydrolyzable silyl groups in one molecule is preferably 1 to 2. When the number of hydrolyzable silyl groups in the polyoxyalkylene polymer (B) is within the above range, the toughness of the cured product of the curable composition is improved.

[0049] The polyoxyalkylene polymer (B) may be a commercially available product. Polyoxypropylene polymers (B) having a main chain skeleton of polyoxypropylene and a hydrolyzable silyl group at one end of the main chain skeleton are commercially available under the trade names "SAT135" and "SAT145" from Kaneka Corporation, "Exestar S1000N" from AGC Corporation, and "XM20" from Wacker.

[0050] The number average molecular weight of the polyoxyalkylene polymer (B) is preferably 30,000 or less, more preferably 25,000 or less, and more preferably 20,000 or less. The number average molecular weight of the polyoxyalkylene polymer (B) is preferably 3,000 or more, more preferably 4,000 or more, and more preferably 5,000 or more. When the number average molecular weight of the polyoxyalkylene polymer (B) is 30,000 or less, the viscosity of the curable composition can be kept low, the handleability of the curable composition can be improved, and excellent coatability can be imparted to the curable composition. When the number average molecular weight of the polyoxyalkylene polymer (B) is 3,000 or more, the excellent flexibility of the cured product of the curable composition can be maintained, and excellent normal adhesion can be imparted to the cured product.

[0051] In the curable composition, the ratio (mass ratio) of the content of the polyoxyalkylene polymer (A) to the content of the polyoxyalkylene polymer (B) [parts by mass of the polyoxyalkylene polymer (A) / parts by mass of the polyoxyalkylene polymer (B)] is at least 1, preferably at least 1.1, and more preferably at least 1.2. The ratio (mass ratio) of the content of the polyoxyalkylene polymer (A) to the content of the polyoxyalkylene polymer (B) [parts by mass of the polyoxyalkylene polymer (A) / parts by mass of the polyoxyalkylene polymer (B)] is preferably 5 or less, more preferably 4 or less, and more preferably 3.5 or less. When the ratio (mass ratio) of the content of the polyoxyalkylene polymer (A) to the content of the polyoxyalkylene polymer (B) [parts by mass of the polyoxyalkylene polymer (A) / parts by mass of the polyoxyalkylene polymer (B)] is 1 or more, the cured product of the curable composition can be improved in water-resistant adhesion while maintaining excellent flexibility, and excellent toughness can be imparted to the cured product. When the ratio (mass ratio) of the content of the polyoxyalkylene polymer (A) to the content of the polyoxyalkylene polymer (B) [parts by mass of the polyoxyalkylene polymer (A) / parts by mass of the polyoxyalkylene polymer (B)] is 5 or less, the cured product of the curable composition can be imparted with toughness while maintaining flexibility.

[0052] [Inorganic filler] The curable composition may contain an inorganic filler. By using the inorganic filler in combination with the polyoxyalkylene polymers (A) and (B), it is possible to impart excellent toughness to the cured product of the curable composition while maintaining excellent flexibility of the cured product.

[0053] The inorganic filler is not particularly limited, and examples thereof include calcium carbonate, magnesium carbonate, calcium oxide, silicic acid hydrate, silicic acid anhydride, finely powdered silica, calcium silicate, titanium dioxide, clay, talc, carbon black, and glass balloons, with calcium carbonate being preferred. The inorganic filler may be used alone or in combination of two or more kinds.

[0054] Preferred examples of calcium carbonate include ground calcium carbonate and precipitated calcium carbonate.

[0055] Ground calcium carbonate can be obtained, for example, by grinding natural calcium carbonate such as natural chalk, marble, or limestone into a fine powder.

[0056] Precipitated calcium carbonate can be produced, for example, by using limestone as a raw material through a chemical reaction. Examples of precipitated calcium carbonate include light calcium carbonate and colloidal calcium carbonate, with colloidal calcium carbonate being preferred. The light calcium carbonate preferably has a primary particle size of 1 to 3 μm. The light calcium carbonate preferably has a spindle or columnar shape. The colloidal calcium carbonate preferably has a primary particle size of 0.02 to 0.1 μm. The colloidal calcium carbonate preferably has a cubic shape.

[0057] As the calcium carbonate, either heavy calcium carbonate or precipitated calcium carbonate may be used, or both may be used. By using a combination of heavy calcium carbonate and precipitated calcium carbonate, it is possible to impart thixotropy to the curable composition and prevent coating unevenness.

