Resin molded product having a printed portion and method for printing on resin molded product
Laser-irradiated grooves on resin molded products enhance adhesion and image quality, addressing peeling issues and design limitations in conventional methods.
Patent Information
- Application Number
- JP2020073797
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-02
- Filing Date
- 2020-04-17
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2040-04-17
AI Technical Summary
Conventional surface roughening methods for resin molded products, such as sandblasting and laser irradiation, fail to provide sufficient adhesion strength and high-quality printing, leading to peeling issues and design limitations.
A resin molded product with a laser-irradiated treated portion featuring grooves of 5 to 100 μm depth, preferably 20% or more of the printed area, coated with paint and optionally a primer, to enhance adhesion and image quality.
The method improves the adhesion strength and image quality of printed layers on resin molded products, preventing peeling and ensuring clear, durable prints.
Smart Images

Figure 0007590815000003 
Figure 0007590815000004 
Figure 0007590815000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin molded product having a printed portion and a method of printing on a resin molded product. [Background technology]
[0002] Resin molded products are used in various fields including automobiles, electrical appliances, industrial equipment, etc., due to their freedom of shape, and their application fields are not limited to mechanical parts, but also extend to external parts such as housings that require design. Accordingly, decorative techniques such as printing on the surface of resin molded products are required as a method of imparting design to resin molded products.
[0003] Patent Document 1 discloses a method for forming a coating film on a resin molded product, which comprises roughening at least a portion of the surface of a molded product made of a crystalline thermoplastic resin by sandblasting, shot blasting, or liquid honing so that the ten-point average roughness Rz is 10 μm≦Rz≦40 μm, and then applying a two-component curing resin composition in the form of a coating film to the roughened surface and curing it.
[0004] Patent Document 2 discloses a method for manufacturing a composite molded product by integrating a resin molded product with another molded product. In this method, a resin molded product containing a fibrous inorganic filler is irradiated with a laser to remove a portion of the resin, and a grooved resin molded product having grooves in which the inorganic filler is exposed in a bridging manner is obtained. The grooved surface of the grooved resin molded product is then integrated with another molded product made of a thermoplastic resin or a thermosetting resin, with the grooved surface being the contact surface. According to this method, the inorganic filler exposed in a bridging manner plays the role of an anchor at the interface between the grooved resin molded product and the other molded product, and as a result, the strength of the composite molded product can be significantly increased. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 2002-97292 [Patent Document 2] Patent No. 5632567 Summary of the Invention [Problem to be solved by the invention]
[0006] Conventional techniques for roughening the surface of molded products by grinding, such as sand blasting, shot blasting, liquid honing, or filing, have been able to improve the adhesion strength of the printed layer on the roughened printed area to a certain extent, but for molded products used in harsh environments, such as molded products used outdoors or molded products where the printed area comes into contact with other materials, peeling of the printed layer can be a problem, and there is a demand for further improvement in the adhesion strength of the printed layer.In addition, from the perspective of design, a high level of appearance (image quality) of the print is also required.
[0007] The present invention has been made to solve the above-mentioned problems, and its object is to provide a resin molded product having a printed portion with excellent design and high adhesion strength, and a printing method for a resin molded product. [Means for solving the problem]
[0008] The present inventors have achieved the above object by the following means.
[0009] 1. A resin molded product made of a resin composition having a printing portion for printing with paint, The resin composition is a resin composition that does not contain an inorganic filler, The printed part has a treated area formed by irradiation with laser light, and the treated area has a groove having a depth of 5 to 100 μm. 2. The resin molded product according to 1 above, wherein the groove is formed over an area of 20% or more of the printed portion. 3. The resin molded product according to any one of 1 to 2 above, wherein the printed portion is coated with the paint. 4. The resin molded product according to any one of 1 to 3 above, wherein a primer is applied to the printed portion, and then the paint is applied thereto. 5. A method for printing on a resin molded product made of a resin composition that does not contain an inorganic filler, comprising the steps of providing a printing area on the surface of the resin molded product, the printing area including a treatment area formed by irradiating a laser beam, and applying paint to the printing area to form a printing layer. 6. A printed matter having a printed layer on the grooves of a resin molded article having grooves, the grooves having a depth of 5 to 100 μm, and the resin molded article being made of a resin composition that does not contain a filler. Effect of the Invention
[0010] According to the present invention, it is possible to obtain a molded article having a printed portion which has excellent appearance of the print and which solves the problem of peeling of the printed layer from the resin molded article. [Brief description of the drawings]
[0011] [Figure 1] 1 is a photograph of a printed matter on which a sample image is printed in Example 1. [Diagram 2] This is a photograph of the sample image in Example 1, in which a grid pattern was cut into the sample image with a cutter knife. [Diagram 3] 1 is a photograph of the printed matter of Example 1 after a peeling test using cellophane tape. [Figure 4] 1 is a photograph of the printed matter of Example 4 after a peeling test using cellophane tape. [Diagram 5] 13 is a photograph of the printed matter of Comparative Example 3 after a peeling test using cellophane tape. [Figure 6] 13 is a photograph of the printed matter of Comparative Example 5 after a peeling test using cellophane tape. [Figure 7] 1 is a photograph of a printed matter according to an embodiment of the present invention, in which the area surrounded by the dashed line is a laser processing area. [Figure 8] 8 is a photograph of the printed matter in FIG. 7 after testing. The area within the dashed line is the laser-treated part. [Figure 9] 4 is a photograph of a print according to another embodiment of the present invention. [Figure 10] 10 is an enlarged photograph of an unpainted portion of the print in FIG. 9. [Figure 11]10 is an enlarged photograph of the printed portion of the print in FIG. 9. [Figure 12] 10 is an enlarged photograph of an unpainted portion of the printed matter according to FIG. 9 after testing. [Figure 13] 10 is an enlarged photograph of the printed portion of the print of FIG. 9 after testing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The following describes in detail the embodiments of the present invention, but the present invention is not limited to the following embodiments and can be modified as appropriate within the scope of the object of the present invention. Note that, where the description overlaps, the description may be omitted as appropriate, but this does not limit the gist of the invention.
[0013] <Resin molded products> The resin molded product of the present invention is a resin molded product made of a resin composition having a printed portion for printing with paint, the resin composition being a resin composition that does not contain an inorganic filler, the printed portion having a treated portion formed by irradiation with laser light, and the treated portion having a groove having a depth of 5 to 100 μm.
[0014] <Resin> The resin contained in the resin composition constituting the resin molded product of the present invention is not particularly limited as long as it is capable of forming a processed portion by laser irradiation described below, and examples of the resin include crystalline resins such as polyamide (PA), polybutylene terephthalate (PBT), polyethylene terephthalate (PET), polyphenylene sulfide (PPS), and liquid crystal polymer (LCP), and amorphous resins such as acrylonitrile-styrene copolymer (AS), acrylonitrile-butadiene-styrene (ABS), polycarbonate (PC), and polystyrene (PS).
[0015] In addition, since it is desirable for the resin molded product to be opaque when processing the resin using the method described below, it is preferable to use a crystalline resin as the resin, and the proportion of crystalline resin in the total resin component is preferably 40 mass % or more, more preferably 50 mass % or more, and even more preferably 60 mass % or more.
[0016] Since it is preferable that the resin constituting the resin composition of the present invention is opaque, it is also preferable to add a colorant (light absorber) such as a dye or pigment to the resin composition, and it is more preferable to add an inorganic colorant (e.g., carbon black) rather than an organic colorant.
[0017] By adding such a colorant, it becomes possible to remove the resin from transparent amorphous resins using the method described below. However, since amorphous resins usually have low chemical resistance (i.e., high affinity with paints and inks) and are therefore easier to print with than crystalline resins, the present invention is more effective with crystalline resins, which have high demands for printability.
[0018] <Processing section> The treated area of the present invention is a portion of the resin surface that has been treated by laser irradiation. The treated area that has been irradiated with the laser becomes foamed by the heat of the laser, or forms a groove having a bubble-like surface (a shape where bubbles have burst, hereinafter also referred to as a bubble shape).