[0058] The calcium carbonate may or may not be surface-treated. Surface-treated calcium carbonate and non-surface-treated calcium carbonate may be used alone or in combination of two or more. When the calcium carbonate is surface-treated, the surface treatment is preferably performed using a fatty acid, a fatty acid ester, or the like.

[0059] The content of the inorganic filler in the curable composition is preferably 100 parts by mass or more, more preferably 150 parts by mass or more, per 100 parts by mass of the polyoxyalkylene polymer (A). The content of the inorganic filler in the curable composition is preferably 500 parts by mass or less, more preferably 400 parts by mass or less, per 100 parts by mass of the polyoxyalkylene polymer (A). When the content of the inorganic filler is 100 parts by mass or more, excellent toughness can be imparted to the cured product of the curable composition. When the content of the inorganic filler is 500 parts by mass or less, excellent flexibility can be imparted to the cured product of the curable composition, and the water-resistant adhesion of the cured product can be improved.

[0060] [Silane coupling agents] The curable composition may contain a silane coupling agent. By containing a silane coupling agent, it is possible to impart excellent normal adhesion and water-resistant adhesion, particularly normal adhesion, to a cured product of the curable composition.

[0061] Examples of the silane coupling agent include aminosilane coupling agents, epoxysilane coupling agents, isocyanate silane coupling agents, mercaptosilane coupling agents, carboxysilane coupling agents, halogen silane coupling agents, carbamate silane coupling agents, alkoxysilane coupling agents, and acid anhydride silane coupling agents. Among them, the combined use of an aminosilane coupling agent and an epoxysilane coupling agent is preferred because the normal adhesion and water-resistant adhesion of the curable composition are improved by the synergistic effect with the polyoxyalkylene polymers (A) and (B).

[0062] Examples of the aminosilane coupling agent include 3-aminopropyltrimethoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, N,N'-bis-[3-(trimethoxysilyl)propyl]ethylenediamine, N,N'-bis-[3-(triethoxysilyl)propyl]ethylenediamine, N,N'-bis-[3-(methyldimethoxysilyl)propyl]ethylenediamine, N,N'-bis-[3-(trimethoxysilyl)propyl]hexamethylenediamine, and N,N'-bis-[3-(triethoxyl)propyl]hexamethylenediamine.

[0063] Among these, preferred examples of the aminosilane coupling agent include 3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, and N-(2-aminoethyl)-3-propyltriethoxysilane, and more preferred example is N-(2-aminoethyl)-3-aminopropyltrimethoxysilane.

[0064] The epoxy silane coupling agent refers to a compound that contains a silicon atom with an alkoxy group bonded to it in one molecule and a functional group that contains an epoxy group.The epoxy silane coupling agent is not particularly limited, and can be, for example, 3-glycidoxypropyl trimethoxysilane, 3-glycidoxypropyl triethoxysilane, 3-glycidoxypropyl methyl dimethoxysilane, 3-glycidoxypropyl ethyl diethoxysilane, and 2-(3,4 epoxycyclohexyl) ethyl trimethoxysilane, and is preferably 3-glycidoxypropyl triethoxysilane.

[0065] The content of the silane coupling agent in the curable composition is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, based on 100 parts by mass of the polyoxyalkylene polymer (A). The content of the silane coupling agent in the curable composition is preferably 20 parts by mass or less, more preferably 15 parts by mass or less, based on 100 parts by mass of the polyoxyalkylene polymer (A). When the content of the silane coupling agent is 0.5 parts by mass or more, sufficient normal state adhesion can be imparted to the cured product of the curable composition. When the content of the silane coupling agent is 20 parts by mass or less, the storage stability and handling of the curable composition can be improved.

[0066] [Silanol condensation catalyst] The curable composition may contain a silanol condensation catalyst. The silanol condensation catalyst is a catalyst for promoting a dehydration condensation reaction between silanol groups formed by, for example, hydrolysis of a hydrolyzable silyl group contained in a polyoxyalkylene polymer.