[0019] The grooves in the resin molded product of the present invention are preferably formed by irradiating the surface of the resin molded product with a laser beam before the grooves are formed, and partially removing the resin. The conditions such as the type, wavelength, output, and irradiation time of the laser beam may be appropriately selected depending on the resin composition constituting the target resin molded product, but it is preferable to adjust the depth of the grooves to 5 to 100 μm.
[0020] From the viewpoint of print adhesion strength and image quality, the depth of the groove is more preferably 10 to 80 μm, further preferably 15 to 60 μm, and particularly preferably 20 to 50 μm.
[0021] The reason why the adhesion strength of the print and the image quality are improved in the present invention is believed to be that the laser beam irradiation forms bubbles on the surface of the resin molded product, which improves the adhesion strength between the print layer of paint such as ink and the resin molded product, improves the wettability of the ink, etc., and at the same time suppresses excessive spreading. The bubbles are formed on both the bottom and side surfaces of the grooves.
[0022] In order to ensure image quality and adhesion strength, the area of the grooves to be formed is preferably 20% or more of the area of the printed part, more preferably 30% or more, even more preferably 40% or more, and particularly preferably 50% or more. There is no particular upper limit, and the laser light may be irradiated over the entire surface (100%) of the printed part.
[0023] This is the case where the line width of the laser light irradiated for forming the groove is larger than the scanning pitch during laser light irradiation.
[0024] When laser light is irradiated over the entire surface of a resin molded product to create grooves over the entire surface of the surface (i.e., when the entire surface of the surface is dredged), it may be difficult to determine the depth of the groove (i.e., how deep the surface layer has been removed) from the resin molded product after the treatment. However, the above-mentioned groove depth is set taking into consideration that if the groove is too deep, paint such as ink will sink into the deep groove, which will degrade the smoothness and color development of the printing surface and reduce image quality. Therefore, for products whose entire surface has been treated in the same way, there is no need to take the groove depth into consideration.
[0025] If the presence of a carbonized resin layer can be confirmed by Raman spectroscopic analysis of the groove portion, it can be determined that the groove has been formed by irradiation with laser light.
[0026] The resin composition constituting the resin molded product may contain other known additives (antioxidants, stabilizers, ultraviolet absorbers, lubricants, release agents, plasticizers, toughness improvers, flow improvers, hydrolysis resistance improvers, etc.) In particular, in the present invention, in order to promote the formation of bubbles in the grooves, a foaming agent, particularly a chemical foaming agent that generates gas by heat upon irradiation with laser light, may be contained.
[0027] In addition, when a resin composition that does not contain a component that foams the resin, such as the foaming agent described above, is used, the resin contained in the resin composition melts due to the energy of the laser light, and decomposes and sublimes when further exposed to energy. The gas generated during this process traps air bubbles in the molten resin, and the resin molded product takes on the foam shape described above.
[0028] Here, if there is a large difference between the melting point or softening temperature of the resin and the decomposition temperature, even if the resin is melted by irradiating it with laser light, it is necessary to irradiate it with higher energy in order to further promote foaming due to the generation of decomposition gas.
[0029] Therefore, if the irradiation energy is insufficient due to the settings of the laser irradiation device or limitations in the specifications, even if the resin can be melted, foaming due to decomposition may be insufficient, resulting in less formation of bubbles. Chemical foaming agents are advantageous in such cases.
[0030] It is also preferable to select a resin having as small a difference between its melting point and decomposition temperature as possible. The difference between the melting point and decomposition temperature (the value obtained by subtracting the melting point from the decomposition temperature) is, for example, preferably 250°C or less, more preferably 220°C or less, even more preferably 200°C or less, particularly preferably 180°C or less, and most preferably 160°C or less.
[0031] The thermal decomposition temperature referred to here means the temperature at which weight loss of 1% is measured using thermogravimetric analysis (TGA) in air (flow rate 100 ml / min) at a heating rate of 10° C. / min.
[0032] <Step of forming a printing layer on a resin molded product having grooves> Printing on the resin molded product having grooves of the present invention is carried out by applying paint such as ink to the printing portion having the grooves formed therein as described above.
[0033] As for paints, in addition to general paints, UV-curable paints, inks, etc., paints for undercoats used in vacuum deposition, sputtering, and ion plating, catalyst-containing paints as base coats for plating, etc. can also be used. In addition, additives contained in paints can impart functions to the printed layer (and thus to the printed matter, which is a resin molded product on which the printed layer is formed).
[0034] For example, if the material contains an antistatic agent or a conductive agent, it can impart various functions to the printed matter, such as antistatic properties or conductivity (or electromagnetic wave shielding properties or thermal conductivity); if the material contains an antibacterial agent or antifungal agent, it can impart antibacterial properties, antifungal properties, weather resistance agents or reflective agents; if the material contains a phosphorescent agent, it can impart weather resistance, high solar reflectivity, phosphorescence, and other functions.
[0035] In addition, the effect of the present invention can be obtained even if the step of forming the printing layer is performed after the step of forming the grooves, but it is preferable to leave as little time as possible between the steps in order to avoid deterioration of image quality due to adhesion of dust and the like to the grooves and deterioration of the adhesive strength of the paint. It is also preferable to use a continuous process.
[0036] The method of applying the paint is not limited to application with a brush or the like, and various methods commonly used in printing, such as spraying, transfer, and inkjet, can be selected as appropriate depending on the material and shape of the resin molded product, the size and type of image to be printed (photograph, text, fill-in, etc.), etc.
[0037] In addition, taking into consideration the affinity between the resin composition and the paint, a base such as a primer may be applied in advance to the printed portion of the resin molded product, and then the paint may be applied on top of that. EXAMPLES
[0038] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0039] Example 1 A polyacetal resin composition (DURACON (registered trademark) POM M90-44 CD3068, melting point 165°C, thermal decomposition temperature 281°C) manufactured by Polyplastics Co., Ltd., which was colored black with carbon black, was injection molded into a flat resin molded product measuring 80 mm x 80 mm x 3 mm at a cylinder temperature of 200°C, a mold temperature of 80°C, an injection speed of 16 mm / sec, and a holding pressure of 60 MPa.
[0040] A 64 mm x 64 mm central area of the smooth surface side of the obtained resin molded product, without any ejection pin marks, was irradiated with laser light at a wavelength of 1064 nm and an output of 90% using a Keyence laser marker MD-X1520 to create a printed area having a processed area in which grooves were formed in a grid pattern (diagonal grid pattern at ±45° to the flow direction) with a width of 100 μm and a pitch of 250 μm to a depth of 30 μm.
[0041] Next, a specified sample image was printed in the central 56 mm x 56 mm area of the printing section having the processing section using a Mimaki Engineering flatbed UV inkjet printer UJF-3042 with Mimaki Engineering genuine UV curable ink to form a printed layer and produce a printed matter.
[0042] Example 2 A printed layer was formed on a resin molded product in the same manner as in Example 1, except that the groove depth was set to 15 μm.
[0043] Example 3 A printed layer was formed on a resin molded product in the same manner as in Example 1, except that the groove depth was set to 5 μm.
[0044] Comparative Example 1 A printed layer was formed on a resin molded product in the same manner as in Example 1, except that the groove depth was set to 200 μm.
[0045] Comparative Example 2 A printed layer was formed on a resin molded product in the same manner as in Example 1, except that the groove depth was set to 1 μm.
[0046] Comparative Example 3 A printed layer was formed on a resin molded product in the same manner as in Example 1, except that laser light was not irradiated and grooves were not formed.
[0047] Comparative Example 4 Instead of irradiating the resin molded product with laser light, the surface of the molded product was polished to a depth of 15 μm with sandpaper having a grain size of P120 as specified in JIS R6010, and otherwise a printed layer was formed on the resin molded product in the same manner as in Example 1.
[0048] Example 4 A printing layer was formed on a resin molded product in the same manner as in Example 1, except that a polybutylene terephthalate resin composition manufactured by Polyplastics Co., Ltd. (Duranex (registered trademark) PBT 2002 ED3002, melting point 224°C, thermal decomposition temperature 379°C) colored black with carbon black was used as the resin composition.
[0049] Example 5 A printed layer was formed on a resin molded product in the same manner as in Example 4, except that the groove depth was set to 15 μm.
[0050] Example 6 A printed layer was formed on a resin molded product in the same manner as in Example 4, except that the groove depth was set to 5 μm.