[0067] Examples of silanol condensation catalysts include dibutyltin dilaurate, dibutyltin oxide, dibutyltin diacetate, dibutyltin phthalate, bis(dibutyltin laurate) oxide, dibutyltin bis(acetylacetonate), dibutyltin bis(monoester maleate), tin octoate, dibutyltin octoate, dioctyltin oxide, dibutyltin bis(triethoxysilicate), dioctyltin bis(triethoxysilicate), dioctyltin dilaurate, bis(dibutyltin bistriethoxysilicate) oxide, and dibutyltin oxybisethoxysilane. Organotin compounds such as tetra-n-butoxy titanate and tetraisopropoxy titanate; cycloamidine compounds such as 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1,8-diazabicyclo[5.4.0]undec-7-ene, 6-dibutylamino-1,8-diazabicyclo[5.4.0]undec-7-ene, and 1,5-diazabicyclo[4.3.0]non-5-ene; dibutylamine-2-ethylhexoate. Other acidic and basic catalysts can also be used as silanol condensation catalysts. These silanol condensation catalysts may be used alone or in combination of two or more.

[0068] Among these, as the silanol condensation catalyst, an organotin compound is preferred, and dibutyltin bis(triethoxysilicate) is more preferred, since it can uniformly cure the curable composition.

[0069] The content of the silanol condensation catalyst in the curable composition is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, per 100 parts by mass of the polyoxyalkylene polymer (A). The content of the silanol condensation catalyst in the curable composition is preferably 10 parts by mass or less, more preferably 6 parts by mass or less, per 100 parts by mass of the polyoxyalkylene polymer (A). When the content of the silanol condensation catalyst is 0.1 parts by mass or more, the curability of the curable composition is improved. When the content of the silanol condensation catalyst is 10 parts by mass or less, the cured product of the curable composition has excellent normal adhesion.

[0070] [Plasticizer] The curable composition may contain a plasticizer that does not have a reactive group. The plasticizer is not particularly limited, and examples thereof include phthalates such as dibutyl phthalate, di(2-ethylhexyl)phthalate, diisononyl phthalate, diisodecyl phthalate, and butyl benzyl phthalate; non-aromatic dibasic acid esters such as dioctyl adipate, dioctyl sebacate, dibutyl sebacate, and isodecyl succinate; aliphatic esters such as butyl oleate and methyl acetyl ricinoleate; esters of polyalkylene glycols such as diethylene glycol dibenzoate, triethylene glycol dibenzoate, and pentaerythritol ester; phosphates such as tricresyl phosphate and tributyl phosphate; trimellitic acid esters; polybutadiene, polybutene, polyisobutylene, butadiene-acrylonitrile, polychloroprene, polyisobutylene ... Examples of suitable plasticizers include: chlorinated paraffins; hydrocarbon oils such as alkyl diphenyls and partially hydrogenated terphenyls; process oils; polyether polyols such as polyethylene glycol, polypropylene glycol, and polytetramethylene glycol, and polyether polyols such as derivatives in which the hydroxyl groups of polyether polyols are converted to ester groups, ether groups, and the like; epoxy plasticizers such as epoxidized soybean oil and epoxy benzyl stearate; polyester plasticizers obtained from dibasic acids such as sebacic acid, adipic acid, azelaic acid, and phthalic acid and dihydric alcohols such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, and dipropylene glycol; and vinyl polymers obtained by polymerizing vinyl monomers such as acrylic plasticizers by various methods. The plasticizers may be used alone or in combination of two or more.

[0071] The number average molecular weight of the plasticizer is preferably 1000 or more, more preferably 1500 or more. The number average molecular weight of the plasticizer is more preferably 2900 or less, more preferably 2800 or less, and more preferably 2500 or less. When the number average molecular weight of the plasticizer is 1000 or more, it is preferable that the cured product of the curable composition can be given flexibility while also being tough. When the number average molecular weight of the plasticizer is 2900 or less, it is possible to suppress the viscosity of the curable composition to improve the handleability and to improve the flexibility of the cured product of the curable composition.

[0072] [Other additives] The curable composition may contain other additives such as antioxidants, dehydrating agents, UV absorbers, light stabilizers, thixotropic agents, pigments, dyes, antisettling agents, and solvents. Of these, antioxidants are preferred.

[0073] Examples of the antioxidant include hindered phenol-based antioxidants, monophenol-based antioxidants, bisphenol-based antioxidants, polyphenol-based antioxidants, etc., and the hindered phenol-based antioxidants are preferred. The content of the antioxidant in the curable composition is preferably 0.1 to 20 parts by mass, more preferably 0.3 to 10 parts by mass, based on 100 parts by mass of the polyoxyalkylene polymer (A).

[0074] [Dehydrating agent] The curable composition preferably contains a dehydrating agent, which can prevent the curable composition from being cured due to moisture contained in the air or the like during storage of the curable composition.