[0051] Comparative Example 5 A printed layer was formed on a resin molded product in the same manner as in Example 4, except that the groove depth was set to 1 μm.
[0052] Example 7 A polyphenylene sulfide resin composition manufactured by Polyplastics Co., Ltd. (Durafide (registered trademark) PPS 0220A9 HD9100, melting point 278°C, thermal decomposition temperature 494°C) colored black with carbon black manufactured by Polyplastics Co., Ltd. was used as the resin composition, and a printing layer was formed on a resin molded product in the same manner as in Example 1, except that the groove depth was 20 μm.
[0053] Comparative Example 6 A printed layer was formed on a resin molded product in the same manner as in Example 7, except that the groove depth was set to 3 μm.
[0054] <Result> For each example and comparative example, a cutter knife was used to make six cuts in the vertical and horizontal directions at 2 mm intervals on the coating surface, forming a total of 25 2 mm squares, and Nichiban cellophane tape was applied on top of the grid in accordance with JIS K5400 (1990), which was then adhered to the coating surface. The cellophane tape was then peeled off, and the peeling state of the coating surface was observed, and the evaluation score for the cross-cut test was confirmed. The test was performed five times for each level, and the evaluation score was the average of the five times.
[0055] JIS K5400 has six evaluation points: 10, 8, 6, 4, 2, and 0. The six points are based on the following criteria. Rating score: 10: Each cut is small and smooth on both sides, with no peeling at the intersections of the cuts or at any of the squares. Evaluation score 8: There is slight peeling at the intersections of the cuts, there is no peeling in any of the squares, and the area of the missing parts is within 5% of the total square area. Score 6: There is peeling on both sides and at the intersection of the incision, and the area of the missing part is more than 5% but less than 15% of the total square area. Evaluation score 4: The width of the peeling due to the cut is wide, and the area of the missing part is more than 15% but less than 35% of the total square area. Evaluation score 2: The width of the peeling due to the cut is wider than 4 points, and the area of the missing part is more than 35% but less than 65% of the total square area. Evaluation score: 0: The peeled area exceeds 65% of the total square area. Additionally, the print clarity was visually observed.
[0056] The results for the polyacetal resin composition were as follows: Example 1 and Example 2 received 10 points, Example 3 received 8 points, Comparative Examples 2 and 3 received 0 points, and Comparative Example 4 received 2 points. Comparative Example 1 received 10 points for the peeling state, but the ink had sunk into the image quality grooves before the peeling test, making the image dull, and clear printing was not possible.
[0057] The results for the polybutylene terephthalate resin composition were 10 points for Example 4, 8 points for Examples 5 and 6, and 2 points for Comparative Example 5. The image quality before the peel test was clear in all cases.
[0058] The results for the polyphenylene sulfide resin composition were 8 points for Example 7 and 2 points for Comparative Example 6. The image quality before the peel test was clear in all cases.
[0059] [Table 1]
[0060] [Table 2]
[0061] The indications in the table have the following meanings. * :Printing is unclear **: Treated with sandpaper
[0062] A polyacetal resin composition (DURACON (registered trademark) POM M90-44 CD3068, melting point 165°C, thermal decomposition temperature 281°C) manufactured by Polyplastics Co., Ltd., which was colored black with carbon black, was injection molded into a 50 mm x 70 mm x 3 mm plate-shaped resin molded product at a cylinder temperature of 200°C, a mold temperature of 80°C, an injection speed of 16 mm / sec, and a holding pressure of 60 MPa.
[0063] Using a Keyence laser marker MD-X1520, a 40mm x 40mm section in the center of the obtained resin molded product was irradiated with laser light at a wavelength of 1064nm and an output of 90% to form a lattice-like groove (a diagonal lattice at ±45° to the flow direction) with a width of 100μm and a pitch of 250μm, with a depth of 20μm, to provide a printed section, and one side of the resin molded product including the printed section was undercoated with a two-component urethane paint, after which a film of aluminum was formed by vacuum deposition to a thickness of about 10μm to produce a printed product. Figure 7 shows the printed product after film formation.