[0075] Examples of the dehydrating agent include silane compounds such as vinyltrimethoxysilane, dimethyldimethoxysilane, tetraethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, tetramethoxysilane, phenyltrimethoxysilane, and diphenyldimethoxysilane; and ester compounds such as methyl orthoformate, ethyl orthoformate, methyl orthoacetate, and ethyl orthoacetate.The dehydrating agent is preferably nivyltrimethoxysilane.The dehydrating agent may be used alone or in combination of two or more.

[0076] The content of the dehydrating agent in the curable composition is preferably 0.5 to 20 parts by mass, more preferably 1 to 15 parts by mass, and particularly preferably 1 to 5 parts by mass, based on 100 parts by mass of the polyoxyalkylene polymer (A). When the content of the dehydrating agent is 0.5 parts by mass or more, the storage stability of the curable composition is improved. When the content of the dehydrating agent is 20 parts by mass or less, the storage stability and handleability of the curable composition are improved.

[0077] The curable composition can be produced by mixing the polyoxyalkylene polymer (A) and the polyoxyalkylene polymer (B), and optionally other additives. The mixing is preferably carried out under reduced pressure, and the curable composition is preferably stored in a sealed container to prevent reaction with moisture in the outside air.

[0078] The viscosity of the curable composition at 23°C is preferably 15,000 mPa·s or more, and more preferably 20,000 mPa·s or more. The viscosity of the curable composition at 23°C is preferably 150,000 mPa·s or less, and more preferably 80,000 mPa·s or less. The viscosity of the curable composition at 23°C refers to a value measured using a B-type viscometer in accordance with JIS K6833 at 23°C and a rotation speed of 10 rpm.

[0079] The maximum stress (Tmax) of the cured product of the curable composition is preferably 1.3 or more. The maximum stress (Tmax) of the cured product of the curable composition is preferably 5 or less. When the maximum stress (Tmax) of the cured product is 1.3 or more, the normal adhesion and water-resistant adhesion of the cured product of the curable composition are improved.

[0080] The elongation (Emax) of the cured product of the curable composition is preferably 150% or more. The elongation (Emax) of the cured product of the curable composition is preferably 800% or less. When the elongation (Emax) of the cured product is 150% or more, the cured product can maintain excellent flexibility and can be imparted with excellent water-resistant adhesion.

[0081] The maximum stress (Tmax) and elongation (Emax) of the cured product of the curable composition refer to values ​​measured as follows. The curable composition is applied to a polyethylene plate so as to have a film thickness of 2.0 mm, and then cured for 14 days under an environment of 23°C and a relative humidity of 50% to cure the curable composition and produce a cured product sheet. The obtained cured product sheet is cut into a No. 3 dumbbell shape according to JIS K 6251 to prepare a test piece, and then a tensile test of the test piece is performed at a crosshead speed of 500 mm / min using an Instron tensile tester (e.g., manufactured by Instron Japan Co., Ltd.) to measure the maximum tensile stress (Tmax) and the displacement of the gauge length when the test piece breaks, and the elongation (Emax) is obtained.

[0082] The curable composition can be suitably used as an adhesive, a sealant, etc., and can be more suitably used as a construction adhesive (for example, a floor adhesive, etc.) The curable composition cures due to moisture (water) in the air or moisture (water) contained in an adherend such as a floor finishing material or a floor underlayment, and can bond and integrate the adherends with sufficient adhesive strength.

[0083] The curable composition is used, for example, in constructing a floor structure. The floor structure is constructed, for example, by adhering and integrating a floor finishing material onto a floor underlayment laid on a floor base via a cured product layer formed by curing the curable composition. The floor structure includes a floor base, a floor underlayment laid on the floor base, a cured product layer formed by curing the curable composition and formed on the floor underlayment and adhesively integrated with the floor underlayment, and a floor finishing material laid on the cured product layer and adhesively integrated with the cured product layer.

[0084] Examples of materials constituting floor finishing materials include wood-based materials such as plywood and medium density fiberboard (MDF), tiles, polyvinyl chloride sheets, and stone materials.

[0085] Examples of materials that make up the underfloor material include plywood, particle board, wooden joists, gypsum board, slate boards, and concrete boards. Effect of the Invention

[0086] The curable composition of the present invention has a low viscosity before curing and therefore has excellent handleability and coatability.

[0087] The curable composition of the present invention produces a cured product by curing, and this cured product has excellent water-resistant adhesion because the gap between molecules is small and swelling caused by water absorption is suppressed while maintaining excellent flexibility. Furthermore, the cured product also has excellent toughness, smoothly follows the distortion or deformation of the adherend without causing damage such as breakage, and exhibits excellent normal adhesion.

[0088] As described above, the cured product of the curable composition of the present invention maintains excellent flexibility, and therefore, when bonding adherends having different linear expansion coefficients, smoothly follows the distortion associated with the difference in the degree of deformation of the two adherends, and has excellent normal state adhesion. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0089] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0090] The following raw materials were used in producing the curable compositions of the Examples and Comparative Examples.

[0091] [Polyoxyalkylene polymer (A)] Polyoxyalkylene polymer (A1) (polyoxypropylene polymer having a polyoxypropylene main chain and a branched chain, hydrolyzable silyl group (bonded to the end of the main chain): dimethoxysilyl group, number of carbon atoms in the branched chain: 2 or more and 12 or less, number average molecular weight: 15,000, product name "Exestar 6250" manufactured by AGC) Polyoxyalkylene polymer (A2) (polyoxypropylene polymer having a polyoxypropylene main chain and a branched chain, hydrolyzable silyl group (bonded to the end of the main chain): dimethoxysilyl group, number of carbon atoms in the branched chain: 2 or more and 12 or less, number average molecular weight: 38,000, product name "S303" manufactured by Kaneka Corporation)

[0092] [Polyoxyalkylene polymer (B)] Polyoxyalkylene polymer (B1) (polyoxypropylene polymer with a linear polyoxypropylene main chain, no branched chain in the main chain, hydrolyzable silyl groups (bonded to both ends of the main chain): dimethoxysilyl groups, hydrolyzable silyl groups bonded to the ends of the main chain via alkylene groups, number average molecular weight: 21,000, AGC product name "Exestar 2420") Polyoxyalkylene polymer (B2) (polyoxypropylene polymer with a linear polyoxypropylene main chain, no branched chain in the main chain, hydrolyzable silyl group (bonded only to one end of the main chain): dimethoxysilyl group, hydrolyzable silyl group bonded to the end of the main chain via an alkylene group, number average molecular weight: 8500, Kaneka Corporation product name "SAT145") Polyoxyalkylene polymer (B3) (polyoxypropylene polymer whose main chain is a linear polyoxypropylene, no branched chain in the main chain, hydrolyzable silyl group (bonded to both ends of the main chain): dimethoxysilyl group, hydrolyzable silyl group bonded to the end of the main chain via an alkylene group, number average molecular weight: 4500, Kaneka Corporation product name "SAT015")

[0093] [Plasticizer] Polypropylene glycol (without hydrolyzable silyl groups, number average molecular weight: 2000)

[0094] [Inorganic filler] Surface-treated precipitated calcium carbonate (calcium carbonate 1, average particle size of primary particles: 0.05 μm, surface treatment with fatty acid, manufactured by Maruo Calcium Co., Ltd., product name "Kalfine 200M") Heavy calcium carbonate with untreated surface (calcium carbonate 2, no surface treatment, average particle size of primary particles: 5 μm, Toyo Fine Chemical Co., Ltd. product name "Whiten P-30")

[0095] [Silane coupling agents] Amino group-containing silane coupling agent [N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, Shin-Etsu Chemical Co., Ltd. product name "KBM-603"]

[0096] [Silanol condensation catalyst] Dibutyltin bis(triethoxysilicate) (manufactured by Nitto Kasei Co., Ltd., product name "Neostan S-303")

[0097] (Examples 1 to 8, Comparative Examples 1 to 5) The polyoxyalkylene polymers (A) and (B), polypropylene glycol, calcium carbonates 1 and 2, the amino group-containing silane coupling agent, and the silanol condensation catalyst were mixed uniformly in a sealed stirrer under reduced pressure in the amounts shown in Table 1 to prepare curable compositions.

[0098] The viscosity of the obtained curable composition at 23° C. was measured in the manner described above. The normal adhesion and water-resistant adhesion of the obtained curable composition were measured in the manner described below.

[0099] For the obtained cured product of the curable composition, the maximum stress (Tmax) and elongation (Emax) were measured in the manner described above.

[0100] (normal adhesion) A slate board was used as the floor underlayment, and a polymer floor sheet commercially available from Takiron Co., Ltd. under the product name "Takistron" was used as the floor finishing material. The curable composition was applied to the entire surface of the floor underlayment with a comb trowel at a rate of 350 g / mm. 2 After that, a floor finishing material was placed on the curable composition, and the floor finishing material was pressed onto the floor base material with a load of 5 kg. The curable composition was then cured for one week in an environment of 23°C and 50% relative humidity, and the state of destruction of the peeled surface was visually observed in accordance with JIS A5536 6.3.3 Floor finishing adhesive peel strength, and evaluated based on the following criteria.