[0064] Using a cutter knife, 6 scratches were made in both the vertical and horizontal directions at 2 mm intervals in the printed area that had been laser-treated on the obtained print, forming a total of 25 2 mm squares, and Nichiban cellophane tape was attached on top of the squares in accordance with JIS K5400 (1990), and after it was pressed against the film-forming surface, the cellophane tape was peeled off and the peeling state of the paint / film-forming area was observed. Figure 8 is a photograph of the print after the test, and the peeling state of the laser-treated area was rated 8 points, while the non-laser-treated area was completely peeled off and rated 0 points.
[0065] A polyacetal resin composition (DURACON (registered trademark) POM M90-44 CD3068, melting point 165°C, thermal decomposition temperature 281°C) manufactured by Polyplastics Co., Ltd., which was colored black with carbon black, was injection molded into a 50 mm x 70 mm x 3 mm plate-shaped resin molded product at a cylinder temperature of 200°C, a mold temperature of 80°C, an injection speed of 16 mm / sec, and a holding pressure of 60 MPa.
[0066] A 40mm x 40mm central part of the obtained resin molded product was irradiated with laser light at a wavelength of 1064 nm and an output of 90% using a Keyence laser marker MD-X1520 to form a lattice-like groove (diagonal lattice at ±45° to the flow direction) with a width of 100 μm and a pitch of 250 μm to a depth of 30 μm to provide a printed part, and a 35 x 35 mm part of the printed part was printed with Mimaki Engineering's genuine UV-curable ink using a flatbed UV inkjet printer UJF-3042 manufactured by Mimaki Engineering. Figure 9 shows the printed part. Figure 10 is an enlarged photograph of the unpainted part of the printed part in Figure 9, and Figure 11 is an enlarged photograph of the printed part of Figure 9.
[0067] The print obtained above was treated for 600 hours with an ultraviolet carbon arc lamp and a black panel temperature of 83°C. Figure 12 is an enlarged photograph of the unpainted part of the print, and streaky cracks have appeared on the surface. Figure 13 is an enlarged photograph of the printed part, and no cracks have appeared.
Claims
1. A resin molded product made of a resin composition having a printing portion for printing with paint, the resin composition is a polyacetal resin composition, a polybutylene terephthalate resin composition, or a polyphenylene sulfide resin composition that does not contain an inorganic filler; The printed part has a processed part formed by irradiation with laser light, and the processed part has a diagonal lattice-shaped groove having a depth of 5 to 100 μm and angled at ±45° to the flow direction (excluding the processed part which is irradiated with laser light on the entire surface).
2. The resin molded product according to claim 1 , wherein the groove is formed in an area of at least 20% of the printed portion.
3. The resin molded product according to claim 1 or 2, wherein the paint is applied to the printed portion.
4. 4. The resin molded product according to claim 1, wherein a primer is applied to the printed portion, and then the paint is applied to the printed portion.
5. A method for printing on a resin molded product made of a polyacetal resin composition, a polybutylene terephthalate resin composition, or a polyphenylene sulfide resin composition that does not contain an inorganic filler, comprising the steps of: providing a printing portion including a processing portion formed by irradiating a laser beam on a surface of the resin molded product; A step of applying paint to the printed portion to form a printed layer; having The processing portion has diagonal lattice-shaped grooves having a depth of 5 to 100 μm and angled at ±45° with respect to the flow direction.
6. A printed matter having a print layer on a groove of a resin molded product having a groove made of a resin composition having a printing portion for printing with a paint, The printing unit has a processing unit that uses laser light irradiation, The grooves are 5 to 100 μm deep and have a diagonal lattice pattern at an angle of ±45° to the flow direction, The resin molded article is a polyacetal resin composition, a polybutylene terephthalate resin composition, or a polyphenylene sulfide resin composition that does not contain a filler. Printed matter (excluding processed areas that are entirely irradiated with laser light).
Citation Information
Patent Citations
Inorganic thickkwall screen printing ink
JP1981032567A
Preparation of plastic molding
JP2000154266A
Method of forming coating on crystalline thermoplastic resin molding
JP2002097292A
Printing / coating method to polyacetal resin shaped article
JP2006167507A
Method of surface-treating aromatic polyether ketone resin-processed product, and the aromatic polyether ketone resin-processed product
JP2013253132A