[0101] A: Cohesive failure of the hardened product of the hardening composition or floor failure on 100% (entire surface) of the peeled surface. Material destruction occurred in the base material or floor finishing material. B. Cohesive failure of the cured product of the curable composition on 80% or more and less than 100% of the peeled surface. Or material destruction occurred in the floor underlayment or floor finishing material. C. Cohesive failure of the cured product of the curable composition on 50% or more and less than 80% of the peeled surface Or, material destruction occurs in the floor underlayment or floor finishing material, and other peeling surfaces occur. Interfacial destruction occurred between the floor underlayment or floor finishing material and the cured product of the curable composition. . D: Cohesive failure of the cured product of the curable composition on 1% or more and less than 50% of the peeled surface. Or, material destruction occurs in the floor underlayment or floor finishing material, and other peeling surfaces occur. Interfacial destruction occurred between the underfloor material or floor finishing material and the cured product of the curable composition. E. Cohesive failure of the hardened composition or the floor underlayment on less than 1% of the peeled surface. or destruction of the floor finishing material occurs, and on other peeling surfaces, damage to the floor underlayment or floor finishing material occurs. Interfacial destruction occurred between the bonding material and the cured product of the curable composition.

[0102] (Water resistant adhesive) Slate boards were used as the floor underlayment, and polymer floor sheeting sold by Takilon under the product name "Takistron" was used as the floor finish material. After curing for one week in an environment of 23°C and 50%, the material was immersed in 23°C water for one week, and measurements were made in accordance with JIS A5536 6.3.3 Floor finish adhesive peel strength. The state of destruction was visually observed and evaluated according to the following criteria.

[0103] A: Cohesive failure of the hardened composition or the floor underlayment on 80% or more of the peeled surface. Material destruction had occurred in the floor covering or floor finishing materials. B. Cohesive failure of the cured product of the curable composition on 50% or more and less than 80% of the peeled surface Or, material destruction occurs in the floor underlayment or floor finishing material, and other peeling surfaces occur. Interfacial destruction occurred between the floor underlayment or floor finishing material and the cured product of the curable composition. . C. Cohesive failure of the cured product of the curable composition on 1% or more and less than 50% of the peeled surface. Or, material destruction occurs in the floor underlayment or floor finishing material, and other peeling surfaces occur. Interfacial destruction occurred between the underfloor material or floor finishing material and the cured product of the curable composition. D. Cohesive failure of the hardened composition or failure of the underfloor material in less than 1% of the peeled surface. or destruction of the floor finishing material occurs, and on other peeling surfaces, damage to the floor underlayment or floor finishing material occurs. Interfacial destruction occurred between the bonding material and the cured product of the curable composition.

[0104]

Table 1

Claims

1. a polyoxyalkylene polymer (A) having a branched main chain and a hydrolyzable silyl group at a molecular end; a polyoxyalkylene polymer (B) having a linear main chain, a hydrolyzable silyl group at only one end of the main chain, and a number average molecular weight of 3,000 or more and 8,500 or less; An aminosilane coupling agent, A curable composition for direct application to an adherend, characterized in that the ratio of the content of the polyoxyalkylene polymer (A) to the content of the polyoxyalkylene polymer (B) [parts by mass of polyoxyalkylene polymer (A) / parts by mass of polyoxyalkylene polymer (B)] is 1 or more (however, excluding a (meth)acrylic monomer having two or more (meth)acrylic groups in the molecule, and a photopolymerizable composition containing a photopolymerization initiator).

2. 2. The curable composition according to claim 1, wherein the polyoxyalkylene polymer (A) has a number average molecular weight of 18,000 or less.

3. 3. The curable composition according to claim 1, which is used as a construction adhesive.

4. 3. The curable composition according to claim 1, which is used as a floor adhesive.

Citation Information

Patent Citations

  • Silicone carbide fiberrreinforced ni alloy composite material and manu facturing process thereof

    JP1977026314A

  • Optically polymerizable composition, moisture-hardenable type pressure-sensitive adhesive sheet and connection of member

    JP2000273418A

  • Curable resin composition and adhesive composition

    JP2009155407A

  • Curable composition

    JP2011219554A

  • Curable composition

    JP2012126881A